Electromagnetic wave absorbing material, electromagnetic wave absorber, and electronic element, electronic component, or electronic device provided with said electromagnetic wave absorber
An electromagnetic wave absorbing material with a high volume ratio of non-magnetic metal powder in an insulating matrix addresses high-frequency absorption challenges by leveraging dielectric loss, achieving efficient and cost-effective wave absorption across a broad frequency range.
Patent Information
- Application Number
- JP2021053512
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-03-26
AI Technical Summary
Existing electromagnetic wave absorbers face challenges in achieving high-frequency absorption characteristics due to limitations imposed by Snoek's limit and difficulties in achieving high filling rates of magnetic or dielectric materials, leading to narrow absorption bands and increased costs for ceramic materials.
An electromagnetic wave absorbing material composed of an electrically insulating matrix with non-magnetic metal powder, such as copper or silver, dispersed at a high volume ratio of 55% or more, with controlled aspect ratio and particle size, utilizing dielectric loss for improved absorption.
The material achieves significant dielectric loss, enabling effective electromagnetic wave absorption in high frequency bands with a transmission attenuation rate of 10 dB or more from 0.1 GHz to 13 GHz, overcoming previous limitations and reducing production costs.
Smart Images

Figure 0007567615000009 
Figure 0007567615000010 
Figure 0007567615000011
Abstract
Description
[Technical field]
[0001] The present invention relates to an electromagnetic wave absorbing material, an electromagnetic wave absorber, and an electronic element, electronic component, or electronic device provided with the electromagnetic wave absorber. [Background technology]
[0002] With the rapid development of electronic, information and communication technology in recent years, the use of electromagnetic waves (radio waves) has increased rapidly, and the frequency and bandwidth of the electromagnetic waves used are becoming higher. Specifically, in addition to systems in the quasi-microwave band, such as mobile phones (1.5 GHz, 2.0 GHz) and wireless LAN (2.45 GHz), new systems using radio waves in the millimeter wave band, such as high-speed wireless LAN (65 GHz) and collision prevention radar (76.5 GHz), are being introduced.
[0003] As the use of electromagnetic waves expands and their frequencies increase, electromagnetic interference issues, such as malfunctions of electronic devices due to electromagnetic noise and adverse effects on the human body, are coming to the forefront, and there is a growing demand for EMC measures.One known method of EMC measures is to use electromagnetic wave absorbers (radio wave absorbers) to absorb unnecessary electromagnetic waves and prevent their intrusion.
[0004] An example of the basic structure of an electromagnetic wave absorber is shown in a schematic cross-sectional view in Figure 1. The electromagnetic wave absorber (1) is composed of an absorber body (2) and a metal film (3) that backs the absorber body (2). The absorber body (2) is composed of an electromagnetic wave absorbing material. An incident wave (4) that enters the absorber body (2) is partially reflected (5) by the absorber surface, and the remainder penetrates into the absorber. The penetrating electromagnetic wave is reflected by the metal film (3), and part of it is radiated outside the absorber as a reflected wave (6).
[0005] Electromagnetic wave attenuation mechanisms are classified into two types: attenuation due to interference between the reflected wave (5) from the absorber surface and the reflected wave (6) from the absorber back surface (interference attenuation), and attenuation due to absorption inside the absorber body (2). Interference attenuation utilizes the phenomenon in which the reflected wave (5) from the absorber surface and the reflected wave (6) from the absorber back surface cancel each other out when the thickness (d) of the absorber body (2) and the wavelength (λ) of the incident electromagnetic wave have a specific relationship. The interference phenomenon requires strict control of the thickness of the absorber body (2), and there is a problem that the absorption characteristics decrease depending on the angle of incidence of the electromagnetic wave. Another problem is that the absorption band is narrow. In contrast, absorption attenuation utilizes the phenomenon in which the absorber body (2) absorbs the energy of the incident electromagnetic wave (electromagnetic wave energy), converts it into thermal energy, and radiates it. The absorption phenomenon has the advantage that the thickness of the absorber body (2) can be controlled to a certain extent freely, and the absorption band can be widened.
[0006] In order to effectively utilize absorption attenuation, it is important to use an absorber (absorbent material) that exhibits excellent absorption characteristics. Specifically, for practical purposes, it is desirable for the transmission attenuation rate of the absorber to be 10 dB or more in the absorption band.
[0007] Electromagnetic wave absorption utilizes the magnetic loss, dielectric loss, or resistive loss of the material that makes up the absorber, and absorbers that utilize these losses are called magnetic electromagnetic wave absorbers, dielectric electromagnetic wave absorbers, and resistive electromagnetic wave absorbers, respectively. Of these, magnetic electromagnetic wave absorbers are widely used because they exhibit excellent absorption properties.
[0008] Magnetic electromagnetic wave absorbers utilize the loss that occurs due to the magnetic resonance of ferromagnetic materials. That is, ferromagnetic materials have a magnetic moment based on the spin angular momentum of electrons (3d electrons) bound to atoms of magnetic elements (Fe, Ni, Co, etc.). The magnetic moments are aligned through exchange interactions and other actions, resulting in spontaneous magnetization. When electromagnetic waves are irradiated onto a magnetic material, the direction of magnetization fluctuates (magnetization oscillation) due to domain wall movement in the low frequency range and due to magnetization rotation in the high frequency range. As the frequency increases, the magnetization oscillation interferes with the electromagnetic wave at a specific frequency, resulting in the phenomenon of magnetization resonance, that is, magnetic resonance. At the frequency at which magnetic resonance occurs, the imaginary part of magnetic permeability (μ'') peaks and the loss is maximized. Loss due to magnetic resonance is called magnetic loss.
[0009] Soft magnetic metals and ferrites (iron oxides) have been known as materials for magnetic electromagnetic wave absorbers. Of these, soft magnetic metals have the advantage of being higher in saturation magnetization and magnetic permeability than ferrites, and are widely used as absorber materials. For example, Patent Document 1 discloses a high-frequency electromagnetic wave absorber characterized by being formed by dispersing soft magnetic flat powder with a powder thickness of 3 μm or less in an insulating base material (claim 1 of Patent Document 1). Patent Document 1 also describes that as the powder thickness is reduced, the peak frequency fr of μ″ (loss term of complex permeability) shifts to the high-frequency side, and μ″ characteristics exceeding the limit line (S; snake line) are obtained, and that high-frequency electromagnetic waves of 2 GHz or more that could not be absorbed in the past can be absorbed well (
[0012] and
[0014] of Patent Document 1).
[0010] Patent Document 2 discloses a flat powder for an electromagnetic wave absorber, which is characterized by consisting of, by mass, 9-12% Si, 1-5% Al, 1-5% Cr, with the remainder being Fe and impurities, and an electromagnetic wave absorber, which is characterized by being obtained by dispersing and kneading the flat powder in a flexible insulating material (Claims 1-3 of Patent Document 2).
[0011] On the other hand, dielectric electromagnetic wave absorbers that utilize dielectric loss are also known. For example, Patent Document 3 discloses that a dielectric loss material containing a conductive material such as boron carbide, conductive carbon powder, and silicon carbide and an insulating material is applied to an electromagnetic wave absorber (claims 1 to 10 of Patent Document 3). Patent Document 3 also describes that the electromagnetic wave absorber is lightweight and exhibits excellent electromagnetic wave absorbing properties with a wide absorption frequency band in the high frequency range (
[0007] of Patent Document 3).
[0012] [Patent Document 1] Japanese Patent Application Publication No. 11-087117 [Patent Document 2] JP 2008-050644 A [Patent Document 3] JP 2007-019287 A Summary of the Invention [Problem to be solved by the invention]
[0013] Although electromagnetic wave absorbers that utilize magnetic loss or dielectric loss (magnetic electromagnetic wave absorbers, dielectric electromagnetic wave absorbers) have been proposed in the past, there is still room for improvement in the electromagnetic wave absorption characteristics. That is, a theory called Snoek's limit is known regarding magnetism, and according to this theory, there is a relationship between the upper limit of magnetic permeability and the resonance frequency of a magnetic material. For example, in materials with small magnetic anisotropy, the product of the upper limit of magnetic permeability and the resonance frequency is constant. Therefore, it is not possible to increase the resonance frequency while maintaining a high magnetic permeability.
[0014] In Patent Documents 1 and 2, flat soft magnetic powder is used to improve the absorption characteristics at high frequencies by utilizing the magnetic anisotropy caused by the shape anisotropy. However, it is still difficult to break through the snake's limit and significantly improve the absorption characteristics at high frequencies. In addition, since the flat powder has poor packing properties, it is difficult to manufacture an absorber containing magnetic powder at a high packing rate. Therefore, there are limitations in improving the absorption characteristics and increasing the frequency. In addition, Patent Document 3 aims at a dielectric electromagnetic wave absorber, but it is necessary to prepare a conductive ceramic material such as boron carbide. These ceramic materials require special methods such as high temperature and high pressure synthesis to manufacture them, which has the problem of easily leading to increased costs.
[0015] The present inventors have conducted extensive research in light of the above-mentioned conventional circumstances. As a result, they have found that in a material containing an electrically insulating matrix and non-magnetic metal powder, the dielectric loss has a maximum value by controlling the shape and content ratio of the non-magnetic metal powder. They have also found that by utilizing this dielectric loss, it is possible to obtain an electromagnetic wave absorbing material and an electromagnetic wave absorber that can be used in practical applications in the high frequency band.
[0016] The present invention was completed based on such findings, and an object of the present invention is to provide an electromagnetic wave absorbing material and an electromagnetic wave absorber that utilize dielectric loss and can be put to practical use in high frequency bands. [Means for solving the problem]
[0017] The present invention includes the following aspects (1) to (10). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."
[0018] (1) An electromagnetic wave absorbing material comprising an electrically insulating matrix and a non-magnetic metal powder dispersed in the electrically insulating matrix, The content of the non-magnetic metal powder is 55% by volume or more, The nonmagnetic metal powder has an average aspect ratio of 5.0 or less, The electromagnetic wave absorbing material has a dielectric loss tangent (tanδ) in a frequency band of 0.1 GHz to 13 GHz. E ) peak, and the dielectric tangent (tan δ E ) value is 0.05 or greater.
[0019] (2) The electromagnetic wave absorbing material according to (1) above, wherein the content of the non-magnetic metal powder is 60% by volume or more.
[0020] (3) The electromagnetic wave absorbing material according to (1) or (2) above, wherein the non-magnetic metal powder is at least one selected from the group consisting of copper (Cu) powder, copper (Cu) alloy powder, silver (Ag) powder, and silver (Ag) alloy powder.
[0021] (4) The electromagnetic wave absorbing material according to any one of the above (1) to (3), wherein the non-magnetic metal powder has a volume average particle size (D50) of 2.0 μm or more.
[0022] (5) The electromagnetic wave absorbing material according to any one of the above (1) to (4), wherein the non-magnetic metal powder is a mixed powder of metal powders having different volume average particle sizes (D50).
[0023] (6) The above electricity The electromagnetic wave absorbing material according to any one of the above (1) to (5), wherein the insulating matrix contains at least one of a base oil, a wax, and a rosin.
[0024] (7) An electromagnetic wave absorber comprising a molded article of the electromagnetic wave absorbing material according to any one of (1) to (6) above.
[0025] (8) The electromagnetic wave absorber according to (7) above, wherein the electromagnetic wave absorber has a thickness of 0.5 mm or more in the electromagnetic wave incident direction.
[0026] (9) The electromagnetic wave absorber according to (7) or (8) above, which has a region in which the transmission attenuation rate per mm thickness is 10 dB or more in a frequency band of 0.1 GHz or more and 13 GHz or less.
[0027] (10) An electronic element, electronic part, or electronic equipment comprising the electromagnetic wave absorber according to any one of (7) to (9) above. Effect of the Invention
[0028] According to the present invention, there are provided an electromagnetic wave absorbing material and an electromagnetic wave absorber which utilize dielectric loss and can be put to practical use in high frequency bands. [Brief description of the drawings]
[0029] [Figure 1] FIG. 2 is a conceptual diagram showing an example of an electromagnetic wave absorber. [Diagram 2] 1 is a graph showing a transmission attenuation rate of an electromagnetic wave absorber. [Diagram 3] 1 is a graph showing a transmission attenuation rate of an electromagnetic wave absorber. [Figure 4] 1 is a graph showing the complex relative dielectric constant (real part, imaginary part) of an electromagnetic wave absorber. [Diagram 5] 1 is a graph showing the complex relative permeability (real part, imaginary part) of an electromagnetic wave absorber. [Figure 6] 1 is a graph showing a transmission attenuation rate of an electromagnetic wave absorber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.
[0031] <<1. Electromagnetic wave absorbing materials>> The electromagnetic wave absorbing material (hereinafter sometimes referred to as "material") of this embodiment includes an electrically insulating matrix and non-magnetic metal powder dispersed in the electrically insulating matrix. Here, the electromagnetic wave absorbing material is a precursor for molding it to produce an electromagnetic wave absorber. In other words, by molding the electromagnetic wave absorbing material, an electromagnetic wave absorber having a shape such as a sheet can be produced. In this specification, powder means an aggregate of multiple independent particles. It can also be said that multiple particles constitute the powder.
[0032] (1) Non-magnetic metal powder The non-magnetic metal powder (hereinafter sometimes referred to as "metal powder") is dispersed in an electrically insulating matrix. That is, the particles that make up the metal powder are separated from one another via the components that make up the matrix (matrix components). However, it is not necessary for all particles to be separated. Some particles may be in contact with one another as long as this does not impair the electromagnetic wave absorption properties.
[0033] Non-magnetic metal powders are composed of non-magnetic metals. Non-magnetic metals are metals other than ferromagnetic metals, i.e., metals that do not have spontaneous magnetization at room temperature. More specifically, non-magnetic metals are metals other than ferromagnetic metals, such as iron (Fe), cobalt (Co), nickel (Ni), gadolinium (Gd), and tetragonal ruthenium (Ru). Non-magnetic metal powders do not contain ferromagnetic metals in excess of the impurity amount.
[0034] The material of the non-magnetic metal powder is not limited as long as it is made of a non-magnetic metal. Examples of non-magnetic metals include gold (Au), silver (Ag), palladium (Pd), copper (Cu), aluminum (Al), and zinc (Zn). The metal powder may be made of a single metal or an alloy. Here, the concept of alloy includes not only solid solutions but also intermetallic compounds. The non-magnetic metal powder may be made of only one type of metal powder, or may contain a mixture of multiple types of metal powder. From the viewpoint of reducing conductor loss during non-resonance, the smaller the electrical resistance of the non-magnetic metal powder, the more preferable it is. Preferably, the volume resistivity of the non-magnetic metal powder is 10 -5 It is less than Ωm.
[0035] Preferably, the non-magnetic metal powder is at least one selected from the group consisting of copper (Cu) powder, copper (Cu) alloy powder, silver (Ag) powder, and silver (Ag) alloy powder. These powders are easily available and have low electrical resistance. Therefore, it is possible to reduce conductor loss in frequency ranges other than the absorption band. Furthermore, they are less expensive than gold (Au) and are less susceptible to oxidation than aluminum (Al) and zinc (Zn). Therefore, it is possible to manufacture an absorber with excellent electromagnetic wave absorption properties at low cost.
[0036] In the electromagnetic wave absorbing material of this embodiment, the content of non-magnetic metal powder is 55 volume % or more. By incorporating non-magnetic metal powder at a high filling rate in the absorbing material in this manner, it becomes possible to impart electromagnetic wave absorbing properties based on dielectric loss to the material. Specifically, the imaginary part of the dielectric constant (ε'') becomes maximum at a specific frequency (dielectric loss peak frequency), and the absorbing properties are maximized in the vicinity of that frequency.
[0037] The detailed reason why the electromagnetic wave absorbing material of this embodiment exhibits electromagnetic wave absorbing properties based on dielectric loss is unclear. Although it should not be interpreted in a limited manner based on a specific theory, it is speculated as follows. That is, each particle constituting the metal powder is separated from each other via a matrix component. In other words, the matrix component is interposed between the particles. Since the matrix component has electrical insulation properties, capacitance occurs in the matrix component interposed between the particles. In addition, the higher the filling rate of the metal powder, the smaller the average interval between adjacent particles, i.e., the thickness of the matrix component interposed between the particles. Therefore, the capacitance increases, and as a result, the effective dielectric constant shown by the entire material increases. It is believed that the matrix exhibits a dielectric relaxation phenomenon, or that the capacitance component (C component) of the matrix acts with the resistance component (R component) and / or induction component (L component) of the metal powder to exhibit a resonance phenomenon, thereby increasing the dielectric loss at a specific frequency. On the other hand, it is speculated that if the content of the metal powder is less than 55% by volume, the capacitance component becomes too small, resulting in insufficient electromagnetic wave absorbing properties.
[0038] In order to improve the electromagnetic wave absorption properties, the higher the content of the non-magnetic metal powder, the more preferable. The content may be 60 volume % or more, 65 volume % or more, 70 volume % or more, 75 volume % or more, or 80 volume % or more. On the other hand, if the content is too high, the particles constituting the metal powder are more likely to come into contact with each other. If the particles come into contact with each other, the capacitance component of the matrix will disappear, and there is a risk that the electromagnetic wave absorption properties will deteriorate. The content may be 95 volume % or less, 90 volume % or less, or 85 volume % or less.
[0039] In the electromagnetic wave absorbing material of this embodiment, the average aspect ratio of the nonmagnetic metal powder is 5.0 or less. The average aspect ratio is the average value of the aspect ratios of the multiple particles constituting the metal powder, and the aspect ratio is the ratio of the major axis diameter to the minor axis diameter of each particle (major axis diameter / minor axis diameter). By using a powder with a small average aspect ratio, it is possible to improve the electromagnetic wave absorption characteristics. That is, in a powder with a small average aspect ratio, the sphericity of each particle constituting the powder is high. Therefore, the friction acting between the particles is small, and the particles are densely packed during the material production. Therefore, an electromagnetic wave absorbing material with a high metal powder packing rate can be obtained. In contrast, in conventional magnetic electromagnetic wave absorbing materials, flat powder with large magnetic anisotropy is used. Such flat powder has a large aspect ratio, and it is difficult to increase the packing rate. In the electromagnetic wave absorbing material of this embodiment, since the electromagnetic wave absorption characteristics based on the dielectric loss are utilized, it is possible to use a metal powder with a small aspect ratio that has good packing properties. The average aspect ratio may be 4.0 or less, 3.0 or less, or 2.0 or less.
[0040] The non-magnetic metal powder preferably has a volume average particle size (D50) of 2.0 μm or more. By increasing the particle size, the electromagnetic wave absorption characteristics can be improved. Although the detailed reason is unclear, it is speculated that it is due to the skin effect. D50 is more preferably 2.0 μm or more, and more preferably 8.0 μm or more. There is no upper limit for D50. However, if D50 is excessively large, there is a risk that a homogeneous sheet or coating film cannot be obtained when it is made into a composition such as a sheet, grease, or paint. D50 is preferably 20.0 μm or less, and more preferably 15.0 μm or less. The volume average particle size (D50) can be calculated as the 50% cumulative diameter in the particle size distribution obtained by determining the volume particle size distribution using a method such as laser diffraction scattering.
[0041] The particle size distribution of the nonmagnetic metal powder is not limited. For example, it may show a multimodal particle size distribution or a unimodal particle size distribution. However, it is preferable to show a multimodal particle size distribution. This is because the fine powder fills the gaps between the coarse powder, and as a result, the filling rate of the metal powder is likely to be high. As a metal powder showing a multimodal particle size distribution, a mixed powder of metal powders with different volume average particle sizes (D50) can be mentioned. Specifically, a mixed powder of a fine powder with a volume average particle size (D50) in the range of 0.1 μm or more and less than 1.5 μm, a medium powder with a D50 in the range of 1.5 μm or more and less than 5 μm, and a coarse powder with a D50 in the range of 5 μm or more and 10 μm or less can be mentioned. In this case, the ratio of each powder can be fine powder: 5 vol% to 30 vol%, medium powder: 5 vol% to 30 vol%, and coarse powder: 30 vol% to 70 vol%. Here, the total of the fine powder, medium powder and coarse powder is 100% by volume or less.
[0042] (2) Electrically insulating matrix An electrically insulating matrix (hereinafter sometimes referred to as "matrix") is a base material (substrate) of an electromagnetic wave absorbing material. There are no limitations on the material of the matrix as long as it has electrical insulation. It may be composed of any of solids, liquids, gels, and mixtures thereof. Examples of insulating materials include organic compounds, resins, rubber, glass, and ceramics. In this specification, a material having electrical insulation is one whose volume resistivity (specific resistance) is 10 5 Refers to materials with a resistance of Ωcm or higher.
[0043] electricity The content of the insulating matrix is preferably 5.0% by volume or more and 45% by volume or less. Since the content of the metal powder is limited to 55% by volume or more, electricity The content of the insulating matrix is limited to 45% by volume or less.
[0044] electricity The insulating matrix preferably contains at least one of a base oil, a wax, and a rosin. That is, the insulating matrix may contain any one of a base oil, a wax, and a rosin, or may contain a combination of a plurality of the base oil, the wax, and the rosin. The insulating matrix may contain all of the base oil, the wax, and the rosin.
[0045] electricity The insulating matrix may contain a base oil. The base oil has the characteristics of high wettability to metal particles and excellent electrical insulation. Therefore, a thin electrically insulating coating can be provided on the particle surface using the base oil. In addition, the base oil has the characteristic that the coating formed on the particle surface is not easily destroyed because of its moderate viscosity. Therefore, even if the filling rate of the metal powder is increased, it is possible to prevent direct contact between the particles.
[0046] The type of base oil is not limited. It may be any of mineral oil, synthetic oil, vegetable oil, and animal oil. The mineral oil may be any of paraffin-based and naphthenic-based. As the synthetic oil, a hydrocarbon-based, ester-based, ether-based, silicone-based, fluorine-based, etc. may be used. Ester-based oils are preferable, and polyether esters are particularly preferable.
[0047] The base oil can form an electrically insulating matrix together with other components. The content of the base oil in the absorbent material is preferably 8.0 volume % or more and 40.0 volume % or less, more preferably 10.0 volume % or more and 35.0 volume % or less. By setting the content within the above range, it is possible to more effectively prevent direct contact between particles constituting the metal powder.
[0048] The electrical insulating matrix may contain wax. Wax has the effect of providing lubricity and also functions as a binder. That is, by using wax, the metal particles can slide more smoothly and the filling property is improved. In addition, since the wax solidifies at room temperature after the absorbing material is molded, it has the effect of binding the metal particles together and improving the shape retention. From the viewpoint of improving the dispersibility of the metal powder, it is preferable that the wax has a high acid value. The acid value of the wax is preferably 20 mg / g or more, more preferably 40 mg / g or more. In addition, the type of wax is not limited, but synthetic wax, vegetable wax, and / or petroleum wax are preferable.
[0049] The wax can form an electrically insulating matrix together with other components. The wax content in the absorbent material is preferably 2.0% by volume or more and 15.0% by volume or less, more preferably 4.0% by volume or more and 10.0% by volume or less. By keeping the wax content within the above range, the absorbent material can be given appropriate lubricity and shape retention.
[0050] The electrical insulating matrix may contain rosin. Rosin has the effect of imparting viscosity and also functions as a binder. In other words, the use of rosin has the effect of making the viscosity of the absorbing material appropriate and increasing the shape retention. From the viewpoint of improving the dispersibility of the metal powder, it is preferable that the rosin has a high acid value. The acid value of the rosin is preferably 100 mg / g or more, more preferably 120 mg / g or more. The type of rosin is not limited, but tall rosin, gum rosin, and / or wood rosin are preferred.
[0051] The rosin can form an electrically insulating matrix together with other components. The content of the rosin in the absorbent material is preferably 5.0% by volume or more and 20.0% by volume or less, more preferably 8.0% by volume or more and 15.0% by volume or less. By setting the content within the above range, it is possible to impart appropriate viscosity and shape retention to the absorbent material.
[0052] The electrically insulating matrix may contain a dispersant as necessary. The dispersant has the effect of increasing the affinity between the metal powder and the base oil. Therefore, by adding the dispersant, the dispersibility of the metal powder can be improved. Specifically, even when the filling rate of the metal powder is high, the base oil penetrates into the narrow gaps between the particles constituting the metal powder, and has the effect of suppressing direct contact between the particles.
[0053] The dispersant may be appropriately selected according to the surface state of the acid group and base of the powder. The metal powder often has a basic surface, and the dispersant applied thereto is preferably one with a high acid value. When a dispersant with a high acid value is used, the effect of improving the dispersibility of the metal powder becomes more pronounced. The acid value of the dispersant is preferably 5.0 mg / g or more, more preferably 20.0 mg / g or more. The type of dispersant is not limited, but is preferably polyether carboxylic acid, polyether phosphate ester, and / or higher fatty acid polyester. Furthermore, the content of the dispersant contained in the absorbing material is preferably 0.1 volume % or more and 3.0 volume % or less, more preferably 0.5 volume % or more and 2.0 volume % or less. By setting the content ratio within the above range, it is possible to fully exert the effect of improving the dispersibility.
[0054] The electrically insulating matrix may contain other components in addition to the base oil, wax, rosin, and dispersant. The other components may include rust inhibitors, metal deactivators, rheology control agents, and / or antioxidants. The other components may be appropriately selected depending on the application.
[0055] The electromagnetic wave absorbing material of this embodiment has a maximum value of dielectric loss in a high frequency band. For example, the dielectric loss is maximum in the frequency bands of ultrashort waves (30 MHz to 300 MHz), ultrashort waves (300 MHz to 1 GHz), quasi-microwaves (1 GHz to 3 GHz), and / or microwaves (3 GHz or higher). More specifically, the electromagnetic wave absorbing material has a dielectric loss tangent (tanδ) of 0.1 GHz to 13 GHz. E ) peak. Also, the dielectric tangent (tan δ E It is possible to increase the value (maximum value) of 0.05 or more, 0.10 or more, 0.15 or more, or 0.20 or more.
[0056] <<2. Manufacturing of electromagnetic wave absorbing materials>> The electromagnetic wave absorbing material of this embodiment may be produced by any method as long as it satisfies the above-mentioned requirements. For example, it may be produced by kneading the components constituting the matrix or their precursors with nonmagnetic metal powder. The kneading may be carried out using a known device such as a planetary mill, a planetary mixer, and / or a three-roll mill.
[0057] <<3. Electromagnetic wave absorber>> The electromagnetic wave absorber of this embodiment includes a molded body of the electromagnetic wave absorbing material described above. That is, it is produced by molding an electromagnetic wave absorber. The molding method is not limited. For example, the electromagnetic wave absorbing material may be molded into a sheet by a method such as a rolling roll or a doctor blade method. Alternatively, the electromagnetic wave absorbing material may be applied to a substrate to form a coating film. As long as a molded body can be obtained, the method is not limited.
[0058] The thicker the electromagnetic wave absorber is, the better its absorbing properties will be. The thickness in the electromagnetic wave incident direction is preferably 0.5 mm or more, more preferably 1.0 mm or more, and even more preferably 1.5 mm or more. The thickness in the electromagnetic wave incident direction is the thickness between the front and back surfaces of the electromagnetic wave absorber (electromagnetic wave absorbing material molded body), and the front and back surfaces refer to the surface facing the electromagnetic wave incident direction and the surface opposite thereto.
[0059] The electromagnetic wave absorber may include a member other than the electromagnetic wave absorbing material compact. For example, an impedance matching layer or a surface protection layer may be provided on the surface. A reflective member may be provided on the back surface. An example of the impedance matching layer is a layer in which magnetic powder or dielectric powder is dispersed in a resin. An example of the surface protection layer is a layer made of resin or glass. An example of the reflective member is a film-like, foil-like, or mesh-like metal member.
[0060] The electromagnetic wave absorber is not limited in its use, and may be applied to known uses. For example, it may be applied to an electronic element, electronic component, or electronic device equipped with an electromagnetic wave absorber. It may also be applied to architectural components such as the exterior and interior walls of a building. The manner of use is also not limited, and may be in a known manner. For example, a sheet-like or coated electromagnetic wave absorber may be attached to the exterior or interior surface of an electronic device housing. Alternatively, it may be provided on the exterior surface of an electronic component package. Furthermore, it may be provided with an electromagnetic wave absorber inside an electronic element or electronic component.
[0061] The electromagnetic wave absorber of this embodiment exhibits electromagnetic wave absorbing characteristics based on dielectric loss in high frequency bands. For example, it exhibits practical electromagnetic wave absorbing characteristics in the frequency bands of ultrashort waves (30 MHz to 300 MHz), ultrashort waves (300 MHz to 1 GHz), quasi-microwaves (1 GHz to 3 GHz), and / or microwaves (3 GHz or higher). More specifically, the electromagnetic wave absorber can have a region in which the transmission attenuation rate at a thickness of 1 mm is 10 dB or more, 15 dB or more, 20 dB or more, 25 dB or more, or 30 dB or more in a frequency band of 0.1 GHz to 13 GHz.
[0062] According to this embodiment, it is possible to obtain an electromagnetic wave absorbing material and an electromagnetic wave absorber that utilize dielectric loss and can be used in practical applications in the high frequency band. Such electromagnetic wave absorbing materials and electromagnetic wave absorbers have not been known in the past. For example, Patent Document 1 and Patent Document 2 propose that the soft magnetic powder contained in the electromagnetic wave absorber is flattened to obtain absorption characteristics that exceed the Snake limit. However, the electromagnetic wave absorbers disclosed in these documents utilize magnetic loss caused by ferromagnetic soft magnetic powder, and have a different electromagnetic wave absorption mechanism from the electromagnetic wave absorber of this embodiment that utilizes dielectric loss. In addition, soft magnetic flat powder has large friction between particles, making it difficult to achieve high packing.
[0063] Although Patent Document 3 proposes the application of a dielectric loss material to an electromagnetic wave absorber, the dielectric loss material used is a conductive material such as boron carbide, and is not a metal powder. In fact, Patent Document 3 discloses a comparative sample (Comparative Example 2) that contains 45 volume % aluminum powder, which is a metal powder, but this Comparative Example 2 is said to not exhibit absorption characteristics (Table 2 of Patent Document 3). EXAMPLES
[0064] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0065] [Experimental Example A] In Experimental Example A, copper (Cu) powder, which is a non-magnetic metal powder, was used as a filler, and electromagnetic wave absorbers containing various ratios of filler were fabricated, and the effect of the filler content ratio was investigated.
[0066] (1) Preparation of electromagnetic wave absorber [Example 1 to Example 3] Filler, base oil, dispersant, wax, and rosin were prepared as raw materials. Cu powder A (D50: 8.0 μm) shown in Table 1 below was used as the filler. In addition, the raw materials other than the filler (base oil, dispersant, wax, and rosin) shown in Table 2 below were used.
[0067] Next, the prepared raw materials (filler, base oil, dispersant, wax, and rosin) were weighed, and further kneaded using a planetary mixer (Thinky Corporation, Awatori Rentaro, model ART-930Twin) to obtain a kneaded product. In this way, an electromagnetic wave absorbing material was produced. The weighing was performed so as to obtain the compounding composition shown in Table 3 below. The kneading was performed for 4 minutes at a rotation speed of 1350 rpm.
[0068] The resulting kneaded material was then sandwiched between films and rolled to a predetermined thickness using a heated rolling roll (Imoto Manufacturing Co., Ltd., Model IMC-1A04) to obtain a sheet. The heated rolling was performed at a temperature of 100°C. The resulting sheet had a thickness of 1 mm, and was used for evaluation as an electromagnetic wave absorber.
[0069] [Table 1]
[0070] [Table 2]
[0071] [Table 3]
[0072] (2) Evaluation For Examples 1 to 3, various characteristics were evaluated as follows.
[0073] <Electromagnetic wave absorption characteristics> The electromagnetic wave absorption characteristics were evaluated by measuring the transmission attenuation rate using a microstrip line. Specifically, a sheet-shaped electromagnetic wave absorber was cut into a size of 10 cm x 5 cm to prepare a measurement sample. Next, the measurement sample was placed on a microstrip line (Keycom Corporation, model TF-6C), and a load (500 g) was applied on top of it. With the load applied, a high-frequency signal was input from a network analyzer to the microstrip line, and the reflection characteristics were measured. Then, using the S parameters (S11, S21), the transmission attenuation rate R was calculated according to the following formula (1): TP asked for.
[0074]
number
[0075] (3) Evaluation results The transmission attenuation rates of the samples obtained in Examples 1 to 3 are shown in FIG. 2. An increase in the transmission attenuation rate was observed in all samples in the frequency range around 6 GHz. Therefore, it was found that the samples exhibit electromagnetic wave absorption characteristics in this frequency band. It was also found that the greater the filler content, the higher the attenuation rate. Specifically, in Example 3, where the filler content was 50 volume % or more, the maximum attenuation rate was about 6 dB, whereas in Examples 1 and 2, where the filler content was 55 volume % or more, the maximum attenuation rate was 10 dB or more. From this, it was found that by increasing the filler content to 55 volume % or more, it is possible to realize an electromagnetic wave absorber that can be used in practical applications.
[0076] [Experimental Example B] In Experimental Example B, three types of Cu powder (filler) with different particle sizes were mixed to prepare electromagnetic wave absorbers containing various ratios of filler.
[0077] (1) Preparation of electromagnetic wave absorber [Example 4 to Example 7] Filler, base oil, dispersant, wax, and rosin were prepared as raw materials. As fillers, Cu powder A (D50: 8.0 μm), Cu powder B (D50: 2.0 μm), and Cu powder C (D50: 0.45 μm) shown in Table 1 were used. In addition, the raw materials other than the filler (base oil, dispersant, wax, and rosin) shown in Table 2 were used.
[0078] Next, an electromagnetic wave absorbing material and an electromagnetic wave absorber were prepared in the same manner as in Experimental Example A. The materials were weighed so as to obtain the blended compositions shown in the following Table 4. The thickness of the sheet was set to 1 mm.
[0079] [Table 4]
[0080] (2) Evaluation For Examples 4 to 7, the various characteristics were evaluated in the same manner as in Experimental Example A.
[0081] (3) Evaluation results The transmission attenuation rates of the samples obtained in Examples 4 to 7 are shown in Figure 3. As the filler loading rate increased, the absorption characteristics shifted to the lower frequency side. That is, while the absorption rate increased in the 4 GHz band, it tended to decrease in the 6 GHz band. In addition, the maximum attenuation rate was 20 dB or more in all samples, and in some samples it was 30 dB or more.
[0082] [Experimental Example C] (1) Evaluation In Experimental Example C, the complex relative dielectric constant (ε r =ε r '-jε r '') and complex relative permeability (μ r =μ r '-jμ r The measurement of ε r ' and ε r '' are the real and imaginary parts of the complex dielectric constant, respectively, and μ r ' and μ r'' are the real and imaginary parts of the complex relative permeability, respectively.
[0083] <Dielectric constant> The complex relative permittivity (εr = ε r '-jε r The coaxial tube S-parameter method was used to measure the dielectric constant of the sample. Specifically, a ring-shaped sample (inner diameter 3.06-3.10 mm, outer diameter 6.93-6.96 mm) was prepared and set in a coaxial tube holder. Measurements were then performed using a vector network analyzer (Anritsu Corporation, MS46122A). The real part of the dielectric constant (ε r ') and the imaginary part (ε r '') according to the following formula (2), E ) was calculated.
[0084]
number
[0085] <Magnetic permeability> Complex relative permeability (μ r =μ r '-jμ r The complex relative permeability was measured by the S-parameter reflection method. Specifically, the sheet-like electromagnetic wave absorber was punched into a doughnut-shaped disk to prepare a measurement sample (outer diameter 6.93-6.96 mm, inner diameter 3.06-3.10 mm, film thickness 2 mm). The measurement sample was then set in a jig, and the complex relative permeability was measured by sweeping the frequency using a vector network analyzer. The real part of the relative permeability (μ r ') and the imaginary part (μ r '') to calculate the loss factor (tanδ M ) was calculated.
[0086]
number
[0087] (2) Results The complex relative permittivity and complex relative permeability of the sample of Example 5 (Cu powder, filling rate 70 volume %) are shown in FIG. 4 and FIG. 5, respectively.
[0088] In Example 5, an increase in dielectric loss was confirmed near 7 GHz (Figure 4). That is, in this frequency band, the real part of the relative dielectric constant (ε r ') decreases, and the imaginary part of the relative dielectric constant (ε r '') and dielectric tangent (tanδ E ) was observed. On the other hand, no clear movement was observed in the magnetic permeability (Fig. 5). This shows that when non-magnetic metal powder is used as a filler, dielectric loss occurs, and that this dielectric loss can be utilized for absorption characteristics.
[0089] [Experimental Example D] In Experimental Example D, an electromagnetic wave absorber was produced by mixing three types of silver (Ag) powder (filler) having different particle sizes.
[0090] (1) Preparation of electromagnetic wave absorber [Example 8] Filler, base oil, dispersant, wax, and rosin were prepared as raw materials. As fillers, Ag powder A (D50: 5.0 μm), Ag powder B (D50: 1.5 μm), and Ag powder C (D50: 0.3 μm) shown in Table 1 were used. In addition, the raw materials other than the filler (base oil, dispersant, wax, and rosin) shown in Table 2 were used.
[0091] Next, an electromagnetic wave absorbing material and an electromagnetic wave absorber were produced in the same manner as in Experimental Example A. The components were weighed so as to obtain the blended compositions shown in the following Table 5. The thickness of the sheet was set to 1 mm.
[0092] [Table 5]
[0093] (2) Evaluation For Example 8, the various characteristics were evaluated in the same manner as for Experimental Example A.
[0094] (3) Evaluation results The transmission attenuation rate of the sample obtained in Example 8 is shown in Figure 6. An increase in the transmission attenuation rate was observed in the frequency range around 6 GHz. Therefore, it was found that the sample exhibited electromagnetic wave absorption properties in this frequency band. The maximum attenuation rate was 20 dB or more. This shows that it is possible to realize a practical electromagnetic wave absorber even if Ag powder is used. [Explanation of symbols]
[0095] 1. Electromagnetic wave absorber 2. Absorbent body 3 Metal Film 4 Incident wave 5 Reflected wave 6 Reflected wave
Claims
1. 1. An electromagnetic wave absorbing material comprising an electrically insulating matrix and a non-magnetic metal powder dispersed in the electrically insulating matrix, The content of the non-magnetic metal powder is 55% by volume or more, The nonmagnetic metal powder has an average aspect ratio of 5.0 or less, The electromagnetic wave absorbing material has a dielectric loss tangent (tan δ) in a frequency band of 0.1 GHz to 13 GHz. E ) at the peak, and the dielectric tangent (tan δ E ) is 0.05 or more.
2. 2. The electromagnetic wave absorbing material according to claim 1, wherein the content of the non-magnetic metal powder is 60 volume % or more.
3. 3. The electromagnetic wave absorbing material according to claim 1, wherein the non-magnetic metal powder is at least one selected from the group consisting of copper (Cu) powder, copper (Cu) alloy powder, silver (Ag) powder, and silver (Ag) alloy powder.
4. The electromagnetic wave absorbing material according to any one of claims 1 to 3, wherein the non-magnetic metal powder has a volume average particle size (D50) of 2.0 µm or more.
5. 5. The electromagnetic wave absorbing material according to claim 1, wherein the non-magnetic metal powder is a mixture of metal powders having different volume average particle sizes (D50).
6. The electromagnetic wave absorbing material according to any one of claims 1 to 5, wherein the electrically insulating matrix comprises at least one of a base oil, a wax, and a rosin.
7. An electromagnetic wave absorber comprising a molded article of the electromagnetic wave absorbing material according to any one of claims 1 to 6.
8. 8. The electromagnetic wave absorber according to claim 7, wherein the electromagnetic wave absorber has a thickness of 0.5 mm or more in the electromagnetic wave incidence direction.
9. 9. The electromagnetic wave absorber according to claim 7, having a region in which a transmission attenuation rate per mm thickness is 10 dB or more in a frequency band of 0.1 GHz or more and 13 GHz or less.
10. An electronic element, electronic part, or electronic equipment comprising the electromagnetic wave absorber according to any one of claims 7 to 9.
Citation Information
Patent Citations
Laminated electromagnetic wave absorber and production thereof
JP2000031686A
Wave absorption sheet
JP2006093288A
Noise suppressor, noise suppressing sheet, painted goods, and manufacturing method for these
JP2010087372A