Adhesive for semiconductor and manufacturing method thereof, and semiconductor device and manufacturing method thereof

The semiconductor adhesive with specific resin and flux compound composition addresses void formation in multi-chip curing, enhancing reflow reliability and connection integrity by maintaining adhesive fluidity during bulk curing.

JP7567802B2Active Publication Date: 2024-10-16RESONAC CORP

Patent Information

Application Number
JP2021550588
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-16
Publication Date
2024-10-16
Estimated Expiration
2040-09-16

Smart Images

  • Figure 0007567802000004
    Figure 0007567802000004
  • Figure 0007567802000005
    Figure 0007567802000005
  • Figure 0007567802000006
    Figure 0007567802000006
Patent Text Reader

Abstract

Disclosed is an adhesive for semiconductors which comprises a thermoplastic resin, a thermosetting resin, a hardener having a reactive group, and a flux compound having an acid group. The adhesive for semiconductors, when examined by differential scanning calorimetry in which the adhesive is heated at a rate of 10 °C / min, gives a DSC curve which has a calorific value within the range of 60-155°C of 20 J / g or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive for semiconductors and a manufacturing method thereof, as well as a semiconductor device and a manufacturing method thereof. [Background technology]

[0002] Conventionally, the wire bonding method using thin metal wires such as gold wires has been widely used to connect semiconductor chips and substrates.

[0003] In recent years, in order to meet the demands for higher functionality, higher integration, and higher speed for semiconductor devices, the flip-chip connection method (FC connection method) in which conductive protrusions called bumps are formed on a semiconductor chip or substrate to directly connect the semiconductor chip to the substrate is becoming widespread.

[0004] For example, with regard to the connection between a semiconductor chip and a substrate, the COB (Chip On Board) type connection method that is widely used in BGA (Ball Grid Array), CSP (Chip Size Package), etc., also corresponds to the FC connection method. The FC connection method is also widely used in the COC (Chip On Chip) type connection method in which a connection part (bump or wiring) is formed on a semiconductor chip to connect between semiconductor chips, and the COW (Chip On Wafer) type connection method in which a connection part (bump or wiring) is formed on a semiconductor wafer to connect between a semiconductor chip and a semiconductor wafer (see, for example, Patent Document 1).

[0005] In semiconductor packages, which are strongly required to be smaller, thinner and more functional, chip-stack packages, POP (Package On Package), TSV (Through-Silicon Via), etc., which are stacked and multi-layered versions of the above-mentioned connection methods, are beginning to spread widely. Such stacking and multi-layering technologies arrange semiconductor chips and other components three-dimensionally, making semiconductor packages smaller than methods that arrange them two-dimensionally. Stacking and multi-layering technologies are attracting attention as the next-generation semiconductor wiring technology because they are also effective in improving semiconductor performance, reducing noise, reducing mounting area and saving power.

[0006] Generally, metal bonding is used to connect the connecting parts from the viewpoint of sufficiently ensuring the connection reliability (e.g., insulation reliability). The main metals used for the above-mentioned connecting parts (e.g., bumps and wiring) include solder, tin, gold, silver, copper, nickel, etc., and conductive materials containing a plurality of these metals are also used. The metals used for the connecting parts may have impurities on the connecting surfaces of the connecting parts due to the surface being oxidized to form an oxide film, and impurities such as oxides adhering to the surface. If such impurities remain, the connection reliability (e.g., insulation reliability) between the semiconductor chip and the substrate, or between two semiconductor chips, may decrease, and there is a concern that the advantage of adopting the above-mentioned connecting method may be lost.

[0007] One method to suppress the generation of these impurities is to coat the connection parts with an anti-oxidation film, known as OSP (Organic Solderbility Preservatives) treatment, but this anti-oxidation film can sometimes cause a decrease in solder wettability and connectivity during the connection process.

[0008] In view of this, as a method for removing the above-mentioned oxide film and impurities, a method has been proposed in which a fluxing agent is contained in an adhesive for semiconductors (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2008-294382 A [Patent Document 2] International Publication No. 2013 / 125086 Summary of the Invention [Problem to be solved by the invention]

[0010] In recent years, from the viewpoint of improving productivity, a process has been proposed in which multiple semiconductor chips are mounted and temporarily fixed on a mounting member (semiconductor chip, semiconductor wafer, wiring circuit board, etc.) via a semiconductor adhesive, and then cured and sealed all at once. In this process, heat (approximately 60 to 155°C) is applied to the stage to an extent that the semiconductor adhesive can flow, and the semiconductor chips are temporarily fixed to the mounting member, and then the semiconductor adhesive is cured all at once by reflow at a temperature above the melting point of the connection part (for example, approximately 260°C). This process allows multiple semiconductor packages to be produced efficiently.

[0011] In the above process, voids may remain in the semiconductor adhesive, and in order to prevent the occurrence of these voids, a method of performing batch curing under pressure conditions has been proposed. However, when the number of semiconductor chips increases, voids may remain even in the above method, and it has become clear that there is room for further improvement.

[0012] Therefore, one aspect of the present invention reduces voids that may remain in a semiconductor adhesive in a process in which multiple semiconductor chips are temporarily fixed onto a mounting member via a semiconductor adhesive and then cured and sealed all at once. [Means for solving the problem]

[0013] The present inventors have inferred that when the number of semiconductor chips is large in the above process, the semiconductor adhesive partially hardens during temporary fixation, and as a result, voids are likely to remain in the semiconductor adhesive. That is, in the above process, since the semiconductor chips are mounted sequentially, the semiconductor chips mounted initially and the semiconductor adhesive continue to be subjected to a thermal history by the stage until the mounting of the last semiconductor chip is completed. Therefore, it is inferred that when the number of semiconductor chips is large, the hardening of the semiconductor adhesive that temporarily fixes the semiconductor chips mounted initially progresses partially, and the voids are not removed by the pressure applied during the collective hardening and remain. The present inventors have further studied based on the above inference and completed the present invention.

[0014] Some aspects of the invention provide the following:

[0015] [1] A semiconductor adhesive comprising a thermoplastic resin, a thermosetting resin, a curing agent having a reactive group, and a flux compound having an acid group, wherein the heat generation amount in the range of 60 to 155°C in a DSC curve obtained by differential scanning calorimetry in which the semiconductor adhesive is heated at a heating rate of 10°C / min is 20 J / g or less.

[0016] [2] The adhesive for semiconductors described in [1], wherein the weight average molecular weight (Mw) of the thermoplastic resin is 10,000 or more.

[0017] [3] The adhesive for semiconductors according to [1] or [2], wherein the content of the thermoplastic resin is 1 to 30 mass % based on the total solid content of the adhesive for semiconductors.

[0018] [4] The adhesive for a semiconductor according to any one of [1] to [3], wherein the content of the thermoplastic resin is 5 mass % or more based on the total solid content of the adhesive for a semiconductor.

[0019] [5] The adhesive for a semiconductor according to any one of [1] to [4], wherein the curing agent includes an amine-based curing agent.

[0020] [6] The adhesive for a semiconductor according to any one of [1] to [5], wherein the curing agent comprises an imidazole-based curing agent.

[0021] [7] The adhesive for a semiconductor according to any one of [1] to [6], wherein the content of the curing agent is 2.3 mass % or less based on the total solid content of the adhesive for a semiconductor.

[0022] [8] The adhesive for a semiconductor according to any one of [1] to [7], wherein the flux compound has a melting point of 25 to 230°C.

[0023] [9] The adhesive for a semiconductor according to any one of [1] to [8], wherein the flux compound has a melting point of 100 to 170°C.

[0024]

[10] The adhesive for a semiconductor according to any one of [1] to [9], wherein the thermosetting resin contains an epoxy resin.

[0025]

[11] The adhesive for a semiconductor according to any one of [1] to

[10] , wherein the thermosetting resin is substantially free of an epoxy resin that is liquid at 35°C.

[0026]

[12] The adhesive for a semiconductor according to any one of [1] to

[11] , which is in the form of a film.

[0027]

[13] The adhesive for a semiconductor according to any one of [1] to

[12] , which is cured by application of heat under a pressurized atmosphere. This adhesive for a semiconductor may be used to cure the adhesive for a semiconductor by application of heat under a pressurized atmosphere and seal a connection portion of a semiconductor chip with the cured adhesive for a semiconductor.

[0028]

[14] The adhesive for a semiconductor according to any one of [1] to

[13] , wherein the adhesive for a semiconductor has a minimum melt viscosity of 400 to 2500 Pa·s.

[0029]

[15] A semiconductor adhesive described in any of [1] to

[14] , wherein the ratio of the number of moles of the acid groups in the total amount of the flux compound to the number of moles of the reactive groups in the total amount of the curing agent is 0.01 to 4.8.

[0030]

[16] A method for manufacturing an adhesive for semiconductors, comprising the step of mixing a thermoplastic resin, a thermosetting resin, a curing agent having a reactive group, and a flux compound having an acid group, wherein the curing agent and the flux compound are blended so that the ratio of the number of moles of the acid groups in the total amount of the flux compound to the number of moles of the reactive groups in the total amount of the curing agent is 0.01 to 4.8.

[0031]

[17] The flux compound comprises at least one selected from the group consisting of monocarboxylic acids, dicarboxylic acids, and tricarboxylic acids; The method for producing an adhesive for a semiconductor described in

[16] , wherein in the above step, the curing agent and the flux compound are blended so that the ratio of the number of moles of the monocarboxylic acid to the number of moles of reactive groups in the total amount of the curing agent is 0.01 to 4.8, the ratio of the number of moles of the dicarboxylic acid to the number of moles of reactive groups in the total amount of the curing agent is 0.01 to 2.4, and the ratio of the number of moles of the tricarboxylic acid to the number of moles of reactive groups in the total amount of the curing agent is 0.01 to 1.6.

[0032]

[18] A method for producing an adhesive for semiconductors according to

[16] or

[17] , wherein the weight average molecular weight (Mw) of the thermoplastic resin is 10,000 or more.

[0033]

[19] A method for producing an adhesive for a semiconductor according to any one of

[16] to

[18] , wherein the blending amount of the thermoplastic resin is 1 to 30 mass % based on the total solid content of the adhesive for a semiconductor.

[0034]

[20] A method for producing an adhesive for a semiconductor according to any one of

[16] to

[19] , wherein the blending amount of the thermoplastic resin is 5 mass% or more based on the total solid content of the adhesive for a semiconductor.

[0035]

[21] The method for producing an adhesive for a semiconductor according to any one of

[16] to

[20] , wherein the curing agent includes an amine-based curing agent.

[0036]

[22] The method for producing an adhesive for a semiconductor according to any one of

[16] to

[21] , wherein the curing agent comprises an imidazole-based curing agent.

[0037]

[23] A method for producing an adhesive for a semiconductor according to any one of

[16] to

[22] , wherein the amount of the curing agent is 2.3 mass % or less based on the total solid content of the adhesive for a semiconductor.

[0038]

[24] The method for producing an adhesive for a semiconductor according to any one of

[16] to

[23] , wherein the flux compound has a melting point of 25 to 230°C.

[0039]

[25] The method for producing an adhesive for a semiconductor according to any one of

[16] to

[24] , wherein the flux compound has a melting point of 100 to 170°C.

[0040]

[26] The method for producing an adhesive for a semiconductor according to any one of

[16] to

[25] , wherein the thermosetting resin contains an epoxy resin.

[0041]

[27] The method for producing an adhesive for a semiconductor according to any one of

[16] to

[26] , wherein the thermosetting resin is substantially free of an epoxy resin that is liquid at 35°C.

[0042]

[28] A method for producing a semiconductor adhesive described in any of

[16] to

[27] , further comprising a step of molding a mixture containing the thermoplastic resin, the thermosetting resin, the curing agent, and the flux compound into a film.

[0043]

[29] A method for manufacturing a semiconductor device in which the connection portions of a semiconductor chip and a wiring circuit board are electrically connected to each other, or a semiconductor device in which the connection portions of a plurality of semiconductor chips are electrically connected to each other, comprising a sealing step of curing the semiconductor adhesive according to any one of [1] to

[15] by applying heat, and sealing at least a part of the connection portions with the cured semiconductor adhesive. The semiconductor adhesive may be cured by applying heat in a pressurized atmosphere.

[0044]

[30] The method for manufacturing a semiconductor device described in

[29] , further comprising the steps of: prior to the sealing step, arranging a plurality of semiconductor chips on a stage; and, while heating the stage to 60 to 155°C, sequentially arranging other semiconductor chips on top of each of the plurality of semiconductor chips arranged on the stage via the semiconductor adhesive, thereby obtaining a plurality of stacks each having the semiconductor chips, the semiconductor adhesive, and the other semiconductor chips, stacked in this order.

[0045]

[31] The method for manufacturing a semiconductor device described in

[29] , further comprising the steps of: prior to the sealing step, arranging a wiring circuit board or a semiconductor wafer on a stage; and, while heating the stage to 60 to 155°C, sequentially arranging a plurality of semiconductor chips on the wiring circuit board or semiconductor wafer arranged on the stage, via the semiconductor adhesive, to obtain a laminate having the wiring circuit board, the semiconductor adhesive, and a plurality of the semiconductor chips, which are stacked in this order, or a laminate having the semiconductor wafer, the semiconductor adhesive, and a plurality of the semiconductor chips, which are stacked in this order.

[0046]

[32] A semiconductor device comprising a semiconductor chip having a connection portion and a wiring circuit board having a connection portion, the connection portion of the semiconductor chip and the connection portion of the wiring circuit board being electrically connected to each other, or a semiconductor device comprising a plurality of semiconductor chips having connection portions, the connection portions of the respective semiconductor chips being electrically connected to each other, wherein at least a portion of the connection portion is sealed with a cured product of the adhesive for semiconductor according to any one of [1] to

[15] that is cured by applying heat under a pressurized atmosphere. In other words, this semiconductor device is a semiconductor device in which the respective connection portions of the semiconductor chip and the wiring circuit board are electrically connected to each other, or a semiconductor device in which the respective connection portions of a plurality of semiconductor chips are electrically connected to each other. Effect of the Invention

[0047] According to one aspect of the present invention, in a process in which a plurality of semiconductor chips are temporarily fixed on a mounting member via a semiconductor adhesive and cured and sealed all at once, it is possible to reduce voids that may remain in the semiconductor adhesive. According to another aspect of the present invention, it is possible to provide a semiconductor adhesive capable of reducing such voids and a method for manufacturing the same, as well as a semiconductor device in which such voids are reduced and a method for manufacturing the same. [Brief description of the drawings]

[0048] [Figure 1] FIG. 2 is a schematic diagram showing a method for determining the onset temperature of an exothermic peak from a DSC curve. [Diagram 2] FIG. 2 is a schematic diagram showing a method for determining the calorific value from 60 to 155° C. from a DSC curve. [Diagram 3] FIG. 2 is a schematic diagram showing a method for determining the calorific value from 60 to 155° C. from a DSC curve. [Figure 4] 1 is a schematic cross-sectional view showing an embodiment of a semiconductor device; [Diagram 5] 1 is a schematic cross-sectional view showing an embodiment of a semiconductor device; [Figure 6] 1 is a schematic cross-sectional view showing an embodiment of a semiconductor device; [Figure 7]1A to 1C are schematic cross-sectional views showing an embodiment of a method for manufacturing a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as needed. In the drawings, the same or corresponding parts are given the same reference numerals, and duplicated explanations will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, right, etc. are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.

[0050] The upper and lower limit values ​​of the numerical ranges described in this specification can be combined in any combination. The numerical values ​​described in the examples can also be used as the upper or lower limit values ​​of the numerical ranges. In this specification, "(meth)acrylic" means acrylic or its corresponding methacrylic.

[0051] <Semiconductor adhesive and its manufacturing method> The semiconductor adhesive of this embodiment contains a thermoplastic resin (hereinafter sometimes referred to as "component (a)"), a thermosetting resin (hereinafter sometimes referred to as "component (b)"), a curing agent having a reactive group (hereinafter sometimes referred to as "component (c)"), and a flux compound having an acid group (hereinafter sometimes referred to as "component (d)"). The semiconductor adhesive of this embodiment may contain a filler (hereinafter sometimes referred to as "component (e)") as necessary.

[0052] The heat generation amount of the DSC curve obtained by differential scanning calorimetry (DSC) of the semiconductor adhesive of this embodiment at 60 to 155°C is 20 J / g or less. Here, the differential scanning calorimetry is performed by heating the semiconductor adhesive in an air or nitrogen atmosphere with a weight of 10 mg of the sample semiconductor adhesive, a measurement temperature range of 30 to 300°C, and a temperature rise rate of 10°C / min. The heat generation amount is calculated by integrating the peak area.

[0053] Conventional semiconductor adhesives have an exothermic peak in the temperature range of 60 to 155 ° C. on the DSC curve. It is presumed that the heat generation in this temperature range is due to the reaction between the thermosetting resin in the semiconductor adhesive and the flux compound, and that as this reaction progresses, the semiconductor adhesive partially hardens and its fluidity decreases. On the other hand, the temporary fixing of semiconductor chips with a semiconductor adhesive is usually performed by heating the semiconductor adhesive to, for example, 60 to 155 ° C. and causing it to flow appropriately. Therefore, if a conventional semiconductor adhesive is used in a process in which multiple semiconductor chips are mounted and temporarily fixed on a mounting member (semiconductor chip, semiconductor wafer, wiring circuit board, etc.) via a semiconductor adhesive, and then cured and sealed all at once under pressure conditions, it is presumed that when the semiconductor chips are temporarily fixed, the thermosetting resin in the semiconductor adhesive reacts with the flux compound, causing the semiconductor adhesive to partially harden, and the adhesive will not flow sufficiently when cured all at once under pressure conditions. Since the heat value of the semiconductor adhesive of this embodiment at 60 to 155°C in the DSC curve is 20 J / g or less, the hardening does not proceed easily in the temperature range (for example, 60 to 155°C) where the semiconductor chip is temporarily fixed. Therefore, by using the semiconductor adhesive of this embodiment in the above process, it is possible to temporarily fix multiple semiconductor chips while maintaining sufficient fluidity of the semiconductor adhesive, and it is possible to reduce the occurrence of voids during collective hardening. Furthermore, as a result of reducing the occurrence of voids, it is expected that defects (peeling of the semiconductor adhesive, poor electrical connection at the connection, etc.) are less likely to occur even if the adhesive is heated at a temperature (for example, 260°C) above the melting point of the connection in the reflow process. That is, the semiconductor adhesive of this embodiment tends to improve the reflow reliability (reflow resistance) in the manufacture of semiconductor devices.

[0054] The calorific value of the DSC curve from 60 to 155°C may be 15 J / g or less, or 10 J / g or less, from the viewpoint of easily obtaining the effects of the present invention. The calorific value of the DSC curve from 60 to 155°C may be 20% or less, 15% or less, or 10% or less of the calorific value of the DSC curve from 60 to 280°C, from the viewpoint of easily obtaining the effects of the present invention. The calorific value of the DSC curve from 60 to 280°C may be 50 J / g or more or 100 J / g or more, and may be 200 J / g or less or 180 J / g or less, or may be 50 to 200 J / g, 100 to 200 J / g, or 100 to 180 J / g, from the viewpoint of easily obtaining the effects of the present invention. The DSC curve may not have an exothermic peak with an onset temperature of 155°C or less, from the viewpoint of easily obtaining the effects of the present invention.

[0055] Fig. 1 is a schematic diagram showing a method for determining the onset temperature of an exothermic peak from a DSC curve. The DSC curve shown in Fig. 1 includes a baseline L0 in the temperature range of 60 to 280°C, and an exothermic peak P due to a curing reaction of the adhesive observed halfway through the baseline L0. The onset temperature is the temperature T at the intersection between an extension line L1 of the baseline L0 below the exothermic peak P and a tangent line L2 to the DSC curve at the point where the DSC curve shows the maximum gradient at the exothermic peak P.

[0056] 2 and 3 are schematic diagrams showing a method for determining the calorific value from 60 to 155°C from a DSC curve. As shown in FIG. 2, when the DSC curve includes only the exothermic peak P including a portion below 155°C as an exothermic peak, the calorific value Q1 of the portion below 155°C of the exothermic peak P is the calorific value from 60 to 155°C. The calorific value Q1 is determined from the area of ​​the region below 155°C surrounded by the exothermic peak P and an extension line L1 of the baseline L0. As shown in FIG. 3, when the DSC curve further includes a peak other than the exothermic peak P in the region below 155°C, the sum of the calorific value Q2 of the peak and the calorific value Q1 of the exothermic peak P at 155°C or less is the calorific value from 60 to 155°C. When more exothermic peaks are observed in the region below 60 to 155°C, the calorific value obtained by adding up all the calorific values ​​of those exothermic peaks is the calorific value from 60 to 155°C.

[0057] The semiconductor adhesive of this embodiment showing the above DSC curve can be obtained, for example, by blending a curing agent and a flux compound so that the ratio of the number of moles of acid groups in the total amount of flux compound to the number of moles of reactive groups (groups that react with acid groups of the flux compound) in the total amount of curing agent is 0.01 to 4.8. That is, the manufacturing method of the semiconductor adhesive of this embodiment includes a step of mixing a thermoplastic resin, a thermosetting resin, a curing agent having a reactive group, and a flux compound having an acid group, and in this step, the curing agent and the flux compound are blended so that the ratio of the number of moles of acid groups in the total amount of flux compound to the number of moles of reactive groups in the total amount of curing agent is 0.01 to 4.8. In the semiconductor adhesive obtained by this method, the ratio of the number of moles of acid groups in the total amount of flux compound to the number of moles of reactive groups in the total amount of curing agent is usually 0.01 to 4.8. However, a part of the reactive groups of the curing agent and the acid groups of the flux compound may form a salt. The molar ratio including the number of reactive groups and acid groups forming the salt may be within the above range.

[0058] The present inventors speculate that the reason why the adhesive for semiconductors showing the above DSC curve can be obtained by setting the molar ratio of the curing agent to the flux compound in the above range is as follows. That is, as described above, in the temperature range of 60 to 155°C, the thermosetting resin in the adhesive for semiconductors reacts with the flux compound. However, it is speculated that when the molar ratio of the curing agent to the flux compound is in the above range, the flux compound can form a salt with the curing agent and be stabilized before reacting with the thermosetting resin. Therefore, it is speculated that the reaction between the thermosetting resin and the flux compound is suppressed, and as a result, an adhesive for semiconductors showing the above DSC curve can be obtained.

[0059] Hereinafter, each component constituting the semiconductor adhesive of this embodiment will be described.

[0060] (a) Thermoplastic resin The (a) component is not particularly limited, but examples thereof include phenoxy resin, polyimide resin, polyamide resin, polycarbodiimide resin, cyanate ester resin, acrylic resin, polyester resin, polyethylene resin, polyethersulfone resin, polyetherimide resin, polyvinyl acetal resin, urethane resin, and acrylic rubber. Among these, from the viewpoint of excellent heat resistance and film formability, the thermoplastic resin may be selected from phenoxy resin, polyimide resin, acrylic resin, acrylic rubber, cyanate ester resin, and polycarbodiimide resin, or may be selected from phenoxy resin, polyimide resin, and acrylic resin. These (a) components can be used alone, or can be used as a mixture or copolymer of two or more kinds.

[0061] The weight average molecular weight (Mw) of the (a) component may be 10,000 or more, 40,000 or more, or 60,000 or more. Such a (a) component can further improve the film formability and heat resistance of the adhesive. When the weight average molecular weight is 10,000 or more, flexibility is easily imparted to the film-shaped semiconductor adhesive, so that more excellent processability is easily obtained. The weight average molecular weight of the (a) component may be 1,000,000 or less, or 500,000 or less. Such a (a) component reduces the viscosity of the film, so that embedding into bumps is improved, and mounting can be performed with even less voids. From these viewpoints, the weight average molecular weight of the (a) component may be 10,000 to 1,000,000, 40,000 to 500,000, or 60,000 to 500,000.

[0062] In this specification, the weight average molecular weight refers to a weight average molecular weight measured using GPC (gel permeation chromatography) in terms of polystyrene. An example of the measurement conditions for the GPC method is shown below. Equipment: HCL-8320GPC, UV-8320 (product name, manufactured by Tosoh Corporation), or HPLC-8020 (product name, manufactured by Tosoh Corporation) Column: TSKgel superMultiporeHZ-M x 2, or 2 pieces of GMHXL + 1 piece of G-2000XL Detector: RI or UV detector Column temperature: 25-40℃ Eluent: A solvent that dissolves polymer components is selected. Examples of the solvent include THF (tetrahydrofuran), DMF (N,N-dimethylformamide), DMA (N,N-dimethylacetamide), NMP (N-methylpyrrolidone), and toluene. When a polar solvent is selected, the phosphoric acid concentration may be adjusted to 0.05 to 0.1 mol / L (usually 0.06 mol / L) and the LiBr concentration may be adjusted to 0.5 to 1.0 mol / L (usually 0.63 mol / L). Flow rate: 0.30~1.5mL / min Standard material: polystyrene

[0063] (a) Component content C a Content of component (b) C b Ratio of C b / C a (mass ratio) may be 0.01 or more, 0.1 or more, or 1 or more, and may be 5 or less, 4.5 or less, or 4 or less. b / C a By making the ratio C 0.01 or more, better curing properties and adhesive strength can be obtained. b / C a By setting the ratio C to 5 or less, better film formability can be obtained. b / C a may be 0.01 to 5, 0.1 to 4.5, or 1 to 4.

[0064] The glass transition temperature of component (a) may be -50°C or higher, -40°C or higher, or -30°C or higher from the viewpoint of improving connection reliability, etc. The glass transition temperature of component (a) may be 220°C or lower, 200°C or lower, or 180°C or lower from the viewpoint of lamination, etc. The glass transition temperature of component (a) may be -50 to 220°C, -40 to 200°C, or -30 to 180°C. According to such an adhesive for semiconductors containing component (a), the amount of wafer warpage can be further reduced during a mounting process at the wafer level, and the heat resistance and film formability of the adhesive for semiconductors can be further improved. The glass transition temperature of component (a) can be measured by a differential scanning calorimeter (DSC).

[0065] The content of the component (a) may be 30% by mass or less, 25% by mass or less, or 20% by mass or less based on the total solid content of the semiconductor adhesive. When the content of the component (a) is 30% by mass or less, the semiconductor adhesive can obtain good reliability during a temperature cycle test, and can obtain good adhesive strength at a reflow temperature of about 260°C even after moisture absorption. The content of the component (a) may be 1% by mass or more, 3% by mass or more, or 5% by mass or more based on the total solid content of the semiconductor adhesive. When the content of the component (a) is 1% by mass or more, the semiconductor adhesive can further reduce the amount of wafer warpage during a mounting process at the wafer level, and can further improve the heat resistance and film formability of the semiconductor adhesive. When the content of the component (a) is 5% by mass or more, the occurrence of burrs and chips during processing into the wafer shape can be suppressed. From the above viewpoints, and from the viewpoint of easily imparting flexibility to a film-shaped semiconductor adhesive and easily obtaining even better processability, the content of component (a) may be 1 to 30 mass%, 3 to 30 mass%, or 5 to 30 mass% based on the total solid content of the semiconductor adhesive. The "total solid content of the semiconductor adhesive" refers to the total amount of the semiconductor adhesive minus the amount of the solvent contained in the semiconductor adhesive. In this specification, the "total solid content of the semiconductor adhesive" may be rephrased as "the total amount of components (a), (b), (c), (d) and (e)".

[0066] (b) Thermosetting resin As component (b), any component having two or more reactive groups in the molecule can be used without any particular restrictions. By including a thermosetting resin in the semiconductor adhesive, the adhesive can be cured by heating, and the cured adhesive exhibits high heat resistance and adhesive strength to the chip, resulting in excellent reflow resistance.

[0067] Examples of the (b) component include epoxy resin, phenol resin, imide resin, urea resin, melamine resin, silicon resin, (meth)acrylic compound, and vinyl compound. From the viewpoint of excellent heat resistance (reflow resistance) and storage stability, the thermosetting resin may be selected from epoxy resin, phenol resin, and imide resin, may be selected from epoxy resin and imide resin, or may be epoxy resin. These (b) components can be used alone, or can be used as a mixture or copolymer of two or more kinds. Among conventional semiconductor adhesives, particularly when the thermosetting resin is an epoxy resin, a melamine resin, or a urea resin, the reaction with the flux compound described later tends to proceed in the temperature range of 60 to 155 ° C., and partial curing tends to proceed before the overall curing, but in this embodiment, even if the thermosetting resin contains at least one resin selected from the group consisting of epoxy resin, melamine resin, and urea resin, such a reaction and partial curing are unlikely to occur.

[0068] Examples of epoxy resins and imide resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, triphenylmethane type epoxy resins, dicyclopentadiene type epoxy resins, various polyfunctional epoxy resins, nadimide resins, allylnadimide resins, maleimide resins, amide imide resins, imide acrylate resins, various polyfunctional imide resins, and various polyimide resins. These can be used alone or in a mixture of two or more.

[0069] In order to prevent decomposition and generation of volatile components during connection at high temperatures, component (b) may have a thermal weight loss rate of 5% or less at 250°C when the temperature during connection is 250°C, and may have a thermal weight loss rate of 5% or less at 300°C when the temperature during connection is 300°C.

[0070] Component (b) may be substantially free of epoxy resin that is liquid at 35° C. For example, the content of epoxy resin that is liquid at 35° C. may be 0.1 parts by mass or less per 100 parts by mass of component (b). In this case, mounting can be achieved without the liquid epoxy resin decomposing or volatilizing during thermocompression bonding, and outgassing contamination of the periphery of the chip is suppressed, making it easier to obtain a semiconductor package with even better throughput.

[0071] The content of component (b) may be, for example, 5% by mass or more, 15% by mass or more, or 30% by mass or more, based on the total solid content of the adhesive for semiconductors. The content of component (b) may be, for example, 80% by mass or less, 70% by mass or less, or 60% by mass or less, based on the total solid content of the adhesive for semiconductors. The content of component (b) may be, for example, 5 to 80% by mass, 15 to 70% by mass, or 30 to 60% by mass, based on the total solid content of the adhesive for semiconductors.

[0072] (c) Hardener The component (c) is a compound that reacts with the reactive group of the thermosetting resin or promotes the curing reaction of the thermosetting resin, and may be a compound having a reactive group capable of forming a salt with the fluxing agent described below. Examples of the component (c) include an amine-based curing agent, which is a compound having an amino group as a reactive group, and an imidazole-based curing agent, which is a compound having an imidazole group as a reactive group. When the component (c) contains an amine-based curing agent or an imidazole-based curing agent, it exhibits flux activity that suppresses the formation of an oxide film at the connection portion, and can improve connection reliability and insulation reliability. When the component (c) contains an amine-based curing agent or an imidazole-based curing agent, storage stability is further improved, and decomposition or deterioration due to moisture absorption tends to be less likely to occur. When the component (c) contains an amine-based curing agent or an imidazole-based curing agent, it becomes easy to adjust the curing speed, and the fast curing property makes it easy to realize short-time connection for the purpose of improving productivity.

[0073] Each curing agent will be described below.

[0074] (i) Amine-based hardeners As the amine-based curing agent, for example, dicyandiamide can be used.

[0075] The content of the amine-based curing agent may be 0.1 parts by mass or more, 10 parts by mass or less, or 5 parts by mass or less, relative to 100 parts by mass of the above component (b). When the content of the amine-based curing agent is 0.1 parts by mass or more, the curability tends to be improved. When the content of the amine-based curing agent is 10 parts by mass or less, the semiconductor adhesive does not cure before the metal bond is formed, and connection failure tends to be less likely to occur. From these viewpoints, the content of the amine-based curing agent may be 0.1 to 10 parts by mass, or 0.1 to 5 parts by mass, relative to 100 parts by mass of the component (b).

[0076] (ii) Imidazole-based curing agents Examples of the imidazole-based curing agent include 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, and 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine. -[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and imidazoles. From the viewpoint of excellent curing property, storage stability and connection reliability, the imidazole curing agent is 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine ... The latent curing agent may be selected from the group consisting of 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. These may be used alone or in combination of two or more. Microcapsules containing these may be used as the latent curing agent.

[0077] The content of the imidazole-based curing agent may be 0.1 parts by mass or more, 10 parts by mass or less, 5 parts by mass or less, or 2.3 parts by mass or less, relative to 100 parts by mass of the (b) component. When the content of the imidazole-based curing agent is 0.1 parts by mass or more, the curability tends to improve. When the content of the imidazole-based curing agent is 10 parts by mass or less, the semiconductor adhesive does not cure before the metal bond is formed, and connection failure is unlikely to occur, and the generation of voids is easily suppressed in the curing process under a pressurized atmosphere. From these viewpoints, the content of the imidazole-based curing agent may be 0.1 to 10 parts by mass, 0.1 to 5 parts by mass, or 0.1 to 2.3 parts by mass, relative to 100 parts by mass of the (b) component.

[0078] The (c) component can be used alone or in a mixture of two or more. For example, an imidazole-based curing agent can be used alone or together with an amine-based curing agent. As the (c) component, a curing agent other than the above that functions as a curing agent for the (b) component can also be used.

[0079] The content of the (c) component may be 0.5 parts by mass or more, 20 parts by mass or less, 6 parts by mass or less, or 4 parts by mass or less, relative to 100 parts by mass of the (b) component. When the content of the (c) component is 0.5 parts by mass or more, curing tends to proceed sufficiently. When the content of the (c) component is 20 parts by mass or less, it tends to be possible to prevent the curing from proceeding too quickly and increasing the number of reaction points, and to prevent the molecular chain from becoming shorter or unreacted groups from remaining, which would reduce reliability, and in addition, it is easy to prevent voids from remaining during curing under a pressurized atmosphere. From these viewpoints, the content of the (c) component may be 0.2 to 20 parts by mass, 0.5 to 6 parts by mass, or 0.5 to 4 parts by mass, relative to 100 parts by mass of the (b) component.

[0080] The content of the (c) component may be 0.5% by mass or more, 2.3% by mass or less, 2.0% by mass or less, or 1.5% by mass or less based on the total solid content of the adhesive for semiconductors. When the content of the (c) component is 0.5% by mass or more, curing tends to proceed sufficiently. When the content of the (c) component is 2.3% by mass or less, the curing tends to proceed rapidly and increase in reaction points, and the molecular chain tends to be shortened, unreacted groups tend to remain, and the reliability tends to be prevented from decreasing, and in addition, it is easy to suppress the remaining of voids during curing under a pressurized atmosphere. From these viewpoints, the content of the (c) component may be 0.5 to 2.3% by mass, or 0.5 to 2.0% by mass based on the total solid content of the adhesive for semiconductors.

[0081] When the adhesive for semiconductors contains an amine-based curing agent as component (c), it exhibits flux activity for removing oxide films, and can further improve connection reliability.

[0082] (d) Flux Compounds Component (d) is a compound having flux activity (activity to remove oxides and impurities), such as an organic acid. When the semiconductor adhesive contains component (d), it is possible to remove the oxide film on the metal of the connection portion and the coating caused by the OSP treatment, making it easier to obtain excellent connection reliability. As component (d), one type of flux compound (e.g., organic acid) may be used alone, or two or more types of flux compounds (e.g., organic acids) may be used in combination.

[0083] The component (d) has one or more acid groups. The acid group is, for example, a carboxyl group. When the component (d) is a compound having a carboxyl group (for example, a carboxylic acid), even better connection reliability is likely to be obtained. When the component (d) is a compound having a carboxyl group (for example, a carboxylic acid), from the viewpoint of making it easier to obtain the effects of the present invention, the component (b) may be at least one thermosetting resin selected from the group consisting of epoxy resins, urethane resins, and urea resins, and the component (c) may be at least one curing agent selected from the group consisting of amine-based curing agents and imidazole-based curing agents.

[0084] An example of a compound having a carboxyl group is a compound having a group represented by the following formula (1). [ka] In formula (1), R 1 represents a hydrogen atom or an electron-donating group.

[0085] Examples of the electron-donating group include an alkyl group, a hydroxyl group, an amino group, an alkoxy group, and an alkylamino group.

[0086] The alkyl group may be an alkyl group having 1 to 10 carbon atoms, or an alkyl group having 1 to 5 carbon atoms. When the number of carbon atoms in the alkyl group is within the above range, an excellent balance between electron donating property and steric hindrance is achieved.

[0087] The alkyl group may be linear or branched, or may be linear. When the alkyl group is linear, the number of carbon atoms of the alkyl group may be equal to or less than the number of carbon atoms of the main chain of the flux compound, from the viewpoint of the balance between electron donating property and steric hindrance.

[0088] The alkoxy group may be an alkoxy group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms. When the number of carbon atoms in the alkoxy group is within the above range, an excellent balance between electron donating property and steric hindrance is achieved.

[0089] The alkyl group portion of the alkoxy group may be linear or branched, or may be linear. When the alkoxy group is linear, the number of carbon atoms of the alkoxy group may be equal to or less than the number of carbon atoms of the main chain of the flux compound, from the viewpoint of the balance between electron donating property and steric hindrance.

[0090] Examples of the alkylamino group include a monoalkylamino group and a dialkylamino group. The monoalkylamino group may be a monoalkylamino group having 1 to 10 carbon atoms, or a monoalkylamino group having 1 to 5 carbon atoms. The alkyl group portion of the monoalkylamino group may be linear or branched, or may be linear. The dialkylamino group may be a dialkylamino group having 2 to 20 carbon atoms, or a dialkylamino group having 2 to 10 carbon atoms. The alkyl group portion of the dialkylamino group may be linear or branched, or may be linear.

[0091] The component (d) may be a compound having 1 to 3 acid groups, or may be a compound having 1 to 3 carboxyl groups as the acid groups. The component (d) may include at least one selected from the group consisting of monocarboxylic acids, dicarboxylic acids, and tricarboxylic acids. When a component (d) having 1 to 3 carboxyl groups is used, the increase in viscosity of the adhesive for semiconductors during storage, connection work, etc. can be further suppressed compared to when a compound having 4 or more carboxyl groups is used, and the connection reliability of the semiconductor device can be further improved.

[0092] The (d) component may contain a monocarboxylic acid. For example, when the thermosetting resin is an epoxy resin, a urethane resin, or a urea resin, a part of the (b) component reacts with a part of the (d) component to generate an ester during thermal polymerization (curing), but when a compound having one carboxyl group is used, the ester bond derived from this ester is unlikely to exist in the polymer main chain. Therefore, even if ester hydrolysis occurs due to moisture absorption, the molecular chain is not significantly reduced. Therefore, the adhesion force after moisture absorption (for example, adhesion force to silicon) and the bulk strength of the cured product can be maintained at a high level, and the reflow resistance and connection reliability of the semiconductor device can be further improved.

[0093] The melting point of the (d) component may be 25°C or more, 90°C or more, or 100°C or more, or 230°C or less, 180°C or less, 170°C or less, or 160°C or less. When the melting point of the (d) component is 230°C or less, the flux activity is easily expressed sufficiently before the curing reaction between the thermosetting resin and the curing agent occurs. Therefore, according to such a semiconductor adhesive containing the (d) component, the (d) component melts when the chip is mounted, and the oxide film on the solder surface is removed, thereby realizing a semiconductor device with even better connection reliability. In addition, when the melting point of the (d) component is 25°C or more, the reaction is less likely to start at room temperature, and the storage stability is even better. From these viewpoints, the melting point of the (d) component may be 25 to 230°C, 90 to 180°C or less, 100 to 170°C, or 100 to 160°C.

[0094] (d) The melting points of components can be measured using a general melting point measurement device. The sample for which the melting point is to be measured is ground into a fine powder and a small amount is used to minimize the temperature deviation within the sample. A capillary tube with one end closed is often used as a sample container, but some measurement devices use a container sandwiched between two microscope cover glasses. If the temperature is increased suddenly, a temperature gradient will occur between the sample and the thermometer, resulting in measurement errors, so it is desirable to increase the temperature at the time of measuring the melting point at a rate of less than 1°C per minute.

[0095] As mentioned above, since the sample is prepared as a fine powder, the sample is opaque before melting due to diffuse reflection on the surface. The lower limit of the melting point is usually the temperature at which the sample begins to become transparent, and the upper limit is the temperature at which the sample is completely melted. There are various types of measuring devices, but the most classic device is a device in which a capillary tube filled with the sample is attached to a double-tube thermometer and heated in a hot bath. A highly viscous liquid is used as the hot bath liquid in order to attach the capillary tube to the double-tube thermometer, and concentrated sulfuric acid or silicone oil is often used, and the sample is attached so that it is close to the reservoir at the tip of the thermometer. A melting point measuring device can also be used that uses a metal heat block for heating, and automatically determines the melting point by adjusting the heating while measuring the light transmittance.

[0096] In this specification, a melting point of 230° C. or lower means that the upper limit of the melting point is 230° C. or lower, and a melting point of 25° C. or higher means that the lower limit of the melting point is 25° C. or higher.

[0097] Specific examples of the component (d) include malonic acid, methylmalonic acid, dimethylmalonic acid, ethylmalonic acid, allylmalonic acid, 2,2'-thiodiacetic acid, 3,3'-thiodipropionic acid, 2,2'-(ethylenedithio)diacetic acid, 3,3'-dithiodipropionic acid, 2-ethyl-2-hydroxybutyric acid, dithiodiglycolic acid, diglycolic acid, acetylenedicarboxylic acid, maleic acid, malic acid, 2-isopropylmalic acid, tartaric acid, itaconic acid, 1,3-acetonedicarboxylic acid, tricarbalinic acid, muconic acid, β-hydromuconic acid, succinic acid, methylsuccinic acid, and the like. acetic acid, dimethylsuccinic acid, glutaric acid, α-ketoglutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 2,2-bis(hydroxymethyl)propionic acid, citric acid, adipic acid, 3-tert-butyladipic acid, pimelic acid, phenyloxalic acid, phenylacetic acid, nitrophenylacetic acid, phenoxyacetic acid, nitrophenoxyacetic acid, phenylthioacetic acid, hydroxyphenylacetic acid, dihydroxyphenylacetic acid, mandelic acid, hydroxymandelic acid, dihydroxymandelic acid, 1,2,3 ,4-Butanetetracarboxylic acid, suberic acid, 4,4'-dithiodibutyric acid, cinnamic acid, nitrocinnamic acid, hydroxycinnamic acid, dihydroxycinnamic acid, coumaric acid, phenylpyruvic acid, hydroxyphenylpyruvic acid, caffeic acid, homophthalic acid, tolylacetic acid, phenoxypropionic acid, hydroxyphenylpropionic acid, benzyloxyacetic acid, phenyllactic acid, tropic acid, 3-(phenylsulfonyl)propionic acid, 3,3-tetramethyleneglutaric acid, 5-oxoazelaic acid, azelaic acid, phenylsuccinic acid, 1,2-phenylenediacetic acid, 1,3 -Phenylenediacetic acid, 1,4-phenylenediacetic acid, benzylmalonic acid, sebacic acid, dodecanedioic acid, undecanedioic acid, diphenylacetic acid, benzilic acid, dicyclohexylacetic acid, tetradecanedioic acid, 2,2-diphenylpropionic acid, 3,3-diphenylpropionic acid, 4,4-bis(4-hydroxyphenyl)valeric acid (diphenolic acid), pimaric acid, palustric acid, isopimaric acid, abietic acid, dehydroabietic acid, neoabietic acid, agatic acid, benzoic acid, 2-hydroxybenzoic acid, 3-hydroxybenzoic acid, 4-hydroxybenzoic acid, 2,3-Dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 2,3,4-trihydroxybenzoic acid, 2,4,6-trihydroxybenzoic acid, 3,4,5-trihydroxybenzoic acid, 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,3,5-benzenetricarboxylic acid, 2-[bis(4-hydroxyphenyl)methyl]benzoic acid, 1-naphthoic acid, 2- Naphthoic acid, 1-hydroxy-2-naphthoic acid, 2-hydroxy-1-naphthoic acid, 3-hydroxy-2-naphthoic acid, 6-hydroxy-2-naphthoic acid, 1,4-dihydroxy-2-naphthoic acid, 3,5-dihydroxy-2-naphthoic acid, 3,7-dihydroxy-2-naphthoic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2-phenoxybenzoic acid, biphenyl-4-carboxylic acid, biphenyl-2-carboxylic acid, 2-benzoylbenzoic acid, etc. From the viewpoint of easily obtaining excellent flux activity and easily obtaining the effects of the present invention, the (d) component may contain benzilic acid, diphenylacetic acid, or a combination thereof.

[0098] The content of the (d) component may be 0.1% by mass or more, 10% by mass or less, 5% by mass or less, or 2% by mass or less based on the total solid content of the adhesive for semiconductors. From the viewpoint of connection reliability and reflow resistance during semiconductor device fabrication, the content of the (d) component may be 0.1 to 10% by mass, 0.1 to 5% by mass, or 0.1 to 2% by mass based on the total solid content of the adhesive for semiconductors. When a compound having flux activity corresponds to the components (a) to (c), the content of the (d) component is calculated assuming that the compound also corresponds to the (d) component. The same applies to the molar number of acid groups described later.

[0099] In this embodiment, the ratio of the number of moles of acid groups in the total amount of component (d) to the number of moles of reactive groups in the total amount of component (c) may be 0.01 or more, or 4.8 or less. The above molar ratio may be 0.1 or more, 0.5 or more, 4.0 or less, or 3.0 or less. Some of the reactive groups in component (c) and the acid groups in component (d) may form salts, and in that case, the ratio of the number of moles including the reactive groups and acid groups that form the salt may be within the above range.

[0100] When component (d) contains at least one selected from the group consisting of monocarboxylic acids, dicarboxylic acids, and tricarboxylic acids, the ratio of the number of moles of acid groups in the total amount of component (d) to the number of moles of reactive groups in the total amount of component (c) may be 0.01 to 4.8, and the ratio of the number of moles of monocarboxylic acids to the number of moles of reactive groups in the total amount of component (c) may be 0.01 to 4.8, the ratio of the number of moles of dicarboxylic acids to the number of moles of reactive groups in the total amount of component (c) may be 0.01 to 2.4, and the ratio of the number of moles of tricarboxylic acids to the number of moles of reactive groups in the total amount of component (c) may be 0.01 to 1.6. The ratio of the number of moles of monocarboxylic acid to the number of moles of reactive groups in the total amount of component (c) may be 0.5 to 3.0, the ratio of the number of moles of dicarboxylic acid to the number of moles of reactive groups in the total amount of component (c) may be 0.25 to 1.5, and the ratio of the number of moles of tricarboxylic acid to the number of moles of reactive groups in the total amount of component (c) may be 0.5 / 3 to 1.0.

[0101] (e) Filler The semiconductor adhesive of this embodiment may contain a filler (component (e)) as necessary. Component (e) makes it possible to control the viscosity of the semiconductor adhesive, the physical properties of the cured product of the semiconductor adhesive, and the like. Specifically, component (e) makes it possible, for example, to suppress the generation of voids during connection, reduce the moisture absorption rate of the cured product of the semiconductor adhesive, and the like.

[0102] The component (e) may be an insulating inorganic filler, whiskers, a resin filler, etc. The component (e) may be used alone or in combination of two or more kinds.

[0103] Examples of insulating inorganic fillers include glass, silica, alumina, titanium oxide, carbon black, mica, and boron nitride. The insulating inorganic filler may be selected from silica, alumina, titanium oxide, and boron nitride, or may be selected from silica, alumina, and boron nitride.

[0104] Whiskers include, for example, aluminum borate, aluminum titanate, zinc oxide, calcium silicate, magnesium sulfate, and boron nitride.

[0105] Examples of the resin filler include fillers made of resins such as polyurethane and polyimide.

[0106] The resin filler has a smaller thermal expansion coefficient than organic components (epoxy resin, hardener, etc.), and therefore is excellent in improving connection reliability. The resin filler allows easy adjustment of the viscosity of the semiconductor adhesive. The resin filler has a superior stress relief function compared to inorganic fillers.

[0107] Since inorganic fillers have a smaller coefficient of thermal expansion than resin fillers, the adhesive composition can have a lower coefficient of thermal expansion by using inorganic fillers. Many inorganic fillers are general-purpose products with controlled particle size, which makes them suitable for viscosity adjustment.

[0108] Since the resin filler and the inorganic filler each have advantageous effects, either one may be used depending on the application, or both may be mixed and used to exert the functions of both.

[0109] There are no particular limitations on the shape, particle size, and content of component (e). Component (e) may have its physical properties appropriately adjusted by surface treatment.

[0110] The content of component (e) may be 10 mass% or more, or 15 mass% or more, and 80 mass% or less, or 60 mass% or less, based on the total solid content of the adhesive for semiconductors. The content of component (e) may be 10 to 80 mass%, or 15 to 60 mass%, based on the total solid content of the adhesive for semiconductors.

[0111] The component (e) is preferably made of an insulating material. If the component (e) is made of a conductive material (e.g., solder, gold, silver, copper), the insulation reliability (especially HAST resistance) may decrease.

[0112] (Other Ingredients) The semiconductor adhesive of the present embodiment may contain additives such as an antioxidant, a silane coupling agent, a titanium coupling agent, a leveling agent, and an ion trapping agent. These may be used alone or in combination of two or more. The amount of each additive may be appropriately adjusted so that the effect of each additive is exerted.

[0113] The adhesive for semiconductors of this embodiment may be in the form of a film. In this case, the workability can be improved when sealing the gap between a semiconductor chip and a wiring board or the gap between a plurality of semiconductor chips by the pre-applied method. An example of a method for producing the adhesive for semiconductors (film-like adhesive) of this embodiment formed into a film shape is shown below.

[0114] First, components (a), (b), (c), and (d), as well as component (e) which is added as necessary, are added to an organic solvent, and dissolved or dispersed by stirring, mixing, kneading, etc. to prepare a resin varnish. Thereafter, the resin varnish is applied onto a base film that has been subjected to a release treatment using a knife coater, roll coater, applicator, etc., and the coating film is heated to remove the organic solvent, thereby forming a film-like adhesive on the base film.

[0115] The thickness of the film-like adhesive is not particularly limited, and may be, for example, 0.5 to 1.5 times, 0.6 to 1.3 times, or 0.7 to 1.2 times the height of the bump before connection.

[0116] If the thickness of the film-like adhesive is 0.5 times or more the height of the bump, it is possible to sufficiently suppress the occurrence of voids due to unfilled adhesive, and further improve the connection reliability. If the thickness is 1.5 times or less, it is possible to sufficiently suppress the amount of adhesive pushed out from the chip connection area during connection, and it is possible to sufficiently prevent the adhesive from adhering to unnecessary parts. If the thickness of the film-like adhesive is more than 1.5 times, the bump must eliminate a lot of adhesive, which makes it more likely to cause electrical conduction failure. In response to the weakening of bumps due to narrower pitches and more pins (miniaturization of bump diameter), eliminating a lot of resin may increase the damage to the bumps.

[0117] Since the bumps generally have a height of 5 to 100 μm, the thickness of the film-like adhesive may be 2.5 to 150 μm, or 3.5 to 120 μm.

[0118] The organic solvent used in the preparation of the resin varnish may have the property of dissolving or dispersing each component uniformly. Examples of the organic solvent include dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. These organic solvents can be used alone or in combination of two or more. The stirring and mixing and kneading in the preparation of the resin varnish can be performed using, for example, a stirrer, a mortar and pestle, a three-roll mill, a ball mill, a bead mill, or a homodisper.

[0119] The substrate film is not particularly limited as long as it has heat resistance sufficient to withstand the heating conditions when volatilizing the organic solvent, and examples thereof include polyolefin films such as polypropylene film and polymethylpentene film, polyester films such as polyethylene terephthalate film and polyethylene naphthalate film, polyimide film, and polyetherimide film. The substrate film is not limited to a single layer made of these films, and may be a multilayer film made of two or more materials.

[0120] The drying conditions for volatilizing the organic solvent from the resin varnish applied to the substrate film may be any conditions that allow the organic solvent to volatilize sufficiently, and specifically may be heating at 50 to 200° C. for 0.1 to 90 minutes. The organic solvent may be removed to 1.5% by mass or less based on the total amount of the film-like adhesive.

[0121] The adhesive for semiconductor of this embodiment may be formed directly on a wafer. Specifically, for example, the resin varnish may be directly spin-coated on a wafer to form a film, and then the organic solvent may be removed to form a layer of the adhesive for semiconductor directly on the wafer.

[0122] The minimum melt viscosity of the adhesive for semiconductors of this embodiment may be 400 to 2500 Pa s, from the viewpoint that voids are more easily removed during curing under a pressurized atmosphere and more excellent reflow resistance is obtained. The minimum melt viscosity can be measured by the method described in the Examples. The temperature (melting temperature) at which the adhesive for semiconductors shows the minimum melt viscosity may be 100 to 200°C, or 120 to 170°C.

[0123] From the viewpoint of facilitating temporary fixing of semiconductor chips in a temperature range of 60 to 155° C., the semiconductor adhesive of this embodiment may have a melt viscosity of 2000 to 10000 Pa·s at 80° C., may have a melt viscosity of 500 to 5000 Pa·s at 130° C., or may have a melt viscosity of 2000 to 10000 Pa·s at 80° C. and a melt viscosity of 500 to 5000 Pa·s at 130° C. The above melt viscosity can be measured by the method described in the Examples.

[0124] The semiconductor adhesive of the present embodiment described above can be suitably used in a process of curing by applying heat under a pressurized atmosphere, and can be particularly used in a process in which multiple semiconductor chips are mounted on a mounting member (semiconductor chip, semiconductor wafer, wiring circuit board, etc.) via the semiconductor adhesive and temporarily fixed, and then cured and sealed all at once under pressurized conditions. When the semiconductor adhesive of the present embodiment is used in this process, voids inside the adhesive are easily removed by pressure, making it easier to obtain even better reflow resistance.

[0125] <Semiconductor device> The semiconductor device of this embodiment is a semiconductor device in which the connection parts of a semiconductor chip and a wiring circuit board are electrically connected to each other, or a semiconductor device in which the connection parts of a plurality of semiconductor chips are electrically connected to each other. In this semiconductor device, at least a part of the connection parts is sealed with a cured product of the semiconductor adhesive. Hereinafter, the semiconductor device of this embodiment will be described with reference to Figures 4, 5, and 6. Figures 4, 5, and 6 are each a cross-sectional view showing one embodiment of a semiconductor device that can be manufactured by a method according to an embodiment described later.

[0126] FIG. 4 is a schematic cross-sectional view showing a connection mode of a COB type in which a semiconductor chip and a substrate are connected. The semiconductor device 100 shown in FIG. 4 includes a semiconductor chip 1, a substrate 2 (wired circuit substrate), and an adhesive layer 40 interposed therebetween. In the case of the semiconductor device 100, the semiconductor chip 1 has a semiconductor chip body 10, wiring or bumps 15 arranged on the surface of the semiconductor chip body 10 facing the substrate 2, and solder 30 arranged on the wiring or bumps 15 as a connection part. The substrate 2 has a substrate body 20 and wiring or bumps 16 arranged on the surface of the substrate body 20 facing the semiconductor chip 1 as a connection part. The solder 30 of the semiconductor chip 1 and the wiring or bumps 16 of the substrate 2 are electrically connected by metal bonding. The semiconductor chip 1 and the substrate 2 are flip-chip connected by the wiring or bumps 16 and the solder 30. The wiring or bumps 15, 16 and the solder 30 are sealed by the adhesive layer 40 and are thus isolated from the external environment. The adhesive layer 40 can be a cured product of the above-mentioned adhesive for semiconductors.

[0127] 5 shows a COC type connection in which semiconductor chips are connected to each other. The configuration of a semiconductor device 300 shown in FIG. 5 is the same as that of the semiconductor device 100, except that two semiconductor chips 1 are flip-chip connected via wiring or bumps 15 and solder 30.

[0128] 5 and 6, the connection portion such as wiring or bump 15 may be a metal film (eg, gold plating) called a pad, or may be a post electrode (eg, copper pillar).

[0129] The semiconductor chip body 10 is not particularly limited, and can be a chip formed of various semiconductors such as elemental semiconductors composed of the same type of element, such as silicon, germanium, and compound semiconductors, such as gallium arsenide and indium phosphide.

[0130] The substrate 2 is not particularly limited as long as it is a wired circuit board, and examples that can be used include a circuit board in which wiring (wiring pattern) is formed by etching away unnecessary portions of a metal layer formed on the surface of an insulating substrate whose main component is glass epoxy, polyimide, polyester, ceramic, epoxy, bismaleimide triazine, etc., a circuit board in which wiring (wiring pattern) is formed on the surface of the insulating substrate by metal plating or the like, and a circuit board in which wiring (wiring pattern) is formed by printing a conductive material on the surface of the insulating substrate.

[0131] Gold, silver, copper, solder, tin, nickel, etc. are used as the main component of the connection parts such as the wiring or bumps 15 and 16 and the solder 30. The main component of the solder 30 may be, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, or tin-silver-copper. The connection parts may be composed of only a single component, or may be composed of multiple components. The connection parts may have a structure in which these metals are laminated. Of the metal materials, copper and solder are relatively inexpensive. From the viewpoint of improving connection reliability and suppressing warping, the connection parts may contain solder.

[0132] The main component of the pad may be gold, silver, copper, solder, tin, nickel, or the like. The main component of the solder may be, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, or tin-silver-copper. The pad may be composed of only a single component, or may be composed of multiple components. The pad may have a structure in which these metals are laminated. From the viewpoint of connection reliability, the pad may contain gold or solder.

[0133] A metal layer mainly composed of gold, silver, copper, solder, tin, nickel, etc. may be formed on the surface of the wiring or bumps 15, 16 (wiring pattern). The main component of the solder may be, for example, tin-silver, tin-lead, tin-bismuth, or tin-copper. This metal layer may be composed of only a single component, or may be composed of multiple components. The metal layer may have a structure in which multiple metal layers are laminated. The metal layer may contain relatively inexpensive copper or solder. From the viewpoint of improving connection reliability and suppressing warping, the metal layer may contain solder.

[0134] Semiconductor devices (or semiconductor packages) as shown in FIG. 4 or FIG. 5 may be stacked and electrically connected with gold, silver, copper, solder, tin, nickel, or the like. The main component of the solder may be, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, or tin-silver-copper. The metal for connection may be relatively inexpensive copper or solder. For example, as seen in TSV technology, an adhesive layer may be interposed between semiconductor chips, and flip-chip connection or stacking may be performed, and holes penetrating the semiconductor chips may be formed to connect to electrodes on the pattern surface.

[0135] FIG. 6 is a cross-sectional view showing another embodiment of a semiconductor device. The semiconductor device 500 shown in FIG. 6 is an embodiment of a semiconductor chip stacked TSV. In the semiconductor device 500 shown in FIG. 6, the wiring or bumps 15 formed on the interposer body 50 as a substrate are connected to the solder 30 of the semiconductor chip 1, so that the semiconductor chip 1 and the interposer 5 are flip-chip connected. An adhesive layer 40 is interposed between the semiconductor chip 1 and the interposer 5. On the surface of the semiconductor chip 1 opposite to the interposer 5, the semiconductor chips 1 are repeatedly stacked via the wiring or bumps 15, the solder 30, and the adhesive layer 40. The wiring or bumps 15 on the pattern surfaces on the front and back of the semiconductor chip 1 are connected to each other by the through electrodes 34 filled in the holes penetrating the inside of the semiconductor chip body 10. The material of the through electrodes 34 may be copper, aluminum, or the like.

[0136] Such TSV technology allows signals to be obtained from the back surface of the semiconductor chip, which is not normally used. Furthermore, since the through electrodes 34 are vertically passed through the semiconductor chip 1, the distance between the opposing semiconductor chips 1 and between the semiconductor chip 1 and the interposer 5 can be shortened, enabling flexible connection. In such TSV technology, the adhesive layer can be used as a sealing material between the opposing semiconductor chips 1 and between the semiconductor chip 1 and the interposer 5.

[0137] <Method of Manufacturing Semiconductor Device> One embodiment of the method for manufacturing a semiconductor device includes a lamination step of laminating a first member having a connection portion and a second member having a connection portion via a semiconductor adhesive so that the connection portion of the first member and the connection portion of the second member are arranged opposite each other, and a sealing step of curing the semiconductor adhesive by applying heat and sealing at least a part of the connection portion with the cured semiconductor adhesive. Here, the first member is, for example, a wiring circuit board, a semiconductor chip, or a semiconductor wafer, and the second member is a semiconductor chip. The sealing step includes heating the laminate (hereinafter sometimes referred to as a "temporary fixing body") obtained in the lamination step to a temperature equal to or higher than the melting point of the connection portions arranged opposite each other to bond the connection portions arranged opposite each other so that they are electrically connected, and curing the semiconductor adhesive by applying heat.

[0138] When the first component is a semiconductor chip, the stacking process includes, for example, a step of arranging a plurality of semiconductor chips on a stage, and a temporary fixing step of sequentially arranging other semiconductor chips on each of the plurality of semiconductor chips arranged on the stage via a semiconductor adhesive while heating the stage, to obtain a plurality of temporary fixing bodies which are laminates having semiconductor chips, semiconductor adhesive, and other semiconductor chips, which are stacked in this order.

[0139] When the first component is a wiring circuit board or a semiconductor wafer on which a plurality of semiconductor chips are mounted, the lamination process includes, for example, a step of arranging the wiring circuit board or the semiconductor wafer on a stage, and a temporary fixing step of sequentially arranging a plurality of semiconductor chips on the wiring circuit board or the semiconductor wafer arranged on the stage, via a semiconductor adhesive, while heating the stage, to obtain a temporary fixing body having the wiring circuit board, the semiconductor adhesive, and a plurality of the semiconductor chips, or a temporary fixing body having the semiconductor wafer, the semiconductor adhesive, and a plurality of the semiconductor chips.

[0140] In the temporary fixing step, for example, first, a semiconductor adhesive is placed on a first member or a second member. A film-like semiconductor adhesive may be attached to the first member or the second member. Next, the individual semiconductor chips on the dicing tape are picked up and adsorbed to a bonding tool (bonding head) of a bonding machine, and temporarily fixed to a wiring circuit board, another semiconductor chip, or a semiconductor wafer.

[0141] The method of disposing the semiconductor adhesive is not particularly limited, and for example, when the semiconductor adhesive is in the form of a film, methods such as hot pressing, roll lamination, and vacuum lamination may be used. The area and thickness of the semiconductor adhesive to be disposed are appropriately set depending on the size of the first member and the second member, the height of the connection portion (bump), and the like. The semiconductor adhesive may be disposed on a semiconductor chip. The semiconductor wafer on which the semiconductor adhesive is disposed may be divided into individual pieces by dicing.

[0142] In the temporary fixing process, alignment is required to electrically connect the connecting parts, so a compression bonding machine such as a flip chip bonder is generally used.

[0143] When the pressure bonding tool picks up the semiconductor chip for temporary fixing, the pressure bonding tool may be at a low temperature so that heat is not transferred to the semiconductor adhesive on the semiconductor chip. During pressure bonding (temporary pressure bonding), the semiconductor chip may be heated to a certain high temperature so that the fluidity of the semiconductor adhesive can be increased and the voids involved can be efficiently eliminated. The semiconductor chip may be heated at a temperature lower than the start temperature of the curing reaction of the semiconductor adhesive. In order to shorten the cooling time, the difference between the temperature of the pressure bonding tool when picking up the semiconductor chip and the temperature of the pressure bonding tool when temporarily fixing may be small. This temperature difference may be 100°C or less, 60°C or less, or substantially 0°C. If the temperature difference is 100°C or more, it takes time to cool the pressure bonding tool, which tends to reduce productivity. The start temperature of the curing reaction of the semiconductor adhesive refers to the onset temperature of the exothermic peak of the curing reaction when measured using a DSC (manufactured by PerkinElmer Co., Ltd., DSC-Pyirs1) under the conditions of a sample amount of 10 mg, a heating rate of 10°C / min, and an air or nitrogen atmosphere.

[0144] The load applied for temporary fixing is appropriately set in consideration of the number of connection parts (bumps), absorption of height variations of the connection parts (bumps), control of the deformation amount of the connection parts (bumps), etc. In the temporary fixing process, the opposing connection parts may be in contact with each other after pressure bonding (temporary pressure bonding). If the connection parts are in contact with each other after pressure bonding, metal bonds of the connection parts are easily formed in the pressure bonding (main pressure bonding) in the sealing process, and there is a tendency for the semiconductor adhesive to be less bitten. The load may be large in order to eliminate voids and make the connection parts contact, and may be, for example, 0.009 N to 0.2 N per connection part (e.g., bump).

[0145] The pressure bonding time in the temporary fixing step may be, for example, 5 seconds or less, 3 seconds or less, or 2 seconds or less, from the viewpoint of improving productivity.

[0146] The heating temperature of the stage is lower than the melting point of the connecting portion of the first member and the melting point of the connecting portion of the second member, and is usually 60 to 150° C. By heating at such a temperature, voids trapped in the adhesive for semiconductors can be efficiently eliminated.

[0147] When the lamination step includes the above-mentioned temporary fixing step, in the sealing step following the temporary fixing step, the adhesive for semiconductors in the multiple laminates or the laminate including multiple semiconductor chips may be cured collectively to seal the multiple connection parts collectively. In the sealing step, the opposing connection parts are joined by metallic bonding, and usually the gap between the connection parts is filled with the adhesive for semiconductors.

[0148] In the sealing process, the connection parts may be joined together by heating the temporary fixing body at a temperature equal to or higher than the melting point of at least one of the metals of the opposing connection parts (for example, bump-bump, bump-pad, bump-wiring). For example, when the metal of the connection part is solder, the heating temperature may be 220°C or higher and 330°C or lower. If the heating temperature is low, the metal of the connection part may not melt, and sufficient metal bonding may not be formed. If the heating temperature is excessively high, the effect of suppressing voids may become relatively small, or the solder may tend to easily scatter. For the joining of the connection parts, the temporary fixing body may be heated while being pressurized using a pressure bonding machine. The semiconductor adhesive may be cured by heating for joining the connection parts. The curing reaction of the semiconductor adhesive may be partially promoted during heating for joining the connection parts, and then the semiconductor adhesive may be further cured by applying heat under a pressurized atmosphere. Examples of devices for heating under a pressurized atmosphere include a pressurized reflow furnace and a pressurized oven.

[0149] When pressure is applied to bond the connection parts using a pressure bonding machine, the heat of the pressure bonding machine is not easily transferred to the semiconductor adhesive (fillet) protruding from the side of the connection parts, so that a heat treatment is often required to sufficiently proceed with the hardening of the semiconductor adhesive after the pressure bonding to bond the connection parts. Therefore, the pressure in the sealing process may be applied by air pressure in a pressure reflow oven, a pressure oven, etc., instead of the pressure bonding machine. The connection parts may be bonded and the semiconductor adhesive may be hardened by applying heat under a pressurized atmosphere. If pressure is applied by air pressure, heat can be applied to the entire body, and the heat treatment after pressure bonding can be shortened or eliminated, improving productivity. If pressure is applied by air pressure, it is easy to perform the main pressure bonding of multiple laminates (temporary fixed bodies) or laminates (temporary fixed bodies) including multiple temporarily fixed semiconductor chips all at once. Pressure by air pressure is more advantageous from the viewpoint of suppressing fillets than direct pressure using a pressure bonding machine. Suppressing fillets is important for the trend toward smaller and denser semiconductor devices.

[0150] The pressurized atmosphere in which pressure bonding is performed in the sealing step is not particularly limited, but may be an atmosphere containing air, nitrogen, formic acid, or the like.

[0151] The pressure of the pressure bonding in the sealing step is appropriately set depending on the size and number of the members to be connected. The pressure may be, for example, higher than atmospheric pressure and not more than 1 MPa. From the viewpoint of suppressing voids and improving connectivity, the pressure may be high. From the viewpoint of suppressing fillets, the pressure may be low. Therefore, the pressure may be 0.05 to 0.5 MPa.

[0152] The bonding time for the main bonding varies depending on the constituent metal of the connection, but from the viewpoint of improving productivity, the shorter the bonding time, the better. When the connection is a solder bump, the bonding time may be 20 seconds or less, 10 seconds or less, or 5 seconds or less. In the case of copper-copper or copper-gold metal connection, the bonding time may be 60 seconds or less.

[0153] When multiple semiconductor chips are stacked three-dimensionally, such as in a semiconductor device having a TSV structure, the multiple semiconductor chips may be stacked one by one and temporarily fixed in place, and then the stacked multiple semiconductor chips may be heated and pressurized together to obtain the semiconductor device.

[0154] Fig. 7 is a schematic cross-sectional view showing one embodiment of a method for manufacturing a semiconductor device. In the case of the method shown in Fig. 7, an adhesive layer 40A made of a semiconductor adhesive is interposed between a semiconductor chip 1 having a plurality of solders 30 as connecting parts and a semiconductor wafer 3 having a plurality of solders 32 as connecting parts, and the semiconductor chip 1, the semiconductor wafer 3, and the adhesive layer 40A are heated, so that the connecting parts (solder 30) of the semiconductor chip 1 and the connecting parts (solder 32) of the semiconductor wafer 3 are electrically connected to each other, and a joint 95 is formed in which the electrically connected connecting parts (solder 30, 32) are sealed by the adhesive layer 40 made of a hardened semiconductor adhesive. More specifically, the process of forming the bonded body 95 includes placing the semiconductor wafer 3 on the stage 60 as shown in (a) of FIG. 7; forming a temporary fixing body 90 which is a laminate composed of the semiconductor wafer 3, an adhesive layer 40A, and a semiconductor chip 1 as shown in (b) of FIG. 7; heating and pressurizing the temporary fixing body 90 to a temperature at which at least one of the solders 30 and 32 which are the connection parts melts as shown in (c) of FIG. 7 to form a bonded body 95 in which the solders 30 and 32 which are the connection parts are electrically connected as shown in (d) of FIG. 7; and heating the bonded body 95 in a pressurized atmosphere in a pressurized oven 85 as shown in (e) of FIG. 7 to form a hardened adhesive layer 40 which seals the connection parts (solder 30 and 32).

[0155] The semiconductor chip 1 has a semiconductor chip body 10, wiring or bumps 15 provided on the semiconductor chip body 10, and solder 30 as a connection portion provided on the wiring or bumps 15. The semiconductor wafer 3 has a wafer body 11, wiring or bumps 15 provided on the wafer body 11, solder 32 as a connection portion provided on the wiring or bumps 15, and a passivation film 17 provided on the wafer body 11 and covering the wiring or bumps 15.

[0156] The temporary fixing body 90 is formed by thermocompression bonding the adhesive-attached semiconductor chip 1' to the semiconductor wafer 3 by a compression tool 70 on a heated stage 60. The heating temperature of the stage 60 is lower than the melting points of the solder 30 and the solder 32, and may be, for example, 60 to 150°C, or 70 to 100°C. The temperature of the compression tool 70 may be, for example, 80 to 350°C, or 100 to 170°C. The time of thermocompression bonding to form the temporary fixing body 90 may be, for example, 5 seconds or less, 3 seconds or less, or 2 seconds or less.

[0157] The bonded body 95 is formed by applying pressure to the temporary fixing body 90 on the heated stage 60 while heating it to at least one of the melting point of the solder 30 and the melting point of the solder 32 using the bonding tool 80. The temperature of the bonding tool 80 may be, for example, 180° C. or more, 220° C. or more, or 250° C. or more, and may be 350° C. or less, 320° C. or less, or 300° C. or less. The heating temperature of the stage 60 during the thermocompression bonding to form the bonded body 95 may be 60 to 150° C., or 70 to 100° C. The time of thermocompression bonding by the bonding tool 80 to form the bonded body 95 may be, for example, 5 seconds or less, 3 seconds or less, or 2 seconds or less.

[0158] The adhesive layer 40A is sufficiently cured by heating and pressing in the pressure oven 85. However, the adhesive layer 40A may be partially cured during the heating and pressing process for forming the bonded body 95. The heating temperature in the pressure oven 85 may be a temperature that is lower than the melting point of the solders 30 and 32 and at which the adhesive layer 40A is cured, for example, 170 to 200°C.

[0159] A bonded body 95 having a plurality of semiconductor chips 1 may be formed by sequentially mounting a plurality of semiconductor chips 1 on one semiconductor wafer 3 via an adhesive layer 40, and then the bonded body 95 may be heated and pressurized in a pressure oven 85. In this case, the adhesive layer 40A between the semiconductor chip 1 initially placed on the semiconductor wafer 3 and the semiconductor wafer 3 continues to be subjected to a thermal history by the stage 60 until the mounting of all the semiconductor chips 1 is completed. Even after being subjected to a long period of thermal history, the adhesive layer 40A including the semiconductor adhesive according to the above-mentioned embodiment can provide the bonded body 95 with high reliability. EXAMPLES

[0160] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0161] The compounds used in the examples and comparative examples are as follows. (a) Component: Thermoplastic resin Polyurethane (manufactured by DIC Covestro Polymer Co., Ltd., product name "T-8175N", Tg: -23℃, Mw: 120000) Phenoxy resin (manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., product name "ZX1356-2", Tg: approx. 71°C, Mw: approx. 63,000) Phenoxy resin (product name "FX293", manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., Tg: approx. 160°C, Mw: approx. 40,000)

[0162] (b) Component: Thermosetting resin - Multifunctional solid epoxy resin containing a triphenolmethane skeleton (manufactured by Mitsubishi Chemical Corporation, product name "EP1032H60") Bisphenol F type liquid epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "YL983U")

[0163] (c) Component: Hardener 2,4-Diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (manufactured by Shikoku Chemical Industry Co., Ltd., product name "2MAOK-PW", Mw: 384) 2-Phenyl-4,5-dihydroxymethylimidazole (manufactured by Shikoku Chemical Industry Co., Ltd., product name "2PHZ-PW", Mw: 204)

[0164] (d) Ingredient: Flux compound Diphenolic acid (Tokyo Chemical Industry Co., Ltd., melting point: 177°C, molecular weight: 286) Benzilic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., melting point: 152°C, molecular weight: 228) Diphenylacetic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., melting point: 149°C, molecular weight: 212) Glutaric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., melting point: 98°C, molecular weight: 132)

[0165] (e) Filler Silica filler (manufactured by Admatechs Co., Ltd., product name "SE2030", average particle size 0.5 μm) Epoxy silane surface-treated silica filler (manufactured by Admatechs Co., Ltd., product name "SE2030-SEJ", average particle size 0.5 μm) Methacrylic surface-treated silica filler (manufactured by Admatechs Co., Ltd., product name "YA050C-SM1", average particle size approximately 0.05 μm) Methacrylic surface-treated silica filler (manufactured by Admatechs Co., Ltd., product name "180nm SM-EH1", average particle size approximately 0.18μm)

[0166] (a) The weight-average molecular weight (Mw) of the component was determined by the GPC method. The details of the GPC method are as follows. Apparatus name: HPLC-8020 (product name, manufactured by Tosoh Corporation) Columns: 2 pieces of GMHXL + 1 piece of G-2000XL Detector: RI detector Column temperature: 35 °C Flow rate: 1 mL / min Standard substance: Polystyrene

[0167] <Preparation of the Adhesive for Film状 Semiconductor> A thermoplastic resin, a thermosetting resin, a curing agent, a flux compound, and a filler in the blending amounts (unit: parts by mass) shown in Table 1 were added to an organic solvent (cyclohexanone) so that the NV value ([mass of the adhesive after drying] / [mass of the coating varnish before drying] × 100) became 50%. Into the same container as these mixtures, beads with a diameter of Φ1.0 mm and zirconia beads with a diameter of Φ2.0 mm having the same mass as the blending amount of the solid components (thermoplastic resin, thermosetting resin, curing agent, flux compound, and filler) were added, and the mixture was stirred with a ball mill (Fritsch Japan Co., Ltd., planetary type fine grinder P-7) for 30 minutes. After stirring, the zirconia beads were removed by filtration to prepare a coating varnish.

[0168] The obtained coating varnish was coated on a base film (manufactured by Toyobo Film Solutions Co., Ltd., trade name "Purelex A55") with a small precision coating apparatus (Renjing Precision Machinery). The coating film was dried at 100 °C for 10 minutes with a clean oven (manufactured by ESPEC) to obtain a film状 adhesive with a film thickness of 20 μm.

[0169] <DSC Measurement> The obtained film-like adhesive was weighed in an amount of 10 mg in an aluminum pan (manufactured by Epolead Service Co., Ltd.), covered with an aluminum lid, and the evaluation sample was sealed in the sample pan using a crimper. A differential scanning calorimeter (Thermo plus DSC8235E, manufactured by Rigaku Co., Ltd.) was used to measure DSC in a nitrogen atmosphere at a heating rate of 10°C / min and a measurement temperature range of 30 to 300°C. A partial area analysis method was used as a means of analyzing the amount of heat generated. By instructing analysis in the temperature range of 60°C to 280°C for each DSC curve, the baseline of the analysis temperature range was specified and the peak area was integrated to calculate the total amount of heat generated (unit: J / g). Next, by instructing 155°C as the division temperature, the partial areas of 60 to 155°C and 155 to 280°C were integrated to calculate each amount of heat generated (unit: J / g). On the other hand, as a means for analyzing the onset temperature, a total area (JIS method) analysis method was used, and the analysis was instructed in the temperature range of 60°C to 280°C to calculate the intersection of the baseline of the peak and the maximum slope point in each DSC curve, and the onset temperature (unit: °C) was obtained.

[0170] [Table 1] *In the table, the molar ratio r indicates the ratio of the number of moles of acid groups in the total amount of flux compound to the number of moles of reactive groups in the total amount of hardener.

[0171] The film-like adhesives obtained in the Examples and Comparative Examples were evaluated using the following methods. The evaluation results are shown in Table 2.

[0172] <Film Formability Evaluation> The 20 μm film-like adhesives obtained in the examples and comparative examples were punched out using a punch (φ20 mm) and a hammer from above. If the punched sample was not cracked, it was rated as "A", and if it was cracked and / or chipped, it was rated as "B".

[0173] <High temperature storage stability evaluation> The DSC curve obtained above was analyzed to calculate the calorific value (unit: J / g) from 60 to 280° C. This was defined as the initial calorific value.

[0174] The film-like adhesives (initial samples) obtained in the Examples and Comparative Examples were placed in an oven set at 100° C. and heat-treated for 1 hour. After heat treatment, the samples were removed to obtain evaluation sample A after heat treatment at 100° C.

[0175] The film-like adhesives (initial samples) obtained in the Examples and Comparative Examples were placed in an oven set at 80° C. and heat-treated for 12 hours. After heat treatment, the samples were removed to obtain evaluation sample B after heat treatment at 80° C.

[0176] Using evaluation sample A and evaluation sample B, the calorific value (unit: J / g) from 60 to 280° C. was calculated using the same procedure as before heating. This was defined as the calorific value after treatment.

[0177] The reaction rate was calculated using the two obtained heat values ​​(the heat value of the initial sample and the heat value of evaluation sample A, or the heat value of the initial sample and the heat value of evaluation sample B) according to the following formula. Reaction rate (%) = (initial heat generation amount - heat generation amount after heat treatment) / initial heat generation amount x 100 A response rate of less than 10% was rated as "A," a response rate of 10% or more but less than 20% was rated as "B," and a response rate of 20% or more was rated as "C."

[0178] <Viscosity measurement> Using the initial samples and evaluation sample A of the examples and comparative examples, the melt viscosity at 80°C (80°C viscosity), the melt viscosity at 130°C (130°C viscosity), the minimum melt viscosity, and the temperature showing the minimum melt viscosity (melting temperature) were measured using a rotational rheometer (manufactured by TA Instruments, product name: ARES-G2). [Measurement conditions] Heating rate: 10℃ / min Frequency: 10Hz Temperature range: 30~170℃

[0179] <Void evaluation> (Fabrication of semiconductor devices) The evaluation sample A prepared above was cut into a size of 7.5 mm square, and this was attached to a semiconductor chip with multiple solder bumps (chip size: 7.3 mm × 7.3 mm, thickness 0.1 mm, bump (connection part) height: about 45 μm (total of copper pillar and solder), number of bumps: 1048 pins, pitch 80 μm, product name: WALTS-TEG CC80, manufactured by Waltz Co., Ltd.) at 80 ° C. The semiconductor chip to which the film-like adhesive was attached was sequentially pressure-bonded to another semiconductor chip (chip size: 10 mm × 10 mm, thickness 0.1 mm, number of bumps: 1048 pins, pitch 80 μm, product name: WALTS-TEG IP80, manufactured by Waltz Co., Ltd.) by heating and pressing with a flip chip bonder (FCB3, manufactured by Panasonic Co., Ltd.), and the semiconductor chips were temporarily fixed to each other. The pressure-bonding conditions were 130 ° C, 75 N, and 2 seconds.

[0180] The temporarily fixed laminate (temporarily fixed body) was heat treated in an oven at 100°C for 3 hours, then removed once and heated and pressurized at 200°C for 1 hour at 0.6 MPa in a pressure oven to obtain a sample for void evaluation.

[0181] (Analysis and Evaluation) The appearance image of the above sample was taken by an ultrasonic imaging diagnostic device (Insight-300, manufactured by Insight Co., Ltd.). From the obtained image, an image of the adhesive layer between the chips was captured by a scanner (GT-9300UF, manufactured by Seiko Epson Corporation). In the captured image, voids were identified by color correction and two-tone gradation using image processing software (Adobe Photoshop (trade name)), and the proportion of the voids was calculated using a histogram. The area of ​​the entire adhesive layer including the voids was taken as 100%. When the area ratio of the voids was less than 10%, it was rated as "A", when the area ratio of the voids was 10% or more and less than 30%, it was rated as "B", and when it was 30% or more, it was rated as "C". The evaluation results are shown in Table 2.

[0182] [Table 2] [Explanation of symbols]

[0183] 1...semiconductor chip, 2...substrate, 3...semiconductor wafer, 10...semiconductor chip body, 11...wafer body, 15, 16...wiring or bumps, 20...substrate body, 30, 32...solder, 34...through electrode, 40...adhesive layer, 50...interposer body, 90...laminated body (temporary fixed body), 95...bonded body, 100, 300, 500...semiconductor device.

Claims

1. A semiconductor adhesive comprising a thermoplastic resin, a thermosetting resin, a curing agent having a reactive group, and a flux compound having an acid group, The adhesive for semiconductors has a heat generation amount of 20 J / g or less at 60 to 155°C in a DSC curve obtained by differential scanning calorimetry in which the adhesive for semiconductors is heated at a temperature increase rate of 10°C / min.

2. The adhesive for semiconductors according to claim 1 , wherein the thermoplastic resin has a weight average molecular weight of 10,000 or more.

3. 3. The adhesive for semiconductors according to claim 1, wherein the content of the thermoplastic resin is 1 to 30 mass % based on the total solid content of the adhesive for semiconductors.

4. The adhesive for a semiconductor according to any one of claims 1 to 3, wherein the curing agent comprises an amine-based curing agent.

5. The adhesive for a semiconductor according to any one of claims 1 to 4, wherein the curing agent comprises an imidazole-based curing agent.

6. 6. The semiconductor adhesive according to claim 1, wherein the content of the curing agent is 2.3 mass % or less based on the total solid content of the semiconductor adhesive.

7. The adhesive for semiconductors according to any one of claims 1 to 6, wherein the melting point of the flux compound is 25 to 230°C.

8. The semiconductor adhesive according to any one of claims 1 to 7, wherein the thermosetting resin contains an epoxy resin.

9. The adhesive for a semiconductor according to any one of claims 1 to 8, wherein the thermosetting resin is substantially free of an epoxy resin that is liquid at 35°C.

10. The adhesive for semiconductors according to any one of claims 1 to 9, which is in the form of a film.

11. A semiconductor adhesive according to any one of claims 1 to 10, which is used to harden the semiconductor adhesive by applying heat under a pressurized atmosphere and seal the connection portion of a semiconductor chip with the hardened semiconductor adhesive.

12. The adhesive for semiconductors according to any one of claims 1 to 11, wherein the adhesive for semiconductors has a minimum melt viscosity of 400 to 2500 Pa·s.

13. A semiconductor adhesive according to any one of claims 1 to 12, wherein the ratio of the number of moles of the acid groups in the total amount of the flux compound to the number of moles of the reactive groups in the total amount of the curing agent is 0.01 to 4.

8.

14. The method includes a step of mixing a thermoplastic resin, a thermosetting resin, a curing agent having a reactive group, and a flux compound having an acid group, A method for producing a semiconductor adhesive as described in any one of claims 1 to 13, wherein in the process, the curing agent and the flux compound are blended so that the ratio of the number of moles of the acid groups in the total amount of the flux compound to the number of moles of reactive groups in the total amount of the curing agent is 0.01 to 4.

8.

15. the flux compound comprises at least one selected from the group consisting of monocarboxylic acids, dicarboxylic acids, and tricarboxylic acids; A method for producing an adhesive for a semiconductor as described in claim 14, wherein in the process, the curing agent and the flux compound are blended so that the ratio of the number of moles of the monocarboxylic acid to the number of moles of the reactive groups in the total amount of the curing agent is 0.01 to 4.8, the ratio of the number of moles of the dicarboxylic acid to the number of moles of the reactive groups in the total amount of the curing agent is 0.01 to 2.4, and the ratio of the number of moles of the tricarboxylic acid to the number of moles of the reactive groups in the total amount of the curing agent is 0.01 to 1.

6.

16. The method for producing an adhesive for a semiconductor according to claim 14 or 15, wherein the weight average molecular weight of the thermoplastic resin is 10,000 or more.

17. The method for producing a semiconductor adhesive according to any one of claims 14 to 16, wherein the blending amount of the thermoplastic resin is 1 to 30 mass % based on the total solid content of the semiconductor adhesive.

18. The method for producing a semiconductor adhesive according to any one of claims 14 to 17, wherein the curing agent comprises an amine-based curing agent.

19. The method for producing a semiconductor adhesive according to any one of claims 14 to 18, wherein the curing agent comprises an imidazole-based curing agent.

20. A method for producing a semiconductor adhesive according to any one of claims 14 to 19, wherein the blending amount of the curing agent is 2.3 mass% or less based on the total solid content of the semiconductor adhesive.

21. The method for producing a semiconductor adhesive according to any one of claims 14 to 20, wherein the melting point of the flux compound is 25 to 230°C.

22. The method for producing a semiconductor adhesive according to any one of claims 14 to 21, wherein the thermosetting resin contains an epoxy resin.

23. The method for producing an adhesive for a semiconductor according to any one of claims 14 to 22, wherein the thermosetting resin does not substantially contain an epoxy resin that is liquid at 35°C.

24. The method for producing a semiconductor adhesive according to any one of claims 14 to 23, further comprising a step of forming a mixture containing the thermoplastic resin, the thermosetting resin, the curing agent, and the flux compound into a film.

25. A method for manufacturing a semiconductor device in which the connection portions of a semiconductor chip and a wiring circuit board are electrically connected to each other, or a method for manufacturing a semiconductor device in which the connection portions of a plurality of semiconductor chips are electrically connected to each other, comprising a sealing step of hardening a semiconductor adhesive described in any one of claims 1 to 13 by applying heat, and sealing at least a portion of the connection portions with the hardened semiconductor adhesive.

26. Before the sealing step, placing a plurality of semiconductor chips on a stage; 26. The method for manufacturing a semiconductor device according to claim 25, further comprising a temporary fixing process of sequentially arranging other semiconductor chips on each of the plurality of semiconductor chips arranged on the stage via the semiconductor adhesive while heating the stage to 60 to 155°C, to obtain a plurality of stacks each having the semiconductor chip, the semiconductor adhesive, and the other semiconductor chip, stacked in this order.

27. Before the sealing step, placing a printed circuit board or a semiconductor wafer on a stage; The method for manufacturing a semiconductor device according to claim 25, further comprising a temporary fixing process in which, while heating the stage to 60 to 155°C, a plurality of semiconductor chips are sequentially arranged on the wiring circuit board or semiconductor wafer arranged on the stage via the semiconductor adhesive, to obtain a laminate having the wiring circuit board, the semiconductor adhesive, and a plurality of the semiconductor chips, which are stacked in this order, or a laminate having the semiconductor wafer, the semiconductor adhesive, and a plurality of the semiconductor chips, which are stacked in this order.

28. A semiconductor device comprising a semiconductor chip having a connection portion and a wiring circuit board having a connection portion, the connection portion of the semiconductor chip and the connection portion of the wiring circuit board being electrically connected to each other; or A semiconductor device comprising a plurality of semiconductor chips each having a connection portion, the connection portions of the semiconductor chips being electrically connected to each other, A semiconductor device, wherein at least a portion of the connection portion is sealed with a cured product of the semiconductor adhesive according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Method for bonding semiconductor wafer and method for manufacturing semiconductor device

    JP2008294382A

  • Sheet for circuit member connection and method for producing semiconductor device

    JP2018145346A

  • Adhesive for semiconductor, fluxing agent, manufacturing method for semiconductor device, and semiconductor device

    WO2013125086A1

  • Adhesive for semiconductors, method for producing semiconductor device, and semiconductor device

    WO2018235854A1

Cited By

  • Adhesive for semiconductor, and semiconductor device

    JP2025163231A