Porous body and fuel cell including same
A porous body with a three-dimensional network structure, composed of nickel, cobalt, and specific additives, addresses the strength issues of current collectors in fuel cells, maintaining conductivity and preventing cracking for efficient electricity generation.
Patent Information
- Application Number
- JP2021567188
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-24
- Filing Date
- 2020-12-09
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Existing porous metal bodies used as current collectors for fuel cell electrodes lack appropriate strength, particularly for air and hydrogen electrodes, necessitating improvements for effective performance in high-temperature environments.
A porous body with a three-dimensional network structure composed of nickel, cobalt, a first element (boron, iron, or calcium), and a second element (sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, or tin) is developed, with specific mass ratios and oxygen content to enhance strength and conductivity, allowing it to function as a current collector in fuel cells.
The porous body maintains high conductivity and appropriate strength in high-temperature environments, preventing cracking and ensuring efficient electricity generation in fuel cells, even after prolonged operation.
Smart Images

Figure 0007567810000006 
Figure 0007567810000007 
Figure 0007567810000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a porous body and a fuel cell including the same. This application claims priority based on Japanese Patent Application No. 2019-232469, filed on December 24, 2019. All contents of the Japanese Patent Application are incorporated herein by reference. [Background technology]
[0002] 2. Description of the Related Art Porous bodies such as porous metal bodies have been used for a variety of purposes, such as battery electrodes, catalyst supports, metal composite materials, and filters, because of their high porosity and large surface area. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-154517 [Patent Document 2] JP 2012-132083 A [Patent Document 3] JP 2012-149282 A Summary of the Invention
[0004] A porous body according to one embodiment of the present disclosure is a porous body having a skeleton with a three-dimensional network structure, the main body of the skeleton contains nickel, cobalt, a first element, and a second element as constituent elements; a mass ratio of the cobalt to the total mass of the nickel and the cobalt is 0.2 or more and 0.8 or less; The first element is at least one element selected from the group consisting of boron, iron, and calcium, The second element is at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin, The ratio of the total mass of the first element and the second element to the mass of the main body of the skeleton is 5 ppm or more and 50,000 ppm or less.
[0005] A fuel cell according to one aspect of the present disclosure is a fuel cell including an air electrode current collector and a hydrogen electrode current collector, wherein at least one of the air electrode current collector or the hydrogen electrode current collector includes the porous body. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a schematic partial cross-sectional view showing an outline of a partial cross-section of a skeleton in a porous body according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a cross section perpendicular to the longitudinal direction of the skeleton. [Figure 3A] FIG. 3A is an enlarged schematic view focusing on one of the cells in a porous body to explain the three-dimensional network structure of the porous body according to one embodiment of the present disclosure. [Figure 3B] FIG. 3B is a schematic diagram showing one embodiment of the shape of the cell portion. [Figure 4A] FIG. 4A is a schematic diagram showing another embodiment of the shape of the cell portion. [Figure 4B] FIG. 4B is a schematic diagram showing still another embodiment of the shape of the cell portion. [Diagram 5] FIG. 5 is a schematic diagram showing an embodiment of two joined cell parts. [Figure 6] FIG. 6 is a schematic diagram showing an embodiment of four joined cell parts. [Figure 7] FIG. 7 is a schematic diagram showing one embodiment of a three-dimensional network structure formed by bonding a plurality of cells. [Figure 8] FIG. 8 is a schematic cross-sectional view showing a fuel cell according to one embodiment of the present disclosure. [Figure 9] FIG. 9 is a schematic cross-sectional view showing a fuel cell according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Problem that this disclosure aims to solve] As an example of a method for producing such a porous metal body, Japanese Patent Application Laid-Open No. 11-154517 (Patent Document 1) discloses a method for producing a porous metal body by treating a foamed resin or the like to impart electrical conductivity, forming an electroplated layer made of metal on the foamed resin, and, if necessary, burning and removing the foamed resin.
[0008] Furthermore, JP 2012-132083 A (Patent Document 2) discloses a metal porous body having a skeleton mainly composed of a nickel-tin alloy as a metal porous body having oxidation resistance and corrosion resistance properties, and JP 2012-149282 A (Patent Document 3) discloses a metal porous body having a skeleton mainly composed of a nickel-chromium alloy as a metal porous body having high corrosion resistance.
[0009] As described above, various porous bodies such as porous metal bodies are known. However, when these are used as current collectors for battery electrodes, particularly as current collectors for electrodes of solid oxide fuel cells (SOFCs) (e.g., current collectors for air electrodes and current collectors for hydrogen electrodes), there is room for further improvement, such as adjusting the strength of the porous body.
[0010] The present disclosure has been made in consideration of the above circumstances, and has an object to provide a porous body having appropriate strength as a current collector for an air electrode and a current collector for a hydrogen electrode of a fuel cell, and a fuel cell including the same.
[0011] [Effects of this disclosure] According to the above, it is possible to provide a porous body having an appropriate strength as an air electrode current collector and a hydrogen electrode current collector of a fuel cell, and a fuel cell including the porous body.
[0012] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. [1] A porous body according to one embodiment of the present disclosure is a porous body having a skeleton with a three-dimensional network structure, the main body of the skeleton contains nickel, cobalt, a first element, and a second element as constituent elements; a mass ratio of the cobalt to the total mass of the nickel and the cobalt is 0.2 or more and 0.8 or less; The first element is at least one element selected from the group consisting of boron, iron, and calcium, The second element is at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin, The ratio of the total mass of the first element and the second element to the mass of the main body of the skeleton is 5 ppm to 50,000 ppm. A porous body having such characteristics can have an appropriate strength as a current collector for an air electrode and a current collector for a fuel cell.
[0013] [2] The mass ratio of the cobalt to the total mass of the nickel and the cobalt is preferably 0.2 to 0.45 or 0.6 to 0.8. A porous body having such characteristics can have a suitable strength for use as an air electrode current collector and a hydrogen electrode current collector in a fuel cell.
[0014] [3] The mass ratio of the first element to the mass of the main body of the skeleton is preferably 4 ppm to 40,000 ppm. A porous body having such characteristics can have an appropriate strength for use as an air electrode current collector and a hydrogen electrode current collector in a fuel cell.
[0015] [4] The mass ratio of the second element is preferably 1 ppm or more and 10,000 ppm or less relative to the mass of the main body of the skeleton. A porous body having such characteristics can further have an appropriate strength.
[0016] [5] The main body of the skeleton preferably further contains oxygen as a constituent element. This embodiment means that the porous body is in an oxidized state due to use. Even in this state, the porous body can maintain high electrical conductivity in a high-temperature environment.
[0017] [6] The oxygen content in the main body of the skeleton is preferably 0.1% by mass to 35% by mass, which makes it possible to more effectively maintain high electrical conductivity in high-temperature environments.
[0018] [7] The main body of the skeleton preferably contains a spinel-type oxide, which also makes it possible to more effectively maintain high electrical conductivity in high-temperature environments.
[0019] [8] When the cross section of the main body of the skeleton is observed at a magnification of 3000 times to obtain an image, it is preferable that the number of voids with a major axis of 1 μm or more that appear in any 10 μm square region in the observed image is 5 or less, which can sufficiently improve the strength.
[0020] [9] The skeleton is preferably hollow, which allows the porous body to be lightweight and reduces the amount of metal required.
[0021]
[10] The porous body preferably has a sheet-like appearance and a thickness of 0.2 mm to 2 mm, which makes it possible to form thinner air electrode current collectors and hydrogen electrode current collectors than before, thereby reducing the amount of metal required and enabling the production of compact fuel cells.
[0022]
[11] A fuel cell according to an embodiment of the present disclosure includes an air electrode current collector and a hydrogen electrode current collector, and at least one of the air electrode current collector and the hydrogen electrode current collector includes the porous body. A fuel cell having such characteristics can maintain high conductivity in a high-temperature environment, and can generate electricity efficiently.
[0023] [Details of the embodiment of the present invention] Hereinafter, one embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described. However, the present embodiment is not limited thereto. In this specification, the notation in the form of "A to Z" means the upper and lower limits of a range (i.e., A or more and Z or less). When no unit is specified for A and a unit is specified only for Z, the unit of A and the unit of Z are the same.
[0024] <Porous body> The porous body according to this embodiment is a porous body having a skeleton having a three-dimensional network structure. The main body of the skeleton contains nickel, cobalt, a first element, and a second element as constituent elements. The mass ratio of the cobalt is 0.2 to 0.8 with respect to the total mass of the nickel and the cobalt. The first element contains at least one element selected from the group consisting of boron, iron, and calcium. The second element contains at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin. In one aspect of this embodiment, the first element is preferably at least one element selected from the group consisting of boron, iron, and calcium. The second element is preferably at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin. The ratio of the total mass of the first element and the mass of the second element is 5 ppm to 50,000 ppm with respect to the mass of the main body of the skeleton. A porous body having such characteristics can have an appropriate strength as a current collector for an air electrode and a current collector for a hydrogen electrode of a fuel cell. Here, examples of the "porous body" in this embodiment include a porous body made of a metal, a porous body made of an oxide of the metal, and a porous body containing a metal and an oxide of the metal.
[0025] A porous body in which the mass ratio of cobalt to the total mass of nickel and cobalt in the main body of the skeleton is 0.2 or more has high strength, and the skeleton is less likely to crack even if it is deformed during stacking in an SOFC. In addition, a porous body in which the mass ratio of cobalt to the total mass of nickel and cobalt in the main body of the skeleton is 0.8 or less, even if a fuel cell is manufactured using the porous body as a cathode current collector or a hydrogen electrode current collector, the solid electrolyte, which is a component of the fuel cell, is less likely to crack. Therefore, when the mass ratio of cobalt to the total mass of nickel and cobalt in the main body of the skeleton is 0.2 or more and 0.8 or less, the porous body having the skeleton has an appropriate strength as an cathode current collector and a hydrogen electrode current collector of a fuel cell.
[0026] The porous body can have various shapes such as a sheet, a rectangular parallelepiped, a sphere, and a cylinder. In particular, the porous body has a sheet-like appearance and preferably has a thickness of 0.2 mm or more and 2 mm or less. The thickness of the porous body is more preferably 0.5 mm or more and 1 mm or less. When the thickness of the porous body is 2 mm or less, the porous body is thinner than conventional porous bodies, which reduces the amount of metal required and allows the production of compact fuel cells. When the thickness of the porous body is 0.2 mm or more, the required strength can be provided. The thickness can be measured, for example, by a commercially available digital thickness gauge.
[0027] <Skeleton> The porous body has a skeleton having a three-dimensional network structure as described above. The skeleton body contains nickel, cobalt, a first element, and a second element as constituent elements. The mass ratio of the cobalt to the total mass of the nickel and the cobalt is 0.2 to 0.8.
[0028] As shown in FIG. 1, the skeleton has a three-dimensional mesh structure having pores 14. Details of the three-dimensional mesh structure will be described later. The skeleton 12 is composed of a main body 11 (hereinafter sometimes referred to as "skeleton main body 11") containing nickel, cobalt, a first element, and a second element as constituent elements, and a hollow interior 13 surrounded by this skeleton main body 11. The skeleton main body 11 forms support parts and node parts described later. In this way, it is preferable that the skeleton is hollow.
[0029] Furthermore, as shown in FIG. 2, it is preferable that the cross-sectional shape of the skeleton 12 perpendicular to its longitudinal direction is triangular. However, the cross-sectional shape of the skeleton 12 should not be limited to this. The cross-sectional shape of the skeleton 12 may be a polygon other than a triangle, such as a square or a hexagon. In this embodiment, the concept of "triangle" includes not only a geometric triangle, but also an approximately triangular shape (for example, a shape with a chamfered apex angle, a shape with an R added to the apex angle, etc.). The same applies to other polygons. In one aspect of this embodiment, the cross-sectional shape of the skeleton 12 may be circular.
[0030] That is, it is preferable that the skeleton 12 has a hollow cylindrical shape with an interior 13 surrounded by the skeleton body 11, and a cross section perpendicular to the longitudinal direction is a triangle or other polygon, or a circle. Since the skeleton 12 is cylindrical, the skeleton body 11 has an inner wall forming the inner surface of the cylinder, and an outer wall forming the outer surface of the cylinder. Since the skeleton 12 has a hollow interior 13 surrounded by the skeleton body 11, the porous body can be made very lightweight. However, the skeleton is not limited to being hollow, and may be solid. When the interior 13 is solid, the strength of the porous body can be improved.
[0031] The framework has a total weight of nickel and cobalt of 200g / m 2 More than 1000g / m 2 The weight per unit area is preferably 250 g / m or less. 2 More than 900g / m 2As described later, the above-mentioned basis weight can be appropriately adjusted, for example, when nickel-cobalt alloy plating is performed on a conductive resin molded body that has been subjected to a conductive treatment to impart conductivity.
[0032] The total weight of nickel and cobalt described above can be converted into the mass per unit volume of the skeleton (apparent density of the skeleton) as follows. That is, the apparent density of the skeleton is 0.14 g / cm 3 More than 0.75g / cm 3 It is preferable that the density is 0.18 g / cm or less. 3 More than 0.65g / cm 3 It is more preferable that the apparent density of the skeleton is equal to or less than 1. Here, the "apparent density of the skeleton" is defined by the following formula. Skeleton apparent density (g / cm 3 )=M(g) / V(cm 3 ) M: Mass of the skeleton [g] V: Volume of the external shape in the skeleton [cm 3 ].
[0033] The skeleton preferably has a porosity of 40% or more and 98% or less, more preferably 45% or more and 98% or less, and most preferably 50% or more and 98% or less. When the skeleton has a porosity of 40% or more, the porous body can be made very lightweight and the surface area of the porous body can be increased. When the skeleton has a porosity of 98% or less, the porous body can be provided with sufficient strength.
[0034] The porosity of the skeleton is defined as follows: Porosity (%) = [1-{M / (V×d)}]×100 M: Mass of the skeleton [g] V: Volume of the external shape in the skeleton [cm 3 ] d: Density of the material that constitutes the skeleton [g / cm 3 ].
[0035] The skeleton preferably has an average pore diameter of 60 μm or more and 3500 μm or less. When the skeleton has an average pore diameter of 60 μm or more, the strength of the porous body can be increased. When the skeleton has an average pore diameter of 3500 μm or less, the bendability (bending processability) of the porous body can be increased. From these viewpoints, the skeleton has an average pore diameter of more preferably 60 μm or more and 1000 μm or less, and most preferably 100 μm or more and 850 μm or less.
[0036] The average pore size of the skeleton can be determined by the following method. First, a microscope is used to prepare observation images of at least 10 fields of view in which the surface of the skeleton is magnified 3000 times. Next, the number of pores per inch (25.4 mm = 25400 μm) in the skeleton is determined in each of the 10 fields of view. Furthermore, the number of pores in the 10 fields of view is averaged (n c ) and then substituting this into the following formula to calculate the value, which is the average pore diameter of the skeleton. Average pore size (μm) = 25400μm / n c .
[0037] Here, the porosity and average pore diameter of the skeleton can also be understood as the porosity and average pore diameter of the porous body.
[0038] When the cross section of the skeleton body is observed at a magnification of 3000 times to obtain an observation image, the number of voids with a major axis of 1 μm or more that appear in any 10 μm square region in the observation image is preferably 5 or less. In this embodiment, the "major axis" means the longest distance between any two points on the outer edge of the void in the observation image. The number of voids is more preferably 3 or less. This can sufficiently improve the strength of the porous body. Furthermore, since the number of voids in the skeleton body is 5 or less, it is understood that the skeleton body is different from a molded body made by sintering fine powder. The lower limit of the number of voids observed is, for example, 0. Here, the "number of voids" means the number average of voids obtained by observing multiple (for example, 10) "10 μm square regions" in the cross section of the skeleton body.
[0039] The cross section of the skeleton can be observed using an electron microscope. Specifically, it is preferable to determine the above-mentioned "number of voids" by observing the cross section of the skeleton body in 10 fields of view. The cross section of the skeleton body may be a cross section perpendicular to the longitudinal direction of the skeleton (e.g., FIG. 2), or a cross section parallel to the longitudinal direction of the skeleton (e.g., FIG. 1). In the observed image, the voids can be distinguished from other parts by color contrast (difference between light and dark). The upper limit of the major axis of the voids should not be limited, but is, for example, 10,000 μm.
[0040] The average thickness of the skeleton body is preferably 10 μm or more and 50 μm or less. Here, the "thickness of the skeleton body" means the shortest distance from the inner wall, which is the interface with the hollow inside of the skeleton, to the outer wall outside the skeleton. The average value of the "thickness of the skeleton body" measured at multiple points is defined as the "average thickness of the skeleton body." The thickness of the skeleton body can be measured by observing the cross section of the skeleton with an electron microscope.
[0041] Specifically, the average thickness of the skeleton body can be determined by the following method. First, a sheet-like porous body is cut so that the cross section of the skeleton body appears. One of the cut cross sections is selected and observed under an electron microscope at a magnification of 3000 times to obtain an observation image. Next, the thickness of any one side of a polygon (for example, the triangle in FIG. 2) forming one skeleton shown in this observation image is measured at the center of the side, and this is taken as the thickness of the skeleton body. Furthermore, such measurements are performed on 10 observation images (10 fields of view) to obtain the thicknesses of the skeleton body at 10 points. Finally, the average of these measurements can be calculated to obtain the average thickness of the skeleton body.
[0042] (Three-dimensional mesh structure) The porous body includes a skeleton having a three-dimensional mesh structure. In this embodiment, the term "three-dimensional mesh structure" refers to a three-dimensional mesh structure. The three-dimensional mesh structure is formed by the skeleton. The three-dimensional mesh structure will be described in detail below.
[0043] As shown in FIG. 7, the three-dimensional mesh structure 30 is formed by joining a plurality of cell parts 20, with the cell part 20 being the basic unit. As shown in FIG. 3A and FIG. 3B, the cell part 20 includes a support part 1 and a node part 2 connecting the plurality of support parts 1. For convenience, the support part 1 and the node part 2 are described separately, but there is no clear boundary between them. That is, the cell part 20 is formed by integrating a plurality of support parts 1 and a plurality of node parts 2, and the three-dimensional mesh structure 30 is formed with the cell part 20 as a constituent unit. In the following, for ease of understanding, the cell part in FIG. 3A will be described as a regular dodecahedron in FIG. 3B.
[0044] First, the frame portion 10, which is a planar polygonal structure, is formed by the presence of a plurality of support portions 1 and a plurality of node portions 2. In FIG. 3B, the polygonal structure of the frame portion 10 is a regular pentagon, but it may be a polygon other than a regular pentagon, such as a triangle, a rectangle, or a hexagon. Here, the structure of the frame portion 10 can be understood as a planar polygonal hole being formed by a plurality of support portions 1 and a plurality of node portions 2. In this embodiment, the hole diameter of the planar polygonal hole means the diameter of a circle circumscribing the planar polygonal hole defined by the frame portion 10. A plurality of frame portions 10 are combined to form a cell portion 20, which is a three-dimensional polyhedral structure. At this time, one support portion 1 and one node portion 2 are shared by a plurality of frame portions 10.
[0045] As shown in the schematic diagram of Fig. 2 described above, the support part 1 has a hollow cylindrical shape and preferably has a triangular cross section, but should not be limited thereto. The cross section of the support part 1 may be a polygon other than a triangle, such as a square or hexagon, or may be a circle. The shape of the node part 2 may be a sharp-edged shape having a vertex, a flat shape with the vertex chamfered, or a curved shape with the vertex given an arc.
[0046] The polyhedral structure of the cell portion 20 is a dodecahedron in FIG. 3B, but may be other polyhedrons such as a cube, an icosahedron (FIG. 4A), or a truncated icosahedron (FIG. 4B). Here, the structure of the cell portion 20 can be understood as a three-dimensional space (pore portion 14) surrounded by a virtual plane A defined by each of the multiple frame portions 10. In this embodiment, the pore diameter of the three-dimensional space (hereinafter also referred to as "pore diameter") can be understood as the diameter of a sphere circumscribing the three-dimensional space defined by the cell portion 20. However, the average pore diameter of the porous body in this embodiment is calculated based on the above-mentioned calculation formula for convenience. In other words, the average value of the pore diameter (pore diameter) of the three-dimensional space defined by the cell portion 20 is considered to be the average pore diameter of the skeleton.
[0047] A plurality of cell portions 20 are combined to form a three-dimensional mesh structure 30 (FIGS. 5 to 7). At this time, the frame portion 10 is shared by two cell portions 20. The three-dimensional mesh structure 30 can be understood as including the frame portion 10 or as including the cell portions 20.
[0048] As described above, the porous body has a three-dimensional mesh structure that forms planar polygonal holes (frame portion) and three-dimensional spaces (cell portion). Therefore, it can be clearly distinguished from two-dimensional mesh structures (such as punched metal, mesh, etc.) that have only planar holes. Furthermore, since the porous body has a three-dimensional mesh structure formed by integrating a plurality of support parts and a plurality of node parts, it can be clearly distinguished from structures such as nonwoven fabrics formed by intertwining fibers, which are constituent units. Since the porous body has such a three-dimensional mesh structure, it can have interconnected pores.
[0049] In this embodiment, the three-dimensional mesh structure is not limited to the above-mentioned structure. For example, the cell part may be formed by a plurality of frame parts each having a different size and planar shape. Furthermore, the three-dimensional mesh structure may be formed by a plurality of cell parts each having a different size and three-dimensional shape. The three-dimensional mesh structure may include a frame part in which a planar polygonal hole is not formed, or may include a cell part in which a three-dimensional space is not formed (a cell part with a solid interior).
[0050] (nickel and cobalt) The main body of the skeleton contains nickel, cobalt, the first element, and the second element as constituent elements, as described above. The main body of the skeleton does not exclude the inclusion of other components than nickel, cobalt, the first element, and the second element, as long as the action and effect of the porous body of the present disclosure is not affected. In one aspect of the present embodiment, the main body of the skeleton is preferably composed of the above four components (nickel, cobalt, the first element, and the second element) as metal components. Specifically, the main body of the skeleton preferably contains a nickel-cobalt alloy composed of nickel and cobalt, the first element, and the second element. The nickel-cobalt alloy is preferably the main component of the main body of the skeleton. Here, the "main component" of the main body of the skeleton refers to a component that occupies the largest mass ratio in the main body of the skeleton. More specifically, it refers to a component that occupies a mass ratio of more than 50 mass% in the main body of the skeleton.
[0051] The total ratio of the nickel mass and the cobalt mass in the skeleton body is preferably 80 mass% or more, more preferably 90 mass% or more, and even more preferably 95 mass% or more, relative to the mass of the skeleton body, for example, in a state before the porous body is used as an air electrode current collector or a hydrogen electrode current collector of an SOFC, i.e., in a state before the porous body is exposed to a high temperature of 700° C. or more. The upper limit of the total ratio of the nickel mass and the cobalt mass may be less than 100 mass%, or may be 99 mass% or less, or may be 95 mass% or less, relative to the mass of the skeleton body.
[0052] When the porous body is used as an SOFC air electrode current collector or hydrogen electrode current collector, the higher the total mass ratio of nickel and cobalt, the higher the proportion of the oxides produced that are spinel-type oxides consisting of at least one of nickel and cobalt and oxygen tends to be. This allows the porous body to maintain high electrical conductivity even when used in high-temperature environments.
[0053] (Mass ratio of cobalt to the total mass of nickel and cobalt) The mass ratio of cobalt to the total mass of nickel and cobalt is 0.2 to 0.8. When a porous material having a skeleton with such a composition is used as an air electrode current collector or a hydrogen electrode current collector of an SOFC, Ni 3-x Co x O4 (where 0.6≦x≦2.4), typically a spinel oxide with the chemical formula NiCo2O4 or Ni2CoO4, is generated in the framework. Oxidation of the framework itself may generate a spinel oxide with the chemical formula CoCo2O4. Spinel oxides exhibit high electrical conductivity, and therefore the porous body can maintain high electrical conductivity even when the entire framework itself is oxidized due to use in a high-temperature environment.
[0054] The mass ratio of the cobalt is preferably 0.2 to 0.45 or 0.6 to 0.8 relative to the total mass of nickel and cobalt, and more preferably 0.2 to 0.45. When the mass ratio of cobalt to the total mass of nickel and cobalt in the main body of the skeleton is 0.6 to 0.8, the strength of the porous body is higher, and the main body of the skeleton is less likely to crack even if it is deformed during stacking of SOFCs. In addition, when the mass ratio of cobalt to the total mass of nickel and cobalt in the main body of the skeleton is 0.2 to 0.45, the solid electrolyte, which is a component of the fuel cell, is less likely to crack even when the porous body is used as a current collector for an air electrode or a current collector for a hydrogen electrode to manufacture a fuel cell.
[0055] (oxygen) The main body of the skeleton preferably further contains oxygen as a constituent element. Specifically, the main body of the skeleton more preferably contains oxygen in an amount of 0.1% by mass to 35% by mass. The oxygen in the main body of the skeleton can be detected, for example, after the porous body is used as a current collector for an air electrode or a current collector for a hydrogen electrode of an SOFC. That is, after the porous body is exposed to a high temperature of 700° C. or more, the main body of the skeleton preferably contains oxygen in an amount of 0.1% by mass to 35% by mass. The main body of the skeleton more preferably contains oxygen in an amount of 10% by mass to 30% by mass, and even more preferably contains oxygen in an amount of 25% by mass to 28% by mass.
[0056] When the main body of the above-mentioned skeleton contains oxygen in an amount of 0.1% by mass or more and 35% by mass or less as a constituent element, it is possible to infer that the porous body has a thermal history of being exposed to a high temperature of 700° C. or more. Furthermore, when the porous body is used as an air electrode current collector or a hydrogen electrode current collector of an SOFC and exposed to a high temperature of 700° C. or more, and a spinel-type oxide consisting of at least one of nickel and cobalt and oxygen is generated in the skeleton, the main body of the above-mentioned skeleton tends to contain oxygen in an amount of 0.1% by mass or more and 35% by mass or less as a constituent element.
[0057] That is, the main body of the skeleton preferably contains a spinel-type oxide. This allows the porous body to more effectively maintain high electrical conductivity even when oxidized. If the mass ratio of oxygen in the main body of the skeleton is outside the above range, the porous body tends not to be able to effectively maintain high electrical conductivity as desired when oxidized.
[0058] (first element) The first element includes at least one element selected from the group consisting of boron, iron, and calcium. The first element is preferably at least one element selected from the group consisting of boron, iron, and calcium. The first element is believed to be present at the grain boundaries of crystal grains containing nickel and cobalt. The present inventors believe that the presence of the first element at the grain boundaries of the crystal grains suppresses the coarsening of the crystal grains, thereby improving the hardness (strength) of the skeletal body.
[0059] The mass ratio of the first element is preferably 4 ppm or more and 40000 ppm or less, more preferably 20 ppm or more and 10000 ppm or less, based on the mass of the main body of the skeleton. When multiple types of the first element are included, the mass ratio of the first element means the total mass ratio of these multiple types of elements. The mass ratio of the first element can be obtained by an EDX device (energy dispersive X-ray analyzer) described later.
[0060] (Second element) The second element includes at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin. The second element is preferably at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin. The second element is considered to be present at the grain boundaries of crystal grains containing nickel and cobalt. The present inventors believe that the presence of the second element at the grain boundaries of the crystal grains suppresses the coarsening of the crystal grains, thereby improving the hardness (strength) of the skeletal body.
[0061] In addition, it is believed that the second element, together with the first element, is contained in the skeletal body, thereby preventing the grain boundary diffusion of the first element. On the other hand, it is believed that the first element, together with the second element, is contained in the skeletal body, thereby preventing the grain boundary diffusion of the second element. In other words, the present inventors believe that the inclusion of both the first element and the second element in the skeletal body prevents the grain boundary diffusion of both elements, thereby efficiently suppressing the coarsening of the crystal grains.
[0062] The mass ratio of the second element is preferably 1 ppm or more and 10000 ppm or less, more preferably 1 ppm or more and 5000 ppm or less, based on the mass of the main body of the skeleton. When multiple types of the second element are included, the mass ratio of the second element means the total mass ratio of these multiple types of elements. The mass ratio of the second element can be determined by an EDX device described later.
[0063] In one aspect of this embodiment, the first element may be boron, and the second element may be at least one element selected from the group consisting of sodium, aluminum, zinc, and tin. The first element may be iron, and the second element may be at least one element selected from the group consisting of magnesium, copper, potassium, and aluminum. The first element may be calcium, and the second element may be at least one element selected from the group consisting of sodium, tin, chromium, titanium, and silicon.
[0064] In one aspect of this embodiment, the first element may be boron and calcium and the second element may be sodium, aluminum and silicon. The first element may be boron and iron and the second element may be magnesium and tin. The first element may be boron, iron and calcium and the second element may be sodium, aluminum, silicon and tin.
[0065] The ratio of the total mass of the first element and the second element to the total mass of the skeleton is 5 ppm to 50,000 ppm, preferably 10 ppm to 10,000 ppm, and more preferably 55 ppm to 477 ppm. When multiple types of the first element are included, the mass of the first element means the total mass of these multiple types of elements. The same applies to the second element.
[0066] (Other ingredients) The main body of the skeleton may contain other components as constituent elements as described above, so long as the effects of the porous body of the present disclosure are not affected. The skeleton may contain, for example, carbon, tungsten, phosphorus, silver, gold, molybdenum, nitrogen, sulfur, fluorine, and chlorine as other components. Furthermore, the main body of the skeleton may contain the above-mentioned oxygen as other components before the porous body is used as an air electrode current collector or a hydrogen electrode current collector of an SOFC. The other components in the main body of the skeleton are preferably each individually 5% by mass or less, and preferably 10% by mass or less in total.
[0067] In one aspect of this embodiment, the skeleton body may further include at least one nonmetallic element selected from the group consisting of nitrogen, sulfur, fluorine, and chlorine as a constituent element. The nonmetallic elements may have a total mass ratio of 5 ppm to 10,000 ppm relative to the skeleton body. Preferably, the nonmetallic elements have a total mass ratio of 10 ppm to 8,000 ppm relative to the skeleton body.
[0068] The skeleton body may further contain phosphorus as a constituent element. In this case, the mass ratio of phosphorus may be 5 ppm or more and 50,000 ppm or less with respect to the mass of the skeleton body. Preferably, the mass ratio of phosphorus is 10 ppm or more and 40,000 ppm or less with respect to the mass of the skeleton body.
[0069] In another aspect of this embodiment, the skeletal body may further contain at least two nonmetallic elements selected from the group consisting of nitrogen, sulfur, fluorine, chlorine, and phosphorus as constituent elements. The nonmetallic elements may have a total mass ratio of 5 ppm to 50,000 ppm relative to the mass of the skeletal body. Preferably, the nonmetallic elements have a total mass ratio of 10 ppm to 10,000 ppm relative to the mass of the skeletal body.
[0070] When the porous body is used as an air electrode current collector or a hydrogen electrode current collector in a fuel cell, it is exposed to a high-temperature environment of 700°C or higher as described above. However, since the main body of the skeleton contains the nonmetallic elements as constituent elements, it is possible to maintain an appropriate strength.
[0071] (Method for measuring the mass ratio of each element) The mass percentage (mass%) of each element (e.g., oxygen) in the main body of the skeleton can be determined by analyzing an observation image (electron microscope image) of a cross section of the cut skeleton using an EDX device (e.g., SEM part: product name "SUPRA35VP", manufactured by Carl Zeiss Microscopy Co., Ltd., EDX part: product name "octane super", manufactured by Ametech Co., Ltd.) attached to an electron microscope (SEM). The EDX device can also determine the mass percentages of nickel, cobalt, the first element, and the second element in the main body of the skeleton. Specifically, based on the atomic concentration of each element detected by the EDX device, the mass percentages and mass ratios of nickel, cobalt, the first element, and the second element in the main body of the skeleton can be determined. When oxygen is contained in the main body of the skeleton, the mass percentage of oxygen in the main body of the skeleton can also be determined by the same method. Furthermore, whether or not the main body of the skeleton contains a spinel-type oxide consisting of at least one of nickel and cobalt, and oxygen can be identified by using an X-ray diffraction (XRD) method in which X-rays are irradiated to the cross section and the diffraction pattern is analyzed.
[0072] As a measuring device for determining whether the main body of the skeleton contains a spinel-type oxide, for example, an X-ray diffraction device (for example, product name (model number): "Empyrean", manufactured by Spectris, Inc., analysis software: "Integrated Powder X-ray Analysis Software PDXL") can be used. The measurement conditions may be, for example, as follows.
[0073] (Measurement conditions) X-ray diffraction method: θ-2θ method Measurement system: Parallel beam optical mirror Scan range (2θ): 10~90° Integration time: 1 second / step Step: 0.03°.
[0074] ≪Fuel cell≫ The fuel cell according to the present embodiment is a fuel cell including an air electrode current collector and a hydrogen electrode current collector. At least one of the air electrode current collector and the hydrogen electrode current collector includes the porous body. The air electrode current collector and the hydrogen electrode current collector include a porous body having an appropriate strength as a current collector for a fuel cell as described above. Therefore, the air electrode current collector and the hydrogen electrode current collector are suitable as at least one of the air electrode current collector and the hydrogen electrode current collector of a SOFC. In the fuel cell, since the porous body includes nickel, cobalt, a first element, and a second element, it is more suitable to use the porous body as the air electrode current collector.
[0075] 8 is a schematic cross-sectional view showing a fuel cell according to one embodiment of the present disclosure. A fuel cell 150 includes a hydrogen electrode current collector 110, an air electrode current collector 120, and a fuel cell cell 100. The fuel cell cell 100 is provided between the hydrogen electrode current collector 110 and the air electrode current collector 120. Here, the "hydrogen electrode current collector" refers to a current collector on the side that supplies hydrogen in the fuel cell. The "air electrode current collector" refers to a current collector on the side that supplies a gas containing oxygen (e.g., air) in the fuel cell.
[0076] FIG. 9 is a schematic cross-sectional view showing a fuel cell according to one embodiment of the present disclosure. The fuel cell 100 includes an air electrode 102, a hydrogen electrode 108, an electrolyte layer 106 provided between the air electrode 102 and the hydrogen electrode 108, and an intermediate layer 104 provided between the electrolyte layer 106 and the air electrode 102 to prevent a reaction between them. For example, an oxide of LaSrCo (LSC) is used as the air electrode. For example, an oxide of Zr doped with Y (YSZ) is used as the electrolyte layer. For example, an oxide of Ce doped with Gd (GDC) is used as the intermediate layer. For example, a mixture of YSZ and NiO2 is used as the hydrogen electrode.
[0077] The fuel cell 150 further includes a first interconnector 112 having a fuel flow path 114, and a second interconnector 122 having an oxidant flow path 124. The fuel flow path 114 is a flow path for supplying a fuel (e.g., hydrogen) to the hydrogen electrode 108. The fuel flow path 114 is provided on a main surface of the first interconnector 112, which faces the hydrogen electrode current collector 110. The oxidant flow path 124 is a flow path for supplying an oxidant (e.g., oxygen) to the air electrode 102. The oxidant flow path 124 is provided on a main surface of the second interconnector 122, which faces the air electrode current collector 120.
[0078] <Method for manufacturing porous body> The porous body according to the present embodiment can be produced by appropriately using a conventionally known method. Therefore, the method for producing the porous body is not particularly limited, but is preferably the following method.
[0079] That is, it is preferable to manufacture a porous body by a method for manufacturing a porous body including a step (first step) of forming a conductive coating layer on a resin molded body having a three-dimensional mesh structure to obtain a conductive resin molded body, a step (second step) of plating a nickel-cobalt alloy on the conductive resin molded body to obtain a porous body precursor, and a step (third step) of performing a heat treatment on the porous body precursor to burn and remove the resin component in the conductive resin molded body to obtain a porous body. Here, in this embodiment, the "nickel-cobalt alloy" means an alloy mainly composed of nickel and cobalt and may contain other elements (for example, an alloy mainly composed of nickel and cobalt and containing the first element and the second element).
[0080] <1st process> First, a sheet of a resin molded body having a three-dimensional mesh structure (hereinafter, simply referred to as "resin molded body") is prepared. As the resin molded body, a polyurethane resin, a melamine resin, or the like can be used. Furthermore, as a conductive treatment for imparting conductivity to the resin molded body, a conductive coating layer is formed on the surface of the resin molded body. As this conductive treatment, for example, the following methods can be mentioned. (1) A conductive paint containing conductive particles such as carbon or conductive ceramic and a binder is applied to the surface of a resin molded body by means of coating, impregnation, etc. (2) forming a layer of a conductive metal such as nickel or copper on the surface of a resin molded body by electroless plating; (3) Forming a layer of conductive metal on the surface of the resin molded body by vapor deposition or sputtering, thereby obtaining a conductive resin molded body.
[0081] <Second process> Next, the conductive resin molded body is plated with a nickel-cobalt alloy to obtain a porous body precursor. Although electroless plating can be used for the nickel-cobalt alloy plating, electroplating (so-called alloy electroplating) is preferred from the viewpoint of efficiency. In the nickel-cobalt alloy electroplating, the conductive resin molded body is used as a cathode.
[0082] A known plating bath can be used for electroplating nickel-cobalt alloys. For example, a Watts bath, a chloride bath, a sulfamic acid bath, etc. can be used. The following are examples of bath compositions for electroplating nickel-cobalt alloys.
[0083] (Bath composition) Salt (aqueous solution): Nickel sulfamate and cobalt sulfamate (total amount of Ni and Co is 350-450g / L) However, the mass ratio of Ni and Co is adjusted from Co / (Ni+Co)=0.2 to 0.8 depending on the desired mass ratio of Co to the total mass of Ni and Co. Salt containing the first element as a constituent element Salts containing secondary elements as constituent elements Boric acid: 30~40g / L pH: 4~4.5.
[0084] Examples of salts containing the above-mentioned first element as a constituent element include Na2B4O5(OH)4·8H2O, FeSO4·7H2O, and CaSO4·2H2O.
[0085] Examples of salts containing the above-mentioned second element as a constituent element include Na2SO4, Al2(SO4)3, Na2SiO3, MgSO4, CuSO4·5H2O, K2SO4, SnSO4, Cr2(SO4)3·nH2O, Ti(SO4)2, and ZnSO4·7H2O.
[0086] The electrolytic conditions for electrolytic plating of a nickel-cobalt alloy are, for example, as follows. (Electrolysis conditions) Temperature: 40~60℃ Current density: 0.5~10A / dm 2 Anode: Insoluble anode.
[0087] In this manner, a porous body precursor can be obtained in which a nickel-cobalt alloy is plated on a conductive resin molded body. In addition, when adding nonmetallic elements such as nitrogen, sulfur, fluorine, chlorine, and phosphorus, various additives can be added to the plating bath to include them in the porous body precursor. Examples of various additives include sodium nitrate, sodium sulfate, sodium fluoride, sodium chloride, and sodium phosphate, but are not necessarily limited to these, and any nonmetallic element may be included.
[0088] <3rd process> Next, the porous body precursor is subjected to a heat treatment to burn off the resin components in the conductive resin molded body and remove them to obtain a porous body. This makes it possible to obtain a porous body having a skeleton with a three-dimensional network structure. The temperature and atmosphere of the heat treatment for removing the resin components may be, for example, 600° C. or higher, and an oxidizing atmosphere such as air may be used.
[0089] The average pore diameter of the porous body obtained by the above method is almost equal to the average pore diameter of the resin molded body. Therefore, the average pore diameter of the resin molded body used to obtain the porous body may be appropriately selected depending on the application to which the porous body is applied. Since the porosity of the porous body is ultimately determined by the amount of metal (weight per unit area) to be plated, the weight per unit area of the nickel-cobalt alloy to be plated may be appropriately selected depending on the porosity required in the porous body, which is the final product. The porosity and average pore diameter of the resin molded body are defined in the same way as the porosity and average pore diameter of the skeleton described above, and can be calculated based on the above formula by replacing "skeleton" with "resin molded body".
[0090] The porous body according to the present embodiment can be manufactured through the above steps. The porous body has a skeleton having a three-dimensional network structure, and the main body of the skeleton contains nickel, cobalt, a first element, and a second element as constituent elements. Furthermore, the mass ratio of the cobalt is 0.2 to 0.8 with respect to the total mass of nickel and cobalt. The first element contains at least one element selected from the group consisting of boron, iron, and calcium, and the second element contains at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin, and the sum of the mass ratio of the first element and the mass ratio of the second element is 5 ppm to 50,000 ppm with respect to the main body of the skeleton. Thus, the porous body can have an appropriate strength as a current collector for an air electrode or a current collector for a fuel cell.
[0091] The above description includes the following additional features. (Appendix 1) A porous body having a skeleton with a three-dimensional network structure, the main body of the skeleton contains nickel, cobalt, a first element, and a second element as constituent elements; a mass ratio of the cobalt to the total mass of the nickel and the cobalt is 0.2 or more and 0.8 or less; The first element includes at least one element selected from the group consisting of boron, iron, and calcium, The second element includes at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin, A porous body, wherein the ratio of the total mass of the first element and the second element to the mass of the main body of the skeleton is 5 ppm or more and 50,000 ppm or less. (Appendix 2) 2. The porous body according to claim 1, wherein the mass ratio of the cobalt is 0.2 or more and 0.45 or less with respect to the total mass of the nickel and the cobalt. (Appendix 3) 2. The porous body according to claim 1, wherein the ratio of the total mass of the first element and the second element to the mass of the skeleton body is 55 ppm or more and 477 ppm or less. (Appendix 4) 2. The porous body according to claim 1, wherein a total mass percentage of the nickel and the cobalt in the main body of the skeleton is 80 mass % or more and less than 100 mass %. (Appendix 5) 2. The porous body according to claim 1, wherein the first element is boron, and the second element is at least one element selected from the group consisting of sodium, aluminum, zinc, and tin. (Appendix 6) 2. The porous body according to claim 1, wherein the first element is iron, and the second element is at least one element selected from the group consisting of magnesium, copper, potassium, and aluminum. (Appendix 7) 2. The porous body according to claim 1, wherein the first element is calcium, and the second element is at least one element selected from the group consisting of sodium, tin, chromium, titanium, and silicon. (Appendix 8) 2. The porous body according to claim 1, wherein the first element is boron and calcium, and the second element is sodium, aluminum, and silicon. (Appendix 9) 2. The porous body according to claim 1, wherein the first element is boron and iron, and the second element is magnesium and tin. (Appendix 10) 2. The porous body according to claim 1, wherein the first elements are boron, iron and calcium, and the second elements are sodium, aluminum, silicon and tin. EXAMPLES
[0092] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.
[0093] <Preparation of porous bodies> <Sample 1 to Sample 12> The porous bodies of Samples 1 to 12 were prepared according to the following procedure. (1st step) First, a 1.5 mm thick polyurethane resin sheet was prepared as a resin molded body having a three-dimensional network structure. The porosity and average pore diameter of this polyurethane resin sheet were calculated based on the above-mentioned formula, and the porosity was 96% and the average pore diameter was 450 μm.
[0094] Next, the resin molded body was impregnated with a conductive paint (slurry containing carbon black), and then squeezed with a roll and dried to form a conductive coating layer on the surface of the resin molded body, thereby obtaining a conductive resin molded body.
[0095] (2nd process) The conductive resin molded body was used as the cathode and electrolytic plating was carried out under the following bath composition and electrolytic conditions. As a result, 660 g / m of nickel-cobalt alloy was deposited on the conductive resin molded body. 2 Thus, a porous body precursor was obtained.
[0096] <Bath composition> Salt (aqueous solution): an aqueous solution of nickel sulfamate and cobalt sulfamate. The total amount of Ni and Co was 400 g / L. The mass ratio of Co / (Ni+Co) was set to 0.22, 0.58, or 0.78. Na2B4O5(OH)4·8H2O was added to the plating bath so that boron, as the first element, was contained in the porous body at the mass ratio shown in Table 1. Na2SO4, Al2(SO4)3, ZnSO4·7H2O or SnSO4 was added to the plating bath so that sodium, aluminum, zinc or tin was contained in the porous body as the secondary element in the mass ratio shown in Table 1. Boric acid: 35g / L pH: 4.5.
[0097] <Electrolysis conditions> Temperature: 50℃ Current density: 5A / dm 2 Anode: Insoluble anode.
[0098] (3rd step) The porous body precursor was subjected to a heat treatment to burn off and remove the resin component in the conductive resin molded body, thereby obtaining the porous bodies of Samples 1 to 12. At this time, the temperature of the heat treatment for removing the resin component was 650° C., and the atmosphere during the heat treatment was the air atmosphere.
[0099] <Sample 13 to Sample 24> In the second step, FeSO4·7H2O was added to the plating bath so that iron as the first element was contained in the porous body in the mass ratio shown in Table 1, and MgSO4, CuSO4·5H2O, K2SO4 or Al2(SO4)3 was added to the plating bath so that magnesium, copper, potassium or aluminum as the second element was contained in the porous body in the mass ratio shown in Table 1. The porous bodies of Samples 13 to 24 were produced in the same manner as <Samples 1 to 12>, except that
[0100] <Sample 25 to Sample 36> In the second step, CaSO4·2H2O was added to the plating bath so that calcium was contained in the porous body as the first element in the mass ratio shown in Table 2, and Na2SO4, SnSO4, Cr2(SO4)3·nH2O or Ti(SO4)2 was added to the plating bath so that sodium, tin, chromium or titanium was contained in the porous body as the second element in the mass ratio shown in Table 2. The porous bodies of Samples 25 to 36 were produced in the same manner as <Samples 1 to 12>, except that
[0101] <Sample 37 to Sample 39> In the second step, CaSO4·2H2O was added to the plating bath so that calcium, as the first element, was contained in the porous body in the mass ratio shown in Table 2, and Na2SiO3 was added to the plating bath so that silicon and sodium, as the second elements, were contained in the porous body in the mass ratio shown in Table 2. The porous bodies of Samples 37 to 39 were produced in the same manner as <Samples 1 to 12>, except that
[0102] <Sample 40 to Sample 42> In the second step, Na2B4O5(OH)4·8H2O and CaSO4·2H2O were added to the plating bath so that boron and calcium were contained in the porous body as the first elements in the mass ratios shown in Table 3, and Al2(SO4)3 and Na2SiO3 were added to the plating bath so that aluminum, silicon and sodium were contained in the porous body as the second elements in the mass ratios shown in Table 3. The porous bodies of Samples 40 to 42 were produced in the same manner as <Samples 1 to 12>, except that
[0103] <Sample 43 to Sample 45> In the second step, Na2B4O5(OH)4·8H2O and FeSO4·7H2O were added to the plating bath so that boron and iron as the first elements were contained in the porous body in the mass ratios shown in Table 3, and MgSO4 and SnSO4 were added to the plating bath so that magnesium and tin as the second elements were contained in the porous body in the mass ratios shown in Table 3. The porous bodies of Samples 43 to 45 were produced in the same manner as <Samples 1 to 12>, except that in the second step, Na2B4O5(OH)4·8H2O and FeSO4·7H2O were added to the plating bath so that boron and iron as the first elements were contained in the porous body in the mass ratios shown in Table 3.
[0104] <Sample 46 to Sample 48> In the second step, Na2B4O5(OH)4·8H2O, FeSO4·7H2O and CaSO4·2H2O were added to the plating bath so that the first elements of boron, iron and calcium were contained in the porous body in the mass ratios shown in Table 3, and Al2(SO4)3, Na2SiO3 and SnSO4 were added to the plating bath so that the second elements of aluminum, silicon, tin and sodium were contained in the porous body in the mass ratios shown in Table 3. The porous bodies of Samples 46 to 48 were produced in the same manner as <Samples 1 to 12>, except that
[0105] <Sample 101 to Sample 103> In the second step, the porous bodies of Samples 101 to 103 were prepared in the same manner as in <Samples 1 to 12>, except that salts corresponding to the first element and the second element were not added to the plating bath (Table 4). In Table 4 and Table 5 described later, the places indicated with "-" in the columns for "First element" and "Second element" indicate that the corresponding element was not contained in the porous body.
[0106] <Sample 104 to Sample 112> The porous bodies of Samples 104 to 112 were prepared in the same manner as <Samples 1 to 12>, except that in the second step, no salt corresponding to the first element was added to the plating bath, and SnSO4, Na2SO4 or Cr2(SO4)3·nH2O was added to the plating bath so that tin, sodium or chromium was contained in the porous body in the mass ratio shown in Table 4 as the second element.
[0107] <Sample 113 to Sample 121> In the second step, Na2B4O5(OH)4·8H2O, FeSO4·7H2O or CaSO4·2H2O was added to the plating bath so that boron, iron or calcium was contained in the porous body as the first element in the mass ratio shown in Table 5, and no salt corresponding to the second element was added to the plating bath (Table 5).The porous bodies of Samples 113 to 121 were produced in the same manner as Samples 1 to 12, except that.
[0108] <Sample 122 to Sample 130> In the second step, Na2B4O5(OH)4·8H2O, FeSO4·7H2O or CaSO4·2H2O was added to the plating bath so that the first element, boron, iron or calcium, was contained in the porous body in the mass ratio shown in Table 5, and Al2(SO4)3 was added to the plating bath so that the second element, aluminum, was contained in the porous body in the mass ratio shown in Table 5. The porous bodies of Samples 122 to 130 were produced in the same manner as <Samples 1 to 12>, except that.
[0109] By the above procedure, porous bodies of Samples 1 to 48 and Samples 101 to 130 were obtained. Here, Samples 1 to 48 correspond to Examples, and Samples 101 to 130 correspond to Comparative Examples.
[0110] <Performance evaluation of porous bodies> <Analysis of physical properties of porous materials> The mass ratio of cobalt to the total mass of nickel and cobalt in the skeleton body of the porous bodies of Samples 1 to 48 and Samples 101 to 130 obtained by the above-mentioned method was examined using an EDX device (SEM part: product name "SUPRA35VP", manufactured by Carl Zeiss Microscopy Co., Ltd., EDX part: product name "octane super", manufactured by Ametech Co., Ltd.) attached to the SEM. Specifically, the porous body of each sample was first cut. Next, the cross section of the skeleton of the cut porous body was observed by the EDX device, and the mass ratio of the cobalt was calculated based on the atomic concentration of each element detected. As a result, the mass ratio of cobalt to the total mass of nickel and cobalt in the skeleton body of the porous bodies of Samples 1 to 48 and Samples 101 to 130 all matched the mass ratio of cobalt to the total mass of nickel and cobalt (mass ratio of Co / (Ni+Co)) contained in the plating bath used to prepare them.
[0111] Furthermore, the average pore size and porosity of the skeleton of the porous bodies of Samples 1 to 48 and Samples 101 to 130 were calculated according to the above-mentioned formula. As a result, the porosity and average pore size were consistent with those of the resin molded body, the porosity was 96%, and the average pore size was 450 μm. Furthermore, the porous bodies of Samples 1 to 48 and Samples 101 to 130 had a thickness of 1.4 mm. The total basis weight of nickel and cobalt in the porous bodies of Samples 1 to 48 and Samples 101 to 130 was 660 g / m, as described above. 2 It was.
[0112] <Power generation evaluation> Furthermore, the porous bodies of Samples 1 to 48 and the porous bodies of Samples 101 to 130 were used as air electrode current collectors to fabricate fuel cells (FIG. 8) together with a YSZ cell (FIG. 9) manufactured by Elcogen. Power generation was evaluated based on the following evaluation items.
[0113] (Evaluation of cracks in solid electrolyte) The cracking of the solid electrolyte was evaluated by the following procedure. That is, the YSZ cell after the fuel cell was operated for 2000 hours was visually inspected to check for the presence or absence of cracks. The results are shown in Tables 1 to 5.
[0114] (Evaluation of the operating voltage maintenance rate after 2000 hours of power generation) For the produced fuel cells, the initial operating voltage V1 and the operating voltage V2 after 2000 hours were determined, and the operating voltage retention rate after 2000 hours was calculated using the following formula, and the results are shown in Tables 1 to 5 below. In Table 5, "-" indicates that the operating voltage retention rate could not be measured. Each operating voltage V1 and V2 was measured three times and the results were averaged to determine the result. Operating voltage maintenance rate after 2000 hours of power generation (%) = (V2 / V1) x 100
[0115] [Table 1]
[0116] [Table 2]
[0117] [Table 3]
[0118] [Table 4]
[0119] [Table 5]
[0120] <Consideration> According to the results of Tables 1 to 3, when the main body of the skeleton contains nickel, cobalt, a first element, and a second element, and the sum of the mass ratio of the first element and the mass ratio of the second element is 5 ppm or more and 50,000 ppm or less with respect to the main body of the skeleton, it was found that no cracks were observed in the solid electrolyte contained in the fuel cell. Furthermore, it was found that the operating voltage retention rate of the fuel cell after 2000 hours of power generation exceeds 90%, which is good. In particular, when the mass ratio of the cobalt is 0.22 with respect to the total mass of the nickel and the cobalt, it was found that the operating voltage retention rate after 2000 hours of power generation is particularly good compared to when the mass ratio of the cobalt is 0.58 or 0.78. From the above, it was found that the porous bodies according to the examples have an appropriate strength for use as air electrode current collectors and hydrogen electrode current collectors in fuel cells.
[0121] According to the results of Tables 4 and 5, when the main body of the skeleton contains nickel and cobalt but does not contain the first element, the second element, or both of them, no cracks were observed in the solid electrolyte contained in the fuel cell. However, in these fuel cells, the operating voltage retention rate after 2000 hours of power generation was 62% or less. (Samples 101 to 121). In the fuel cells of Samples 101 to 121, the strength of the air electrode current collector (porous body) is relatively weak, and it is considered that the contact between the air electrode current collector and the fuel cell or the interconnector became weak after 2000 hours of power generation. As a result, it is considered that the contact resistance increased and the operating voltage retention rate decreased. Also, according to the results of Table 5, when the main body of the skeleton contains nickel, cobalt, the first element, and the second element, but the total of the mass ratio of the first element and the mass ratio of the second element exceeds 50,000 ppm with respect to the main body of the skeleton, cracks were observed in the solid electrolyte contained in the fuel cell (Samples 122 to 130). As described above, in the fuel cells of Samples 122 to 130, cracks were present in the solid electrolyte, and therefore the operating voltage retention rate 2000 hours after power generation could not be measured.
[0122] Although the embodiments and examples of the present invention have been described above, it is also intended from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined.
[0123] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered as limiting. The scope of the present invention is indicated by the claims, not by the embodiments and examples described above, and is intended to include the meaning equivalent to the claims and all modifications within the scope. [Explanation of symbols]
[0124] 1 support portion, 2 node portion, 10 frame portion, 11 skeleton body, 12 skeleton, 13 interior, 14 pore portion, 20 cell portion, 30 three-dimensional mesh structure, 100 fuel cell cell, 102 air electrode, 104 intermediate layer, 106 electrolyte layer, 108 hydrogen electrode, 110 hydrogen electrode current collector, 112 first interconnector, 114 fuel flow path, 120 air electrode current collector, 122 second interconnector, 124 oxidant flow path, 150 fuel cell, A imaginary plane
Claims
1. A porous body having a skeleton with a three-dimensional network structure, the main body of the skeleton contains nickel, cobalt, a first element, and a second element as constituent elements; a mass ratio of the cobalt to a total mass of the nickel and the cobalt is 0.2 or more and 0.8 or less; the first element is at least one element selected from the group consisting of boron, iron, and calcium; the second element is at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, titanium, chromium, copper, zinc, and tin; a ratio of the total mass of the first element and the second element to the mass of the main body of the skeleton is 5 ppm or more and 50,000 ppm or less; A porous material used as a current collector in fuel cells.
2. The porous body according to claim 1 , wherein a mass ratio of the cobalt to a total mass of the nickel and the cobalt is 0.2 or more and 0.45 or less, or 0.6 or more and 0.8 or less.
3. 3. The porous body according to claim 1, wherein a mass ratio of the first element is 4 ppm or more and 40,000 ppm or less with respect to a mass of the main body of the skeleton.
4. 4. The porous body according to claim 1, wherein a mass ratio of the second element is 1 ppm or more and 10,000 ppm or less with respect to a mass of the main body of the skeleton.
5. The porous body according to claim 1 , wherein the main body of the skeleton further contains oxygen as a constituent element.
6. The porous body according to claim 5 , wherein the oxygen content in the main body of the skeleton is 0.1% by mass or more and 35% by mass or less.
7. 7. The porous body according to claim 5, wherein the main body of the skeleton contains a spinel-type oxide.
8. 8. The porous body according to claim 1, wherein when a cross-section of the main body of the skeleton is observed at a magnification of 3000 times, the number of voids having a major axis of 1 μm or more that appear in any 10 μm square region of the observed image is 5 or less.
9. The porous body according to claim 1 , wherein the skeleton is hollow.
10. The porous body according to claim 1 , which has a sheet-like appearance and a thickness of 0.2 mm or more and 2 mm or less.
11. A fuel cell comprising an air electrode current collector and a hydrogen electrode current collector, A fuel cell, wherein at least one of the air electrode current collector and the hydrogen electrode current collector comprises the porous body according to claim 1 .
Citation Information
Patent Citations
Metallic porous body for secondary battery and its manufacture
JP1999154517A
Metallic porous body having high corrosion resistance, and method for manufacturing therefor
JP2012132083A
Porous metal having high corrosion resistance, and process for producing the same
JP2012149282A
Membrane-electrode assembly, manufacturing method of membrane-electrode assembly, fuel cell and manufacturing method of fuel cell
JP2016015217A
Air electrode current collector for solid oxide fuel cells and solid oxide fuel cells containing the same
JP2017507452A