Conductive resin composition, master batch, molded body, and methods for producing the same
A conductive resin composition formed by binding carbon nanotubes with glass fibers in a crosslinked structure addresses the challenge of achieving high electromagnetic shielding and conductivity without compromising mechanical properties, resulting in molded articles with enhanced performance across high-frequency bands.
Patent Information
- Application Number
- JP2024508719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-08
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2043-08-31
AI Technical Summary
Existing high-frequency electromagnetic shielding materials, such as those using magnetic metals or carbon black, face challenges in achieving effective shielding without compromising mechanical properties, and carbon nanotubes are difficult to disperse in resin materials for optimal performance.
A conductive resin composition is developed by binding carbon nanotubes with glass fibers using a binder resin to form a crosslinked structure, which is then blended with thermoplastic resin, allowing for high electromagnetic shielding and conductivity without reducing mechanical properties.
The resulting molded articles exhibit excellent electromagnetic shielding and conductivity across high-frequency bands, including the millimeter wave range, while maintaining or improving mechanical strength and impact resistance.
Smart Images

Figure 0007568165000006 
Figure 0007568165000007 
Figure 0007568165000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive resin composition, a masterbatch, a molded article, and methods for producing the same. [Background technology]
[0002] As 5G communication technology and millimeter wave radar become more widespread, noise suppression at high frequencies is being considered. Molding materials are sometimes used for high frequency shielding materials for electrical equipment cases and sheets. However, it is difficult for magnetic metal compounds such as ferrite to provide electromagnetic shielding at high frequencies, and carbon black compounds require high concentrations of additives to provide electromagnetic shielding, which causes problems such as reduced mechanical properties such as impact resistance. Therefore, although there was a demand for the use of carbon nanotubes that can exhibit high electromagnetic shielding properties without compromising mechanical properties, there was a problem in that they were difficult to disperse when kneaded with resin materials, making it difficult to achieve the expected electromagnetic shielding properties. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-108524 A Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, the problem that the present invention aims to solve is to provide a molded article having high electromagnetic shielding properties or electrical conductivity without impairing mechanical properties, a conductive resin composition and a masterbatch that provide the molded article, and methods for producing the same. [Means for solving the problem]
[0005] The conductive resin composition, master batch, molded article, and methods for producing the same according to the present invention are as follows [1] to [9].
[0006] [1] A thermoplastic resin and a carbon nanostructure are melt-kneaded as essential raw materials, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, 1. A conductive resin composition comprising a carbon nanostructure in an amount of 0.1 to 30 parts by mass per 100 parts by mass of a thermoplastic resin.
[0007] [2] The conductive resin composition according to [1], wherein the carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin to form a crosslinked structure.
[0008] [3] A masterbatch comprising: The conductive resin composition according to [1] or [2], wherein the carbon nanostructure is 1 to 30 parts by mass per 100 parts by mass of the thermoplastic resin.
[0009] [4] The conductive resin composition according to any one of [1] to [3], wherein the thermoplastic resin includes at least one selected from the group consisting of polyamide-based resins, polyethylene-based resins, polypropylene-based resins, and polyphenylene-based resins.
[0010] [5] A molded article obtained by molding the conductive resin composition according to any one of [1] to [4].
[0011] [6] The molded article according to [5], which is a conductive material or an electromagnetic wave shielding material.
[0012] [7] A process for melt-kneading a thermoplastic resin and a carbon nanostructure, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, 1. A method for producing a conductive resin composition, comprising the steps of: per 100 parts by mass of a thermoplastic resin; and wherein the carbon nanostructure is 0.1 to 30 parts by mass.
[0013] [8] A step of melt-kneading a thermoplastic resin and a carbon nanostructure in a ratio of 0.1 to 30 parts by mass of the carbon nanostructure per 100 parts by mass of the thermoplastic resin to produce a master batch; The method for producing a conductive resin composition further comprises a step of melt-kneading the obtained masterbatch with a thermoplastic resin.
[0014] [9] A method for producing a molded product, comprising a step of melt-molding a conductive resin composition containing a thermoplastic resin and a carbon nanostructure, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, 1. A method for producing a molded article, comprising the steps of: mixing 0.1 to 30 parts by mass of a carbon nanostructure with respect to 100 parts by mass of a thermoplastic resin; Effect of the Invention
[0015] According to the present invention, it is possible to provide a molded article having high electromagnetic shielding properties or electrical conductivity without impairing mechanical properties, a conductive resin composition and a masterbatch which provide the molded article, and methods for producing the same. [Brief description of the drawings]
[0016] [Figure 1] 1 is a Raman spectrum diagram (excitation wavelength 633 nm) of the fillers used in Examples 1 to 6. [Diagram 2] 1 is a Raman spectrum (excitation wavelength 785 nm) of the fillers used in Examples 1 to 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, in this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0018] The conductive resin composition of the present invention is obtained by melt-kneading a thermoplastic resin and a carbon nanostructure as essential raw materials, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, The composition is characterized in that the carbon nanostructure is contained in an amount of 0.1 to 30 parts by mass per 100 parts by mass of the thermoplastic resin.
[0019] thermoplastic resin The thermoplastic resin used in the present invention is not particularly limited, and can be appropriately selected from known resins in consideration of the type of carbon nanostructure to be blended, the product quality required when a molded body is formed, and the like. The thermoplastic resin used in the present invention may be one type only, or two or more types may be mixed. When two or more types are mixed, it is preferable to use a combination of resins with high compatibility. Furthermore, the thermoplastic resin may be a commercially available product or a synthetic product.
[0020] Specific examples of the thermoplastic resin used in the present invention include polyolefin resins such as polyethylene, polypropylene, poly(4-methyl-1-pentene), and poly(1-butene); polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamide resins such as polyamide-6 (nylon-6), polyamide 66 (nylon-66), and polymetaxylene adipamide; ethylene-unsaturated ester copolymers such as ethylene-vinyl ester copolymers and ethylene-unsaturated carboxylic acid ester copolymers; and ethylene-unsaturated carboxylic acid copolymers or ionomer resins thereof. ; poly(meth)acrylic resins such as poly(meth)acrylic acid ester resins; chlorine-based resins such as polyvinyl chloride and polyvinylidene chloride; fluorine-based resins such as polytetrafluoroethylene, ethylene tetrafluoroethylene copolymer, polyvinylidene fluoride, and polyvinyl fluoride; polystyrene resins; polyether-based resins such as polyether ether ketone resins and polyether ketone resins; polycarbonate resins; polyphenylene-based resins such as polyarylene sulfide resins represented by polyphenylene oxide resins and polyphenylene sulfide resins; polyvinyl acetate resins; polyacrylonitrile resins; thermoplastic elastomers, etc. Among these, polyolefin-based resins, polyester-based resins, polyamide-based resins, and polyolefin-based resins are preferred. In addition, one type selected from these thermoplastic resins may be used alone, or two or more types may be used in combination.
[0021] The polyolefin resin is a polyolefin resin obtained by polymerizing at least one kind of olefin, and may be a homopolymer or a copolymer. Examples of such olefins include α-olefins having 4 to 12 carbon atoms, including ethylene, propylene, isobutylene, and isobutene (1-butene), butadiene, isoprene, (meth)acrylic acid esters, (meth)acrylic acid, (meth)acrylamide, vinyl alcohol, vinyl acetate, vinyl chloride, styrene, and acrylonitrile.
[0022] Examples of the α-olefins having 4 to 12 carbon atoms include 1-butene, 2-methyl-1-propene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-ethyl-1-butene, 2,3-dimethyl-1-butene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3,3-dimethyl-1-butene, 1-heptene, methyl-1-hexene, and dimethyl 1-pentene, ethyl-1-pentene, trimethyl-1-butene, methylethyl-1-butene, 1-octene, methyl-1-pentene, ethyl-1-hexene, dimethyl-1-hexene, propyl-1-heptene, methylethyl-1-heptene, trimethyl-1-pentene, propyl-1-pentene, diethyl-1-butene, 1-nonene, 1-decene, 1-undecene, and 1-dodecene.
[0023] Examples of polyolefin resins include polyethylene resins, polypropylene resins, polyisobutylene resins, polyisobutene resins, polyisoprene resins, and polybutadiene resins. Among these resins, polyethylene resins and polypropylene resins are preferred. When classified by density or shape, high density polyethylene (HDPE), low density polyethylene (LDPE), very low density polyethylene (VLDPE), linear low density polyethylene (LLDPE), and ultra-high molecular weight polyethylene (UHMW-PE) are included, and among these, high density polyethylene is preferred.
[0024] Carbon Nanostructures The carbon nanostructure used in the present invention is formed by binding carbon nanotubes and glass fibers with a binder resin. The carbon nanostructure is preferably formed by binding carbon nanotubes and glass fibers with a binder resin to have a network structure. The carbon nanostructure is preferably formed by binding carbon nanotubes and glass fibers with a binder resin to form a branched structure, a mutually interpenetrating structure, a mutually entangled structure, or a cross-linked structure, and the structure may be a dendrimer shape. The respective proportions of the carbon nanotubes, the glass fibers, and the binder resin are preferably such that the proportion of the carbon nanotubes is 70 to 98 mass%, the proportion of the glass fibers is 1 to 15 mass%, and the proportion of the binder resin is 1 to 15 mass%, based on the total of the carbon nanotubes, the glass fibers, and the binder resin.
[0025] As the carbon nanotubes, single-walled carbon nanotubes (SWCNTs) having an average diameter of 5 to 100 nanometers (nm) or multi-walled carbon nanotubes (MWCNTs) in which the single carbon nanotubes are linked together in multiple layers (two or more layers) can be used.
[0026] Glass fibers include silicon dioxide (SiO 2 The glass composition may be prepared by melting a glass composition component mainly composed of the above-mentioned glass powder, cooling it, and then forming it into a fine powder. For example, glass powder such as glass powder (for example, glass powder represented by CAS65997-17-3 or a standard product for quasi-drug raw materials) can be mentioned.
[0027] The carbon nanostructure used in the present invention is preferably a composite containing carbon nanotubes (CNTs) having a G / D ratio of 0.5 to 1.0 at an excitation wavelength of 633 nm and / or a G / D ratio of 0.1 to 0.5 at 785 nm as measured by Raman spectroscopy, and glass powder. Note that "G" and "D" respectively refer to the peaks at approximately 1586 cm when excited at the excitation wavelength in Raman spectroscopy. -1 Near, 1367cm -1This is the height of the peak that appears near
[0028] The binder resin may be any known one that is used as a sizing agent for carbon fibers or glass fibers. Specific examples include, but are not limited to, fluorinated polymers such as poly(vinyldifluoroethylene) (PVDF), poly(vinyldifluoroethylene-co-hexafluoropropylene) (PVDF-HFP), and poly(tetrafluoroethylene) (PTFE), polyimides, and water-soluble resins such as poly(ethylene) oxide, polyvinyl-alcohol (PVA), cellulose, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, and polyvinylpyrrolidone (PVP), as well as copolymers and mixtures thereof; polyurethane (PU), thermoplastic polyurethane (TPU), polyethylene glycol (PEG), epoxy resin, polyester resin, vinyl ether, and the like. Examples of the resins that can be used include ster resins, polyetherimide resins, polyetherketoneketone resins, polyphthalamide resins, polyetherketone resins, polyetheretherketone resins, polyimide resins, phenol-formaldehyde resins, bismaleimide resins, acrylonitrile-butadiene styrene (ABS) resins, polycarbonate resins, polyethyleneimine resins, polyvinyl chloride resins, polystyrene resins, polyolefin resins, polypropylene resins, polyethylene resins, polytetrafluoroethylene resins, elastomeric resins such as polyisoprene, polybutadiene, butyl rubber, nitrile rubber, ethylene-vinyl acetate polymers, silicone polymers, and fluorosilicone polymers, and combinations thereof.
[0029] As such carbon nanostructures, commercially available products can be used, for example, "ATHLOS(TM)100 Carbon Nanostructure Pellets" (Cabot Corporation).
[0030] The ratio of the thermoplastic resin to the carbon nanostructure is preferably 0.1 to 30 parts by mass, and more preferably 1 to 15 parts by mass, of the carbon nanostructure relative to 100 parts by mass of the thermoplastic resin.
[0031] In addition to the above essential components, the conductive resin composition of the present invention can contain known additives as other components. Specific examples include antioxidants, ultraviolet absorbers, colorants, pigments, dyes, foaming agents, lubricants, flame retardants, fillers, etc. (referred to as additives in the present invention). When other components are used as optional components, the blending ratio is within a range that does not impair the effects of the present invention, and the desired function can be freely adjusted by adjusting the type and amount of these components. For example, the thermoplastic resin can be used in a range of 10 parts by mass or less, further 5 parts by mass or less, and further 1 part by mass or less, relative to 100 parts by mass of the thermoplastic resin.
[0032] The method for producing a conductive resin composition according to the present invention includes a step of melt-kneading a thermoplastic resin and a carbon nanostructure as essential raw materials. The kneaded product obtained by this step can be directly melt-molded into a molded product, or it can be first shaped into a powder, granule, pellet, chip, or other particulate material, and then melt-molded into a molded product.
[0033] The process of melt-kneading the thermoplastic resin and the carbon nanostructure as essential raw materials involves first blending at least the thermoplastic resin and the carbon nanostructure as essential blending components in the above-mentioned ratio, further blending known additives as necessary, and then mixing uniformly using a tumbler or Henschel mixer (registered trademark) as necessary, and then feeding the mixture into a melt-kneading extruder such as a twin-screw kneading extruder to melt-knead the mixture in a temperature range from the melting temperature of the thermoplastic resin to the temperature plus 100°C, for example, in a temperature range of 180°C to 300°C. This allows the thermoplastic resin to be a continuous phase, and a morphology in which the carbon nanostructure or its crushed material is dispersed can be formed. The melting temperature of the thermoplastic resin refers to the melting point for crystalline resins and the softening point (glass transition point) for amorphous resins (hereinafter the same).
[0034] When the kneaded material is first made into particles, for example, the kneaded material can be extruded into a strand shape and then left at room temperature or cooled by immersing in water at a temperature range of 5° C. to 60° C., and then cut into particles in the form of pellets, chips, etc. Thereafter, the obtained particles can be freeze-pulverized as necessary to obtain powder or granules having a desired size.
[0035] The conductive resin composition of the present invention is preferably produced via a masterbatch.
[0036] The masterbatch of the present invention is prepared by melt-kneading a thermoplastic resin and a carbon nanostructure as essential raw materials, and is characterized in that the amount of the carbon nanostructure is 1 to 30 parts by mass per 100 parts by mass of the thermoplastic resin.
[0037] The thermoplastic resin and the carbon nanostructures are the same as those described above, and the method for producing the masterbatch is also the same as that described above, except that the blending ratio of the carbon nanostructures to the thermoplastic resin is different.
[0038] When the conductive resin composition of the present invention is produced via a masterbatch, the method for producing the conductive resin composition of the present invention further includes a step of melting and mixing or kneading the obtained masterbatch and a thermoplastic resin as a diluent resin.
[0039] The thermoplastic resin used as the diluting resin can be exemplified by the same ones as those mentioned above, but it is also possible to use a resin of a different type from the thermoplastic resin used in producing the master batch, or to use the same type of resin.
[0040] The blending ratio of the dilution resin to the master batch can be adjusted so that the carbon nanostructure is ultimately 1 to 30 parts by mass per 100 parts by mass of the thermoplastic resin in the conductive resin composition. By producing a conductive resin composition via a master batch in this manner and then producing a molded body, it is possible to more uniformly disperse carbon nanostructures or their crushed materials in the molded body, and as a result, it is possible to fully impart the desired functions and characteristics to the molded body.
[0041] Molded body By molding the conductive resin composition according to the present invention, a molded article having excellent electrical conductivity and electromagnetic shielding properties can be obtained. That is, according to another aspect of the present invention, there is provided a molded article obtained from the conductive resin composition according to the present invention.
[0042] The molding method for the molded body is not particularly limited, and examples thereof include a pouring method such as casting, injection molding using a mold, compression molding, and melt molding methods such as extrusion molding using a T-die or the like, and blow molding.
[0043] In the production of the molded article, the molded article may be formed only from the resin composition according to the present invention, or the resin composition according to the present invention and other resin compositions may be used as raw materials. For example, the entire molded article may be molded from the resin composition according to the present invention, or only a part of the molded article may be molded from the resin composition according to the present invention.
[0044] The molded article obtained by molding the conductive resin composition of the present invention by melt molding or the like has a morphology in which carbon nanostructures or crushed pieces thereof are dispersed in the thermoplastic resin that constitutes a continuous phase, and therefore has excellent electrical conductivity and electromagnetic shielding properties. 8 ~10 -1 The molded article of the present invention can also have a conductivity of Ω / □. Furthermore, the molded article of the present invention has excellent electromagnetic wave shielding properties, and even when the carbon nanostructure is contained in a ratio of 0.1 to 1.0 part by mass per 100 parts by mass of thermoplastic resin, the molded article of the present invention has electromagnetic wave shielding properties up to the so-called millimeter wave band (100 MHz to 90 GHz band).
[0045] For this reason, the molded article of the present invention is particularly suitable for use as housings for office automation equipment and housings for electrical and electronic equipment. Examples of devices to which the molded article can be applied include notebook computers, electronic organizers, mobile phones, PDAs, and the like. One application that can best utilize the electromagnetic wave shielding properties that are a feature of the present invention is the housing of a notebook computer. EXAMPLES
[0046] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following examples, the notations "%" and "parts" are used, but they represent "% by mass" and "parts by mass" unless otherwise specified.
[0047] [Examples 1 and 2, Comparative Examples 1 and 2] The filler and polymer were melt-kneaded in the compositions and ratios shown in the table using a twin-screw extruder TEM-26SX (Shibaura Machine Co., Ltd.) (cylinder temperature 220°C (PP) or 260°C (PBT), screw rotation speed 300 rpm, extrusion rate 10 kg / hr) to obtain resin compositions. The obtained resin compositions were evaluated as follows. The results are shown in Table 1.
[0048] (conductivity) The obtained resin composition was dried in a gear oven at 80°C for the PP-based product and 120°C for the PBT-based product for 5 hours, and then the sample was placed on a mold and preheated at 240°C for the PP-based product and 280°C for the PBT-based product for 5 minutes at a pressure of 2MPa in a heating press, and pressed for 2 minutes at a pressure of 20MPa. Then, the sample was cooled to room temperature and the test piece was removed to produce a flat plate with a thickness of 2mm x 150mm x 150mm. The center of the plate was then cut into a 60mm x 60mm square to create a test piece. The surface resistivity of this test piece was measured using an ultra-high resistance meter R8340A manufactured by Advantest Corporation in accordance with JISK6723.
[0049] (Electromagnetic wave shielding) The 150mm square plate obtained above was measured in the frequency range of 0.1MHz to 1GHz by the KEC method, and in two frequency ranges of 26.5-40GHz and 60-90GHz by the free space method. In the free space method, a vector network analyzer was used to measure the S parameters (S21, S11) with two pairs of lens antennas arranged horizontally, and the shielding and absorption characteristics were calculated as follows, with the power standard. S21 = (electromagnetic field strength of transmitted wave / electromagnetic field strength of incident wave) S11 = (electromagnetic field strength of reflected wave / electromagnetic field strength of incident wave) Shielding characteristics (dB)=10×log 10 (S21 2 ) Reflectance (%)=100×S11 2 Transmittance (%)=100×S21 2 Absorption rate (%) = 100 - reflectance rate - transmittance rate
[0050] (Mechanical properties) The resulting resin compositions were dried for 5 hours in a gear oven at 80°C for the PP-based product and 120°C for the PBT-based product, and then injection-molded into JIS K7139 multipurpose test pieces A-type at a cylinder temperature of 230°C for the PP and 270°C for the PBT in an injection molding machine, and then cut to prepare type 1 notch type A test pieces as specified in JIS K7111. Charpy impact strength was measured at a measurement temperature of 23°C using a method in accordance with JIS K7111.
[0051] [Table 1]
[0052] The raw materials used in the table are as follows: "Athlos100" - Carbon nanostructure "ATHLOS(TM)100 Carbon Nanostructure Pellets" (Cabot Corporation). Raman spectra are shown in Figures 1 and 2. The Raman spectra were measured using the following method.
[0053] "NC7000" Multi-walled carbon nanotubes (manufactured by Nanosil)
[0054] "PP" Polypropylene resin (random polypropylene with MFR of 5 to 10 g / 10 min at 230°C and 2.16 kg) "PBT" Polybutylene terephthalate (MFR is 60-80g / 10min at 240℃ and 2.16kg) The MFR was measured by placing the sample in a melt indexer (orifice diameter 2.1 mm), applying the above load, and preheating for 5 minutes, after which the melt flow rate was measured.
[0055] Comparing Example 1 with Comparative Example 1, it was found that Example 1 has a lower surface resistivity, excellent electrical conductivity, and also has a superior electromagnetic shielding performance at 1 GHz to 70 GHz, while maintaining or improving impact resistance, compared to Comparative Example 1. Also, comparing Example 2 with Comparative Example 2, it was found that Example 2 has a lower surface resistivity, excellent electrical conductivity, and also has a superior electromagnetic shielding performance at 1 GHz to 70 GHz, while maintaining or improving impact resistance, compared to Comparative Example 2.
[0056] [Examples 3 and 4, Comparative Examples 3 and 4] The filler and polymer were melt-kneaded in the compositions and ratios shown in the table using a twin-screw extruder TEM-26SX (Shibaura Machine Co., Ltd.) (cylinder temperature 220°C (PP) or 260°C (PBT), screw rotation speed 300 rpm, extrusion rate 10 kg / hr) to obtain resin compositions. The obtained resin compositions were evaluated as described above. The results are shown in Tables 2 and 3.
[0057] [Examples 5 and 6, Comparative Examples 5 and 6] The resin compositions obtained in Example 1 and Comparative Example 1 were used as masterbatches, and the polymers were blended and diluted so that the final filler ratio in the masterbatches was the ratio shown in Tables 2 and 3. The mixture was melt-kneaded in a twin-screw extruder TEM-26SX (manufactured by Shibaura Machine Co., Ltd.) (cylinder temperature 220°C (PP) or 260°C (PBT), screw rotation speed 300 rpm, discharge rate 10 kg / hr) to obtain resin compositions. The obtained resin compositions were evaluated as described above. The results are shown in Tables 2 and 3.
[0058] [Table 2]
[0059] [Table 3]
[0060] Comparing Example 3 with Comparative Example 3, it was found that Example 3 maintained or improved impact resistance, had a low surface resistivity and excellent conductivity, and was excellent in electromagnetic wave shielding performance and electromagnetic wave absorbing performance at 1 GHz to 70 GHz, compared to Comparative Example 3. Comparing Example 4 with Comparative Example 4, it was found that Example 4 maintained or improved impact resistance, had a low surface resistivity and excellent conductivity, and was excellent in electromagnetic wave shielding performance and electromagnetic wave absorbing performance at 1 GHz to 70 GHz, compared to Comparative Example 4. Comparing Example 5 with Comparative Example 5, it was found that Example 5 maintained or improved impact resistance, had a low surface resistivity and excellent conductivity, and was excellent in electromagnetic wave shielding performance and electromagnetic wave absorbing performance at 1 GHz to 70 GHz, compared to Comparative Example 5. Comparing Example 6 with Comparative Example 6, it was found that Example 6 maintained or improved impact resistance, had a low surface resistivity and excellent conductivity, and was excellent in electromagnetic wave shielding performance and electromagnetic wave absorbing performance at 1 GHz to 70 GHz, compared to Comparative Example 6.
[0061] In addition, it was revealed from the results of Examples 3 and 4 and Examples 5 and 6 that similar performance was exhibited whether directly compounded or diluted with a master batch. In addition, although the electromagnetic wave shielding performance of Examples 3 to 6 was lower than that of Example 1, the electromagnetic wave absorbing performance was improved, and it was revealed that they are particularly suitable for applications requiring reduction in reflected noise.
[0062] (Raman spectrum measurements and results) A sample (Athlos100) was collected on a slide glass and subjected to Raman analysis (n=5). Raman device: NRS5500 (JASCO) Excitation wavelength 633nm, 785nm Gratings: 600 Exposure time: 100 seconds Number of times: 2 Crystalline Si(520cm -1 ) wavenumber correction was performed. G(1586cm -1 ) and D(1367cm -1 ) peak height was determined and the G / D ratio was calculated (Table 4).
[0063] [Table 4]
[0064] [Examples 7 to 9] The filler and polymer were melt-kneaded in the compositions and ratios shown in the table using a twin-screw extruder TEX-25αIII (manufactured by The Japan Steel Works, Ltd.) (cylinder temperature 300°C, screw rotation speed 200 rpm, discharge rate 15 kg / hr) to obtain a resin composition. The obtained resin composition was evaluated as follows. The results are shown in Table 5.
[0065] (conductivity) The obtained resin composition was dried in a gear oven at 140° C. for 2 hours, and then a test piece of 100 mm×100 mm×2 mm was produced using an injection molding machine at a cylinder temperature of 320 to 330° C. The surface resistivity of this test piece was measured in the same manner as above.
[0066] (Electromagnetic wave shielding) The electromagnetic shielding properties of the 100 mm square plate obtained above were measured and calculated in the same manner as above.
[0067] (Mechanical properties) Test pieces of 10 mm x 80 mm were cut in the material flow direction from the 100 mm square plate obtained above, and the Charpy impact strength was measured at a measurement temperature of 23°C using a method in accordance with JIS K7111.
[0068] [Table 5]
[0069] The raw materials used in the table are as follows:
[0070] "PPS" Polyphenylene sulfide resin (melt viscosity is 310℃, shear rate is 1000sec ―1 10-20 Pa·s
[0071] It was revealed that in Examples 7 to 9, while impact resistance was maintained or improved, the surface resistivity was reduced, resulting in excellent electrical conductivity, and the electromagnetic wave shielding performance, absorption performance, and mechanical strength at 1 GHz to 70 GHz were also excellent.
Claims
1. The thermoplastic resin and the carbon nanostructure are melted and kneaded as essential raw materials, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, A conductive resin composition for use as an electromagnetic shielding material, comprising 0.1 to 30 parts by mass of a carbon nanostructure relative to 100 parts by mass of a thermoplastic resin.
2. 2. The conductive resin composition for use as an electromagnetic shielding material according to claim 1, wherein the carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin to form a crosslinked structure.
3. A masterbatch comprising:
2. The conductive resin composition for electromagnetic shielding material according to claim 1, wherein the carbon nanostructure is 1 to 30 parts by mass per 100 parts by mass of the thermoplastic resin.
4. 2. The conductive resin composition for use as an electromagnetic shielding material according to claim 1, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyamide-based resins, polyolefin-based resins, polyester-based resins, and polyphenylene-based resins.
5. 2. A molded article which is an electromagnetic wave shielding material, obtained by molding the conductive resin composition for an electromagnetic wave shielding material according to claim 1.
6. The molded body of claim 5 which is a sheet or plate.
7. The method includes a step of melt-kneading a thermoplastic resin and a carbon nanostructure, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, A method for producing a conductive resin composition for use as an electromagnetic shielding material, characterized in that the carbon nanostructure is 0.1 to 30 parts by mass per 100 parts by mass of a thermoplastic resin.
8. A step of melt-kneading a thermoplastic resin and a carbon nanostructure in a ratio of 1 to 30 parts by mass of the carbon nanostructure per 100 parts by mass of the thermoplastic resin to produce a master batch; Further, the method includes a step of melt-kneading the obtained masterbatch with a thermoplastic resin. The method for producing a conductive resin composition for use as an electromagnetic shielding material, wherein the carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin.
9. A method for producing a molded product, comprising a step of melt-molding a conductive resin composition for an electromagnetic shielding material, the conductive resin composition comprising a thermoplastic resin and a carbon nanostructure, the method comprising the steps of: The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, A method for producing a molded article which is an electromagnetic wave shielding material, characterized in that the carbon nanostructure is 0.1 to 30 parts by mass per 100 parts by mass of a thermoplastic resin.
10. A method for absorbing and / or shielding electromagnetic waves using a molded body, comprising: The molded body, The thermoplastic resin and the carbon nanostructure are melted and kneaded as essential raw materials, The carbon nanostructure is formed by binding carbon nanotubes and glass fibers with a binder resin, The method comprises molding a conductive resin composition, the carbon nanostructure being present in an amount of 0.1 to 30 parts by mass per 100 parts by mass of a thermoplastic resin.
11. The method according to claim 10, wherein the electromagnetic waves are in the 100 MHz to 90 GHz band.
Citation Information
Patent Citations
Polyphenylene ether-based resin composition, and molded product
JP2012057082A
CNT leached fibers in thermoplastic matrix
JP2013513020A
Conductive resin composition, conductive master batch, molded body, and production method of the same
JP2016108524A
Composite materials with improved mechanical properties and molded articles containing them