Manufacturing method for {100} textured electrical steel sheet

The method of hot-rolling steel with specific compositions and controlled heat treatments addresses productivity and cost issues in producing {100} textured electrical steel sheets, achieving stable magnetic properties and cost-effective industrial production.

JP7568414B2Active Publication Date: 2024-10-16JFE STEEL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020057812
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-27
Publication Date
2024-10-16
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Existing methods for producing {100} textured electrical steel sheets face challenges in industrial productivity and cost due to the need for vacuum atmospheres and complex processes, making them impractical for continuous production.

Method used

A method involving hot-rolling steel with specific compositions and controlled heat treatments, including multiple cycles of heating and cooling, to achieve abnormal grain growth and stabilize the {100} texture without requiring vacuum, enabling low-cost production.

Benefits of technology

Stable production of {100} textured electrical steel sheets with excellent magnetic properties is achieved, suitable for rotating equipment and transformers, through controlled heat treatments and abnormal grain growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568414000004
    Figure 0007568414000004
  • Figure 0007568414000005
    Figure 0007568414000005
  • Figure 0007568414000006
    Figure 0007568414000006
Patent Text Reader

Abstract

To provide a manufacturing method of electrical steel sheet with {100}texture by which excellent magnetic properties can be obtained inexpensively and stably.SOLUTION: According to the manufacturing method of electrical steel sheet with {100}texture in the present invention, a steel material containing Si of 2.0 to 5.0 mass% and Ni of 0.5 to 10.0 mass% is hot-rolled and then cold-rolled once or cold-rolled twice or more with intermediate annealing in between to obtain a cold-rolled sheet with a final thickness, the cold-rolled sheet is heated from a room temperature to a high temperature range of A4 transformation point or higher so as to form a bcc single phase structure and is held for a predetermined time, and is subsequently cooled to a low temperature range between A3 transformation point and A4 transformation point so that the bcc single phase changes to a (bcc+fcc) phase and is held for a predetermined time at the temperature range, then cooling and reheating is repeated more than once, in which the steel is heated to the high temperature range of A4 transformation point or higher so as to form a bcc single phase structure again and is held for a predetermined time, and further the steel is cooled to the room temperature from the high temperature range of A4 transformation point or higher so as to be a bcc single phase structure. A volume fraction of the fcc phase in the low temperature range is controlled in a range of 30 to 80% during the series of heat treatments are performed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing electrical steel sheet with a {100} texture that has excellent magnetic properties within the rolled surface and is suitable for use in electric motors, generators, transformers, etc. [Background technology]

[0002] Conventionally, magnetic steel sheets have been used as magnetic core materials for electric motors, generators, transformers, etc. Magnetic steel sheets are required to have two magnetic properties: low magnetic energy loss in an AC magnetic field, and high magnetic flux density in a practical magnetic field. To achieve these, it is necessary to increase the resistivity of the steel and to optimize the bcc lattice, which is the direction of easy magnetization. <100> It is considered effective to align the axes in the direction of the magnetic field used.

[0003] If the {100} plane is parallel to the plate surface, <100> Since the axis is parallel to the sheet surface, it is suitable for use in rotating machines. Electrical steel sheets with this texture are called {100} textured electrical steel sheets. <100> The direction of the axis is arbitrary, but the direction of the axis is the rolling direction and the width direction of the plate. <100> Axes are accumulated {100} <001> Those with texture exhibit excellent magnetic properties in both directions, and are therefore called bi-directional electrical steel sheets. Such electrical steel sheets with texture are ideal not only for rotating machines, but also for applications in which magnetic flux flows in both the rolling direction and the sheet width direction, such as transformer cores that use stacked cores.

[0004] As a technique for producing such a {100} textured silicon steel sheet, for example, Patent Document 1 proposes a method utilizing cross cold rolling. Patent Document 2 discloses a production method utilizing high-temperature annealing that causes decarburization or decarburization and de-Mnization, specifically, a method for producing a silicon steel sheet having a texture in which the {100} plane is parallel to the sheet surface by tight coil annealing or stack annealing using a substance that promotes decarburization or a substance that promotes decarburization and de-Mnization as an annealing separator on a cold-rolled silicon steel sheet containing, by weight, 1% or less C, 0.2-6.5% Si, and 0.05-5% Mn. Non-Patent Document 1 discloses a method of annealing in a vacuum at a high temperature of 1050°C or higher for about 1 hour. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 01-139722 [Patent Document 2] Japanese Patent Application Publication No. 07-173542 [Non-patent literature]

[0006] [Non-Patent Document 1] Journal of the Japan Institute of Metals, Vol. 48 (1984), p482-488 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the technology using cross cold rolling disclosed in the above Patent Document 1, the second rolling direction is perpendicular to the first rolling direction, so it is impossible to continuously manufacture products in a coil shape like grain-oriented electrical steel sheets. In addition, in order to continuously manufacture, a process of shearing the first rolled sheet and joining it in some way is necessary, so it is difficult to put it into practical use. In addition, the method of high-temperature annealing disclosed in the above Patent Document 2 can manufacture {100} textured silicon steel sheets with excellent magnetic properties, but it requires long-term annealing in a vacuum to remove C and Mn. In addition, the method disclosed in the above Non-Patent Document 1 is a technology that utilizes the surface energy difference, so it requires a vacuum atmosphere and the sheet thickness to be about 0.10 mm or less. As described above, although the conventional technologies for manufacturing {100} textured silicon steel sheets are excellent technologies, there is room for further improvement in terms of industrial productivity and manufacturing costs before they can be put into practical use.

[0008] The present invention has been made in consideration of the above-mentioned problems associated with the conventional techniques, and has an object to provide a manufacturing method for {100} textured electrical steel sheet that does not require a vacuum atmosphere, is capable of industrial laminate annealing and coil annealing of steel sheets, and further, can be manufactured with short continuous annealing, and can stably obtain excellent magnetic properties. [Means for solving the problem]

[0009] In order to solve the above problems, the inventors have conducted extensive research focusing on the abnormal grain growth behavior of {100} textured electrical steel sheets due to repeated heat treatment. As a result, they have found that in order to stably manufacture {100} textured electrical steel sheets with excellent magnetic properties at low cost, it is effective to cause abnormal grain growth by repeatedly heating the sheet to a high temperature range above the A4 transformation point where the sheet becomes a bcc single phase, then cooling to a low temperature range between the A4 transformation point and the A3 transformation point where the sheet becomes a (bcc+fcc)2 phase, and then reheating to a high temperature range above the A4 transformation point where the sheet becomes a bcc single phase. Here, the abnormal grain growth is a phenomenon found in copper-based shape memory alloys, and the abnormal grain growth is caused by the driving force of subgrains generated by repeated transformations (see Science. 2013; 341(6153):1500-1502).

[0010] The present invention, developed based on the above findings, is a method for producing a steel material containing 2.0 to 5.0 mass% Si, 0.5 to 10.0 mass% Ni, and the balance being Fe and unavoidable impurities, by hot rolling and cold rolling once or by cold rolling two or more times with intermediate annealing therebetween to produce a cold-rolled sheet of a final thickness, and then heating the cold-rolled sheet from room temperature to a high temperature range equal to or higher than the A4 transformation point at which the bcc single phase is formed and holding the sheet for a predetermined time, followed by cooling to a low temperature range between the A3 transformation point and the A4 transformation point at which the bcc single phase is converted to a (bcc+fcc) phase and holding the sheet for a predetermined time, and then We propose a method for producing {100} textured electrical steel sheet by repeating this process, once or more, of heating again to a high temperature range above the A4 transformation point where the material becomes a bcc single phase, holding for a prescribed time, and then cooling again, and then performing a series of heat treatments in which the material is cooled from a high temperature range above the A4 transformation point where the material becomes a bcc single phase to room temperature, wherein the holding times in the high and low temperature ranges in the above heat treatments are set to 1 minute or more, and the volume fraction of the fcc phase in the low temperature range is controlled in the range of 30% or more and 80% or less.

[0011] The method for producing a {100} texture electrical steel sheet of the present invention is characterized in that the heating rate and cooling rate in the above heat treatment (excluding the cooling rate when cooling from a high temperature range to room temperature) are each in the range of 0.1 to 2000°C / min.

[0012] The method for producing a {100} texture electrical steel sheet of the present invention is also characterized in that the cooling rate when cooling from the high temperature range in the heat treatment to room temperature is 300° C. / min or more or 1° C. / min or less.

[0013] The steel material used in the method for producing a {100} texture electrical steel sheet of the present invention is characterized in that it contains, in addition to the above-mentioned Si and Ni, one or more elements selected from C: 0.01-0.10 mass%, Mn: 0.01-0.50 mass%, Sb: 0.01-0.10 mass%, Sn: 0.01-0.20 mass%, Cr: 0.01-0.50 mass%, Mo: 0.01-0.20 mass%, Cu: 0.01-0.50 mass%, Nb: 0.01-0.10 mass%, and P: 0.01-0.10 mass%. Effect of the Invention

[0014] According to the present invention, the magnetic material has excellent magnetic properties. <001> The present invention makes it possible to stably and inexpensively manufacture {100} textured electrical steel sheets having two axes within the sheet surface, and therefore provides a material suitable for use as an iron core material for rotating equipment and transformers. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a diagram illustrating a heat pattern of the heat treatment in Example 1. [Diagram 2] FIG. 13 is a diagram illustrating a heat pattern of the heat treatment in Example 2. [Diagram 3] FIG. 11 is a diagram illustrating a heat pattern of the heat treatment in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] First, the chemical composition of the steel material used in the production of the {100} textured electrical steel sheet of the present invention will be described. Si: 2.0~5.0mass% Silicon is an effective element for increasing the electrical resistance of steel and reducing iron loss, and in order to obtain a sufficient iron loss reduction effect, it is preferable to add 2.0 mass% or more. On the other hand, the addition of more than 5.0 mass% not only reduces the magnetic flux density, but also significantly impairs rollability, making manufacturing difficult. Therefore, the silicon content is set to the range of 2.0 to 5.0 mass%, and preferably to the range of 2.5 to 3.5 mass%.

[0017] Ni: 0.5 to 10.0 mass% Ni is an element necessary for causing γ transformation in steel and causing abnormal grain growth when cooling from a high temperature range to a low temperature range and reheating from a low temperature range to a high temperature range are repeated, as described below, and in order to ensure a sufficient amount of γ transformation, 0.5 mass% or more is contained. On the other hand, if Ni is contained at 10.0 mass% or more, the amount of γ transformation becomes too large, making it difficult for abnormal grain growth to occur. Therefore, Ni is set to the range of 0.5 to 10.0 mass%, and preferably to the range of 1.0 to 5.0 mass%.

[0018] The remaining components other than the above-mentioned Si and Ni in the steel material used in the present invention are Fe and unavoidable impurities, but C, Mn, Sb, Sn, Cr, Mo, Cu, Nb and P may be contained within the following ranges.

[0019] C: 0.01 to 0.10 mass% C is an element effective in improving the hot-rolled sheet structure, and is preferably contained in the range of 0.01 to 0.10 mass%, and more preferably in the range of 0.02 to 0.08 mass%. Note that, when C is contained, it is necessary to reduce the C content to 0.0050 mass% or less, at which point decarburization annealing is performed during the manufacturing process and magnetic aging does not occur.

[0020] Mn: 0.01 to 0.50 mass% Mn is an element effective in improving hot workability, and in order to obtain the above effect, it is preferable to add 0.01 mass% or more. On the other hand, adding more than 0.5 mass% leads to a decrease in magnetic flux density. Therefore, Mn is preferably in the range of 0.01 to 0.50 mass%, and more preferably in the range of 0.05 to 0.30 mass%.

[0021] One or more selected from the group consisting of Sb: 0.01-0.10 mass%, Sn: 0.01-0.20 mass%, Cr: 0.01-0.50 mass%, Mo: 0.01-0.20 mass%, Cu: 0.01-0.50 mass%, Nb: 0.01-0.10 mass%, and P: 0.01-0.10 mass%. Sb, Sn, Cr, Mo, Cu, Nb and P are surface segregation elements that have the effect of lowering the surface energy of the {100} plane and promoting the development of the {100} texture. However, if the content of each of the above components is less than the lower limit, the texture improvement effect is insufficient, while if the content exceeds the upper limit, the appearance of abnormal grain growth is inhibited, and the texture is deteriorated. Therefore, it is preferable to contain one or more of Sb, Sn, Cr, Mo, Cu, Nb and P within the above range. More preferable ranges are as follows: Sb: 0.02 to 0.06 mass%, Sn: 0.05 to 0.15 mass%, Cr: 0.05 to 0.30 mass%, Mo: 0.02 to 0.10 mass%, Cu: 0.05 to 0.30 mass%, Nb: 0.02 to 0.05 mass%, and P: 0.02 to 0.06 mass%, respectively.

[0022] Next, a method for producing the electrical steel sheet of the present invention will be described. The steel material (slab) used in the manufacturing method of the electrical steel sheet of the present invention is not limited other than that it satisfies the above-described chemical composition compatible with the present invention, and the manufacturing method may be a conventional method in which steel having a predetermined chemical composition is melted in a normal refining process, and then slabs are formed by a continuous casting method or an ingot making-blooming rolling method.

[0023] The steel material (slab) is heated to a predetermined temperature and then hot-rolled to a hot-rolled sheet of a predetermined thickness. In the case of grain-oriented electrical steel sheets in which secondary recrystallization is caused by the use of inhibitors, the slab heating temperature must be as high as nearly 1400°C in order to dissolve the inhibitor components. However, in the present invention, secondary recrystallization using inhibitors is not required, so the slab heating temperature may be any temperature at which hot rolling is possible. Therefore, after casting, direct rolling may be performed in which hot rolling is performed immediately without reheating. In the case of thin cast pieces, hot rolling may be omitted and the subsequent steps may be performed directly.

[0024] Next, the hot-rolled sheet obtained by the above hot rolling may be annealed in accordance with a conventional method as necessary. The steel sheet after hot rolling or hot-rolled sheet annealing is then pickled and cold-rolled once or two or more times with intermediate annealing therebetween to produce a cold-rolled sheet having a desired final thickness.

[0025] Next, the cold-rolled sheet having the final thickness is subjected to the most important heat treatment in the present invention. This heat treatment comprises step 1 of heating from room temperature to a high temperature range equal to or higher than the A4 transformation point where the bcc single phase is formed and holding the temperature there for a predetermined time, step 2 of cooling from the high temperature range to a low temperature range between the A3 transformation point where the bcc single phase is formed and the A4 transformation point where the bcc single phase is formed and holding the temperature there for a predetermined time, and then step 2 of heating again to a high temperature range equal to or higher than the A4 transformation point where the bcc single phase is formed and holding the temperature there for a predetermined time, repeating this cooling and reheating process at least once, and step 3 of cooling from the high temperature range equal to or higher than the A4 transformation point where the bcc single phase is formed to room temperature after step 2 is completed.

[0026] Here, in order to further enhance the effect of the present invention, in the above step 2, it is preferable to control the volume fraction of the fcc phase in the low temperature region between the A3 transformation point and the A4 transformation point where the bcc single phase becomes the (bcc+fcc) phase to a range of 30% to 80%. By controlling the volume fraction of the fcc phase to the above range, the {100} texture can be stably developed. On the other hand, when the volume fraction of the fcc phase is out of the above range, the amount of abnormal grain growth that occurs is insufficient, and the development of the {100} texture becomes insufficient. A more preferable volume fraction of the fcc phase is in the range of 50 to 70%.

[0027] The temperature of the high temperature region in step 2, in which the cooling and heating are repeated, is preferably 30°C higher than the A4 transformation point, thereby shortening the time required for abnormal grain growth to occur. More preferably, the temperature is 40°C higher than the A4 transformation point.

[0028] In addition, the holding time in step 1, in which the material is heated and held at a high temperature above the A4 transformation point where the bcc single phase is formed, is preferably 1 minute or more. If the holding time is less than 1 minute, the amount of abnormal grain growth is insufficient, and the development of the {100} texture becomes insufficient. There is no particular upper limit to the holding time, but from the viewpoints of productivity and manufacturing costs, it is preferably about 120 minutes. More preferably, it is in the range of 2 to 60 minutes.

[0029] In addition, the step 2, which is performed after the step 1, is performed by cooling to a low temperature range between the A3 transformation point and the A4 transformation point where the bcc single phase becomes the (bcc+fcc) phase, holding the temperature range for a predetermined time, and then heating to a high temperature range above the A4 transformation point where the bcc single phase becomes the (bcc+fcc) phase and holding the temperature range for a predetermined time, and repeating the cooling and heating at least once, and the holding time at the low temperature range and the high temperature range is preferably 1 min or more. If the holding time is less than 1 min, the amount of abnormal grain growth is insufficient, and the development of the {100} texture becomes insufficient. There is no particular upper limit to the holding time, but it is preferably about 120 min from the viewpoint of productivity and manufacturing costs. It is more preferably in the range of 2 to 60 min.

[0030] The cooling rate and heating rate in step 2 are preferably in the range of 0.1 to 2000°C / min. If the cooling rate and heating rate are less than 0.1°C / min, the annealing time becomes long, adversely affecting productivity and manufacturing costs. On the other hand, if they exceed 2000°C / min, the amount of abnormal grain growth is insufficient, and the development of the {100} texture becomes insufficient. More preferably, they are in the range of 0.5 to 1000°C / min.

[0031] In addition, the cooling rate in step 3, which follows step 2 and involves cooling from a high temperature range equal to or higher than the A4 transformation point where the bcc single phase is formed, to room temperature is preferably 300° C. / min or more for rapid cooling or 1° C. / min or less for slow cooling so that the non-magnetic fcc phase does not remain until room temperature, and more preferably 600° C. / min or more or 0.5° C. / min or less.

[0032] In addition, the atmosphere in step 2, in which cooling and heating are repeated, is preferably a non-oxidizing atmosphere such as Ar, H2, or N2, or a vacuum atmosphere. However, if the C content of the material is higher than 0.0050 mass%, a wet hydrogen atmosphere may be used initially to decarburize, and then the atmosphere may be changed to the non-oxidizing atmosphere or vacuum atmosphere.

[0033] Moreover, the number of repetitions of step 2, in which cooling and heating are repeated, must be at least one, and is preferably three or more in order to further promote abnormal grain growth. However, if the number of repetitions is increased unnecessarily, the above-mentioned effects will be saturated and there will be adverse effects on productivity and manufacturing costs, so the upper limit is preferably about five.

[0034] At present, it is not entirely clear why repeated cooling and heating that satisfies the above conditions results in abnormal grain growth and results in a steel sheet having a {100} texture. However, the inventors believe that this is because, when the sheet thickness is thin compared to the longitudinal and transverse dimensions of the steel sheet, the {100} crystal grains, which have the smallest Young's modulus in the sheet thickness direction, most effectively relax the strain that occurs with transformation.

[0035] Next, the {100} textured electrical steel sheet of the present invention will be described. The {100} textured electrical steel sheet obtained by the above-described manufacturing method of the present invention basically has a {100} texture. <001> It has a {100} texture of the {100} type or a {100}<0vw> type {100} texture. <100> Steel sheet with texture exhibits excellent magnetic properties in both the rolling direction and the sheet width direction, and steel sheet with {100}<0vw> texture exhibits nearly equal magnetic properties in all directions within the rolled plane.

[0036] In the steel sheet having the {100} texture according to the present invention, the area ratio of crystal grains having {100} planes at an angle of 15° or less to the sheet surface is preferably 70% or more, more preferably 80% or more, of the observation surface (cross section parallel to the sheet surface). The deviation angle from the {100} plane can be measured by the X-ray Laue method. EXAMPLES

[0037] A steel having a composition containing 3.0 mass% Si and 2.0 mass% Ni, with the balance being Fe and unavoidable impurities, was melted in a high-frequency melting furnace and cast into a steel ingot. The ingot was then heated to a temperature of 1200°C and hot-rolled into a hot-rolled sheet having a thickness of 2.4 mm. The hot-rolled sheet was then pickled and descaled, and cold-rolled into a cold-rolled sheet having a final thickness of 0.30 mm. The hot-rolled sheet was then subjected to a heat treatment in an Ar atmosphere according to the heat pattern shown in FIG. 1 and Table 1. The transformation temperatures of the above steels were determined by measuring the change in heat quantity when the steel plate was heated from a low temperature to a high temperature using a differential scanning calorimetry (DSC) measuring device. The A3 transformation point (bcc → bcc + fcc) was 960°C, and the A4 transformation point (bcc + fcc → bcc) was 1260°C. The volume fraction of the fcc phase when held in the low temperature range between the A4 transformation point and the A3 transformation point was determined by holding the material at the low temperature range for 2 minutes, then quenching and observing the structure. In addition, a 30 × 280 mm region of the heat-treated steel sheet was analyzed by the X-ray Laue method to measure the area ratio of crystal grains having {100} faces within 15° to the sheet surface.

[0038] The results of the above measurements are also shown in Table 1. It can be seen from this table that by performing heat treatment under conditions compatible with the present invention, it is possible to obtain an electrical steel sheet having a {100} texture in which the area ratio of crystal grains having {100} planes at 15° or less to the sheet surface is 70% or more of the sheet surface.

[0039] [Table 1] EXAMPLES

[0040] A steel having a composition containing 3.0 mass% Si and 2.0 mass% Ni, with the balance being Fe and unavoidable impurities, was melted in a high-frequency melting furnace and cast into a steel ingot. The ingot was then heated to a temperature of 1200°C and hot-rolled into a hot-rolled sheet having a thickness of 2.4 mm. The hot-rolled sheet was then pickled and descaled, and cold-rolled into a cold-rolled sheet having a final thickness of 0.30 mm. The hot-rolled sheet was then subjected to heat treatment in a mixed atmosphere of 25 vol% H and 75 vol% N, according to the heat pattern shown in FIG. 2 and Table 2. The transformation temperatures of the above steels were determined by measuring the change in heat quantity when the material was heated from a low temperature to a high temperature using a differential scanning calorimetry (DSC) measuring device. The A3 transformation point (bcc → bcc + fcc) was 960°C, and the A4 transformation point (bcc + fcc → bcc) was 1260°C. The volume fraction of the fcc phase when held in the low temperature range between the A4 transformation point and the A3 transformation point was determined by holding the material at the low temperature range for 2 minutes, then quenching and observing the structure. In addition, a 30 × 280 mm region of the heat-treated steel sheet was analyzed by the X-ray Laue method to measure the area ratio of crystal grains having {100} faces within 15° to the sheet surface.

[0041] The results of the above measurements are also shown in Table 2. It can be seen from this table that by performing heat treatment under conditions compatible with the present invention, it is possible to obtain an electrical steel sheet having a {100} texture in which the area ratio of crystal grains having {100} planes at 15° or less to the sheet surface is 70% or more of the sheet surface.

[0042] [Table 2] EXAMPLES

[0043] Steel having the chemical composition shown in Table 3, with the balance being Fe and unavoidable impurities, was melted in a high-frequency melting furnace and cast into a steel ingot. The ingot was then heated to a temperature of 1200°C and hot-rolled into a hot-rolled sheet having a thickness of 2.2 mm. The hot-rolled sheet was then pickled and descaled, and cold-rolled into a cold-rolled sheet having a final thickness of 0.22 mm. The cold-rolled sheet was then subjected to a heat treatment in an Ar atmosphere according to the heat pattern shown in FIG. 3 and Table 3. The transformation temperatures of the above steels are shown in Table 3. The volume fraction of the fcc phase when held in the low temperature range between the A4 transformation point and the A3 transformation point was determined by holding the material at the low temperature range for 2 minutes, then quenching and observing the structure. In addition, a 30 × 280 mm region of the heat-treated steel sheet was analyzed by the X-ray Laue method to measure the area ratio of crystal grains having {100} faces within 15° to the sheet surface.

[0044] The results of the above measurements are also shown in Table 3. It can be seen from this table that by performing heat treatment under conditions compatible with the present invention, it is possible to obtain an electrical steel sheet having a {100} texture in which the area ratio of crystal grains having {100} planes at 15° or less to the sheet surface is 70% or more of the sheet surface.

[0045] [Table 3] [Industrial Applicability]

[0046] The technology of the present invention is <100> The present invention can also be applied to the field of Fe-based shape memory alloys or superelastic materials, which have excellent directional properties.

Claims

1. A steel material containing 2.0 to 5.0 mass% Si, 1.0 to 5.0 mass% Ni, and the balance being Fe and unavoidable impurities, is hot-rolled, and cold-rolled once or two or more times with intermediate annealing to obtain a cold-rolled sheet of a final thickness. Then, the cold-rolled sheet is added with A, which becomes a bcc single phase from room temperature. 4 After heating to a high temperature range above the transformation point and holding it for a certain period of time, the bcc single phase changes to the (bcc + fcc) phase. 3 Transformation point and A 4 After cooling to a low temperature range between the transformation points and holding the temperature range for a predetermined time, the A phase becomes a bcc single phase again. 4 Heat to a high temperature range above the transformation point and hold for a specified time. Cool and reheat are repeated one or more times, and then the bcc single phase is formed. 4 A method for producing a {100} textured electrical steel sheet by carrying out a series of heat treatments from a high temperature range above the transformation point to room temperature, comprising the steps of: The holding time in the high temperature region and the low temperature region in the heat treatment is 1.0 min or more, The volume fraction of the fcc phase in the low temperature range is controlled to a range of 30% to 80%, When the steel material contains more than 0.0050 mass% C, the heat treatment includes decarburization annealing to reduce the C content to 0.0050 mass% or less.

2. The method for producing a {100} texture electrical steel sheet according to claim 1, characterized in that the heating rate and cooling rate in the heat treatment (excluding the cooling rate when cooling from a high temperature range to room temperature) are each in the range of 0.1 to 2000°C / min.

3. 3. The method for producing a {100} textured electrical steel sheet according to claim 1, wherein the cooling rate during cooling from the high temperature range in the heat treatment to room temperature is 300° C. / min or more or 1° C. / min or less.

4. The method for producing a {100} texture electrical steel sheet according to any one of claims 1 to 3, characterized in that the steel material contains, in addition to the Si and Ni, one or more selected from C: 0.01 to 0.10 mass%, Mn: 0.01 to 0.50 mass%, Sb: 0.01 to 0.10 mass%, Sn: 0.01 to 0.20 mass%, Cr: 0.01 to 0.50 mass%, Mo: 0.01 to 0.20 mass%, Cu: 0.01 to 0.50 mass%, Nb: 0.01 to 0.10 mass%, and P: 0.01 to 0.10 mass%.

Citation Information

Patent Citations

  • Manufacture of bidirectional oriented magnetic steel sheet

    JP1989139722A

  • Production of silicon steel sheet excellent in magnetic property

    JP1995173542A

  • Production of nonoriented silicon steel sheet excellent in magnetic property in entire peripheral direction

    JP1999001723A

  • Method for producing bi-directional magnetic steel sheet

    JP2004084034A

  • Method for forming a surface {100} in iron and iron-based alloys, method for manufacturing non-oriented electrical steel sheets using the same, and non-oriented electrical steel sheets manufactured using the same.

    JP2010513716A