Austenitic stainless steel strip or hot-rolled austenitic stainless steel sheet and method for producing austenitic stainless steel
Austenitic stainless steel with controlled C and N content and optimized hot rolling processes achieves high strength and surface quality, addressing manufacturing challenges and enabling applications in electronic devices.
Patent Information
- Application Number
- JP2020178303
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-23
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Existing methods for manufacturing austenitic stainless steel sheets are complex, costly, and struggle to achieve high strength and excellent surface properties, particularly in thicker forms, while also failing to address issues like intergranular cracking and surface defects during hot rolling.
Austenitic stainless steel with specific C and N content, combined with controlled hot rolling processes including a first pass rolling ratio of 30% or less, total rolling reduction of 60% or more, and cooling rates of 5°C/s or higher, along with controlled temperature ranges, to minimize intergranular cracking and achieve high hardness and surface quality.
The method produces austenitic stainless steel with high strength and excellent surface properties, minimizing intergranular cracking and surface defects, enabling applications in electronic device components without complex forging processes.
Smart Images

Figure 0007568473000001 
Figure 0007568473000002 
Figure 0007568473000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an austenitic stainless steel and a method for producing the same. [Background technology]
[0002] There is a high demand for small, lightweight, and stylish portable electronic devices, such as smartphones. Therefore, in the manufacture of metal exterior components for such portable electronic devices, a method of forming by cutting after cold forging under harsh conditions has come to be widely used in order to accommodate processing into complex shapes. Furthermore, depending on the design of the portable electronic device, mirror polishing may be performed after cutting. Here, the exterior components of portable electronic devices are not only required to be nonmagnetic to avoid adverse effects on geomagnetic sensors and the like built into the device, but also to have high strength. In addition, since the electronic devices are portable and often used in outdoor environments, the exterior components are also required to have higher corrosion resistance than electronic device components intended for indoor use.
[0003] As a metal material used in manufacturing the above-mentioned exterior member, for example, Patent Document 1 discloses a non-magnetic austenitic stainless steel plate (hereinafter simply referred to as "stainless steel plate") that is made into a non-magnetic member by cold forging and cutting.
[0004] Furthermore, high surface quality is required for stainless steel. Here, one surface defect resulting from hot rolling, which is one of the manufacturing processes for stainless steel, is a mountain-shaped crack called scab. Surface defects such as scab reduce the yield of stainless steel and lead to a significant increase in costs. As a method for improving such surface defects, for example, Patent Document 2 discloses a manufacturing method for stainless steel sheet in which the strain rate during hot rolling and the rolling reduction ratio per pass are specified. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2018-109215 [Patent Document 2] Japanese Patent Application Publication No. 8-103802 Summary of the Invention [Problem to be solved by the invention]
[0006] The stainless steel sheet manufacturing method described in Patent Document 1 is a method that can produce non-magnetic, high-strength parts, but it has problems in that the manufacturing process is complicated and costly, and it cannot be used for some product shapes.
[0007] It is also known that cold rolling (temper rolling) is generally used to increase the strength of austenitic stainless steel, but cold rolling tends to result in a thin plate, making it difficult to produce austenitic stainless steel with a certain or greater plate thickness using a manufacturing method that includes cold rolling.
[0008] In addition, although Patent Document 2 describes the conditions of the hot rolling process for improving surface defects, there is room for improvement in the conditions of the hot rolling process. For example, Patent Document 2 does not disclose specific conditions such as whether or not the surface of the cast piece is ground, and the rolling reduction rate of a specific pass in the process of rough hot rolling of about 1 to 7 passes.
[0009] An object of one aspect of the present invention is to realize an austenitic stainless steel or the like that has high strength and excellent surface properties despite having a certain degree of thickness or more. [Means for solving the problem]
[0010] In order to solve the above problems, an austenitic stainless steel according to one embodiment of the present invention has a combined C and N content of 0.08% or more by mass, an average hardness of a cross section parallel to the thickness direction of 250 HV or more, a thickness of 3 mm or more, and an average depth of scab defects caused by grain boundary cracking during hot rolling of 10 μm or less.
[0011] An austenitic stainless steel according to one embodiment of the present invention may contain, by mass%, C: 0.003% or more and 0.120% or less, Si: 2.0% or less, Mn: 2.0% or less, P: 0.04% or less, S: 0.03% or less, Ni: 6.0% or more and 15.0% or less, Cr: 16.0% or more and 22.0% or less, N: 0.005% or more and 0.200% or less, with the balance being Fe and unavoidable impurities.
[0012] An austenitic stainless steel according to one embodiment of the present invention may further contain, by mass%, one or more of the following: Mo: 0.01% or more and 3.00% or less, Cu: 0.01% or more and 3.50% or less, Al: 0.008% or less, O: 0.001% or more and 0.010% or less, V: 0.01% or more and 0.50% or less, B: 0.0003% or more and 0.0100% or less, and Ti: 0.01% or more and 0.50% or less.
[0013] An austenitic stainless steel according to one embodiment of the present invention may further contain, by mass%, one or more of the following: Co: 0.01% or more and 0.50% or less, Zr: 0.01% or more and 0.10% or less, Nb: 0.01% or more and 0.10% or less, Mg: 0.0005% or more and 0.0030% or less, Ca: 0.0003% or more and 0.0030% or less, Y: 0.01% or more and 0.20% or less, REM (rare earth metal): 0.01% or more and 0.10% or less, Sn: 0.001% or more and 0.500% or less, Sb: 0.001% or more and 0.500% or less, Pb: 0.01% or more and 0.10% or less, and W: 0.01% or more and 0.50% or less.
[0014] The austenitic stainless steel according to one aspect of the present invention may have a relative magnetic permeability μ of 1.1 or less.
[0015] In order to solve the above-mentioned problems, a method for producing an austenitic stainless steel according to one embodiment of the present invention comprises heating a slab produced by casting to a temperature of 1000° C. or more and 1300° C. or less, followed by rough hot rolling, the slab having a chemical composition containing, by mass%, C: 0.003% or more and 0.120% or less, Si: 2.0% or less, Mn: 2.0% or less, P: 0.04% or less, S: 0.03% or less, Ni: 6.0% or more and 15.0% or less, Cr: 16.0% or more and 22.0% or less, and N: 0.005% or more and 0.200% or less, with the combined content of C and N being 0.08% or more by mass, and the balance being Fe and unavoidable impurities. The method includes a rough hot rolling process in which the slab is subjected to a rough hot rolling process, a finish hot rolling process in which finish hot rolling is performed on the steel strip obtained by the rough hot rolling process, and a cooling process in which the steel strip after the finish hot rolling process is cooled, wherein in the rough hot rolling process, the slab is not surface-ground, and the rolling reduction rate of the first pass of the rough hot rolling is 30% or less, in the finish hot rolling process, the total rolling reduction rate of the finish hot rolling is 60% or more, the finish hot rolling temperature is 600°C or more and 1100°C or less, and the final pass temperature of the finish hot rolling is 950°C or less, and in the cooling process, the steel strip is cooled to 750°C or less at a cooling rate of 5°C / s or more when the final pass temperature of the finish hot rolling is 750°C or more.
[0016] In one embodiment of the method for producing an austenitic stainless steel according to the present invention, the slab may further contain, by mass%, one or more of the following: Mo: 0.01% or more and 3.00% or less, Cu: 0.01% or more and 3.50% or less, Al: 0.008% or less, O: 0.001% or more and 0.010% or less, V: 0.01% or more and 0.50% or less, B: 0.0003% or more and 0.0100% or less, and Ti: 0.01% or more and 0.50% or less.
[0017] In one embodiment of the method for producing an austenitic stainless steel according to the present invention, the slab may further contain, by mass%, one or more of the following: Co: 0.01% or more and 0.50% or less, Zr: 0.01% or more and 0.10% or less, Nb: 0.01% or more and 0.10% or less, Mg: 0.0005% or more and 0.0030% or less, Ca: 0.0003% or more and 0.0030% or less, Y: 0.01% or more and 0.20% or less, REM (rare earth metal): 0.01% or more and 0.10% or less, Sn: 0.001% or more and 0.500% or less, Sb: 0.001% or more and 0.500% or less, Pb: 0.01% or more and 0.10% or less, and W: 0.01% or more and 0.50% or less. Effect of the Invention
[0018] According to one aspect of the present invention, it is possible to realize austenitic stainless steel and the like that has high strength and excellent surface properties despite having a certain degree of thickness or more. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a process diagram showing the flow of each process in a method for producing an austenitic stainless steel according to one embodiment. [Diagram 2] FIG. 2 is a diagram showing chemical compositions of austenitic stainless steels according to examples and comparative examples. [Diagram 3] FIG. 2 is a diagram showing the physical properties of an austenitic stainless steel according to an embodiment of the present invention. [Figure 4] FIG. 4 is a diagram showing physical properties of an austenitic stainless steel according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] An embodiment of the present invention will be described in detail below. Note that the following description is for the purpose of better understanding the gist of the invention, and does not limit the present invention unless otherwise specified. In this specification, the concentration of each component is expressed in mass% unless otherwise specified.
[0021] [Points and Objects of the Invention] Key features of the present invention include the following (i) and (ii).
[0022] (i) Despite having a certain thickness (3 mm or more), the average hardness of the cross section parallel to the thickness direction is 250 HV or more, there are few scabs caused by intergranular cracking during hot rolling, and the austenitic stainless steel has excellent surface properties.
[0023] (ii) A slab produced by continuous casting is heated to a high temperature without surface grinding, and the rolling reduction ratio of the first pass of multiple passes of rough hot rolling is set to 30% or less. The total rolling reduction ratio of the subsequent finish hot rolling is set to 60% or more, the finish hot rolling temperature is set to 600°C or more and 1100°C or less, and the final pass temperature of the finish hot rolling is set to 950°C or less. If the final pass temperature of the finish hot rolling is 750°C or more, the steel strip after the finish hot rolling is cooled to 750°C or less at a cooling rate of 5°C / s or more. It has been discovered that the austenitic stainless steel shown in (i) above can be obtained by a manufacturing method including these steps.
[0024] Here, scab marks refer to mountain-shaped cracks that occur on the surface of austenitic stainless steel. In austenitic single-phase steel that does not contain δ-ferrite, it is believed that grain boundary cracks on the slab surface that occur in the early stage of hot rolling are the cause of scab marks. Such grain boundary cracks occur when deformation cannot follow the stress during hot rolling due to the segregation of S (sulfur), a typical impurity that deteriorates hot workability, at the grain boundaries and the fragile grain boundary strength when the grain size is large.
[0025] Up until now, for example, intergranular cracking has been improved by reducing the S content and forming a small amount of δ-ferrite with a large S solid solubility limit to suppress the segregation of S to the grain boundaries. In addition, the increase in grain boundary area due to the refinement of the crystal grain size dilutes the grain boundary segregation concentration of S and increases the grain boundary strength, which is effective in reducing the occurrence of intergranular cracking, i.e., scabs. In addition, recrystallization during hot rolling is known to be one of the factors that suppress intergranular cracking, since it not only increases the grain boundary strength due to the refinement of the crystal grains, but also eliminates the old grain boundaries where S was segregated, preventing the occurrence of intergranular cracking.
[0026] On the other hand, the fact that the production method shown in (ii) above can reduce the occurrence of scab defects in austenitic stainless steel is a novel finding obtained as a result of extensive investigations by the present inventors.
[0027] As a specific evaluation index of the surface quality of austenitic stainless steel, when the average depth of scabs caused by grain boundary cracking during hot rolling is 10 μm or less, it can be said that "the occurrence of scabs is low and the surface quality is excellent." Furthermore, it is more preferable if the average depth of the scabs is 5 μm or less.
[0028] The "average depth of scabs" may be, for example, the average value of a plurality of measurement results obtained by measuring the depth of each scab in a plurality of portions on the surface of the austenitic stainless steel where scabs occur. The depth of scabs may be measured, for example, by obtaining a cross section parallel to the thickness direction of the portion of the austenitic stainless steel where scabs occur, mirror-polishing the cross section, and then observing and measuring the surface layer with an optical microscope. In other words, the depth of scabs is the depth in the thickness direction of the austenitic stainless steel.
[0029] The advantages of an austenitic stainless steel having an average hardness of 250 HV or more in a cross section parallel to the thickness direction are as follows:
[0030] Structural members of electronic devices such as smartphones are generally manufactured by cold forging and cutting. Steel generally undergoes work hardening, which increases the strength of the steel as it is processed. However, the degree of processing in cold forging is not uniform and varies depending on the part, so soft parts may remain. If soft parts remain in the steel, the surface is easily scratched, and the value of the product is reduced. When the austenitic stainless steel according to one embodiment of the present invention is applied as the structural member, the average hardness of the cross section parallel to the thickness direction is 250HV or more, so that no soft parts remain and the quality of the product is stabilized.
[0031] In addition, the "austenitic stainless steel" described in this specification includes both an austenitic stainless steel strip and an austenitic stainless steel plate. In other words, the present invention is applicable to both an austenitic stainless steel strip and an austenitic stainless steel plate.
[0032] The present invention aims to provide an austenitic stainless steel having high strength and excellent surface properties, resulting in high yield and quality, and a method for producing the same. By using such an austenitic stainless steel, structural members of electronic devices such as smartphones can be produced by cutting, etching, electric discharge machining, etc., without complex forging.
[0033] [Method of manufacturing austenitic stainless steel] As shown in Fig. 1, an austenitic stainless steel according to one embodiment of the present invention can be manufactured by carrying out each process of steelmaking, rough hot rolling, finish hot rolling, and cooling. More specifically, first, molten steel is obtained using a general steelmaking method, and a slab is manufactured by casting (steelmaking process). The slab manufactured by casting has a chemical composition shown in [Chemical composition of austenitic stainless steel] described later. The slab is heated to 1000°C or more and 1300°C or less without surface grinding, and then rough hot rolling is performed to obtain a rough bar (steel strip) having a thickness of, for example, 35 mm (rough hot rolling process). In the rough hot rolling process, the rolling ratio of the first pass of rough hot rolling is set to 30% or less.
[0034] The rough bar is then finish hot rolled at 600°C or more and 1100°C or less (finish hot rolling process). In the finish hot rolling process, the total rolling reduction ratio of the finish hot rolling is 60% or more, and the final pass temperature of the finish hot rolling is 950°C or less. If the final pass temperature of the finish hot rolling is 750°C or more, the steel strip after the finish hot rolling process is cooled to 750°C or less at a cooling rate of 5°C / s or more (cooling process). By satisfying these conditions, it is possible to obtain an austenitic stainless steel that has excellent surface properties due to fewer scabs, and has the desired hardness in a cross section parallel to the thickness direction.
[0035] Furthermore, the obtained austenitic stainless steel may be subjected to pickling treatment as necessary in order to remove oxide scale formed in the hot rolling process. Generally, the pickling treatment is carried out in an annealing and pickling line in which the annealing process and the pickling process are connected. When carrying out the pickling treatment, heat may be applied to the austenitic stainless steel within a temperature range in which the hardness of the austenitic stainless steel does not decrease (specifically, 900°C or less).
[0036] Furthermore, the pickled austenitic stainless steel may be subjected to temper rolling, if necessary, for the purpose of adjusting the surface properties or strength. Generally, temper rolling is performed in a cold rolling process, and if the purpose is to adjust the surface properties, the total rolling reduction is performed so that the total rolling reduction is several percent or less, and if the purpose is to adjust the strength, the total rolling reduction is performed so that the total rolling reduction is several percent to about 50%. On the other hand, in the present invention, high strength is achieved by controlling the conditions during hot rolling. Therefore, when temper rolling is performed on the pickled austenitic stainless steel for the purpose of adjusting the strength, temper rolling may be performed within a range of total rolling reduction that does not excessively increase the strength (specifically, 30% or less).
[0037] According to the above-mentioned steps, it is possible to provide an austenitic stainless steel having high strength and excellent surface properties, in which the average hardness of a cross section parallel to the thickness direction is 250 HV or more, and the average depth of scab defects caused by intergranular cracking during hot rolling is 10 μm or less, despite the thickness being 3 mm or more.
[0038] The "average hardness of a cross section parallel to the thickness direction" refers to the average value of the results of measuring Vickers hardness at multiple points with a load of 1 kg so that the variation in hardness at each measurement position can be understood for the cross section parallel to the thickness direction. Vickers hardness can be measured, for example, by a method conforming to JIS Z2244.
[0039] (C+N) A certain amount of C (carbon) and N (nitrogen) is necessary because they are effective in solid solution strengthening and work hardening of the austenite phase. As a result of various investigations, in order to stably obtain a hardness of 250HV or more, the C+N amount is adjusted to 0.08% or more. The C+N amount refers to the combined content of C and N. In addition, the C+N amount may include cases where C is 0% or N is 0%.
[0040] (relative permeability) In characterizing austenitic stainless steel, the relative magnetic permeability μ is generally preferably 1.1 or less, and more preferably 1.05 or less.
[0041] In the austenitic stainless steel whose chemical composition has been adjusted as described above, no processing-induced martensite phase is generated in the normal steel plate manufacturing process and the subsequent cold forging process. Therefore, magnetization caused by processing-induced martensite phase can be avoided. However, when the slab is melted, a δ ferrite phase may be generated at high temperatures, and if the δ ferrite phase remains, non-magnetic properties with a relative permeability μ of 1.1 or less cannot be obtained. In addition, if the δ ferrite phase is mixed as a different phase in the austenitic stainless steel product, the appearance of the mirror-polished product may be impaired. Therefore, it is necessary that the δ ferrite phase disappears at the stage of the steel plate, which is the material to be subjected to cold forging. In this regard, in the manufacturing method according to one embodiment of the present invention, the remaining δ ferrite phase is prevented by performing finish rolling at 600 ° C or higher. Since the δ ferrite phase is ferromagnetic, its presence or absence can be evaluated by the relative permeability μ.
[0042] (Target characteristics) For austenitic stainless steel, the average hardness of the cross section parallel to the thickness direction was aimed for at 250HV or more (SUS304CSP-1 / 2H standard). The thickness was also aimed for at 3mm or more, since the thickness range of SUS301CSP from Tokushu Kinzoku Excel is about 2.5mm or less. In addition, the aim was to reduce the occurrence of scab defects caused by grain boundary cracking during hot rolling.
[0043] (Slab surface grinding) Slabs produced by casting are left as cast without surface grinding. During rough hot rolling, the crystal grains in the surface layer of the hot-rolled material are refined by recrystallization. The surface layer of the slab produced by casting is composed of crystal grains of 1 mm or less, called chill crystals, in an area of about 5 mm from the surface. The area directly below the chill crystals is composed of giant crystal grains, called columnar crystals, that are roughly cylindrical with a short diameter of 1 mm or more and a long diameter of 5 mm or more. The larger the crystal grains, the weaker the grain boundary strength, and tiny grain boundary cracks occur during hot rolling, causing scabs, which are surface defects caused by hot rolling. Therefore, it is preferable for the crystal grains in the extreme surface layer to be small in order to reduce the occurrence of scabs.
[0044] Therefore, by not grinding the surface of the slab, chill crystals having small crystal grains remain on the surface layer of the slab, and the occurrence of scab defects due to hot rolling can be reduced. Furthermore, if surface grinding is not required, the number of steps can be reduced, thereby improving productivity and yield.
[0045] (Rolling ratio of the first pass of rough hot rolling) During hot rolling, recrystallization occurs due to the application of strain to the hot-rolled material at high temperatures. The finer the grain size before hot rolling, the finer the grain size after recrystallization tends to be. In other words, from the viewpoint of grain refinement, it is preferable to perform hot rolling in a state in which the surface layer of the slab contains relatively fine chill crystals. In other words, by recrystallizing the surface layer of the slab during the first pass of rough hot rolling, the occurrence of scab defects due to grain boundary cracking caused by hot rolling can be effectively reduced.
[0046] The rolling ratio of the rough hot rolling in the rough hot rolling process is preferably 5% or more and 30% or less, more preferably 10% or more and 20% or less. In the rough hot rolling process, the crystal grains are refined by recrystallization in the surface layer of the hot rolled material. Here, if the rolling ratio of the first pass of the rough hot rolling is too large, there is a concern that grain boundary cracks will occur before the crystal grains are sufficiently refined. Therefore, the rolling ratio of the first pass of the rough hot rolling is preferably 30% or less, more preferably 20% or less. In addition, if the rolling ratio of the first pass of the rough hot rolling is too small, the number of hot rolling passes until the plate is rolled to a predetermined thickness increases, and the hot rolling resistance increases due to an excessive decrease in the hot rolling temperature, which leads to a decrease in hot rolling property, resulting in a decrease in productivity and an increase in production load. Therefore, it is desirable to set the rolling ratio of the first pass of the rough hot rolling to 5% or more.
[0047] (Total reduction ratio of finishing hot rolling) The total rolling ratio of the finish hot rolling is preferably 60% or more. If the total rolling ratio of the finish hot rolling is less than 60%, the rolling strain is not sufficiently imparted and the target hardness cannot be obtained. When the thickness of the steel strip before the finish hot rolling process is h1 and the thickness of the steel strip after the finish hot rolling process is h2, the relational expression Total rolling ratio = (h1-h2) / h1 is established.
[0048] (Finishing hot rolling temperature) The temperature of the finish hot rolling is preferably 600°C or more and 1100°C or less. In addition, the final pass temperature (final pass rolling temperature) of the finish hot rolling is preferably 950°C or less. If the temperature of the finish hot rolling and the final pass rolling temperature are lower than 600°C, the amount of rolling strain imparted to the surface layer of the steel strip becomes larger than that of the central part in the thickness direction, and there is a possibility that the strength is not sufficiently increased partially. On the other hand, if the temperature of the finish hot rolling exceeds 1100°C, the rolling strain becomes the driving force for recrystallization, and recrystallization occurs immediately after rolling, making it impossible to obtain the desired hardness, and the temperature is too high, making it difficult to adjust the final pass rolling temperature to 950°C or less. In addition, if the final pass rolling temperature exceeds 950°C, the rolling strain becomes the driving force for recrystallization, and recrystallization occurs immediately after rolling, making it impossible to obtain the desired hardness.
[0049] (cooling process) After the above-mentioned finish hot rolling step, it is preferable to include a cooling step in which the steel strip subjected to finish hot rolling is cooled to 750°C or less at a cooling rate of 5°C / s or more when the final pass temperature of the finish hot rolling is 750°C or more. The rolling strain accumulated in the hot rolled material by the finish hot rolling decreases immediately after the finish hot rolling if the material is kept at a high temperature. In order to retain a level of rolling strain preferable for increasing strength, it is preferable to quickly cool the steel strip after the finish hot rolling to a temperature range where no significant reduction in rolling strain occurs.
[0050] [Chemical composition of austenitic stainless steel] The chemical composition of an austenitic stainless steel according to one embodiment of the present invention preferably contains, in mass%, C: 0.003% or more and 0.120% or less, Si: 2.0% or less, Mn: 2.0% or less, P: 0.04% or less, S: 0.03% or less, Ni: 6.0% or more and 15.0% or less, Cr: 16.0% or more and 22.0% or less, N: 0.005% or more and 0.200% or less, with the balance being Fe and unavoidable impurities.
[0051] An austenitic stainless steel according to one embodiment of the present invention may further contain, in addition to the above chemical composition, one or more of the following, by mass%, Mo: 0.01% or more and 3.00% or less, Cu: 0.01% or more and 3.50% or less, Al: 0.008% or less, O: 0.001% or more and 0.010% or less, V: 0.01% or more and 0.50% or less, B: 0.0003% or more and 0.0100% or less, and Ti: 0.01% or more and 0.50% or less.
[0052] An austenitic stainless steel according to one embodiment of the present invention may further contain, in addition to the above chemical composition, one or more of the following, by mass%, Co: 0.01% or more and 0.50% or less, Zr: 0.01% or more and 0.10% or less, Nb: 0.01% or more and 0.10% or less, Mg: 0.0005% or more and 0.0030% or less, Ca: 0.0003% or more and 0.0030% or less, Y: 0.01% or more and 0.20% or less, REM (rare earth metals): 0.01% or more and 0.10% or less, Sn: 0.001% or more and 0.500% or less, Sb: 0.001% or more and 0.500% or less, Pb: 0.01% or more and 0.10% or less, and W: 0.01% or more and 0.50% or less.
[0053] Hereinafter, "%" in the chemical composition of the austenitic stainless steel means mass % unless otherwise specified.
[0054] C (carbon) is an interstitial element that contributes to high strength through work hardening and strain aging. C is also an austenite-forming element that stabilizes the austenite phase, and is effective in maintaining non-magnetic properties. It is preferable for austenitic stainless steel to have a C content of 0.003% or more. However, since excessive C content hardens austenitic stainless steel and reduces its cold forgeability, it is preferable to limit the C content to 0.12% or less.
[0055] Silicon (Si) is an element used as a deoxidizer for steel in the steelmaking process. In addition, silicon has the effect of improving age hardening in the stress relief heat treatment performed after cold forging. On the other hand, since silicon has a large solid solution strengthening effect and has the effect of reducing stacking fault energy and increasing work hardening, excessive silicon content is a factor that reduces cold forgeability. Therefore, it is preferable that the Si content is limited to 2.0% or less.
[0056] Mn (manganese) is an element that constitutes oxide-based inclusions in the form of MnO. Mn also has a small effect on solid solution strengthening, and is an austenite-forming element that inhibits processing-induced martensitic transformation, making it an effective element for ensuring cold forgeability and maintaining non-magnetic properties. However, excessive Mn content can cause a decrease in corrosion resistance. Therefore, it is preferable to limit the Mn content to 2.0% or less.
[0057] P (phosphorus) is an element that reduces corrosion resistance, and an excessive reduction in P content increases the steelmaking load, so the P content is preferably 0.04% or less.
[0058] S (sulfur) forms MnS, which deteriorates corrosion resistance, and excessive desulfurization increases the steelmaking load. Therefore, the S content is preferably limited to 0.03% or less.
[0059] Ni (nickel) is an element effective in improving corrosion resistance. It is preferable that austenitic stainless steel has a Ni content of 6.0% or more. However, excessive Ni content increases material costs. Therefore, it is preferable that the Ni content is limited to 15.0% or less.
[0060] Cr (chromium) is an element that improves corrosion resistance. In order to ensure corrosion resistance suitable for exterior members of portable electronic devices, it is preferable for austenitic stainless steel to have a Cr content of 16.0% or more. However, a large amount of Cr content can cause a decrease in cold forgeability. Therefore, it is preferable that the upper limit of the Cr content is limited to 22.0%.
[0061] Like C, N (nitrogen) is an interstitial element that contributes to high strength through work hardening and strain aging. N also stabilizes the austenite phase and is effective in maintaining non-magnetic properties. It is preferable for austenitic stainless steel to have an N content of 0.005% or more. However, excessive N content hardens austenitic stainless steel and reduces cold forgeability. Therefore, it is preferable to limit the N content to 0.20% or less.
[0062] Mo (molybdenum) is an element that is effective in improving the corrosion resistance of austenitic stainless steel. In austenitic stainless steel, Mo is added as necessary after ensuring the above-mentioned Cr content, but adding a large amount of Mo increases costs, so if Mo is added, the Mo content is set to 0.01% or more and 3.00% or less.
[0063] It is known that Cu (copper) suppresses the work hardening of the austenite phase and is effective in improving cold forgeability. It is also known that Cu is an element that brings about age hardening in the heating temperature range of the stress relief heat treatment performed after cold forging. As a result of various investigations, if Cu is contained, the Cu content is set to 0.01% or more and 3.50% or less.
[0064] Al (aluminum) has a higher oxygen affinity than Si and Mn, and if the Al content is 0.003% or more, coarse oxide-based inclusions that become the starting point of internal cracks during cold forging are likely to form. In addition, excessively low Al content increases costs, so after various investigations, if Al is contained, the Al content is set to 0.008% or less.
[0065] When the O (oxygen) content is low, Mn, Si, etc. are less likely to oxidize, and the ratio of Al2O3 in the inclusions increases. Also, when the O content is excessively high, coarse inclusions with particle sizes exceeding 5 μm are likely to form. As a result of various investigations, when O is contained, the O content is set to 10 ppm (0.001%) or more and 100 ppm (0.010%) or less, preferably 80 ppm (0.008%) or less.
[0066] V (vanadium) has the effect of increasing the age hardening ability during the heating for stress relief heat treatment performed after cold forging. Although V has an age hardening effect, the inclusion of a large amount of V leads to increased costs. If V is included, the V content should be 0.01% or more and 0.50% or less.
[0067] Regarding B (boron), a large amount of B can cause a decrease in workability due to the formation of borides, so when B is contained, the B content is set to 0.0003% or more and 0.0100% or less, preferably 0.0050% or less.
[0068] Titanium (Ti) is a carbonitride-forming element that fixes C and N and suppresses the decrease in corrosion resistance caused by sensitization. This effect is exhibited when the Ti content is 0.01% or more. Therefore, when Ti is contained, the Ti content is set to 0.01% or more. On the other hand, when the Ti content exceeds 0.50%, Ti precipitates as carbides with non-uniform sizes and localized non-uniformly in the steel, inhibiting regular recrystallized grain growth. In addition, since Ti is very expensive, the upper limit of the Ti content is set to 0.50%.
[0069] Co (cobalt) has the effect of improving crevice corrosion resistance. On the other hand, excessive Co content hardens the austenitic stainless steel and adversely affects the bendability. Therefore, when Co is contained, the Co content is set to 0.01% or more and 0.50% or less, preferably 0.10% or less.
[0070] Zr (zirconium) is an element with high affinity for C and N, and precipitates as carbides or nitrides during hot rolling, reducing the amount of dissolved C and N in the matrix and improving workability. On the other hand, excessive Zr content hardens austenitic stainless steel and adversely affects bendability. Therefore, when Zr is contained, the Zr content is set to 0.01% or more and 0.10% or less, preferably 0.05% or less.
[0071] Nb (niobium) is an element with high affinity for C and N, and precipitates as carbides or nitrides during hot rolling, reducing the amount of dissolved C and N in the matrix and improving workability. On the other hand, excessive Nb content hardens austenitic stainless steel and adversely affects bendability. Therefore, when Nb is contained, the Nb content is set to 0.01% or more and 0.10% or less, preferably 0.05% or less.
[0072] Magnesium (Mg) forms Mg oxide together with Al in molten steel and acts as a deoxidizer. On the other hand, excessive Mg content reduces the toughness of austenitic stainless steel and decreases manufacturability. Therefore, when Mg is contained, the Mg content is set to 0.0005% or more and 0.0030% or less, preferably 0.0020% or less.
[0073] Ca (calcium) is an element that improves hot workability. On the other hand, if an excessive amount of Ca is contained, the toughness of the austenitic stainless steel decreases, leading to a decrease in manufacturability, and furthermore, the corrosion resistance decreases due to the precipitation of CaS. Therefore, when Ca is contained, the Ca content is set to 0.0003% or more and 0.0030% or less, preferably 0.0020% or less.
[0074] Y (yttrium) is an element that reduces the viscosity decrease of molten steel and improves cleanliness. On the other hand, if Y is contained in excess, the effect is saturated and further, workability is reduced. Therefore, when Y is contained, the Y content is set to 0.01% or more and 0.20% or less, preferably 0.10% or less.
[0075] REM (rare earth metals: elements with atomic numbers 57 to 71, such as La, Ce, and Nd) are elements that improve high-temperature oxidation resistance. On the other hand, if REM is contained in excess, the effect is saturated, and furthermore, surface defects occur during hot rolling, reducing manufacturability. Therefore, when REM is contained, the REM content is set to 0.01% or more and 0.10% or less, preferably 0.05% or less.
[0076] Sn (tin) is effective in improving workability by promoting the formation of deformation bands during rolling. On the other hand, if excessive Sn is contained, the effect is saturated and workability is further reduced. Therefore, when Sn is contained, the Sn content is set to 0.001% or more and 0.500% or less, preferably 0.200% or less.
[0077] Sb (antimony) is effective in improving workability by promoting the formation of deformation bands during rolling. On the other hand, if Sb is contained in excess, the effect saturates and workability further decreases. Therefore, when Sb is contained, the Sb content is set to 0.001% or more and 0.500% or less, preferably 0.200% or less.
[0078] Pb (lead) lowers the melting point of grain boundaries and reduces the bonding strength of grain boundaries, which may lead to deterioration of hot workability, such as liquation cracking due to grain boundary melting. Therefore, if Pb is contained, its content should be 0.01% or more and 0.10% or less.
[0079] W (tungsten) has the effect of improving high-temperature strength without impairing ductility at room temperature. However, excessive addition of W generates coarse eutectic carbides, which causes a decrease in ductility, so if W is contained, the W content is set to 0.01% or more and 0.50% or less.
[0080] [Additional Notes] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in the different embodiments. Furthermore, new technical features can be formed by combining the technical means disclosed in the respective embodiments. EXAMPLES
[0081] Figure 2 shows the chemical compositions of austenitic stainless steels according to an example of the present invention and a comparative example. The values shown in Figure 2 represent the mass percent concentration of each component contained in the austenitic stainless steel. The austenitic stainless steels according to an example of the present invention were Steel Nos. A1 to A4, and the austenitic stainless steels according to the comparative examples were Steel Nos. B1 and B2. Both Steel Nos. B1 and B2 had a C+N content of less than 0.08%.
[0082] Figure 3 shows the physical properties of an austenitic stainless steel according to an embodiment of the present invention. Figure 4 shows the physical properties of an austenitic stainless steel according to a comparative example. The final pass rolling temperature in Figures 3 and 4 refers to the temperature of the steel sheet when rolling is performed in the final pass of finish hot rolling.
[0083] Regarding the evaluation results, "average cross-sectional hardness" indicates the average value of the results of measuring Vickers hardness at 10 points on a cross section parallel to the thickness direction with a load of 1 kg. The Vickers hardness was measured according to the method in accordance with JIS Z2244.
[0084] The surface properties were evaluated by measuring the depth of scabs. A scab depth of 5 μm or less was marked with ◎, a depth of more than 5 μm but less than 10 μm was marked with ◯, and a depth of more than 10 μm was marked with ×. To measure the depth of scabs, five locations where scabs had occurred were taken from the manufactured austenitic stainless steel strip as samples. After mirror polishing a cross section of the sample parallel to the thickness direction and hot rolling direction of the austenitic stainless steel strip, the surface layer of the sample was observed under an optical microscope to measure the depth of the scabs. Figures 3 and 4 show the average value of the measurement results of the samples taken from the five locations as the "scab depth."
[0085] The austenitic stainless steel produced by the manufacturing method satisfying the conditions of the manufacturing method according to one embodiment of the present invention had excellent surface properties, with an average hardness of 250 HV or more in a cross section parallel to the thickness direction and an average scab depth of 10 μm or less. On the other hand, as shown in FIG. 4, the austenitic stainless steel produced by the method not satisfying the conditions of the manufacturing method had an average hardness of less than 250 HV in a cross section parallel to the thickness direction or an average scab depth of more than 10 μm, and was in a state of poor surface properties. The conditions of the manufacturing method specifically refer to at least one of the C+N content, surface grinding of the continuously cast piece, the rolling ratio of the first pass of rough hot rolling, the total rolling ratio and final pass temperature of finish hot rolling, and the cooling rate. [Industrial Applicability]
[0086] The present invention can be used for austenitic stainless steel strips and the like that are suitable for applications requiring relatively thick, high-strength stainless steel, such as structural components for electronic devices such as smartphones, steel belts, press plates, and the like.
Claims
1. The combined content of C and N is 0.08% or more by mass%, The average hardness of a cross section parallel to the thickness direction is 250 HV or more, The thickness is 3 mm or more, The average depth of scab defects caused by grain boundary cracking during hot rolling is 10 μm or less, A hot-rolled austenitic stainless steel strip or a hot-rolled austenitic stainless steel plate containing, by mass%, C: 0.003% or more and 0.120% or less, Si: 2.0% or less, Mn: 2.0% or less, P: 0.04% or less, S: 0.0012% or less, Ni: 6.0% or more and 15.0% or less, Cr: 16.0% or more and 22.0% or less, N: 0.005% or more and 0.200% or less, with the balance being Fe and unavoidable impurities.
2. 2. The austenitic stainless steel strip or hot-rolled austenitic stainless steel sheet according to claim 1, further containing, in mass%, one or more of Mo: 0.01% or more and 3.00% or less, Cu: 0.01% or more and 3.50% or less, Al: 0.008% or less, O: 0.001% or more and 0.010% or less, V: 0.01% or more and 0.50% or less, B: 0.0003% or more and 0.0100% or less, and Ti: 0.01% or more and 0.50% or less.
3. 3. The austenitic stainless steel strip or hot-rolled austenitic stainless steel sheet according to claim 1 or 2, further containing, by mass%, one or more of Co: 0.01% or more and 0.50% or less, Zr: 0.01% or more and 0.10% or less, Nb: 0.01% or more and 0.10% or less, Mg: 0.0005% or more and 0.0030% or less, Ca: 0.0003% or more and 0.0030% or less, Y: 0.01% or more and 0.20% or less, REM (rare earth metal): 0.01% or more and 0.10% or less, Sn: 0.001% or more and 0.500% or less, Sb: 0.001% or more and 0.500% or less, Pb: 0.01% or more and 0.10% or less, and W: 0.01% or more and 0.50% or less.
4. 4. The austenitic stainless steel strip or hot-rolled austenitic stainless steel sheet according to claim 1, having a relative magnetic permeability μ of 1.1 or less.
5. A rough hot rolling process in which the slab produced by casting contains, by mass%, C: 0.003% to 0.120%, Si: 2.0% or less, Mn: 2.0% or less, P: 0.04% or less, S: 0.0012% or less, Ni: 6.0% to 15.0% or less, Cr: 16.0% to 22.0% or less, and N: 0.005% to 0.200% or less, and the total content of C and N is 0.08% or more by mass%, with the balance being Fe and unavoidable impurities, and the slab is heated to a temperature of 1000 ° C. to 1300 ° C. and then subjected to rough hot rolling; A finish hot rolling process in which the steel strip obtained by the rough hot rolling process is subjected to finish hot rolling; A cooling step of cooling the steel strip after the finish hot rolling step, In the rough hot rolling process, Without surface grinding the slab, The rolling ratio of the first pass of the rough hot rolling is 30% or less, In the finish hot rolling process, The total rolling ratio of the finish hot rolling is 60% or more, The temperature of the finish hot rolling is 600° C. or more and 1100° C. or less, The final pass temperature of the finish hot rolling is 950° C. or less, In the cooling step, When the final pass temperature of the finish hot rolling is 750° C. or higher, the steel strip is cooled to 750° C. or lower at a cooling rate of 5° C. / s or higher; To manufacture an austenitic stainless steel having an average hardness of 250 HV or more in a cross section parallel to the thickness direction and an average depth of scab defects caused by grain boundary cracking during hot rolling of 10 μm or less. , a method for producing austenitic stainless steel.
6. 6. The method for producing an austenitic stainless steel according to claim 5, wherein the slab further contains, by mass%, one or more of the following: Mo: 0.01% or more and 3.00% or less, Cu: 0.01% or more and 3.50% or less, Al: 0.008% or less, O: 0.001% or more and 0.010% or less, V: 0.01% or more and 0.50% or less, B: 0.0003% or more and 0.0100% or less, and Ti: 0.01% or more and 0.50% or less.
7. 7. The method for producing an austenitic stainless steel according to claim 5 or 6, wherein the slab further contains, by mass%, one or more of Co: 0.01% or more and 0.50% or less, Zr: 0.01% or more and 0.10% or less, Nb: 0.01% or more and 0.10% or less, Mg: 0.0005% or more and 0.0030% or less, Ca: 0.0003% or more and 0.0030% or less, Y: 0.01% or more and 0.20% or less, REM (rare earth metal): 0.01% or more and 0.10% or less, Sn: 0.001% or more and 0.500% or less, Sb: 0.001% or more and 0.500% or less, Pb: 0.01% or more and 0.10% or less, and W: 0.01% or more and 0.50% or less.
8. A method for producing an austenitic stainless steel described in any one of claims 5 to 7, comprising a pickling process in which a pickling treatment is performed after the cooling process.
9. A method for producing an austenitic stainless steel as described in claim 8, comprising a temper rolling process in which temper rolling is performed with a total rolling reduction ratio of 30% or less after the pickling process.
Citation Information
Patent Citations
Manufacture of cr-ni base stainless steel alloy without generating surface flaw
JP1994304606A
Nonmagnetic stainless steel excellent in surface property and production thereof
JP1995113144A
Production of austenitic stainless steel excellent in surface condition
JP1996103802A
Manufacture of austenitic stainless steel sheet on which flaw is not generated at time of hot rolling
JP1999319910A
Method for hot rolling austenitic stainless steel billet
JP2004137540A