Martensitic stainless steel material and its manufacturing method

A martensitic stainless steel material with controlled Cu content and treatment processes achieves reduced electrical and surface contact resistance, along with improved scratch resistance, addressing the limitations of existing techniques for martensitic stainless steel.

JP7568497B2Active Publication Date: 2024-10-16NIPPON STEEL CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020205230
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-10
Publication Date
2024-10-16
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

Existing techniques for reducing electrical resistance and surface contact resistance in stainless steel materials, such as those described in Patent Documents 1, 2, and 3, face challenges in cost, material limitations, and inefficiencies, particularly for martensitic stainless steel, which requires improvements in both electrical resistance and surface contact resistance without increasing manufacturing costs.

Method used

A martensitic stainless steel material containing 1.0% to 15.0% Cu by mass, with a Cu-rich phase of less than 500 nm grain size in the matrix, is produced through specific aging and pickling treatments, including a mixed acid solution at controlled temperatures, to form a Cu-enriched surface layer, reducing electrical resistance and surface contact resistance.

Benefits of technology

The resulting martensitic stainless steel material achieves reduced electrical resistance to 60 μΩ·cm or less and surface contact resistance to 45 mΩ or less, with improved scratch resistance and stability for electrical contact components, while maintaining cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568497000004
    Figure 0007568497000004
  • Figure 0007568497000005
    Figure 0007568497000005
  • Figure 0007568497000001
    Figure 0007568497000001
Patent Text Reader

Abstract

To provide a martensitic stainless steel and a method for producing the same in which both electrical resistance and surface contact resistance are reduced.SOLUTION: The martensitic stainless steel contains Cu of 1.0 mass% or more and 15.0 mass% or less, and has (i) a base material in which a first Cu-rich phase having a particle size of less than 500 nm is formed in the matrix, and (ii) a Cu-enriched surface layer part formed on the surface of the martensitic stainless steel and having Cu more enriched than the base material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a martensitic stainless steel material and a method for producing the same. [Background technology]

[0002] 2. Description of the Related Art Conventionally, various techniques have been proposed for improving the electrical conductivity of stainless steel materials in order to apply the stainless steel materials to conductive parts (for example, electrical contact parts) and the like.

[0003] For example, techniques are known for reducing the surface contact resistance of stainless steel material by forming a layer made of Ni or a Ni alloy on the surface of the stainless steel material (Patent Document 1) or by modifying the surface of the stainless steel material (Patent Document 2).

[0004] Patent Document 2 describes modifying the surface of a stainless steel material, specifically describing (i) concentrating Cu in the passive film or the outermost layer of the stainless steel material, and (ii) precipitating a second phase mainly composed of Cu on the surface of the stainless steel material to partially inhibit the formation of the passive film.

[0005] Furthermore, for example, Patent Document 3 describes a stainless steel material in which a Cu-rich phase is precipitated by aging in a ferrite phase matrix, thereby reducing the electrical resistance of the base material. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2013-087329 A [Patent Document 2] JP 2001-089865 A [Patent Document 3] JP 2004-277807 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the technology described in Patent Document 1 requires that the base material of the stainless steel material be an austenitic stainless steel and that a Ni-containing layer be formed on the surface of the base material, making it difficult to reduce manufacturing costs. In addition, in general, the electrical resistance of the base material of stainless steel tends to increase as the content of alloy components increases (high alloy content).

[0008] While the technique described in Patent Document 2 can reduce the surface contact resistance of the stainless steel material, there is room for improvement in terms of reducing the electrical resistance of the base metal in the stainless steel material.

[0009] While the technique described in Patent Document 3 can reduce the electrical resistance of the base metal in the stainless steel material, there is room for improvement in terms of reducing the surface contact resistance of the stainless steel material.

[0010] One aspect of the present invention has been devised in consideration of the above-mentioned conventional problems, and its object is to provide a martensitic stainless steel material and a manufacturing method thereof in which both electrical resistance and surface contact resistance are reduced. [Means for solving the problem]

[0011] In order to solve the above problems, a martensitic stainless steel material according to one embodiment of the present invention is a martensitic stainless steel material containing 1.0 mass % or more and 15.0 mass % or less of Cu, and is provided with a base material in which a first Cu-rich phase having a grain size of less than 500 nm is formed in a matrix, and a Cu-enriched surface layer portion formed on the surface of the martensitic stainless steel material, in which Cu is more concentrated than in the base material.

[0012] A method for producing a martensitic stainless steel material according to one embodiment of the present invention includes an annealing step of heating a rolled material having a composition of martensitic stainless steel containing 1.0 mass % or more and 15.0 mass % or less of Cu at a temperature of 780° C. or more and 830° C. or less for 6 hours or more, an aging treatment step of forming a first Cu-rich phase having a grain size of less than 500 nm in a matrix by performing an aging treatment on a first intermediate material obtained by performing an intermediate step including at least a first pickling step after the annealing step under conditions in which the A value defined by the following formula (1) is 15.0 to 20.0, and a second pickling step of performing a pickling treatment on a second intermediate material obtained by the aging treatment step using a mixed solution containing (i) 50 g / L to 150 g / L of nitric acid and (ii) 5 g / L to 15 g / L of hydrofluoric acid, with the mixed solution temperature being set to 30° C. to 60° C.; A = T(20+logt) × 10 -3 (1) (where: T: Aging temperature (K) t: aging time (h) (It is.) Effect of the Invention

[0013] According to one aspect of the present invention, it is possible to provide a martensitic stainless steel material having reduced electrical resistance and surface contact resistance, and a method for producing the same. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view showing a martensitic stainless steel material according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing an example of a change in Cu intensity in the depth direction near the surface of a martensitic stainless steel material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment of the present invention will be described below. Note that the following description is for better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified. In this specification, "A to B" indicates A or more and B or less.

[0016] A martensitic stainless steel material according to one embodiment of the present invention is a martensitic stainless steel material containing 1.0% by mass to 15.0% by mass of Cu, and includes a base material in which a first Cu-rich phase having a grain size of less than 500 nm is formed in a matrix, and a Cu-enriched surface layer portion formed on the surface of the martensitic stainless steel material, in which Cu is more concentrated than in the base material.

[0017] The matrix contained in the base material may include a multi-phase structure of a ferrite phase and 50% by volume or more of a martensite phase. The multi-phase structure means that the part (base material) other than the Cu-rich phase in the metal structure of the base material is substantially composed of a multi-phase structure of a ferrite phase and a martensite phase. The martensite phase contained in the part other than the Cu-rich phase accounts for 50% by volume or more of the entire metal structure of the base material. "Substantially" means that the mixture of other phases (for example, precipitates and inclusions) is allowed in a range of about 3% by volume or less. The matrix of the base material may be substantially a martensite single-phase structure. The martensite single-phase structure means that the part (base material) other than the Cu-rich phase in the metal structure of the base material is substantially composed of a martensite phase. "Substantially" has the same meaning as above.

[0018] (Definition of terms) The "martensitic stainless steel material" is not limited to a specific shape such as a steel strip or a steel plate. In this embodiment, a martensitic stainless steel strip will be described as an example of a martensitic stainless steel material. In addition, since a "steel plate" can be considered to be a part of a "steel strip", the term "martensitic stainless steel plate" is used to include a "martensitic stainless steel strip".

[0019] In addition, the "surface contact resistance value" is an index representing the contact electrical resistance on the surface of a stainless steel material, and generally, the surface contact resistance value of a stainless steel material is high. This is because a passive film exists on the surface of the stainless steel material.

[0020] "Electrical resistivity" is an index that indicates the difficulty of electric current flowing through the entire steel of a stainless steel material. In general, stainless steel materials exhibit a relatively high electrical resistivity because they are high alloys.

[0021] "Scratch resistance" refers to the property of how difficult it is for scratches to occur on the surface of a stainless steel material. It can be said that the harder the surface of a stainless steel material is, the more improved the scratch resistance is.

[0022] The "Cu-rich phase" refers to a second phase that is mainly composed of Cu and is formed in the material structure of Cu-containing stainless steel, and is a phase that contains 80 atomic % or more of Cu.

[0023] (General manufacturing process) First, an example of a general manufacturing process for stainless steel strip will be described in outline. In one example, the general manufacturing process for stainless steel strip includes a steelmaking process, a hot rolling process, an annealing process, a pickling process, a cold rolling process, an annealing and pickling process, and a finish rolling process in this order. Each of these steps in the conventional manufacturing process is publicly known, and therefore detailed description will be omitted except for the following description.

[0024] The steps after the hot rolling step are usually carried out using a coil formed from a wound stainless steel strip, that is, the stainless steel strip is unwound from the coil and then continuously treated, and the treated stainless steel strip is wound again into a coil.

[0025] In recent years, in the above-mentioned annealing process, the stainless steel strip is often continuously annealed from the viewpoint of cost reduction, in which case the stainless steel strip drawn from the coil is continuously annealed in an annealing line. In contrast to this, there is also a method in which the above-mentioned coil is directly annealed for a relatively long time in a heating furnace (e.g., a bell-type annealing furnace), and this type of method is called batch annealing (also called box annealing or bell annealing).

[0026] When pickling the annealed stainless steel strip, various methods are used to remove scale from the surface of the stainless steel strip. For example, the pickling solution used for pickling is a mixture of nitric acid and hydrofluoric acid, an acid solution containing sulfuric acid, etc. In addition, the annealed stainless steel strip may be subjected to electrolytic pickling using, for example, nitric acid.

[0027] (Summary of the findings of the invention) When stainless steel materials are applied to conductive parts, etc., the stainless steel materials are required to have low surface contact resistance and low electrical resistance of the base material.

[0028] In addition, the use of stainless steel materials for electrical contact parts, which are a type of conductive parts, is being considered. For example, parts such as terminals can have scratches on their surfaces when they are inserted and removed when connecting to other circuits. Such surface scratches reduce the stability of the parts.

[0029] Therefore, stainless steel materials for electrical contact parts are required to have reduced electrical resistance and surface contact resistance, as well as improved scratch resistance, and are also required to be manufactured at low cost.

[0030] The present inventors have conducted extensive research into relatively inexpensive martensitic stainless steel materials that can be suitably applied to electrical contact parts, etc. As a result, they have obtained the following findings and arrived at the present invention.

[0031] That is, a large amount of Cu-rich phase with a relatively large grain size can be precipitated in the base material by performing long-term batch annealing on a steel material having a component composition of martensitic stainless steel containing Cu. Then, an intermediate material (first intermediate material) obtained by performing intermediate treatment after batch annealing is subjected to aging treatment to further precipitate the Cu-rich phase in the base material. By specifying the conditions for this aging treatment, a fine Cu-rich phase (first Cu-rich phase) with a smaller grain size and finer than the Cu-rich phase (second Cu-rich phase) generated by the batch annealing can be precipitated in the base material.

[0032] Among a plurality of pickling treatments that may be included in the manufacturing process of the martensitic stainless steel material, at least the conditions of the pickling treatment after the aging treatment are specified. As a result, the following phenomenon occurs in the pickling treatment after the aging treatment. That is, Cu ions dissolved from the surface of the intermediate material (second intermediate material) after the aging treatment and contained in the pickling solution are reattached to the surface of the intermediate material during the pickling treatment. Here, the base material of the intermediate material contains a Cu-rich phase and a fine Cu-rich phase due to the batch annealing and aging treatment. Therefore, the Cu-rich phase and the fine Cu-rich phase present in the vicinity of the surface of the intermediate material are dissolved, thereby increasing the concentration of Cu ions dissolved in the pickling solution. As a result, a Cu-enriched portion can be appropriately formed on the surface of the martensitic stainless steel material and in its vicinity. In this specification, the surface of the martensitic stainless steel material on which the Cu-enriched portion is formed and its vicinity are referred to as a Cu-enriched surface layer portion. This Cu-enriched surface layer contains a Cu adhesion layer formed by the precipitation of Cu ions in the pickling solution, a Cu-rich phase, and a fine Cu-rich phase, which can reduce the surface contact resistance.

[0033] In addition, the fine Cu-rich phase, like the Cu-rich phase, is a phase that is mainly composed of Cu and is generated in the material structure of stainless steel containing Cu, and is a phase that contains 80 atomic % or more of Cu.

[0034] These effects have realized a martensitic stainless steel material in which both electrical resistance and surface contact resistance are reduced while improving surface hardness. In addition, the matrix of the base material of the martensitic stainless steel material in one embodiment of the present invention is a multiphase structure of a ferrite phase and a martensite phase that accounts for 50 volume % or more of the base material, or a martensite single phase structure. Furthermore, the martensitic stainless steel material contains a fine Cu-rich phase in the Cu-enriched surface layer. With these configurations, the martensitic stainless steel material has improved surface hardness and scratch resistance. By using such a martensitic stainless steel material, electrical contact parts having stable electrical conductivity can be manufactured.

[0035] <Martensitic stainless steel material> A martensitic stainless steel material in one embodiment of the present invention will be described below with reference to Fig. 1. Fig. 1 is a cross-sectional view that shows a schematic view of a martensitic stainless steel material 1 in one embodiment of the present invention.

[0036] As shown in Fig. 1, the martensitic stainless steel material 1 of this embodiment has a fine Cu-rich phase (first Cu-rich phase) 21 having a grain size of less than 500 nm and a Cu-rich phase (second Cu-rich phase) 22 having a grain size of 500 nm or more formed in a matrix 25. In addition, the martensitic stainless steel material 1 of this embodiment has a Cu-enriched surface layer portion 10 in which Cu is more concentrated than in the matrix 25 formed on the surface of the base material 20 and in its vicinity. The matrix 25 is the main phase (parent phase) in the base material 20, and is a multi-phase structure of a ferrite phase and a martensite phase that accounts for 50 volume % or more of the base material 20, or a martensite single-phase structure.

[0037] The Cu-enriched surface portion 10 includes a passive film 11, a Cu adhesion layer 13, and a matrix surface layer 25A which is a surface portion of the matrix 25. The matrix surface layer 25A includes a fine Cu-rich phase 21 and a Cu-rich phase 22. Each of these portions will be described in detail later.

[0038] In addition, in FIG. 1, the structure of the Cu-enriched surface layer portion 10 and the base material 20 is shown typically, but the shape, size, and position of each part included in the Cu-enriched surface layer portion 10 and the base material 20 are provisionally set for the purpose of illustration and do not limit the invention.

[0039] (composition) The martensitic stainless steel material 1 contains Cu: 1.0 mass% or more and 15.0 mass% or less. The martensitic stainless steel material 1 has a composition based on the composition of martensitic stainless steel and contains Cu. That is, the martensitic stainless steel material 1 has a Ni content of 1.0 mass% or less.

[0040] Cu is added to improve the electrical conductivity of the martensitic stainless steel material 1. If the Cu content is less than 1.0 mass%, the electrical conductivity cannot be sufficiently improved by the treatment described below. On the other hand, if the Cu content is too high, the hot workability and corrosion resistance may decrease, so the Cu content is limited to 15.0 mass% or less. Note that, when manufacturing steel plate, etc., where the cost increase due to the deterioration of hot workability becomes significant, it is desirable to contain Cu in the range of 8.0 mass% or less.

[0041] Cr is an essential element for improving the corrosion resistance of steel, and the martensitic stainless steel material 1 preferably contains Cr: 9.0 mass% or more and 13.0 mass% or less. Excessive addition of Cr can cause a decrease in electrical conductivity and deterioration of manufacturability, so the Cr content is limited to 13.0 mass% or less.

[0042] In consideration of the balance between hot workability and electrical resistance, the martensitic stainless steel material 1 preferably contains Cu: 1.5% by mass to 5.0% by mass, and Cr: 11.0% by mass to 13.0% by mass.

[0043] As for alloying elements other than Cr and Cu, the mass percent is C+N: 0.10% or less, Mn: 2.0% or less, Si: 2.0% or less, and if necessary, one or two of Ti: 0.5% or less and Nb: 0.5% or less may be contained, with the balance being Fe and unavoidable impurities. In addition, if necessary, one or more of these elements may be contained within the following ranges: Mo: 3.0% or less, Al: 5.0% or less, V: 2.0% or less, W: 2.0% or less, Zr: 1.0% or less, REM: 0.1% or less.

[0044] When one or both of Ti: 0.5% or less and Nb: 0.5% or less are contained, it is desirable to satisfy the following formula (2): 7(C+N)≦Ti+Nb≦7(C+N)+0.3···(2).

[0045] (Cu-rich phase / fine Cu-rich phase) The fine Cu-rich phase 21 is an aging precipitate dispersed in the matrix 25 by the aging precipitation treatment described later. The particle size of the fine Cu-rich phase 21 is greater than 0 and less than 500 nm. The lower limit of the particle size is not particularly limited, and it is sufficient as long as the particle size can be observed using a transmission electron microscope. The particle size of the fine Cu-rich phase 21 is preferably 5 nm or more and 20 nm or less. The particle size of each particle of the fine Cu-rich phase 21 is represented by the maximum diameter of the particle. Although it is difficult to quantitatively measure the particle size of each extremely fine particle, it is sufficiently possible to determine whether the particle size of the heterogeneous phase dispersed in the matrix 25 is within a range of less than 500 nm by observing using a transmission electron microscope. It is also possible to determine whether the particle size of the fine Cu-rich phase 21 is within a range of 5 nm or more and 20 nm or less.

[0046] The Cu-rich phase 22 is precipitates dispersed in the matrix 25 by the batch annealing treatment described later. The grain size of the Cu-rich phase 22 is 500 nm or more, and preferably 1500 nm or more.

[0047] The martensitic stainless steel material in one embodiment of the present invention contains at least a fine Cu-rich phase 21 in the matrix 25. This allows the electrical resistivity of the base material 20 to be reduced. The martensitic stainless steel material 1 in this embodiment has a structure in which the fine Cu-rich phase 21 and the Cu-rich phase 22 coexist in the matrix 25, allowing the electrical resistivity of the base material 20 to be reduced more effectively. In particular, the fine Cu-rich phase 21 having a grain size of 5 nm or more and 20 nm or less and the Cu-rich phase 22 having a grain size of 1500 nm or more are coexisted and dispersed in the matrix 25, which is a martensitic phase, thereby increasing the effect of improving electrical conductivity.

[0048] The reason for this is not clear, but it is thought that, for example, in the base material 20, the distance between the fine Cu-rich phases 21 and the Cu-rich phases 22 becomes shorter, forming an electrical conduction path.

[0049] (Cu enriched surface layer) As shown in FIG. 1, a Cu-enriched surface layer 10 is formed on the surface of the martensitic stainless steel material 1, in which Cu is more concentrated than in the matrix 25. The Cu-enriched surface layer 10 is formed by making the base material 20 contain at least a Cu-rich phase 22 by a batch annealing treatment and an aging treatment described later, and then performing a pickling treatment (pickling treatment using a mixed acid) described later. Hereinafter, in this specification, the pickling treatment that forms the Cu-enriched surface layer 10 is referred to as a Cu-adhesive pickling treatment. This Cu-adhesive pickling treatment is performed as at least the final pickling treatment in the manufacturing process of the martensitic stainless steel material 1. It is preferable that the Cu-adhesive pickling treatment is also performed in an intermediate process between the batch annealing and the final pickling treatment. The reason for this will be described later.

[0050] The Cu-enriched surface layer portion 10 will be described with reference to Fig. 2. Fig. 2 is a graph showing an example of a change in Cu intensity in the depth direction detected by performing glow discharge optical emission surface analysis on the surface of a martensitic stainless steel material 1. Specifically, the distribution state of Cu in the depth direction from the surface of the martensitic stainless steel material 1 was measured by glow discharge optical emission surface analysis (GDS) using a test piece having a width of 50 mm and a length of 50 mm. The Cu concentration of the matrix 25 was adopted as an average value in a portion having a depth of, for example, 40 nm to 50 nm.

[0051] As shown in FIG. 2, when the martensitic stainless steel material 1 of this embodiment is subjected to a composition analysis, the Cu concentration (surface layer strength I) at the surface and its vicinity is obviously greater than the intensity I0 of the Cu concentration in the matrix 25. Such a surface layer portion in the martensitic stainless steel material 1 is referred to as the Cu-enriched surface layer portion 10. The Cu-enriched surface layer portion 10 is formed in a region from the surface of the martensitic stainless steel material 1 to a depth of about 3 nm. The surface layer strength I means the intensity of a peak in a graph showing the Cu concentration in the Cu-enriched surface layer portion 10. In the example shown in FIG. 2, the surface layer strength I is about 0.84. In the martensitic stainless steel material 1 of this embodiment, the ratio of the surface layer strength I in the Cu-enriched surface layer portion 10 to the intensity I0 of the Cu concentration in the matrix 25 (surface layer Cu intensity ratio) is 1.5 or more, for example, 1.6 or more and 2.5 or less. From the viewpoint of the stability of the surface contact resistance value, the martensitic stainless steel material 1 preferably has a surface layer Cu intensity ratio of 1.7 or more. The martensitic stainless steel material 1 preferably has a surface layer Cu intensity ratio of 2.0 or less. This is because if the surface layer Cu intensity ratio exceeds 2.0, the corrosion resistance of the martensitic stainless steel material 1 may decrease. The martensitic stainless steel material 1 preferably has a surface layer Cu intensity ratio of 1.7 or more and 2.0 or less.

[0052] Although the detailed structure of the Cu-enriched surface layer portion 10 is not clear, since the surface layer Cu intensity ratio is 1.5 or more as described above, it is considered to have a structure including a Cu adhesion layer 13, a passive film 11, and a matrix surface layer 25A. The matrix surface layer 25A is a portion near the outermost surface of the matrix 25 (for example, a portion from the outermost surface to a depth of several nm), and includes a fine Cu-rich phase 21 and a Cu-rich phase 22 (see FIG. 1). The matrix surface layer 25A is a part of the matrix 25.

[0053] The Cu-enriched surface portion 10 includes a Cu adhesion layer 13 formed by Cu ions dissolved in the pickling solution in the Cu adhesion pickling treatment adhering (re-adhering) to the surface of the base material 20. The Cu adhesion layer 13 is a phase containing 80 atomic % or more of Cu, and may contain oxidized or hydroxided Cu. The Cu adhesion layer 13 has a thickness of, for example, 2 nm to 20 nm. The Cu adhesion layer 13 is formed in a spatially sparse state (for example, a porous state) by the Cu ions adhering to the surface of the base material 20. Therefore, the Cu adhesion layer 13 is formed to have a communicating hole that communicates between the atmosphere and the matrix surface layer 25A. The communicating hole has a shape that allows at least oxygen to move from the atmosphere to the matrix surface layer 25A.

[0054] The Cu-enriched surface layer portion 10 of the martensitic stainless steel material 1 in this embodiment has a passive film 11 formed on the lower surface of the Cu adhesion layer 13 in the atmosphere.

[0055] The passive film 11 is formed on at least a portion of the interface between the Cu adhesion layer 13 and the matrix surface layer 25A by a reaction between (i) oxygen that comes into contact with the matrix surface layer 25A through the porous Cu adhesion layer 13 (specifically, the above-mentioned communicating holes) and (ii) Cr and other elements contained in the matrix surface layer 25A.

[0056] More specifically, in the above-mentioned Cu adhesion pickling treatment, the passivation film that existed before the treatment is destroyed, and a Cu adhesion layer 13 is formed on the surface of the matrix 25 (or the matrix surface layer 25A). After the above-mentioned Cu adhesion pickling treatment, oxygen is supplied through the Cu adhesion layer 13 in a porous state in the atmosphere, so that a passivation film 11 is formed at the interface between the matrix surface layer 25A and the Cu adhesion layer 13.

[0057] Moreover, the matrix surface layer 25A in the Cu-enriched surface portion 10 includes a fine Cu-rich phase 21 and a Cu-rich phase 22.

[0058] 1, in the Cu-enriched surface layer portion 10, the passivation film 11 may not be formed in the region where the fine Cu-rich phase 21 or Cu-rich phase 22 is present on the surface of the matrix 25 (i.e., the interface between the Cu adhesion layer 13 and the matrix surface layer 25A). This is because the amount of Cr present in this region is insufficient, making it difficult to form the passivation film 11. In this case, the Cu adhesion layer 13 may be in contact with the fine Cu-rich phase 21 or Cu-rich phase 22.

[0059] In addition, in areas of the Cu-enriched surface portion 10 where the supply of oxygen through the porous Cu adhesion layer 13 is insufficient, the Cu adhesion layer 13 and the matrix surface layer 25A may be in contact with each other, forming a relatively highly conductive area.

[0060] The Cu-enriched surface portion 10 includes a Cu adhesion layer 13 and a matrix surface layer 25A on the surface, and includes a passive film 11 on at least a part of the interface therebetween. In the Cu-enriched surface portion 10, an electrical conduction path having a relatively high electrical conductivity is formed by the Cu adhesion layer 13 and the fine Cu-rich phase 21 or the Cu-rich phase 22. This allows the martensitic stainless steel material 1 to have a lower surface contact resistance than a general martensitic stainless steel material.

[0061] (Conductive) The martensitic stainless steel material 1 of the present embodiment has an electrical resistivity reduced to 60 μΩ·cm or less and a surface contact resistance reduced to 45 mΩ or less. The martensitic stainless steel material 1 preferably has an electrical resistivity reduced to 60 μΩ·cm or less and a surface contact resistance reduced to 30 mΩ or less.

[0062] <Manufacturing method> An example of a method for manufacturing the martensitic stainless steel sheet of this embodiment will be described below.

[0063] (Pretreatment process) In the pretreatment step, first, a vacuum melting furnace is used to produce steel having a composition adjusted to fall within the range of the present invention. This steel is then cast to produce a steel ingot.

[0064] (Hot rolling process) In the hot rolling process, the steel ingot after the pretreatment process is hot rolled to produce a hot rolled steel strip. The temperature in the rolling process may be within a general range, for example, about 800°C to 1250°C.

[0065] (First annealing process) The manufacturing method of the martensitic stainless steel sheet of this embodiment includes an annealing step in which the hot rolled steel strip is annealed (batch annealing) using, for example, a batch annealing furnace (bell annealing furnace) to anneal the rolled material having the component composition of martensitic stainless steel. This annealing step is referred to as the first annealing step (batch annealing step). The heating temperature in the first annealing step is 780°C or higher and 830°C or lower, and the heating time is 6 hours or longer. In the first annealing step, the hot rolled steel strip is held at the heating temperature for the treatment time. In the first annealing step, annealing is performed in an air atmosphere or a N 2 and H 2 The annealing may be performed in either an atmosphere or a mixture atmosphere of the above.

[0066] By subjecting the hot-rolled steel strip to the first annealing step, a large amount of Cu-rich phase 22 can be precipitated in the matrix 25. In the first annealing step, the heating temperature is set to 780° C. or higher, thereby softening the hot-rolled steel strip.

[0067] In the first annealing step, the heating temperature is set to 830°C or lower so as to prevent phase transformation (α phase to γ ​​phase) in the matrix 25 of the hot rolled steel strip. The matrix 25 of the hot rolled steel strip may have a temperature region (a γ loop in a phase diagram) in which the matrix 25 transforms into an austenite phase depending on the steel composition. The austenite phase transforms into a martensite phase after cooling, which may reduce the toughness of the steel strip and cause manufacturing defects.

[0068] Therefore, the heating temperature range in the first annealing step is specified as a relatively narrow range of 780°C or higher and 830°C or lower.

[0069] (intermediate process) In the method for producing the martensitic stainless steel material 1 in this embodiment, after the first annealing step, an intermediate step including at least a first pickling step is performed.

[0070] The annealed steel strip (first annealed material) obtained in the first annealing step is subjected to a pickling treatment in a first pickling step, in which descaling of the annealed steel strip is carried out.

[0071] In the first pickling step, it is preferable to carry out pickling treatment for Cu adhesion using a mixed acid under the same conditions as in the final pickling step described later. Specifically, it is preferable to carry out the pickling treatment on the annealed steel strip using a pickling solution (mixed acid) containing (i) nitric acid at 50 g / L to 150 g / L and (ii) hydrofluoric acid at 5 g / L to 15 g / L, and to set the temperature of the pickling solution at 30°C to 60°C.

[0072] In the manufacturing method of the martensitic stainless steel material 1 in this embodiment, a case will be described in which in the first pickling step, pickling treatment for Cu adhesion is performed under the same conditions as in the final pickling step described later.

[0073] In the first pickling step, the Cu adhesion pickling process is performed, whereby descaling occurs on the surface of the annealed steel strip, and a part of the matrix 25 (including the Cu-rich phase 22) dissolves, and Cu ions are eluted into the pickling solution. In the first pickling step, the Cu ions contained in the pickling solution are redeposited on the surface of the annealed steel strip. As a result, a Cu adhesion layer is formed on the surface of the annealed steel strip. Hereinafter, the Cu adhesion layer formed on the surface of the treated material during the manufacturing process of the martensitic stainless steel material 1 is referred to as an intermediate Cu adhesion layer to distinguish it from the Cu adhesion layer 13 in the martensitic stainless steel material 1. This intermediate Cu adhesion layer may have the same composition as the Cu adhesion layer 13. The total amount of Cu contained in the intermediate Cu adhesion layer is relatively smaller than the total amount of Cu contained in the Cu adhesion layer 13.

[0074] The intermediate step may include a cold rolling step subsequent to the first pickling step. When the intermediate step includes a cold rolling step, the annealed steel strip descaled in the first pickling step is cold rolled at a rolling reduction of, for example, 50 to 80% to form a cold-rolled steel strip.

[0075] The intermediate process may include a second annealing process and a second pickling process in which the cold rolled steel strip is subjected to an annealing treatment and a pickling treatment following the cold rolling process.

[0076] This second annealing step may be continuous annealing, and the treatment time may be, for example, several tens of seconds to several minutes. The soaking temperature in the second annealing step is 1000°C or higher. The second annealing step is performed to transform the cold-rolled steel strip from the ferrite phase to the austenite phase (martensite phase after cooling). In the second annealing step, the steel strip after heating is air-cooled.

[0077] Next, the annealed steel strip after the second annealing step is subjected to a second pickling step. The annealed steel strip is descaled by the second pickling step. In the second pickling step, it is preferable to perform Cu adhesion pickling under the same conditions as the final pickling step described below. Specifically, it is preferable to use a pickling solution containing (i) nitric acid of 50 g / L to 150 g / L and (ii) hydrofluoric acid of 5 g / L to 15 g / L, and to perform the pickling treatment on the annealed steel strip with the temperature of the pickling solution being 30°C to 60°C.

[0078] In the second pickling step, scale is removed from the surface of the annealed steel strip, and the intermediate Cu adhesion layer, the passive film 11, and part of the matrix 25 (including the Cu-rich phase 22) are dissolved. Here, the intermediate Cu adhesion layer and part of the matrix surface layer 25A are dissolved on the surface of the annealed steel strip, thereby making it possible to increase the concentration of Cu ions in the pickling solution.

[0079] As a result, an intermediate Cu adhesion layer is effectively formed on the surface of the annealed steel strip after the second pickling step.

[0080] (Aging treatment process) The method for producing the martensitic stainless steel material 1 of this embodiment includes an aging treatment step in which the steel strip of the intermediate product (first intermediate material) after the above-mentioned intermediate step is aged under conditions in which the A value defined by the following formula (1) is 15.0 or more and 20.0 or less. A = T(20+logt) × 10 -3 (1) where T is the aging temperature (K) and t is the aging time (h).

[0081] By carrying out the aging treatment step as described above, it is possible to cause the fine Cu-rich phase 21 to be dispersed and precipitated in the matrix 25 of the steel strip of the intermediate product.

[0082] In the aging treatment step, the aging time t is preferably 0.016 h or more (approximately 60 sec or more) assuming a treatment on an operating line, and the aging temperature T is preferably 830° C. or less at which a large amount of fine Cu-rich phase 21 can be precipitated.

[0083] In addition, in the manufacturing method of the martensitic stainless steel material 1 in this embodiment, ΔHV calculated by the following formula (2) is greater than 35HV; ΔHV = HV2 - HV1 (2) Here, HV1 is the hardness of the intermediate product (first intermediate material) before the aging treatment process, and HV2 is the hardness of the intermediate product (second intermediate material) after the aging treatment process.

[0084] The martensitic stainless steel material 1 includes a fine Cu-rich phase 21 in a matrix 25 and has a Cu-enriched surface layer portion 10. This allows the material to be manufactured so that ΔHV is greater than 35HV. As a result, the surface hardness can be increased. Thus, the scratch resistance is improved. Moreover, the martensitic stainless steel material 1 preferably has ΔHV greater than 60HV, and more preferably greater than 200HV.

[0085] (Final pickling process) The manufacturing method of the martensitic stainless steel material 1 in this embodiment includes a final pickling process in which a final pickling process is performed on the intermediate product (second intermediate material) obtained by the aging treatment process. In the final pickling process, a mixed acid is used for pickling (mixed acid treatment). The pickling solution (mixed acid) used in the final pickling process contains 50 g / L of nitric acid and 3 to 15 g / L of hydrofluoric acid, and has a solution temperature of 30 to 60°C.

[0086] In mixed acid treatment, Cu ions in the dissolved oxide scale or base material are preferentially deposited (adhered) to the surface compared to other ions. As a result, Cu is concentrated in the surface layer. This effect makes it possible to reduce the surface contact resistance. On the other hand, in nitric acid electrolysis, the surface is constantly dissolved by the electrolytic treatment, so no deposition (adhesion) of dissolved ions is observed.

[0087] As in the first and second pickling steps described above, the final pickling step forms a Cu adhesion layer 13 on the surface of the treated material. As a result, a martensitic stainless steel material 1 having a Cu-enriched surface layer portion 10 can be obtained.

[0088] (Beneficial Effects) As described above, in the martensitic stainless steel material 1 in this embodiment, the base material 20 contains the fine Cu-rich phase 21 and the Cu-rich phase 22, so that the electrical resistance of the base material 20 is reduced. In addition, the surface contact resistance is reduced by providing the Cu-enriched surface layer portion 10. Furthermore, as described above, the hardness of the surface can be increased. That is, the martensitic stainless steel material 1 has reduced electrical resistance and surface contact resistance, and has improved scratch resistance.

[0089] The martensitic stainless steel material 1 has a Cu adhesion layer 13 formed as follows. That is, as described above, an intermediate Cu adhesion layer is formed on the surface of the first intermediate material by performing mixed acid treatment in the intermediate step. Then, in the subsequent aging treatment step, Cu in the intermediate Cu adhesion layer is diffused into the temper color (thin oxide scale) to form a Cu-rich temper color. Then, the Cu-rich temper color is dissolved in the final pickling step. As a result, more Cu can be adhered to the surface of the matrix surface layer 25A in the final pickling step, and the Cu adhesion layer 13 can be formed.

[0090] In addition, the martensitic stainless steel material 1 has a low Ni content and does not require a special coating on the surface, which can prevent the manufacturing cost from increasing.

[0091] Therefore, when the martensitic stainless steel material 1 is applied to, for example, electrical contact parts, it has excellent electrical conductivity because both electrical resistance and surface contact resistance are reduced. In addition, since the scratch resistance is improved, it is possible to reduce the possibility of electrical conductivity being deteriorated, and as a result, the electrical contact parts can be used stably. Therefore, the martensitic stainless steel material 1 can be suitably used as an electrical contact part.

[0092] [Additional notes] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the above description are also included in the technical scope of the present invention. EXAMPLES

[0093] Hereinafter, examples of the martensitic stainless steel material according to one embodiment of the present invention will be described, but the present invention is not limited to these examples.

[0094] In this embodiment, the martensitic stainless steel of the steel type shown in Table 1 was melted in a vacuum melting furnace and hot-rolled (1200°C, 2 hours) to form a hot-rolled sheet with a thickness of 3 mm. Next, batch annealing was performed by heating in a heating furnace at 600 to 800°C for 6 hours. Then, pickling was performed and cold rolling was performed to form a cold-rolled sheet with a thickness of 1.0 mm. Each cold-rolled sheet was annealed by soaking at 1050°C for 1 minute and air-cooling, and then pickling treatment was performed. Then, aging treatment was performed at various temperatures from 350°C to 900°C, and pickling treatment using mixed acid (see the above-mentioned embodiment for the composition) or pickling treatment using nitric acid electrolysis was performed. The aging treatment conditions are shown in Tables 2 and 3.

[0095] [Table 1]

[0096] Although numerical values ​​are omitted in Table 1, the Ni content of steel types C1 to C8 was 1.0 mass% or less. In the "classification" of Table 1, steel types containing 1.0 mass% or more and 15.0 mass% or less of Cu are referred to as "steels subject to the present invention," and steel types with a Cu content of less than 1.0 mass% are referred to as "comparative steels."

[0097] The steel sheets after batch annealing and aging treatment were observed with a transmission electron microscope to examine the grain size of the Cu-rich phase dispersed in the martensite matrix. Regarding the steel sheets after aging treatment, in order to distinguish between the Cu-rich phase precipitated after batch annealing and that after aging treatment, a steel sheet that was not batch annealed was separately manufactured, and this steel sheet was subjected to aging treatment to observe the grain size of the Cu-rich phase after aging treatment.

[0098] In addition, the steel sheets after aging were tested for surface contact resistance, electrical resistivity, and Cu concentration in the surface layer. Surface contact resistance was measured with an electrical contact simulator using a test piece 50 mm wide x 50 mm long. Electrical resistivity was measured with a four-terminal method (JIS C 2525) using a test piece 3 mm wide x 100 mm long. The Cu distribution in the depth direction from the surface in the surface layer was measured with GDS using a test piece 50 mm wide x 50 mm long. The surface layer Cu intensity ratio was determined by dividing the surface layer intensity I, which is the peak value of the Cu concentration in the Cu-enriched surface layer 10, by the intensity I0 of the Cu concentration in the base material (matrix 25).

[0099] In addition, the surface hardness of the steel sheet before the aging treatment and the surface hardness of the steel sheet after the aging treatment were measured, and the difference therebetween was calculated.

[0100] The results are shown in Tables 2 and 3. In Table 3, steel sheets having the following properties (A) and (B) are listed as "invention steels." In Table 2, steel sheets not having either property (A) or (B) are listed as "comparative steels." Characteristic (A): Surface contact resistance is 45 mΩ or less. Characteristic (B): Electrical resistivity is 60 μΩ·cm or less.

[0101] [Table 2]

[0102] [Table 3]

[0103] As shown in Table 2, in Comparative Examples 2, 4, and 6 in which nitric acid electrolysis was performed in the final pickling treatment, the surface contact resistance was high regardless of whether or not aging treatment was performed. In Comparative Example 4, although a fine Cu-rich phase 21 was formed, the surface contact resistance was high. This is thought to be because the Cu-enriched surface layer 10, especially the Cu adhesion layer 13, was not sufficiently formed. In Comparative Example 4, the surface layer Cu intensity ratio was 1.1, which is smaller than the reference value of 1.5, so it is presumed that the Cu-enriched surface layer 10 was not sufficiently formed.

[0104] Furthermore, as can be seen from the results of Comparative Example No. 1, when steel type C1 having a low Cu concentration was used, the surface contact resistance value and electrical resistivity could not be reduced even with the manufacturing method of the above embodiment.

[0105] In Comparative Examples 3 and 5, the conditions for the aging treatment were outside the scope of the present invention, and precipitation of the fine Cu-rich phase hardly occurred. In particular, in Comparative Example 5, the temperature and time for the aging treatment were high, so that the fine Cu-rich phase dissolved and Cu became solid-soluble in the base material. In Comparative Example 7, aging treatment was not performed, and precipitation of the fine Cu-rich phase hardly occurred. As a result, in Comparative Examples 3, 5, and 7, the electrical resistivity of the base material was higher than 60 μΩ·cm, and the ΔHV indicating the surface hardness was 35 or less.

[0106] In contrast, as shown in Table 3, the steel sheets of Examples 11 to 25 produced under conditions within the range of the present invention had reduced surface contact resistance and electrical resistivity, and also had large ΔHV and excellent scratch resistance. [Explanation of symbols]

[0107] 1. Martensitic stainless steel 10 Cu enriched surface layer 11 Passive film 13 Cu adhesion layer 20 Base material 21 Fine Cu-rich phase 22 Cu-rich phase 25 Matrix 25A Matrix surface

Claims

1. A steel sheet comprising, by mass%, Cu: 1.0% to 15.0%, Cr: 9.0% to 13.0%, C+N: 0.10% or less, Mn: 2.0% or less, and Si: 2.0% or less, Further, if necessary, one or both of Ti: 0.5% or less and Nb: 0.5% or less are contained; The Ni content is 1.0 mass% or less, A martensitic stainless steel material having a chemical composition consisting of the balance being Fe and unavoidable impurities, A base material in which a first Cu-rich phase having a grain size of less than 500 nm is formed in a matrix; A Cu-enriched surface layer portion formed on a surface of the martensitic stainless steel material, in which Cu is enriched more than in the base material, A ratio of a peak value of Cu intensity in the Cu-enriched surface layer portion to a value of Cu intensity in the base material, which is detected by a composition analysis of Cu, is 1.5 or more; The base material has a second Cu-rich phase having a grain size of 500 nm or more and 2000 nm or less formed in the matrix, The Cu-enriched surface portion includes: (i) a porous Cu adhesion layer containing 80 atomic % or more of Cu; and (ii) a passive film partially located at the interface between the Cu adhesion layer and a surface layer of the matrix, A martensitic stainless steel material having an electrical resistivity of 60 μΩ·cm or less and a surface contact resistance of 45 mΩ or less.

2. The Cu-enriched surface layer has a ratio of peak values ​​of the Cu intensity of 1.7 or more, 2. The martensitic stainless steel material according to claim 1, wherein the surface contact resistance is 10 mΩ or less.

3. The Cu adhesion layer is The thickness is 2 to 20 nm, having communicating holes communicating with a surface layer of the matrix, 3. The martensitic stainless steel material according to claim 1, wherein the communicating pores have a shape that allows oxygen to move from the atmosphere to a surface layer of the matrix.

4. The martensitic stainless steel material according to any one of claims 1 to 3, wherein the grain size of the first Cu-rich phase is 5 nm or more and 20 nm or less.

5. The martensitic stainless steel material according to any one of claims 1 to 4, wherein the matrix contains a multi-phase structure of a ferrite phase and a martensite phase that accounts for 50 volume % or more of the base material, or is a martensite single-phase structure.

6. A martensitic stainless steel material as described in any one of claims 1 to 5, wherein the first Cu-rich phase and the second Cu-rich phase located on the surface layer of the matrix are in contact with the Cu adhesion layer.

7. A steel sheet comprising, by mass%, Cu: 1.0% to 15.0%, Cr: 9.0% to 13.0%, C+N: 0.10% or less, Mn: 2.0% or less, and Si: 2.0% or less, Further, if necessary, one or both of Ti: 0.5% or less and Nb: 0.5% or less are contained; The Ni content is 1.0 mass% or less, An annealing process in which a rolled material having a component composition of martensitic stainless steel, the balance of which is Fe and unavoidable impurities, is heated at a temperature of 780°C to 830°C for 6 hours or more; After the annealing step, an aging treatment step is performed on a first intermediate material obtained by performing an intermediate step including at least a first pickling step, under conditions in which the A value defined by the following formula (1) is 15.0 or more and 20.0 or less, thereby forming a first Cu-rich phase having a grain size of less than 500 nm in a matrix; a final pickling step of subjecting the second intermediate material obtained by the aging treatment step to a pickling treatment using a mixed solution containing (i) 50 g / L or more and 150 g / L or less of nitric acid and (ii) 5 g / L or more and 15 g / L or less of hydrofluoric acid, with the mixed solution having a liquid temperature of 30° C. or more and 60° C. or less; a method for producing a martensitic stainless steel material, wherein the martensitic stainless steel material obtained by the final pickling step has an electrical resistivity of 60 μΩ cm or less and a surface contact resistance of 45 mΩ or less; A=T(20+logt)×10 -3 ...(1) (where: T: Aging temperature (K) t: aging time (h) (It is.)

8. 8. The method for producing a martensitic stainless steel material according to claim 7, wherein in the first pickling step, the first annealed material obtained by the annealing step is subjected to a pickling treatment using a mixed solution containing (i) nitric acid at 50 g / L or more and 150 g / L or less and (ii) hydrofluoric acid at 5 g / L or more and 15 g / L or less, with the mixed solution having a liquid temperature of 30°C or more and 60°C or less.

9. The method for producing a martensitic stainless steel material according to claim 7 or 8, wherein ΔHV calculated by the following formula (2) is greater than 35HV; ΔHV=HV2-HV1...(2) (where: HV1: hardness of the first intermediate material HV2: hardness of the second intermediate material (It is.)

10. The martensitic stainless steel material obtained by the final pickling step is A base material in which the first Cu-rich phase is formed in a matrix; A Cu-enriched surface layer portion formed on a surface of the martensitic stainless steel material, in which Cu is enriched more than in the base material, A ratio of a peak value of Cu intensity in the Cu-enriched surface layer portion to a value of Cu intensity in the base material, which is detected by a composition analysis of Cu, is 1.5 or more; The base material has a second Cu-rich phase having a grain size of 500 nm or more and 2000 nm or less formed in the matrix, The method for producing a martensitic stainless steel material according to any one of claims 7 to 9, wherein the Cu-enriched surface layer portion includes: (i) a porous Cu adhesion layer containing 80 atomic % or more of Cu; and (ii) a passive film partially located at the interface between the Cu adhesion layer and a surface layer of the matrix.

11. The Cu-enriched surface layer has a ratio of peak values ​​of the Cu intensity of 1.7 or more, The method for producing a martensitic stainless steel material according to claim 10, wherein the surface contact resistance is 10 mΩ or less.

Citation Information

Patent Citations

  • Stainless steel sheet low in contact resistance and its producing method

    JP2001089865A

  • Electric wiring terminal-manufacturing stainless steel plate excellent in surface contact electric resistance and punchability

    JP2004010993A

  • HIGH Cr STEEL MATERIAL FOR CURRENT-CARRYING PARTS HAVING IMPROVED ELECTRIC CONDUCTIVITY

    JP2004277807A

  • Stainless steel sheet with excellent fatigue characteristic and low surface contact electric resistance, and its manufacturing method

    JP2005029827A

  • MARTENSITE-CONTAINING HIGH-Cr STEEL SHEET FOR ENERGIZING COMPONENT WITH IMPROVED CONDUCTIVITY AND SPRING CHARACTERISTICS, AND MANUFACTURING METHOD THEREFOR