Production of acrolein or acrylic acid with high yield and low impurities from allyl alcohol
A two-step process using Mo-Bi and Mo-V mixed metal oxide catalysts efficiently converts allyl alcohol to acrolein and acrylic acid with minimal by-products, addressing the challenges of high by-product formation and fossil fuel reliance, achieving high yields and sustainable production.
Patent Information
- Application Number
- JP2022514687
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-18
- Filing Date
- 2020-09-10
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-10
AI Technical Summary
Existing processes for producing acrylic acid from allyl alcohol face challenges such as high by-product formation, particularly propionic acid, which is difficult to separate due to similar boiling points, and the reliance on fossil fuel-based feedstocks, with a need for more efficient and biomass-derived methods.
A two-step process using mixed metal oxide catalysts, first converting allyl alcohol to acrolein over a Mo-Bi catalyst and then to acrylic acid over a Mo-V catalyst, with optional additional elements, in the gas phase with oxygen presence, minimizing by-products like propionaldehyde and propionic acid.
Achieves high yields of acrolein and acrylic acid (>80%) with minimal by-products, utilizing biomass-derived allyl alcohol and reducing the mass ratio of propionic acid to acrylic acid to less than 0.001, facilitating efficient separation and production from renewable resources.
Smart Images

Figure 0007568715000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for the selective oxidation of allyl alcohol to produce acrolein, and further to a process for the selective oxidation of the produced acrolein to produce acrylic acid. [Background technology]
[0002] Various processes for preparing acrylic acid are readily known in the art. Most commercial acrylic acid is produced using fossil fuel based feedstocks such as propylene.
[0003] Acrylic acid can also be made from other starting materials, such as allyl alcohol. However, most commercially available allyl alcohol is also made from fossil fuel-based feedstocks. For example, allyl alcohol can be produced from the saponification of allyl chloride obtained by chlorination of propylene. Alternatively, allyl alcohol can be produced by hydrolysis of allyl acetate from the acetoxylation of propylene with acetic acid in the presence of oxygen. In particular, both of these processes require the use of propylene to form allyl alcohol. Therefore, it is economically more favorable to produce acrylic acid directly from propylene than to use allyl alcohol.
[0004] Allyl alcohol can also be produced from biomass-derived feedstocks such as glycerol, 1,2-propanediol, or 1,3-propanediol.
[0005] Mannan and Sekar disclose that allyl alcohol can be easily oxidized to acrylic acid with high efficiency in the liquid phase at room temperature using anhydrous tert-butyl hydroxide in the presence of CuCl catalyst (Mannan and Sekar, Tetra. Lett., 49, 2457 (2008)). A yield of acrylic acid of 75% was reported.
[0006] The oxidation of allyl alcohol to produce acrylic acid using manganese dioxide was reported in about 80% yield. Fatiadi, Syntheses 1976, 65.
[0007] Allyl alcohol has also been oxidized in the gas phase over supported metal catalysts. For example, U.S. Patents 4,051,181, 4,107,204, and 4,144,398 reported the use of bimetallic catalysts containing palladium and a second metal selected from copper or silver. The selectivity for the combined acrylic acid and acrolein reached a constant percentage below the 80s, while the by-products propionaldehyde and propionic acid exceeded 5%.
[0008] EP 3015448 and Kim and Lee, Sustainable Chem. Eng. 5, 11371 (2017) disclose the oxidation of allyl alcohol to acrylic acid using gold supported on ceria in the liquid phase. The large amount of 3-hydroxypropionic acid by-product required an additional dehydration step to reduce yield loss.
[0009] Japanese Patent Application Publication No. JP 2008-162907 and US Patent Application Publication No. 2018 / 0215696 disclose the gas-phase oxidation of allyl alcohol to acrylic acid over a molybdenum / vanadium mixed oxide catalyst. Acrylic acid was produced directly from allyl alcohol, and large amounts of propionic acid were produced. The mass ratio of propionic acid to acrylic acid ranged from 0.014 to 0.85.
[0010] Due to the small difference in boiling points between propionic acid and acrylic acid, removal of propionic acid from acrylic acid by distillation is very difficult, therefore it is desirable to minimize the formation of by-products such as propionic acid.
[0011] It is further desirable to produce acrolein and acrylic acid from biomass-derived feedstocks.
[0012] A need exists for more efficient processes that address one or more of these challenges. Summary of the Invention
[0013] The present invention relates to a process for preparing acrolein from allyl alcohol, and further to a process for producing acrylic acid from acrolein.
[0014] According to one aspect of the invention, a method includes selectively oxidizing allyl alcohol over a first mixed metal oxide catalyst in the presence of oxygen in a gas phase to produce acrolein, the first mixed metal oxide catalyst comprising oxides of molybdenum and bismuth.
[0015] Another embodiment of the invention further comprises selectively oxidizing acrolein over a second mixed metal oxide catalyst in the presence of oxygen in the gas phase, the second mixed metal oxide catalyst having a different composition than the first mixed metal oxide catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] As used herein, the terms "a", "an", "the", "at least one", and "one or more" are used interchangeably. The terms "comprise", "include", "contain" and variations thereof do not have a limiting meaning when these terms appear in the present specification and claims. That is, for example, a mixture containing a polymerization inhibitor can be interpreted to mean that the mixture contains at least one polymerization inhibitor.
[0017] As used herein, the recitation of numerical ranges by endpoints includes all numbers contained within that range (e.g., 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc.). For purposes of the present invention, it is to be understood that numerical ranges are intended to include and support all possible subranges contained within the range, consistent with what one of skill in the art would understand. For example, the range 1 to 100 is intended to convey 1.1 to 100, 1 to 99.99, 1.01 to 99.99, 40 to 6, 1 to 55, etc.
[0018] As used herein, numerical ranges and / or recitations of values, including such recitations in the claims, may be read as including the term "about." In such cases, the term "about" refers to numerical ranges and / or values that are substantially the same as those recited herein.
[0019] Unless stated to the contrary or implicit from the context, all parts and percentages are by weight and all test methods are as of the filing date of this application. For purposes of United States patent practice, the contents of any referenced patent, patent application, or published specification are incorporated by reference in their entirety, or the equivalent United States version thereof, particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure), and general knowledge in the art.
[0020] One aspect of the present invention relates to a method for producing acrolein from allyl alcohol.
[0021] In the process of the present invention, allyl alcohol is selectively oxidized in the presence of oxygen in the gas phase over a first mixed metal oxide catalyst.
[0022] The first mixed metal oxide catalyst is a solid catalyst comprising oxides of molybdenum (Mo) and bismuth (Bi). The first mixed metal oxide catalyst may also comprise at least one additional element selected from iron (Fe), cobalt (Co), nickel (Ni), or a combination thereof. When the first mixed metal oxide catalyst comprises at least one additional element, molybdenum and bismuth are the main metal elements present. Preferably, the first mixed metal oxide catalyst comprises at least 40 wt%, for example at least 50 wt%, at least 60 wt%, or at least 70 wt%, molybdenum and bismuth, based on the total weight of the metals in the first mixed metal oxide catalyst.
[0023] The first mixed metal oxide catalyst can be any commercially available catalyst used in the oxidation of propylene to acrolein.
[0024] The yield of acrolein based on the allyl alcohol feed is preferably greater than 80% and the mass ratio of the reaction by-product propionaldehyde to acrolein is preferably less than 0.001.
[0025] Another aspect of the present invention relates to the production of acrylic acid from allyl alcohol. The process of the present invention for producing acrylic acid from allyl alcohol is a two-step process. In the first step, allyl alcohol is selectively oxidized over a first mixed metal oxide catalyst to form acrolein, as described above.
[0026] Then, in a second step, acrolein is selectively oxidized in the presence of oxygen in the gas phase over a second mixed metal oxide catalyst, the second mixed metal oxide catalyst having a different composition than the first mixed metal oxide catalyst.
[0027] The second mixed metal oxide catalyst is a solid catalyst comprising oxides of molybdenum (Mo) and vanadium (V). The second mixed metal oxide catalyst may also comprise at least one additional element selected from tungsten (W), copper (Cu), iron (Fe), antimony (Sb), and phosphorus (P). When the second mixed metal oxide catalyst comprises at least one additional element, molybdenum and vanadium are the main metal elements present. Preferably, the second mixed metal oxide catalyst comprises at least 40 wt%, for example at least 50 wt%, at least 60 wt%, or at least 70 wt%, molybdenum and vanadium, based on the total weight of the metals in the second mixed metal oxide catalyst.
[0028] The second mixed metal oxide catalyst can be any commercially available mixed metal oxide catalyst used in the oxidation of acrolein to acrylic acid.
[0029] The yield of acrylic acid based on allyl alcohol feed is preferably greater than 80% and the weight ratio of the reaction by-product propionic acid to acrylic acid is preferably less than 0.001.
[0030] In the selective oxidation reaction to form acrolein and / or acrylic acid, oxygen can be present in the form of purified oxygen, oxygen in air, or lattice oxygen of a mixed metal oxide catalyst. Preferably, the oxygen is from air or lattice oxygen of a mixed metal oxide catalyst.
[0031] In either the selective oxidation of allyl alcohol to produce acrolein or the selective oxidation of acrolein to produce acrylic acid, steam can be added to aid the reaction.
[0032] Purification of the acrolein and / or acrylic acid can be accomplished by one or more techniques readily known in the art, such as, for example, absorption using water or organic solvents, extraction, fractional distillation, or melt crystallization.
[0033] Preferably, allyl alcohol is produced from a biomass-derived feedstock. For example, allyl alcohol can be produced from a biomass-derived feedstock such as glycerol, 1,2-propanediol, or 1,3-propanediol.
[0034] All living organisms, plants and animals alike, require a certain amount of carbon-14( 14 C), which is produced in the atmosphere and fixed by plants during photosynthesis. 14 C vs. 12 The ratio of C is 1 to 1.5x10 -12 Carbon-14 is a radioactive substance with a half-life of about 5,700 years. Therefore, biomass-derived materials have the same carbon content as living organisms. 14 C vs. 12 C ratio, i.e., about 1 to 1.5x10 -12 Includes:
[0035] Preferably, the acrolein and / or acrylic acid produced by the process of the present invention is at least 0.5x10 -13 of 14 C: 12 More preferably, the acrolein and / or acrylic acid produced by the process of the present invention has a ratio of at least 0.75x10 -13 of 14 C: 12 Even more preferably, the acrolein and / or acrylic acid produced by the process of the present invention has a ratio of at least 0.8x10 -13 of 14 C: 12 Most preferably, the feedstock used in the process of the present invention is sourced entirely from biomass-derived materials, 14 C vs. 12 The ratio of C is the same as that found in nature, i.e., about 1 to 1.5x10 -12 It is. EXAMPLES
[0036] The following examples illustrate the present invention but are not intended to limit the scope of the invention.
[0037] Example 1 - Oxidation of allyl alcohol to acrylic acid in two steps involving different catalysts The oxidation of allyl alcohol to acrylic acid was carried out in two stages. First, allyl alcohol was oxidized to mainly acrolein in a first stage reactor, in this case a tubular reactor, which is similar to the first stage of a two-stage propylene oxidation process to produce acrylic acid. The catalyst used in the first stage reactor was a Mo, Bi-based mixed oxide catalyst, abbreviated as R1 catalyst. In this example, 15 ml (15.1 grams) of Mo and Bi-based R1 catalyst from Nippon Kayaku Co. (Tokyo, Japan) was mixed with 15 ml of 1 / 8 inch Denstone™ 57 beads (Saint-Gobain Norpro, Stow, OH) and then loaded into a 2.54 cm (1 inch) outside diameter (OD) stainless steel (SS) first stage tubular reactor (0.834 inch ID).
[0038] The product mixture from the first stage reactor, abbreviated as R1-Discharge, was sent to the second stage reactor in a 1 / 4 inch SS tube heated by an electric heating tape. The surface temperature was controlled at about 170±10°C.
[0039] The second stage reactor contained a Mo, V-based mixed oxide catalyst, abbreviated as R2 catalyst. In this example, 15 ml (15.84 grams) of Mo, V-based commercial R2 catalyst from Nippon Kayaku Co., Tokyo, Japan, was mixed with 15 ml of 1 / 8 inch Denstone™ beads. The mixture was loaded into the feed inlet side of a U-shaped SS tube with 1 inch OD and 0.834 inch OD. The other inner space of the U-tube was filled with Denstone™ beads. The U-tube was placed in a fluidized sand bath furnace and the catalyst bed was immersed in the sand bath. Air was used to fluidize the sand at a flow rate of 3.3-3.5 SCFM (standard cubic feet per minute). The temperature difference in the bath was controlled to less than 3°C by maintaining a high air flow rate. The bath temperature was adjusted to achieve the desired conversion of acrolein to acrylic acid. The effluent from the second stage reactor was designated as R2-effluent.
[0040] First, the reactor tube was heated to above 300 °C in a clamshell-type electric furnace with a N2 flow rate of 35.4 ml / min. Then, 208.3 ml / min of air was added. All gas flow values were under standard temperature (0 °C) and pressure (101.3 kPa) conditions. Allyl alcohol was obtained from Sigma Aldrich with an assay of greater than 99%. Allyl alcohol was mixed with deionized water (54.2 wt% of allyl alcohol) and injected into the SS mixer vessel at a rate of 0.114 ml / min when the reactor reached the desired temperature. The residence time of the reactants on the catalyst bed was approximately 2.7 seconds. The SS mixer vessel was heated to 160-170 °C, and the steam was carried to the reactor by air inlet.
[0041] The R2-effluent was collected and analyzed. The R2-effluent was first passed through trap 1, a 100-500 ml stainless steel container wrapped in a 1 / 4 inch copper coil connected to a recirculating chiller set at 0-1 °C. Gas escaping trap 1 passed through trap 2, a second trap immersed in water / ice, and the third and fourth traps (traps 3A and 3B) immersed in a dry ice / isopropanol mixture. Trap 2 served primarily as a protective trap to prevent large amounts of water or acrylic acid from entering the dry ice / isopropanol trap, as water / AA could freeze in the dry ice / isopropanol trap and cause an increase in pressure. Trap collection times were typically 2-4 hours. To prevent polymer formation, 6-12 grams of inhibitor solution was injected into traps 2, 3A, and 3B prior to sample collection. Trap 2 collected only small amounts of material in most cases. 0.2 wt% hydroquinone in isopropanol was used as the inhibitor solution.
[0042] The off-gas from the dry ice / isopropanol trap was analyzed online by a GC equipped with a thermal conductivity detector and a 5 Å molecular sieve / silica gel column. The main gas components of the off-gas typically included nitrogen, oxygen, unreacted propylene, carbon monoxide, and carbon dioxide. The liquids collected from trap 1 and trap 2 (if present) were combined into one sample, labeled as the T-1 sample. The liquids collected from trap 3A and trap 3B were labeled as the T-3A and T-3B samples, respectively. The T-1, T-3A, and T-3B samples were sent for offline analysis by a GC equipped with a flame ionization detector and a capillary column (DB-FFAP 123-3232E). The propylene conversion and carbon mass balance were calculated using the following equations: Propylene conversion (%) = (moles of propylene fed - R2 - moles of propylene in discharge) / moles of propylene fed Carbon mass balance (%) = (total amount of carbon from molecules in R2-emission including CO2, CO, propylene, formaldehyde, acetaldehyde, acrolein, acetic acid, propionic acid, and acrylic acid) / (total amount of carbon from propylene fed)*100
[0043] Acrylic acid, acrolein, acetaldehyde, propionaldehyde, propionic acid, acetic acid, CO after the second stage reactor x The yields of major products or by-products such as (CO and CO2) were calculated using the following formula: Product yield (%) = (R2 - moles of product in discharge) / moles of propylene fed * 100 If an empty tube is used as the R2 reactor, the R2-output is equal to the R1-output.
[0044] Tests were conducted at two different reactor temperatures (330 and 340 °C) in the first stage. The peak temperature (PT) of the first stage catalyst bed was 30-40 °C higher than the reactor temperature (RT). The bath temperature (RT) of the second stage reactor was maintained at 310 °C. The results are listed in Table 1. The carbon mass balance was adjusted to 100% by adjusting the yield of acrylic acid. The yield of acrylic acid was above 83% due to the almost complete conversion of allyl alcohol. The yield of propionic acid was very low at about 0.02-0.03%, resulting in a mass ratio of PA / AA below 0.00036.
[0045] [Table 1]
[0046] The oxidation of allyl alcohol was carried out in one step over Mo, V-based oxide catalysts. The experiment was similar to Example 1, except that the first-stage reactor tube was empty. Allyl alcohol was directly oxidized over the commercial R2 catalyst from NK, which contains Mo and V as the main components.
[0047] The tests were carried out at two different bath temperatures in the second stage reactor (287 and 335°C). Acrolein was formed along with propionaldehyde at low temperatures in addition to acrylic acid. Acrylic acid became the main product at higher reaction temperatures. The yield of AA reached almost 71% with a 95.7% conversion of allyl alcohol at a reactor temperature of 335°C. However, the AA yield (70.9%) was much lower compared to Example 1 (83.6%). Moreover, in this case, the mass ratio of PA / AA was 0.01, about 30 times that of Example 1.
[0048] The results are similar to those reported in US Patent Application Publication No. 2018 / 0215696, a mixed oxide containing Mo and V with Fe as an optional component. AA yields of up to 78.8% were reported at a high PA / AA mass ratio of 0.014 when allyl alcohol was completely converted.
[0049] Example 2 - Oxidation of Allyl Alcohol to Acrolein Allyl alcohol can be primarily oxidized to acrolein over Mo, Bi-based oxide catalysts. The experiment was similar to Example 1, except that no second stage reaction occurred after the first stage reactor.
[0050] The R1-effluent was collected and analyzed similarly to the collection and analysis of the R2-effluent in Example 1.
[0051] The test results are shown in Table 1. The acrolein yield was adjusted to obtain a carbon mass balance of 100%. Acrolein could be obtained in high yields up to 86% from allyl alcohol oxidation over the R1 catalyst. Higher reaction temperatures were preferred to limit the by-product propionaldehyde.
Claims
1. A process for producing acrolein by selectively oxidizing allyl alcohol over a first mixed metal oxide catalyst in the presence of oxygen in a gas phase; selectively oxidizing the acrolein over a second mixed metal oxide catalyst in the presence of oxygen in a gas phase; the first mixed metal oxide catalyst comprises oxides of molybdenum and bismuth; The method wherein the second mixed metal oxide catalyst has a different composition than the first mixed metal oxide catalyst.
2. The method of claim 1 , wherein the second mixed metal oxide catalyst comprises oxides of molybdenum and vanadium.
3. 3. The method of claim 2, wherein the second mixed metal oxide catalyst further comprises at least one additional element selected from the group consisting of tungsten, copper, iron, antimony, and phosphorus.
4. The method of any one of claims 1 to 3, wherein the first mixed metal oxide catalyst further comprises at least one additional element selected from the group consisting of iron, cobalt, and nickel.
5. A method according to any one of claims 1 to 4, wherein the oxygen is present in the form of purified oxygen, air, or lattice oxygen of the mixed metal oxide.
6. 6. The method of any one of claims 1 to 5, wherein the allyl alcohol is produced from a biomass-derived feedstock selected from glycerol, 1,2-propanediol, and 1,3-propanediol.
7. The acrolein is at least 0.5×10 -13 of 14 C: 12 The method according to any one of claims 1 to 6, having a ratio of C.
8. The method according to any one of claims 1 to 7, wherein the mass ratio of propionic acid to acrylic acid is less than 0.
001.
9. A process for producing acrolein comprising selectively oxidizing allyl alcohol to acrolein over a first mixed metal oxide catalyst in the presence of oxygen in a gas phase; the first mixed metal oxide catalyst comprises oxides of molybdenum and bismuth; The method, wherein the allyl alcohol is produced from a biomass-derived feedstock selected from glycerol, 1,2-propanediol, and 1,3-propanediol.
10. The method of claim 9, wherein the mass ratio of propionaldehyde to acrolein is less than 0.001.
Citation Information
Patent Citations
Method for producing acrylic acid, acrylonitrile and 1,4-butanediol from 1,3-propanediol
JP2016534131A