Polyamide industrial yarn, its manufacturing method and applications
Polyamide 5X yarn, produced by polymerizing 1,5-pentanediamine and linear aliphatic dibasic acids, addresses the issues of high water absorption and variable dimensional stability in existing yarns, offering improved strength and stability for industrial applications.
Patent Information
- Application Number
- JP2022548717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing high-strength industrial yarns, such as polyamide 6 and polyamide 66, suffer from high water absorption and variable dimensional stability, leading to deformation and poor performance in applications like tire cords and conveyor belts.
Manufacture polyamide industrial yarns using polyamide 5X, produced from polymerizing 1,5-pentanediamine and linear aliphatic dibasic acids, through a process involving melting, drawing, heat treatments, and multi-stage stretching to achieve low water absorption and excellent dimensional stability.
The resulting polyamide 5X yarn exhibits low water absorption, high breaking strength, good heat resistance, and improved dimensional stability, suitable for applications like tire cords and conveyor belts.
Smart Images

Figure 0007568730000001 
Figure 0007568730000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to industrial yarns, and in particular to polyamide industrial yarns that have low water absorption and good dimensional stability. [Background technology]
[0002] High-strength yarns made of Tetoron or nylon have characteristics such as high strength, low elongation, excellent dimensional stability, fatigue resistance and aging resistance, and are therefore widely used in fields such as tire cords, canvas, conveyor belts, airbags, parachutes, ropes, seat belts, industrial filter cloths and tents.
[0003] There are two processes for producing high-strength yarn: one uses direct spinning through thickening of the melt, and the other uses indirect spinning through solid-state thickening of the pieces.
[0004] At present, high-strength industrial yarns include polyester, polyamide 6 and polyamide 66, but polyester industrial yarns have poor abrasion resistance and poor adhesion to rubber.Polyamide 6 and polyamide 66 have high water absorption, so the polyamide industrial yarns produced therefrom have high moisture content, are prone to water absorption and deformation in subsequent applications, and have large variations in dimensional stability. Summary of the Invention [Problem to be solved by the invention]
[0005] The main object of the present disclosure is to provide a high-strength industrial polyamide yarn having low water absorption, excellent dimensional stability, and good heat resistance, the raw materials for which include at least 1,5-pentanediamine and a linear aliphatic dibasic acid, or polyamide 5X obtained by polymerizing 1,5-pentanediamine and a linear aliphatic dibasic acid as monomers. [Means for solving the problem]
[0006] An embodiment of the present disclosure further provides a method for producing a polyamide industrial yarn, the method comprising: (1) heating a raw material including a polyamide 5X resin until the raw material is in a molten state to form a melt; (2) drawing yarn from the melt to form an undrawn yarn; (3) subjecting the low-oriented yarn to a heat-retention treatment, a cooling treatment, an oiling treatment, a pre-interlacing treatment, a multi-stage drawing treatment, a main-interlacing treatment and a winding treatment to produce the polyamide industrial yarn, and performing a tension heat-setting treatment or a relaxation heat-setting treatment in any one of the drawing stages of the multi-stage drawing treatment.
[0007] An embodiment of the present disclosure further provides for the use of said polyamide industrial yarn in sewing thread, tire cord, airbag yarn, release cloth, water cloth, canvas, seat belt, rope, fishing net, industrial filtration cloth, conveyor belt, parachute, tent or box bag. Effect of the Invention
[0008] The polyamide industrial yarn according to one embodiment of the present disclosure is characterized by low water absorption, excellent dimensional stability, high breaking strength, and good heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Representative embodiments for embodying the features and advantages of the present invention are described in detail in the following description. It should be understood that the present disclosure can be modified in various ways in different embodiments, without departing from the scope of the present disclosure. The description is illustrative in nature, and is not intended to limit the present disclosure.
[0010] One embodiment of the present disclosure provides an industrial yarn, the raw material for production of which includes at least 1,5-pentanediamine and a linear aliphatic dibasic acid, or polyamide 5X obtained by polymerizing 1,5-pentanediamine and a linear aliphatic dibasic acid as monomers.
[0011] In one embodiment, the straight chain aliphatic diacid contains 6 to 18, for example, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 carbon atoms. In one embodiment, the straight chain aliphatic diacid may be a saturated diacid. In one embodiment, the straight chain aliphatic diacid may contain one carbon-carbon double bond.
[0012] In one embodiment, the straight chain aliphatic diacid may be one or more of adipic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, Δ9-1,18 octadecenedioic acid.
[0013] In one embodiment, the straight chain aliphatic diacid may be one or more of sebacic acid, undecanedioic acid, dodecanedioic acid.
[0014] In one embodiment, 1,5-pentanediamine and / or linear aliphatic diacids can be produced by fermentation or enzymatic conversion processes.
[0015] According to one embodiment of the present disclosure, the industrial yarn comprises polyamide 5X and is also referred to as polyamide 5X industrial yarn. In one embodiment, the polyamide 5X industrial yarn comprises one or more of polyamide 56, polyamide 510, polyamide 511, polyamide 512, polyamide 513, polyamide 514, polyamide 515, polyamide 516, polyamide 517, and polyamide 518. In one embodiment, the polyamide 5X industrial yarn comprises one or more of polyamide 510, polyamide 511, polyamide 512.
[0016] In one embodiment, the moisture regain of the polyamide 5X industrial yarn is ≦2.2%, furthermore ≦2.1%, furthermore ≦1.9%, such as 0.9%, 1.5%, 1.8%, 2.0%, etc. In one embodiment, the moisture regain of the polyamide 5X industrial yarn may be 0.9-2.2%.
[0017] In one embodiment, the breaking strength of the polyamide 5X industrial yarn is 7.5 to 9.5 cN / dtex, and may further be 7.8 to 9.0 cN / dtex, and may further be 8.0 to 8.5 cN / dtex, such as 7.9 cN / dtex, 8.1 cN / dtex, 8.2 cN / dtex, 8.3 cN / dtex, 8.4 cN / dtex, etc.
[0018] In one embodiment, the polyamide 5X industrial yarn has a heat tenacity retention of ≧85%, or even ≧88%, or even ≧92%, such as 90%, 91%, 92%, 93%, 94%, 95%, etc., after being heat treated at 160° C. for 4 hours. In one embodiment, the heat tenacity retention of the polyamide 5X industrial yarn is 85-95%. In one embodiment, the polyamide 5X industrial yarn has a heat tenacity retention rate of 85-95% after being heat treated at 160° C. for 4 hours.
[0019] In one embodiment, the polyamide 5X industrial yarn has a breaking strength retention after humidity conditioning of ≧92%, or even ≧94%, or even ≧96%, indicating that the polyamide 5X industrial yarn has low water absorption and high breaking strength retention.
[0020] In one embodiment, the breaking elongation of the polyamide 5X industrial yarn is 16-24%, and may further be 18-22%, and may further be 19-21%, such as 19.5%, 20%, 20.5%, etc.
[0021] In one embodiment, the modulus of the polyamide 5X industrial yarn is ≧35 cN / dtex, and may even be ≧38 cN / dtex, and even more ≧42 cN / dtex, such as 42.5 cN / dtex, 43 cN / dtex, 43.5 cN / dtex, 44 cN / dtex, 44.5 cN / dtex, 45 cN / dtex, 45.5 cN / dtex, 46 cN / dtex, 46.5 cN / dtex, 47 cN / dtex, 47.5 cN / dtex, 48 cN / dtex, etc. In one embodiment, the modulus of the polyamide 5X industrial yarn is between 35 and 50 cN / dtex.
[0022] In one embodiment, the dry heat shrinkage of the polyamide 5X industrial yarn is ≦10.0%, or even ≦8.0%, or even ≦6.0%, such as 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, etc. In one embodiment, the dry heat shrinkage of the polyamide 5X industrial yarn is 6.0 to 10.0%.
[0023] In one embodiment, the boiling water shrinkage of the polyamide 5X industrial yarn is ≦9.0%, or even ≦8.0%, or even ≦7.0%, such as 6.0%, 6.2%, 6.5%, 6.8%, 7.0%, 7.5%, 7.9%, etc. In one embodiment, the boiling water shrinkage of the polyamide 5X industrial yarn is 6.0 to 9.0%.
[0024] In one embodiment, the polyamide 5X industrial yarn has an elongation after boiling water treatment of ≦25.0%, such as 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, etc. In one embodiment, the polyamide 5X industrial yarn has an elongation after boiling water treatment of 20 to 25%.
[0025] In one embodiment, the number of single yarn breaks of the polyamide 5X industrial yarn is ≦5 / 24h, furthermore ≦3 / 24h, furthermore ≦2 / 24h, for example ≦4 / 24h. In one embodiment, the number of single yarn breakages of the polyamide 5X industrial yarn is 2 to 5 breakages / 24 hours.
[0026] In one embodiment, the broken filaments of the polyamide 5X industrial yarn are ≦10 / 1 bobbin (10 kg winding), and can also be ≦8 / 1 bobbin, and even more can be ≦5 / 1 bobbin, such as 2 / 1 bobbin, 3 / 1 bobbin, 4 / 1 bobbin, 5 / 1 bobbin, 7 / 1 bobbin, etc.
[0027] In one embodiment, the filament breakage of the polyamide 5X industrial yarn is 2-10 pieces / bobbin.
[0028] In one embodiment, the retention of the polyamide 5X industrial yarn is ≧90%, and may even be ≧93%, and even more so ≧95%, such as 96%, 97%, 98%, etc.
[0029] In one embodiment, polyamide 5X industrial yarn is produced by a spinning process from a spinning feedstock comprising polyamide 5X resin.
[0030] In one embodiment, the relative viscosity of the polyamide 5X resin to 96% sulfuric acid is 2.8 to 4.0, and may further be 3.0 to 3.7, or may further be 3.3 to 3.6, for example, 2.9, 3.1, 3.2, 3.4, 3.5, 3.8, 3.9, or the like. In one embodiment, the polyamide 5X resin includes an additive.
[0031] In one embodiment, polyamide 5X resin is produced from 1,5-pentanediamine and a linear aliphatic diacid. The process used may be conventional.
[0032] In one embodiment, a method for preparing a polyamide 5X resin includes first mixing 1,5-pentanediamine, a linear aliphatic diacid and water to prepare a salt solution of polyamide 5X, and then subjecting the resulting polyamide 5X salt solution to polycondensation and dehydration to obtain a polyamide 5X resin.
[0033] In one embodiment, a method for producing a polyamide 5X resin includes the steps of: S1: uniformly mixing 1,5-pentanediamine, linear aliphatic dibasic acid and water to prepare a salt solution of polyamide 5X, where the molar ratio of 1,5-pentanediamine to linear aliphatic dibasic acid is (1-1.05):1; S2: Heating the salt solution of polyamide 5X to carry out a polymerization reaction to obtain polyamide 5X.
[0034] In one embodiment, step S2 includes steps of heating a salt solution of polyamide 5X, increasing the pressure in the reaction system to 0.3 to 2.5 MPa, evacuating, maintaining the pressure, setting the temperature of the reaction system at the end of maintaining the pressure to 232 to 265°C, further reducing the pressure in the reaction system to 0 to 0.2 MPa (gauge pressure) and maintaining this for 5 to 30 minutes, setting the temperature of the reaction system after the reduction in pressure to 245 to 280°C, and drawing a vacuum.
[0035] In one embodiment, additives may be added in one or more of steps S1 and S2 above, and may be added in step S1 or before heating and carrying out the polymerization reaction in step S2.
[0036] In one embodiment, the additive comprises a thermal stabilizer and / or a second additive, and the thermal stabilizer comprises one or more of copper acetate, potassium iodide, copper chloride, cuprous iodide, copper oxide, and cuprous oxide.
[0037] In one embodiment, the amount of the heat stabilizer added is 20 to 3000 ppm, preferably 80 to 2500 ppm, and more preferably 200 to 2200 ppm, of the total weight of the polyamide 5X salt produced by the reaction of 1,5-pentanediamine with a linear aliphatic dibasic acid.
[0038] In one embodiment, the heat stabilizer includes copper acetate and potassium iodide, and the molar ratio of copper acetate to potassium iodide is 1:(1-15), and may further be 1:(5-13), such as 1:6, 1:8, 1:10, 1:12, etc.
[0039] In one embodiment, the second additive may include one or more of a matting agent, a flame retardant, an antioxidant, an ultraviolet absorber, an infrared absorber, a crystal nucleating agent, an optical brightener, and an antistatic agent. In one embodiment, the second additive comprises an antioxidant and / or a nucleating agent.
[0040] In one embodiment, the antioxidant may include one, two or more of antioxidant 1010, antioxidant 1076, antioxidant TPP, antioxidant TNP, antioxidant 164, antioxidant DNP, sodium hypophosphite, calcium hypophosphite.
[0041] In one embodiment, the nucleating agent may include one or more of nano-montmorillonite, nano-talc, nano-SiO2, nano-Al2O3, nano-ZrO2, nano-TiO2, nano-P200.
[0042] In one embodiment, the amount of the second additive added is 0 to 1000 ppm, for example 1 ppm, 5 ppm, 10 ppm, 50 ppm, 100 ppm, 200 ppm, 500 ppm, 800 ppm, etc., of the total weight of the polyamide 5X salt produced by the reaction of 1,5-pentanediamine with a linear aliphatic dibasic acid.
[0043] One embodiment of the present disclosure provides a method for producing the above polyamide 5X industrial yarn, said method comprising: (1) heating a spinning material including a polyamide 5X resin until the material is in a molten state to form a melt; (2) conveying the melt through a melt conduit to a spinning box and drawing yarn to form a low-oriented yarn; (3) The low-oriented yarn is subjected to heat retention, cooling, oiling, pre-interlacing, multi-stage drawing, main interlacing, and winding to obtain polyamide 5X industrial yarn, and a tension heat-setting process or a relaxation heat-setting process is performed in any one of the drawing stages of the multi-stage drawing.
[0044] In one embodiment, the polyamide 5X resin in step (1) is a high-viscosity polyamide 5X resin, and the relative viscosity of the high-viscosity polyamide 5X resin to 96% sulfuric acid is 2.8 to 4.0, and may further be 3.0 to 3.7, and may further be 3.3 to 3.6, for example, 2.9, 3.1, 3.2, 3.4, 3.5, 3.8, 3.9, etc.
[0045] In one embodiment, by adding an additive to the polyamide 5X resin, copper ions are contained in the spinning raw material, and the content of copper ions is 0 to 300 ppm, and may further be 30 to 200 ppm, and may further be 50 to 100 ppm, and the above content is based on the total weight of the high-viscosity polyamide 5X resin.
[0046] In one embodiment, the water content of the high-viscosity polyamide 5X resin is 100 to 1000 ppm, may be 200 to 800 ppm, may be 400 to 600 ppm, for example, 150 ppm, 300 ppm, 350 ppm, 500 ppm, 550 ppm, 700 ppm, 900 ppm, etc. By maintaining the water content of the high-viscosity polyamide 5X resin within the above range, it is possible to prevent the melt from being decomposed during the manufacturing process of the industrial yarn, and thus the manufactured industrial yarn has high breaking strength, high modulus, small number of single yarn breaks and filament breaks, and high yield.
[0047] In one embodiment, a method for producing a high-viscosity polyamide 5X resin includes the steps of first subjecting a low-viscosity polyamide 5X resin having a relative viscosity of 2.2 to 2.7 to a high-temperature drying treatment to obtain a thickened polyamide 5X resin, and then subjecting the thickened polyamide 5X resin to a resin humidity adjustment treatment to obtain a high-viscosity polyamide 5X resin.
[0048] In one embodiment, the relative viscosity of the low-viscosity polyamide 5X resin to 96% sulfuric acid may be 2.2 to 2.7, or may be 2.4 to 2.6, for example, 2.3, 2.5, etc. In one embodiment, the high-temperature drying process is performed by evacuation (negative pressure state) or in an inert gas atmosphere, and the degree of vacuum during evacuation is −0.06 to −0.1 MPa, for example, −0.07 MPa, −0.08 MPa, or −0.09 MPa. In one embodiment, the temperature in the high-temperature drying treatment is 130 to 160°C, and may further be 140 to 150°C, for example, 135°C, 145°C, 155°C, and the like.
[0049] In one embodiment, the time for the high-temperature drying treatment is 10 to 25 hours, and may further be 15 to 20 hours, for example, 12 hours, 16 hours, 18 hours, 22 hours, or 24 hours. In one embodiment, the high temperature drying equipment is a vacuum drum dryer or a continuous dehumidifying thermal nitrogen gas dryer.
[0050] In one embodiment, the temperature in the resin moisture conditioning treatment is 85 to 110°C, for example, 90°C, 95°C, 100°C, 105°C, and the like.
[0051] In one embodiment, nitrogen gas and water vapor are mixed to perform resin moisture conditioning treatment, and the dew point of the nitrogen gas is controlled in the range of -15 to 15°C, for example, -12°C, -10°C, -8°C, -5°C, 0°C, 2°C, 5°C, 8°C, 10°C, 12°C, etc.
[0052] In one embodiment, in step (1), heating is performed using a screw extruder, which is divided into five zones for heating, the temperature of the first zone being 220 to 250°C, e.g., 225°C, 230°C, 235°C, 240°C, 245°C, etc., and the temperature of the second zone being 230 to 260°C, e.g., 235°C, 240°C, 245°C, 250°C, 255°C, etc. the temperature of the third zone is 240 to 270°C, for example, 245°C, 250°C, 255°C, 260°C, 265°C, etc.; the temperature of the fourth zone is 250 to 280°C, for example, 255°C, 260°C, 265°C, 270°C, 275°C, etc.; and the temperature of the fifth zone is 260 to 290°C, for example, 265°C, 270°C, 275°C, 280°C, 285°C, etc.
[0053] In one embodiment, the threading in step (2) comprises discharging the melt obtained in step (1) through a spinneret of a spinning box to obtain a low-oriented thread. In one embodiment, the temperature of the spinning box is from 260 to 290°C, and may further be from 270 to 285°C, and may further be from 275 to 280°C. In one embodiment, the pressure of the spin pack in the spin box is between 10 and 22 MPa, and may further be between 14 and 20 MPa, and may further be between 17 and 18 MPa.
[0054] In one embodiment, in step (3), the heat retention treatment is performed by an annealing device, and the annealing height may be 100 to 300 mm, and may further be 200 to 250 mm, for example, 120 mm, 150 mm, 220 mm, 230 mm, 240 mm, etc. The annealing temperature may be 200 to 300°C, and may further be 230 to 280°C, for example, 210°C, 240°C, 250°C, 260°C, 270°C, etc.
[0055] In one embodiment, the cooling treatment in step (3) is performed by wind-cooling using a side air blow or a ring air blow, the wind speed in the wind-cooling may be 0.5 to 0.9 m / s, and may also be 0.6 to 0.8 m / s, the air temperature in the wind-cooling may be 16 to 23°C, and may also be 18 to 20°C, and the humidity in the wind-cooling may be 60 to 90%, and may also be 75 to 85%.
[0056] In one embodiment, the concentration of the oil used in the oiling in step (3) is 8 to 100 wt %. In one embodiment, the oil solution has a concentration of 100 wt% and is undiluted.
[0057] In one embodiment, the oil may be N-350 (provided by Matsumoto Yushi Seiyaku Co., Ltd.), N-353 (provided by Matsumoto Yushi Seiyaku Co., Ltd.), NEOTEX-903(A) (Shanghai Become chemical co., ltd), D-3088 (provided by Nantong Hengrun Chemical Industry Co., Ltd.), TCP-60 nylon industrial yarn / tire cord oil (provided by Tianjin University of Technology Spinning Auxiliaries Co., Ltd.), TCP-80 nylon industrial yarn / tire cord oil (provided by Tianjin University of Technology Spinning Auxiliaries Co., Ltd.), TC1152 (provided by Zschimmer & Schwarz), TC1355 (provided by Zschimmer & Schwarz), TC-14686 (GOULSTON TECHNOLOGIES, Inc., 700 North Johnson The polymer may be one or more selected from the group consisting of TC1355, TC-14686, TCP-60, and TCP-80.
[0058] In one embodiment, the concentration of the oil is 8 to 25 wt%, may further be 9 to 15 wt%, and may further be 10 to 12 wt%.
[0059] In one embodiment, the oiling may use one or two of the following oiling methods: an oiling nozzle, an oiling ring, and an oiling lip. In one embodiment, the oiling uses a combination oiling system of two oiling lips, one oiling ring and one oiling lip.
[0060] In one embodiment, the height of the oiling lip from the spinneret is ≧2.5 m, and may even be ≧3.0 m, and even more preferably ≧4.0 m. In one embodiment, the oiling rate may be 0.7 to 1.2%, further may be 0.8 to 1.1%, and further may be 0.9 to 1.0%.
[0061] In one embodiment, the pre-interlacing pressure in step (3) may be 1 to 2.5 bar, and may further be 1.5 to 2.0 bar.
[0062] In one embodiment, the drawing process in step (3) is as follows. Drawing is performed using four or more pairs of heat rolls, and may be performed in four stages using, for example, five pairs of heat rolls. In the drawing process, first, the low-oriented yarn after oiling is placed in the first pair of heat rolls, and the first stage of pre-drawing is performed between the first pair of heat rolls and the second pair of heat rolls, then the second stage of main drawing is performed between the second pair of heat rolls and the third pair of heat rolls, the third stage of main drawing and tension heat setting are performed between the third pair of heat rolls and the fourth pair of heat rolls, and then the fourth stage of secondary drawing and relaxation heat setting are performed between the fourth pair of heat rolls and the fifth pair of heat rolls.
[0063] In one embodiment, the magnitude of the speed contraction between the fourth pair of heat rolls and the fifth pair of heat rolls may be 30-100 m / min, and may even be 50-80 m / min, where "magnitude of contraction" refers to the difference in rotation speed between different heat rolls.
[0064] In one embodiment, the total draw ratio in the step (3) may be 4.5 to 6.0, and may further be 4.8 to 5.3.
[0065] In one embodiment, the temperature in tension heat setting may be 150 to 200°C, or may be 160 to 180°C, for example, 155°C, 165°C, 170°C, 175°C, 178°C, 190°C, or the like. In one embodiment, the temperature in the relaxation heat setting may be 100 to 160°C, or may be 120 to 140°C, for example, 110°C, 125°C, 130°C, 135°C, 138°C, 150°C, etc.
[0066] In one embodiment, the main interlacing pressure may be 2.5 to 4.0 bar, and may further be 3.0 to 3.5 bar.
[0067] In one embodiment, the winding speed may be 2000 to 3500 m / min, further 2300 to 3200 m / min, and even further 2600 to 2800 m / min, for example, 2500 m / min, 2700 m / min, 3000 m / min, etc.
[0068] An embodiment of the present disclosure provides the use of said polyamide 5X industrial yarn in sewing thread, tire cord, airbag thread, release cloth, water cloth, canvas, seat belt, rope, fishing net, industrial filter cloth, conveyor belt, parachute, tent or box bag field.
[0069] The raw materials for producing the high-viscosity polyamide 5X resin used in one embodiment of the present disclosure are produced by biological methods, and have a 100% bio-based content. They are green materials, so they do not depend on petroleum resources and do not cause serious pollution, and can reduce carbon dioxide emissions and reduce the greenhouse effect.
[0070] The polyamide 5X industrial yarn according to one embodiment of the present disclosure has a low number of single yarn breaks and filament breaks during the production process, high production efficiency, and low production costs.
[0071] The polyamide 5X industrial yarn according to one embodiment of the present disclosure can be produced by conventional polyamide 6 and polyamide 66 industrial yarn equipment, without the need to improve the spinning equipment. By optimizing the mass of high-viscosity polyamide 5X resin and the spinning process, the yield can be improved, the production cost can be reduced, and huge benefits can be brought to spinning enterprises.
[0072] The following is a detailed description of the polyamide 5X industrial yarn and its manufacturing method according to an embodiment of the present disclosure, with reference to specific examples. Unless otherwise specified, all raw materials used may be commercially available. The relevant performance parameters and measurement methods are as follows:
[0073] (1) Breaking strength: Measured according to GB / T14344-2008. (2) Modulus: Measured according to GB / T14344-2008. (3) Heat resistance retention rate: Retention rate of heat resistance strength = (breaking strength after heat treatment / breaking strength before heat treatment) x 100%, where the breaking strength is measured according to GB / T14344-2008. The heat treatment device is an oven, the oven temperature is 160°C, and the treatment time is 4h.
[0074] (4) Breaking strength retention after humidity conditioning treatment = (breaking strength after humidity conditioning treatment / breaking strength before humidity conditioning treatment) x 100%. Humidity conditioning treatment: The polyamide industrial yarn was placed in a temperature and humidity chamber at a temperature of 20°C and a relative humidity of 65%, and conditioned to equilibrium according to GB / T6529-2008. (5) Breaking elongation: Measured according to GB / T14344-2008.
[0075] (6) Dry heat shrinkage rate: The heat treatment was carried out according to the FZ / T50004 standard, with the heat treatment temperature set to 160°C and the time set to 2 minutes. (7) Moisture content: The moisture content is measured by drying the washed polyamide fiber in an oven in a loose state, and then placing the dried polyamide fiber sample in the standard atmosphere specified in GB / T6529 until it reaches equilibrium, and measuring the moisture content of the sample after humidity adjustment. The moisture content measurement is performed according to GB / T6503, where the oven drying temperature is 105°C and the sample is dried until it reaches a constant weight.
[0076] (8) Boiling water shrinkage rate: Here, the boiling water shrinkage was measured according to GB / 6505-2008. Specifically, a piece of industrial yarn sample was taken, and a tension of 0.05±0.005cN / dtex was applied in advance. Both ends of the industrial yarn were marked at a distance of 50.00 cm from the center, and the sample was wrapped in gauze and boiled in boiling water for 30 minutes. After that, the sample was dried, and the length between the two marks was measured, and the boiling water shrinkage was calculated according to the following formula: Boiling water shrinkage rate = ((initial length - length after shrinkage) / initial length) x 100%.
[0077] (9) Breaking elongation after boiling water treatment: After the industrial yarn was treated with boiling water for 30 min, the sample was dried and then its breaking elongation was measured according to (5) Breaking elongation, which was measured in accordance with GB / T14344-2008. (10) Moisture content: The measurement was performed using a Karl Fischer titrator.
[0078] (11) Relative Viscosity: The measurement was performed using a concentrated sulfuric acid method using an Ubbelohde viscometer, and the steps are as follows: 0.25±0.0002 g of a dried polyamide resin sample was accurately weighed, and 50 mL of concentrated sulfuric acid (96%) was added to dissolve it, and the time t0 at which the concentrated sulfuric acid flowed and the time t at which the polyamide resin solution flowed were measured and recorded in a thermostatic water bath at 25°C. The formula for calculating relative viscosity is VN=t / t0. t - time for solution to flow; t0 - time for solvent flow.
[0079] (12) Yarn breakage (number of times / 24 hours): The number of yarn breakages was manually counted during the process of obtaining polyamide 5X industrial yarn by performing heat retention, cooling, oiling, pre-interlacing, multi-stage drawing, main interlacing, and winding on low-oriented yarn. (13) Number of broken filaments: The number of broken filaments was measured using a fuzz detector during the process of winding 10 kg of industrial yarn.
[0080] (14) Yield: Yield = (weight of textile products produced / total weight of resin input) × 100%. (15) Measurement of dyeing uniformity: Measure according to FZ / T50008, and the dyeing temperature is 110-120°C.
[0081] Example 1 Polyamide 510 Industrial Yarn Manufacturing A low-viscosity polyamide 510 resin with a relative viscosity of 2.5 was subjected to high-temperature drying treatment to obtain a thickened polyamide 510 resin. Here, the high-temperature drying was performed by evacuation, the degree of vacuum during evacuation was -0.1 MPa, the treatment temperature was 140°C, the treatment time was 15 hours, and the treatment device was a vacuum drum dryer.
[0082] The resulting thickened polyamide 510 resin was subjected to a resin humidity conditioning treatment to obtain a high-viscosity polyamide 510 resin. The high-viscosity polyamide 510 resin had a relative viscosity of 3.3 to 96% sulfuric acid and a water content of 500 ppm. Here, the resin humidity conditioning treatment was performed by mixing nitrogen gas and water vapor, controlling the dew point of the nitrogen gas to 10°C, and setting the temperature in the resin humidity conditioning treatment to 100°C.
[0083] The high viscosity polyamide 510 resin was spun into fibers, and the spinning process was as follows: (1) A high-viscosity polyamide 510 resin was heated until it was in a molten state to form a polyamide 510 melt. Heating was performed in a screw extruder. The screw extruder was divided into five heating zones. Here, the temperature of the first zone was 235°C, the temperature of the second zone was 245°C, the temperature of the third zone was 255°C, the temperature of the fourth zone was 265°C, and the temperature of the fifth zone was 275°C.
[0084] (2) The polyamide 510 melt obtained in step (1) was conveyed through a melt line to a spinning box to be drawn into a low-oriented yarn, where the temperature of the spinning box was 280° C. and the spin pack pressure of the box was 16 MPa.
[0085] (3) The low-oriented yarn obtained in step (2) was subjected to heat retention, cooling, oiling, pre-interlacing, multi-stage drawing, main interlacing, and winding to obtain polyamide 510 industrial yarn.
[0086] For heat retention, an annealing device was used, the annealing height was 250 mm, and the annealing temperature was 260°C. For cooling, wind cooling was performed using a side air blower, the wind speed during wind cooling was 0.8 m / s, the wind temperature during wind cooling was 20°C, and the humidity during wind cooling was 80%. For oiling, an oil agent with model number TCP-80 was used, the oil agent concentration was 100 wt%, and it was not diluted. An oiling method using two oiling nozzles was used. The height of the oiling lip from the spinneret was 4.0 m, the oiling rate was 1.1%, and the pre-interlacing pressure was 2.0 bar.
[0087] The drawing process was divided into four stages using five pairs of heat rolls. Specifically, the low oriented yarn after oiling was first placed in the first pair of heat rolls, and the first stage of pre-drawing was performed between the first pair of heat rolls and the second pair of heat rolls. Then, the second stage of main drawing was performed between the second pair of heat rolls and the third pair of heat rolls, the third stage of main drawing and tension heat setting were performed between the third pair of heat rolls and the fourth pair of heat rolls, and then, the fourth stage of secondary drawing and relaxation heat setting were performed between the fourth pair of heat rolls and the fifth pair of heat rolls. The total draw ratio was 5.0, and the magnitude of speed contraction between the fourth pair of heat rolls and the fifth pair of heat rolls was 80 m / min.
[0088] The temperature in tension heat set is 180° C., the temperature in relaxation heat set is 120° C., the main interlacing pressure is 3.0 bar, and the winding speed is 2500 m / min. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0089] Example 2 Polyamide 510 Industrial Yarn Manufacturing A low-viscosity polyamide 510 resin with a relative viscosity of 2.5 was subjected to high-temperature drying treatment to obtain a thickened polyamide 510 resin. Here, the high-temperature drying was performed by evacuation, the degree of vacuum during evacuation was -0.1 MPa, the treatment temperature was 140°C, the treatment time was 15 hours, and the treatment device was a vacuum drum dryer.
[0090] The resulting thickened polyamide 510 resin was subjected to a resin humidity conditioning treatment to obtain a high-viscosity polyamide 510 resin. The high-viscosity polyamide 510 resin had a relative viscosity of 3.3 to 96% sulfuric acid and a water content of 1000 ppm. Here, the resin humidity conditioning treatment was performed by mixing nitrogen gas and water vapor, controlling the dew point of the nitrogen gas to 13°C, and setting the temperature in the resin humidity conditioning treatment to 100°C.
[0091] The high viscosity polyamide 510 resin was spun, and the spinning steps and process conditions were the same as those in Example 1. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0092] Example 3 Polyamide 510 Industrial Yarn Manufacturing A low-viscosity polyamide 510 resin with a relative viscosity of 2.5 was subjected to high-temperature drying treatment to obtain a thickened polyamide 510 resin. Here, the high-temperature drying was performed by evacuation, the degree of vacuum during evacuation was -0.1 MPa, the treatment temperature was 130°C, the treatment time was 15 hours, and the treatment device was a vacuum drum dryer.
[0093] The resulting thickened polyamide 510 resin was subjected to a resin humidity conditioning treatment to obtain a high-viscosity polyamide 510 resin. The high-viscosity polyamide 510 resin had a relative viscosity of 2.9 to 96% sulfuric acid and a water content of 500 ppm. Here, the resin humidity conditioning treatment was performed by mixing nitrogen gas and water vapor, controlling the dew point of the nitrogen gas to 10°C, and setting the temperature in the resin humidity conditioning treatment to 100°C.
[0094] The high viscosity polyamide 510 resin was spun, and the spinning steps and process conditions were the same as those in Example 1. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0095] Example 4 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, with the only difference being that in step (3), the TCP-80 oil solution was diluted with water to a concentration of 10 wt%, and oiling was performed. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0096] Example 5 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, with the only difference being that the model number of the oil in step (3) was TC1355. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0097] Example 6 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 5, with the only difference being that in step (3), the TC1355 oil solution was diluted with water to a concentration of 10 wt%, and oiling was performed. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0098] Example 7-1 Polyamide 510 Industrial Yarn Manufacturing A low-viscosity polyamide 510 resin with a relative viscosity of 2.5 was subjected to high-temperature drying treatment to obtain a thickened polyamide 510 resin. Here, the high-temperature drying was performed by evacuation, the degree of vacuum during evacuation was -0.1 MPa, the treatment temperature was 140°C, the treatment time was 15 hours, and the treatment device was a vacuum drum dryer.
[0099] The resulting thickened polyamide 510 resin was subjected to a resin humidity conditioning treatment to obtain a high-viscosity polyamide 510 resin. The high-viscosity polyamide 510 resin had a relative viscosity of 3.3 to 96% sulfuric acid and a water content of 500 ppm. Here, the resin humidity conditioning treatment was performed by mixing nitrogen gas and water vapor, controlling the dew point of the nitrogen gas to 10°C, and setting the temperature in the resin humidity conditioning treatment to 100°C.
[0100] Here, the obtained high-viscosity polyamide 510 resin contains a heat stabilizer which is a blend of copper acetate and potassium iodide, the weight of copper acetate being 250 ppm of the total weight of polyamide 510 salt (a salt formed from the raw materials 1,5-pentanediamine and sebacic acid in the process of producing polyamide 510 resin), and the weight of potassium iodide being 1,800 ppm of the total weight of polyamide 510 salt.
[0101] The high viscosity polyamide 510 resin was spun, and the spinning steps and process conditions were the same as those in Example 1. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0102] Example 7-2 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this embodiment are almost the same as those in Example 7-1, and the only difference is that the heat stabilizer contained in the high-viscosity polyamide 510 resin used is a mixture of copper acetate and potassium iodide, and the amount of copper acetate added is 200 ppm of the total weight of the polyamide 510 salt, and the amount of potassium iodide added is 1400 ppm of the total weight of the polyamide 510 salt.
[0103] Example 7-3 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this embodiment are almost the same as those in Example 7-1, and the only difference is that the heat stabilizer contained in the high-viscosity polyamide 510 resin used is a mixture of copper acetate and potassium iodide, and the amount of copper acetate added is 150 ppm of the total weight of the polyamide 510 salt, and the amount of potassium iodide added is 1000 ppm of the total weight of the polyamide 510 salt.
[0104] Example 7-4 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this embodiment are almost the same as those in Example 7-1, and the only difference is that the heat stabilizer contained in the high-viscosity polyamide 510 resin used is a mixture of copper acetate and potassium iodide, and the amount of copper acetate added is 200 ppm of the total weight of the polyamide 510 salt, and the amount of potassium iodide added is 800 ppm of the total weight of the polyamide 510 salt.
[0105] Example 8 Polyamide 510 Industrial Yarn Manufacturing A low-viscosity polyamide 510 resin with a relative viscosity of 2.5 was subjected to high-temperature drying treatment to obtain a thickened polyamide 510 resin. Here, the high-temperature drying was performed by evacuation, the degree of vacuum during evacuation was -0.1 MPa, the treatment temperature was 140°C, the treatment time was 15 hours, and the treatment device was a vacuum drum dryer.
[0106] The resulting thickened polyamide 510 resin was subjected to a resin humidity conditioning treatment to obtain a high-viscosity polyamide 510 resin. The high-viscosity polyamide 510 resin had a relative viscosity of 3.3 to 96% sulfuric acid and a water content of 500 ppm. Here, the resin humidity conditioning treatment was performed by mixing nitrogen gas and water vapor, controlling the dew point of the nitrogen gas to 10°C, and setting the temperature in the resin humidity conditioning treatment to 100°C.
[0107] The obtained high-viscosity polyamide 510 resin contains nano-montmorillonite as a nucleating agent, and its weight is 50 ppm of the total weight of polyamide 510 salt (a salt formed from 1,5-pentanediamine and sebacic acid, which are raw materials in the process of producing polyamide 510 resin).
[0108] The high viscosity polyamide 510 resin was spun, and the spinning steps and process conditions were the same as those in Example 1. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0109] Example 9 Polyamide 511 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example are almost the same as those in Example 1, and the only difference is that the high-viscosity resin used is polyamide 511, the relative viscosity of polyamide 511 to 96% sulfuric acid is 3.3, and the water content is 500 ppm. The performance results of the resulting polyamide 511 industrial yarn are shown in Table 1.
[0110] Example 10 Polyamide 512 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example are almost the same as those in Example 1, and the only difference is that the high-viscosity resin used is polyamide 512, the relative viscosity of polyamide 512 to 96% sulfuric acid is 3.3, and the water content is 500 ppm. The performance results of the resulting polyamide 512 industrial yarn are shown in Table 1.
[0111] Example 11 Polyamide 513 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example are almost the same as those in Example 1, and the only difference is that the high-viscosity resin used is polyamide 513, the relative viscosity of polyamide 513 to 96% sulfuric acid is 3.3, and the water content is 500 ppm. The performance results of the resulting polyamide 513 industrial yarn are shown in Table 1.
[0112] Example 12 Polyamide 516 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example are almost the same as those in Example 1, and the only difference is that the high-viscosity resin used is polyamide 516, the relative viscosity of polyamide 516 to 96% sulfuric acid is 3.3, and the water content is 500 ppm. The performance results of the resulting polyamide 516 industrial yarn are shown in Table 1.
[0113] Example 13 Polyamide 510 Industrial Yarn Manufacturing A low-viscosity polyamide 510 resin with a relative viscosity of 2.5 was subjected to high-temperature drying treatment to obtain a thickened polyamide 510 resin. Here, the high-temperature drying was performed by evacuation, the degree of vacuum during evacuation was -0.1 MPa, the treatment temperature was 100°C, the treatment time was 8 hours, and the treatment device was a vacuum drum dryer.
[0114] The resulting thickened polyamide 510 resin was subjected to a resin humidity conditioning treatment to obtain a high-viscosity polyamide 510 resin. The high-viscosity polyamide 510 resin had a relative viscosity of 3.3 to 96% sulfuric acid and a water content of 500 ppm. Here, the resin humidity conditioning treatment was performed by mixing nitrogen gas and water vapor, controlling the dew point of the nitrogen gas to 10°C, and setting the temperature in the resin humidity conditioning treatment to 100°C. The spinning steps and process conditions were the same as in Example 1. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0115] Example 14 Polyamide 510 Industrial Yarn Manufacturing A polyamide 510 resin having a relative viscosity of 2.6 and a water content of 500 ppm was heated to a molten state to form a melt, and then spun. The steps and process conditions of the spinning process were the same as those in Example 1. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0116] Example 15 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, and the only difference was that the annealing height of the annealing device used for the warming in step (3) was 30 mm, and the annealing temperature was 30°C. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0117] Example 16 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, with the only difference being that the height of the oiling lip from the spinneret in step (3) was 1.2 m. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0118] Example 17 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, and the only difference was that the magnitude of the speed contraction between the fourth pair of heated rolls and the fifth pair of heated rolls in step (3) was 0 m / min. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0119] Example 18 Polyamide 510 Industrial Yarn Manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, with the only difference being that the pre-interlacing pressure in step (3) was 0.5 bar. The performance results of the resulting polyamide 510 industrial yarn are shown in Table 1.
[0120] Example 19 Polyamide 56 industrial yarn manufacturing The raw materials, steps, process conditions, etc. used in this embodiment are almost the same as those in Example 1, and the only difference is that the high-viscosity resin used is polyamide 56, the relative viscosity of the polyamide 56 resin is 3.3, and the moisture content is 500 ppm. The performance results of the resulting polyamide 56 industrial yarn are shown in Table 1.
[0121] Example 20 Polyamide 56 industrial yarn manufacturing The raw materials, steps, process conditions, etc. used in this example were almost the same as those in Example 1, with the only differences being that the high-viscosity resin used was polyamide 56, the relative viscosity of the polyamide 56 resin was 3.3, the moisture content was 500 ppm, and the temperature in the tension heat setting in step (3) was 215°C. The performance results of the resulting polyamide 56 industrial yarn are shown in Table 1.
[0122] Example 21 Polyamide 56 industrial yarn manufacturing The raw materials, steps, process conditions, etc. used in this example are almost the same as those in Example 20, with the only difference being that the water content of the polyamide 56 resin used is 1000 ppm. The performance results of the resulting polyamide 56 industrial yarn are shown in Table 1.
[0123] Comparative Example 1 Manufacturing of polyamide 6 industrial yarn The raw materials, steps, process conditions, etc. used in Comparative Example 1 were almost the same as those in Example 1, with the only difference being that the high-viscosity resin used was polyamide 6, the relative viscosity of the polyamide 6 resin was 3.3, and the moisture content was 500 ppm. The performance results of the obtained polyamide 6 industrial yarn are shown in Table 1.
[0124] [Table 1] TIFF0007568730000002.tif35170
[0125] As can be seen from the results of the above examples and Table 1, by using polyamide 5X resin having a wide range of moisture content as a spinning raw material, industrial yarn with better overall performance can be produced. In particular, the moisture content range of polyamide 510 resin may be wider than that of polyamide 56. Specifically, the moisture contents of polyamide 510 in Examples 1 and 2 are 500 ppm and 1000 ppm, respectively, and the produced polyamide 510 industrial yarn has a breaking strength of ≧7.8 cN / dtex, a modulus of ≧44.3 cN / dtex, a boiling water shrinkage rate of ≦7.2%, and a dry heat shrinkage rate of ≦7.8%, and is excellent in strength and dimensional stability. In addition, as is abundantly clear from the results of the Examples and Table 1, if the water content of the polyamide resin used is too high, a decomposition reaction occurs during the high-temperature melting process, reducing the breaking strength and modulus of the industrial yarn produced, and if the viscosity of the polyamide resin used is too low (the molecular weight is relatively low), the performance of the yarn obtained after the subsequent multi-stage high-ratio drawing is poor.
[0126] As is further evident from the results of the Examples and Table 1, polyamide 510 industrial yarn can be subjected to a lower temperature during heat setting than polyamide 56 without affecting the performance of the industrial yarn. For example, when the temperature in tension heat setting using polyamide 510 as the raw material was 180°C, the overall performance of the resulting polyamide industrial yarn was excellent. In contrast, the overall performance of the industrial yarn obtained in Example 19 using polyamide 56 as the raw material and tension heat setting at 180°C was lower than that of the industrial yarn obtained in Example 20 (heat setting temperature of 215°C).
[0127] Meanwhile, the process conditions of step (3) have a significant impact on the performance of the industrial yarn. For example, if a low annealing height and temperature are used, it is disadvantageous for the subsequent multi-stage high-ratio drawing. If the height of the oiling lip from the spinneret is low, the filament breakage and broken single yarns are likely to increase. If there is no shrinkage step in the drawing process, i.e., the shrinkage magnitude is 0 m / min, the dimensional stability of the resulting polyamide industrial yarn is deteriorated. If a low pre-interlacing pressure is used, it is disadvantageous for the subsequent multi-stage high-ratio drawing and is likely to cause a lot of filament breakage.
[0128] Application Examples The industrial yarns obtained in the above Examples and Comparative Examples were twisted together and woven, and then the dyeing uniformity was measured. The dyeing uniformity levels are as follows: The industrial yarns of Examples 1 to 12 are at level 3.5 or higher, the industrial yarns of Examples 13 to 19, Example 21, and Comparative Example 1 are at level 3, and the industrial yarn of Example 20 is at level 3.5.
[0129] In addition, the polyamide 5X industrial yarn according to the present disclosure has a small change in yarn performance after water absorption, so it has a greater advantage in terms of dimensional stability in subsequent processing and application. If the boiling water shrinkage rate of the polyamide fiber is large, the shrinkage is serious during the dyeing process, and color unevenness is likely to occur. In particular, in the process of cheese dyeing, which is commonly used in the spinning field, if the shrinkage rate of the industrial yarn after water absorption is large, the tension inside and outside the yarn is different, so that the yarn closer to the bobbin has a higher tension, making it difficult for the dye to penetrate and dye, and color difference occurs in the dyeing of the inner and outer layers. Next, in the unwinding process of the bobbin yarn, the tension after shrinkage is different, making unwinding difficult and prone to yarn breakage, and the difficulty of processing increases, so the manufacturing cost increases. In addition, if the boiling water shrinkage rate is large, the width shrinkage of the fabric is likely to be large during the dyeing process, so the width is difficult to control, and especially after the fabric is made into a garment and washed with hot water, the shrinkage is large, so the shape retention is poor.
[0130] Unless otherwise limited, all terms used in this disclosure have the same meaning as commonly understood by one of ordinary skill in the art. The embodiments described in this disclosure are used for illustrative purposes only and are not intended to limit the protection scope of the present invention. Those skilled in the art may make various other substitutions, modifications and improvements within the scope of the present disclosure, so the present disclosure is not limited to the above embodiments, but is limited only by the scope of the claims.
Claims
1. A polyamide industrial yarn, the manufacturing raw material of which contains at least a polyamide 5X resin, The polyamide 5X resin is one or more selected from polyamide 510, polyamide 511, polyamide 512, polyamide 513, and polyamide 516; The polyamide industrial yarn has a moisture content of ≦2.2% and a breaking strength retention rate after humidity conditioning treatment of ≧94%.
2. The polyamide 5X resin is composed of 1,5-pentanediamine and a linear aliphatic dibasic acid, 2. Polyamide industrial yarn according to claim 1, wherein the linear aliphatic diacid is one or more selected from sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, and hexadecanedioic acid.
3. 2. The polyamide industrial yarn according to claim 1, wherein the breaking strength of the polyamide industrial yarn is 7.5-9.5 cN / dtex and the retention of heat tenacity of the polyamide industrial yarn is 85-95%.
4. 2. Polyamide industrial yarn according to claim 1, having a breaking elongation of 16 to 24%.
5. 2. Polyamide industrial yarn according to claim 1, having a modulus > 35 cN / dtex.
6. 2. Polyamide industrial yarn according to claim 1, having a dry heat shrinkage of ≦10.0%.
7. 2. Polyamide industrial yarn according to claim 1, having a boiling water shrinkage of ≦9.0% and an elongation after boiling water treatment of ≦25.0%.
8. 2. Polyamide industrial yarn according to claim 1, wherein the polyamide 5X resin comprises a heat stabilizer and / or a second additive, the heat stabilizer comprising one or more of copper acetate, potassium iodide, copper chloride, cuprous iodide, copper oxide, cuprous oxide, and the second additive comprising one or more of matting agents, flame retardants, antioxidants, ultraviolet absorbers, infrared absorbers, crystal nucleating agents, optical brighteners and antistatic agents.
9. (1) heating a spinning material including a polyamide 5X resin until the material is in a molten state to form a melt; (2) drawing yarn from the melt to form a low-oriented yarn; (3) subjecting the low-oriented yarn to a heat retention treatment, a cooling treatment, an oiling treatment, a pre-interlacing treatment, a multi-stage drawing treatment, a main interlacing treatment and a winding treatment to produce the polyamide industrial yarn, and performing a tension heat setting treatment and / or a relaxation heat setting treatment in any one of the drawing stages of the multi-stage drawing treatment.
10. The method for producing the polyamide 5X resin comprises: subjecting a polyamide 5X resin having a relative viscosity of 2.2-2.7 to 96% sulfuric acid to a high-temperature drying treatment to obtain a thickened polyamide 5X resin; and subjecting the thickened polyamide 5X resin to a resin humidity conditioning treatment to obtain the polyamide 5X resin having a relative viscosity of 3.3 to 4.
0.
11. The high-temperature drying treatment is carried out in a negative pressure state or in an inert gas atmosphere, and the degree of vacuum in the negative pressure state is −0.06 to −0.1 MPa; The method according to claim 10, wherein the temperature in the high-temperature drying treatment is 130 to 160° C., and the treatment time is 10 to 25 h.
12. The method according to claim 10, wherein the temperature in the resin moisture conditioning treatment is 85 to 110 ° C., the resin moisture conditioning treatment is performed by mixing nitrogen gas and water vapor, and the dew point of the nitrogen gas is controlled to -15 to 15 ° C.
13. 10. The method according to claim 9, wherein the heating in step (1) is performed in a screw extruder, and the screw extruder is divided into five heating zones, the temperature of the first zone being 220-250°C, the temperature of the second zone being 230-260°C, the temperature of the third zone being 240-270°C, the temperature of the fourth zone being 250-280°C, and the temperature of the fifth zone being 260-290°C.
14. 10. The method of claim 9, wherein the step (2) comprises discharging the melt through a spinneret of a spinning box to obtain a low-oriented yarn, the temperature of the spinning box being 260-290°C, and the pressure of a spin pack of the spinning box being 10-22 MPa.
15. In the step (3), the temperature is maintained by an annealing device, the annealing height is 100 to 300 mm, and the annealing temperature is 200 to 300° C.; The cooling process is performed by air cooling using a side air blow or a ring air blow, In the oiling process, the height of the oiling lip from the spinneret is ≧2.5 m, and the oiling rate is 0.7-1.2%; The pressure in the pre-interlacing process is 1 to 2.5 bar; The total draw ratio of the multistage drawing process is 4.5 to 6.0, The temperature in the tension heat set treatment is 150 to 200° C. The method according to claim 9, wherein the temperature in the relaxation heat-setting treatment is 100 to 160°C.
16. 9. Use of the polyamide industrial yarn according to any one of claims 1 to 8 in sewing threads, tire cords, airbag threads, release fabrics, water fabrics, canvas, seat belts, ropes, fishing nets, industrial filtration fabrics, conveyor belts, parachutes, tents or boxes and bags.
Citation Information
Patent Citations
Polyester-mixed filament yarn
JP2005029933A
Polyamide 56 filament, and fiber structure and air-bag base cloth each comprising the same
WO2009119302A1