High volume, dispensable getter

A dispensable getter composition with palladium oxide and zeolite adsorbents, combined with a bisphenol resin binder, addresses the capacity and integration issues of existing getters, providing effective moisture and hydrogen removal in electronic devices.

JP7568731B2Active Publication Date: 2024-10-16SAES GETTERS SPA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022548770
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-12
Filing Date
2021-02-09
Publication Date
2024-10-16
Estimated Expiration
2041-02-09

AI Technical Summary

Technical Problem

Existing getter solutions are inadequate for modern electronic devices due to limited capacity and integration challenges, particularly in miniaturized devices like high-speed optical transceivers and microwave modules, where hydrogen and moisture levels can cause rapid deterioration of electrical properties.

Method used

A dispensable getter composition comprising palladium oxide as a hydrogen adsorbent (5-25 wt%), zeolite as a moisture adsorbent (35-55 wt%), and a bisphenol resin binder (30-50 wt%), with optional additives, achieving high adsorption capacity and ease of integration through a viscosity range of 40,000 to 90,000 cP for dispensing.

Benefits of technology

The composition effectively adsorbs moisture and hydrogen, maintaining high capacity even after exposure, and can be easily integrated into devices without specialized equipment, ensuring device performance and longevity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568731000002
    Figure 0007568731000002
  • Figure 0007568731000003
    Figure 0007568731000003
  • Figure 0007568731000001
    Figure 0007568731000001
Patent Text Reader

Abstract

A high volume, dispensable moisture and hydrogen getter to be used as a sealant in electronically or optoelectronically sensitive devices and / or to control the levels of these substances, its use for sealing or semi-sealing such electronically or optoelectronically sensitive devices, and methods for controlling the levels of contaminants therein.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high volume, dispensable moisture and hydrogen getter, to be used to control the levels of these substances, for example in electronic or optoelectronic devices. [Background technology]

[0002] The presence of moisture and hydrogen, even at low levels (generally as low as 5000 ppm moisture and 1000 ppm hydrogen are considered lethal), is detrimental to the operation of most sealed devices. As perfect hermeticity is an ideal and unattainable condition, their concentrations inside the device will increase over time due to external factors such as penetration into the device through the case / sealing elements from the outside environment, and internal factors, primarily outgassing from device components.

[0003] Various references describe the detrimental role of hydrogen and moisture in hermetic devices. For example, Albarghouti et al., "Moisture and Hydrogen Release in Optoelectronic Hermetic Packages," Journal of Microelectronics and Electronic Packaging (2014) 11, 75-79, discloses that one undesirable moisture action in optoelectronic hermetic packages is the penetration and retention of moisture in microcracks, which causes hermeticity problems when the moisture freezes and expands. Hydrogen also has a high affinity for oxygen, which can react with surface oxides inside hermetic packages and cause moisture formation. A white paper by DfR Solutions, "Reliability Issues for Optical Transceivers," highlights the corrosion caused by hydrogen trapped in metallized Kovar packages and moisture sensitivity of device components for optical transceivers. Components that seem to be largely and primarily affected by hydrogen, such as fiber optic cables, also benefit from the presence of a combined hydrogen and moisture absorber, since moisture itself can be a source of hydrogen in the cables. See, for example, 2004 White Paper WP9007, Corning on the detrimental role of hydrogen, "The Impact of Hydrogen on Optical Fiber," and Ohnishi et al., "Loss stability assurance against hydrogen for submarine optical cable," Journal of Lightwave Technology, issue 2 (1988).

[0004] Thin film transistors (TFTs) are also reported as a type of device where the combined action of moisture and hydrogen can cause rapid degradation of electrical properties. Nam et al. reported in RCS Adv. 2018, 8, 5622-5628 that hydrogen impurities affect the electrical properties of TFTs based on amorphous oxide semiconductors. Lee and Jeong also described that the field-effect mobility of the same type of device is significantly reduced when exposed to high humidity conditions (IEEE Journal of the Electron Devices Society (2019, 7, 26-32)).

[0005] Another type of device in which the simultaneous presence of hydrogen and moisture is detrimental is a spatial light modulator, such as that described in US Pat. No. 6,958,846.

[0006] The adverse effects of hydrogen and moisture on microwave or even hybrid modules are explained in the technical pages reported under the links https: / / www.microwaves101.com / encyclopedias / hybrid-modules and https: / / www.microwaves101.com / encyclopedias / hermeticity.

[0007] Problems associated with the presence of hydrogen and moisture in encapsulated electronic devices and components are addressed in U.S. Patent Application Publication No. 2016 / 0175805, which discloses compacting a composite getter into a tablet form by adding a suitable binder.

[0008] One of the crucial aspects to be considered is also the amount of getter that should be added to ensure the required device lifetime, since the getter capacity is clearly related to the amount of getter material. However, considering the constant trend towards miniaturization, the available space is decreasing and tablet-shaped getters are not suitable for electronic devices, especially for newly developed devices such as communication chips for the latest standards (5G) as described in WO2019 / 066987.

[0009] U.S. Pat. No. 5,888,925 describes a hydrogen and moisture getter that proposes using a binder, such as a vulcanized silicone, to hold the getter in place and conform to a particular shape, but again does not address the problem of maximizing the amount of getter material that can be contained in a dispensable solution.

[0010] Thus, in the manufacture of hermetically sealed devices, it would be highly useful to have a water and / or hydrogen removing composition, generally referred to in the art and herein as a "getter", that can be easily dispensed in an appropriate amount of getter material and easily integrated in the manufacturing process of said devices. In the context of the present invention, the term "dispensable" also means "applicable", which is used to indicate a composition that can be easily dispensed, applied, distributed or deposited on a variety of surfaces and / or in a variety of shapes, and that can also be easily integrated into devices of the type described herein. The term dispensable composition, according to the present invention, refers to a composition that can be easily applied, applied, distributed or deposited on a variety of surfaces and / or in a variety of shapes, and that can also be easily integrated into devices of the type described herein. -1 It can also refer to a composition having a viscosity comprised between 40.000 cP and 90.000 cP at a shear rate of 100 .mu.m.

[0011] The advantage of the getter composition of the present invention is its dispensable characteristic, which allows its easy integration and at the same time a high adsorption capacity, which ensures its advantageous use in the most demanding devices, also in the light of the adoption of new communication standards (5G) and the associated new technical requirements and constraints. Exemplary devices in which the use of the solution of the present invention is particularly beneficial are optical transceivers, in particular so-called high-speed optical transceivers (i.e. devices with data transfer rates of more than 100 Gbps), optical receivers, microwave GaAs-based modules.

[0012] Dispensable getter compositions have long been known in the art, see for example U.S. Patent No. 5,244,707, which generally discloses the use of powders dispersed in a suitable matrix, U.S. Patent No. 5,997,829, which discloses a mixture of metal oxide and sorbent particles dispersed in a suitable matrix, or U.S. Patent No. 9,845,416, in the name of the present applicant, which describes a dispensable adhesive based on an epoxy resin with no active material contained therein. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] U.S. Patent No. 6,958,846 [Patent Document 2] US Patent Application Publication No. 2016 / 0175805 [Patent Document 3] WO2019 / 066987 [Patent Document 4] U.S. Patent No. 5,888,925 [Patent Document 5] U.S. Patent No. 5,244,707 [Patent Document 6] U.S. Patent No. 5,997,829 [Patent Document 7] U.S. Patent No. 9,845,416 [Non-patent literature]

[0014] [Non-Patent Document 1] Albarghouti et al. “Moisture and Hydrogen Release in Optoelectronic Hermetic Packages”, Journal of Microelectronics and Electronic Packaging (2014) 11, 75-79 [Non-Patent Document 2] White Paper “Reliability Issues for Optical Transceivers”, DfR Solutions [Non-Patent Document 3] Corning, "The Impact of Hydrogen on Optical Fiber," 2004 White Paper WP9007 [Non-Patent Document 4] Ohnishi et al., “Loss stability assurance against hydrogen for submarine optical cable,” Journal of Lightwave Technology, issue 2 (1988) [Non-Patent Document 5] Nam et al., RCS Adv. 2018, 8, 5622-5628 [Non-Patent Document 6] Lee and Jeong, IEEE Journal of the Electron Devices Society (2019, 7, 26-32) [Non-Patent Document 7] https: / / www.microwaves101.com / encyclopedias / hybrid-modules [Non-Patent Document 8] https: / / www.microwaves101.com / encyclopedias / hermeticity Summary of the Invention [Problem to be solved by the invention]

[0015] Accordingly, one object of the present invention is to overcome the limitations of getter-based solutions known in the art by providing a dispensable, high volume moisture and hydrogen getter. [Means for solving the problem]

[0016] Accordingly, a first aspect of the present invention is a dispensable getter composition comprising a binder, a moisture sorbent and a hydrogen sorbent, the hydrogen sorbent is palladium oxide in an amount between 5 wt. % and 25 wt. % of the weight of the dispensable getter composition; the moisture adsorbent is a zeolite in an amount between 35 wt % and 55 wt % of the weight of the dispensable getter composition; the organic binder is present in an amount between 30 wt % and 50 wt % of the weight of the dispensable getter composition; additional materials such as heat hardeners, pigments, and stabilizers up to 10 wt%, and preferably up to 5 wt%, preferably the amount of heat hardener is 1 wt% or more; The dispensable getter composition is characterized in that the organic binder is a bisphenol resin selected from F-type, S-type, or a combination thereof.

[0017] The dispensable compositions of the invention may also contain getters for other impurities, such as volatile organic compounds (VOCs), in any case up to a limit of 10 wt%, with the preferred case of hardeners in amounts of 1 wt% or more up to 9 wt%. The most common VOCs are benzene, toluene, xylene, heptene, heptane, dodecane, undecane, their alkyl (e.g. methyl) derivatives, ethylene glycol and other ethers, aldehydes, formaldehyde, ketones, amines, methylene chloride, tetrachloroethylene, 1,3-butadiene and other conjugated dienes, silanols and their alkyl derivatives.

[0018] The getter composition of the present invention is capable of achieving a water capacity comprised between 8 and 15 wt. % and a hydrogen capacity comprised between 20 and 60 Torr / gram, while maintaining the characteristic of being dispensable by the most common techniques and equipment, i.e., its viscosity is less than 50 sec. -1 The shear rate is between 40,000 cP and 90,000 cP.

[0019] The present invention is not limited to a particular thermal curing agent or a particular class of curing agents, and any curing agent compatible with bisphenol resins can be used, such as primary and secondary amines (aliphatic, cycloaliphatic and aromatic), organic acid anhydrides, or polyamides. It should be emphasized that the selection of a suitable curing agent is information that is readily available to those skilled in the art and can be easily retrieved. See, for example, the 1980 book "FRP Technology Fibre Reinforced Resin Systems" by RG Weatherhead, Applied Science Publishers LTD London Editor, especially Chapter 12 "Curing agents for epoxide resins", pages 266 to 283.

[0020] It should also be emphasized that the term hardener is similar to a cross-linking element. Suitable hardeners / cross-linking elements are, for example, polyfunctional amines, acid anhydrides, phenols, alcohols and thiols.

[0021] The invention is further explained with the aid of the following figures. [Brief description of the drawings]

[0022] [Figure 1] 1 is a graph showing moisture capacity test results for dispensable getter samples made in accordance with the present invention. [Diagram 2] 1 is a graph showing hydrogen capacity test results for dispensable getter samples made in accordance with the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The inventors have surprisingly discovered that by using a specific bisphenol resin, selected between F, S or a mixture thereof, a suitable viscosity is achieved that allows the inventive getter to be delivered to a syringe to be loaded and used in a standard dispensing device, even with a cumulatively large amount of moisture and hydrogen getter (40 wt% or more). This is possible because the inventive dispensable getter has a viscosity (obviously before curing) that is typically comprised between 40.000 centipoise cP and 90.000 cP at a shear rate of 50 sec-1. This result was not a priori predictable, as the comparative example described below shows.

[0024] Other additional advantages of the present invention are that the composite getter does not contemplate the use of environmentally harmful solvents, it can be dispensed in air without significantly impairing its hydrogen capacity and only partially saturating its moisture capacity (50% loss after 10 minutes of exposure to air for the dispensed getter layer), and the moisture adsorption capacity can be fully restored through heat treatment, e.g., heating at 100°C-150°C for 1-3 hours.

[0025] The moisture sorbent is a zeolite, preferably Linde Type A Zeolite (LTA), and in a further embodiment said LTA zeolite is combined with at least one zeolite selected in the group consisting of faujasite, MFI and mordenite. According to the present invention the moisture sorbent may be in the form of particles, at least 90% of the particles being less than 10 μm in size (diameter), and the dispensable getter composition is so uniform that the above size conditions can be observed over any gram of the dispensable getter composition according to any of the embodiments disclosed herein.

[0026] The hydrogen sorbent is palladium metal oxide in the form of particles with at least 90% of the particles being less than 15 μm in size (diameter), and the above size condition can be observed across any gram of the dispensable getter composition because the dispensable getter composition is highly uniform.

[0027] Since the particles may not be perfectly spherical, for purposes of determining the diameter of an equivalent sphere, these diameters are intended as the diameter of the enclosing sphere. The distribution should be evaluated numerically, and any suitable technique can be used, such as the use of commercially available laser diffraction equipment.

[0028] It should be emphasized that although the dispensable getter compositions of the present invention are most effectively employed in hermetic devices, they can also be effectively employed in so-called semi-hermetic devices.

[0029] An airtight device is defined based on its leakage rate according to standard TM 1014.11, and more specifically, an airtight device is: - 5*10 for volumes less than 0.01cc -8 Air below atm cc / s - 1*10 for volumes between 0.01cc and 0.4cc -7 Air below atm cc / s - 1*10 for volumes over 0.4cc -6 Air below atm cc / s It has the following characteristics.

[0030] On the other hand, while there is no strict definition of semi-hermetic devices, for purposes of the present invention, they can be considered to be devices that have air leakage rates up to two orders of magnitude higher than hermetic devices.

[0031] The composition according to any one of the embodiments disclosed above can be used to seal or fill a device, preferably an electronic or optoelectronic device, and / or to control the level of contaminants, such as hydrogen and moisture, in said device. Alternatively, the composition according to any one of the embodiments disclosed above can be used to obtain a deposit of a getter on a support surface, the support being advantageously used, for example, as part of a device package or housing. Thus, the present invention also refers to using the composition according to any one of the embodiments disclosed herein to seal or fill a device, preferably an electronic or optoelectronic device, or to provide a getter deposit support or support surface to be included therein, thereby controlling the level of contaminants in the device.

[0032] In particular, the inventive dispensable getter composition may be used in hermetic devices, for example as an active deposit or even as a filler, and / or as an (active) sealant in semi-hermetic devices.

[0033] In its second aspect, the present invention covers the use of a dispensable getter composition comprising a binder, a moisture sorbent and a hydrogen sorbent, the hydrogen sorbent is palladium oxide in an amount between 5 wt. % and 25 wt. % of the weight of the dispensable getter composition; the moisture adsorbent is a zeolite in an amount between 35 wt % and 55 wt % of the weight of the dispensable getter composition; the organic binder is present in an amount between 30 wt % and 50 wt % of the weight of the dispensable getter composition; the organic binder is a bisphenol resin selected from 4,4'-methylenediphenol (bisphenol F type), 4,4'-sulfonyldiphenol (bisphenol S type) or a mixture thereof; Up to 10 wt. %, and preferably up to 5 wt. % of additional materials such as hardeners, pigments, stabilizers, the amount of hardener preferably being 1 wt. % or more; The support is advantageously used as part of the housing of the device to obtain a hardened, solidified deposit of the getter on the support surface.

[0034] Apparently after curing, the dispensed getter composition should exhibit only negligible amounts of unreacted hardener. As a result of the curing process, the bisphenol is transformed into an epoxy resin with very limited flow properties, i.e. a viscosity of 500.000 cP or more at a shear rate of 50 sec-1.

[0035] The getter can be deposited, for example, on the surface of the support (that will be exposed inside the device). Thus, another aspect of the present invention is a support or support surface covered with or having a getter composition according to any one of the embodiments disclosed herein. Suitable surface support materials are, for example, silicon, glass, polyamide, polyimide, polyethylene naphthalate, cyclic olefin copolymers and other polymeric substrates with suitable thermal stability or metals. Preferred metal or metallized supports are kovar, gold-plated kovar, gold-plated iron, nickel-plated iron. In some embodiments, the entire support is made of the materials listed above, while in others the majority of it is made of a different material, and only its surface on which the getter is to be deposited is made of the materials listed above.

[0036] The most useful formats for the hardened getter deposits are those having an average thickness comprised between 100 μm and 300 μm, while the area is a parameter strongly related to the sensitive device and its dimensions, which are not an obvious feature of the invention but of the device itself.

[0037] Preferably the support with the solidified deposit of getter material is used as or is part of the lid of the device.

[0038] The use of a support coated with or having a hardened, dispensable getter composition according to the present invention is advantageous as it allows the device manufacturer to just integrate the support in the manufacturing process of the device and therefore does not require dispensing and curing equipment (off-line getter integration).

[0039] The support with the cured, dispensable getter can therefore be considered as a semi-finished product to be shipped to the device manufacturer, and in this respect its dispensable feature (before curing) remains an interesting feature, as it allows to easily produce different formats for integration in different types of devices or devices with different requirements in terms of size or amount of material.

[0040] In its third aspect, the present invention covers a method of controlling contaminant levels within a sensitive device with a dispensable getter composition comprising an organic binder, a moisture sorbent, and a hydrogen sorbent, comprising: the hydrogen sorbent is palladium oxide in an amount between 5 wt. % and 25 wt. % of the weight of the dispensable getter composition; the moisture adsorbent is a zeolite in an amount between 35 wt % and 55 wt % of the weight of the dispensable getter composition; the organic binder is present in an amount between 30 wt % and 50 wt % of the weight of the dispensable getter composition; the organic binder is a bisphenol resin selected from 4,4'-methylenediphenol (bisphenol F type), 4,4'-sulfonyldiphenol (bisphenol S type) or a mixture thereof; Up to 10 wt % of additional materials such as hardeners, pigments, stabilizers, and preferably up to 5 wt %, with the amount of hardener preferably being 1 wt % or more.

[0041] The term "sensitive device" refers to an electronic or optoelectronic device whose performance or life is impaired by the presence of relatively high levels of moisture or hydrogen, such as greater than 5000 parts per million (ppm) for moisture and greater than 1000 ppm for hydrogen. Exemplary devices are optical transceivers, transmitters, receivers, amplifiers, laser diodes, multiplexers, photodiodes, RF devices, microwave modules or hybrid modules.

[0042] The present invention also refers to methods which envisage using the dispenseable getters as active sealants and / or fillers for devices or as getters inside devices with no specific adhesive function, i.e. the adsorption function is addressed by the dispenseable getters of the present invention and separated from the sealing function.

[0043] Therefore, another object of the present invention is a method for sealing or filling a device, preferably an airtight or semi-airtight device, and / or for controlling the level of contaminants therein, Dispensing a dispensable getter composition onto one or more surfaces of a device, into the device, and / or onto a support or supporting surface to be included in said device, according to any one of the embodiments disclosed herein; and then curing the device, the support or a surface thereof, respectively; Includes.

[0044] According to one embodiment of the present invention, the hardened getter composition is isolated from the environment outside the electronic device and has an average thickness comprised between 100 μm and 300 μm, or the hardened dispensable getter composition is in contact with the environment outside the electronic device and has an average thickness comprised between 1 mm and 4 mm.

[0045] According to one embodiment of the present invention, the term encapsulant, when applied as a dispensable getter encapsulant, refers to the placement of the dispensable getter composition in an electronic device package, i.e. as an intervening element between the internal volume of the sensitive device and the external environment. In this respect, it is important to emphasize that the encapsulant according to the present invention can be in direct contact with the outside of the device or can be in contact with other elements, such as the getterless encapsulants as described in the previously mentioned US Patent No. 9,845,416 in the name of the applicant.

[0046] The high capacity dispensable moisture and hydrogen getter of the present invention is typically provided in a syringe, dispensed by a needle dispensing tool, and then subjected to a curing process, typically by thermal curing, at a temperature ranging from 100° C. to 250° C. for a duration comprised between 0.5 hours and 4 hours, obviously the lower the temperature the longer the duration of the curing process. The present invention is not limited to this particular dispensing technique, and others such as doctor blading, bar coating, slot die coating, screen printing can also typically be used.

[0047] When the method envisages its use as a getter (without sealing function), the inventive dispensable composition after curing has the form of a continuous deposit of material whose average thickness is preferably comprised between 100 and 300 μm and whose area is adjusted to the dimensions of the sensitive device, whereas when used as an active sealant, its average thickness is preferably comprised between 1 and 4 mm.

[0048] One advantage of a dispensable getter composition, and the method of controlling contaminant levels through its use, is that device manufacturers have the possibility to choose the best way to integrate the getter, either with a semi-finished product (deposition support) if they do not have the required equipment (off-line solution), or in a dispensable solution that can be easily implemented through standard dispensing equipment (in-line solution).

[0049] The invention is further illustrated with the aid of the following non-limiting examples.

[0050] Preparation of sample S1 according to the present invention 10 grams of a dispensable getter composition according to the present invention was prepared by adding 1.5 grams of palladium oxide particles (90% by number) having a diameter less than 10 μm and 4.5 grams of LTA type zeolite particles (90% by number) having a diameter less than 10 μm to a bisphenol F matrix containing 0.4 grams of a cyanate ester as a hardener.

[0051] The dispensable getter composition was then subjected to a speed mixing process to obtain a homogenous composition / particle distribution and later to a rolling process.

[0052] A portion of the dispensable getter composition is then inserted into a 3 cc syringe and deposited onto aluminum foil as a series of ten 9×5 mm rectangles with an average height of 100 μm, and another portion is saved for rheological property testing.

[0053] The foil is then cured by a two-step heating process, first at 150° C. for 1 hour, followed by a final heating at 200° C. for 1 hour. The foil is then cut into samples, each containing a single getter deposit, which are activated at an elevated temperature of 100° C. for 3 hours under vacuum. This further activation step removes any water physisorbed by the zeolite during sample preparation.

[0054] Preparation of Comparative Sample C1 0.4 grams of palladium oxide particles (90% by number) with diameters less than 10 μm and 3.0 grams of LTA type zeolite particles (90% by number) with diameters less than 10 μm were added to bisphenol A diglycidyl ether and methylphthalic anhydride epoxy resin to prepare 10 grams of a dispensable getter composition outside the scope of the present invention. The dispensable getter composition was then subjected to a speed mixing process to obtain a homogenous composition / particle distribution and later to a rolling process.

[0055] Preparation of comparative sample C2 0.4 grams of palladium oxide particles (90% by number) with diameters less than 10 μm and 1.5 grams of LTA type zeolite particles (90% by number) with diameters less than 10 μm were added to bisphenol A diglycidyl ether and methylphthalic anhydride epoxy resin to prepare 10 grams of a dispensable getter composition outside the scope of the present invention. The dispensable getter composition was then subjected to a speed mixing process to obtain a homogenous composition / particle distribution and later to a rolling process.

[0056] Moisture Capacity Test of Sample S1 Four of the ten samples were tested simultaneously in a microbalance held under dynamic conditions at room temperature, exposed to a partial pressure of 5 mbar up to saturation, achieving an overall capacity of 12 wt %.

[0057] Figure 1 shows the results of the above test, where t1 indicates the start time of exposure to 5 mbar moisture pressure.

[0058] Hydrogen capacity test of sample S1 Four of the ten samples were simultaneously tested at room temperature in a volumetric bench at a constant pressure of 8 Torr of pure hydrogen to saturation, and the total capacity of the tested samples was 33 Torr liters / gram, corresponding to a relative weight gain of the composite getter of 0.36 wt %.

[0059] Figure 2 shows the results of the above test.

[0060] The much smaller weight gain due to hydrogen trapping relative to water is related to the low molecular weight of hydrogen as well as the adsorbent ratios selected for the preparation of sample S1.

[0061] Rheological Property Testing The rheological properties of sample S1 made according to the invention (made with bisphenol F) are compared to comparative examples C1 and C2 (both made with bisphenol A). The following table 1 reports the sample loadings and measured rheological properties of the adsorbent materials.

[0062] [Table 1]

[0063] The samples reported in Table 1 were tested by rheological analysis and -1 The viscosity is determined at a shear rate of 50 sec. -1 A material viscosity in the range of 10,000 to 90,000 cP at a shear rate of 1000 rpm is required. As is evident from the results, sample S1 exhibits good viscosity at high amounts of moisture and hydrogen getter, as opposed to comparative examples C1 and C2, which are characterized by high viscosity at low getter loading.

[0064] For both the hydrogen and moisture adsorbents, it can be observed that even with the reduced loading of adsorbent material, comparative samples C1 and C2 were both outside the ranges described above useful for most common dispensing techniques.

Claims

1. 1. A dispensable getter composition comprising an organic binder, a moisture sorbent, and a hydrogen sorbent, a. the hydrogen sorbent is palladium oxide in an amount between 5 wt % and 25 wt % of the weight of the dispensable getter composition; b. the moisture adsorbent is a zeolite in an amount between 35 wt % and 55 wt % of the weight of the dispensable getter composition; c. the organic binder is present in an amount between 30 wt % and 50 wt % of the weight of the dispensable getter composition; The dispensable getter composition further comprises up to 10 wt % of additional materials such as thermal curatives, pigments, and stabilizers, the thermal curative being 1 wt % or more.

2. A dispensable getter composition comprising: A dispensable getter composition, characterized in that said organic binder is a bisphenol resin of the F type.

2. 10. The dispensable getter composition of claim 1, wherein the additional material comprises up to 9 wt% of a volatile organic compound getter.

3. 3. The dispensable getter composition of claim 1 or 2, wherein the moisture adsorbent is an LTA zeolite.

4. 4. The dispensable getter composition of claim 3, wherein the LTA zeolite is combined with at least one zeolite selected from the group consisting of faujasite, MFI and mordenite.

5. 5. A dispensable getter composition according to any one of claims 1 to 4, wherein the moisture adsorbent is in the form of particles, at least 90% of the particles having a size less than 10 μm.

6. 6. A dispensable getter composition according to any one of claims 1 to 5, wherein the palladium oxide is in the form of particles, at least 90% of the particles having a size of less than 15 μm.

7. 1. Use of a dispensable getter composition comprising an organic binder, a moisture sorbent and a hydrogen sorbent, a. the hydrogen sorbent is palladium oxide in an amount between 5 wt % and 25 wt % of the weight of the dispensable getter composition; b. the moisture adsorbent is a zeolite in an amount between 35 wt % and 55 wt % of the weight of the dispensable getter composition; c. the organic binder is present in an amount between 30 wt % and 50 wt % of the weight of the dispensable getter composition; The dispensable getter composition further comprises additional materials such as thermal curing agents, pigments, and stabilizers up to 10 wt %, the thermal curing agent being 1 wt % or more. In using the dispensable getter composition, Viscosity is 50sec -1 2. Use of a dispensable getter composition, characterized in that the organic binder is a bisphenol resin of type F, to obtain a solidified, hardened getter deposited on a supporting surface having a viscosity of 500 Pa·s (500.000 cP) or more at a shear rate of 1000 rpm.

8. 8. Use of the dispensable getter composition according to claim 7, wherein said support surface is made of silicon, metal, glass, polyamide, polyimide, polyethylene naphthalate, cyclic olefin copolymer.

9. 9. Use of a dispensable getter composition according to claim 8, wherein the average thickness of the solidified getter deposit is comprised between 100 μm and 300 μm.

10. 1. A method for controlling contaminant levels within a sensitive device by dispensing and curing a dispensable getter composition comprising an organic binder, a moisture sorbent, and a hydrogen sorbent, comprising: a. the hydrogen sorbent is palladium oxide in an amount between 5 wt % and 25 wt % of the weight of the dispensable getter composition; b. the moisture adsorbent is a zeolite in an amount between 35 wt % and 55 wt % of the weight of the dispensable getter composition; c. the organic binder is present in an amount between 30 wt % and 50 wt % of the weight of the dispensable getter composition; d. the organic binder is a bisphenol resin of the F type; The method, wherein the dispensable getter composition further comprises additional materials such as thermal curatives, pigments, stabilizers up to 10 wt %, wherein the amount of the thermal curative is 1 wt % or more.

Citation Information

Patent Citations

  • Getter slurry for absorbing air tightness packaging device harmful gas, preparation method of getter slurry and acquired coating

    CN106810982A

  • Thick film getter paste composition using for suppressing moisture

    JP2005144448A

  • Getter composition

    US20160175805A1

  • Combination moisture and hydrogen getter

    US4405487A

  • Enclosure for electronic devices

    US5244707A