Non-oriented electromagnetic steel sheet
A non-oriented electrical steel sheet with controlled chemical composition and manufacturing parameters achieves uniform magnetic properties and reduced width-direction deviations, addressing cogging torque and noise issues in motors.
Patent Information
- Application Number
- JP2024509324
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-30
- Filing Date
- 2023-09-29
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2043-09-29
AI Technical Summary
Existing non-oriented electrical steel sheets with non-transformation type chemical composition face significant deviations in magnetic properties in the width direction, which lead to cogging torque and noise during motor rotation, despite methods like rapid heating and controlled annealing processes.
A non-oriented electrical steel sheet with a specific chemical composition (C: 0.0030% or less, Si: 1.0 to 3.5%, Al: 0.10 to 2.00%, Mn: 0.1 to 2.0%, P: 0.20% or less, S: 0.0030% or less, N: 0.0030% or less, Ti: 0.0030% or less, B: 0.0020% or less, Sn: 0~0.200%, Sb: 0~0.1000%, balance Fe and impurities) and controlled manufacturing conditions, including a finish annealing temperature of 850°C or higher and a finish annealing parameter PT (W×t×L×T/Vc) greater than 100, to minimize magnetic property deviations.
The solution results in a steel sheet with uniform magnetic properties across the width direction, reducing cogging torque and rotation noise, and maintaining low iron loss, suitable for applications in motors and electric vehicles.
Smart Images

Figure 0007568998000004 
Figure 0007568998000001 
Figure 0007568998000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel sheet. This application claims priority based on Japanese Patent Application No. 2022-157340, filed on September 30, 2022, the contents of which are incorporated herein by reference. [Background technology]
[0002] In the field of motors, especially in the field of electrical equipment such as compressors for air conditioners and refrigerators, small and medium-sized transformers, and electrical equipment, there is a need to reduce electricity consumption worldwide, conserve energy, and reduce CO 2 In the context of the movement to protect the global environment, such as through the reduction of emissions, there is an ever-increasing demand for more efficient and more compact motors.
[0003] In the automotive field, non-oriented electrical steel sheets are used as cores for the drive motors of hybrid and electric vehicles. Automakers at home and abroad have publicly declared their intention to increase production of the above-mentioned electric vehicles, so the demand for the non-oriented electrical steel sheets used therein is growing significantly.
[0004] In this context, it is important to improve the magnetic properties of non-oriented electrical steel sheets used as motor core materials, as well as to make the magnetic properties uniform across the width of the steel sheets. This is because the deviation in the magnetic properties across the width of the steel sheets causes a torque called cogging torque when the motor rotates, which makes the rotation jerky and leads to noise when the motor rotates. On the other hand, if we try to avoid the generation of this cogging torque, there is a problem that it is necessary to shorten the length of the hoop that can be taken from the coil.
[0005] Conventional methods for improving the magnetic properties of non-oriented electrical steel sheets include adding alloy elements such as Si, reducing impurity elements such as C, S, and N, and controlling the annealing temperature in the finish annealing process after cold rolling to control the grain size to an appropriate level. If the annealing temperature is high during this finish annealing, residual strain that affects the magnetic properties will occur in the cooling process after annealing. This strain affects the magnetic properties by preventing domain wall movement when a magnetic field is applied, and the residual strain varies in the width direction, causing deviations in the magnetic properties in the width direction. In the case of general-purpose varieties of non-oriented electrical steel sheets, the final annealing temperature is low. Therefore, the cooling rate after the final temperature is slow, and the amount of residual strain introduced into the steel sheet is small. As a result, the deviation in magnetic properties in the width direction is small. On the other hand, in the case of high-grade varieties, the final annealing temperature must be high to reduce iron loss through coarsening of the crystal grain size, and the cooling rate of the non-oriented electrical steel sheet becomes fast, so the amount of residual strain introduced into the steel sheet increases and variation occurs in the width direction. As a result, the deviation in magnetic properties in the width direction increases.
[0006] To address these issues, Patent Document 1 discloses a method for inexpensively producing a non-oriented electrical steel sheet with little in-plane anisotropy. Patent Document 1 discloses that a non-oriented electrical steel sheet can be obtained in which the magnetic properties at each angle from the rolling direction to the width direction of the sheet are uniformly controlled. However, in Patent Document 1, in order to achieve the above-mentioned object, it is assumed that the final annealing is performed by rapid heating, and the γ transformation occurs in the temperature range reached by the rapid heating, which is equal to or higher than the Ac3 point. In other words, the target is limited to transformation-type components (component systems in which α → γ transformation occurs by heating).
[0007] Patent Document 2 discloses a method for producing an electromagnetic steel sheet having uniform magnetic properties in the coil width direction, characterized in that, in producing an electromagnetic steel sheet by a series of steps including a hot rolling step in which an electromagnetic steel sheet slab is rough hot rolled, the obtained sheet bar is wound into a coil and then finish rolling is performed while rewinding, a cold rolling step in which the final sheet thickness is achieved by one or more cold rolling steps with intermediate annealing in between, and a magnetic treatment step in which final magnetic properties are expressed in the product by primary recrystallization annealing or primary recrystallization annealing and secondary recrystallization annealing, the rough rolling stage of the hot rolling step involves width-direction thickness control such that the thickness of the width-direction ends of the sheet bar and the thickness of the width-direction central portion satisfy a predetermined relationship, and then the sheet bar is wound up. However, in Patent Document 2, the sheet bar after rough hot rolling needs to be wound, which increases the number of steps, and the control of the deviation of magnetic properties in the sheet width direction is also insufficient. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Publication No. 07-054052 [Patent Document 2] Japanese Patent Publication No. 09-316536 Summary of the Invention [Problem to be solved by the invention]
[0009] In the conventional technology, the deviation of magnetic properties in the sheet width direction has not been sufficiently controlled in non-oriented electrical steel sheets with a chemical composition that is non-transformation-based (wherein α→γ transformation does not occur by heating). Therefore, there is a demand for a technology that can homogenize magnetic properties without additional processes.
[0010] In view of the above demands, the present invention has an object to provide a non-oriented electrical steel sheet having a Si content of 1.0% or more and 3.5% or less and having a high soaking temperature in finish annealing of 850°C or more (i.e., requiring low iron loss), which has good magnetic properties and small deviation in the magnetic properties in the width direction. [Means for solving the problem]
[0011] In order to solve the above problems, the present inventors have conducted extensive research into the effects of chemical composition and manufacturing conditions on the deviation in magnetic properties in the width direction, and have found that the deviation in magnetic properties in the width direction of a steel sheet can be reduced by controlling the distribution of precipitates in the width direction by controlling the cooling rate, and by controlling the length between hearth rolls in the soaking zone in the finish annealing process, the tension applied to the steel sheet, and the cooling rate after finish annealing. The present invention has been made based on the above findings, and the gist of the present invention is as follows.
[0012] [1] A non-oriented electrical steel sheet according to one embodiment of the present invention includes a steel sheet, and a chemical composition of the steel sheet is, in mass%, C: 0.0030% or less, Si: 1.0 to 3.5%, Al: 0.10 to 2.00%, Mn: 0.1 to 2.0%, P: 0.20% or less, S: 0.0030% or less, N: 0.0030% or less, Ti: 0.0030% or less, B: 0.0020% or less, Sn: 0 to 0.200%, Sb: 0 to 0.1000%, and the balance: The steel plate consists of Fe and impurities, and satisfies the following formula (1) where the Sn content, in mass%, is [Sn] and the Sb content, in mass%, is [Sb]. When the width of the steel plate is W, the ratio of the maximum value WH to the minimum value WL of iron loss W10 / 400, which is WH / WL, is 1.10 or less in a W / 10 part that is a portion at W / 10 position from the end in the width direction to the sheet width, a W / 4 part that is a portion at W / 4 position, and a W / 2 part that is a portion at W / 2 position. [Sn]+2×[Sb]≦0.200 (1) [2] In the non-oriented electrical steel sheet according to [1], the [Sn] and the [Sb] may satisfy the following formula (2): 0.020≦[Sn]+2×[Sb]≦0.200 (2) [3] The non-oriented electrical steel sheet according to [1] or [2] may have an insulating coating formed on the surface of the steel sheet. Effect of the Invention
[0013] According to the above-mentioned aspects of the present invention, it is possible to produce a non-oriented electrical steel sheet having a transformation or non-transformation chemical composition, excellent magnetic properties, and small deviations in the magnetic properties in the width direction. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a diagram showing the relationship between the parameter PT in the soaking zone of a finish annealing furnace and the deviation of magnetic properties in the width direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] A non-oriented electrical steel sheet according to one embodiment of the present invention (hereinafter, sometimes referred to as "the electrical steel sheet according to this embodiment") will be described. The electrical steel sheet according to this embodiment includes a steel sheet. The electrical steel sheet according to this embodiment may consist of only a steel sheet, but may also have an insulating coating on the surface (one side or both sides) of the steel sheet. In addition, the electrical steel sheet according to the present embodiment has a chemical composition, in mass%, of C: 0.0030% or less, Si: 1.0 to 3.5%, Al: 0.10 to 2.00%, Mn: 0.1 to 2.0%, P: 0.20% or less, S: 0.0030% or less, N: 0.0030% or less, Ti: 0.0030% or less, B: 0.0020% or less, Sn: 0 to 0.200%, Sb: 0 to 0.1000%, and the balance: Fe and impurities. When the Sn content, in mass%, is [Sn] and the Sb content is [Sb], the relationship [Sn]+2×[Sb]≦0.200 is satisfied, and when the width of the steel plate is W, WH / WL, which indicates the ratio of the maximum value WH to the minimum value WL of iron loss W10 / 400, is 1.10 or less in a W / 10 part that is a portion at W / 10 position from the end in the width direction of the plate, a W / 4 part that is a portion at W / 4 position, and a W / 2 part that is a portion at W / 2 position of the plate.
[0016] The electromagnetic steel sheet and the manufacturing method according to this embodiment will be described below.
[0017] <Steel plate> The steel sheet (also called base steel sheet) included in the non-oriented electrical steel sheet will be described below.
[0018] [Chemical composition] The reasons for limiting the chemical composition of the steel sheet included in the electrical steel sheet according to this embodiment (when the non-oriented electrical steel sheet is composed of only a steel sheet, it can also be said to be the chemical composition of the non-oriented electrical steel sheet) will be explained below. Unless otherwise specified, "%" relating to the content of each element constituting the chemical composition means "% by mass".
[0019] C: 0.0030% or less C is an element that causes magnetic aging and increases iron loss. C also has a large effect on the deviation of magnetic properties. Therefore, the C content is set to 0.0030% or less. The C content is preferably 0.0025% or less, and more preferably 0.0020% or less. The lower the C content, the more preferable, and 0% is acceptable; however, an excessive reduction in the C content leads to increased costs, so the C content may be 0.0005% or more.
[0020] Silicon: 1.0 to 3.5% Silicon is an element that increases the electrical resistance of steel sheets, reduces eddy current loss, and reduces iron loss. It is also an element that has a large effect on the deviation of magnetic properties. If the Si content is less than 1.0%, the electrical resistance of the steel sheets does not increase and the iron loss does not decrease. Therefore, the Si content is set to 1.0% or more. The Si content is preferably 1.8% or more, and more preferably 2.0% or more. On the other hand, if the Si content exceeds 3.5%, the magnetic flux density and punching workability are significantly reduced, and the manufacturing cost increases. Therefore, the Si content is set to 3.5% or less. The Si content is preferably 3.3% or less, and more preferably 3.2% or less.
[0021] Al: 0.10-2.00% Al is inevitably mixed in from ores and refractories, but it contributes to deoxidation and, like Si, is an element that has the effect of increasing electrical resistance, reducing eddy current loss, and reducing iron loss. If the Al content is less than 0.10%, fine AlN is formed and has an adverse effect on core loss, so the Al content is set to 0.10% or more, preferably 0.20% or more, and more preferably 0.50% or more. On the other hand, if the Al content exceeds 2.00%, the saturation magnetic flux density decreases, and the magnetic flux density decreases, so the Al content is set to 2.00% or less, preferably 1.50% or less, and more preferably 1.20% or less.
[0022] Mn: 0.1-2.0% Mn is an element that increases electrical resistance, reduces eddy current loss, and inhibits the precipitation of fine sulfides such as MnS, which are detrimental to the growth of crystal grains. If the Mn content is less than 0.1%, the effect is not sufficiently obtained. Therefore, the Mn content is set to 0.1% or more. The Mn content is preferably 0.2% or more, and more preferably 0.4% or more. On the other hand, if the Mn content exceeds 2.0%, the growth of crystal grains during annealing decreases and iron loss increases. Therefore, the Mn content is set to 2.0% or less. The Mn content is preferably 1.5% or less, and more preferably 1.2% or less.
[0023] P:0.20% or less If the P content exceeds 0.20%, the toughness of the steel plate decreases and the steel plate becomes more susceptible to fracture. Therefore, the P content is set to 0.20% or less. The P content is preferably 0.15% or less, and more preferably 0.12% or less. There is no particular lower limit for the P content (it may be 0%), but in consideration of the manufacturing cost, 0.001% is the substantial lower limit.
[0024] S: 0.0030% or less S is an element that forms fine sulfides such as MnS and inhibits recrystallization and grain growth during final annealing. If the S content exceeds 0.0030%, recrystallization and grain growth during final annealing are significantly inhibited, and magnetic properties are reduced. Therefore, the S content is set to 0.0030% or less. The S content is preferably 0.0020% or less, and more preferably 0.0015% or less. There is no particular lower limit for the S content (it may be 0%), but in consideration of industrial purification technology, the lower limit is 0.0001%, and in consideration of production costs, the practical lower limit is 0.0003%.
[0025] N: 0.0030% or less N is an element that forms precipitates and increases iron loss. If the N content exceeds 0.0030%, the increase in iron loss is significant. Therefore, the N content is set to 0.0030% or less. The N content is preferably 0.0020% or less, and more preferably 0.0015% or less. There is no particular lower limit for the N content (it may be 0%), but 0.0005% is the practical lower limit in consideration of the manufacturing cost.
[0026] Ti: 0.0030% or less Ti is an element that forms precipitates and increases iron loss. If the Ti content exceeds 0.0030%, the increase in iron loss is significant, so the Ti content is set to 0.0030% or less. The Ti content is preferably 0.0020% or less, and more preferably 0.0015% or less. There is no particular lower limit for the Ti content (it may be 0%), but 0.0005% is the practical lower limit in consideration of the manufacturing cost.
[0027] B: 0.0020% or less B is an element that forms precipitates and increases iron loss. If the B content exceeds 0.0020%, the increase in iron loss is significant. Therefore, the B content is set to 0.0020% or less. The B content is preferably 0.0010% or less, and more preferably 0.0005% or less. There is no particular lower limit for the B content (it may be 0%), but in consideration of industrial purification technology, 0.0001% is the practical lower limit.
[0028] Sn: 0 to 0.200% Sb: 0 to 0.1000% Sn and Sb are elements that suppress surface nitridation and contribute to reducing iron loss, so the electrical steel sheet according to this embodiment may contain one or both of Sn and Sb in the chemical composition of the steel sheet. Sn and Sb are elements that have similar effects, but the degree of their influence differs. Therefore, when the Sn content in mass percent is [Sn] and the Sb content is [Sb], the range of [Sn] + 2 × [Sb] is controlled. Specifically, in order to obtain the effect of improving the magnetic properties, it is preferable that [Sn]+2×[Sb] is 0.020 or more, and more preferably 0.050 or more. On the other hand, if [Sn] + 2 × [Sb] exceeds 0.200, the toughness of the steel plate deteriorates. Therefore, [Sn] + 2 × [Sb] is set to 0.200 or less, and preferably 0.100 or less. The respective contents of Sn and Sb are in the ranges that satisfy [Sn]+2×[Sb]≦0.200, that is, the Sn content is 0 to 0.200%, and the Sb content is 0 to 0.1000%.
[0029] Remainder: Fe and impurities In the electrical steel sheet according to this embodiment, the balance excluding the above elements may be Fe and impurities. Impurities are elements that are mixed in the steel raw materials and / or the steelmaking process and are permissible within a range that does not impair the properties of the electrical steel sheet according to this embodiment. On the other hand, other elements may be contained in place of a part of Fe. For example, Cu and Ni may be contained as long as their contents do not exceed 0.1% each. Other elements may also be contained within a range not exceeding 0.05% each.
[0030] The chemical composition of steel plate may be measured by a general analysis method for steel. For example, the chemical composition may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, the chemical composition is identified by measuring a test piece taken from the steel plate with a specified measuring device under conditions based on a previously prepared calibration curve. C and S may be measured using the combustion-infrared absorption method, and N may be measured using the inert gas fusion-thermal conductivity method. If the surface has an insulating coating, it may be mechanically removed using a minitor or the like before being subjected to analysis.
[0031] <WH / WL (deviation of magnetic properties), which is the ratio of the maximum value WH to the minimum value WL of iron loss W10 / 400, is 1.10 or less> The magnetic steel sheet according to the present embodiment has a small deviation in magnetic properties in the width direction of the steel sheet. Specifically, assuming that the sheet width of the steel sheet of the non-oriented magnetic steel sheet is W, W10 / 400 (measurement value of iron loss at 400 Hz and magnetic flux density of 1.0 T) is measured by the SST method (Single Sheet Tester method) defined in JIS C2556:2015 at a W / 10 part, a W / 4 part, and a W / 2 part located at W / 2 of the sheet width from the end in the width direction, and WH / WL (deviation of magnetic properties), which is the ratio of the maximum value WH to the minimum value WL, is calculated. WH / WL is 1.10 or less. If the WH / WL ratio exceeds 1.10, when non-oriented electrical steel sheets are laminated to make a motor, the cogging torque, i.e., rotation irregularities, will increase, and the sound generated during rotation will be loud, which is undesirable. Therefore, by controlling the magnetic property deviation WH / WL to 1.10 or less, the cogging torque, i.e., rotation irregularities, can be reduced, and the sound generated during rotation can be reduced (for example, to 40db or less). It is believed that the suppression of deviation in magnetic properties in the width direction is achieved by controlling the distribution of inclusions and the state of distortion in minute regions, but since it is not easy to accurately evaluate these, the electrical steel sheet according to this embodiment is characterized by the above-mentioned WH / WL. In addition, in this embodiment, the ratio of the maximum value WH to the minimum value WL of W10 / 400 is specified, instead of other iron loss values such as W15 / 50. W10 / 400 is a characteristic required for devices in which it is expected to be used, but since it is easily affected by residual strain, it is more difficult to control than other iron loss values such as W15 / 50, and the variation is likely to be large. Therefore, even if the ratio of the maximum value to the minimum value of W15 / 50 is 1.10 or less, for example, WH / WL is not necessarily 1.10 or less.
[0032] Measuring W10 / 400 at W / 10 parts using the SST method (Single Sheet Tester method) specified in JISC2556:2015 means taking a 55mm square sample so that it contains W / 10 parts, and measuring W10 / 400 using the sample using the SST method. The same applies to measurements at W / 4 parts and W / 2 parts.
[0033] Furthermore, in the electrical steel sheet according to this embodiment, it is preferable that the deviation in magnetic properties in the width direction is small even in the case of a weaker magnetic field. For example, when W5 / 400 is measured by the SST method specified in JIS C2556:2015 for W / 10 parts, W / 4 parts, and W / 2 parts, and WH2 / WL2 (deviation of magnetic properties) is calculated as the ratio of the maximum value WH2 to the minimum value WL2, it is preferable that WH2 / WL2 is 1.10 or less. WH2 / WL2 can be measured in a manner similar to WH / WL.
[0034] The wider the width of the steel sheet (sheet width), the greater the deviation in magnetic properties in the width direction tends to be, but with the electrical steel sheet according to this embodiment, as described above, the deviation in magnetic properties can be reduced at least when the width is 1000 mm or less. By carrying out stricter control, the deviation in magnetic properties can be reduced when the width is 1300 mm or less.
[0035] <Insulating coating> The electrical steel sheet according to this embodiment may have an insulating coating formed on the surface of the steel sheet. This insulating coating may be a known coating. For example, Al 2 O 3 An example of the coating is a coating made of
[0036] <Manufacturing method of non-oriented electrical steel sheet> The method for producing the electrical steel sheet according to this embodiment is not particularly limited, but is preferably a method that includes the following steps, each of which is carried out under preferred conditions. (I) a hot rolling process in which the slab is heated and hot rolled to obtain a hot-rolled sheet; (II) A hot-rolled sheet annealing process for annealing a hot-rolled sheet (coil); (III) a cold rolling process in which the hot-rolled sheet after the hot-rolled sheet annealing process is pickled and cold-rolled to obtain a cold-rolled sheet; (IV) A final annealing process in which the cold-rolled sheet is final annealed. Furthermore, the method may further include the following steps. (V) An insulating coating formation process in which an insulating coating is formed on the steel sheet (non-oriented electrical steel sheet) after the final annealing process. Preferred conditions for each step are described below. Publicly known conditions can be applied to conditions not described.
[0037] [Hot rolling process] In the hot rolling process, the slab is heated and hot rolled to obtain a hot rolled sheet, which is then wound into a coil. The chemical composition of the slab to be used may be determined according to the chemical composition of the steel sheet to be ultimately obtained as the non-oriented electrical steel sheet. The heating temperature of the slab is preferably 1050 to 1250°C. If the heating temperature is less than 1050°C, the coiling temperature cannot be maintained at a certain temperature or higher, which may result in deterioration of the magnetic properties of the product. On the other hand, if the heating temperature exceeds 1250°C, the precipitates may be excessively dissolved, and fine precipitates may be formed during hot rolling, which may deteriorate the iron loss of the product. More preferably, the slab heating temperature is 1100 to 1200°C. The temperature at the time of passing through the final stand of the finish rolling in the hot rolling (finish rolling temperature) is preferably in the range of 800 to 1000°C. Outside this range, it is difficult to set the coiling temperature within the range described below. The finish rolling temperature is more preferably 820 to 950°C, and further preferably 900 to 1000°C. If the thickness of the hot rolled sheet is too thick, the magnetic properties of the product sheet deteriorate, whereas if it is too thin, the necessary temperature cannot be ensured, so the thickness is preferably 1.6 to 2.8 mm, and more preferably 1.8 to 2.5 mm. The coiling temperature in hot rolling is preferably in the range of 650 to 900°C. If the coiling temperature is less than 650°C, the finish rolling temperature will be low, and there is a concern that the rolling load will be high, and if the coiling temperature exceeds 900°C, the coil surface may be oxidized, causing deterioration of the appearance. The coiling temperature is more preferably in the range of 680 to 850°C, and even more preferably in the range of 700 to 800°C.
[0038] [Hot-rolled sheet annealing process] In the hot-rolled sheet annealing process, the hot-rolled sheet after the hot rolling is annealed (hot-rolled sheet annealing). The soaking temperature is preferably 850 to 1000°C. If the soaking temperature is less than 850°C, the magnetic properties may deteriorate. On the other hand, if the soaking temperature is more than 1000°C, the toughness may decrease. The soaking temperature is more preferably in the range of 900°C to 950°C. The soaking time is preferably 10 to 180 seconds. In consideration of the magnetic properties and productivity, the soaking time is more preferably 15 to 120 seconds. Annealing may be performed in a coiled state, but annealing may be performed after rewinding as necessary.
[0039] [Cold rolling process] The hot-rolled sheet after the hot-rolled sheet annealing process is uncoiled, pickled under known conditions, and then cold-rolled. The cold rolling may be a single cold rolling (a series of cold rolling without intermediate annealing) or may be two or more cold rollings with intermediate annealing. The thickness of the cold-rolled sheet after the cold rolling process (equivalent to the base steel sheet of the final product) is preferably 0.20 to 0.50 mm from the viewpoint of magnetic properties. Furthermore, in consideration of productivity, the thickness of the cold-rolled sheet is more preferably in the range of 0.25 to 0.50 mm. The total rolling ratio in the final cold rolling step is preferably 75 to 90% from the viewpoint of magnetic properties, and more preferably 80 to 88% in consideration of magnetic properties and productivity.
[0040] [Finish annealing process] In the finish annealing process, the cold-rolled steel sheet (cold-rolled sheet) is subjected to finish annealing. The heating conditions in the final annealing step are not particularly limited. From the viewpoint of magnetic properties, the soaking temperature during the final annealing is preferably 950 to 1100°C, more preferably 1000 to 1100°C. As for the annealing time, the soaking time is preferably 10 to 180 seconds. In consideration of the magnetic properties and productivity, the soaking time is more preferably 15 to 60 seconds.
[0041] In the finish annealing process, annealing is performed in a continuous annealing furnace so that PT = W × t × L × T / Vc > 100, where W (mm) is the width of the cold-rolled sheet to be subjected to the finish annealing, t (mm) is the thickness, L (m) is the length between the hearth rolls in the soaking zone in the continuous annealing furnace (the distance between the centers of adjacent hearth rolls), T (MPa) is the tension applied to the steel sheet during annealing, and Vc (°C / sec) is the average cooling rate from the end of soaking to 650°C. By making PT exceed 100, the deviation of the magnetic properties in the width direction can be made small (1.10 or less). There is no upper limit for PT, but it may be, for example, 1000 or less. PT may be 200 or more, or 400 or more.
[0042] The reason why PT is set to more than 100 will be explained based on an experimental example conducted by the present inventors.
[0043] (Experimental Example 1) The slab, which contained the following chemical composition by mass: C: 0.001%, Si: 3.0%, Al: 0.50%, Mn: 0.2%, P: 0.010%, S: 0.0100%, N: 0.0010%, Ti: 0.0010%, and B: 0.0010%, was heated to 1160°C, and then hot-rolled to a finish rolling temperature of 850°C to obtain a hot-rolled sheet with a thickness of 2.0 mm. This hot-rolled sheet was wound into a coil at 650°C (coiling temperature). The coil was uncoiled, heated to 1000° C. and held at temperature for 60 seconds, then uncoiled and air cooled. The coil was recoiled, pickled, and then cold rolled to obtain a cold rolled sheet having a width of 1000 mm and a thickness of 0.50 mm. This cold-rolled sheet was subjected to finish annealing by heating to 1000° C. (soaking temperature) and holding (soaking) for 30 seconds. During the final annealing, the length L between the hearth rolls in the soaking zone is set to 2.0 to 5.0 m, and the tension T applied to the steel sheet is set to 2 to 6 N / mm 2 The average cooling rate Vc from the end of soaking to 650°C was changed from 4 to 10°C / sec. Samples of 55 mm square size were sheared from the steel sheet after final annealing at each location of the W / 10, W / 4, and W / 2 sections, and W10 / 400 (the measured value of iron loss at 400 Hz with a magnetic flux density of 1.0 T) was measured using the SST method (Single Sheet Tester method) of JIS C2556:2015, and the ratio of the maximum value WH to the minimum value WL was taken as the magnetic property deviation. As a result, Fig. 1 to As shown, by setting the PT to over 100, the WH / WL ratio could be controlled to 1.10 or less.
[0044] Therefore, in the method for producing an electrical steel sheet according to this embodiment, finish annealing is performed so that PT is more than 100. The reason why it is preferable to increase the distance between the hearth rolls is that when the distance between the hearth rolls is increased, the catenary of the steel sheet in the width direction becomes larger, and large strain is uniformly imparted in the width direction. Since the residual strain due to cooling is smaller than the strain caused by the catenary, it is considered that even if the residual strain due to cooling is non-uniform in the width direction, the effect is small.
[0045] In addition, the reason why it is preferable to increase the tension is believed to be because increasing the tension imparts a large strain uniformly in the width direction. Normally, increasing the tension reduces the catenary somewhat, but the impact of iron loss degradation caused by the elongation of the steel sheet itself is large. Since the residual strain caused by cooling is small compared to the strain caused by increasing the tension, even if the residual strain caused by cooling is non-uniform in the width direction, the impact is believed to be small. On the other hand, the reason why it is better to have a smaller average cooling rate to 650°C after the soaking in the final annealing is presumably because, when the average rate is large, the effect of residual strain due to cooling cannot be ignored, and the deviation of the magnetic properties in the width direction becomes large. Even if the recrystallization rate is controlled by, for example, hot-rolled sheet annealing before the finish annealing process to reduce the deviation in the recrystallization rate depending on the steel sheet position, the magnetic properties will vary unless the subsequent processes are adequately controlled. Therefore, the cold rolling conditions and finish annealing are important.
[0046] In order to achieve a predetermined magnetic property deviation even with a wider sheet width, it is preferable to increase the soaking temperature in the finish annealing step, for example to 1000° C. or higher. In addition, in order to reduce the deviation of low magnetic field iron loss, PT is preferably set to 600 or more, and more preferably set to 700 or more.
[0047] [Insulating film formation process] When the electrical steel sheet according to this embodiment is a non-oriented electrical steel sheet having an insulating coating on the surface of the steel sheet (base steel sheet), in addition to the above steps, an insulating coating forming step may be provided in which an insulating coating is formed on the surface of the steel sheet after the finish annealing step, as in the manufacturing process of conventional non-oriented electrical steel sheets. The conditions for the insulating coating forming step may be the same as those for the insulating coating step of conventional non-oriented electrical steel sheets. EXAMPLES
[0048] The slabs with the adjusted chemical composition were cast, heated under one of the conditions in Table 2, hot-rolled to form hot-rolled sheets, and then coiled. The hot-rolled sheets were subjected to hot-rolled sheet annealing under any of the conditions in Table 2, and then cooled to room temperature. Thereafter, the steel sheet was pickled and cold rolled to obtain a steel sheet (cold rolled sheet) having a thickness of 0.25 to 0.50 mm. This steel sheet (cold rolled sheet) was subjected to finish annealing under any of the conditions shown in Table 2 to obtain a non-oriented electrical steel sheet. An insulating coating was formed on the surface of some of the non-oriented electrical steel sheets.
[0049] The chemical composition of the steel sheet of the obtained non-oriented electrical steel sheet was measured and it was found to contain the chemical components shown in Table 1, with the remainder being Fe and impurities.
[0050] For non-oriented electrical steel sheets (C1 to C20, c1 to c20) having any of the chemical compositions shown in Table 1 and manufactured by any of the manufacturing methods shown in Table 2, W10 / 400 (measured iron loss value at 400 Hz at a magnetic flux density of 1.0 T) was measured at each location of W / 10, W / 4, and W / 2 by the SST method (Single Sheet Tester method) of JISC2556:2015. At that time, samples were taken from each of W / 10, W / 4, and W / 2 at a certain rolling direction position, and the values were taken as the iron loss value at each position. In addition, WH / WL (deviation of magnetic properties), which is the ratio of the maximum value WH to the minimum value WL of the iron loss values at each position, was calculated. In addition, for some examples, the ratio WH2 / WL2 of the maximum value WH2 to the minimum value WL2 of W5 / 400 was obtained as the deviation of the magnetic properties of the iron loss in a lower magnetic field. The above measurements were carried out three times at positions spaced apart by one hoop turn in the rolling direction, and the values at the positions where WH / WL and WH2 / WL2 were the largest were shown in Table 3. The results are shown in Table 3. When the iron loss at each position was 25.0 W / kg or less and the WH / WL was 1.10 or less, it was determined that the magnetic properties were good and the deviation of the magnetic properties in the width direction was small.
[0051] [Table 1]
[0052] [Table 2]
[0053] [Table 3]
[0054] As shown in Tables 1 to 3, steel sheets having a specified chemical composition and subjected to finish annealing under conditions where the parameter PT of the finish annealing conditions was greater than 100 had good magnetic properties and small deviation in the width direction. Furthermore, when PT was higher, the deviation in the width direction of iron loss was small even in a low magnetic field. Furthermore, when the soaking temperature in the finish annealing was high, the deviation in the width direction of iron loss was small even in the case of a wide width. On the other hand, in the comparative examples in which the chemical composition was outside the range of the present invention and / or the manufacturing method was outside the preferred range, the deviation in the magnetic properties (iron loss) in the width direction was large. [Industrial Applicability]
[0055] According to the present invention, it is possible to produce a non-oriented electrical steel sheet having good magnetic properties and small deviation in the magnetic properties in the width direction. Such non-oriented electrical steel sheets have a high industrial applicability because they can suppress cogging torque, i.e., rotation irregularities, when laminated to form a motor.
Claims
1. Including steel plate, The chemical composition of the steel sheet is, in mass%, C: 0.0030% or less, Si: 1.0-3.5%, Al: 0.10-2.00%, Mn: 0.1 to 2.0%, P: 0.20% or less, S: 0.0030% or less, N: 0.0030% or less, Ti: 0.0030% or less, B: 0.0020% or less, Sn: 0-0.200%, Sb: 0 to 0.1000%, and The balance is composed of Fe and impurities. When the Sn content, in mass%, is [Sn] and the Sb content is [Sb], the following formula (1) is satisfied: When the width of the steel plate is W, in a W / 10 portion, which is a portion at a position W / 10 of the plate width from an end in the width direction, a W / 4 portion, which is a portion at a position W / 4, and a W / 2 portion, which is a portion at a position W / 2, a ratio WH / WL of a maximum value WH and a minimum value WL of an iron loss W10 / 400 is 1.10 or less. A non-oriented electrical steel sheet. [Sn]+2×[Sb]≦0.200 (1)
2. The [Sn] and [Sb] satisfy the following formula (2): The non-oriented electrical steel sheet according to claim 1 . 0.020≦[Sn]+2×[Sb]≦0.200 (2)
3. An insulating coating is formed on the surface of the steel plate. The non-oriented electrical steel sheet according to claim 1 or 2.
Citation Information
Patent Citations
Method for preparing high-strength non-oriented silicon steel based on nano Cu precipitation strengthening
CN106282781A
Manufacture of nonoriented electrical steel sheet having remarkably small iron loss
JP1988047333A
Manufacture of nonoriented silicon steel sheet
JP1995054052A
Manufacture of silicon steel sheet having magnetic property uniform in coil-width direction
JP1997316536A
Non-oriented silicon steel sheet for electric vehicle motor and its production
JP1999222653A