Groove depth monitoring system, electromagnetic steel sheet manufacturing apparatus, groove depth monitoring method, and groove depth monitoring program

The groove depth monitoring system addresses the issue of shallow grooves in electromagnetic steel sheets by using torque and spatter detection to ensure adequate groove depth, improving iron loss performance.

JP7569000B1Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024538493
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-08
Filing Date
2024-03-01
Publication Date
2024-10-17
Estimated Expiration
2044-03-01

AI Technical Summary

Technical Problem

Existing methods for monitoring groove depth in electromagnetic steel sheets formed by laser or electron beam irradiation fail to detect decreases in beam output or focus shift, leading to shallow grooves that reduce iron loss improvement in electrical steel sheets.

Method used

A groove depth monitoring system that utilizes a torque acquisition unit to measure rotational torque from a polishing brush roll and a sputter amount acquisition unit to detect spatter, determining groove depth based on predefined reference values to ensure grooves meet minimum depth requirements.

Benefits of technology

The system effectively detects and prevents shallow grooves by accurately monitoring beam output and focus shift, maintaining optimal groove depth and enhancing iron loss improvement in electromagnetic steel sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569000000001
    Figure 0007569000000001
  • Figure 0007569000000002
    Figure 0007569000000002
  • Figure 0007569000000003
    Figure 0007569000000003
Patent Text Reader

Abstract

The groove depth monitoring system includes a torque acquisition unit that acquires the rotational torque generated when an abrasive brush roll is used to remove material adhering to the surface of a steel plate on which a groove has been formed by a beam, and a groove depth determination unit that determines whether the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired by the torque acquisition unit and a predetermined reference rotational torque.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in the present application relates to a groove depth monitoring system, an electromagnetic steel sheet manufacturing apparatus, a groove depth monitoring method, and a groove depth monitoring program. [Background technology]

[0002] There is a manufacturing method for grain-oriented electrical steel sheet in which a laser beam is irradiated onto the surface of the grain-oriented electrical steel sheet to form grooves, thereby subdividing the magnetic domains of the grain-oriented electrical steel sheet and improving iron loss (see, for example, JP 2017-122264 A).

[0003] There is also a laser groove processing monitoring method that monitors the shape of a groove formed on the surface of a grain-oriented electrical steel sheet by a laser beam (see, for example, JP 2019-512047 A).

[0004] The laser groove processing monitoring method disclosed in JP 2019-512047 A monitors the spatter that occurs when a laser beam is irradiated onto the surface of a grain-oriented electromagnetic steel sheet to form a groove, and determines the shape of the groove formed on the surface of the grain-oriented electromagnetic steel sheet based on the spatter. Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, when forming grooves by irradiating the surface of a rolled steel sheet, which is the material for the electromagnetic steel sheet, with a beam such as a laser beam or an electron beam, if the output of the beam decreases or the focus of the beam on the surface is shifted, the grooves will become shallower and the iron loss improvement rate of the electromagnetic steel sheet may decrease.

[0006] However, simply monitoring the amount of spatter generated when a beam is irradiated onto the surface of a rolled steel sheet to form grooves may not be enough to detect a decrease in beam output or a shift in the focus of the beam relative to the surface of the rolled steel sheet, which may result in the depth of the grooves formed on the surface of the electromagnetic steel sheet being shallow.

[0007] The technology disclosed in the present application takes into consideration the above-mentioned circumstances and aims to prevent the depth of grooves formed in the surface of an electromagnetic steel sheet from becoming shallow. [Means for solving the problem]

[0008] The groove depth monitoring system according to the first aspect comprises: a torque acquisition unit that acquires a rotational torque generated when an abrasive brush roll is used to remove deposits that have adhered to the surface of the steel plate on which grooves have been formed by the beam; a groove depth determination unit that determines whether or not a depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired by the torque acquisition unit and a predetermined reference rotational torque; Equipped with.

[0009] According to the above aspect, the torque acquisition unit acquires the rotational torque generated when the abrasive brush roll removes deposits attached to the surface of the steel plate on which the grooves are formed by the beam. The groove depth determination unit determines whether the depth of the grooves formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired by the torque acquisition unit and a predetermined reference rotational torque.

[0010] Here, for example, by monitoring the rotational torque acquired by the torque acquisition unit, it is possible to detect a steel plate in which the depth of the groove is less than the reference value due to a decrease in the output of the beam, and therefore it is possible to prevent the depth of the groove formed on the surface of the steel plate from becoming shallow.

[0011] A groove depth monitoring system according to a second aspect is the groove depth monitoring system according to the first aspect, a sputter amount acquisition unit that acquires an amount of sputtering generated when the beam is irradiated onto the surface of the steel plate to form the groove, The groove depth determination unit determines whether the depth of the groove formed on the surface of the steel plate is equal to or greater than a standard value based on the sputter amount acquired by the sputter amount acquisition unit, a predetermined standard sputter amount, the rotational torque acquired by the torque acquisition unit, and the standard rotational torque.

[0012] According to the above aspect, the sputter amount acquisition unit acquires the amount of sputtering generated when a groove is formed on the surface of the steel sheet by irradiating a beam on the surface of the steel sheet, and the groove depth determination unit determines whether the depth of the groove formed on the surface of the steel sheet is equal to or greater than a reference value based on the amount of sputtering acquired by the sputter amount acquisition unit, a predetermined reference amount of sputtering, the rotational torque acquired by the torque acquisition unit, and the reference rotational torque.

[0013] This makes it possible to detect steel plates in which the depth of grooves is less than the reference value due to, for example, a decrease in beam output, a deviation in focus of the beam with respect to the surface of the steel plate, etc. Therefore, it is possible to prevent the depth of grooves formed on the surface of the steel plate from becoming shallow.

[0014] Here, the amount of sputtering generated when a groove is formed on the surface of a steel sheet by irradiating the surface with a beam basically decreases as the depth of the groove formed on the surface becomes shallower. Therefore, by monitoring the amount of sputtering acquired by the sputtering amount acquisition unit, the depth of the groove formed on the surface of the steel sheet can be estimated.

[0015] However, in a range where the beam defocus amount with respect to the steel sheet surface is small, as the beam defocus amount increases, the sputter amount decreases once and then increases again. Therefore, in a range where the beam defocus amount with respect to the steel sheet surface is small, it may not be possible to detect the beam defocus amount by simply monitoring the sputter amount acquired by the sputter amount acquisition unit.

[0016] Here, in the range where the deviation of the focus of the beam from the surface of the steel sheet is small, the viscosity of the spatter generated increases due to changes in the surface temperature of the steel sheet, etc., and the particle size of the spatter and other deposits on the surface of the steel sheet increases. As a result, the rotational torque generated when the deposits on the surface of the steel sheet are removed by the abrasive brush roll also increases.

[0017] Therefore, the groove depth determination unit monitors the rotational torque acquired by the torque acquisition unit in addition to the sputter amount acquired by the sputter amount acquisition unit. This makes it possible to detect the beam focus deviation even in a range where the beam focus deviation from the steel sheet surface is small. This makes it possible to further prevent the depth of the groove formed on the steel sheet surface from becoming shallow.

[0018] A groove depth monitoring system according to a third aspect is the groove depth monitoring system according to the second aspect, The groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when the sputtering amount acquired by the sputtering amount acquisition unit is equal to or greater than the reference sputtering amount and the rotational torque acquired by the torque acquisition unit is equal to or less than the reference rotational torque.

[0019] According to the above aspect, when the sputter amount acquired by the sputter amount acquisition unit is equal to or greater than the reference sputter amount and the rotational torque acquired by the torque acquisition unit is equal to or less than the reference rotational torque, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value. This makes it possible to easily determine whether the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value.

[0020] A groove depth monitoring system according to a fourth aspect is the groove depth monitoring system according to the second or third aspect, the reference sputter amount is determined based on the amount of sputtering generated when forming the groove having the reference depth on the surface of the steel plate, The reference rotational torque is determined based on the rotational torque generated when the abrasive brush roll removes the adhesions attached to the surface of the steel plate in which the grooves having the reference depth are formed.

[0021] According to the above aspect, the reference sputter amount is determined based on the amount of sputter generated when grooves having a reference depth are formed on the surface of the steel sheet, and the reference rotational torque is determined based on the rotational torque generated when deposits attached to the surface of the steel sheet on which grooves having a reference depth are formed are removed by the abrasive brush roll.

[0022] The groove depth determination unit determines whether the depth of the groove formed on the surface of the steel sheet is equal to or greater than a reference value based on the sputter amount obtained by the sputter amount acquisition unit, the predetermined reference sputter amount, the rotational torque obtained by the torque acquisition unit, and the reference rotational torque. This improves the determination accuracy of the groove depth determination unit. Therefore, it is possible to further prevent the depth of the groove formed on the surface of the steel sheet from becoming shallow.

[0023] A groove depth monitoring system according to a fifth aspect is the groove depth monitoring system according to the fourth aspect, the reference sputter amount is determined based on the amount of sputtering generated when the groove is formed on the surface of the steel sheet by the beam when the amount of focus shift of the beam irradiated on the surface of the steel sheet is 0 and the power of the beam is a reference value; the reference rotational torque is determined based on a rotational torque generated when the deposit attached to the surface of the steel plate in which the grooves are formed by the beam is removed by the abrasive brush roll in a case where the amount of focus shift of the beam irradiated to the surface of the steel plate is 0 and the power of the beam is a reference value; When formula (1) is satisfied, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value. 1 ≥ S / S0 ≥ C1, and C2 ≤ T / T0 ≤ C3 (1) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1:S1 / S0 S1: The minimum amount of spatter generated when forming a groove of a standard depth on the surface of a steel plate T: Rotational torque acquired by the torque acquisition unit T0: Reference rotation torque C2:T1 / T0 T1: The minimum rotational torque generated when removing the deposits on the surface of a steel plate with grooves of a reference depth by an abrasive brush roll. C3:T2 / T0 T2: The maximum rotational torque generated when removing the deposits on the surface of a steel plate with grooves of a reference depth by using an abrasive brush roll. It is.

[0024] According to the above aspect, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when formula (1) is satisfied, which makes it easy to determine whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value.

[0025] A groove depth monitoring system according to a sixth aspect is the groove depth monitoring system according to the fifth aspect, The C1 is set to 0.83, The C2 is set to 0.89, The C3 is set to 1.11.

[0026] According to the above aspect, it is possible to easily determine whether or not the depth of a groove formed on the surface of a steel plate is equal to or greater than a reference value.

[0027] A groove depth monitoring system according to a seventh aspect is the groove depth monitoring system according to the fourth aspect, the reference sputter amount is determined based on the amount of sputtering generated when the groove is formed on the surface of the steel sheet by the beam when the amount of focus shift of the beam irradiated on the surface of the steel sheet is 0 and the power of the beam is a reference value; the reference rotational torque is determined based on a rotational torque generated when the deposit attached to the surface of the steel plate in which the grooves are formed by the beam is removed by the abrasive brush roll when the amount of focus shift of the beam irradiated to the surface of the steel plate is 0 or the power of the beam is a reference value; When formula (2) is satisfied, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value. 1 ≥ S / S0 ≥ C1, and T1 ≤ T ≤ T2 (2) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1:S1 / S0 S1: The minimum amount of spatter generated when forming a groove of a standard depth on the surface of a steel plate T: Rotational torque acquired by the torque acquisition unit T1: Reference rotational torque. The minimum rotational torque that occurs when removing deposits from the surface of a steel plate with grooves of a reference depth by an abrasive brush roll. T2: Reference rotational torque. This is the maximum rotational torque that occurs when removing deposits from the surface of a steel plate on which grooves with a reference depth are formed using an abrasive brush roll. It is.

[0028] According to the above aspect, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when formula (2) is satisfied, which makes it easy to determine whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value.

[0029] A groove depth monitoring system according to an eighth aspect is the groove depth monitoring system according to the seventh aspect, The C1 is set to 0.83, The T1 is set to 800 [Nm], The T2 is set to 1000 [Nm].

[0030] According to the above aspect, it is possible to easily determine whether or not the depth of a groove formed on the surface of a steel plate is equal to or greater than a reference value.

[0031] A groove depth monitoring system according to a ninth aspect is the groove depth monitoring system according to the first aspect, The reference rotational torque is determined based on the rotational torque generated when the abrasive brush roll removes the adhesion material attached to the surface of the steel plate in which the groove of the reference depth has been formed by the beam when the focus deviation of the beam irradiated onto the surface of the steel plate is 0.

[0032] According to the above aspect, the reference rotational torque is determined based on the rotational torque generated when an abrasive brush roll removes adhesions that have adhered to the surface of a steel plate in which a groove of a reference depth has been formed by the beam when the focus deviation of the beam irradiated onto the surface of the steel plate is 0.

[0033] The groove depth determination unit determines whether the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired by the torque acquisition unit and a predetermined reference rotational torque. Therefore, it is possible to prevent the depth of the groove formed on the surface of the steel plate from becoming shallow.

[0034] A groove depth monitoring system according to a tenth aspect is the groove depth monitoring system according to the ninth aspect, the reference rotational torque is determined based on a rotational torque generated when removing, by the abrasive brush roll, the deposit attached to the surface of the steel plate in which the groove having the depth of the reference value is formed by the beam, when the amount of focus shift of the beam irradiated to the surface of the steel plate is 0 and the power of the beam is a reference value; When formula (3) is satisfied, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value. T1≦T≦T0 (3) however, T: Rotational torque acquired by the torque acquisition unit It is. T0: Reference rotation torque T1: The minimum rotational torque generated when removing the deposits on the surface of a steel plate with grooves of a reference depth by an abrasive brush roll. It is.

[0035] A groove depth monitoring system according to an eleventh aspect is the groove depth monitoring system according to the tenth aspect, The T0 is set to 900 [Nm]. The T1 is set to 800 [Nm].

[0036] According to the above aspect, the groove depth determination unit determines that the depth of the groove formed on the surface of the steel sheet is equal to or greater than the reference value when formula (3) is satisfied, which makes it easy to determine whether or not the depth of the groove formed on the surface of the steel sheet is equal to or greater than the reference value.

[0037] The steel plate manufacturing apparatus according to the twelfth aspect comprises: a beam irradiation device that irradiates a beam onto a surface of a steel plate, which is a material for the steel plate, to form grooves; an abrasive brush roll for removing deposits adhering to the surface of the steel plate in which the grooves are formed; A steel plate groove depth monitoring system according to any one of the first to eleventh aspects; Equipped with.

[0038] According to the above aspect, it is possible to manufacture a steel plate having grooves formed on the surface thereof, the grooves having a depth equal to or greater than the reference value.

[0039] A groove depth monitoring method according to a thirteenth aspect includes the steps of: a torque acquisition step of acquiring a rotational torque generated when removing, by an abrasive brush roll, deposits attached to the surface of the steel plate on which the grooves are formed by the beam; a groove depth determination step of determining whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired in the torque acquisition step and a predetermined reference rotational torque; Equipped with.

[0040] According to the above aspect, in the torque acquisition step, a rotational torque generated when an abrasive brush roll is used to remove deposits from the surface of the steel plate on which grooves have been formed by the beam is acquired. In the groove depth determination step, it is determined whether or not the depth of the grooves formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired in the torque acquisition step and a predetermined reference rotational torque.

[0041] Here, for example, by monitoring the rotational torque acquired in the torque acquisition process, it is possible to detect a steel plate in which the depth of the groove is less than the reference value due to a decrease in the output of the beam, and therefore it is possible to prevent the depth of the groove formed on the surface of the steel plate from becoming shallow.

[0042] A groove depth monitoring program according to a fourteenth aspect of the present invention includes: a torque acquisition step of acquiring a rotational torque generated when removing, by an abrasive brush roll, deposits attached to the surface of the steel plate on which the grooves are formed by the beam; a groove depth determination step of determining whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired in the torque acquisition step and a predetermined reference rotational torque; The method causes a computer to execute a process including the steps of:

[0043] According to the above aspect, it is possible to obtain the same effects and advantages as the groove depth monitoring method according to the thirteenth aspect. Effect of the Invention

[0044] According to the technique disclosed in the present application, it is possible to prevent the depth of grooves formed in the surface of an electromagnetic steel sheet from becoming shallow. [Brief description of the drawings]

[0045] [Figure 1] 1 is a side view of a manufacturing apparatus for a grain-oriented electrical steel sheet according to an embodiment, viewed from the width direction of a cold-rolled steel sheet. FIG. [Diagram 2] 1 is a side view of a manufacturing apparatus for a grain-oriented electrical steel sheet according to an embodiment, viewed from the width direction of a cold-rolled steel sheet. FIG. [Diagram 3] 1 is a flowchart showing an example of a method for manufacturing a grain-oriented electrical steel sheet according to an embodiment. [Figure 4] 1 is a perspective view of a groove depth monitoring system provided in a manufacturing apparatus for manufacturing grain-oriented electrical steel sheet according to one embodiment, viewed from the front side in the conveying direction of a cold-rolled steel sheet. FIG. [Diagram 5] FIG. 2 is a hardware configuration diagram of a control device of the groove depth monitoring system according to one embodiment. [Figure 6] FIG. 2 is a functional block diagram of a control device of the groove depth monitoring system according to one embodiment. [Figure 7] 10 is a flowchart illustrating an example of a groove depth monitoring process according to an embodiment. [Figure 8] 1 is a table showing test results of a manufacturing test of a grain-oriented electrical steel sheet according to an embodiment. [Figure 9] 1 is a graph showing a relationship between the depth of grooves formed in the surface of a grain-oriented electrical steel sheet and the iron loss improvement rate of the grain-oriented electrical steel sheet in a production test of the grain-oriented electrical steel sheet according to one embodiment. [Figure 10] 1 is a graph showing the relationship between the amount of focus shift of a laser beam with respect to the surface of a grain-oriented electrical steel sheet and the depth of grooves formed on the surface of the grain-oriented electrical steel sheet in a manufacturing test of the grain-oriented electrical steel sheet according to one embodiment. [Figure 11] 1 is a graph showing the relationship between the amount of focus shift of a laser beam with respect to the surface of a grain-oriented electromagnetic steel sheet and the amount of spatter generated when a laser beam is irradiated onto the surface of the grain-oriented electromagnetic steel sheet to form grooves in a manufacturing test of the grain-oriented electromagnetic steel sheet according to one embodiment. [Figure 12] 1 is a graph showing the relationship between the amount of focus shift of a laser beam with respect to the surface of a grain-oriented electromagnetic steel sheet and the rotational torque generated in an abrasive brush roll when the surface of the grain-oriented electromagnetic steel sheet is polished with an abrasive brush roll in a manufacturing test of the grain-oriented electromagnetic steel sheet according to one embodiment. [Figure 13] 1 is a graph showing the relationship between the amount of sputtering generated when a laser beam is irradiated onto the surface of a grain-oriented electromagnetic steel sheet to form grooves, and the depth of the grooves formed on the surface of the grain-oriented electromagnetic steel sheet, in a manufacturing test of the grain-oriented electromagnetic steel sheet according to one embodiment. [Figure 14] 1 is a graph showing the relationship between the rotational torque generated in an abrasive brush roll when the surface of a grain-oriented electromagnetic steel sheet is polished with an abrasive brush roll and the depth of grooves formed on the surface of the grain-oriented electromagnetic steel sheet in a manufacturing test of the grain-oriented electromagnetic steel sheet according to one embodiment. [Figure 15] 1 is a graph showing the relationship between the ratio of the sputter amount to the reference sputter amount and the rotational torque generated in an abrasive brush roll when the surface of a grain-oriented electromagnetic steel sheet is polished with an abrasive brush roll in a manufacturing test of the grain-oriented electromagnetic steel sheet according to one embodiment. [Figure 16] 1 is a graph showing the relationship between the ratio of the sputter amount to a reference sputter amount and the ratio of rotational torque T to a reference rotational torque in a production test of a grain-oriented electrical steel sheet according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] Hereinafter, an embodiment will be described with reference to the drawings. In each drawing, the same or equivalent components are given the same reference numerals. Furthermore, unless otherwise specified, each component is not limited to one, and may be present in multiples.

[0047] (Grain-oriented electrical steel sheet) First, the configuration of the grain-oriented electrical steel sheet according to this embodiment will be described.

[0048] Grain-oriented electrical steel sheets are made by applying a magnetization force to the grains. <100> A grain-oriented electromagnetic steel sheet is an electromagnetic steel sheet in which the magnetization direction (direction) is approximately aligned with the rolling direction (longitudinal direction, transport direction) of the steel sheet. A grain-oriented electromagnetic steel sheet has multiple magnetic domains whose magnetization direction is aligned with the rolling direction. Note that grain-oriented electromagnetic steel sheet is one example of an electromagnetic steel sheet.

[0049] Grain-oriented electromagnetic steel sheets have the characteristic of having less iron loss than normal steel sheets due to their characteristic magnetic domain structure. In order to further reduce the iron loss of grain-oriented electromagnetic steel sheets, a laser beam is irradiated onto the surface of the grain-oriented electromagnetic steel sheet (or the cold-rolled steel sheet that is the material for the grain-oriented electromagnetic steel sheet) to form multiple grooves. The multiple grooves are formed to extend in the width direction of the grain-oriented electromagnetic steel sheet (the direction perpendicular to the rolling direction of the grain-oriented electromagnetic steel sheet) or in a direction slightly inclined from the width direction of the grain-oriented electromagnetic steel sheet, and are arranged at regular intervals in the rolling direction of the grain-oriented electromagnetic steel sheet. These grooves subdivide the magnetic domains of the grain-oriented electromagnetic steel sheet, improving the iron loss of the grain-oriented electromagnetic steel sheet.

[0050] Grain-oriented electromagnetic steel sheets have the property of being easily magnetized in the rolling direction of the grain-oriented electromagnetic steel sheets, and are therefore used as materials for wound iron cores (iron core materials) of winding transformers in which the direction of magnetic field lines is approximately constant. Wound iron cores are formed, for example, by laminating multiple grain-oriented electromagnetic steel sheets and bending (winding) the laminated grain-oriented electromagnetic steel sheets into the shape of an iron core.

[0051] In addition, when forming grooves on the surface of the grain-oriented electromagnetic steel sheet, it is desirable to form the grooves so as to extend in the width direction of the grain-oriented electromagnetic steel sheet, since this can improve the efficiency of improving iron loss. However, for example, when the grain-oriented electromagnetic steel sheet with the grooves formed therein is folded along the folding line along the width direction of the grain-oriented electromagnetic steel sheet in order to use the grain-oriented electromagnetic steel sheet as a winding core of a transformer, the possibility of the grain-oriented electromagnetic steel sheet breaking from the groove increases. Therefore, the grooves are formed so as to extend in a direction slightly inclined from the width direction of the grain-oriented electromagnetic steel sheet. In this case, although the efficiency of improving the iron loss of the grain-oriented electromagnetic steel sheet is somewhat deteriorated, the possibility of breaking when bending the grain-oriented electromagnetic steel sheet can be reduced. When forming grooves on the surface of the grain-oriented electromagnetic steel sheet that extend in a direction slightly inclined from the width direction of the grain-oriented electromagnetic steel sheet, the angle of inclination of the grooves can be appropriately set. Taking into consideration the efficiency of improving the iron loss of the grain-oriented electromagnetic steel sheet and the possibility of breaking, it is preferable to set the angle of inclination of the grooves to, for example, greater than 0° and less than 20°.

[0052] The grain-oriented electrical steel sheet is made of an iron alloy containing Si. The grain-oriented electrical steel sheet has a composition, for example, of Si; 2.5% by mass to 4.0% by mass, C; 0.001% by mass to 0.10% by mass, Mn; 0.05% by mass to 0.20% by mass, acid-soluble Al; 0.001% by mass to 0.040% by mass, N; 0.0002% by mass to 0.012% by mass, S01% by mass to 0.030% by mass, P; 0.01% by mass to 0.04% by mass, with the balance being Fe and unavoidable impurities. The grain-oriented electrical steel sheet has a thickness of, for example, 0.15 mm or more and 0.35 mm or less.

[0053] The surface of the grain-oriented electrical steel sheet is coated with a glass coating. The glass coating is made of, for example, forsterite (Mg2SiO4), spinel (MgAl2O4), and cordierite (Mg2Al4Si5O 18 The glass coating is made of a composite oxide such as Cr, Fe, and H. The thickness of this glass coating is, for example, 1 μm.

[0054] The glass coating is further coated with an insulating coating, which is made of, for example, an insulating coating agent (coating liquid) mainly composed of colloidal silica and phosphate (magnesium phosphate, aluminum phosphate, etc.) or an insulating coating agent (coating liquid) mixed with alumina sol and boric acid.

[0055] (Grain-oriented electrical steel sheet manufacturing equipment) Next, the configuration of the manufacturing apparatus for the grain-oriented electrical steel sheet according to this embodiment will be described.

[0056] 1 and 2 show side views of a grain-oriented electromagnetic steel sheet manufacturing apparatus 10 according to this embodiment, as viewed from the width direction of a cold-rolled steel sheet 12. The grain-oriented electromagnetic steel sheet manufacturing apparatus 10 (hereinafter also referred to as "manufacturing apparatus 10") is an apparatus that manufactures a grain-oriented electromagnetic steel sheet 14 (see FIG. 2). FIGS. 1 and 2 are continuous as a manufacturing line of the manufacturing apparatus 10. A hot-rolled steel sheet, which is a material for the grain-oriented electromagnetic steel sheet 14, is processed by each device included in the manufacturing apparatus 10 as shown in FIG. 1, and then processed by each device included in the manufacturing apparatus 10 as shown in FIG. 2 to become a grain-oriented electromagnetic steel sheet 14 with improved iron loss. The cold-rolled steel sheet is an example of a rolled steel sheet and a steel sheet.

[0057] The manufacturing equipment 10 includes, for example, a finishing rolling machine 15, an oil film removing device 20, a beam irradiation device 30, a polishing device 40, a decarburization annealing device 50, an annealing separator application device 55, a final finish annealing device 60, an insulating coating agent application device 70, and a flattening annealing device 80. The finishing rolling machine 15, the oil film removing device 20, the beam irradiation device 30, the polishing device 40, the decarburization annealing device 50, the annealing separator application device 55, the final finish annealing device 60, the insulating coating agent application device 70, and the flattening annealing device 80 are arranged in this order along a manufacturing line for the grain-oriented electrical steel sheet 14 (see FIG. 2 ) in the transport direction of the grain-oriented electrical steel sheet 14.

[0058] (Finishing rolling mill) As shown in Fig. 1, the finishing mill 15 is a rolling mill that rolls (cold rolls) a hot-rolled steel sheet, which is produced by rolling with a plurality of known roughing mills and is a material for the grain-oriented electrical steel sheet 14 (see Fig. 2), to a desired thickness, thereby producing a cold-rolled steel sheet 12. As the finishing mill 15 according to this embodiment, a known finishing mill can be appropriately used.

[0059] The arrow X indicates the transport direction and rolling direction of the cold-rolled steel sheet 12 (grain-oriented electromagnetic steel sheet 14). In the following, the direction indicated by the arrow X is referred to as the transport direction X. The transport direction X also coincides with the longitudinal direction of the cold-rolled steel sheet 12 (grain-oriented electromagnetic steel sheet 14).

[0060] (Oil film removal device) The oil film removing device 20 is a device that removes oil films adhering to the front surface 12A and the back surface 12B of the cold rolled steel sheet 12 produced by the finishing mill 15.

[0061] Here, when the cold rolled steel sheet 12 is produced by the finishing rolling mill 15, in order to reduce friction between the rolling rolls of the finishing rolling mill 15 and the cold rolled steel sheet 12 (hot rolled steel sheet), oil (rolling oil) is applied to at least one of the rolling rolls and the cold rolled steel sheet 12 (hot rolled steel sheet) before the cold rolled steel sheet 12 (hot rolled steel sheet) is rolled. Therefore, the rolling oil adheres as an oil film to the front surface 12A and the back surface 12B of the cold rolled steel sheet 12 immediately after rolling. The oil film removing device 20 removes the rolling oil (oil film) thus adhered to the front surface 12A and the back surface 12B of the cold rolled steel sheet 12.

[0062] The oil film removing device 20 has a pair of cleaning brush rolls 22. The pair of cleaning brush rolls 22 are arranged on the front surface 12A side and the back surface 12B side of the cold rolled steel sheet 12.

[0063] The cleaning brush roll 22 has a roll 22A and cleaning brushes 22B. The roll 22A is arranged so that the direction of its rotation axis is parallel to the width direction of the cold rolled steel sheet 12. In addition, both ends of the roll 22A in the axial direction are rotatably supported by bearings (not shown). The roll 22A, i.e., the cleaning brush roll 22, is rotated by a motor (not shown). The rotation direction of the cleaning brush roll 22 is not particularly limited. However, it is preferable to rotate the cleaning brush roll 22 in the opposite direction to the conveying direction X of the cold rolled steel sheet 12, because this allows efficient cleaning of the front surface 12A and the back surface 12B of the cold rolled steel sheet 12.

[0064] The cleaning brush 22B has a plurality of bristles extending radially from the roll 22A. The cleaning brush 22B is arranged so that the tips of the plurality of bristles come into contact with the front surface 12A or the back surface 12B of the cold rolled steel sheet 12 so as to be able to remove the oil film adhering to the front surface 12A or the back surface 12B of the cold rolled steel sheet 12. The bristles of the cleaning brush 22B are made of nylon or the like which is softer than the polishing brush 44B described later so as not to cause damage such as scratches to the front surface 12A or the back surface 12B of the cold rolled steel sheet 12. A cleaning agent capable of removing the oil film is supplied to this cleaning brush 22B from a cleaning liquid supply nozzle (not shown). For example, an alkaline cleaning agent is used as the cleaning agent. The oil film removing device 20 rubs the plurality of bristles of the cleaning brush 22B sequentially against the front surface 12A or the back surface 12B of the cold rolled steel sheet 12 according to the rotation of the roll 22A. Thereby, the oil film removing device 20 can scrape off the oil film that has spread on the front surface 12A or the back surface 12B of the cold rolled steel sheet 12 while appropriately using a cleaning agent.

[0065] In addition, immediately after the oil film removing device 20, a dryer (not shown) for drying the cleaning agent and the like adhering to the front surface 12A and the back surface 12B of the cold rolled steel sheet 12 may be provided.

[0066] (Beam irradiation device) The beam irradiation device 30 is, for example, a device that irradiates the surface 12A of the cold-rolled steel sheet 12 from which the oil film has been removed by the oil film removing device 20 with a laser beam L to form grooves.

[0067] Specifically, the beam irradiation device 30 irradiates the front surface 12A of the cold rolled steel sheet 12 with a laser beam L, out of the front surface 12A and the back surface 12B of the cold rolled steel sheet 12. Then, the beam irradiation device 30 scans the front surface 12A of the cold rolled steel sheet 12 with the laser beam L to form grooves on the front surface 12A extending in a direction parallel to the width direction of the cold rolled steel sheet 12 or in a direction inclined at a predetermined angle (preferably an angle greater than 0° and equal to or less than 20°) from the width direction of the cold rolled steel sheet 12 (these directions are also referred to as scanning directions).

[0068] Furthermore, the beam irradiation device 30 forms a plurality of grooves extending in the scanning direction at a predetermined pitch in the conveying direction X of the cold-rolled steel sheet 12. These grooves subdivide the magnetic domains of the grain-oriented electromagnetic steel sheet 14 (see FIG. 2), thereby improving the iron loss of the grain-oriented electromagnetic steel sheet 14.

[0069] The type of laser beam L may be, for example, a fiber laser, a YAG laser, or a CO2 laser. The wavelength of the laser beam L may be, for example, 1060 to 1090 nm or 10.6 μm. The wavelength of the laser beam L may be, for example, 150 nm to 11000 nm (11 μm). The depth of each groove is, for example, 20 μm. The width of the groove is, for example, 50 μm. The interval (pitch) between the grooves is, for example, 3 mm.

[0070] Moreover, the beam irradiation device 30 is not limited to a laser beam, and may be, for example, a device that irradiates the surface 12A of the cold-rolled steel sheet 12 with an electron beam to form grooves.

[0071] (polishing equipment) The polishing device 40 is a device that polishes or grinds off adhesions such as molten protrusions and scattered material that have adhered to the surface 12A of the cold-rolled steel sheet 12 due to sputtering and molten material generated when forming grooves on the surface 12A after irradiation of the laser beam L by the beam irradiation device 30 and before decarburization annealing in the decarburization annealing device 50 described below.

[0072] The polishing device 40 has a pair of backup rolls 42 and a polishing brush roll 44. The backup roll 42 is arranged so that the direction of its rotation axis is parallel to the width direction of the cold-rolled steel sheet 12. In addition, both ends of the backup roll 42 in the axial direction are rotatably supported by bearings (not shown). The backup roll 42 is arranged on the back surface 12B side, which is not formed with grooves, of the front surface 12A and the back surface 12B of the cold-rolled steel sheet 12, and supports the back surface 12B.

[0073] The abrasive brush roll 44 is disposed on the opposite side of the backup roll 42 with respect to the cold rolled steel sheet 12 (the side of the surface 12A on which the grooves are formed). This abrasive brush roll 44 has a roll 44A and an abrasive brush 44B. The roll 44A is disposed so that the direction of its rotation axis is parallel to the width direction of the cold rolled steel sheet 12. In addition, both ends of the roll 44A in the axial direction are rotatably supported by bearings not shown. The roll 44A, i.e., the abrasive brush roll 44, is rotated by a motor or the like not shown. The rotation direction of the abrasive brush roll 44 is not particularly limited. However, it is preferable that the rotation direction of the abrasive brush roll 44 is opposite to the conveying direction X of the cold rolled steel sheet 12, since the surface 12A of the cold rolled steel sheet 12 can be polished efficiently.

[0074] The polishing brush 44B has a plurality of bristles extending radially from the roll 44A. The plurality of bristles are made of nylon harder than the cleaning brush 22B described above, nylon containing abrasive grains, or the like. The tips of the plurality of bristles are arranged so as to contact the surface 12A of the cold-rolled steel sheet 12. The polishing device 40 rubs the tips of the bristles of the polishing brush 44B sequentially against the surface 12A of the cold-rolled steel sheet 12 in accordance with the rotation of the polishing brush roll 44. In this way, the polishing device 40 can scrape off deposits such as molten protrusions protruding from the surface 12A of the cold-rolled steel sheet 12.

[0075] In this embodiment, the direction of the rotation axis of the cleaning brush roll 22 and the polishing brush roll 44 is parallel to the width direction of the cold rolled steel sheet 12, regardless of whether the scanning direction of the laser beam L of the beam irradiation device 30 described above is parallel to the width direction of the cold rolled steel sheet 12 or inclined at a predetermined angle from the width direction of the cold rolled steel sheet 12. However, when the scanning direction of the laser beam L is inclined at a predetermined angle from the width direction of the cold rolled steel sheet 12 and the meandering of the cold rolled steel sheet 12 can be suppressed by adjusting the conveying speed of the cold rolled steel sheet 12, the direction of the rotation axis of the cleaning brush roll 22 and the polishing brush roll 44 may be inclined with respect to the width direction of the cold rolled steel sheet 12 within the range from the direction parallel to the width direction of the cold rolled steel sheet 12 to the above-mentioned predetermined angle. In addition, immediately after the polishing device 40, a dryer (not shown) for drying the abrasive, moisture, and the like adhering to the front surface 12A and back surface 12B of the cold-rolled steel sheet 12 may be provided.

[0076] (Decarburization annealing equipment) The decarburization annealing device 50 is a device that decarburizes and anneals the cold-rolled steel sheet 12 on which grooves are formed. More specifically, the decarburization annealing device 50 decarburizes and anneals (continuous annealing) the cold-rolled steel sheet 12 on which grooves are formed at a predetermined temperature (e.g., 700°C to 900°C) and a predetermined heating time (e.g., 1 minute to 3 minutes). As a result, as described later, primary recrystallization (grain size: 10 to 30 μm) is generated in the cold-rolled steel sheet 12, and an oxide layer mainly composed of silica (SiO2) is formed on the front surface 12A and the back surface 12B of the cold-rolled steel sheet 12.

[0077] Here, when the cold-rolled steel sheet 12 is decarburized and annealed by the decarburization annealing device 50, the cold-rolled steel sheet 12 is decarburized and primary recrystallization (grain size: 10 to 30 μm) is generated in the cold-rolled steel sheet 12. In addition, when the cold-rolled steel sheet 12 is decarburized and annealed, an oxide layer mainly composed of silica (SiO2) is formed on the front surface 12A and the back surface 12B of the cold-rolled steel sheet 12.

[0078] In addition, for example, during or after decarburization annealing and before applying an annealing separator to the front surface 12A and back surface 12B of the cold-rolled steel sheet 12, it is also possible to nitride the cold-rolled steel sheet 12 by heat treatment in an ammonia-containing atmosphere (e.g., 150 to 300 ppm).

[0079] (Annealing separator application device) The annealing separator applicator 55 is an apparatus that applies an annealing separator mainly composed of magnesia (MgO) onto the oxide layers formed by decarburization annealing on the front surface 12A and the back surface 12B of the cold rolled steel sheet 12. After the annealing separator is applied to the cold rolled steel sheet 12 by the annealing separator applicator 55, the cold rolled steel sheet 12 is wound into a coil by a winding device (not shown).

[0080] (Final annealing equipment) As shown in FIG. 2, the final annealing device 60 is a device that anneals the cold rolled steel sheet 12 that has been decarburized and annealed by the decarburization annealing device 50, and generates secondary recrystallization. More specifically, the final annealing device 60 inserts the coil-shaped cold rolled steel sheet 12 that has been decarburized and annealed by the decarburization annealing device 50 and coated with an annealing separator by the annealing separator coating device 55 into a batch furnace and performs heat treatment. The heat treatment conditions are, for example, a heating temperature of 1100°C to 1300°C and a heating time of 20 to 24 hours. This heat treatment causes so-called Goss grains, in which the conveying direction X of the cold rolled steel sheet 12 and the magnetization easy axis coincide with each other, to preferentially grow crystals (generate secondary recrystallization) in the cold rolled steel sheet 12. As a result, a grain-oriented electrical steel sheet 14 with high crystal orientation (crystal orientation) is obtained. During final annealing by the final annealing device 60, the oxide layer reacts with the annealing separator to form a glass coating made of forsterite (Mg2SiO4) on the front surface 12A and back surface 12B of the cold-rolled steel sheet 12, thereby forming a grain-oriented electrical steel sheet 14.

[0081] (insulating coating agent application device) The insulating coating agent applicator 70 unwinds the grain-oriented electrical steel sheet 14 that has been wound into a coil shape and on which secondary recrystallization has occurred, thereby stretching it into a sheet shape. The insulating coating agent applicator 70 also applies an insulating coating agent (coating liquid) that can impart electrical insulation and can impart a predetermined tension to the surface 14A and the back surface 14B of the stretched grain-oriented electrical steel sheet 14, onto the glass coating on the front surface 14A and the back surface 14B.

[0082] (flattening annealing equipment) The flattening annealing apparatus 80 anneals the grain-oriented electromagnetic steel sheet 14 coated with the insulating coating agent at a predetermined temperature (e.g., 800°C to 850°C) and a predetermined time (e.g., 10 seconds or more and 120 seconds or less) while transporting the grain-oriented electromagnetic steel sheet 14 by a transport device, thereby baking the insulating coating agent on the front surface 14A and the back surface 14B of the grain-oriented electromagnetic steel sheet 14. In addition, tension (sheet passing tension) is applied to the grain-oriented electromagnetic steel sheet 14 from the transport device in the transport direction X of the grain-oriented electromagnetic steel sheet 14. As a result, the curl and distortion applied to the grain-oriented electromagnetic steel sheet 14 during the final annealing are removed, and the grain-oriented electromagnetic steel sheet 14 is flattened. In addition, the insulating coating on the front surface 14A and the back surface 14B of the grain-oriented electromagnetic steel sheet 14 imparts electrical insulation to the grain-oriented electromagnetic steel sheet 14.

[0083] (Method of manufacturing grain-oriented electrical steel sheet) Next, an example of a method for manufacturing the grain-oriented electrical steel sheet according to this embodiment will be described.

[0084] As shown in FIG. 3, the method for producing a grain-oriented electrical steel sheet according to this embodiment includes, as an example, a casting process, a hot rolling process, an annealing process, a cold rolling process, an oil film removal process, a beam irradiation process, a polishing process, a decarburization annealing process, an annealing separator application process, a final finish annealing process, an insulating coating agent application process, and a planarization annealing process.

[0085] (Casting process - Annealing process) First, in the casting process (step P10, continuous casting process), a slab is formed by a continuous casting machine (not shown). Next, in the hot rolling process (step P12), the slab is hot rolled by a roughing mill (not shown) or the like to form a steel plate of a predetermined thickness (hereinafter referred to as "hot rolled steel plate"). Next, in the annealing process (step P14), the hot rolled steel plate is annealed at a predetermined temperature.

[0086] (Cold rolling process) Next, as shown in FIG. 1, in the cold rolling process (step P16), for example, the hot-rolled steel sheet, which has rolling oil (cold-rolling oil) applied to its front and back sides, is rolled by a finishing mill 15 and stretched in the conveying direction X to form a cold-rolled steel sheet 12 of a predetermined thickness.

[0087] (Oil film removal process) Next, in the oil film removal step (step P18), the oil film adhering to the front surface 12A and the back surface 12B on both sides of the cold-rolled steel sheet 12 is removed using an oil film removal device 20.

[0088] (Beam irradiation process) Next, in the beam irradiation process (step P20), a laser beam L is irradiated onto the surface 12A of the cold-rolled steel sheet 12, which is transported by a transport device and from which the oil film has been removed, using a beam irradiation device 30 to form multiple grooves (laser grooves).

[0089] Specifically, a laser beam L is irradiated from a beam irradiation device 30 onto a surface 12A of a cold-rolled steel plate 12 transported by a transport device, and a groove is formed on the surface 12A along a direction parallel to the width direction of the cold-rolled steel plate 12 or a direction inclined at a predetermined angle (preferably an angle greater than 0° and less than 20°) from the width direction of the cold-rolled steel plate 12.

[0090] Furthermore, the beam irradiation device 30 forms a plurality of grooves on the surface 12A of the cold-rolled steel sheet 12 at a predetermined interval (pitch) in the conveying direction X of the cold-rolled steel sheet 12. These grooves subdivide the magnetic domains of the grain-oriented electromagnetic steel sheet 14, improving the iron loss of the grain-oriented electromagnetic steel sheet 14.

[0091] (polishing process) Next, in the polishing process (step P22), any adhesions such as molten protrusions and splashes adhering to the surface 12A of the cold-rolled steel sheet 12 on which grooves have been formed by the laser beam L are removed using a polishing device 40 before the cold-rolled steel sheet 12 is decarburized annealed in a decarburization annealing device 50.

[0092] Specifically, in the polishing device 40, a polishing liquid containing abrasive grains is supplied from a polishing liquid supply nozzle (not shown) to the surface 12A of the cold rolled steel sheet 12, while a polishing brush roll 44 is rotated by a motor (not shown). Alternatively, in the polishing device 40, a polishing brush roll 44 having bristles such as nylon containing abrasive grains is rotated by a motor (not shown) while a polishing liquid consisting of water is supplied from a polishing liquid supply nozzle to the surface 12A of the cold rolled steel sheet 12. As a result, deposits attached to the surface 12A of the cold rolled steel sheet 12 are polished and removed by the polishing brush 44B attached to the rotating polishing brush roll 44.

[0093] (Decarburization annealing process) Next, in the decarburization annealing step (step P24), the cold-rolled steel sheet 12 with the grooves formed therein is decarburized annealed (continuous annealing) at a predetermined temperature (for example, 700°C to 900°C) using a decarburization annealing apparatus 50. As a result, the cold-rolled steel sheet 12 is decarburized, and primary recrystallization (grain size: 10 to 30 μm) is generated in the cold-rolled steel sheet 12. In addition, by decarburizing the cold-rolled steel sheet 12, an oxide layer mainly composed of silica (SiO2) is formed on the front surface 12A and the back surface 12B of the cold-rolled steel sheet 12.

[0094] (Annealing separator application process) Next, in an annealing separator application process (step P26), an annealing separator mainly composed of magnesia (MgO) is applied onto the oxide layers formed on the front surface 12A and back surface 12B of the cold rolled steel sheet 12 during decarburization annealing, using an annealing separator application device 55. Thereafter, the cold rolled steel sheet 12 is wound into a coil by a winding device (not shown).

[0095] (Final annealing process) 2, in the final annealing process (step P28), the coiled cold-rolled steel sheet 12 is annealed (batch annealed) at a predetermined temperature (e.g., about 1200°C) and for a predetermined time (e.g., about 20 hours) using a final annealing apparatus 60. The heat treatment conditions are, for example, a heating temperature of 1100 to 1300°C and a heating time of 20 to 24 hours.

[0096] As a result, secondary recrystallization occurs in the cold-rolled steel sheet 12, a crystal orientation occurs in which the axis of easy magnetization is substantially aligned with the conveying direction X of the cold-rolled steel sheet 12, and a glass coating is formed on the front surface 12A and the back surface 12B of the cold-rolled steel sheet 12. As a result, a grain-oriented electrical steel sheet 14 is formed. Thereafter, the coil-shaped grain-oriented electrical steel sheet 14 is unwound.

[0097] Here, the grain-oriented electrical steel sheet 14 contains an inhibitor such as MnS or AlN. As a result, in the final annealing process, crystal grains in the Goss orientation, in which the magnetization easy axis is substantially aligned in the transport direction X of the grain-oriented electrical steel sheet 14, preferentially grow. As a result, a grain-oriented electrical steel sheet 14 with high crystal orientation (crystal orientation) is formed.

[0098] (Insulating coating agent application process) Next, in the insulating coating agent application process (step P30), an insulating coating agent (coating liquid) that has electrical insulation properties and can impart a predetermined tension to the front surface 14A and back surface 14B of the grain-oriented electrical steel sheet 14 is applied to the front surface 14A and back surface 14B of the grain-oriented electrical steel sheet 14 using an insulating coating agent application device 70. Note that application of the insulating coating agent by the insulating coating agent application device 70 is usually performed after residual unreacted magnesia on the front surface 14A and back surface 14B of the grain-oriented electrical steel sheet 14 has been washed away and dried.

[0099] (flattening annealing process) Next, in the flattening annealing process (step P32), the grain-oriented electrical steel sheet 14 to which the insulating coating agent has been applied is annealed (flattened) at a predetermined temperature (e.g., 800°C to 850°C) for a predetermined time (e.g., 10 seconds or more and 120 seconds or less) using a flattening annealing apparatus 80 while being transported by a transport device.

[0100] At this time, tension (sheet passing tension) is applied to the grain-oriented electromagnetic steel sheet 14 from the conveying device in the conveying direction X of the grain-oriented electromagnetic steel sheet 14. This removes the curling tendency and distortion of the grain-oriented electromagnetic steel sheet 14 during the final annealing, and flattens the grain-oriented electromagnetic steel sheet 14.

[0101] Furthermore, when the grain-oriented electrical steel sheet 14 is annealed in the flattening annealing process, an insulating coating agent is baked onto the front surface 14A and the back surface 14B of the grain-oriented electrical steel sheet 14, and the front surface 14A and the back surface 14B of the grain-oriented electrical steel sheet 14 are insulated by the insulating coating agent. Thereafter, the grain-oriented electrical steel sheet 14 is cooled.

[0102] (Groove Depth Monitoring System) Next, a groove depth monitoring system provided in the manufacturing apparatus for grain-oriented electrical steel sheet according to this embodiment will be described.

[0103] FIG. 4 is a perspective view of the groove depth monitoring system 100 according to this embodiment, seen from the front side in the conveying direction X of the cold-rolled steel sheet 12. The groove depth monitoring system 100 according to this embodiment is a system that monitors whether the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value. As shown in FIG. 4, this groove depth monitoring system 100 includes a control device 130. In the embodiment shown in FIG. 4, the groove depth monitoring system 100 includes the control device 130, a spatter amount detection device 110, and a torque detection device 120. The spatter amount detection device 110 and the torque detection device 120 (see FIG. 1) are connected to the control device 130 so as to be able to communicate with each other by wire or wirelessly.

[0104] (Sputter amount detection device) The sputter amount detection device 110 is a device that detects the amount of sputtering generated when the grooves G are formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30. This sputter amount detection device 110 includes an imaging device 112 and a neutral density filter 114.

[0105] The imaging device (imaging section) 112 is, for example, a camera that captures spatter SP scattered around the groove G when the groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30. As an example, when the groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30, this imaging device 112 captures an image of a predetermined area around the groove G from the outside in the width direction of the cold-rolled steel sheet 12 transported by the transport device 16, and outputs the captured image information to a control device 130 described later.

[0106] The imaging device 112 may capture a moving image of a predetermined area around the groove G, or may capture a still image.

[0107] The neutral density filter 114 is a filter that attenuates light other than the sputter SP that is incident on the imaging device 112 when the sputter SP is photographed by the imaging device 112. The neutral density filter 114 has a light attenuation rate set to, for example, 75%.

[0108] The light attenuation rate of the neutral density filter 114 is preferably 10% or more, and more preferably 50% or more. The light attenuation rate of the neutral density filter 114 is preferably 95% or less, and more preferably 75% or less.

[0109] (torque detector) The torque detection device 120 detects the rotational torque generated in the polishing brush roll 44 when the polishing brush roll 44 removes deposits attached to the surface 12A of the cold-rolled steel sheet 12. That is, as shown in Fig. 1, the torque detection device 120 is a device that detects the rotational torque generated in the polishing brush roll 44 when the polishing device 40 removes deposits such as spatter SP (see Fig. 4) that are attached to the surface 12A of the cold-rolled steel sheet 12 when the groove G is formed by the beam irradiation device 30.

[0110] The torque detector 120 is, for example, an ammeter that measures a current value supplied to a motor (not shown) that rotates and drives the abrasive brush roll 44. The torque detector 120 outputs the measured current value to the control device 130, which will be described later.

[0111] (Overview of the control device) The control device 130 controls the overall operation of the groove depth monitoring system 100. The control device 130 also judges whether or not the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value. If the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is less than the reference value, for example, a warning or the like is displayed on a display unit of an input / output device 148 (see FIG. 5) described later.

[0112] (Control device hardware configuration) First, the hardware configuration of the control device 130 will be described.

[0113] The control device 130 is realized, for example, by a computer 140 shown in Fig. 5. The computer 140 includes a CPU (Central Processing Unit) 142, a memory 144 as a temporary storage area, and a non-volatile storage unit 146. The computer 140 also includes an input / output device 148. The CPU 142, the memory 144, the storage unit 146, and the input / output device 148 are connected to one another via a bus 149. The CPU 142 is an example of a control unit.

[0114] The storage unit 146 is realized by, for example, a hard disk drive (HDD), a solid state drive (SSD), a flash memory, etc. The storage unit 146 as a recording medium stores in advance a groove depth monitoring program for causing the computer 140 to function as the control device 130. The storage unit 146 also has a storage area for storing various data.

[0115] The input / output device 148 includes a pointing device such as a mouse, a keyboard, and a display unit, and is used for performing various inputs.

[0116] The CPU 142 reads out the groove depth monitoring program from the storage unit 146, loads it into the memory 144, and executes it. In this way, the computer 140 that has executed the groove depth monitoring program functions as the control device 130.

[0117] (Control device functions) Next, the function of the control device 130 will be described.

[0118] 6, when executing the above-mentioned groove depth monitoring program, the control device 130 realizes various functions using the above-mentioned hardware resources. Specifically, the control device 130 functionally has a sputter amount acquisition unit 132, a torque acquisition unit 133, a groove depth determination unit 134, and an alarm unit 136. The sputter amount acquisition unit 132, the groove depth determination unit 134, and the alarm unit 136 are realized by the CPU 142 reading out and executing the groove depth monitoring program stored in the memory unit 146.

[0119] (Sputter amount acquisition unit) The sputter amount acquisition unit 132 acquires the amount of sputter detected by the sputter amount detection device 110. Specifically, the sputter amount acquisition unit 132 processes image information captured by the imaging device 112 of the sputter amount detection device 110, and calculates and acquires the amount of sputter scattered around the groove G when the groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30.

[0120] The amount of sputtering refers to the amount of sputtering SP (see FIG. 4) that scatters around the groove G when the groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30.

[0121] As an example, the sputter amount acquiring unit 132 classifies each pixel of the image information input from the imaging device 112 into a plurality of ranks (for example, 256 levels (0 to 255)) according to brightness (luminance value). Then, the sputter amount acquiring unit 132 calculates (counts) the number of pixels of the image information input from the imaging device 112 that are ranked equal to or higher than a reference rank as the sputter amount (number of sputter pixels).

[0122] The reference rank is set to, for example, 150. The reference rank of this pixel is set appropriately based on the light attenuation rate of the neutral density filter 114 and the illuminance of the environment in which the sputter SP is photographed. The amount of sputter (number of sputter pixels) can be regarded as the area of ​​a region in a predetermined region (photographed region) around the groove G photographed by the imaging device 112, in which the pixel brightness rank is equal to or higher than the reference rank.

[0123] (Torque acquisition part) The torque acquisition unit 133 acquires the rotational torque of the abrasive brush roll 44 detected by the torque detection device 120. Specifically, the torque acquisition unit 133 acquires from the torque detection device 120 the motor current value detected by the torque detection device 120, and calculates the rotational torque of the abrasive brush roll 44 based on the acquired current value.

[0124] For example, the torque obtaining unit 133 calculates the rotational torque based on the following formula. Rotational torque (N m) = Kt × Ia however, Kt: Torque constant (N m / A) Ia: Motor current value (A) It is.

[0125] The torque constant Kt is set according to the specifications of the abrasive brush 44B (material, length, etc.), the specifications of the abrasive liquid (type, supply amount, etc.), and the specifications of the motor that rotates the abrasive brush roll 44 (output, etc.).

[0126] Furthermore, the torque detector 120 is not limited to detecting the current value supplied to the motor that rotates the abrasive brush roll 44, and may detect the rotational torque of the abrasive brush roll 44 by a known method.

[0127] In this embodiment, the torque acquisition unit 133 calculates the rotation torque of the abrasive brush roll 44 based on the current value detected by the torque detection device 120. However, the torque detection device 120 may be provided with a function for calculating the rotation torque of the abrasive brush roll 44. In this case, the torque acquisition unit 133 acquires the rotation torque of the abrasive brush roll 44 from the torque detection device 120.

[0128] (Groove depth determination section) The groove depth determination unit 134 determines whether the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value based on the sputtering amount acquired by the sputtering amount acquisition unit 132, a predetermined reference sputtering amount, the rotational torque of the abrasive brush roll 44 acquired by the torque acquisition unit 133, and a predetermined reference rotational torque.

[0129] Specifically, the groove depth determination unit 134 determines that the depth of the groove G is equal to or greater than the reference value when the following formula (1) obtained from the results of a manufacturing test described later is satisfied. On the other hand, the groove depth determination unit 134 determines that the depth of the groove G is less than the reference value when the following formula (1) is not satisfied.

[0130] 1 ≥ S / S0 ≥ C1, and C2 ≤ T / T0 ≤ C3 (1) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1:S1 / S0 S1: The minimum amount of spatter that occurs when forming a groove with a standard depth on the surface of a cold-rolled steel sheet (steel sheet) T: Rotational torque acquired by the torque acquisition unit T0: Reference rotation torque C2:T1 / T0 T1: The minimum rotational torque generated when removing deposits from the surface of a cold-rolled steel plate (steel plate) with grooves of a reference depth using an abrasive brush roll. C3:T2 / T0 T2: The maximum rotational torque generated when removing deposits from the surface of a cold-rolled steel plate (steel plate) with grooves of a standard depth using an abrasive brush roll. It is.

[0131] The formula (1) will be described later in the manufacturing test.

[0132] (Notification Department) When the groove depth determination unit 134 determines that the depth of the groove G is less than the reference value, the notification unit 136 displays a message such as a warning on the display unit of the input / output device 148. Note that the notification unit 136 is not limited to a message such as a warning, and may be configured to issue, for example, an alarm.

[0133] (Method of monitoring groove depth in grain-oriented electrical steel sheets) Next, an example of a groove depth monitoring method for a grain-oriented electrical steel sheet will be described while explaining the operation of the control device 130.

[0134] During the running of the cold rolled steel sheet 12 described above (during the manufacture of the grain-oriented electromagnetic steel sheet 14), for example, a groove depth monitoring process is periodically executed in the control device 130. The groove depth monitoring process has a spatter amount acquisition process, a torque acquisition process, and a groove depth determination process. The groove depth monitoring process is one example of a groove depth monitoring method for an electromagnetic steel sheet. The spatter amount acquisition process and the torque acquisition process may be performed during the running of the cold rolled steel sheet 12, and the groove depth determination process may be performed during the running of the cold rolled steel sheet 12. The groove depth determination process may be performed after the manufacture of the grain-oriented electromagnetic steel sheet 14.

[0135] (Sputter amount acquisition process) As shown in FIG. 7, first, in step S10, the CPU 142 performs a sputter amount acquisition process in parallel with the above-mentioned beam irradiation process, and acquires the sputter amount S generated when forming a groove G on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30.

[0136] Specifically, the CPU 142 may control the imaging device 112 of the spatter amount detection device 110 when the groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30. As a result, when the groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30, the spatter SP scattered around the groove G is photographed by the imaging device 112, and the photographed image information is output to the control device 130. The CPU 142 determines the location with a high brightness value based on the image information output from the imaging device 112, thereby calculating (detecting) the spatter amount S.

[0137] (Torque acquisition process) Next, in step S12, the CPU 142 performs a torque acquisition process in parallel with the polishing process described above, and acquires the rotational torque T generated in the abrasive brush roll 44 when the abrasive brush roll 44 polishes the deposits adhering to the surface 12A of the cold-rolled steel sheet 12.

[0138] Specifically, the CPU 142 may control the torque detection device 120 when the abrasive brush roll 44 is used to polish the deposits on the surface 12A of the cold rolled steel sheet 12. The torque detection device 120 detects a current value supplied to a motor (not shown) that rotates the abrasive brush roll 44 when the abrasive brush roll 44 of the polishing device 40 is used to polish the deposits on the surface 12A of the cold rolled steel sheet 12, and outputs the detected current value to the control device 130. The CPU 142 calculates the rotational torque T generated in the abrasive brush roll 44 based on the current value output from the torque detection device 120, thereby acquiring the rotational torque T.

[0139] The spatter amount obtaining step and the torque obtaining step are carried out continuously or periodically while the cold rolled steel sheet 12 is being threaded (while the grain-oriented electrical steel sheet 14 is being manufactured).

[0140] (Groove depth determination process) Next, in step S14, the CPU 142 performs a groove depth determination process, and determines whether the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value based on the sputtering amount S acquired in the sputtering amount acquisition process, the reference sputtering amount S0, the rotational torque T of the abrasive brush roll 44 acquired in the torque acquisition process, and the reference rotational torque.

[0141] Specifically, when the above formula (1) is satisfied, the CPU 142 determines that the depth of the groove G is equal to or greater than the reference value, and ends the process. On the other hand, when the above formula (1) is not satisfied, the CPU 142 determines that the depth of the groove G is less than the reference value, and proceeds to step S16.

[0142] In step S16, the CPU 142 displays a warning or the like on the display unit of the input / output device 148, and ends the process.

[0143] (Action and Effects) Next, the operation and effects of this embodiment will be described.

[0144] The groove depth monitoring system 100 according to this embodiment acquires the amount of spatter S generated when a laser beam L is irradiated from a beam irradiation device 30 onto a surface 12A of a cold-rolled steel sheet 12 to form grooves G. The groove depth monitoring system 100 also acquires the rotational torque generated in the abrasive brush roll 44 when the abrasive brush roll 44 removes deposits attached to the surface 12A of the cold-rolled steel sheet 12 in which grooves G have been formed by the laser beam L of the beam irradiation device 30.

[0145] Then, the groove depth monitoring system 100 judges whether or not the depth of the groove G formed on the surface 12A of the cold rolled steel sheet 12 is equal to or greater than a reference value based on the acquired sputter amount S, a predetermined reference sputter amount S0, the acquired rotational torque T of the abrasive brush roll 44, and a predetermined reference rotational torque T0. More specifically, the monitoring system 100 judges whether or not the depth of the groove G formed on the surface 12A of the cold rolled steel sheet 12 is equal to or greater than a reference value based on the above formula (1).

[0146] This makes it possible to detect a cold-rolled steel sheet 12 in which the depth of the groove G is less than the reference value due to, for example, a decrease in the output of the laser beam L of the beam irradiation device 30 and a shift in focus of the laser beam L on the surface 12A of the cold-rolled steel sheet 12. Therefore, it is possible to prevent the depth of the groove G formed on the surface 14A of the grain-oriented electromagnetic steel sheet 14 from becoming shallow.

[0147] Furthermore, the groove depth monitoring system 100 monitors in real time the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12. This makes it possible to detect at an early stage the cold-rolled steel sheet 12 in which the depth of the groove G is less than the reference value. This makes it possible to reduce the production volume of grain-oriented electrical steel sheets 14 in which the depth of the groove G is less than the reference value.

[0148] Here, the amount of spatter S generated when the grooves G are formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30 basically decreases as the depth of the grooves G formed on the surface 12A becomes shallower. Therefore, by monitoring the amount of spatter S detected by the spatter amount detection device 110, the depth of the grooves G formed on the surface 12A of the cold-rolled steel sheet 12 can be estimated.

[0149] However, in a range where the amount of defocus of the laser beam L relative to the surface 12A of the cold-rolled steel sheet 12 is small, the amount of spatter S decreases once and then increases again as the amount of defocus of the laser beam L increases. Therefore, by simply monitoring the amount of spatter S detected by the spatter amount detection device 110, it may not be possible to detect the defocus of the laser beam L in a range where the amount of defocus of the laser beam L relative to the surface 12A of the cold-rolled steel sheet 12 is small.

[0150] Here, in the range where the amount of deviation of the focus of the laser beam L with respect to the surface 12A of the cold rolled steel sheet 12 is small, the viscosity of the spatter generated increases due to temperature changes on the surface 12A of the cold rolled steel sheet 12, and the particle size of the spatter and other deposits adhering to the surface 12A of the cold rolled steel sheet 12 increases. As a result, the abrasive brush roll 44 can easily grind the surface 12A of the cold rolled steel sheet 12 with a high degree of accuracy. When the deposits adhering to 12A are polished, the rotational torque T generated in the polishing brush roll 44 also increases.

[0151] Therefore, in the groove depth monitoring system 100, in addition to the sputter amount S detected by the sputter amount detection device 110, the rotational torque T of the abrasive brush roll 44 detected by the torque detection device 120 is also monitored.

[0152] Specifically, the CPU 142 of the groove depth monitoring system 100 determines that the depth of the groove G formed on the surface 12A of the cold rolled steel sheet 12 is equal to or greater than a reference value when the above formula (1) is satisfied. This makes it possible to detect the deviation of the focus of the laser beam L even in a range where the deviation of the focus of the laser beam L with respect to the surface 12A of the cold rolled steel sheet 12 is small. This improves the determination accuracy of the groove depth monitoring system 100. In addition, it is possible to further prevent the depth of the groove G formed on the surface 12A of the cold rolled steel sheet 12 from becoming shallow.

[0153] (Production testing) Next, the manufacturing test will be described.

[0154] In the present manufacturing tests, first, in Test 1, grain-oriented electrical steel sheets were manufactured by the above-mentioned manufacturing method using the amount of focus deviation of the laser beam with respect to the surface of the grain-oriented electrical steel sheet as a parameter. Then, the groove depth and iron loss improvement rate of the manufactured grain-oriented electrical steel sheet were evaluated.

[0155] Next, in Test 2, grain-oriented electrical steel sheets were manufactured by the above-mentioned manufacturing method using the laser power (output) of the laser beam irradiated from the beam irradiation device onto the surface of the grain-oriented electrical steel sheet as a parameter. Then, the groove depth and iron loss improvement rate of the manufactured grain-oriented electrical steel sheet were evaluated.

[0156] (Groove machining conditions) The processing conditions for forming grooves on the surface of the grain-oriented electrical steel sheet by the beam irradiation device are as follows. Laser beam scanning speed: 45 [m / s] Groove pitch (spacing): 3 mm Laser beam shape: 25×50[μm] Laser power (Test 1): 2000 [W], Laser power (Test 2): See Figure 8

[0157] (Abrasive brush roll) Materials of the polishing brush: nylon brush with abrasive grains, wire diameter (diameter) 1.4 mm, abrasive grain size 80, 3-bundle type Abrasive brush roll rotation speed: 1200[rpm] Rotation direction of the abrasive brush roll: Opposite to the conveying direction of the grain-oriented electromagnetic steel sheet Abrasive brush roll compression: 3mm Polishing fluid: Water (does not contain abrasive grains) Polishing solution temperature: 50℃ Number of passes: 1: Backup roll method Conveying speed of grain-oriented electrical steel sheet: 60 [m / m] Torque constant Kt: 9.5 (N m / A)

[0158] (Test Results) Figure 8 shows the test results of Tests 1 and 2. Figure 9 shows the relationship between the depth of the grooves formed on the surface of the grain-oriented electrical steel sheet and the iron loss improvement rate η in Tests 1 and 2.

[0159] As shown in FIG. 8, in each of Tests 1 and 2, grain-oriented electrical steel sheets that were equal to or greater than the following standard values ​​were deemed to have passed (Examples), and grain-oriented electrical steel sheets that were below the standard values ​​were deemed to have been comparative examples. <Reference value> Groove depth: 20[μm] Iron loss improvement rate η:18[%]

[0160] The reference value of the groove depth can be changed as appropriate and is set, for example, in the range of 20 μm to 25 μm. Similarly, the reference value of the iron loss improvement rate η can also be changed as appropriate.

[0161] The depth of the grooves formed on the surface of the grain-oriented electrical steel sheet was measured with a measuring device (Keyence (registered trademark) WI-5000, WI-001). The depth of the groove can be obtained, for example, by measuring the length corresponding to the difference (H0-H) between the average height of the surface of the grain-oriented electrical steel sheet measured in an arbitrary area without grooves, H0 (>0), and the maximum depth of the groove (the height of the bottom of the groove), H (>0), using the measuring device.

[0162] The iron loss improvement rate η of the grain-oriented electrical steel sheet was calculated from the following formula using the iron loss of the base steel sheet as a reference. Iron loss improvement rate η [%] = ((iron loss of base steel sheet - iron loss of grain-oriented electrical steel sheet) / iron loss of base steel sheet) x 100

[0163] Here, the manufacturing method of the base steel sheet differs from the manufacturing method according to the above embodiment in that the beam irradiation step and the polishing step are not performed, i.e., no grooves are formed in the base steel sheet.

[0164] The iron loss [W / kg] of each of the base steel sheets, Examples 1 to 6, and Comparative Examples 1 to 10 was measured by a single sheet tester (SST) when a magnetic field with a maximum magnetic flux density of 1.7 Tesla and 50 Hz was applied to the following 10 test pieces. The iron loss of the base steel sheets was 0.86 [W / kg]. <Test piece> Test piece dimensions: 60 x 300 [mm] Test piece thickness: 0.23 mm

[0165] In this manufacturing test, in the case of the groove processing conditions in Example 1, that is, when the laser beam focus deviation amount is 0 [mm] and the laser beam power is the reference value (2000 [W]), the sputter amount acquired by the sputter amount acquisition unit 132 was set to the reference sputter amount S0 (= 120000 [pixels]). Similarly, in the case of the groove processing conditions in Example 1, the rotational torque of the polishing brush roll 44 acquired by the torque acquisition unit 133 was set to the reference rotational torque T0 (= 900 [Nm]).

[0166] Then, for each of Examples 1 to 6 and Comparative Examples 1 to 10, the ratio (S / S0) of the sputter amount S to the reference sputter amount S0 and the ratio (T / T0) of the rotational torque T to the reference rotational torque T0 were determined.

[0167] The relationship between the amount of deviation from the focus of the laser beam and the depth of the groove is shown in Fig. 10. As shown in Fig. 10, as the amount of deviation from the focus of the laser beam increases, the depth of the groove becomes shallower.

[0168] Next, Fig. 11 shows the relationship between the amount of defocus of the laser beam and the amount of sputtering S. As shown in Fig. 11, when the amount of defocus of the laser beam is 0.6 [mm] or more, the amount of sputtering S decreases as the amount of defocus of the laser beam increases.

[0169] In contrast, when the laser beam defocus amount is 0.6 [mm] or less, the following occurs: In other words, when the laser beam defocus amount is in the range of 0 to 0.3 [mm], the sputter amount S decreases as the laser beam defocus amount increases. On the other hand, when the laser beam defocus amount is in the range of 0.3 to 0.6 [mm], the sputter amount S increases as the laser beam defocus amount increases.

[0170] From this, it can be seen that simply monitoring the sputter amount S detected by the sputter amount detection device 110 makes it difficult to detect the focus shift of the laser beam relative to the surface 12A of the cold-rolled steel sheet 12 in a range where the focus shift of the laser beam relative to the surface 12A of the cold-rolled steel sheet 12 is small (0.6 mm or less).

[0171] Next, Fig. 12 shows the relationship between the laser beam defocus amount and the rotational torque T. As shown in Fig. 12 and the above-mentioned Fig. 11, when the laser beam defocus amount is in the range of 0.3 to 0.6 [mm], the rotational torque T and the sputter amount S show the same tendency. In other words, when the laser beam defocus amount is in the range of 0.3 to 0.6 [mm], the rotational torque T and the sputter amount S increase as the laser beam defocus amount increases.

[0172] Here, when the laser beam defocus amount is in the range of 0.3 to 0.6 [mm], the viscosity of the generated spatter increases due to temperature changes and the like on the surface 12A of the cold-rolled steel sheet 12, and the particle size of the deposits such as spatters adhering to the surface 12A of the cold-rolled steel sheet 12 increases. Therefore, it is considered that when the laser beam defocus amount is in the range of 0.3 to 0.6 [mm], the rotational torque T generated when polishing the deposits adhering to the surface 12A of the cold-rolled steel sheet 12 becomes large.

[0173] This shows that it is possible to detect the laser beam focus deviation in the range of 0.3 to 0.6 mm by monitoring the rotational torque T. In other words, by monitoring the rotational torque T in addition to the sputter amount S, the estimation accuracy of the groove depth can be improved.

[0174] Specifically, FIG. 13 shows the relationship between the amount of sputtering S and the depth of the groove. As shown in FIG. 13, the condition for the amount of sputtering S to make the groove depth equal to or greater than the reference value of 20 μm is 100,000 pixels or more. FIG. 14 shows the relationship between the rotational torque T and the depth of the groove. As shown in FIG. 14, the condition for the rotational torque T to make the groove depth equal to or greater than the reference value of 20 μm is 800 Nm or more and 1,000 Nm or less. In other words, the condition for the amount of sputtering S and the rotational torque T to make the groove depth equal to or greater than the reference value of 20 μm is given by the following formula (a).

[0175] S≧100000[pixels] and 800[Nm]≦T≦1000[Nm] (a) however, S: sputter amount acquired by the sputter amount acquisition unit T: Rotational torque acquired by the torque acquisition unit It is.

[0176] Here, if the condition of the sputter amount S in the above formula (a) is generalized, it becomes equal to or more than the minimum sputter amount (100000 [pixels]) generated when the groove G having a reference depth is formed on the surface 12A of the cold rolled steel sheet 12 by the beam irradiation device 30. In addition, if the condition of the rotational torque T in the above formula (a) is generalized, it becomes equal to or less than the maximum rotational torque (1000 [Nm]) generated on the polishing brush roll 44 when the polishing brush roll 44 removes the deposits attached to the surface 12A of the cold rolled steel sheet 12 in which the groove G having a reference depth is formed by the beam irradiation device 30. Therefore, in the above formula (a), the above minimum sputter amount becomes the reference sputter amount, and the above maximum rotational torque becomes the reference rotational torque.

[0177] In this case, in the above formula (a), when the sputtering amount S acquired by the sputtering amount acquisition unit 132 is equal to or greater than the reference sputtering amount and the rotational torque T acquired by the torque acquisition unit 133 is equal to or less than the reference rotational torque, it is possible to determine whether the depth of the groove formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than the reference value.

[0178] 8, when the sputter amount S acquired by the sputter amount acquisition unit 132 is equal to or greater than the reference sputter amount (100,000 [pixels]), the rotational torque T acquired by the torque acquisition unit 133 is equal to or greater than 800 [Nm]. Therefore, the lower limit (800 [Nm]) of the rotational torque T in the above formula (a) can be omitted.

[0179] 15 shows the relationship between the ratio (S / S0) of the sputter amount S to the reference sputter amount S0 and the rotational torque T. As described above, the reference sputter amount S0 here is the sputter amount (=120000 [pixels]) acquired by the sputter amount acquisition unit 132 in the case of the groove processing conditions in Example 1, that is, when the defocus amount of the laser beam is 0 [mm] and the laser power of the laser beam is the reference value (2000 [W]).

[0180] As shown in FIG. 15, the condition for the groove depth to be equal to or greater than the reference value (20 μm) is given by the following formula (2). 1 ≥ S / S0 ≥ C1, and T1 ≤ T ≤ T2 (2) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1:S1 / S0 S1: The minimum amount of spatter that occurs when forming a groove with a standard depth on the surface of a cold-rolled steel sheet (steel sheet) T: Rotational torque acquired by the torque acquisition unit T1: Reference rotational torque, which is the minimum rotational torque generated when removing deposits from the surface of a cold-rolled steel plate (steel plate) with grooves of a reference depth using an abrasive brush roll. T2: Reference rotational torque. This is the maximum rotational torque that occurs when removing deposits from the surface of a cold-rolled steel plate (steel plate) with grooves of a reference depth using an abrasive brush roll. It is.

[0181] In this manufacturing test, C1 is 0.83, T1 is 800 [Nm], and T2 is 1000 [Nm], but C1, T1, and T2 can be changed as appropriate.

[0182] 16 also shows the relationship between the ratio (S / S0) of the sputter amount S to the reference sputter amount S0 and the ratio (T / T0) of the rotational torque T to the reference rotational torque T0. As described above, the reference rotational torque T0 is the rotational torque (=900 [Nm]) of the abrasive brush roll 44 acquired by the torque acquisition unit 133 under the groove machining conditions in Example 1.

[0183] As shown in FIG. 16, the condition for the groove depth to be equal to or greater than the reference value (20 [μm]) is as shown in the above-mentioned formula (1).

[0184] 1 ≥ S / S0 ≥ C1, and C2 ≤ T / T0 ≤ C3 (1) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1:S1 / S0 S1: The minimum amount of spatter that occurs when forming a groove with a standard depth on the surface of a cold-rolled steel sheet (steel sheet) T: Rotational torque acquired by the torque acquisition unit T0: Reference rotation torque C2:T1 / T0 T1: The minimum rotational torque generated when removing deposits from the surface of a cold-rolled steel plate (steel plate) with grooves of a reference depth using an abrasive brush roll. C3:T2 / T0 T2: The maximum rotational torque generated when removing deposits from the surface of a cold-rolled steel plate (steel plate) with grooves of a standard depth using an abrasive brush roll. It is.

[0185] In this manufacturing test, C1 is 0.83, C2 is 0.89, and C3 is 1.11, but C1, C2, and C3 can be changed as appropriate.

[0186] By using equation (a), equation (1), or equation (2) in this manner, it is possible to determine whether the depth of the groove formed on surface 12A of cold-rolled steel sheet 12 is equal to or greater than a reference value (20 μm).

[0187] (Modification) Next, a modification of the above embodiment will be described.

[0188] In the above formula (a), the reference sputter amount may be, for example, the sputter amount obtained by multiplying the above minimum sputter amount by a predetermined safety factor. Also, in the above formula (a), the reference sputter amount may be, for example, the average value of the multiple measured sputter amounts measured multiple times when forming grooves G having a depth equal to or greater than a reference value on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30.

[0189] In this way, the reference sputter amount in formula (a) can be determined based on the amount of sputtering that occurs when grooves G having a depth equal to or greater than the reference value are formed on the surface 12A of the cold-rolled steel sheet 12 by the beam irradiation device 30.

[0190] In the above formula (a), the reference rotational torque may be, for example, a rotational torque obtained by multiplying the maximum rotational torque by a predetermined safety factor. In the above formula (a), the reference rotational torque may be, for example, an average value of a plurality of rotational torques measured by measuring the rotational torque generated in the abrasive brush roll 44 multiple times when the abrasive brush roll 44 is used to remove deposits that are attached to the surface 12A of the cold-rolled steel sheet 12 in which grooves G having a depth equal to or greater than a reference value are formed by the beam irradiation device 30.

[0191] In this way, the reference rotational torque in equation (a) can be determined based on the rotational torque generated in the abrasive brush roll 44 when the abrasive brush roll 44 removes deposits attached to the surface 12A of a cold-rolled steel sheet 12 in which grooves G of a depth equal to or greater than a reference value have been formed by the beam irradiation device 30.

[0192] Next, in the above formulas (1) and (2), the reference sputter amount S0 may be, for example, a sputter amount obtained by multiplying a sputter amount generated when a groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the laser beam L when the defocus amount of the laser beam L irradiated on the surface 12A of the cold-rolled steel sheet 12 is 0 and the laser power of the laser beam L is a reference value by a predetermined safety factor. Also, the reference sputter amount S0 may be, for example, an average value of a plurality of measured sputter amounts generated when a groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the laser beam L when the defocus amount of the laser beam L irradiated on the surface 12A of the cold-rolled steel sheet 12 is 0 and the laser power of the laser beam L is a reference value, by measuring the sputter amount generated multiple times.

[0193] In this way, the reference sputter amount S0 in the above equations (1) and (2) can be determined based on the amount of sputtering generated when a groove G is formed on the surface 12A of the cold-rolled steel sheet 12 by the laser beam L when the focus shift amount of the laser beam L irradiated to the surface 12A of the cold-rolled steel sheet 12 is 0 and the laser power of the laser beam L is a reference value.

[0194] In addition, in the above formulas (1) and (2), the reference rotational torque T0 may be a rotational torque obtained by multiplying a rotational torque generated when the abrasive brush roll 44 removes the deposits attached to the surface 12A of the cold-rolled steel sheet 12 on which the grooves G are formed by the laser beam L when the amount of focus shift of the laser beam L irradiated to the surface 12A of the cold-rolled steel sheet 12 is 0 and the laser power of the laser beam L is a reference value, by a predetermined safety factor. In addition, in the above formulas (1) and (2), the reference rotational torque T0 may be, for example, an average value of a plurality of rotational torques measured by measuring the rotational torque generated when the abrasive brush roll 44 removes the deposits attached to the surface 12A of the cold-rolled steel sheet 12 on which the grooves G are formed by the laser beam L when the amount of focus shift of the laser beam L irradiated to the surface 12A of the cold-rolled steel sheet 12 is 0 and the laser power of the laser beam L is a reference value.

[0195] In this way, the reference rotational torque T0 in the above equations (1) and (2) can be determined based on the rotational torque generated when the abrasive brush roll 44 removes adhesion material attached to the surface 12A of the cold-rolled steel sheet 12 in which grooves G are formed by the laser beam L when the focus deviation of the laser beam L irradiated to the surface 12A of the cold-rolled steel sheet 12 is 0 and the laser power of the laser beam L is at a reference value.

[0196] In addition, in the above embodiment, the control device 130 (groove depth determination unit 134) determines whether the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value based on the sputter amount S detected by the sputter amount detection device 110, a predetermined reference sputter amount S0, the rotational torque T of the abrasive brush roll 44 detected by the torque detection device 120, and a predetermined reference rotational torque.

[0197] However, for example, when there is no misfocus of the laser beam L irradiated from the beam irradiation device 30 to the surface 12A of the cold rolled steel sheet 12, or when the misfocus is so small that it can be ignored, the control device 130 (groove depth determination unit 134) may be configured as follows: That is, the control device 130 (groove depth determination unit 134) may determine whether the depth of the groove G formed on the surface 12A of the cold rolled steel sheet 12 is equal to or greater than a reference value, based on the rotational torque T of the abrasive brush roll 44 detected by the torque detection device 120 and a predetermined reference rotational torque T0.

[0198] More specifically, the control device 130 (groove depth determination unit 134) may determine whether the depth of the groove G formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value when the following formula (3) is satisfied. Note that the reference rotational torque T0 in the following formula (3) is determined based on the rotational torque generated when, for example, the abrasive brush roll 44 removes deposits attached to the surface 12A of the cold-rolled steel sheet 12 in which grooves G having a depth of a reference value are formed by the laser beam L when the amount of focus shift of the laser beam L irradiated to the surface 12A of the cold-rolled steel sheet 12 is 0.

[0199] T1≦T≦T0 (3) however, T: Rotational torque acquired by the torque acquisition unit T0: Reference rotation torque T1: The minimum rotational torque generated when removing the deposits on the surface of a steel plate with grooves of a reference depth by an abrasive brush roll. It is.

[0200] In this case, as can be seen from the results of Test 2 shown in Fig. 8, it is possible to detect cold-rolled steel sheets 12 in which the depth of the grooves G formed on the surface 12A of the cold-rolled steel sheet 12 is less than the reference value by reducing the output of the laser beam from the beam irradiation device 30. Therefore, it is possible to prevent the depth of the grooves G formed on the surface 12A of the cold-rolled steel sheet 12 from becoming shallow.

[0201] In the above manufacturing test, T0 is 900 [Nm] and T1 is 800 [Nm], but T0 and T1 can be changed as appropriate.

[0202] Furthermore, the criteria for determining whether the depth of the groove formed on the surface 12A of the cold-rolled steel sheet 12 is equal to or greater than a reference value are not limited to formulas (a), (1), (2), and (3), and can be changed as appropriate.

[0203] Moreover, the shape, size, rotation speed, rotation direction, and material of the abrasive brush 44B in the above embodiment can be appropriately changed as necessary.

[0204] In the above embodiment, the manufacturing apparatus 10 is provided with the finishing rolling mill 15, the oil film removing device 20, the decarburization annealing device 50, the annealing separator applicator 55, the final finish annealing device 60, the insulating coating agent applicator 70, and the planarization annealing device 80. However, the finishing rolling mill 15, the oil film removing device 20, the decarburization annealing device 50, the annealing separator applicator 55, the final finish annealing device 60, the insulating coating agent applicator 70, and the planarization annealing device 80 may be provided in the manufacturing apparatus 10 as necessary, and may be omitted as appropriate.

[0205] In the above embodiment, the groove depth monitoring process executed by the CPU 142 by reading the software (program) may be executed by various processors other than the CPU 142. Examples of the processor in this case include a PLD (Programmable Logic Device) such as an FPGA (Field-Programmable Gate Array) whose circuit configuration can be changed after manufacture, and a dedicated electric circuit such as an ASIC (Application Specific Integrated Circuit) which is a processor having a circuit configuration designed exclusively for executing a specific process. The groove depth monitoring process may be executed by one of these various processors, or may be executed by a combination of two or more processors of the same or different types (for example, a plurality of FPGAs, a combination of a CPU and an FPGA, etc.). The hardware structure of these various processors is, more specifically, an electric circuit that combines circuit elements such as semiconductor elements.

[0206] In the above embodiment, the groove depth monitoring program is pre-stored in the storage unit 146. However, the groove depth monitoring program can be stored in a CD-ROM (Compact Disk Read Only Memory), a DVD-ROM (Digital Versatile Disk Read Only Memory), and a USB (Universal The program may be provided in a form recorded on a recording medium (non-transitory recording medium, computer-readable recording medium) such as a USB (Serial Bus) memory. The program may also be downloaded to the control device 130 from an external device via a network.

[0207] Although one embodiment has been described above, the present disclosure is not limited to such an embodiment, and one embodiment and various modified examples may be used in appropriate combination, and it is of course possible to implement the present disclosure in various forms without departing from the gist of the present disclosure.

[0208] In addition, the disclosure of Japanese Patent Application No. 2023-036047, filed on March 8, 2023, is incorporated by reference in its entirety into this specification. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.

[0209] In addition, the following supplementary notes are disclosed regarding the above embodiment.

[0210] (Appendix 1) An apparatus for manufacturing grain-oriented electrical steel sheets, comprising: a laser irradiation device that irradiates a laser beam onto a surface of a cold-rolled steel sheet, which is a material for the grain-oriented electrical steel sheet, to form grooves; an abrasive brush roll that rotates to abrade and remove deposits adhering to the surface of the cold-rolled steel sheet on which the grooves are formed; A groove depth monitoring system that determines the depth of a groove formed on the surface of the cold rolled steel sheet; having The groove depth monitoring system comprises: a sputter amount detection unit that detects the amount of sputtering generated when forming a groove on the surface of the cold-rolled steel sheet using the laser irradiation device; a polishing torque detection unit that detects a torque generated in the polishing brush roll when removing deposits attached to the surface of the cold-rolled steel sheet by the polishing brush roll; a groove depth determination unit that determines whether or not the depth of the groove formed on the surface of the cold-rolled steel sheet is equal to or greater than a reference value based on the amount of sputtering detected by the sputter amount detection unit, a predetermined reference amount of sputtering, the torque of the polishing brush roll detected by the polishing torque detection unit, and a predetermined reference polishing torque; An apparatus for manufacturing grain-oriented electrical steel sheets comprising: (Appendix 2) The reference sputter amount is a minimum sputter amount generated when a groove having a depth equal to or greater than the reference value is formed on the surface of the cold-rolled steel sheet using the laser irradiation device, 2. The manufacturing apparatus for grain-oriented electrical steel sheet according to claim 1, wherein the reference polishing torque is a maximum torque generated in the abrasive brush roll when the abrasive brush roll removes adhesions adhered to the surface of the cold-rolled steel sheet in which grooves having a depth of the reference value have been formed using the laser irradiation device. (Appendix 3) The grain-oriented electrical steel sheet manufacturing apparatus according to Appendix 2, wherein the groove depth determination unit determines that the depth of the groove formed on the surface of the cold-rolled steel sheet is equal to or greater than the reference value when the sputter amount detected by the sputter amount detection unit is equal to or greater than the reference sputter amount and the torque of the abrasive brush roll detected by the polishing torque detection unit is equal to or less than the reference polishing torque. (Appendix 4) The manufacturing apparatus for grain-oriented electrical steel sheet according to Appendix 2, wherein the groove depth determination unit determines that the depth of the groove formed on the surface of the cold-rolled steel sheet is equal to or greater than the reference value when the reference polishing torque is 1000 [Nm] and satisfies formula (1). S / S0≧0.83 and 800[Nm]≦T≦1000[Nm] (1) however, S: Amount of sputtering detected by the sputtering amount detector S0: Reference sputter amount T: Torque of the polishing brush roll detected by the polishing torque detector It is. (Appendix 5) 3. The manufacturing apparatus for grain-oriented electrical steel sheet according to claim 2, wherein the groove depth determination unit determines that the depth of the groove formed on the surface of the cold-rolled steel sheet is equal to or greater than the reference value when formula (2) is satisfied. S / S0≧0.83 and 0.89≦T / T0≦1.11 (2) however, S: Amount of sputtering detected by the sputtering amount detector S0: Reference sputter amount T: Torque of the polishing brush roll detected by the polishing torque detector T0: Reference grinding torque It is. (Appendix 6) A method for producing a grain-oriented electrical steel sheet, comprising the steps of: a laser irradiation device that irradiates a laser beam onto a surface of a cold-rolled steel sheet, which is a material for the grain-oriented electrical steel sheet, to form grooves; an abrasive brush roll that rotates to abrade and remove deposits adhering to the surface of the cold-rolled steel sheet on which the grooves are formed; A groove depth monitoring system that determines the depth of a groove formed on the surface of the cold rolled steel sheet; Using a manufacturing apparatus having Using the groove depth monitoring system, a sputter amount detection step of detecting an amount of sputter generated when forming a groove on a surface of the cold-rolled steel sheet using the laser irradiation device in a sputter amount detection unit; a polishing torque acquisition step of detecting a torque generated in the polishing brush roll when removing deposits from the surface of the cold-rolled steel sheet by the polishing brush roll in a polishing torque detection unit; a groove depth determination step in which a groove depth determination unit determines whether or not the depth of the groove formed on the surface of the cold-rolled steel sheet is equal to or greater than a reference value based on the amount of sputtering detected by the sputter amount detection unit, a predetermined reference amount of sputtering, the torque of the polishing brush roll detected by the polishing torque detection unit, and a predetermined reference polishing torque; A method for producing a grain-oriented electrical steel sheet comprising the steps of:

Claims

1. a torque acquisition unit that acquires a rotational torque generated when an abrasive brush roll is used to remove deposits that have adhered to the surface of the steel plate on which grooves have been formed by the beam; a groove depth determination unit that determines whether or not a depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired by the torque acquisition unit and a predetermined reference rotational torque; A groove depth monitoring system comprising:

2. a sputter amount acquisition unit that acquires an amount of sputtering generated when the beam is irradiated onto the surface of the steel plate to form the groove, the groove depth determination unit determines whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value, based on the sputter amount acquired by the sputter amount acquisition unit, a predetermined reference sputter amount, the rotational torque acquired by the torque acquisition unit, and the reference rotational torque.

2. The groove depth monitoring system of claim 1.

3. the groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when the sputter amount acquired by the sputter amount acquisition unit is equal to or greater than the reference sputter amount and the rotational torque acquired by the torque acquisition unit is equal to or less than the reference rotational torque.

3. The groove depth monitoring system of claim 2.

4. the reference sputter amount is determined based on the amount of sputtering generated when forming the groove having the reference depth on the surface of the steel plate, The reference rotational torque is determined based on a rotational torque generated when removing the deposit attached to the surface of the steel plate in which the groove having the reference depth is formed by the abrasive brush roll. A groove depth monitoring system according to claim 2 or 3.

5. the reference sputter amount is determined based on the amount of sputtering generated when the groove is formed on the surface of the steel sheet by the beam when the amount of focus shift of the beam irradiated on the surface of the steel sheet is zero and the power of the beam is a reference value; the reference rotational torque is determined based on a rotational torque generated when the abrasive brush roll removes the deposit attached to the surface of the steel plate in which the grooves are formed by the beam, when the amount of focus shift of the beam irradiated onto the surface of the steel plate is zero and the power of the beam is a reference value; The groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when formula (1) is satisfied.

5. The groove depth monitoring system of claim 4. 1 ≧ S / S0 ≧ C1, and C2 ≦ T / T0 ≦ C3 (1) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1: S1 / S0 S1: The minimum amount of spatter generated when forming a groove having a reference depth on the surface of a steel sheet T: Rotational torque acquired by the torque acquisition unit T0: Reference rotation torque C2: T1 / T0 T1: The minimum rotational torque generated when removing deposits attached to the surface of a steel plate on which grooves of a reference depth are formed using an abrasive brush roll C3: T2 / T0 T2: Maximum rotational torque generated when removing deposits attached to the surface of a steel plate on which grooves of a reference depth are formed using an abrasive brush roll It is.

6. The C1 is set to 0.83, The C2 is set to 0.89, The C3 is set to 1.

11.

6. The groove depth monitoring system of claim 5.

7. the reference sputter amount is determined based on the amount of sputtering generated when the groove is formed on the surface of the steel sheet by the beam when the amount of focus shift of the beam irradiated on the surface of the steel sheet is zero and the power of the beam is a reference value; the reference rotational torque is determined based on a rotational torque generated when removing, by the abrasive brush roll, the deposit attached to the surface of the steel plate in which the grooves are formed by the beam when the amount of focus shift of the beam irradiated onto the surface of the steel plate is zero or the power of the beam is a reference value; The groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when formula (2) is satisfied.

5. The groove depth monitoring system of claim 4. 1 ≧ S / S0 ≧ C1, and T1 ≦ T ≦ T2 (2) however, S: sputter amount acquired by the sputter amount acquisition unit S0: Reference sputter amount C1: S1 / S0 S1: The minimum amount of spatter generated when forming a groove having a reference depth on the surface of a steel sheet T: Rotational torque acquired by the torque acquisition unit T1: Reference rotational torque, which is the minimum rotational torque generated when removing deposits attached to the surface of a steel plate having grooves with a reference depth formed thereon by an abrasive brush roll T2: Reference rotational torque, which is the maximum rotational torque generated when removing deposits attached to the surface of a steel plate having grooves with a reference depth formed thereon by an abrasive brush roll It is.

8. The C1 is set to 0.83, The T1 is set to 800 [Nm], The T2 is set to 1000 [Nm].

8. The groove depth monitoring system of claim 7.

9. The reference rotational torque is determined based on a rotational torque generated when removing, by the abrasive brush roll, the deposit attached to the surface of the steel plate in which the groove having the depth of the reference value is formed by the beam when the amount of focus deviation of the beam irradiated on the surface of the steel plate is zero.

2. The groove depth monitoring system of claim 1.

10. the reference rotational torque is determined based on a rotational torque generated when removing, by the abrasive brush roll, the deposit attached to the surface of the steel plate in which the groove having the depth of the reference value is formed by the beam, when the amount of focus shift of the beam irradiated onto the surface of the steel plate is zero and the power of the beam is a reference value; The groove depth determination unit determines that the depth of the groove formed on the surface of the steel plate is equal to or greater than the reference value when formula (3) is satisfied.

10. The groove depth monitoring system of claim 9. T1≦T≦T0 (3) however, T: Rotational torque acquired by the torque acquisition unit T0: Reference rotation torque T1: The minimum rotational torque generated when removing deposits attached to the surface of a steel plate on which grooves of a reference depth are formed using an abrasive brush roll It is.

11. The T0 is set to 900 [Nm]. The T1 is set to 800 [Nm]. The groove depth monitoring system of claim 10.

12. a beam irradiation device that irradiates a beam onto a surface of a steel sheet, which is a material for the electromagnetic steel sheet, to form grooves; an abrasive brush roll for removing deposits adhering to the surface of the steel plate in which the grooves are formed; A groove depth monitoring system for an electrical steel sheet according to any one of claims 1 to 3 and claims 9 to 11; An electromagnetic steel sheet manufacturing apparatus comprising:

13. a torque acquisition step of acquiring a rotational torque generated when removing, by an abrasive brush roll, deposits attached to the surface of the steel plate on which the grooves are formed by the beam; a groove depth determination step of determining whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired in the torque acquisition step and a predetermined reference rotational torque; A groove depth monitoring method comprising:

14. a torque acquisition step of acquiring a rotational torque generated when removing, by an abrasive brush roll, deposits attached to the surface of the steel plate on which the grooves are formed by the beam; a groove depth determination step of determining whether or not the depth of the groove formed on the surface of the steel plate is equal to or greater than a reference value based on the rotational torque acquired in the torque acquisition step and a predetermined reference rotational torque; A groove depth monitoring program that causes a computer to execute a process including the steps of:

Citation Information

Patent Citations

  • Production of grain oriented silicon steel sheet reduced in iron loss

    JP1995331332A

  • Laser groove processing monitoring method, laser groove processing monitoring device, laser groove processing device, and grain oriented silicon steel sheet production device

    JP2017122264A

  • Oriented electromagnetic steel sheet

    WO2016171129A1