HOT-ROLLED STEEL SHEET AND ITS MANUFACTURING METHOD

A high-strength hot-rolled steel sheet with controlled composition and processing achieves improved bending, stretch, and shrinkage flangeability, addressing the limitations of conventional steel sheets in complex automobile parts.

JP7569029B2Active Publication Date: 2024-10-17JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024504863
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-16
Filing Date
2023-09-19
Publication Date
2024-10-17
Estimated Expiration
2043-09-19

AI Technical Summary

Technical Problem

Conventional high-strength steel sheets face issues with poor shrinkage flangeability and stretch flangeability due to ferritic main phases with Ti carbides or bainitic structures, which also suffer from cracking and low formability, limiting their application in complex automobile parts.

Method used

A hot-rolled steel sheet with a specific composition and manufacturing process that includes controlled heating, rolling, and cooling to form a structure with nano-sized Ti or Nb carbides, low-angle grain boundaries, and limited ferrite content, enhancing strength and formability.

Benefits of technology

The solution results in a steel sheet with a yield strength of 650 MPa or more, exhibiting excellent bending, stretch, and shrinkage flangeability, suitable for weight reduction in automobile parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569029000001
    Figure 0007569029000001
  • Figure 0007569029000002
    Figure 0007569029000002
  • Figure 0007569029000003
    Figure 0007569029000003
Patent Text Reader

Abstract

The present invention provides a hot-rolled steel sheet having a yield strength of not less than 650 MPa, and having excellent bending workability, stretch flange formability, and shrink flange formability. The present invention also provides a method for producing the same. Provided is a hot-rolled steel sheet having a component composition arbitrarily selected of C, Si, Mn, P, S, Al, N, B, Ti, and Nb, having a metal structure which, in terms of area ratio, is 0-75% ferrite, with the total of bainite, martensite, tempered martensite, and residual austenite being not more than 3%, and crystal grains including a small angle boundary being not less than 25%, said hot-rolled steel sheet comprising a carbide including Ti or Nb with a mean particle size of not more than 8 nm, wherein yield strength is not less than 650 MPa. Also provided is a method for producing a hot-rolled steel sheet, said method comprising: a rough rolling step in which a steel raw material having the above component composition is heated or not heated; a finish rolling step in which a starting temperature is higher than 1000°C, the rolling reduction in each of a first pass and a second pass is not less than 35%, and the total rolling reduction from a third pass to rolling completion is not more than 85%; a cooling step; and a winding step.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot-rolled steel sheet having a yield strength of 650 MPa or more and excellent stretch flange formability and shrink flange formability, and a method for producing the same. TECHNICAL FIELD The hot-rolled steel sheet of the present invention is suitable as a material for automobile parts. [Background technology]

[0002] In recent years, from the perspective of protecting the global environment, the entire automobile industry has been oriented toward improving automobile fuel efficiency in order to regulate CO2 emissions. The most effective way to improve automobile fuel efficiency is to reduce the weight of automobiles by making the parts thinner, so in recent years the amount of high-strength steel sheets used as materials for automobile parts has been increasing. Generally, the formability of steel sheets tends to deteriorate as the strength of the steel sheets increases, so that improvement of the formability is essential to further expand the use of high-strength steel sheets. In particular, hot-rolled steel sheets are often used for suspension arm parts that are formed into complex shapes, and therefore excellent bendability, stretch flangeability, and shrink flangeability are required.

[0003] In order to solve these problems, various techniques have been proposed to increase the strength and improve the formability of steel sheets.

[0004] For example, Patent Document 1 discloses a hot-rolled steel sheet in which a ferrite phase with an area ratio of more than 95% is used as the main phase of the matrix, and Ti carbides with an average particle size of less than 10 nm are finely precipitated within the ferrite grains. This results in a high-strength hot-rolled steel sheet with excellent workability and a tensile strength of 780 MPa or more.

[0005] Patent Document 2 discloses a method for manufacturing a hot-rolled steel sheet, which includes hot rolling, which is performed by rough rolling at a rolling start temperature of 1200°C or higher and finish rolling at a rolling end temperature of 900°C or higher, and coiling at 580°C or higher. The hot-rolled steel sheet has a ferrite phase with an area ratio of 95% or higher and fine carbides containing TiN with an average particle size of 20 nm or more and Ti with an average particle size of less than 6 nm dispersed in the metal structure. As a result, it is said that a high-tensile hot-rolled steel sheet with a tensile strength of 590 MPa to 750 MPa and excellent punchability and stretch flangeability can be obtained.

[0006] In Patent Document 3, 1.0% or more of Mn is added for the purpose of improving hardenability, and the main phase is upper bainite with an area ratio of 75.0% or more and less than 97.0%, and the number density of second phase particles of 0.5 μm or more is 150,000 pieces / mm 2 The following hot-rolled steel sheet is disclosed. As a result, it is said that a high-strength hot-rolled steel sheet having a tensile strength of 980 MPa or more can be obtained. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-95996 A [Patent Document 2] JP 2013-133525 A [Patent Document 3] International Publication No. 2018 / 150955 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the conventional techniques disclosed in the above-mentioned patent documents have the following problems.

[0009] In the technologies proposed in Patent Documents 1 and 2, the main phase is a ferrite phase in which a large amount of Ti-containing carbides are finely dispersed, and therefore the shrink flangeability is poor and cracks may occur specifically at the shrink flange portion.

[0010] In addition, in Patent Document 3, a large amount of Mn, which has an adverse effect on shrink flangeability, is added. In addition, the main phase is an upper bainite structure (including a structure without Fe-based carbides and retained austenite) having Fe-based carbides and / or retained austenite between bainitic ferrite having a lath-like form. The lath-like structure means that transformation is performed at low temperatures, and there has been no precedent for the precipitation of carbides containing Ti in a structure having this lath-like structure. Furthermore, the bainite structure obtained at low temperatures in the past was often mixed with martensite and retained austenite, resulting in poor stretch flangeability.

[0011] The present invention has been developed in consideration of the above-mentioned problems associated with the conventional technology, and has an object to provide a hot-rolled steel sheet having a yield strength of 650 MPa or more and excellent bending workability, stretch flangeability, and shrink flangeability, and a manufacturing method thereof. [Means for solving the problem]

[0012] In order to solve the above problems, the inventors have conducted extensive research into the requirements for hot-rolled steel sheets to have both stretch flangeability and shrink flangeability as well as high strength. The thickness of the hot-rolled steel sheets in this study is 1.0 mm or more and 35.0 mm or less. It has been found that shrink flangeability is correlated with toughness, and it has been concluded that good shrink flangeability cannot be obtained with ferrite-based steels that have poor toughness. On the other hand, conventional bainite-based steels inevitably produce hard martensite and retained austenite, and therefore do not achieve the required bending workability or stretch flangeability.

[0013] Therefore, we attempted to precipitate carbides containing Ti or Nb in steel and then modify the parent phase structure to a structure other than ferrite, which has been mainly used in the past, at a coiling temperature of 600°C or higher, which is the temperature range in which the carbides precipitate. B was added as a component that sufficiently increases the driving force for the transformation from austenite to ferrite and to further increase hardenability, and conditions were set such that the degree of deformation of austenite during hot rolling would not be excessively high. It was found that this resulted in a new structure that was different from conventional ferrite, and that the bendability, stretch flangeability, and shrink flangeability of the hot-rolled steel sheet having this new structure were good.

[0014] The hot-rolled steel sheet according to the present invention, which has been developed based on the above findings, has the following configuration. [1] In mass%, C: 0.045% or more and less than 0.110%, Si: 1.5% or less, Mn: 0.7% or less, P: 0.05% or less, S: 0.010% or less, Al: 0.005% or more and 0.080% or less, N: 0.0060% or less, B: 0.0002% or more and 0.0050% or less, and further, one or both of Ti and Nb are contained within a range satisfying the following formula (1), Optionally, the composition further contains one or more of V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se in a total amount of 1% or less, with the balance being Fe and unavoidable impurities; The hot-rolled steel sheet has a metal structure with an area ratio of ferrite of 0% or more and 75% or less, a total of bainite, martensite, tempered martensite and retained austenite of 3% or less, crystal grains containing low-angle grain boundaries of 25% or more, carbides containing Ti or Nb with an average grain size of 8 nm or less, and a yield strength of 650 MPa or more. 0.09≦([%Nb] / 2)+[%Ti*]···(1) Here, [%Ti*] = [%Ti] - 48 [%N] / 14, and [%M] (M = Nb, Ti, N) is the content of Nb, Ti, and N in mass%. [2] In the above [1], the hot-rolled steel sheet has a plating layer on a surface thereof.

[0015] The method for producing a hot-rolled steel sheet according to the present invention, which was developed based on the above findings, is configured as follows. [3] A method for producing a hot-rolled steel sheet, comprising: a rough rolling step of heating a steel material having the composition described in [1] above to a heating temperature of 1200°C or higher, or without heating after casting, to a sheet bar, a finish rolling step of finish rolling the sheet bar to a hot-rolled steel sheet at a rolling start temperature exceeding 1000°C, with rolling reductions of 35% or more in the first and second passes, and a total rolling reduction of 85% or less from the third pass to the end of rolling, a cooling step of cooling the hot-rolled steel sheet at an average cooling rate of 40°C / s or more to a cooling stop temperature of 600°C to 700°C, and a coiling step of coiling the cooled hot-rolled steel sheet at a coiling temperature of 600°C to 700°C. [4] In the above [3], a method for producing a hot-rolled steel sheet includes a casting step of casting a steel material having a thickness of 35 mm or more and 200 mm or less and having the component composition described in [1] before the rough rolling step or the finish rolling step, and producing a sheet bar with or without applying the rough rolling step. [5] The method for producing a hot-rolled steel sheet according to [3] above further comprises a joining step of joining the roughly rolled sheet bar and a preceding sheet bar at 1,070°C or higher between the rough rolling step and the finish rolling step, and in the finish rolling step, the joined sheet bar is finish-rolled. [6] In any one of the above [3] to [5], the method for producing a hot-rolled steel sheet further includes a hot-rolled sheet annealing step of annealing the hot-rolled steel sheet at an annealing temperature of 720°C or less, and a plating step of plating the annealed hot-rolled steel sheet. [7] The method for producing a hot-rolled steel sheet according to the above [6], further comprising an alloying step of subjecting the plated hot-rolled steel sheet to an alloying treatment at a temperature of 460°C or higher and 600°C or lower. Effect of the Invention

[0016] According to the present invention, it is possible to manufacture a hot-rolled steel sheet having a high strength of 650 MPa or more in yield strength and excellent bendability, stretch flangeability, and shrink flangeability. If the hot-rolled steel sheet according to the present invention is applied to automobile parts, further weight reduction of the automobile parts can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the hot-rolled steel sheet according to this embodiment will be described. <Chemical composition of hot-rolled steel sheet> The composition of the hot-rolled steel sheet is, in mass%, C: 0.045% or more and less than 0.110%, Si: 1.5% or less, Mn: 0.7% or less, P: 0.05% or less, S: 0.010% or less, Al: 0.005% or more and 0.080% or less, N: 0.0060% or less, B: 0.0002% or more and 0.0050% or less, and further contains one or both of Ti and Nb in a range that satisfies the following formula (1): 0.09≦([%Nb] / 2)+[%Ti*]···(1) Here, [%Ti*] = [%Ti] - 48 [%N] / 14, and [%M] (M = Nb, Ti, N) is the content of Nb, Ti, and N in mass%. Each component is explained below. In the following explanation, "%" representing the content of a component means "% by mass."

[0018] C: 0.045% or more and less than 0.110% C contributes to increasing the strength of steel sheets by combining with Ti and Nb. To obtain a steel sheet with a yield strength of 650 MPa or more, it is necessary to ensure sufficient hardenability to suppress the progress of ferrite transformation after the completion of finish rolling, and the C content is set to 0.045% or more. On the other hand, if the C content is 0.110% or more, coarse cementite precipitates, making it impossible to obtain good bending workability and stretch flangeability. Therefore, the C content is set to 0.045% or more and less than 0.110%. Preferably, it is 0.050% or more and 0.100% or less.

[0019] Si: 1.5% or less Silicon is an element that increases the driving force for the transformation from austenite to ferrite and is effective in modifying the matrix structure at coiling temperatures of 600°C or higher. However, if the Si content exceeds 1.5%, the driving force for the transformation from austenite to ferrite becomes excessively high, increasing the risk of ferrite formation during the cooling process after hot rolling. Therefore, the Si content is set to 1.5% or less. It is preferably set to 0.15% or more and 1.1% or less.

[0020] Mn: 0.7% or less Mn reduces the driving force for transformation from austenite to ferrite. It is also an element that is prone to segregation, which reduces shrink flangeability. Therefore, the Mn content must be reduced as much as possible, and is set to 0.7% or less. The Mn content is preferably less than 0.50%. In manufacturing, 0.05% is inevitably mixed in, but even if it is 0%, the effect of the present invention is not impaired. In addition, from the viewpoint of improving the driving force for transformation from austenite to ferrite and hardenability, it is preferable that the following formula (2) is satisfied. 0.35≦0.8[%Si]+[%Mn]≦1.35···(2) Here, [%M] (M=Si, Mn) is the content of Si and Mn in mass %.

[0021] P:0.05% or less Since P is a harmful element that segregates at grain boundaries and reduces shrink flangeability, it is necessary to reduce the P content as much as possible to 0.05% or less. The P content is preferably 0.04% or less, but for use under more severe shrink flange processing conditions, it is more preferable to keep it at 0.02% or less. However, there are cases where 0.002% P is inevitably mixed in during manufacturing.

[0022] S: 0.010% or less S forms coarse sulfides in steel, which expand during hot rolling to become wedge-shaped inclusions, adversely affecting stretch flangeability. Therefore, since S is also a harmful element, it is preferable to reduce it as much as possible, and the S content is set to 0.010% or less. The S content is preferably 0.003% or less, but for use under more severe stretch flange forming conditions, it is more preferable to set it to 0.001% or less. In manufacturing, 0.0001% S may be inevitably mixed in.

[0023] Al: 0.005% or more and 0.080% or less When Al is added as a deoxidizer at the steelmaking stage, the Al content is 0.005% or more. Al forms oxides, which reduces stretch flangeability. Therefore, the Al content is set to 0.080% or less. The Al content is preferably 0.010% or more and 0.070% or less.

[0024] N: 0.0060% or less N is a harmful element that combines with Ti and Nb to form coarse carbonitrides, thereby adversely affecting workability, stretch flangeability, and strength. Therefore, the N content is reduced as much as possible to 0.0060% or less. The N content is preferably 0.0050% or less. In manufacturing, about 0.0005% of N may be inevitably mixed in.

[0025] B: 0.0002% or more and 0.0050% or less B is considered to contribute to the formation of crystal grains containing small angle grain boundaries, and is also an effective element for improving hardenability, and in order to obtain a bainitic ferrite structure, the B content is 0.0002% or more. However, even if the B content exceeds 0.0050%, the effect on the hardenability of the steel is saturated, so the B content is set to 0.0050% or less. Preferably, the B content is 0.0004% or more and 0.0030% or less.

[0026] Contains one or both of Ti and Nb within the range satisfying formula (1). 0.09≦([%Nb] / 2)+[%Ti*]···(1) Here, [%Ti*] = [%Ti] - 48 [%N] / 14, and [%M] (M = Nb, Ti, N) is the content of Nb, Ti, and N in mass%. Ti and Nb combine with C and contribute to increasing the strength of steel plate. Ti and Nb must satisfy formula (1) to stably obtain a yield strength of 650 MPa or more. To obtain a yield strength of 650 MPa or more, one or both of Ti and Nb are contained, and preferably, the Ti content is 0.06% or more and 0.18% or less, and the Nb content is 0.02% or more and 0.18% or less.

[0027] While C contributes to the formation of a structure with large crystal distortion, it also combines with Ti and Nb to form carbides. This use of C to form carbides reduces the hardenability of the steel. However, if C is contained in excess of Ti and Nb, coarse TiC cannot be dissolved when the slab is reheated, resulting in a decrease in strength and bending workability. From the above perspective, it is preferable that C, Ti, and Nb satisfy formula (3). 1.8≦([%C] / 12) / ([%Nb] / 93+[%Ti*] / 48)≦4.0 (3) Here, [%Ti*]=[%Ti]-48[%N] / 14, and [%M] (C, Nb, Ti, N) are the contents of C, Nb, Ti, and N in mass%.

[0028] The above is the basic composition of the hot-rolled steel sheet according to this embodiment, but optionally, it may further contain one or more of V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se in a total amount of 1% or less. This is because if the total content of any one or more elements is 1% or less, there is little effect on the properties of the hot-rolled steel sheet according to this embodiment. Preferably, the content of each element is 0.03% or less.

[0029] The chemical composition of the hot-rolled steel sheet according to this embodiment contains the above elements, with the balance being Fe and unavoidable impurities.

[0030] <Metal structure of hot-rolled steel sheet> Next, the metal structure of the hot-rolled steel sheet will be described. The metal structure of the hot-rolled steel sheet according to this embodiment has an area ratio of ferrite of 0% or more and 75% or less, a total area ratio of bainite, martensite, tempered martensite and retained austenite of 3% or less, crystal grains containing low-angle grain boundaries of 25% or more, and carbides containing Ti or Nb with an average particle size of 8 nm or less. In the following description, "%" representing the metal structure means "area ratio".

[0031] Ferrite: 0% to 75% Ferrite is a structure that reduces shrink flangeability. Ferrite does not contain small angle grain boundaries and is a structure with poor toughness, which also has a negative effect on shrink flangeability. In order to obtain the desired shrink flangeability, the area ratio of ferrite is 75% or less. Preferably, the area ratio of ferrite is 0% or more and 65% or less.

[0032] The total of bainite, martensite, tempered martensite, and retained austenite is 3% or less (including 0%) Bainite, martensite, tempered martensite, and retained austenite deteriorate bending workability and stretch flangeability, so it is preferable to reduce them as much as possible, and the total content of the above structures is 3% or less. The total content of the above structures may be 0%, and is preferably 0% or more and 2% or less. Bainite, martensite, and tempered martensite can be separated by crystal structure using electron backscatter diffraction pattern (EBSD) analysis. For example, whether or not bainite, martensite, and tempered martensite that satisfy the Kurdjumov-Sachs relationship with the parent phase corresponds to the (001) α pole figure of a single prior γ (austenite) grain region can be determined.

[0033] More than 25% of grains contain small angle boundaries The hot-rolled steel sheet according to the present embodiment is characterized in that nano-sized carbides containing Ti or Nb are precipitated in the crystal grains containing the low-angle grain boundaries. The crystal grains containing the low-angle grain boundaries make it possible to achieve both high strength with a yield strength of 650 MPa or more and workability, stretch flangeability, and shrink flangeability. For this reason, the crystal grains containing the low-angle grain boundaries are 25% or more. Preferably, the crystal grains containing the low-angle grain boundaries are 30% or more.

[0034] The average particle size of carbides containing Ti or Nb is 8 nm or less In the hot-rolled steel sheet according to the present embodiment, the steel sheet is strengthened by carbides containing Ti or Nb. To obtain a high-strength hot-rolled steel sheet having a yield strength of 650 MPa or more, it is necessary to set the average particle size of the carbides containing Ti or Nb dispersed in the steel to 8 nm or less. To stably obtain a yield strength of 650 MPa or more, it is preferable to set the average particle size of the carbides containing Ti or Nb to 5 nm or less. The carbides containing Ti or Nb may be composite carbides or single carbides containing either the element Ti or Nb. Furthermore, in the manufacture of the hot-rolled steel sheet according to the present embodiment, when the coiling temperature of the hot-rolled steel sheet is 600°C or higher, Nb, even though it is a substitutional element, diffuses sufficiently in the steel. By utilizing this property of Ti or Nb and diffusing and precipitating Ti or Nb in the steel, a steel sheet with a yield strength of 650 MPa or more can be obtained even if the structure of bainite, martensite, and tempered martensite, which are often used in high-strength steel sheets, is small. To obtain a steel sheet with a yield strength of 650 MPa or more, 80% or more of the contained Ti or Nb is utilized for precipitation. Preferably, 85% or more of the contained Ti or Nb is utilized for precipitation.

[0035] The hot-rolled steel sheet according to the present embodiment preferably has a plating layer on the surface. Even if the plating layer is formed, the function of the hot-rolled steel sheet is not impaired. The composition of the plating layer is preferably one or more selected from Zn, Si, Al, Ni, and Mg. The plated steel sheet in the present invention includes steel sheets that have been subjected to hot-dip galvanizing treatment (GI), steel sheets that have been subjected to hot-dip galvanizing treatment followed by alloying treatment (GA), and steel sheets that have been subjected to electrolytic galvanizing treatment (EG).

[0036] Next, a first embodiment of the method for producing a hot-rolled steel sheet according to the present embodiment will be described. In general, hot-rolled steel sheets are manufactured by casting a slab (steel material), loading the slab (steel material) that has been cooled to 1000°C or less into a heating furnace, heating it for a short time, and then reducing the thickness to a specified thickness in a hot rolling line and winding it into a coil. Alternatively, after casting a slab (steel material), the slab (steel material) that has once cooled to room temperature is heated for a long time in a heating furnace, and then reducing the thickness to a specified thickness in a hot rolling line and winding it into a coil. There is also a manufacturing method in which the cast slab (steel material) is directly sent to a hot rolling line without being heated in a heating furnace, and reduced to a specified thickness and wound into a coil. The manufacturing method of the hot-rolled steel sheet according to this embodiment can be applied not only to a process in which the steel material is heated after casting, but also to a process in which the steel material is directly sent to a hot rolling line without being heated after casting.

[0037] <First form steel material> The smelting method for producing the steel material of this embodiment is not particularly limited, and known smelting methods such as converters and electric furnaces can be adopted. Secondary refining may also be performed in a vacuum degassing furnace. The molten steel thus adjusted to the above-mentioned composition is then preferably made into a slab (steel material) by a continuous casting method, taking into consideration productivity and quality. Alternatively, the slab may be made into a slab by an ingot casting-blooming rolling method or other known casting methods.

[0038] <First type of rough rolling process> In this embodiment, the steel material is heated to a heating temperature of 1200° C. or higher, or is not heated after casting, and is roughly rolled to form a sheet bar. <First type of finish rolling process> Next, the steel is subjected to hot rolling, in which the starting temperature of the finish rolling exceeds 1000°C, the reduction rates of the first and second passes are each 35% or more, and the total reduction rate from the third pass to the end of rolling is 85% or less, to produce a hot-rolled steel sheet. <Cooling step of the first embodiment> Next, the hot-rolled steel sheet is cooled to a cooling stop temperature of 600° C. or more and 700° C. or less at an average cooling rate of 40° C. / s or more. <Winding process of the first embodiment> Thereafter, the cooled hot-rolled steel sheet is coiled at a coiling temperature of 600°C or higher and 700°C or lower.

[0039] Heating of steel material: Heating to 1200℃ or above, or not heating By dissolving the coarse carbides containing Ti or Nb precipitated in the slab (steel material) in a heating process before hot rolling, fine carbides containing Ti or Nb are precipitated after hot rolling. Therefore, in order to obtain carbides containing Ti or Nb with an average particle size of 8 nm or less, the slab (steel material) is heated to 1200°C or higher. The temperature is preferably 1220°C or higher, and when the Nb content is 0.12% or more, it is more preferable to heat the slab (steel material) to 1240°C or higher. There is no particular upper limit, but 1300°C is a manufacturing constraint in order to avoid thermal damage to the heating furnace. If the steel material is directly sent to the hot rolling line after being kept at 1200°C or higher after casting, the steel material is not heated after casting.

[0040] Finish rolling start temperature: Over 1000℃ Since the hot-rolled steel sheet according to the present embodiment has a steel composition with an increased driving force for the transformation from austenite to ferrite, ferrite is generated at a high temperature range of 600°C or higher under normal hot rolling conditions, and the desired steel structure cannot be obtained. Therefore, it is necessary to increase the hot rolling temperature and avoid rolling in the non-recrystallization temperature range of austenite. Therefore, the start temperature of the finish rolling is set to be more than 1000°C. Preferably, the start temperature of the finish rolling is 1010°C or higher. Due to the nature of the steel, there is no particular upper limit set for the start temperature of the finish rolling. Unless there is a heating device in the hot rolling line, the slab heating temperature is the substantial upper limit temperature for the start temperature of the finish rolling, and is often 1200°C or lower.

[0041] The reduction ratios for the first and second passes are 35% or more each. By increasing the reduction rate in the high temperature region where austenite recrystallizes, the degree of austenite processing at the end of finish rolling is reduced, and as a result, the nucleation of ferrite is suppressed and a metal structure with crystal grains containing low-angle grain boundaries is obtained. To obtain a metal structure with crystal grains containing low-angle grain boundaries, the reduction rates of the first and second passes are each 35% or more. Preferably, the reduction rates of the first and second passes are each 38% or more. The reduction ratios in the first and second passes can be calculated using the following formulas (4) and (5), respectively. Reduction rate of first pass = (t0-t1) / t0 (4) Reduction rate of the second pass = (t1-t2) / t1 (5) Here, t0, t1, and t2 are the plate thickness before finish rolling, the plate thickness after one pass, and the plate thickness after two passes, respectively.

[0042] Total reduction from the third pass to the end of rolling: 85% or less By controlling the degree of austenite processing until the completion of finish rolling and reducing the density of ferrite nucleation sites, the generation of polygonal ferrite is suppressed and the formation of a structure containing low-angle grain boundaries is promoted. To obtain a structure containing low-angle grain boundaries, the total reduction rate from the third pass to the completion of rolling is 85% or less. Preferably, the total reduction rate from the third pass to the completion of rolling is 80% or less. In addition, the total reduction rate from the third pass to the end of rolling can be calculated using equation (6). Total reduction rate from the third pass to the end of rolling = (t2-t f ) / t2···(6) Here, t f is the plate thickness after finish rolling is completed.

[0043] Cooling stop temperature after finish rolling is 600℃ to 700℃, with an average cooling rate of 40℃ / s or more If the cooling rate to 700°C or less after hot rolling is slow, polygonal ferrite (ferrite), which is coarse and has small crystal distortion within the grains, will form at high temperatures. To suppress the formation of this ferrite, it is necessary to cool the material at an average cooling rate of 40°C / s or more after hot rolling, and it is preferable to cool the material to 700°C or less within 2 seconds after hot rolling at an average cooling rate of 50°C / s or more. On the other hand, if the cooling stop temperature is below 600°C, it is difficult to obtain carbides containing Ti or Nb, and a steel sheet having a yield strength of 650 MPa or more cannot be obtained. Therefore, the cooling stop temperature is set to 600°C or more and 700°C or less. Preferably, the cooling stop temperature is 610°C or more and 690°C or less. Here, the average cooling rate may be calculated by {(cooling start temperature)-(cooling completion temperature)} / (forced cooling time other than natural cooling) after hot rolling, in which forced cooling other than natural cooling is performed. An example of the forced cooling method is water cooling.

[0044] Winding temperature: 600℃ or more and 700℃ or less For the same reason as the cooling stop temperature, the coiling temperature is set to 600° C. or higher and 700° C. or lower, and preferably 610° C. or higher and 690° C. or lower. If coiling is performed in this temperature range, the generation of ferrite, bainite, martensite, and retained austenite can be suppressed.

[0045] Next, a second embodiment of the method for producing a hot-rolled steel sheet according to the present embodiment will be described. In this embodiment, the difference from the first embodiment will be described. <Second type casting process> The hot rolled steel sheet according to the present embodiment can also be produced by the thin slab continuous casting method. When produced by the thin slab continuous casting method, a steel material having a thickness of 35 mm or more and 200 mm or less is cast. <Second type of rough rolling process> The cast steel material is heated to a heating temperature of 1200° C. or higher, or is not heated after casting, and is roughly rolled as necessary to form a sheet bar. The process after the finish rolling step is the same as that of the first embodiment.

[0046] Here, we will explain the slab (steel material) thickness that is specific to the thin slab continuous casting method.

[0047] Slab (steel material) thickness: 35mm to 200mm Unlike the continuous casting method, the thin slab before hot rolling is thin in the thin slab casting method, so the degree of austenite reduction in the hot rolling is low. If the slab thickness is less than 35 mm, the required reduction ratio cannot be obtained from the first pass to the second pass, or from the third pass to the end of rolling. On the other hand, if the slab thickness exceeds 200 mm, the casting speed of the steel material slows down, and the productivity advantage of the thin slab casting method compared to the continuous casting method is lost. Therefore, the slab thickness in the thin slab casting method is set to 35 mm or more and 200 mm or less.

[0048] Next, a third embodiment of the method for producing a hot-rolled steel sheet according to the present embodiment will be described. In this embodiment, the difference from the first and second embodiments will be described. In the third embodiment, a continuous hot rolling technique can be applied. <Third type of joining process> The sheet bar obtained in the first or second form is joined to the preceding sheet bar at 1070°C or higher before finish rolling. If the temperature is lower than 1070°C, it becomes difficult to roll at the finish rolling start temperature of 1000°C or higher. The preferred heating temperature for the sheet bar during joining is 1100°C or higher. The steps after the cooling step are the same as those in the first embodiment.

[0049] In the manufacturing method of the hot-rolled steel sheet according to the present embodiment, an annealing step of annealing in a continuous annealing line with an annealing temperature of 720°C or less and a plating step of plating in a continuous plating line can be applied. Furthermore, an alloying step of heating the plated hot-rolled steel sheet to 460°C or more and 600°C or less and performing an alloying treatment may be included. This annealing treatment or this plating treatment does not affect the material properties of the hot-rolled steel sheet according to the present embodiment. Therefore, it is possible to further perform a plating treatment on the surface of the hot-rolled steel sheet to provide a plating layer on the steel sheet surface.

[0050] As described above, the coating process and the composition of the coating bath do not affect the material properties of the hot-rolled steel sheet according to the present embodiment, and therefore, any of hot-dip galvanizing, galvannealing, and electrolytic galvanizing processes can be applied as the coating process. The composition of the coating bath can include one or more of Zn, Al, Mg, Si, and Ni. That is, the composition of the coating layer formed on the surface of the hot-rolled steel sheet in the coating process can include one or more of Zn, Al, Mg, Si, and Ni. EXAMPLES

[0051] The embodiments of the present invention will be further described with reference to examples. Note that the present invention is not limited to the manufacturing conditions and product performance shown in the following examples. The embodiments can achieve the desired performance within the scope of the present invention.

[0052] <First form using continuous casting method> Steel material having a thickness of 250 mm and having the chemical composition shown in Table 1 was hot rolled under the rough rolling and finish rolling conditions shown in Table 2, and then temper rolled at an elongation rate of 0.1 to 0.5% and pickled to produce steel plates for evaluation.

[0053] <Second form using thin slab continuous casting method> Steel having the chemical composition shown in Table 1 was hot rolled into thin slabs under the conditions shown in Table 3, and then the slabs were temper rolled to an elongation rate of 0.1 to 0.5% and pickled to produce steel sheets for evaluation.

[0054] <Third form by hot continuous rolling method> Steel having the chemical composition shown in Table 1 was joined into a sheet bar under the conditions shown in Table 4, and the joined sheet bar was hot rolled, temper rolled to an elongation rate of 0.1 to 0.5%, and pickled to produce the steel plate to be evaluated.

[0055] <Manufacturing process for adding a plating layer to hot-rolled steel sheets> The hot-rolled coil produced under the conditions in Table 2 was pickled, and then the hot-rolled steel sheet was galvanized in a continuous hot-dip galvanizing line (CGL) under the conditions shown in Table 5. In this manner, a continuous hot-dip galvanized steel sheet (GI) and an alloyed hot-dip galvanized steel sheet (GA) were produced.

[0056] [Table 1]

[0057] [Table 2]

[0058] [Table 3]

[0059] [Table 4]

[0060] [Table 5]

[0061] [Table 6]

[0062] The hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5 were evaluated in terms of metal structure, tensile properties, bending workability, stretch flangeability, and shrink flangeability by the following methods. The results are shown in Table 6.

[0063] (i) Area ratio of metal structure Test pieces were cut out from the hot-rolled steel plate so that the cross section parallel to the rolling direction was the observation surface, and the center of the plate thickness was etched with 1% nital to reveal the structure. Photographs of the 1 / 4t portion of the plate thickness were then taken using a scanning electron microscope (SEM) at 2000x magnification and an accelerating voltage of 15 kV, covering 10 fields of view. Ferrite is a crystal grain that does not show any corrosion marks within the grains and is observed with a lower brightness than martensite (gray on SEM). Bainite and tempered martensite are crystal grains in which three or more adjacent lath-shaped corrosion marks with a width of 500 nm or less are observed within the grains. Martensite is a crystal grain that does not show any corrosion marks within the grains, but is observed with a higher brightness than ferrite (white on SEM). The area ratio of the metal structure was determined using image analysis software (Photoshop elements and Image J) for the structures separated in the above manner. The retained austenite was measured by grinding the surface of the test piece to 3 / 4 of the total thickness, chemically polishing it to 0.1 mm or more, and then measuring the polished surface by X-ray diffraction. The volume fraction of the retained austenite was measured from the peaks of (200)α, (211)α, (220)α, (200)γ, (220)γ, and (311)γ using MoKα radiation as the incident radiation source. The volume fraction of the retained austenite phase obtained in this way was taken as the area fraction of the retained austenite. The procedure for determining the area fraction was to first obtain the fractions of bainite, martensite, and cementite, which are lath-shaped structures, from SEM images, then obtain the fraction of retained austenite from XRD, and finally obtain the fraction of crystal grains that do not have a lath morphology and contain low-angle grain boundaries using EBSD. The remainder of these crystal grains were calculated as the ferrite fraction, thereby deriving the fraction of each structure.

[0064] The area ratio of the structure of crystal grains containing small angle grain boundaries is 1 mm 2The above fields of view were analyzed by electron backscatter diffraction (EBSD). Using OIM Analysis software manufactured by TSL, grain boundaries with an angle difference of 15° or more were defined as high-angle grain boundaries, and grain boundaries with an angle difference of 2° or more and less than 15° were defined as low-angle grain boundaries, and the area ratio of crystal grains containing low-angle grain boundaries in grain boundaries surrounded by high-angle grain boundaries was calculated. For bainite and martensite, low-angle grain boundaries are also included in high-angle grain boundaries. Therefore, the area ratio of crystal grains containing low-angle grain boundaries in the hot-rolled steel sheet according to the present embodiment was determined by subtracting the area ratios of bainite, tempered martensite, and martensite from the area ratio of crystal grains containing low-angle grain boundaries obtained by EBSD analysis.

[0065] (ii) Average particle size of carbides containing Ti or Nb A thin film for observation was taken from a location equivalent to 1 / 4 of the plate thickness of the test piece, and 300 or more Ti or Nb-containing carbides were photographed at a magnification of 600,000 times or more using a transmission electron microscope. The circle equivalent diameters of the photographed Ti or Nb-containing carbides were calculated, and the average value was used as the average particle size. Carbides containing Ti or Nb can be identified by checking the presence or absence of a peak derived from Nb using EDX attached to the TEM.

[0066] (iii) Analysis of carbide precipitation amount containing Ti or Nb The front and back surfaces of the test piece were ground by 25% of the plate thickness, then dissolved in a 10% AA electrolytic solution, the solution was filtered through a filter with a mesh size of 0.2 μm, and the Ti and Nb concentrations in the filtered electrolytic solution were analyzed using ICP-MS. The amount of carbide precipitation containing Ti and Nb was determined by subtracting the Ti and Nb concentrations in the electrolytic solution from the amount of Ti and Nb contained.

[0067] (iv) Tensile test From the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, tensile test pieces of JIS No. 5 were prepared in the direction perpendicular to the rolling direction, and tensile tests conforming to the provisions of JIS Z 2241 (2011) were performed five times to obtain the average tensile strength (TS). The crosshead speed of the tensile test was 10 mm / min. In Table 6, the samples with a yield strength of 650 MPa or more were considered to be examples of the invention.

[0068] (v) Bending test From the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, test pieces with a width of 35 mm and a length of 100 mm were taken with the end faces ground, and a bending test was performed five times using the V-block method described in JIS Z 2248. Test pieces with an R / t of 0.5 or less are considered to have the characteristics required by the present invention and are marked with "◯" in the results in Table 6, while test pieces in which cracks were found on the surface of the test piece at least once out of the five tests under the above conditions are considered to not have the characteristics required by the present invention and are marked with "X".

[0069] (vi) Stretch flangeability Three test pieces of 120 mm x 120 mm were taken from the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, and a hole expansion test in accordance with JFST1001 (Japan Iron and Steel Federation standard) was performed five times to determine the average hole expansion ratio λ (%) and evaluate the stretch flangeability. In Table 6, λ of 80% or more is regarded as an inventive example, and is the mechanical property of the steel sheet required for the steel of the present invention.

[0070] (vii) Shrinkage flangeability Five samples for deep drawing with a diameter of 110 mm were taken from the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, and cylindrical drawing was performed using a φ50 mm punch with a punch shoulder radius of 5 mm. The cylindrically drawn product was then immersed in ice water for 30 minutes. Immediately after that, the cylindrically drawn product was placed under a 10 kg weight with a truncated cone punch with a tip angle of 45°, which was adjusted so that it would not hit the bottom of the cylindrically drawn product, located 1 m above the sample. The truncated cone punch was placed at a position where the center of the cylindrically drawn product coincided with the center of the cylindrically drawn product, with the opening of the cylindrically drawn product facing upward. The upper weight was immediately allowed to fall freely in the vertical direction toward the cylindrically drawn product, and the presence or absence of cracks in the cylindrically drawn product after the weight was dropped was confirmed. In Table 6, cylindrical drawn products that did not crack in any of the five repeated tests are marked with an "O" as the characteristic required by the present invention, while cylindrical drawn products that cracked in any of the five repeated tests or that cracked at least once due to the impact of the falling weight are marked with an "X".

[0071] All of the examples of the present invention had a yield strength (YS) of 650 MPa or more, and good bending workability, stretch flangeability and shrink flangeability were obtained. On the other hand, the comparative examples outside the range of the present invention either had a yield strength not reaching 650 MPa or did not obtain the bending workability, stretch flangeability or shrink flangeability required in the present invention.

Claims

1. In mass percent, C: 0.045% or more and less than 0.110%; Si: 1.5% or less, Mn: 0.7% or less, P: 0.05% or less, S: 0.010% or less, Al: 0.005% or more and 0.080% or less, N: 0.0060% or less, B: 0.0002% or more and 0.0050% or less; Further, one or both of Ti: 0.18% or less and Nb: 0.19% or less are contained within a range satisfying the following formula (1), Optionally, one or more of V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se are each contained in an amount of 0.03% or less, and in total, 1% or less; The balance is Fe and unavoidable impurities. The area ratio of the metal structure is Ferrite is 0% or more and 75% or less, The total of bainite, martensite, tempered martensite and retained austenite is 3% or less; The percentage of crystal grains containing small angle boundaries is 25% or more, A hot-rolled steel sheet having a yield strength of 650 MPa or more and containing carbides containing Ti or Nb with an average grain size of 8 nm or less. Note 0.09≦([%Nb] / 2)+[%Ti*]...(1) Here, [% Ti*] = [% Ti] - 48 [% N] / 14, and [% M] (M = Nb, Ti, N) is the content of Nb, Ti, and N in mass%.

2. The hot-rolled steel sheet according to claim 1, further comprising a plating layer on a surface of the hot-rolled steel sheet.

3. A rough rolling process in which the steel material having the composition according to claim 1 is roughly rolled into a sheet bar by heating the steel material to a heating temperature of 1200 ° C. or more, or by not heating the steel material after casting; a finish rolling process in which the sheet bar is finish-rolled at a rolling start temperature exceeding 1000°C, with rolling reductions of 35% or more in the first and second passes, and with a total rolling reduction of 85% or less from the third pass to the end of rolling, to obtain a hot-rolled steel sheet; A cooling step of cooling the hot-rolled steel sheet to a cooling stop temperature of 600° C. or more and 700° C. or less at an average cooling rate of 40° C. / s or more; a coiling step of coiling the cooled hot-rolled steel sheet at a coiling temperature of 600° C. or more and 700° C. or less; Including, The obtained hot-rolled steel sheet has the following area ratio of metal structure: Ferrite is 0% or more and 75% or less, The total content of bainite, martensite, tempered martensite and retained austenite is 3% or less, The percentage of crystal grains containing small angle grain boundaries is 25% or more, A method for producing a hot-rolled steel sheet, comprising the steps of: having carbides containing Ti or Nb having an average particle size of 8 nm or less; and having a yield strength of 650 MPa or more.

4. A casting process is included prior to the rough rolling process or the finish rolling process, in which a steel material having a thickness of 35 mm or more and 200 mm or less and having the component composition according to claim 1 is cast, The method for producing a hot-rolled steel sheet according to claim 3, characterized in that the rough rolling step is applied or not applied to produce a sheet bar.

5. Between the rough rolling step and the finish rolling step, a joining step of joining the roughly rolled sheet bar and a preceding sheet bar at 1070 ° C. or more is included, The method for producing a hot-rolled steel sheet according to claim 3, characterized in that, in the finish rolling step, the joined sheet bar is finish-rolled.

6. Further, a hot-rolled steel sheet annealing process is performed in which the hot-rolled steel sheet is annealed at an annealing temperature of 720° C. or less. A plating process for plating the annealed hot-rolled steel sheet; The method for producing a hot-rolled steel sheet according to any one of claims 3 to 5, further comprising the steps of:

7. The method for producing a hot-rolled steel sheet according to claim 6, further comprising an alloying step of subjecting the plated hot-rolled steel sheet to an alloying treatment at a temperature of 460°C or higher and 600°C or lower.

Citation Information

Patent Citations

  • High-strength hot-rolled steel sheet having excellent workability and method for producing the same

    JP2013095996A

  • High-tensile hot-rolled steel sheet excellent in blanking property and stretch flange formability, and manufacturing method therefor

    JP2013133525A

  • HOT-DIP Zn-Al-Mg BASED PLATED STEEL SHEET AND METHOD FOR PRODUCING SAME

    JP2021055135A

  • High-strength steel plate with excellent formability and stability of material properties, and method for manufacturing same

    WO2012147898A1

  • High-strength hot-rolled steel sheet and manufacturing process therefor

    WO2014119259A1