Adhesive tape

The adhesive tape with a controlled silicone compound distribution addresses the adhesion-peelability trade-off by ensuring strong fixation and easy release of semiconductor packages, enhancing manufacturing efficiency and reducing defects.

JP7569161B2Active Publication Date: 2024-10-17SEKISUI CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020078637
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-27
Publication Date
2024-10-17
Estimated Expiration
2040-04-27

AI Technical Summary

Technical Problem

Existing adhesive tapes for semiconductor packages face a trade-off between adhesion and easy peelability, making it difficult to securely fix and easily release the semiconductor packages during manufacturing processes, especially with the increasing susceptibility to high-frequency noise and device compactness in communication devices.

Method used

An adhesive tape with a silicone compound layer irradiated by 405 nm ultraviolet rays, achieving a specific Si ion intensity ratio range (A/B) through TOF-SIMS and sputtering, ensuring both strong adhesion and easy peelability by controlling the distribution of the silicone mold release agent.

Benefits of technology

The adhesive tape provides sufficient adhesion to securely fix semiconductor packages during manufacturing while allowing easy release without residue, improving dicing and pickup performance and reducing contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569161000001
    Figure 0007569161000001
  • Figure 0007569161000002
    Figure 0007569161000002
  • Figure 0007569161000003
    Figure 0007569161000003
Patent Text Reader

Abstract

To provide a pressure-sensitive adhesive tape that achieves both an easy release property and an adhesion property capable of sufficiently fixing an adherend.SOLUTION: The pressure-sensitive adhesive tape has a pressure-sensitive adhesive layer containing a silicone compound. After a surface of the pressure-sensitive adhesive layer is irradiated with the UV of 405 nm such that the amount of irradiation of the pressure-sensitive adhesive layer surface is 2500 mJ / cm2, a Si ionic strength ratio 0 (Si ionic strength / total ionic strength) of the pressure-sensitive adhesive layer surface is measured using the TOF-SIMS. Subsequently, sputtering is applied once to the surface portion of the pressure-sensitive adhesive layer of which the Si ionic strength ratio 0 is measured, and then a Si ionic strength ratio 1 is measured using the TOF-SIMS. Subsequently, the sputtering and measurement step is performed n times to obtain Si ionic strength ratios 0 to n. Then, the ratio (A / B) of the average (A) for the Si ionic strength ratios 1 to 5 to the average (B) for the Si ionic strength ratios 20 to 25 is from 1.1 to 3.0 inclusive.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive tape. [Background technology]

[0002] In the manufacture of electronic components such as semiconductor packages, each component may be temporarily fixed with an adhesive tape. For example, in the manufacture of semiconductor packages, dicing is performed to divide a large number of undiced semiconductor packages made on a wafer into individual semiconductor packages. In this process, an adhesive tape (dicing tape) is used to prevent misalignment and damage to the semiconductor packages. For example, Patent Document 1 discloses a dicing tape that has a photocurable adhesive layer and that can suppress chip jumping and ensure excellent pick-up properties by setting the breaking elongation of the adhesive layer before curing within a specific range. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-149398 A Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, communication devices such as mobile phones are becoming increasingly high-frequency due to faster communication speeds and an increase in the amount of information they handle, and this high-frequency noise is causing problems with malfunctions of semiconductor packages. In particular, in recent years, communication devices have become more compact, resulting in increased device density and lower device voltages, making semiconductor packages more susceptible to the effects of high-frequency noise, and the problem of malfunctions has become more pronounced. To solve this problem, a method has been proposed in which the semiconductor package is covered with a metal film by sputtering to block high frequencies. In such a method of manufacturing a semiconductor package that includes a sputtering process, an adhesive tape is attached to the semiconductor package as a protective tape, and sputtering is performed after dicing. After sputtering, the package is peeled off from the adhesive tape by a needle pick-up or the like.

[0005] When the process from dicing to picking up is performed as a series of steps with the adhesive tape attached, adhesion that can reliably fix the semiconductor package is required during dicing, while easy releasability is required during picking up to prevent pick-up failure. However, since there is a trade-off between adhesion and easy releasability, it is difficult to obtain an adhesive tape that has both adhesion and easy releasability.

[0006] An object of the present invention is to provide a pressure-sensitive adhesive tape which combines sufficient adhesion to secure an adherend with easy releasability. [Means for solving the problem]

[0007] The present invention relates to an adhesive tape having an adhesive layer containing a silicone compound, the adhesive layer being irradiated with 405 nm ultraviolet light at an irradiation dose of 2500 mJ / cm2. 2 the pressure-sensitive adhesive layer surface is irradiated so as to obtain a value of 0, and then a Si ion intensity ratio 0 (Si ion intensity / total ion intensity) on the surface of the pressure-sensitive adhesive layer is measured using TOF-SIMS; then, sputtering is performed once on the surface portion of the pressure-sensitive adhesive layer where the Si ion intensity ratio 0 was measured, and a Si ion intensity ratio 1 is measured using TOF-SIMS; and then, the sputtering and measurement steps are performed n times, and when Si ion intensity ratios 0 to n are obtained, the ratio (A / B) of the average value (A) of Si ion intensity ratios 1 to 5 and the average value (B) of Si ion intensity ratios 20 to 25 is 1.1 or more and 3.0 or less. The present invention will be described in detail below.

[0008] The pressure-sensitive adhesive tape of the present invention has a pressure-sensitive adhesive layer containing a silicone compound, and is irradiated with 405 nm ultraviolet light on the surface of the pressure-sensitive adhesive layer at an irradiation dose of 2500 mJ / cm2. 2 After irradiating the adhesive layer so as to obtain a Si ion intensity ratio of 0, the Si ion intensity ratio 0 (Si ion intensity / total ion intensity) on the surface of the adhesive layer is measured using TOF-SIMS, and then sputtering is performed once on the surface portion of the adhesive layer where the Si ion intensity ratio 0 was measured, and the Si ion intensity ratio 1 is measured using TOF-SIMS. The sputtering and measurement steps are then performed n times to obtain Si ion intensity ratios of 0 to n, and the ratio (A / B) of the average value (A) of Si ion intensity ratios 1 to 5 to the average value (B) of Si ion intensity ratios 20 to 25 is 1.1 or more and 3.0 or less. In the above measurement, TOF-SIMS plays a role of indicating the amount of silicone release agent present on the surface of the adhesive layer in the form of an ion intensity ratio, and sputtering plays a role of scraping the surface of the adhesive layer in the thickness direction. By performing the above measurement, the distribution of the release agent in the thickness direction of the adhesive layer of the adhesive tape can be obtained. By the ratio of the average value of the Si ion intensity ratio of 1 to 5, that is, the amount of release agent near the surface of the adhesive layer to the average value of the Si ion intensity ratio of 20 to 25, that is, the amount of release agent inside the adhesive layer, being within the above range, the adhesive tape can be easily peeled off when it is no longer needed while exhibiting adhesion that can sufficiently fix the adherend. If the above A / B is less than 1.1, the release agent does not sufficiently bleed out to the interface with the adherend, so that the peelability is reduced, and if the above A / B is 3.0 or more, the amount of release agent present at the interface with the adherend becomes too large, so that the adhesion is reduced. From the viewpoint of achieving both adhesion and easy releasability, the A / B is preferably 1.2 or more, more preferably 1.3 or more, even more preferably 1.4 or more, even more preferably 1.6 or more, and particularly preferably 1.8 or more. From the viewpoint of achieving both adhesion and easy releasability, the A / B is preferably 2.9 or less, more preferably 2.8 or less, even more preferably 2.6 or less, and even more preferably 2.4 or less. The A / B can be adjusted by the type of adhesive, the type of release agent, and the manufacturing method of the adhesive tape. For example, when an acrylic adhesive is used as the adhesive, the silicone compound works effectively, so that the A / B is easily satisfied. In addition, with regard to the manufacturing method, the A / B can be adjusted by the stirring conditions, drying conditions, curing conditions, and other conditions during the manufacturing of the adhesive tape.

[0009] Time-of-Flight Secondary Ion Mass Spectrometry (TOF-SIMS) is a method in which a solid sample is irradiated with an ion beam (primary ions) and the ions (secondary ions) emitted from the surface are mass-separated using the difference in their flight times (flight time is proportional to the square root of weight). TOF-SIMS can obtain spectral information on elements and molecular species present in a region of 1 nm from the sample surface in the thickness direction with high detection sensitivity.

[0010] Sputtering involves ejecting high-pressure gas such as argon in a vacuum, ionizing the formed gas clusters, oxygen, cesium, etc., and irradiating the target surface with an ion beam at high speed, making it possible to cut the target surface to a depth on the order of nanometers to micrometers.

[0011] It is possible to obtain a depth profile from the spectrum information obtained by alternately repeating the above sputtering and the above TOF-SIMS measurement. Specifically, the measurement values ​​are plotted with the number of sputterings on the horizontal axis and the intensity ratio of the secondary ions at the number of sputterings on the vertical axis, and the relationship between the number of sputterings and the secondary ion intensity ratio is graphed, whereby a depth profile can be obtained and the distribution of each ion from the pressure-sensitive adhesive layer surface in the depth direction can be evaluated. The analytical device used for TOF-SIMS is the "PHInanoTOFII" manufactured by ULVAC-PHI, Inc. In addition, in the above measurement, the Si ion intensity ratio is calculated by dividing the Si ion intensity ratio by the Si ion intensity ratio by the Si ion intensity ratio by the Bi3 ++ The measurements are performed using a dual beam method in which an ion gun (voltage: 30 KV, current: 0.5 μA) is used as the primary ion source for measurement and argon cluster ions (voltage: 5 KV, 5 nA) are used as the sputtering source (secondary ion source) for sputtering. Here, the argon gas cluster ions used are those formed by gathering together several thousand argon atoms to form clusters.

[0012] The average value of the above-mentioned Si ion intensity ratios 1 to 5 is preferably 0.001 or more and 0.03 or less. By setting the average value of the Si ion intensity ratio near the surface of the pressure-sensitive adhesive layer within the above range, it is easy to adjust to the above A / B range, and it is possible to more easily achieve both adhesion and easy releasability. From the viewpoint of more easily achieving both adhesion and easy releasability, the average value of the Si ion intensity ratios 1 to 5 is more preferably 0.002 or more, even more preferably 0.003 or more, and even more preferably 0.006 or more. From the viewpoint of more easily achieving both adhesion and easy releasability, the average value of the Si ion intensity ratios 1 to 5 is more preferably 0.025 or less, even more preferably 0.02 or less, and even more preferably 0.015 or less.

[0013] The adhesive (hereinafter simply referred to as adhesive) constituting the adhesive layer is not particularly limited, and may contain either a non-curing type adhesive or a curing type adhesive. Specific examples include rubber-based adhesives, acrylic-based adhesives, vinyl alkyl ether-based adhesives, silicone-based adhesives, polyester-based adhesives, polyamide-based adhesives, urethane-based adhesives, and styrene-diene block copolymer-based adhesives. Among them, acrylic-based adhesives are preferred because they tend to satisfy the above A / B, and acrylic curing type adhesives are more preferred.

[0014] Examples of the curable adhesive include photocurable adhesives that are crosslinked and cured by irradiation with light, and thermosetting adhesives that are crosslinked and cured by heating. The photocurable pressure-sensitive adhesive may, for example, be a photocurable pressure-sensitive adhesive containing a polymerizable polymer as a main component and a photopolymerization initiator. The thermosetting adhesive may be, for example, a thermosetting adhesive containing a polymerizable polymer as a main component and a thermal polymerization initiator. Among them, a photocurable adhesive is preferred because it is less likely to damage the adherend and can be easily cured.

[0015] The above-mentioned polymerizable polymer can be obtained, for example, by previously synthesizing a (meth)acrylic polymer having a functional group in the molecule (hereinafter referred to as a functional group-containing (meth)acrylic polymer), and reacting it with a compound having a functional group reactive with the above-mentioned functional group and a radically polymerizable unsaturated bond in the molecule (hereinafter referred to as a functional group-containing unsaturated compound).

[0016] The functional group-containing (meth)acrylic polymer is obtained by copolymerizing an acrylic acid alkyl ester and / or a methacrylic acid alkyl ester, the carbon number of which in the alkyl group is usually in the range of 2 to 18, a functional group-containing monomer, and, if necessary, another modifying monomer copolymerizable therewith. The weight average molecular weight of the functional group-containing (meth)acrylic polymer is usually about 200,000 to 2,000,000.

[0017] Examples of the functional group-containing monomer include carboxyl group-containing monomers such as acrylic acid and methacrylic acid, hydroxyl group-containing monomers such as hydroxyethyl acrylate and hydroxyethyl methacrylate, and epoxy group-containing monomers such as glycidyl acrylate and glycidyl methacrylate. Other examples include isocyanate group-containing monomers such as isocyanate ethyl acrylate and isocyanate ethyl methacrylate, and amino group-containing monomers such as aminoethyl acrylate and aminoethyl methacrylate.

[0018] Examples of the other copolymerizable modifying monomers include various monomers used in general (meth)acrylic polymers, such as vinyl acetate, acrylonitrile, and styrene.

[0019] As the functional group-containing unsaturated compound to be reacted with the functional group-containing (meth)acrylic polymer, the same as the functional group-containing monomer described above can be used according to the functional group of the functional group-containing (meth)acrylic polymer. For example, when the functional group of the functional group-containing (meth)acrylic polymer is a carboxyl group, an epoxy group-containing monomer or an isocyanate group-containing monomer is used. When the functional group is a hydroxyl group, an isocyanate group-containing monomer is used. When the functional group is an epoxy group, a carboxyl group-containing monomer or an amide group-containing monomer such as acrylamide is used. When the functional group is an amino group, an epoxy group-containing monomer is used.

[0020] To obtain the functional group-containing (meth)acrylic polymer, the raw material monomers may be subjected to a radical reaction in the presence of a polymerization initiator. As a method for radically reacting the raw material monomers, i.e., a polymerization method, a conventionally known method may be used, such as solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc. The polymerization initiator used in the radical reaction for obtaining the functional group-containing (meth)acrylic polymer is not particularly limited, and examples thereof include organic peroxides and azo compounds. Examples of the organic peroxides include 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxy-3,5,5-trimethylhexanoate, and t-butylperoxylaurate. Examples of the azo compounds include azobisisobutyronitrile and azobiscyclohexanecarbonitrile. These polymerization initiators may be used alone or in combination of two or more.

[0021] Examples of the photopolymerization initiator contained in the photocurable adhesive include those that are activated by irradiation with light having a wavelength of 250 to 800 nm. Examples of such photopolymerization initiators include acetophenone derivative compounds such as methoxyacetophenone, benzoin ether compounds such as benzoin propyl ether and benzoin isobutyl ether, ketal derivative compounds such as benzyl dimethyl ketal and acetophenone diethyl ketal, and phosphine oxide derivative compounds. Other examples include bis(η5-cyclopentadienyl)titanocene derivative compounds, benzophenone, Michler's ketone, chlorothioxanthone, todecylthioxanthone, dimethylthioxanthone, diethylthioxanthone, α-hydroxycyclohexylphenyl ketone, and 2-hydroxymethylphenylpropane. These photopolymerization initiators may be used alone or in combination of two or more.

[0022] The thermal polymerization initiator contained in the thermosetting adhesive may be one that is decomposed by heat to generate active radicals that initiate polymerization curing. Specific examples of the thermal polymerization initiator include dicumyl peroxide, di-t-butyl peroxide, t-butyl peroxybenzoyl, t-butyl hydroperoxide, benzoyl peroxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, and di-t-butyl peroxide. Among these thermal polymerization initiators, commercially available ones are not particularly limited, but for example, Perbutyl D, Perbutyl H, Perbutyl P, Perpenta H (all manufactured by NOF Corp.), etc. are suitable. These thermal polymerization initiators may be used alone or in combination of two or more kinds.

[0023] The pressure-sensitive adhesive layer may further contain a radically polymerizable polyfunctional oligomer or monomer. By containing a radically polymerizable polyfunctional oligomer or monomer, the photocurability and thermocurability are improved. The polyfunctional oligomer or monomer preferably has a weight-average molecular weight of 10,000 or less, and more preferably has a molecular weight of 5,000 or less and has 2 to 20 radically polymerizable unsaturated bonds in the molecule, so that the pressure-sensitive adhesive layer is efficiently three-dimensionally reticulated by heating or light irradiation. In the present invention, the weight-average molecular weight can be determined by gel permeation chromatography, for example, by using an HSPgel HR MB-M 6.0×150 mm column and THF as an eluent at 40° C. and determining the weight-average molecular weight based on polystyrene standards.

[0024] Examples of the polyfunctional oligomer or monomer include trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol monohydroxypentaacrylate, dipentaerythritol hexaacrylate, and the above-mentioned methacrylates. Other examples include 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, commercially available oligoester acrylates, and the above-mentioned methacrylates. These polyfunctional oligomers or monomers may be used alone or in combination of two or more.

[0025] The pressure-sensitive adhesive layer contains a silicone compound. By containing a silicone compound in the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer is prevented from burning even when placed in a high-temperature environment of 200° C. or more, and the silicone compound bleeds out to the adherend interface during peeling, making peeling easy. In addition, by distributing the silicone compound in the pressure-sensitive adhesive layer so as to satisfy the above-mentioned A / B, a pressure-sensitive adhesive tape having sufficient adhesion to the adherend while also having excellent easy peelability can be obtained.

[0026] The silicone compound preferably has a functional group capable of crosslinking with the pressure-sensitive adhesive. Since the silicone compound has a functional group capable of crosslinking with the pressure-sensitive adhesive, it chemically reacts with the pressure-sensitive adhesive upon irradiation with light or heating, and the silicone compound is incorporated into the pressure-sensitive adhesive, thereby preventing the silicone compound from adhering to and contaminating the adherend.

[0027] The silicone skeleton of the silicone compound is not particularly limited, and may be either a D-form or a DT-form. The silicone compound preferably has a functional group capable of crosslinking with the pressure-sensitive adhesive on a side chain or end of the silicone skeleton. In particular, when a silicone compound is used that has a D-type silicone skeleton and a functional group at the end that can be crosslinked with the above-mentioned pressure-sensitive adhesive, it exhibits high adhesion and can be peeled off without leaving any adhesive residue even after chemical treatment or high-temperature treatment at 200°C or higher.

[0028] The functional group capable of crosslinking with the pressure-sensitive adhesive is appropriately selected depending on the pressure-sensitive adhesive. For example, when the pressure-sensitive adhesive is a photocurable adhesive or a thermosetting adhesive mainly composed of a (meth)acrylic acid alkyl ester-based polymerizable polymer having a radically polymerizable unsaturated bond in the molecule, a functional group capable of crosslinking with a (meth)acrylic group is selected. The functional group capable of crosslinking with the (meth)acrylic group is a functional group having an unsaturated double bond, and specific examples thereof include a vinyl group, a (meth)acrylic group, an allyl group, and a maleimide group.

[0029] The functional group equivalent of the silicone compound is not particularly limited, but the preferred lower limit is 1 and the preferred upper limit is 20. When the functional group equivalent is 1 or more, the silicone compound is sufficiently incorporated into the pressure-sensitive adhesive, which can suppress contamination of the adherend and also exhibit higher releasability. When the functional group equivalent is 20 or less, sufficient adhesive strength can be obtained. The more preferred upper limit of the functional group equivalent is 10, the more preferred lower limit is 2, and the even more preferred upper limit is 6.

[0030] The weight average molecular weight of the silicone compound is not particularly limited, but the preferred lower limit is 300 and the preferred upper limit is 50000. If the weight average molecular weight is 300 or more, the chemical resistance and heat resistance are improved, and if it is 50000 or less, the mixture with the pressure-sensitive adhesive is improved. The more preferred lower limit of the weight average molecular weight is 400 and the more preferred upper limit is 10000, and the even more preferred lower limit is 500 and the even more preferred upper limit is 5000.

[0031] The method of synthesizing the silicone compound is not particularly limited.The method of synthesizing the silicone compound having functional group that can be crosslinked with the pressure-sensitive adhesive can be, for example, made the silicone resin having SiH group react with the vinyl compound having functional group that can be crosslinked with the pressure-sensitive adhesive by hydrosilylation reaction, and the functional group that can be crosslinked with the pressure-sensitive adhesive can be introduced into the silicone resin.In addition, the method of condensation reaction of siloxane compound with the siloxane compound having functional group that can be crosslinked with the pressure-sensitive adhesive can also be mentioned.

[0032] Among the silicone compounds, commercially available ones include silicone compounds having methacryl groups at both ends, such as X-22-164, X-22-164AS, X-22-164A, X-22-164B, X-22-164C, and X-22-164E manufactured by Shin-Etsu Chemical Co., Ltd. In addition, silicone compounds having methacryl groups at one end, such as X-22-174DX, X-22-2426, and X-22-2475 manufactured by Shin-Etsu Chemical Co., Ltd., and silicone compounds having an acrylic group, such as EBECRYL350 and EBECRYL1360 manufactured by Daicel-Allnex Corporation, are also included. Further examples include silicone compounds having an acrylic group, such as AC-SQ TA-100 and AC-SQ SI-20 manufactured by Toagosei Co., Ltd., and silicone compounds having a methacrylic group, such as MAC-SQ TM-100, MAC-SQ SI-20, and MAC-SQ HDM manufactured by Toagosei Co., Ltd.

[0033] Among these, the above silicone compounds have particularly high chemical resistance and heat resistance, and are highly polar, so that they easily bleed out from the pressure-sensitive adhesive tape. Therefore, silicone compounds having a (meth)acrylic group in a siloxane skeleton, represented by the following general formula (I), general formula (II), or general formula (III), are preferred.

[0034] [ka]

[0035] In the formula, X and Y each independently represent an integer of 0 to 1200 (excluding the case where both X and Y are 0), and R represents a functional group having an unsaturated double bond.

[0036] Among the silicone compounds having a (meth)acrylic group in a siloxane skeleton represented by the above general formula (I), general formula (II), and general formula (III), commercially available ones include, for example, EBECRYL350 and EBECRYL1360 (in both cases, R is an acrylic group) manufactured by Daicel-Allnex Corporation.

[0037] The content of the silicone compound is preferably 1 part by weight or more and 40 parts by weight or less relative to 100 parts by weight of the pressure-sensitive adhesive. When the content of the silicone compound is 1 part by weight or more, peeling from the adherend becomes easier, and when it is 40 parts by weight or less, contamination of the adherend can be further suppressed. From the viewpoint of further suppressing peeling from the adherend and contamination, the content of the silicone compound is more preferably 10 parts by weight or more, and more preferably 30 parts by weight or less.

[0038] The pressure-sensitive adhesive layer may further contain an inorganic filler such as fumed silica. The incorporation of an inorganic filler increases the cohesive strength of the pressure-sensitive adhesive layer. Therefore, when the pressure-sensitive adhesive layer contains an inorganic filler such as fumed silica, the pressure-sensitive adhesive tape can be more easily peeled off from the adherend without leaving any adhesive residue when the pressure-sensitive adhesive tape is no longer needed.

[0039] The content of the inorganic filler is not particularly limited, but is preferably 1 part by weight or more and 20 parts by weight or less with respect to 100 parts by weight of the adhesive. When the content of the inorganic filler is 1 part by weight or more, the peelability is further improved, and the pick-up property of the semiconductor package can be further improved. When the content of the inorganic filler is 20 parts by weight or less, the inorganic filler can be stably dispersed in the coating liquid. From the viewpoint of improving the pick-up property of the semiconductor package, the content of the inorganic filler is more preferably 3 parts by weight or more, and more preferably 15 parts by weight or less.

[0040] The pressure-sensitive adhesive layer preferably contains a crosslinking agent. By including a crosslinking agent, the cohesive strength of the pressure-sensitive adhesive layer can be increased, thereby improving the adhesive strength. The crosslinking agent is not particularly limited, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among these, isocyanate-based crosslinking agents are preferred because they provide higher adhesive strength.

[0041] The content of the crosslinking agent in the pressure-sensitive adhesive layer is preferably 0.1 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight of the pressure-sensitive adhesive. By including the crosslinking agent in the above range, the adhesive can be crosslinked appropriately to further increase the adhesive strength. From the viewpoint of further increasing the adhesive strength, the lower limit of the content of the crosslinking agent is more preferably 0.5 parts by weight, even more preferably 1.0 parts by weight, and even more preferably 15 parts by weight, and even more preferably 10 parts by weight.

[0042] The pressure-sensitive adhesive layer may contain known additives such as plasticizers, resins, surfactants, waxes, fine particle fillers, etc. The additives may be used alone or in combination of two or more kinds.

[0043] The pressure-sensitive adhesive layer preferably has a gel fraction of 44% or more and 67% or less. When the gel fraction of the adhesive layer is within the above range, the adhesive layer can be attached to the adherend with sufficient adhesive strength, and the adherend can be more sufficiently fixed. From the viewpoint of improving adhesive strength, the gel fraction of the adhesive layer is more preferably 47% or more, even more preferably 50% or more, more preferably 64% or less, and even more preferably 60% or less. In addition, when the adhesive is a curable adhesive, the gel fraction refers to that before curing.

[0044] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but the preferred lower limit is 5 μm, and the preferred upper limit is 500 μm. When the thickness of the pressure-sensitive adhesive layer is within this range, the pressure-sensitive adhesive layer can be attached to the adherend with sufficient adhesive strength, and the adherend can be sufficiently fixed. From the viewpoint of improving the adhesive strength, the more preferred lower limit of the thickness of the pressure-sensitive adhesive layer is 10 μm, the even more preferred lower limit is 15 μm, the more preferred upper limit is 300 μm, the even more preferred upper limit is 250 μm, and the even more preferred upper limit is 200 μm.

[0045] The adhesive tape of the present invention may be a support type having a substrate, or may be a non-support type having no substrate. When the adhesive tape of the present invention is a support type having a substrate, the substrate is not particularly limited, but is preferably a substrate having heat resistance. Examples of such heat-resistant substrates include polyethylene terephthalate, polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyphenylene ether, polybutylene terephthalate, ultra-high molecular weight polyethylene, syndiotactic polystyrene, polyarylate, polysulfone, polyether sulfone, polyphenylene sulfide, polyether ether ketone, polyimide, polyetherimide, fluororesin, liquid crystal polymer, etc. Among them, polyethylene naphthalate is preferred because of its excellent heat resistance.

[0046] The bending stiffness of the above substrate in the TD direction at 23°C is 2.38×10 -7 N m 2 That's it, 2.98 x 10 -5 N m 2 It is preferable that: When the bending rigidity in the TD direction of the substrate at 23° C. is within the above range, the adhesive tape can more reliably protect the adherend and has excellent handleability. The bending rigidity in the TD direction of the substrate at 23° C. is 4.12×10 -7 N m 2 More preferably, it is 9.76×10 or more. -7 N m 2 More preferably, it is 2.03×10 or more. -5 N m 2 More preferably, it is 1.53×10 -5 N m 2 It is more preferable that the following is satisfied: Here, the TD (Transverse Direction) direction refers to a direction perpendicular to the extrusion direction when the substrate is extruded into a sheet. The bending stiffness is expressed by the product of the tensile modulus E and the second moment of area I. The tensile modulus can be measured using a viscoelasticity spectrometer (e.g., DVA-200, manufactured by IT Measurement and Control Co., Ltd.) under the conditions of a constant temperature rise tensile mode, a temperature rise rate of 10°C / min, and a frequency of 10 Hz. The second moment of area I is expressed by the following formula. I = (thickness of tape substrate) 3 / 12(m 2 )

[0047] The thickness of the substrate is not particularly limited, but the preferred lower limit is 5 μm, and the preferred upper limit is 200 μm. When the thickness of the substrate is within this range, the adhesive tape has a suitable stiffness and is easy to handle. The more preferred lower limit of the thickness of the substrate is 10 μm, and the more preferred upper limit is 150 μm.

[0048] The method for producing the pressure-sensitive adhesive tape of the present invention is not particularly limited, and a conventionally known method can be used. For example, the pressure-sensitive adhesive tape can be produced by applying a pressure-sensitive adhesive solution, which is prepared by mixing the pressure-sensitive adhesive, the silicone compound, and, if necessary, additives such as a crosslinking agent in a solvent, onto a film that has been subjected to a release treatment, drying the solution to form a pressure-sensitive adhesive layer, and laminating the resulting layer to a substrate.

[0049] In the manufacture of the pressure-sensitive adhesive tape of the present invention, the above A / B can be easily satisfied by adjusting the stirring speed when preparing the pressure-sensitive adhesive solution, the amount of heat when drying the pressure-sensitive adhesive layer, and the curing conditions after the pressure-sensitive adhesive tape is made. For example, by increasing the stirring speed, the silicone compound in the pressure-sensitive adhesive layer is more uniformly dispersed, and the value of A / B can be reduced. On the other hand, by decreasing the stirring speed, the silicone compound is less likely to be dispersed, and the value of A / B can be increased. By increasing the amount of heat, the silicone compound in the pressure-sensitive adhesive layer is less likely to bleed, and the value of A / B can be reduced. On the other hand, by decreasing the amount of heat, the bleeding of the silicone compound is promoted, and the value of A / B can be increased. By setting the curing conditions to a high temperature and a long period of time, the bleeding of the silicone compound in the pressure-sensitive adhesive layer is promoted, and the value of A / B can be increased. On the other hand, by setting the curing conditions to a low temperature and a short period of time, the silicone compound is less likely to bleed, and the value of A / B can be reduced. By combining these conditions, the above A / B can be adjusted.

[0050] The pressure-sensitive adhesive tape of the present invention is excellent in adhesion and easy peeling property, and therefore can be advantageously used for temporarily fixing electronic components. In particular, it can be advantageously used as a pressure-sensitive adhesive tape for temporarily fixing components when manufacturing semiconductors (temporary fixing pressure-sensitive adhesive tape for semiconductor manufacturing), and specifically, it can be suitably used as a protective tape for protecting a semiconductor package when dicing, sputtering, and pick-up are performed as a series of steps in the manufacture of a semiconductor package. Effect of the Invention

[0051] According to the present invention, it is possible to provide a pressure-sensitive adhesive tape that combines sufficient adhesion to secure an adherend with easy releasability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0053] (Preparation of the main polymer) A reactor equipped with a thermometer, a stirrer, and a cooling tube was prepared, and 94 parts by weight of 2-ethylhexyl acrylate, 1 part by weight of acrylic acid, 5 parts by weight of 2-hydroxyethyl acrylate, 0.01 parts by weight of lauryl mercaptan, and 180 parts by weight of ethyl acetate were added to the reactor, and the reactor was heated to start reflux. Subsequently, 0.01 parts by weight of 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane was added as a polymerization initiator to start polymerization under reflux. Next, 0.01 parts by weight of 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane was added one hour and two hours after the start of polymerization, and further 0.05 parts by weight of t-hexylperoxypivalate was added four hours after the start of polymerization to continue the polymerization reaction. Then, 8 hours after the start of polymerization, an ethyl acetate solution of a functional group-containing (meth)acrylic polymer having a solid content of 55% by weight and a weight average molecular weight of 600,000 was obtained. To 100 parts by weight of the resin solids content of the obtained ethyl acetate solution containing the functional group-containing (meth)acrylic polymer, 3.5 parts by weight of 2-isocyanatoethyl methacrylate as a functional group-containing unsaturated compound was added and reacted to obtain an ethyl acetate solution of the main polymer, which is the adhesive that constitutes the adhesive layer.

[0054] Example 1 To 100 parts by weight of the solid content of the obtained ethyl acetate solution of the main polymer, 1 part by weight of a silicone compound, 3 parts by weight of a filler, 10 parts by weight of a urethane acrylate, 0.2 parts by weight of a crosslinking agent, and 1 part by weight of a photopolymerization initiator were added, and mixed for 5 minutes at a stirring speed of 100 rpm to obtain an adhesive solution. Next, the adhesive solution was applied to the release-treated surface of a polyethylene terephthalate film whose surface had been subjected to a release treatment with a doctor knife so that the thickness of the dry film was 40 μm, and the adhesive layer was obtained by heating and drying at 105 ° C for 5 minutes. The obtained adhesive layer was bonded to the corona-treated surface of a substrate a whose one side had been subjected to a corona treatment, and cured at 40 ° C for 6 days to obtain an adhesive tape. The substrate a, silicone compound, filler, urethane acrylate, crosslinking agent, and photopolymerization initiator used were as follows. Substrate a: Polyethylene naphthalate, Q83-50, manufactured by Teijin Ltd., thickness 50 μm, bending stiffness in TD direction at 23 °C 1.91 × 10 -6 N m 2 Silicone compound: Silicone diacrylate, EBECRYL 350, Daicel-Allnex, weight average molecular weight 1000 Filler: Silica filler, Leolosil MT-10, manufactured by Tokuyama Corporation Urethane acrylate: UN-5500, manufactured by Negami Chemical Industries, Ltd. Crosslinking agent: Isocyanate-based crosslinking agent, Coronate L, manufactured by Nippon Urethane Industry Co., Ltd. Photopolymerization initiator: Irgacure 369, manufactured by BASF

[0055] (Examples 2 to 19, Comparative Examples 1 to 3) An adhesive tape was obtained in the same manner as in Example 1, except that the amount of release agent, the stirring speed during preparation of the adhesive solution, the amount of heat during formation of the adhesive layer, and the curing conditions were as shown in Tables 1 and 2. However, in Example 4, the content of the crosslinking agent was changed compared to Example 3, and the gel fraction was adjusted. Specifically, the following substrates b and c were used. In Example 2, no substrate was used, and the adhesive layer was used as it was to form the adhesive tape. Substrate b: Polyethylene terephthalate, Lumirror #125-X6K7, Toray Industries, thickness 125 μm, bending stiffness in TD direction at 23 °C 2.98 × 10 -5 N m 2 Substrate c: Polyethylene naphthalate, Q83-25, manufactured by Teijin Ltd., thickness 25 μm, bending stiffness in TD direction at 23 °C 1.22 × 10 -7 N m 2

[0056] <Physical Properties> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were subjected to the following measurements. The results are shown in Tables 1 and 2.

[0057] (Measurement of gel fraction of adhesive layer) 0.1 g of the adhesive layer of the obtained adhesive tape was scraped off and immersed in 50 ml of ethyl acetate, and shaken in a shaker at 23°C and 120 rpm for 24 hours (hereinafter, the scraped non-adhesive layer is referred to as the adhesive composition). After shaking, ethyl acetate and the adhesive composition that had absorbed and swollen with ethyl acetate were separated using a metal mesh (opening #200 mesh). The separated adhesive composition was dried at 110°C for 1 hour. The weight of the adhesive composition including the dried metal mesh was measured, and the gel fraction of the adhesive layer was calculated using the following formula. Gel fraction (wt%) = 100 × (W1-W2) / W0 (W0: initial weight of adhesive composition, W1: weight of adhesive composition including metal mesh after drying, W2: initial weight of metal mesh)

[0058] (A / B measurement) The adhesive layer surface of the obtained adhesive tape was irradiated with 405 nm ultraviolet light using a high-pressure mercury ultraviolet irradiator at an irradiation dose of 2500 mJ / cm 2 After that, the adhesive layer surface was irradiated with Bi3 ++ TOF-SIMS measurements were performed using an ion gun as the primary ion source for measurement. From the measurement results obtained, the Si ion intensity ratio (Si ion intensity / total ion intensity) was obtained based on the peak with mass number 28 derived from the silicone compound. Next, ion sputtering was performed once on the surface portion of the adhesive layer where the Si ion intensity ratio 0 was measured, using argon cluster ions (voltage: 5 KV, 5 nA) as a sputtering source (secondary ion source), and a Si ion intensity ratio of 1 was obtained using TOF-SIMS in the same manner as for the above-mentioned Si ion intensity ratio 0. Thereafter, sputtering and TOF-SIMS measurement were repeated to obtain Si ion intensity ratios of 0 to 25. From the obtained Si ion intensity ratios of 0 to 25, the average value (A) of the Si ion intensity ratios of 1 to 5 and the average value (B) of the Si ion intensity ratios of 20 to 25 were calculated, and A / B was calculated based on this. The TOF-SIMS measurement conditions and sputtering conditions are as follows.

[0059] (TOF-SIMS measurement conditions) Equipment: PHI nanoTOFII, manufactured by ULVAC-PHI Primary ion: 30KV, Bi3 ++ , 0.5μA (current value) Primary ion scan range (measurement area): 200 μm x 200 μm Secondary ion detection mode: negative Number of scans: 3 scans / time Charge compensation: E-Neut+I-Neut

[0060] (Sputtering conditions) Sputter ions: Argon cluster ions (5KV, 5nA) Sputtering time: 10s / time Sputtering area: 800μm×800μm

[0061] <Evaluation> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Tables 1 and 2.

[0062] (Semiconductor package manufacturing) The obtained adhesive tape was attached to a semiconductor package of 70 × 150 mm that had already been sealed with a mold resin. Next, a high-pressure mercury ultraviolet irradiator was used to irradiate the adhesive layer surface with 405 nm ultraviolet light at a dose of 2500 mJ / cm. 2 The adhesive layer was cross-linked and cured by irradiating the semiconductor package so that the adhesive layer was 15 mm x 8 mm. The adhesive tape and package were then diced to a size of 15 x 8 mm. The semiconductor package was then sputtered under normal sputtering conditions to form a Cu film. The semiconductor package was then peeled off from the adhesive layer by needle pick-up.

[0063] (Evaluation of dicing ability) In the manufacturing of the above semiconductor packages, 50 semiconductor packages were randomly selected after dicing. The selected semiconductor packages were observed under an optical microscope to check for peeling at the edges, and dicing peeling was evaluated according to the following criteria. S: Of the 50 samples, none were peeled off by 300 μm or more. A: Of the 50 samples, the number of samples that peeled off by 300 μm or more was less than 5%. B: Of the 50 samples, the number of samples that peeled off by 300 μm or more was 5% or more but less than 10%. C: Of the 50 samples, the number of samples that peeled off by 300 μm or more was 10% or more.

[0064] (Evaluation of pick-up ability) Of 100 semiconductor packages obtained in the above-mentioned semiconductor package production, the number of semiconductor packages in which pick-up failure occurred was counted, and the pick-up property was evaluated according to the following criteria. S: None of the packages had pickup problems A: There are 1-2 packages with pickup failure. B: 3 to 10 packages have failed pickup C: There are 11 to 30 packages with pickup failures. D: 31 or more packages have pickup failures

[0065] (Evaluation of staining properties) In the manufacture of the above semiconductor package, the semiconductor package was observed after needle pick-up, and the contamination was evaluated according to the following criteria. S: No tape residue was found on the semiconductor package. A: Residue from tape can be seen on semiconductor packages (less than 1% of the total) when observed with a microscope, etc. B: Residue from tape is visible on some semiconductor packages (less than 1% of the total). C: Residue from tape is visible on 1% to less than 90% of semiconductor packages. D: 90% or more of the semiconductor packages were visually inspected for tape residue.

[0066] [Table 1]

[0067] [Table 2] [Industrial Applicability]

[0068] According to the present invention, it is possible to provide a pressure-sensitive adhesive tape that combines sufficient adhesion to secure an adherend with easy releasability.

Claims

1. A pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer containing a pressure-sensitive adhesive, a silicone compound which is a release agent having a functional group capable of crosslinking with the pressure-sensitive adhesive, a crosslinking agent, and an inorganic filler, The pressure-sensitive adhesive is an acrylic curable pressure-sensitive adhesive, The pressure-sensitive adhesive contains a polymerizable polymer and a urethane acrylate, The polymerizable polymer has a radically polymerizable unsaturated bond, The silicone compound has a functional group having an unsaturated double bond at a side chain or end of a silicone skeleton, The content of the silicone compound is 1 part by weight or more and 40 parts by weight or less relative to 100 parts by weight of the adhesive, The content of the crosslinking agent is 0.1 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight of the adhesive, The content of the inorganic filler is 1 part by weight or more and 20 parts by weight or less relative to 100 parts by weight of the adhesive, The surface of the pressure-sensitive adhesive layer was irradiated with 405 nm ultraviolet light at an irradiation dose of 2500 mJ / cm 2 After irradiating the adhesive layer so as to obtain a Si ion intensity ratio (Si ion intensity / total ion intensity) on the surface of the adhesive layer, the Si ion intensity ratio is measured using a TOF-SIMS. Next, the surface portion of the adhesive layer where the Si ion intensity ratio 0 was measured was subjected to sputtering once under the sputtering conditions of using argon cluster ions (5 kV, 5 nA) as sputter ions, a sputtering time of 10 s, and a sputtering area of ​​800 μm × 800 μm, and then the Si ion intensity ratio of 1 was measured using TOF-SIMS; Next, the sputtering and measurement process is performed n times to obtain Si ion intensity ratios of 0 to n. An adhesive tape, wherein a ratio (A / B) of an average value (A) of Si ion intensity ratios of 1 to 5 to an average value (B) of Si ion intensity ratios of 20 to 25 is 1.1 or more and 3.0 or less.

2. 2. The pressure-sensitive adhesive tape according to claim 1, wherein the average value of the Si ion intensity ratios 1 to 5 is 0.001 or more and 0.03 or less.

3. The substrate has a bending stiffness in the TD direction at 23° C. of 2.38×10 -7 N.m 2 That's it, 2.98 x 10 -5 N.m 2 3. The adhesive tape according to claim 1 or 2, wherein:

4. The pressure-sensitive adhesive tape according to claim 1 , wherein the pressure-sensitive adhesive layer has a gel fraction of 44% or more and 67% or less.

5. 5. The pressure-sensitive adhesive tape according to claim 1, which is used for producing a semiconductor.

Citation Information

Patent Citations

  • Adhesive tape

    JP2008189857A

  • Dicing tape

    JP2015149398A

  • Adhesive tape roll

    JP2017179370A

  • Method for manufacturing semiconductor chip and adhesive tape

    JP2018147987A

  • Adhesive tape roll and optical film laminate

    JP2019059931A