Grain-oriented electrical steel sheet and its manufacturing method

By employing (Nb, Ti)CN precipitates as the primary inhibitor, the method stabilizes secondary recrystallization in grain-oriented electrical steel sheets, enhancing magnetic properties and reducing iron loss.

JP7569380B2Active Publication Date: 2024-10-17CLEANSOLUTION CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022538196
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-20
Filing Date
2020-12-09
Publication Date
2024-10-17
Estimated Expiration
2040-12-09

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheets face challenges in achieving optimal magnetic properties due to the use of traditional grain growth inhibitors like Al-based nitrides and Mn-based sulfides, which require high temperatures, lead to fine grain sizes, and result in increased core loss and reduced magnetic flux density.

Method used

The use of (Nb, Ti)CN precipitates as the primary grain growth inhibitor, controlled through specific elemental compositions and annealing processes, stabilizes secondary recrystallization and enhances magnetic properties.

Benefits of technology

The method produces grain-oriented electrical steel sheets with improved magnetic flux density and reduced iron loss by effectively suppressing abnormal grain growth, ensuring stable secondary recrystallization and optimal grain sizes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569380000001
    Figure 0007569380000001
Patent Text Reader

Abstract

An object of the present invention is to provide a grain-oriented electrical steel sheet with excellent magnetic properties, which uses (Nb, Ti)CN precipitates as a main inhibitor by appropriately adding Ti and Nb, and a method for producing the same. [Solution] The method for producing grain-oriented electrical steel sheet of the present invention is characterized by comprising the steps of hot-rolling a slab containing, by weight, 2.0-6.0% Si, 0.04-0.12% Mn, 0.001-0.022%, 0.027-0.060% C, 0.01-0.08% Nb, and 0.01% or less Ti, with the remainder being Fe and other unavoidable impurities, to produce a hot-rolled sheet, cold-rolling the hot-rolled sheet to produce a cold-rolled sheet, subjecting the cold-rolled sheet to primary recrystallization annealing, and subjecting the cold-rolled sheet after primary recrystallization annealing to secondary recrystallization annealing.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grain-oriented electrical steel sheet and a manufacturing method thereof, and more particularly to a grain-oriented electrical steel sheet having excellent magnetic properties and using (Nb, Ti)CN precipitates as a main inhibitor by appropriately adding Ti and Nb, and a manufacturing method thereof. [Background technology]

[0002] Grain-oriented electrical steel sheets have a texture in the rolling direction of {110} <001> It shows a Goss texture and is a soft magnetic material with excellent magnetic properties in one direction or the rolling direction. In order to develop such a texture, grain growth must occur only in the grains with the Goss texture, and normal grain growth of grains with other textures must be suppressed as much as possible. The phenomenon in which grain growth occurs only in specific grains as mentioned above is called abnormal grain growth or secondary recrystallization. For secondary recrystallization of grains with a Goss texture, a grain growth inhibitor such as a precipitate or segregation element that suppresses the growth of other grains is required.

[0003] The techniques for improving the magnetic properties of grain-oriented electrical steel sheets can be broadly divided into two categories: making more crystal grains in the Goss orientation, and obtaining a secondary recrystallized structure consisting of highly integrated crystal grains in the Goss orientation by improving the grain growth inhibition. The precipitates used for the latter grain growth inhibition are mainly Al-based nitrides, Mn-based sulfides, or MnSe. However, in order to utilize precipitates such as Al-based nitrides, Mn-based sulfides, or MnSe as grain growth inhibitors, finely dispersed precipitation of the precipitates is essential after hot rolling, so the steel slab must be maintained at high temperatures for a long time. However, this causes problems such as the melting of low-melting-point fayalite (Fe2SiO4, fayalite) present in the scale layer of the steel slab, shortening the life of the heating furnace and requiring long and expensive maintenance and repair work. In addition, since the precipitates formed after redissolution at high temperatures are very fine, there is a problem that the grain growth inhibition power is strong, resulting in fine primary recrystallization grains. In order to grow the grains to an appropriate size, a high primary recrystallization annealing temperature is required, and the surface quality of the final product is often deteriorated due to high-temperature oxidation.

[0004] In addition to these precipitates, it has been proposed to add B and Ti to utilize precipitates such as BN and TiN, but since B is added in very small amounts, it is very difficult to control at the steelmaking stage, and since it is prone to forming coarse BN in the steel after addition, there is a problem that the ability to inhibit the growth of crystal grains is weakened. In addition, since Ti is prone to forming TIN or TiC, it remains in the steel sheet even after high-temperature annealing and hinders magnetic domain movement, which can actually increase iron loss and act as a factor in reducing magnetic flux density. Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to provide a grain-oriented electrical steel sheet and a manufacturing method thereof. More specifically, the object of the present invention is to provide a grain-oriented electrical steel sheet with excellent magnetic properties and a manufacturing method thereof, which uses (Nb, Ti)CN precipitates as a main inhibitor by appropriately adding Ti and Nb. [Means for solving the problem]

[0006] A method for producing grain-oriented electrical steel sheet of the present invention includes the steps of hot rolling a slab containing, by weight, 2.0-6.0% Si, 0.04-0.12% Mn, 0.001-0.022% N, 0.027-0.060% C, 0.01-0.08% Nb, 0.01% or less Ti, with the balance being Fe and other unavoidable impurities, to produce a hot-rolled sheet, cold rolling the hot-rolled sheet to produce a cold-rolled sheet, primary recrystallization annealing the cold-rolled sheet, and secondary recrystallization annealing the cold-rolled sheet that has been primarily recrystallized annealed. The cold-rolled sheet that has been subjected to the primary recrystallization annealing contains N in an amount of 0.0010 to 0.0220 wt %.

[0007] The slab may further contain one or more of S: 0.008% or less, P: 0.005% to 0.04%, Sn: 0.01% to 0.07%, Sb: 0.005% to 0.05%, Cr: 0.01 to 0.2%, and acid-soluble Al: 0.04% or less.

[0008] The slab may further contain acid-soluble Al: 0.020% or less.

[0009] The cold-rolled sheet that has been subjected to the primary recrystallization annealing can satisfy the following formula 1. [Formula 1] 3.0≦([Nb]+5×[Ti]) / (10×[N]) 2 <= 100.0 (In formula 1, [Nb], [Ti] and [N] represent the contents (wt%) of Nb, Ti and N in the cold-rolled sheet that has been subjected to the primary recrystallization annealing.)

[0010] The cold-rolled sheet that has been subjected to the primary recrystallization annealing may have precipitates with an average grain size of 30 nm or less.

[0011] The precipitates may include Nb, Ti, or complex carbonitrides thereof.

[0012] The grain-oriented electrical steel sheet of the present invention contains, by weight, 2.0-6.0% Si, 0.04-0.12% Mn, 0.0001-0.006%, 0.005% by weight or less (excluding 0%) C, 0.01-0.08% Nb, and 0.01% or less Ti, with the remainder being Fe and other unavoidable impurities.

[0013] The grain-oriented electrical steel sheet of the present invention may contain precipitates, and the precipitates may have an average grain size of 30 nm or less. The precipitates may contain Ti, Nb or a combination of both. Effect of the Invention

[0014] The method for producing grain-oriented electrical steel sheet of the present invention uses (Nb,Ti)CN precipitates as a main inhibitor to stably induce secondary recrystallization of crystal grains having a Goss texture, thereby producing grain-oriented electrical steel sheet with excellent magnetic properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, the first part, component, region, layer or section described below may be referred to as the second part, component, region, layer or section without departing from the scope of the present invention.

[0016] The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The term "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.

[0017] When an element is referred to as being "on" another element, this means that it is directly on top of the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them.

[0018] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless defined.

[0019] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight.

[0020] In one embodiment of the present invention, the term "additionally containing an additional element" refers to the additional amount of the additional element substituting for the remaining iron (Fe).

[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0022] In the embodiment of the present invention, Al-based nitrides, Mn-based sulfides, or MnSe are not used as the main inhibitor of grain growth, but (Nb,Ti)CN is used as the main inhibitor to inhibit grain growth, thereby stably exhibiting secondary recrystallization of grains having a Goss texture and simultaneously producing a grain-oriented electrical steel sheet with excellent magnetic properties.

[0023] A method for producing grain-oriented electrical steel sheet according to one embodiment of the present invention includes the steps of hot rolling a slab containing, by weight, 2.0-6.0% Si, 0.04-0.12% Mn, 0.001-0.022% N, 0.027-0.060% C, 0.01-0.08% Nb, and 0.01% or less Ti, with the balance being Fe and other unavoidable impurities, to produce a hot-rolled sheet, cold rolling the hot-rolled sheet to produce a cold-rolled sheet, subjecting the cold-rolled sheet to primary recrystallization annealing, and subjecting the cold-rolled sheet after primary recrystallization annealing to secondary recrystallization annealing.

[0024] Each step will be explained in detail below. First, a slab is hot rolled to produce a hot-rolled sheet. The slab contains, by weight, 2.0-6.0% Si, 0.04-0.12% Mn, 0.001-0.022% N, 0.027-0.060% C, 0.01-0.08% Nb, and 0.01% or less Ti, with the remainder being Fe and other unavoidable impurities. The reasons for limiting the amount of each element added will be explained below.

[0025] Si:2.0~6.0wt% Silicon (Si) is a basic component of electrical steel sheets, and plays a role in increasing the resistivity of the material and reducing core loss. If the Si content is too low, the resistivity decreases and eddy current loss increases, the crystal grains of the hot-rolled sheet become excessively coarse, the precipitates are unevenly precipitated, and the secondary recrystallization becomes unstable, as well as the frequency of edge cracks and sheet breakage during rolling increases. On the other hand, if too much Si is added, the brittleness increases rapidly and the toughness decreases, similarly, edge cracks and sheet breakage during the rolling process become serious, the weldability between sheets is also poor, the C content required for controlling the γ phase fraction increases rapidly, decarburization becomes poor, and secondary recrystallization becomes unstable, causing serious damage to magnetism. Therefore, the Si content is 2.0 to 6.0 wt%. More specifically, it may be 2.0 to 4.5 wt%.

[0026] Mn:0.04~0.12wt% Manganese (Mn) has an effect similar to that of Si, that is, it increases resistivity and reduces eddy current loss, thereby reducing overall iron loss. In addition, Mn reacts with S in the raw steel state to form Mn-based sulfides, which are used as a grain growth inhibitor, and has the effect of homogenizing the microstructure of the hot-rolled sheet by inducing austenite phase transformation at a certain temperature or higher. In one embodiment of the present invention, the formation of Mn-based sulfides is minimized to maximize its use as an inhibitor. If Mn is contained in an excessively small amount, the microstructure of the hot-rolled sheet may be formed non-uniformly, secondary recrystallization may become unstable, and magnetic properties may deteriorate. If Mn is contained in an excessively large amount, the amount of Mn-based sulfides formed is large, which can act as an inhibitor. Therefore, Mn may be contained in an amount of 0.04 to 0.12 wt %. More specifically, Mn may be contained in an amount of 0.05 to 0.10 wt %.

[0027] N: 0.001 to 0.022% Nitrogen (N) is an important element that reacts with Si, Nb, Ti, and C to form Si3N4 and (Nb, Ti)CN. In one embodiment of the present invention, the slab does not need to contain a large amount of nitrogen because the nitrogen can be reinforced by the nitriding step. Therefore, the slab can contain 0.001 to 0.022 wt% of N. If the N content is too low, it may react with Si to form only Si3N4, and not form (Nb, Ti)CN. More specifically, the N content in the slab may be 0.0020 to 0.0100 wt %. More specifically, the N content in the slab may be 0.0030 to 0.0060 wt %. After the first recrystallization annealing described below, the steel may contain 0.0010 to 0.0220% by weight of N. If the steel contains too little N after the first recrystallization annealing, the desired (Nb, Ti)CN cannot be properly formed in one embodiment of the present invention. If the steel contains too much N after the first recrystallization annealing, the (Nb, Ti)CN becomes very coarse, and the precipitates remain even after the second recrystallization annealing, causing poor magnetic properties. Therefore, the steel may contain 0.0010 to 0.0220% by weight of nitrogen after the first recrystallization annealing. In particular, the steel may contain 0.0010 to 0.0150% by weight of N after the first recrystallization annealing. More particularly, the steel may contain 0.0030 to 0.0130% by weight of N after the first recrystallization annealing. Some of the N is removed during the secondary recrystallization annealing process, and the amount of N remaining in the final grain-oriented electrical steel sheet is 0.0001 to 0.006 wt %.

[0028] C:0.027~0.060wt% Carbon (C) is an important element that reacts with Si, Nb, Ti, and N to form SiC and (Nb, Ti)CN, and is also an austenite stabilizing element that has the effect of refining columnar crystals during the continuous casting process and coarse crystal grains in the hot-rolled sheet by causing an austenite phase transformation at 800°C or higher. If the slab contains too little C, it reacts preferentially with Si to form only SiC, and (Nb, Ti)CN may not be formed well. Conversely, if the slab contains too much C, not only will NbC and TiC, which have very high melting points, be strongly formed, and (Nb, Ti)CN will not be formed well, but NbC and TiC will remain even after secondary recrystallization annealing, deteriorating the magnetic property. Therefore, the slab may contain 0.027 to 0.060% by weight of C. More specifically, the slab may contain 0.035 to 0.055% by weight of C. Meanwhile, the C content remaining in the finally manufactured grain-oriented electrical steel sheet due to decarburization during the first recrystallization annealing and the second recrystallization annealing is 0.005 wt% or less. In detail, the C content remaining in the finally manufactured grain-oriented electrical steel sheet is 0.003 wt% or less.

[0029] Nb:0.01~0.08wt% Niobium (Nb) has been generally controlled at extremely low levels in the past because it forms high-melting carbides and nitrides that remain even after secondary recrystallization annealing and deteriorate the magnetic properties of the final grain-oriented electrical steel sheet. However, in one embodiment of the present invention, this is reversed and used as a grain growth inhibitor, so it can be said to be the core element of the present invention. That is, Nb is essential for reacting with C, N, and Ti during the steelmaking, continuous casting, and hot rolling stages to precipitate (Nb, Ti)CN, which is a powerful grain growth inhibitor. If Nb is contained in an excessively small amount, Nb(C, N), NbC, NbN, TiC, TiN, etc. are formed, making the secondary recrystallization unstable, and some of the above-mentioned precipitates remain inside the steel sheet even after secondary recrystallization annealing, deteriorating the magnetic properties. In addition, if Nb is contained in an excessively large amount, high-melting NbC and NbN are precipitated together with (Nb, Ti)CN, and remain even after secondary recrystallization annealing, ultimately deteriorating the magnetic properties. Therefore, the Nb content is 0.010 to 0.080% by weight. More specifically, the Nb content is 0.014 to 0.078% by weight.

[0030] Ti: 0.01% by weight or less Titanium (Ti), like Nb, generally forms high melting point carbides and nitrides, which remain even after secondary recrystallization annealing and deteriorate the magnetic properties of the final product, and thus has been conventionally controlled at extremely low levels. However, in one embodiment of the present invention, it must be added as an essential component to form (Nb, Ti)CN. If Ti is contained in an excessive amount, it will additionally form Ti-based carbides and nitrides, hindering the secondary recrystallization, and will ultimately remain in the product sheet and impair the magnetic properties. Therefore, Ti is contained at 0.01 wt% or less. If Ti is not contained at all in the steel, the reaction of forming (Nb, Ti)CN itself will be impossible, so 0wt% is excluded. More specifically, Ti can be contained at 0.0010 to 0.0100 wt%. More specifically, Ti can be contained at 0.0050 to 0.0080 wt%.

[0031] The cold-rolled sheet that has been subjected to the primary recrystallization annealing can satisfy the following formula 1.

[0032] [Formula 1] 3.0≦([Nb]+5×[Ti]) / (10×[N]) 2 <= 100.0 (In formula 1, [Nb], [Ti] and [N] represent the contents (wt%) of Nb, Ti and N in the cold-rolled sheet that has been subjected to the primary recrystallization annealing.)

[0033] In one embodiment of the present invention, in order to properly form (Nb, Ti)CN used as a main growth inhibitor, Nb, Ti, and N can be adjusted within the above-mentioned range. If the value of formula 1 is too small, it means that Nb and Ti are added in small amounts or N is added in excessive amounts, so that (Nb, Ti)CN is not formed sufficiently, the secondary recrystallization becomes unstable, and the magnetic property is poor. On the other hand, if the value of formula 1 is too large, it means that Nb and Ti are added in excessive amounts or N is added in excessively small amounts, so that (Nb, Ti)CN precipitates very coarsely, the grain growth inhibition power is weakened, the secondary recrystallization becomes unstable, or a large amount of NbC and TiC are formed instead of (Nb, Ti)CN, which remain even after secondary recrystallization annealing, and the magnetic property is poor. Specifically, the value of formula 1 may be 4.5 to 90.0.

[0034] The slab may further include one or more of S: 0.008% or less, P: 0.005% to 0.04%, Sn: 0.01% to 0.07%, Sb: 0.005% to 0.05%, Cr: 0.01 to 0.2%, and acid-soluble Al: 0.04% or less. More specifically, the slab may further include S: 0.008% or less, P: 0.005% to 0.04%, Sn: 0.01% to 0.07%, and Cr: 0.01 to 0.2%.

[0035] S: 0.008% by weight or less If sulfur (S) is contained in an excessive amount, a large amount of Mn-based sulfides are formed, which acts as a grain growth inhibitor, and may hinder the effect of (Nb, Ti)CN, which is used as the main grain growth inhibitor in one embodiment of the present invention. In addition, it may also destabilize secondary recrystallization and deteriorate magnetic properties. Therefore, when S is further contained, the content of S in the steel can be actively suppressed. Specifically, it can be contained in an amount of 0.0010 to 0.0070 wt%.

[0036] P:0.005%~0.040wt% Phosphorus (P) segregates at the grain boundaries, hindering the movement of the grain boundaries and at the same time playing an auxiliary role in suppressing the growth of grains. <001> Since it has the effect of improving the texture, it can be added additionally. If the P content is too low, the effect of addition may be insufficient. If the P content is too high, brittleness increases and rollability may be significantly deteriorated. Therefore, when P is further contained, it may be contained in an amount of 0.005 to 0.040 wt %. More specifically, it may be further contained in an amount of 0.010 to 0.030 wt %.

[0037] Sn:0.01%~0.07wt% Tin (Sn), like P, is a grain boundary segregating element that prevents the movement of grain boundaries, and therefore plays a role as a grain growth inhibitor, and can be further added. If too little Sn is added, the above-mentioned effects cannot be obtained sufficiently. Conversely, if too much Sn is added, the grain growth inhibitory power is too strong, making it difficult to obtain stable secondary recrystallization. Therefore, when Sn is further added, it can be contained in an amount of 0.01 to 0.07 wt %. More specifically, it can be further contained in an amount of 0.03 to 0.05 wt %.

[0038] Sb:0.005~0.05wt% Antimony (Sb), like P and Sn, is a grain boundary segregating element that prevents the movement of grain boundaries, and therefore plays a role as a grain growth inhibitor, and can be further added. If too little Sb is added, the above-mentioned effects cannot be sufficiently obtained. Conversely, if too much Sb is added, the grain growth inhibitory power is too strong, making it difficult to obtain stable secondary recrystallization. Therefore, if Sb is further added, it can be contained in an amount of 0.005 to 0.05 wt %. More specifically, it can be further contained in an amount of 0.01 to 0.04 wt %.

[0039] Cr:0.01~0.2wt% Chromium (Cr) is an effective element for forming a hard phase in a hot-rolled sheet, promoting the formation of a Goss texture during cold rolling, and promoting the formation of an oxide layer during decarburization annealing, and can be further added. If too little Cr is added, the above-mentioned effects cannot be sufficiently obtained. If too much Cr is added, the oxide layer is promoted to be formed very densely during the decarburization process, which may hinder the formation of the oxide layer and even hinder decarburization and nitridation. Therefore, when Cr is further added, it may be contained in an amount of 0.01 to 0.20 wt. %. More specifically, it may be further contained in an amount of 0.02 to 0.10 wt. %.

[0040] Acid-soluble Al: 0.04% by weight or less Aluminum (Al), like Si, is an element that has the effect of increasing resistivity and improving iron loss, and is also used as a grain growth inhibitor by forming an Al-based nitride, but is not an essential element in one embodiment of the present invention. However, it can be added additionally to improve iron loss and to play a supplementary role to (Nb, Ti)CN, which is a main grain growth inhibitor. If Al is added in an excessive amount, it combines with Al, Si, and Mn to form nitrides in the form of (Al, Si, Mn)N and AlN, thereby playing a role as a strong grain growth inhibitor, hindering the role of (Nb, Ti)CN, which is a main grain growth inhibitor, and causing the size of primary recrystallized grains to be formed too finely, thereby deteriorating magnetic properties. Therefore, when Al is further included, it may be included in an amount of 0.04 wt % or less. More specifically, it may be further included in an amount of 0.020 wt % or less. More specifically, it may be further included in an amount of 0.005 wt % or less. Acid-soluble Al means Al that dissolves in acid. Specifically, it means the total Al, excluding Al present in Al2O3, etc., which is insoluble in acid.

[0041] The balance is iron (Fe). The steel is also made of inevitable impurities. Inevitable impurities refer to impurities that are inevitably mixed in during the steelmaking and manufacturing process of grain-oriented electrical steel sheets. Since inevitable impurities are widely known, a detailed description of the inevitable impurities will be omitted. In one embodiment of the present invention, the addition of elements other than the above-mentioned alloy components is not excluded, and various elements are included within a range that does not impair the technical idea of ​​the present invention. When an additional element is further included, it is included in place of the balance Fe. For example, it is also possible to include at least one of Cu, Ni, Mo, Zr, Bi, Pb, As, Ge, and Ga in the steel within the composition range of the present invention.

[0042] Returning to the explanation of the manufacturing process, the slab can be heated before hot rolling. When the slab is heated, it is divided into a temperature at which the grain growth inhibitor is incompletely dissolved or a temperature at which the grain growth inhibitor is completely dissolved. However, in one embodiment of the present invention, since there is no problem in expressing the effect of (Nb, Ti)CN regardless of the degree of solution, there is no limit to the reheating temperature. Specifically, it can be heated to a temperature of 1100°C to 1300°C. Since low-melting-point fayalite present in the scale layer on the slab surface can melt down during slab heating and damage the furnace body, the slab can be heated at a temperature of 1300°C or less.

[0043] The slab is hot rolled to produce a hot rolled sheet. The hot rolling can be performed to a thickness of 1.0 to 5.0 mm. The hot-rolled steel sheet can be smoothly rolled to the final product thickness in the subsequent cold rolling process by recrystallizing the hot-rolled deformation structure in the subsequent hot-rolled sheet annealing process. In general, the hot-rolled sheet annealing temperature can be heated to a temperature of 950°C or more for recrystallization and maintained for a certain period of time. Next, the sheet is cooled to a temperature at which cold rolling can be performed, and any of air cooling, water cooling, oil cooling, and furnace cooling can be used for cooling. Prior to this, the appropriate time means the appropriate condition according to various variables such as the size and length of the furnace, heating capacity, and heat capacity. The hot-rolled sheet annealing can be omitted as necessary.

[0044] Next, the hot-rolled sheet is cold-rolled to produce a cold-rolled sheet. The hot-rolled sheet is pickled to remove the oxide layer on the surface of the steel sheet, and then cold-rolled. Cold rolling is a process to reduce the thickness of the steel sheet to the thickness of the final product, and is performed once or more than once including intermediate annealing to roll it to the thickness of the final product. The effect can be achieved even if cold rolling is performed at room temperature or when the sheet is naturally or artificially heated. After cold rolling, the final thickness is 0.10mm~0.50mm.

[0045] Next, the cold-rolled sheet is subjected to primary recrystallization annealing. The cold-rolled sheet is subjected to decarburization annealing including recrystallization of the deformed cold-rolled structure in a mixed gas atmosphere containing nitrogen, hydrogen, and moisture. If necessary, a nitriding treatment may be performed to introduce nitrogen ions into the steel sheet using ammonia gas. Nitriding may be performed simultaneously with decarburization annealing or after decarburization annealing without any functional problems.

[0046] According to an embodiment of the present invention, if only the N content in the steel sheet after the primary recrystallization annealing can be controlled, (Nb, Ti)CN, which is a main grain growth inhibitor, can be sufficiently formed even without performing a nitriding treatment during the primary recrystallization annealing process. However, when the nitriding treatment is performed, (Nb, Ti)CN is additionally formed to strengthen the grain growth inhibitory power and to improve the integration degree of the secondary recrystallized Goss orientation grains, thereby further improving the magnetic properties.

[0047] For the nitriding treatment, the first recrystallization annealing can be performed in an atmosphere containing ammonia gas. The first recrystallization annealing temperature can be in the range of 750°C to 900°C. If the temperature is too low, the ammonia gas is not decomposed, so that the nitrogen ions are not introduced into the steel sheet and are discharged to the outside of the annealing furnace. On the other hand, if the temperature is too high, the nitrogen ions are decomposed in advance before being introduced into the steel sheet, which may cause a problem of reduced nitriding efficiency. The annealing time of the first recrystallization annealing does not matter much in terms of achieving the effects of the present invention, but it is usually preferable to perform the treatment within 5 minutes in consideration of productivity.

[0048] The steel sheet after the primary recrystallization annealing may have an average grain size of precipitates of 30 nm or less. Secondary recrystallization occurs stably only when the average grain size of precipitates is smaller than 30 nm, and if it is larger than 30 nm, secondary recrystallization does not occur well and the magnetic properties after secondary recrystallization annealing are inferior. More specifically, it may be 5 to 27 nm. More specifically, it may be 10 to 25 nm.

[0049] In one embodiment of the present invention, the precipitates may include (Nb, Ti)CN, which is used as a main grain growth inhibitor. In other words, the precipitates may include Nb, Ti, or composite carbonitrides thereof. In addition, the precipitates may include carbides of Nb and Ti, MnS, AlN, etc., which inevitably form precipitates. In order to form precipitates with an appropriate grain size, the contents of Ti and Nb and the content of N after the first recrystallization annealing are important. More specifically, formula 1 can be satisfied. The contents of Ti and Nb and the content of N after the first recrystallization annealing have been described above, so a duplicated description will be omitted.

[0050] Next, the cold-rolled sheet that has been subjected to the primary recrystallization annealing is subjected to secondary recrystallization annealing. Cold-rolled sheets that have undergone primary recrystallization annealing are coated with an MgO-based annealing separator, then heated to over 1000°C for a long period of time to cause crack annealing, resulting in secondary recrystallization, with the {110} plane of the steel sheet parallel to the rolling surface, <001> The Goss-oriented texture is formed with its direction parallel to the rolling direction.

[0051] During the secondary recrystallization annealing, the (Nb, Ti)CN precipitates are decomposed as C and N are removed, and Nb and Ti partially diffuse into the base coating layer or remain inside the matrix. Therefore, the number of precipitates after the secondary recrystallization annealing is greatly reduced compared to the number of precipitates after the primary recrystallization annealing. However, the Nb and Ti remaining inside the matrix diffuse into other (Nb, Ti)CN that are not decomposed during the high-temperature annealing and remain, coarsening the grain size of this (Nb, Ti)CN, so in the case of precipitates that remain after the secondary recrystallization, the grain size does not change significantly from that after the primary recrystallization annealing. That is, the average grain size of the precipitates after the secondary recrystallization annealing may be 30 nm or less, more specifically, 5 to 27 nm, and even more specifically, 10 to 25 nm.

[0052] The remaining precipitates may contain Nb, Ti, or a combination of these. The precipitates after the secondary recrystallization annealing may remain in the form of carbides or nitrides due to the removal of C and N from carbonitrides. They may also remain in the form of carbonitrides.

[0053] A grain-oriented electrical steel sheet according to one embodiment of the present invention contains, by weight, 2.0-6.0% Si, 0.04-0.12% Mn, 0.0001-0.006% N, 0.005% by weight or less (excluding 0%) C, 0.01-0.08% Nb, and 0.01% or less Ti, with the remainder being Fe and other unavoidable impurities.

[0054] The grain-oriented electrical steel sheet according to an embodiment of the present invention may contain precipitates, and the precipitates may have an average grain size of 30 nm or less, more specifically, 5 to 27 nm. The precipitates may contain Ti, Nb, or a combination of these elements, and more specifically, may contain carbides, nitrides, or carbonitrides containing Ti, Nb, or a combination of these elements.

[0055] The grain-oriented electrical steel sheet according to an embodiment of the present invention is particularly excellent in core loss and magnetic flux density properties. The grain-oriented electrical steel sheet according to an embodiment of the present invention has a magnetic flux density (B8) of 1.88 T or more and a core loss (W 17 / 50 ) may be 1.05 W / kg or less. In this case, the magnetic flux density B8 is the magnitude (Tesla) of the magnetic flux density induced under a magnetic field of 800 A / m, and the iron loss W 17 / 50 is the magnitude of iron loss (W / kg) induced at 1.7 Tesla and 50 Hz.

[0056] Hereinafter, specific examples of the present invention will be described. However, the following examples are merely specific examples of the present invention, and the present invention is not limited to the following examples. EXAMPLES

[0057] The basic composition was Si: 3.28%, C: 0.051%, S: 0.006%, N: 0.003%, Sn: 0.044%, P: 0.028%, Cr: 0.02%, Mn: 0.08%, and Al: 0.012% by weight. The contents of Nb and Ti were changed as shown in Table 1, and the remaining components were Fe and other unavoidably contained impurities. The slabs were heated to a temperature of 1210°C and then hot-rolled to a thickness of 3.0 mm. The hot-rolled sheets were heated to a temperature of 1000°C, maintained at that temperature for 130 seconds, water-cooled and pickled, and then rolled once to a thickness of 0.30 mm. The cold-rolled sheets were maintained at a temperature of 820°C for 150 seconds in a mixed gas atmosphere of wet hydrogen, nitrogen, and ammonia, and were subjected to decarburization annealing including primary recrystallization annealing and nitriding treatment so that the nitrogen content was changed as shown in Table 1. The steel sheet was coated with MgO as an annealing separator and then subjected to secondary recrystallization annealing, which was performed in a mixed atmosphere of 25% nitrogen and 75% hydrogen by volume up to 1180℃, and after reaching 1180℃, it was maintained in a 100% hydrogen atmosphere for about 4 hours and then furnace cooled. The average size of the precipitates was measured by making replica specimens for the specimens that had completed the primary recrystallization annealing and performing image analysis on the photographs taken by TEM.

[0058] As mentioned above, Table 1 shows the Nb, Ti and nitrogen contents of the steel sheets after the second recrystallization annealing, the average size of (Nb, Ti)CN precipitates and the magnetic properties measured after the second recrystallization annealing.

[0059] [Table 1]

[0060] As shown in Table 1, it can be confirmed that when the Nb, Ti and N after the first recrystallization annealing are appropriately contained, the magnetic flux density and core loss are excellent. On the other hand, it can be confirmed that Comparative Material 1 contains an excessively small amount of Nb, does not satisfy formula 1, forms coarse precipitates, and is inferior in magnetic flux density and core loss. It can be seen that comparative material 2 contains an excessively large amount of Ti, does not satisfy formula 1, forms coarse precipitates, and is inferior in magnetic flux density and core loss. It can be seen that the comparative material 3 does not satisfy formula 1, the precipitates are formed coarsely, and the magnetic flux density and core loss are poor. It can be seen that comparative materials 4 to 6 contain too little Nb and too much Ti, do not satisfy formula 1, form coarse precipitates, and are inferior in magnetic flux density and core loss. It can be seen that comparative material 7 contains an excessively large amount of Ti, does not satisfy formula 1, forms coarse precipitates, and is inferior in magnetic flux density and core loss.

[0061] The present invention is not limited to the above-described embodiments and / or examples, and can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-described embodiments and / or examples are illustrative in all respects and not limiting.

Claims

1. A step of producing a hot-rolled sheet by hot rolling a slab containing, by weight percent, 2.0 to 6.0% Si, 0.04 to 0.12% Mn, 0.001 to 0.022% N, 0.027 to 0.060% C, 0.01 to 0.08% Nb, and 0.0010 to 0.01% Ti, with the balance being Fe and other unavoidable impurities; cold rolling the hot rolled sheet to produce a cold rolled sheet; subjecting the cold-rolled sheet to a primary recrystallization annealing; The cold-rolled sheet that has been subjected to the first recrystallization annealing is subjected to a second recrystallization annealing, The cold-rolled sheet subjected to the first recrystallization annealing contains 0.0010 to 0.0220 wt % of N, The cold-rolled sheet subjected to the first recrystallization annealing satisfies the following formula 1: The produced grain-oriented electrical steel sheet contains precipitates, the precipitates having an average grain size of 30 nm or less, The method for producing a grain-oriented electrical steel sheet, wherein the precipitates contain complex carbonitrides of Nb and Ti. [Formula 1] 3.0≦([Nb]+5×[Ti]) / (10×[N]) 2 ≦100.0 (In formula 1, [Nb], [Ti] and [N] represent the contents (wt%) of Nb, Ti and N in the cold-rolled sheet subjected to primary recrystallization annealing.)

2. 2. The method for producing a grain-oriented electrical steel sheet according to claim 1, wherein the slab further contains, by weight percent, one or more of S: 0.008% or less, P: 0.005% to 0.04%, Sn: 0.01% to 0.07%, Sb: 0.005% to 0.05%, Cr: 0.01 to 0.2%, and acid-soluble Al: 0.04% or less.

3. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, wherein the slab further contains, by weight percent, acid-soluble Al: 0.020% or less.

4. The composition contains, by weight, Si: 2.0-6.0%, Mn: 0.04-0.12%, N: 0.0001-0.006%, C: 0.005 wt% or less (excluding 0%), Nb: 0.01-0.08%, and Ti: 0.0010-0.01%, with the balance being Fe and other inevitable impurities; The precipitates have an average particle size of 30 nm or less, The grain-oriented electrical steel sheet, wherein the precipitates contain complex carbonitrides of Ti and Nb.

Citation Information

Patent Citations

  • Material of high magnetic flux density one directionally orientated el ectromagnetic steel and its treating method

    JP1977024116A

  • Grain-oriented electrical steel sheet and manufacturing method thereof

    JP2018505962A

  • Grain-oriented electrical steel sheets having excellent magnetic properties and method for manufacturing the same

    KR1020130014891A