Achieving electromagnetic interference shielding protection through deposition of highly conductive compositions
Highly conductive compositions applied via electrostatic or ultrasonic spraying achieve uniform, thin coatings on electronic packages, addressing EMI shielding inefficiencies and cost issues in existing technologies.
Patent Information
- Application Number
- JP2018505734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-08-03
- Filing Date
- 2016-07-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2036-07-29
AI Technical Summary
Existing methods for electromagnetic interference (EMI) shielding in electronic packages face challenges with non-uniform three-dimensional thin coatings, low conductivity, and inefficient shielding performance, particularly in small designs, leading to suboptimal protection and high production costs.
Development of highly conductive compositions applied using electrostatic spraying, air spraying, or ultrasonic spraying to create a uniform three-dimensional thin conductive coating on electronic packages, achieving effective EMI shielding with thicknesses as low as 1-2 μm and high conductivity.
The solution provides superior EMI shielding performance, high conductivity, and uniform coatings at very thin thicknesses, enhancing protection and reducing production time and costs compared to traditional methods.
Smart Images

Figure 0007569615000016 
Figure 0007569615000017 
Figure 0007569615000018
Abstract
Description
[Technical field]
[0001] Related Applications This application claims priority to U.S. Provisional Patent Application No. 62 / 200,267, filed Aug. 3, 2015, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a highly conductive composition and a method for its uniform three-dimensional application to a suitable substrate (e.g., on an epoxy molding compound (EMC) surface) using suitable means, such as electrostatic spraying, air spraying, ultrasonic spraying, spin-coating, etc. Highly efficient electromagnetic interference shielding (EMI) protection for electronic packages has been demonstrated at very low coating thicknesses. The present invention also relates to films prepared using the formulations and methods of the present invention. In another aspect, the present invention relates to an article comprising a film as described herein adhered to a suitable substrate. In yet another aspect, the present invention also relates to a method for producing a conductive film that provides electromagnetic interference shielding (EMI) protection to an electronic component. In yet another aspect, the present invention also relates to a method for providing electromagnetic interference shielding (EMI) protection to an electronic component. [Background technology]
[0003] BACKGROUND OF THEINVENTION EMI shielding is the practice of reducing electromagnetic fields in a space by blocking magnetic fields with barriers made of conductive or magnetic materials. Shields are typically applied to enclosures to isolate electrical devices from the outside world. Electromagnetic shields that block high-frequency electromagnetic radiation are also known as RF shields.
[0004] EMI shielding can reduce the coupling of radio waves, electromagnetic fields and electrostatic fields. Conductive enclosures used to block electrostatic fields are also known as Faraday cages. The amount of reduction that can be achieved depends on factors such as the material used, its thickness, the conductivity of the coating, and the frequency of the electromagnetic waves of interest.
[0005] Typical materials used for electromagnetic shielding include formed sheet metal (i.e., metal cans), and metal coatings applied by plating and / or sputtering processes. Another commonly used shielding method, especially with electronic products housed in plastic containers, is the use of conductive coatings.
[0006] Formed metal sheets are typically used for board level shielding where a metal can is applied to an electronic package. Due to its size, this method is not suitable for very small designs and is very inflexible in application.
[0007] Plating methods can provide complete coverage on electronic packages and potentially have good thickness control. Such methods have very good productivity per unit time (UPH) and relatively low material costs. However, these methods require pretreatment of the surface to be coated, requiring tedious masking of the substrate.
[0008] Sputtering is a well-known and widely accepted method for EMI shielding applications. This method can provide very effective EMI shielding due to the typically low material cost but high electrical conductivity of the coating. However, the method requires the use of very expensive equipment. Furthermore, its UPH is very low.
[0009] Currently, conductive paste adhesives are commonly used for EMI shielding protection. Unfortunately, if the paste adhesive does not have high electrical conductivity, a very thick film is required to achieve the desired shielding performance.
[0010] Conductive coatings provide EMI protection to electronic packages through conductive compositions that typically consist of carrier materials including thermosetting and thermoplastic resins loaded with a suitable metal, such as silver, copper, or nickel, in very small particulate form. The coatings are usually applied by a spray or printing process onto the electronic package and, once dry, produce a continuous conductive layer that can be electrically connected to the device's chassis ground, thus providing effective shielding. A limitation of this method is that the effectiveness of the EMI shielding is not as good as pure metal sheets or metal coatings provided by plating and sputtering (because the conductive coating has poor electrical conductivity). Another limitation is that it is difficult to produce uniform, three-dimensional, thin coatings on electronic packages by conventional spray or printing processes.
[0011] These and other limitations of the prior art methods are now addressed by the present invention. Summary of the Invention [Means for solving the problem]
[0012] In accordance with the present invention, highly conductive compositions are provided that are useful for applying conductive materials to suitable substrates, and the resulting coated articles have improved EMI shielding performance compared to articles coated with prior art formulations using prior art methods.
[0013] According to an embodiment of the present invention, a method for producing a conductive film and an article shielded therewith are also provided. The method of the present invention contemplates the use of various application methods, such as electrostatic spraying, air spraying, ultrasonic spraying, spin coating, etc., to achieve a substantially uniform three-dimensional thin conductive coating on the surface of an electronic package. Effective EMI shielding has been demonstrated at very thin coating thicknesses. For example, for a rectangular EMC block, three-dimensional coating means that the conductive composition substantially uniformly covers the top surface and four side walls of the block (see, for example, FIG. 1).
[0014] Electrostatic spraying typically uses very high voltages (about 10 KV) to dispense coating material onto a substrate, during which electrical forces overcome the surface tension of the coating solution, and droplets of coating material break up into a fine, electrically charged mist (nano-sized droplets). Driven by the electric field strength, the fine, electrically charged mist is accelerated toward the workpiece. Compared to other spraying processes, the mist produced by electrostatic spraying tends to be much finer in certain embodiments, which makes it easier to control the coating footprint. This, in some embodiments, makes it easier to create three-dimensional thin coatings on the surface of an electronic package.
[0015] The air spray process is carried out with a pneumatic spray gun, which has a nozzle, a paint reservoir, and an air compressor. When the trigger is pressed, the paint is mixed with the compressed air stream and released in a fine spray.
[0016] Ultrasonic spraying is a coating method that uses high frequency sound waves generated by a piezoelectric transducer acting on a spray nozzle tip to atomize the coating liquid to produce small droplets for coating onto the surface to be coated.
[0017] Compared to the air spray process, the mist generated by the electrostatic spray process is much finer and the coating footprint is much easier to control. This allows for the application of three-dimensional thin coatings to the surface of electronic packages with a nearly 1:1 ratio of sidewall package thickness to top surface thickness. Because the ultrasonic spray mist is similar to that of electrostatic spray, the coating quality from this method is similar to that obtained with the electrostatic method.
[0018] In accordance with the present invention, the limitations of the prior art have been overcome and the superior performance of the compositions of the present invention, as well as methods of making and using same, have been demonstrated as follows: The compositions of the present invention applied in a three-dimensional manner onto an EMC surface (e.g., by electrostatic spraying, air spraying processes, ultrasonic spraying processes, spin coating processes, etc.) provide a three-dimensional thin conductive coating on the EMC surface. The thin coating exhibits excellent adhesion to the EMC. The highly conductive composition according to the present invention improves its EMI shielding performance. Effective EMI shielding performance is achieved at coating thicknesses as low as 1-2 μm. Much higher UPH is obtained with the formulations of the present invention as compared to those obtained with sputtered coatings. Furthermore, the method of the present invention provides similar metal coatings as compared to coatings prepared by sputtering and plating processes.
[0019] In certain embodiments of the present invention, films prepared using the formulations and methods of the present invention are also provided. In further embodiments of the present invention, articles are also provided that include the films described herein adhered to a suitable substrate therefor.
[0020] In summary, highly conductive compositions (and methods for their preparation) have been demonstrated herein. These highly conductive compositions can be applied to EMC surfaces by a variety of methods, such as electrostatic spraying, air spraying, ultrasonic spraying, spin coating, etc. Uniform three-dimensional thin coatings have been achieved on the EMC surfaces (see, e.g., FIG. 1). Test results show that these highly conductive compositions can provide highly effective EMI shielding protection for electronic packages at very low thicknesses.
[0021] The present invention is unique in that it provides a combination of at least the following desirable performance characteristics: a.Good EMI shielding effect (e.g., above 20dB); b.High electrical conductivity at low curing temperatures; c. A very thin but uniform coating; and d.3D EMI shielding coating for IC package protection. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 illustrates the result of using the method of the present invention to apply a conductive coating to the top and side walls of a device for which EMI shielding is desired. [Diagram 2] FIG. 2 shows adhesion of an exemplary conductive composition on EMC after moisture conditioning of composition A (see Example 1). [Diagram 3] FIG. 3 shows the results of scratch-peel testing of the adhesion of cured specimens of composition A1 (see Example 5) to exemplary substrates. [Figure 4] FIG. 4 summarizes the EMI shielding performance of different formulations at a thickness of 5 μm. C850-6L is commercially available from Henkel Electronic Materials LLC. Formulation A1 is described in Example 5. Formulation A is described in Example 1. The Y-axis is the EMI shielding effectiveness. The lower the number, the better the EMI shielding performance. The test results show that significant EMI shielding performance improvements have been achieved with the formulations described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Detailed Description of the Invention According to the present invention, in the range of about 10 to 98.99 weight percent of a particulate conductive filler; an organic matrix in the range of about 0.01 to about 40 weight percent; and in the range of about 1 to about 80 weight percent of an organic diluent; where: the particulate conductive filler is selected from the group consisting of gold, silver, copper, platinum, palladium, nickel, aluminum, indium, alloys of nickel (e.g., alloy 42), alloys of zinc, alloys of iron, alloys of indium, silver plated copper, silver plated aluminum, bismuth, tin, bismuth-tin alloys, silver plated fiber, silver plated graphite, silver plated silicon carbide, silver plated boron nitride, silver plated diamond, silver plated alumina, silver plated alloy 42, cadmium and alloys of cadmium, lead and alloys of lead, antimony and alloys of antimony, and mixtures of two or more thereof; and the particulate conductive filler has a particle size in the range of about 1 nm to about 50 μm; the organic matrix comprises at least one thermoplastic and / or at least one thermosetting resin; and the organic diluent is selected from the group consisting of aromatic hydrocarbons, saturated hydrocarbons, chlorinated hydrocarbons, ethers, polyols, esters, dibasic esters, α-terpineol, β-terpineol, kerosene, dibutyl phthalate, butyl carbitol, butyl carbitol acetate, carbitol acetate, ethyl carbitol acetate, hexylene glycol, high boiling alcohols and their esters, glycol ethers, ketones, amides, heteroaromatic compounds, and mixtures of any two or more thereof; and When the composition is exposed to an elevated temperature of up to about 250° C. Provides at least 20 dB of electromagnetic interference shielding (EMI) protection for electronic packages; When the composition is applied to a three-dimensional substrate by a suitable means, such as electrostatic spraying, air spraying, ultrasonic spraying, spin coating, or the like, to a thickness of less than 25 μm, the composition has a coating thickness of 1×10 -3 Has a volume resistivity of less than ohm-cm It has good adhesion to the substrate. In the case of a rectangular EMC block, three-dimensional coating means that the conductive composition covers the top surface and the four side walls of the block.
[0024] EMI effectiveness can be measured in a variety of ways, such as using a waveguide system (1.7-2.8GHz) that includes two waveguide-to-coaxial adapters and a vector network analyzer. Samples are prepared as thin film layers with target thicknesses coated onto PET film. Sample size is 5x3 inches. This material is suitable for use at frequencies above 14KHz with excellent performance >1GHz.
[0025] Filler In accordance with the present invention, the particulate conductive filler used herein is present in the range of about 10 to about 98.99 wt% of the compositions of the present invention. In some embodiments, the formulations of the present invention include a particulate conductive filler in the range of about 10 to about 95 wt%, in some embodiments, the formulations of the present invention include a particulate conductive filler in the range of about 10 to about 90 wt%, in some embodiments, the formulations of the present invention include a particulate conductive filler in the range of about 10 to about 80 wt%, and in some embodiments, the formulations of the present invention include a particulate conductive filler in the range of about 10 to about 70 wt%. The particulate conductive filler used is present in the range of 20 to about 98.99% by weight of the formulation of the present invention, in some embodiments the formulations of the present invention include about 20 to about 95% by weight of the particulate conductive filler, in some embodiments the formulations of the present invention include about 20 to about 90% by weight of the particulate conductive filler, in some embodiments the formulations of the present invention include in the range of about 20 to about 80% by weight of the particulate conductive filler, and in some embodiments the formulations of the present invention include about 20 to about 70% by weight of the particulate conductive filler. The particulate conductive filler employed is present in the range of 30 to about 98.99% by weight of the formulation of the present invention, in some embodiments the formulations of the present invention include from about 30 to about 95% by weight of the particulate conductive filler, in some embodiments the formulations of the present invention include from about 30 to about 90% by weight of the particulate conductive filler, in some embodiments the formulations of the present invention include from about 30 to about 80% by weight of the particulate conductive filler, and in some embodiments the formulations of the present invention include from about 30 to about 70% by weight of the particulate conductive filler; In some embodiments, the formulations of the present invention comprise in the range of about 40 to about 95% by weight of particulate conductive filler, in some embodiments, the formulations of the present invention comprise in the range of about 40 to about 90% by weight of particulate conductive filler, in some embodiments, the formulations of the present invention comprise in the range of about 40 to about 80% by weight of particulate conductive filler, in some embodiments, the formulations of the present invention comprise in the range of about 40 to about 70% by weight of particulate conductive filler, and in some embodiments, the formulations of the present invention comprise in the range of about 40 to about 60% by weight of particulate conductive filler.
[0026] The particulate conductive fillers used herein may be substantially nanoparticles, or the particulate conductive fillers used herein may be substantially larger and non-nanoparticles, or the particulate conductive fillers used herein may be a combination of nanoparticles and non-nanoparticles.
[0027] For example, in some embodiments of the present invention, up to 100% by weight of the particulate conductive fillers used herein have a particle size in the range of about 2-1000 nm, with an average particle size of about 2-1000 nm, with the remaining particulate conductive fillers having a particle size of 50 μm or less.
[0028] In some embodiments of the present invention, up to 100% by weight of the particulate conductive fillers used herein have a particle size of less than 50 μm and an average particle size in the range of about 1 to 25 μm.
[0029] In some embodiments of the present invention, up to 10% by weight of the particulate conductive fillers used herein have a particle size in the range of about 2-1000 nm, in some embodiments, up to 20% by weight of the particulate conductive fillers used in the practice of the present invention have a particle size in the range of about 2-1000 nm, in some embodiments, up to 30% by weight of the particulate conductive fillers used in the practice of the present invention have a particle size in the range of about 2-1000 nm, in some embodiments, up to 40% by weight of the particulate conductive fillers used in the practice of the present invention have a particle size in the range of about 2-1000 nm, and in some embodiments, up to 50% by weight of the particulate conductive fillers used in the practice of the present invention have a particle size in the range of about 2-1000 nm. Up to 50% by weight of the filler has a particle size in the range of about 2-1000 nm, in some embodiments up to 60% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-1000 nm, in some embodiments up to 70% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-1000 nm, in some embodiments up to 80% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-1000 nm, and in some embodiments up to 90% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-1000 nm.
[0030] In some embodiments, up to 10% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-500 nm, in some embodiments, up to 20% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-500 nm, in some embodiments, up to 30% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-500 nm, in some embodiments, up to 40% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-500 nm, in some embodiments, up to 50% by weight of the particulate conductive filler used in the practice of this invention has a particle size in the range of about 2-500 nm. Up to 50% by weight of the particulate conductive filler used in the practice of this invention have a particle size in the range of about 2-500 nm, in some embodiments up to 60% by weight of the particulate conductive filler used in the practice of this invention have a particle size in the range of about 2-500 nm, in some embodiments up to 70% by weight of the particulate conductive filler used in the practice of this invention have a particle size in the range of about 2-500 nm, in some embodiments up to 80% by weight of the particulate conductive filler used in the practice of this invention have a particle size in the range of about 2-500 nm, and in some embodiments up to 90% by weight of the particulate conductive filler used in the practice of this invention have a particle size in the range of about 2-500 nm.
[0031] In some embodiments, up to 10% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, in some embodiments, up to 20% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, in some embodiments, up to 30% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, in some embodiments, up to 40% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, in some embodiments, up to 50% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm. up to 60% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, in some embodiments up to 70% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, in some embodiments up to 80% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm, and in some embodiments up to 90% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 1 to 25 μm.
[0032] In some embodiments, up to 10% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments, up to 20% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments, up to 30% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments, up to 40% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments, up to 50% by weight of the particulate conductive filler used in the practice of this invention has a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm. up to 60% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments up to 70% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments up to 80% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm, in some embodiments up to 90% by weight of the particulate conductive filler used in the practice of this invention have a particle size of 50 μm or less and an average particle size in the range of about 10 nm to 10 μm.
[0033] Organic Matrix A wide variety of organic matrices are contemplated for use in the present application. Exemplary organic matrices include at least one thermoplastic resin and / or at least one thermosetting resin.
[0034] As used herein, the organic matrix is present in the range of about 0.01 to about 40% by weight of the composition of the present invention. In some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 0.05 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 0.1 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 0.5 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 1 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 2 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 3 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 4 to about 40% by weight, in some embodiments, the formulation of the present invention comprises an organic matrix in the range of about 5 to about 40% by weight.
[0035] In some embodiments, the organic matrix as used herein is present in the range of about 0.01 to about 30% by weight of the composition of the present invention, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.05 to about 30% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.1 to about 30% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.5 to about 30% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 1 to about 30% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 2 to about 30% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 3 to about 30% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 4 to about 30% by weight, and in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 5 to about 30% by weight.
[0036] In some embodiments, the organic matrix as used herein is present in the range of about 0.01 to about 20 wt % of the composition of the present invention, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.05 to about 20 wt %, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.1 to about 20 wt %, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.5 to about 20 wt %, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 1 to about 20 wt %, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 2 to about 20 wt %, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 3 to about 20 wt %, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 4 to about 20 wt %, and in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 5 to about 20 wt %.
[0037] In some embodiments, the organic matrix as used herein is present in the range of about 0.01 to about 10% by weight of the composition of the present invention, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.05 to about 10% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.1 to about 10% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 0.5 to about 10% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 1 to about 10% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 2 to about 10% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 3 to about 10% by weight, in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 4 to about 10% by weight, and in some embodiments, the formulations of the present invention comprise an organic matrix in the range of about 5 to about 10% by weight.
[0038] Exemplary thermoplastics include polyesters, polyacrylates (e.g., polymethacrylate, polybutylmethacrylate), polyurethanes, phenoxy, polyethyloxazolines, polyvinylpyrrolidones, polyvinyl alcohols, polyacrylamides, polyglycols and polyacrylic acids, poly(ethylene glycol), aromatic vinyl polymers, flexible epoxies, polymers with epoxy functionality, polycarbonates, ABS, PC / ABS alloys, nylons, inherently conductive polymers, silicone polymers, siloxane polymers, rubbers, polyolefins, vinyl polymers, polyamides, fluoropolymers, polyphenylene ethers, copolymers, and the like. The polyether ester may be selected from the group consisting of ethylene carbonate, acrylonitrile butadiene styrene copolymer, polyarylate ether sulfone or ketone, polyamide imide, polyetherimide, poly(ethylene terephthalate), poly(1,4-butylene terephthalate), polyethylene, polypropylene, polypropylene-EPDM blends, butadiene, styrene-butadiene, nitrile, chlorosulfonates, neoprene, acrylonitrile butadiene styrene copolymer, polyether ester, styrene / acrylonitrile polymer, polyphenylene sulfide, nitrile rubber, cellulosic resin, and mixtures of any two or more thereof.
[0039] In addition to the presence of at least one thermoplastic resin, the organic matrix contemplated for use herein may optionally include at least one thermosetting resin. Examples of thermosetting resins include epoxies, acrylics, acrylates, vinyls, maleimides, nadimides, itaconimides, cyanate esters, alkyds, cyanate esters, phenolics, benzoxazines, polyimides, functionalized polyimides, oxetanes, vinyl ethers, polyurethanes, melamines, urea-formaldehyde resins, phenol-formaldehyde resins, silicones, melamines, and the like, as well as mixtures of any two or more thereof.
[0040] Epoxy A wide variety of epoxy-functionalized resins are contemplated for use herein, such as liquid epoxy resins based on bisphenol A, solid epoxy resins based on bisphenol A, liquid epoxy resins based on bisphenol F (e.g., Epiclon EXA-835LV), multifunctional epoxy resins based on phenol-novolac resins, dicyclopentadiene type epoxy resins (e.g., Epiclon HP-7200L), naphthalene type epoxy resins, and the like, and mixtures of any two or more thereof.
[0041] Exemplary epoxy-functionalized resins contemplated for use herein include diepoxides of cycloaliphatic alcohols, hydrogenated bisphenol A (commercially available as Epalloy 5000), difunctional cycloaliphatic glycidyl esters of hexahydrophthalic anhydride (commercially available as Epalloy 5200), Epiclon EXA-835LV, Epiclon HP-7200L, and the like, as well as mixtures of any two or more thereof.
[0042] In certain embodiments, the epoxy component may include a combination of two or more different bisphenol-based epoxies. These bisphenol-based epoxies may be selected from bisphenol A, bisphenol F, or bisphenol S epoxies, or combinations thereof. In addition, two or more different bisphenol epoxies within the same type of resin (e.g., A, F, or S) may be used.
[0043] Commercially available examples of bisphenol epoxies contemplated for use herein include bisphenol F type epoxies (e.g., RE-404-S from Nippon Kayaku, Japan, and EPICLON 830 (RE1801), 830S (RE1815), 830A (RE1826), and 830W from Dai Nippon Ink & Chemicals, Inc., and RSL 1738 and YL-983U from Resolution), and bisphenol A type epoxies (e.g., YL-979 and 980 from Resolution).
[0044] The above bisphenol epoxies, available from Dai Nippon, are promoted as liquid undiluted epichlorohydrin-bisphenol F epoxies with much lower viscosities than conventional epoxies based on bisphenol A epoxies, and have similar physical properties to liquid bisphenol A epoxies. The bisphenol F epoxies have lower viscosities than the bisphenol A epoxies, but otherwise the two types of epoxies are the same, providing a lower viscosity and therefore faster flowing underfill sealant material. The EEW of these four bisphenol F epoxies is 165-180. The viscosity at 25°C is 3,000-4,500 cps (except for RE1801, whose viscosity upper limit is 4,000 cps). The hydrolyzable chlorine content is reported to be 200 ppm for RE1815 and 830W, and 100 ppm for RE1826.
[0045] The above bisphenol epoxies, available from Resolution, are recommended as low chlorine content liquid epoxies. The bisphenol A epoxy has an EEW (g / eq) of 180-195 and a viscosity of 100-250 cps at 25°C. The total chlorine content of YL-979 is reported to be 500-700 ppm and that of YL-980 is reported to be 100-300 ppm. The bisphenol F epoxy has an EEW (g / eq) of 165-180 and a viscosity of 30-60 at 25°C. The total chlorine content of RSL-1738 is reported to be 500-700 ppm and that of YL-983U is reported to be 150-350 ppm.
[0046] In addition to bisphenol epoxies, other epoxy compounds are contemplated for use as the epoxy component of the formulation of the present invention. For example, cycloaliphatic epoxies such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarbonate can be used. Monofunctional, difunctional, or multifunctional reactive diluents may also be used to adjust the viscosity and / or lower the Tg of the resulting resin material. Exemplary reactive diluents include butyl glycidyl ether, cresyl glycidyl ether, polyethylene glycol glycidyl ether, or polypropylene glycol glycidyl ether, and the like.
[0047] Suitable epoxies for use herein include polyglycidyl derivatives of phenolic compounds, such as those commercially available under the trade name EPON, e.g., EPON 828, EPON 1001, EPON 1009, EPON 1031 from Resolution; DER 331, DER 332, DER 334, and DER 542 from Dow Chemical Co.; and BREN-S from Nippon Kayaku. Other suitable epoxies include polyepoxides prepared from polyols and the like, and polyglycidyl derivatives of phenol-formaldehyde novolacs, the latter such as DEN 431, DEN 438, and DEN 439 from Dow Chemical. Cresol analogs are also commercially available under the trade name ARALDITE, e.g., ARALDITE ECN 1235, ARALDITE ECN 1273, and ARALDITE ECN 1299 from Ciba Specialty Chemicals Corporation. SU-8 is a bisphenol A type epoxy novolac available from Resolution. Polyglycidyl adducts of amines, aminoalcohols, and polycarboxylic acids are also useful in the present invention, commercially available resins include GLYAMINE 135, GLYAMINE 125, and GLYAMINE 115 from FIC Corporation; ARALDITE MY-720, ARALDITE 0500, and ARALDITE 0510 from Ciba Specialty Chemicals, and PGA-X and PGA-C from Sherwin-Williams Co.
[0048] Suitable monofunctional epoxy co-reactive diluents for optional use herein include those having a viscosity lower than that of the epoxy component, typically less than about 250 cps.
[0049] The monofunctional epoxy co-reactive diluent should have an epoxy group with an alkyl group having from about 6 to about 28 carbon atoms, examples of which include C 6-28 Alkyl glycidyl ether, C6-28 Fatty acid glycidyl ester, C 6-28 Alkylphenol glycidyl ether and the like.
[0050] When such monofunctional epoxy co-reactive diluents are included, they should be used in amounts of about 0.5 weight percent to about 10 weight percent, based on the total weight of the composition; in some embodiments, they should be used in amounts of about 0.25 weight percent to about 5 weight percent, based on the total weight of the composition.
[0051] The epoxy component should be present in the composition in an amount ranging from about 1 weight percent to about 40 weight percent; in some embodiments, the formulations of the present invention include from about 2 weight percent to about 18 weight percent epoxy; in some embodiments, the formulations of the present invention include from about 5 to about 15 weight percent epoxy.
[0052] In some embodiments, the epoxy component used herein is a silane-modified epoxy, for example a composition comprising: (A) an epoxy component encompassed by the following structure:
[0053] [ka] (In the formula: Y may be present or absent, and when Y is present, Y is a direct bond, CH, CH(CH), C=O, or S; where R1 is alkyl, alkenyl, hydroxy, carboxy, and halogen; and where x is 1 to 4); (B) an epoxy-functionalized alkoxysilane encompassed by the structure:
[0054] [ka] (In the formula, R1 is an oxirane-containing moiety, and R 2 is an alkyl or alkoxy substituted alkyl, aryl, or aralkyl group having 1 to 10 carbon atoms; and (C) A reaction product of component (A) and component (B).
[0055] An example of such a silane modified epoxy is formed as the reaction product of an aromatic epoxy, such as a bisphenol A, E, F, or S epoxy, or a biphenyl epoxy, with an epoxy silane, where the epoxy silane is encompassed by the following structure:
[0056] [ka] (In the formula, R 1 is an oxirane-containing moiety, examples of which include 2-(ethoxymethyl)oxirane, 2-(propoxymethyl)oxirane, 2-(methoxymethyl)oxirane, and 2-(3-methoxypropyl)oxirane; and R 2 is an alkyl or alkoxy substituted alkyl, aryl, or aralkyl group having 1 to 10 carbon atoms.
[0057] In one embodiment, R 1 is 2-(ethoxymethyl)oxirane, and R 2 is methyl.
[0058] The ideal structure of the aromatic epoxy used to prepare the silane modified epoxy is:
[0059] [ka] (In the formula, Y may be present or absent, and when Y is present, Y is a direct bond, CH, CH(CH), C=O, or S; R1 is alkyl, alkenyl, hydroxy, carboxy, or halogen; and x is 1 to 4. Examples include:
[0060] Of course, when x is 2 to 4, chain-extended aromatic epoxies are also contemplated as being encompassed by this structure.
[0061] For example, a chain extended version of an aromatic epoxy has the following structure:
[0062] [ka] may be included in the
[0063] In some embodiments, the siloxane modified epoxy resin has the structure:
[0064] [ka] (In the formula: Z is -O-(CH2)3-O-Ph-CH2-Ph-O-(CH2-CH(OH)-CH2-O-Ph-CH2-Ph-O-) n -CH2-oxirane, and (n is in the range of approximately 1 to 4) has.
[0065] In some embodiments, the siloxane modified epoxy resin is prepared by contacting a combination of the following components under conditions suitable to promote the reaction thereof:
[0066] [ka] Oxirane-CH2-O-Ph-CH2-Ph-O-(CH2-CH(OH)-CH2-O-Ph-CH2-Ph-O-) n -CH2-Oxirane (wherein "n" ranges from about 1 to 4).
[0067] The silane modified epoxy may also be a combination of aromatic epoxy, epoxy silane, and the reaction product of aromatic epoxy and epoxy silane. The reaction product may be prepared from aromatic epoxy and epoxy silane in a weight ratio of 1:100 to 100:1, for example, 1:10 to 10:1.
[0068] The amount of epoxy monomer contemplated for use in the compositions of the present invention is sufficient so that the resulting formulation contains about 1-20% by weight of said epoxy. In certain embodiments, the resulting formulation contains about 2-18% by weight of said epoxy. In certain embodiments, the resulting formulation contains about 5-15% by weight of said epoxy.
[0069] Epoxy curing agents are optionally used in combination with the epoxy monomer. Exemplary epoxy curing agents include urea, aliphatic and aromatic amines, amine hardeners, polyamides, imidazoles, dicyandiamides, hydrazides, urea-amine hybrid curing systems, free radical initiators (e.g., peroxyesters, peroxycarbonates, hydroperoxides, alkylperoxides, arylperoxides, azo compounds, etc.), organic bases, transition metal catalysts, phenols, acid anhydrides, Lewis acids, Lewis bases, etc.
[0070] When an epoxy hardener is present, the composition of the present invention comprises an epoxy hardener in the range of about 0.1-2 wt %. In certain embodiments, the composition of the present invention comprises an epoxy hardener in the range of about 0.5-5 wt %.
[0071] Maleimide, nadimide, or itaconimide The maleimides, nadimides, or itaconimides contemplated for use herein have the following structures, respectively:
[0072] [ka] (In the formula: m is 1 to 15; p is 0 to 15; Each R 2 is hydrogen or lower alkyl (e.g., C 1-5 ), and J is a monovalent or polyvalent group containing an organic group or an organosiloxane group. and combinations of two or more thereof.
[0073] In some embodiments of the present invention, J is a monovalent or polyvalent group selected from the following: - a hydrocarbyl or substituted hydrocarbyl species having typically in the range of from about 6 to about 500 carbon atoms, said hydrocarbyl species being selected from alkyl, alkenyl, alkynyl, cycloalkyl, cycloalkenyl, aryl, alkylaryl, arylalkyl, arylalkenyl, alkenylaryl, arylalkynyl, or alkynylaryl, with the proviso that X can be aryl only if X comprises a combination of two or more different species; - a hydrocarbylene or substituted hydrocarbylene species typically having from about 6 to about 500 carbon atoms, the hydrocarbylene species being selected from alkylene, alkenylene, alkynylene, cycloalkylene, cycloalkenylene, arylene, alkylarylene, arylalkylene, arylalkenylene, alkenylarylene, arylalkynylene, or alkynylarylene; -heterocyclic or substituted heterocyclic species, typically having in the range of from about 6 to about 500 carbon atoms; polysiloxane, or - polysiloxane-polyurethane block copolymers, as well as A combination of one or more of the above with a linker selected from the following: a covalent bond, -O-, -S-, -NR-, -NR-C(O)-, -NR-C(O)-O-, -NR-C(O)-NR-, -SC(O)-, -SC(O)-O-, -SC(O)-NR-, -OS(O)2-, -OS(O)2-O-, -OS(O)2-NR-, -OS(O)-, -OS(O)-O-, -OS(O)-NR-, -O-NR-C(O)-, -O-NR-C(O)-O-, -O-NR-C(O)-NR-, -NR-OC(O)-, -NR-OC(O)-O-, -NR-OC (O)-NR-, -O-NR-C(S)-, -O-NR-C(S)-O-, -O-NR-C(S)-NR-, -NR-OC(S)-, -NR-OC(S)-O-, -NR-OC(S)- NR-, -OC(S)-, -OC(S)-O-, -OC(S)-NR-, -NR-C(S)-, -NR-C(S)-O-, -NR-C(S)-NR-, -SS(O)2-, -SS(O )2-O-, -SS(O)2-NR-, -NR-OS(O)-, -NR-OS(O)-O-, -NR-OS(O)-NR-, -NR-OS(O)2-, -NR-OS(O)2-O-, - NR-OS(O)2-NR-, -O-NR-S(O)-, -O-NR-S(O)-O-, -O-NR-S(O)-NR-, -O-NR-S(O)2-O-, -O-NR-S(O)2-NR-, -O-NR-S(O)2-, -OP(O)R2-, -SP(O)R2-, or -NR-P(O)R2- (wherein each R is independently hydrogen, alkyl, or substituted alkyl).
[0074] Exemplary compositions include those where J is: oxyalkyl, thioalkyl, aminoalkyl, carboxyalkyl, oxyalkenyl, thioalkenyl, aminoalkenyl, carboxyalkenyl, oxyalkynyl, thioalkynyl, aminoalkynyl, carboxyalkynyl, oxycycloalkyl, thiocycloalkyl, aminocycloalkyl, carboxycycloalkyl, oxycloalkenyl, thiocycloalkenyl, aminocycloalkenyl, carboxycycloalkenyl, heterocycle, oxyheterocycle, thioheterocycle, aminoheterocycle, carboxyheterocycle, oxyaryl, thioaryl, aminoaryl, carboxyaryl, heteroaryl, oxyheteroaryl, thioheteroaryl, aminoheteroaryl, carboxyheteroaryl, oxyalkylaryl, thioalkylaryl, aminoalkylaryl, carboxyalkylaryl, oxyarylalkyl, thioarylalkyl, aminoarylalkyl, carboxyarylalkyl, oxyarylalkenyl, thioarylalkenyl, aminoarylalkenyl, Carboxyarylalkenyl, oxyalkenylaryl, thioalkenylaryl, aminoalkenylaryl, carboxyalkenylaryl, oxyarylalkynyl, thioarylalkynyl, aminoarylalkynyl, carboxyarylalkynyl, oxyalkynylaryl, thioalkynylaryl, aminoalkynylaryl or carboxyalkynylaryl, oxyalkylene, thioalkylene, aminoalkylene, carboxyalkylene, oxyalkenylene, thioalkenylene, aminoalkenylene, carboxyalkene, aryl, oxyalkynylene, thioalkynylene, aminoalkynylene, carboxyalkynylene, oxycycloalkylene, thiocycloalkylene, aminocycloalkylene, carboxycycloalkylene, oxycycloalkenylene, thiocycloalkenylene, aminocycloalkenylene, carboxycycloalkenylene, oxyarylene, thioarylene, aminoarylene, carboxyarylene, oxyalkylarylene, thioalkylarylene, aminoalkylarylene, carboxyalkylarylene, oxyarylalkylene,Thioaryl alkylene, aminoaryl alkylene, carboxyaryl alkylene, oxyaryl alkenylene, thioaryl alkenylene, aminoaryl alkenylene, carboxyaryl alkenylene, oxyalkenylarylene, thioalkenylarylene, aminoalkenylarylene, carboxyalkenylarylene, oxyaryl alkynylene, thioaryl alkynylene, aminoaryl alkynylene, carboxyaryl alkynylene, oxyalkynylarylene, thioalkynylarylene, aminoalkynylarylene, carboxyalkynylarylene, heteroarylene, oxyheteroarylene, thioheteroarylene, aminoheteroarylene, carboxyheteroarylene, heteroatom-containing divalent or polyvalent cyclic partial structure, oxyheteroatom-containing divalent or polyvalent cyclic partial structure, thioheteroatom-containing divalent or polyvalent cyclic partial structure, aminoheteroatom-containing divalent or polyvalent cyclic partial structure, or carboxyheteroatom-containing divalent or polyvalent cyclic partial structure.
[0075] Acrylates The acrylates contemplated for use in the practice of the present invention are well known in the art, see, for example, U.S. Patent No. 5,717,034, the entire contents of which are incorporated herein by reference.
[0076] Exemplary acrylates contemplated for use herein include monofunctional (meth)acrylates, difunctional (meth)acrylates, trifunctional (meth)acrylates, multifunctional (meth)acrylates, and the like.
[0077] Exemplary monofunctional (meth)acrylates include phenylphenol acrylate, methoxypolyethylene acrylate, acryloyloxyethyl succinate, fatty acid acrylate, methacryloyloxyethyl phthalate, phenoxyethylene glycol methacrylate, fatty acid methacrylate, β-carboxyethyl acrylate, isobornyl acrylate, isobutyl acrylate, t-butyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, dihydrocyclopentadiethyl acrylate, cyclohexyl methacrylate, t-butyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, t-butylaminoethyl methacrylate, 4-hydroxybutyl acrylate, tetrahydrofurfuryl acrylate, benzyl acrylate, ethyl carbitol acrylate, phenoxyethyl acrylate, methoxytriethylene glycol acrylate, monopentaerythritol acrylate, dipentaerythritol acrylate, tripentaerythritol acrylate, polypentaerythritol acrylate, and the like.
[0078] Exemplary difunctional (meth)acrylates include hexanediol dimethacrylate, hydroxyacryloyloxypropyl methacrylate, hexanediol diacrylate, urethane acrylate, epoxy acrylate, bisphenol A type epoxy acrylate, modified epoxy acrylate, fatty acid modified epoxy acrylate, amine modified bisphenol A type epoxy acrylate, allyl methacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, glycerin dimethacrylate, polypropylene glycol diacrylate, propoxylated ethoxylated bisphenol A diacrylate, 9,9-bis(4-(2-acryloyloxyethoxy)phenyl)fluorene, tricyclodecane diacrylate, dipropylene glycol diacrylate, polypropylene glycol diacrylate, PO modified neopentyl glycol diacrylate, tricyclodecane dimethanol diacrylate, 1,12-dodecane diol dimethacrylate, and the like.
[0079] Exemplary trifunctional (meth)acrylates include trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxy triacrylate, polyether triacrylate, glycerin propoxy triacrylate, and the like.
[0080] Exemplary polyfunctional (meth)acrylates include dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxy tetraacrylate, ditrimethylolpropane tetraacrylate, and the like.
[0081] Further exemplary acrylates contemplated for use in the practice of the present invention include those described in US Pat. No. 5,717,034, the entire contents of which are incorporated herein by reference.
[0082] Cyanate ester resin The cyanate ester monomers contemplated for use in the practice of the present invention contain two or more ring-forming cyanate (-OC≡N) groups that undergo cyclotrimerization upon heating to form a substituted triazine ring. Because no leaving groups or volatile by-products are formed during the curing of cyanate ester monomers, the curing reaction is referred to as an addition polymerization. Suitable polycyanate ester monomers that can be used in the practice of the present invention include, for example, 1,1-bis(4-cyanatophenyl)methane, 1,1-bis(4-cyanatophenyl)ethane, 2,2-bis(4-cyanatophenyl)propane, bis(4-cyanatophenyl)-2,2-butane, 1,3-bis[2-(4-cyanatophenyl)propyl]benzene, bis(4-cyanatophenyl)ether, 4,4'-dicyanatodiphenyl, bis(4-cyanato-3,5-dimethylphenyl)methane, tris(4-cyanatophenyl)ethane, cyanated novolak, 1,3-bis[4-cyanatophenyl-1-(1-methylethylidene)]benzene, cyanated phenol dicyclopentadiene adducts, and the like. The polycyanate ester monomers used in accordance with the present invention may be readily prepared by reacting an appropriate dihydric or polyhydric phenol with a cyanogen halide in the presence of an acid acceptor.
[0083] The monomer that can be optionally combined with the polycyanate ester monomer according to the present invention is selected from monomers that undergo addition polymerization. Such monomers include vinyl ether, divinyl ether, diallyl ether, dimethacrylate, dipropargyl ether, mixed propargyl allyl ether, monomaleimide, bismaleimide, etc. Examples of such monomers include cyclohexane dimethanol monovinyl ether, trisallylcynurate, 1,1-bis(4-allyloxyphenyl)ethane, 1,1-bis(4-propargyloxyphenyl)ethane, 1,1-bis(4-allyloxyphenyl-4'-propargyloxyphenyl)ethane, 3-(2,2-dimethyltrimethyleneacetal)-1-maleimidebenzene, 2,2,4-trimethylhexamethylene-1,6-bismaleimide, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, etc.
[0084] Additional cyanate esters contemplated for use in the practice of the present invention are well known in the art, see, for example, U.S. Patent No. 5,718,941, the entire contents of which are incorporated herein by reference.
[0085] silicone Silicones contemplated for use in the practice of the present invention are well known in the art, see, for example, U.S. Patent No. 5,717,034, the entire contents of which are incorporated herein by reference.
[0086] Oxetane Oxetane (i.e., 1,3-propylene oxide) is a heterocyclic organic compound having the molecular formula CHO, which has a four-membered ring with three carbon atoms and one oxygen atom. The term oxetane also generally refers to any organic compound that contains an oxetane ring. See, for example, Burkhard et al. in Angew. Chem. Int. Ed. 2010, 49, 9052-9067, the entire contents of which are incorporated herein by reference.
[0087] Polyester Resin Polyesters as contemplated for use in the practice of the present invention refer to condensation polymers formed by the reaction of polyols (also known as polyhydric alcohols) with saturated or unsaturated dibasic acids. Typical polyols used are glycols, such as ethylene glycol; commonly used acids are phthalic and maleic acids. Water, a by-product of the esterification reaction, is continuously removed to drive the reaction to completion. The use of unsaturated polyesters and additives such as styrene reduces the viscosity of the resin. The initially liquid resin is converted to a solid by cross-linking the chains. This is done by generating free radicals at the unsaturated bonds, which propagate in a chain reaction to other unsaturated bonds in adjacent molecules, linking adjacent chains in the process.
[0088] Polyurethane Resin Polyurethane, as contemplated for use in the practice of this invention, refers to a polymer composed of a chain of organic units linked by carbamate (urethane) bonds. Polyurethane polymers are formed by reacting an isocyanate with a polyol. Both the isocyanate and polyol used to make the polyurethane contain, on average, two or more functional groups per molecule.
[0089] Polyimide Resin Polyimides, as contemplated for use in the practice of the present invention, refer to polymers composed of a chain of organic units linked by imide bonds (i.e., -C(O)-N(R)-C(O)-). Polyimide polymers can be formed by a variety of reactions, i.e., by reacting a dianhydride with a diamine, by reacting a dianhydride with a diisocyanate, etc.
[0090] Melamine Resin Melamine as contemplated for use in the practice of this invention refers to a rigid thermoset plastic material made by polymerization of melamine (i.e., 1,3,5-triazine-2,4,6-triamine) and formaldehyde. In its butylated form, it can be dissolved in n-butanol and / or xylene. The melamine-based resins can be used to crosslink other resins such as alkyd, epoxy, acrylic, and polyester resins.
[0091] Urea-formaldehyde resin Urea-formaldehyde as contemplated for use in the practice of the present invention refers to an opaque thermoset resin or plastic made from urea and formaldehyde heated in the presence of a mild base such as ammonia or pyridine.
[0092] Phenol-formaldehyde resin Phenol-formaldehyde as contemplated for use in the practice of this invention refers to synthetic polymers obtained by the reaction of phenol or substituted phenols with formaldehyde.
[0093] Diluent The non-reactive organic diluents contemplated for use herein facilitate easier handling of the formulations of the present invention as a result of, for example, lower viscosity, improved dispenseability, etc. The boiling point of the diluent is preferably close to the sintering temperature of the filler, so that as the diluent evaporates, the particles come into contact with one another and sinter.
[0094] As used herein, the organic diluent is present in the range of about 1 to about 80 wt% of the compositions of the present invention. In some embodiments, the formulations of the present invention include an organic diluent in the range of about 2 to about 80 wt%, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 5 to about 80 wt%, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 10 to about 80 wt%, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 20 to about 80 wt%, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 30 to about 80 wt%, and in some embodiments, the formulations of the present invention include an organic diluent in the range of about 40 to about 80 wt%.
[0095] In some embodiments, the formulations of the present invention comprise from about 1 to about 60% by weight of the composition of the present invention, in some embodiments, the formulations of the present invention comprise from about 2 to about 60% by weight of the organic diluent, in some embodiments, the formulations of the present invention comprise from about 5 to about 60% by weight of the organic diluent, in some embodiments, the formulations of the present invention comprise from about 10 to about 60% by weight of the organic diluent, in some embodiments, the formulations of the present invention comprise from about 20 to about 60% by weight of the organic diluent, in some embodiments, the formulations of the present invention comprise from about 30 to about 60% by weight of the organic diluent, and in some embodiments, the formulations of the present invention comprise from about 40 to about 60% by weight of the organic diluent.
[0096] In some embodiments, the formulations of the present invention comprise a composition of the present invention in the range of about 1 to about 50% by weight, in some embodiments, the formulations of the present invention comprise an organic diluent in the range of about 2 to about 50% by weight, in some embodiments, the formulations of the present invention comprise an organic diluent in the range of about 5 to about 50% by weight, in some embodiments, the formulations of the present invention comprise an organic diluent in the range of about 10 to about 50% by weight, in some embodiments, the formulations of the present invention comprise an organic diluent in the range of about 20 to about 50% by weight, in some embodiments, the formulations of the present invention comprise an organic diluent in the range of about 30 to about 50% by weight, and in some embodiments, the formulations of the present invention comprise an organic diluent in the range of about 40 to about 50% by weight.
[0097] In some embodiments, the formulations of the present invention include an organic diluent in the range of about 2 to about 40% by weight, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 5 to about 40% by weight, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 10 to about 40% by weight, in some embodiments, the formulations of the present invention include an organic diluent in the range of about 20 to about 40% by weight, and in some embodiments, the formulations of the present invention include an organic diluent in the range of about 30 to about 40% by weight.
[0098] Examples of organic diluents include aromatic hydrocarbons (benzene, toluene, xylene, etc.), saturated hydrocarbons (hexane, cyclohexane, heptane, tetradecane, etc.), chlorinated hydrocarbons (methylene chloride, chloroform, carbon tetrachloride, dichloroethane, trichloroethylene, etc.), ethers (diethyl ether, tetrahydrofuran, dioxane, glycol ether, monoalkyl ether or dialkyl ether of ethylene glycol, etc.), polyols (polyethylene glycol, propylene glycol, polypropylene glycol, etc.), esters (ethyl acetate, butyl acetate, methoxypropyl acetate, etc.), dibasic acids, esters (DBE-9), α-terpineol, β-terpineol, kerosene, diethylene glycol ethyl ether, butyl acetate, butyl cellosolve, dibutyl phthalate, butyl carbitol, butyl carbitol acetate, carbitol acetate, ethyl carbitol acetate, hexylene glycol, high boiling alcohols and their ethers and esters, glycol ethers, ketones (acetone, methyl ethyl ketone, etc.), amides (dimethylformamide, dimethylacetamide, etc.), heteroaromatics (N-methylpyrrolidone and the like), and the like, as well as mixtures of any two or more thereof.
[0099] In some embodiments, the diluent used is butyl acetate, diethylene glycol monoethyl ether acetate (carbitol acetate), dipropylene glycol methyl ether, MEK, acetone, or DBE-9.
[0100] According to a particular embodiment of the present invention, in the range of about 10 to 98.95 weight percent of a particulate conductive filler; an organic matrix in the range of about 0.01 to about 40 weight percent; and In the range of about 1 to about 80% by weight of an organic diluent A conductive composition is provided comprising:
[0101] Optional Additives According to some embodiments of the present invention, the compositions described herein may include one or more flow additives, adhesion promoters, rheology modifiers, toughening agents, fluxing agents, film softeners, phenolic novolac hardeners, epoxy cure catalysts (e.g., imidazole), curing agents (e.g., dicumyl peroxide), as well as mixtures of any two or more thereof.
[0102] As used herein, the term "flow additive" refers to compounds that modify the viscosity of the formulations they are introduced into. Exemplary compounds that impart such properties include silicon polymers, ethyl acrylate / 2-ethylhexyl acrylate copolymers, alkylol ammonium salts of phosphoric esters of ketoximes, and the like, as well as combinations of any two or more thereof.
[0103] As used herein, the term "adhesion promoter" refers to compounds that enhance the adhesive properties of the formulation into which they are incorporated.
[0104] As used herein, the term "rheology modifier" refers to additives that modify one or more physical properties of the formulation into which they are incorporated.
[0105] As used herein, the term "toughener" refers to additives that increase the impact resistance of the formulation into which they are incorporated.
[0106] As used herein, the term "fluxing agent" refers to a reducing agent that prevents oxides from forming on the surface of the molten metal.
[0107] As used herein, the term "film softening agent" refers to an agent that imparts flexibility to films prepared from formulations containing it.
[0108] As used herein, the term "phenolic novolac hardener" refers to a material that participates in further interactions of reactive groups to increase crosslinking, thereby increasing its rigidity.
[0109] As used herein, the term "epoxy curing catalyst" refers to a reactant that promotes the oligomerization and / or polymerization of epoxy-containing moieties (e.g., imidazole).
[0110] As used herein, the term "curing agent" refers to a reactant, such as dicumyl peroxide, that promotes the hardening of monomeric, oligomeric, or polymeric materials.
[0111] According to another embodiment of the present invention, there is provided a film comprising a reaction product obtained by drying, curing and / or sintering to a thickness of at least 1 μm but less than 25 μm of the inventive composition described herein.
[0112] In certain embodiments, the thickness of the film obtained by drying, curing and / or sintering the composition of the present invention is less than 20 μm.
[0113] In certain embodiments, the thickness of the film obtained by drying, curing and / or sintering the composition of the present invention is less than 15 μm.
[0114] In certain embodiments, the thickness of the film obtained by drying, curing and / or sintering the composition of the present invention is less than 10 μm.
[0115] In certain embodiments, the thickness of the film obtained by drying, curing and / or sintering the composition of the present invention is less than 5 μm.
[0116] Articles / assemblies According to yet another aspect of the present invention, there is provided an article / assembly comprising the inventive film described herein adhered to a suitable substrate (e.g., EMC (epoxy molding), laminated substrate, die, stacked die, wafer, flip chip package, hybrid memory cube, TSV device, etc.).
[0117] Substrates contemplated for use herein include polyethylene terephthalate, polymethyl methacrylate, polyolefins (e.g., polyethylene, polypropylene, etc.), polycarbonate, epoxy resins, polyimides, polyamides, polyesters, glass, Si die with silicon nitride passivation, Si die with polyimide passivation, BT substrates, bare Si, SR4 substrates, SR5 substrates, and the like.
[0118] Films coated in accordance with the present invention exhibit good adhesion to the substrate to which they are applied.
[0119] As will be readily appreciated by those skilled in the art, adhesion between the film and the substrate can be determined by a variety of methods, such as the ASTM Standard Cross-Cut Tape Test according to Test Method D 3359-97. Typically, the adhesion between the film and the substrate is at least Level 1B when measured by the ASTM Standard Cross-Cut Tape Test according to Test Method D 3359-97. In some embodiments, adhesion comparable to at least ASTM Level 1B is observed (i.e., at least 35% of the originally attached film surface remains attached to the substrate after the tape test). In certain embodiments of the present invention, adhesion comparable to at least ASTM Level 2B is observed (i.e., at least 65% of the originally attached film surface remains attached to the substrate after the tape test). In certain embodiments of the present invention, adhesion comparable to at least ASTM Level 3B is observed (i.e., at least 85% of the originally attached film surface remains attached to the substrate after the tape test). In certain embodiments of the invention, adhesion is observed that is at least comparable to ASTM Level 4B (i.e., at least 95% of the originally applied film surface remains attached to the substrate after the tape test). In certain embodiments of the invention, adhesion is observed that is at least comparable to ASTM Level 5B (i.e., 100% of the originally applied film surface remains attached to the substrate after the tape test).
[0120] In accordance with yet another aspect of the present invention, there is provided an article comprising a substrate having a substantially uniform coating of the composition of the present invention on all exposed surfaces thereof.
[0121] In some embodiments, the composition of the present invention is substantially uniformly coated on the substrate on the top and any sidewalls of the article of the present invention, hi some embodiments, the composition is applied to a suitable substrate and then dried, cured and / or sintered.
[0122] According to a further embodiment of the present invention, there is provided a method for preparing a conductive film for providing electromagnetic interference shielding (EMI) protection to an electronic component, the method comprising: applying the composition of the present invention to an electronic component by suitable means such as electrostatic spraying, air spraying, ultrasonic spraying, spin coating, etc.; Drying, curing and / or sintering the composition. Includes.
[0123] According to yet another embodiment of the present invention, there is provided a method of providing electromagnetic interference shielding (EMI) protection to an electronic component, the method comprising: applying the composition of the present invention to an electronic component by suitable means such as electrostatic spraying, air spraying, ultrasonic spraying, spin coating, etc.; Drying, curing and / or sintering the composition. Includes.
[0124] According to yet another embodiment of the present invention, there is provided a method for preparing a conductive network, said method comprising the steps of: applying the composition of the present invention to a suitable substrate in a predetermined pattern by suitable means (e.g., electrostatic spraying, air spraying, ultrasonic spraying, spin coating, etc.); and thereafter Drying, curing and / or sintering Includes.
[0125] According to a further embodiment of the present invention there is provided a conductive network prepared by the above-described method.
[0126] The conductive networks contemplated herein typically have a molecular weight of about 1×10 -3 It has a volume resistivity not exceeding ohm·cm.
[0127] Various aspects of the present invention are illustrated by the following non-limiting examples. These examples are for illustrative purposes only and are not a limitation on the practice of the present invention. It will be understood that changes and modifications can be made without departing from the spirit and scope of the present invention. Those skilled in the art can readily know how to synthesize or commercially obtain the reagents and components described herein. EXAMPLES
[0128] Example 1 Several nanoparticle-containing formulations were prepared by adding nanosilver and butyl acetate to a plastic container and mixing by hand until the mixture was homogenous (typically about 2 minutes using a speed mixer), see Table 1.
[0129] [Table 1]
[0130] A portion of the resulting paste is cast and cured at 175°C for 1 hour. The adhesion and volume resistivity are then tested. Both samples were found to have excellent adhesion and volume resistivity (see Figure 2 for exemplary results of the peel test using Formulation A).
[0131] Example 2 Several thermoplastic resin-containing formulations were prepared by dissolving the polymers Elvacite 2021 and Elvacite 2008 in DBE-9, then adding nanoparticulate silver powder to the polymer solution, then mixing by hand (typically using a speed mixer for approximately 2 minutes) until the mixture was homogenous, see Table 2.
[0132] [Table 2]
[0133] A portion of the resulting paste is cast and cured at 175° C. for 1 hour. The volume resistivity is then tested. Each sample is found to have excellent volume resistivity.
[0134] Example 3 Several nanoparticle-containing formulations were prepared by adding nanosilver, regular silver, and butyl acetate to a plastic jar and mixing by hand until the mixture was homogenous (typically for about 2 minutes using a speed mixer), see Table 3.
[0135] [Table 3]
[0136] A portion of the resulting paste is cast and cured at 175° C. for 1 hour. The volume resistivity is then tested. Each sample is found to have excellent volume resistivity.
[0137] Example 4 Several nanoparticle-containing formulations were prepared by adding nanosilver, alloy 42, and butyl acetate to a plastic jar and mixing by hand until the mixture was homogenous (typically about 2 minutes using a speed mixer), see Table 4.
[0138] [Table 4]
[0139] A portion of the resulting paste is cast and cured at 175° C. for 1 hour. The volume resistivity is then tested. Each sample is found to have excellent volume resistivity.
[0140] Example 5 Several formulations were prepared by adding Epiclon EXA 830S, Celloxide 2021 P, EP 7, Silane A 186, Ken React KR, TTS, Dicyanodiamide, Sartomer SR 285 and SF9H to a plastic jar and mixing by hand (typically with a speed mixer for approximately 2 minutes) until the mixture was homogenous. See Table 5.
[0141] [Table 5]
[0142] A portion of the resulting paste is cast and cured at 175° C. for 1 hour. The adhesion and volume resistivity are then tested. The resulting samples have excellent volume resistivity (see FIG. 3 for exemplary results of the peel test with Formulation A1).
[0143] Example 6 A silver-containing formulation was prepared by combining 2-(2-butoxyethoxy)ethyl acetate, dipropylene glycol, Luperox DI (peroxide) and AG-SAB-491 (regular silver flake). The resulting mixture was mixed by hand (typically for about 2 minutes using a speed mixer) until the mixture was homogenous. See Table 6.
[0144] [Table 6]
[0145] A portion of the resulting paste is cast and cured at 175°C for 1 hour. The volume resistivity is then tested. The resulting sample is found to have excellent volume resistivity.
[0146] Example 7 Several nanoparticle-containing formulations were prepared by adding nanosilver, diethylene glycol n-butyl ether, and butyl acetate to a plastic jar and mixing by hand until the mixture was homogenous (typically about 2 minutes using a speed mixer), see Table 7.
[0147] [Table 7]
[0148] A portion of the obtained paste is cast and cured at 100℃-175℃ for 1 hour. Then, the adhesion and volume resistivity are tested. It is found that the obtained sample has excellent volume resistivity at curing temperatures ranging from 100℃-175℃.
[0149] Various modifications of the invention in addition to those shown and described herein will be apparent to those skilled in the art of the above description, and such modifications fall within the scope of the appended claims.
[0150] The patents and publications mentioned in the specification are indicative of the levels of those skilled in the art to which this invention pertains. These patents and publications are herein incorporated by reference to the same extent as if each individual application or publication was specifically and individually indicated to be incorporated by reference.
[0151] The above description is illustrative of certain embodiments of the present invention, but is not intended to limit the practice of the invention. The appended claims, including all equivalents thereof, define the scope of the present invention.
Claims
1. in the range of 40 to 98.99 weight percent of a particulate conductive filler; an organic matrix in the range of 0.01 to 20% by weight; and % by weight of an organic diluent; 1. A sinterable conductive composition for producing a conductive film that provides electromagnetic interference (EMI) shielding protection to electronic components by applying a three-dimensional conductive coating to a top surface and sidewall of an electronic package by electrostatic, air, or ultrasonic spraying processes, comprising: Where: the particulate conductive filler is selected from the group consisting of gold, silver, copper, platinum, palladium, nickel, aluminum, indium, nickel alloys, zinc alloys, iron alloys, indium alloys, silver plated copper, silver plated aluminum, bismuth, tin, bismuth-tin alloys, silver plated fibers, silver plated graphite, silver plated silicon carbide, silver plated boron nitride, silver plated diamond, silver plated alumina, silver plated alloy 42, cadmium and its alloys, lead and its alloys, antimony and its alloys, and mixtures of two or more thereof; and the particulate conductive filler has a particle size in the range of 1 nm to 50 μm; the organic matrix comprises at least one thermoplastic and / or at least one thermosetting resin; and the organic diluent is selected from the group consisting of diethylene glycol n-butyl ether, butyl acetate, diethylene glycol monoethyl ether acetate (carbitol acetate), dipropylene glycol methyl ether, MEK, acetone, DBE-9, and mixtures of any two or more thereof; and When the composition is exposed to high temperatures of up to 250° C. and sintered, providing at least 20 dB of electromagnetic interference (EMI) shielding protection for the electronic package; When the composition is applied to a suitable three-dimensional substrate at a thickness of less than 25 μm, it has a viscosity of 1×10 -3 has a volume resistivity of less than ohm-cm; and A conductive composition having good adhesion to the substrate.
2. 10. The composition of claim 1 further comprising one or more of flow additives, adhesion promoters, rheology modifiers, toughening agents, fluxing agents, film softeners, phenolic novolac hardeners, epoxy cure catalysts, hardeners, and mixtures of two or more thereof.
3. 3. The composition of claim 1 or 2, wherein the organic matrix is selected from the group consisting of polyesters, polyacrylates, polyurethanes, phenoxys, polyethyloxazolines, polyvinylpyrrolidones, polyvinyl alcohols, polyacrylamides, polyglycols and polyacrylic acids, poly(ethylene glycols), aromatic vinyl polymers, polycarbonates, PC / ABS alloys, nylons, silicone polymers, siloxane polymers, polyolefins, vinyl polymers, polyamides, fluoropolymers, polyphenylene ethers, copolyestercarbonates, polyarylate ether sulfones or ketones, polyamideimides, polyetherimides, poly(ethylene terephthalate), poly(1,4-butylene terephthalate), polyethylene, polypropylene, polypropylene-EPDM blends, butadiene rubber, styrene-butadiene rubber, neoprene rubber, acrylonitrile butadiene styrene copolymers, polyetheresters, styrene / acrylonitrile polymers, polyphenylene sulfides, nitrile rubbers, cellulosic resins, and mixtures of any two or more thereof.
4. 3. The composition of claim 1 or 2, wherein the organic matrix comprises at least one thermosetting resin selected from the group consisting of epoxies, acrylates, maleimides, nadimides, itaconimides, cyanate esters, oxetanes, polyurethanes, polyimides, melamines, urea-formaldehyde resins, phenol-formaldehyde resins, and mixtures of two or more thereof.
5. An electromagnetic interference (EMI) shielding protective film for an electronic package comprising a reaction product obtained by drying, curing and / or sintering a composition described in any one of claims 1 to 4, the reaction product having a thickness of at least 1 μm and less than 25 μm.
6. 6. The electromagnetic interference (EMI) shielding protective film of claim 5, wherein the film has a thickness of less than 10 μm.
7. 6. The electromagnetic interference (EMI) shielding protective film of claim 5, wherein the film has a thickness of less than 5 μm.
8. An article comprising the electromagnetic interference (EMI) shielding protective film according to any one of claims 5 to 7 adhered to a suitable substrate.
9. 9. The article of claim 8, wherein the adhesion between the film and the substrate is at least Level 1B as determined by ASTM Standard Cross-Cut Tape Test according to test method D 3359-97.
10. An article comprising a substrate having a substantially uniform electromagnetic interference (EMI) shielding protective coating of the composition of any one of claims 1 to 4 on all exposed surfaces of an electronic package.
11. The article of claim 10, wherein the substrate is coated on the top and on its sidewalls.
12. The article of claim 10 , wherein the composition has been dried, cured and / or sintered.
13. 1. A method for making a conductive film that provides electromagnetic interference (EMI) shielding protection to an electronic component, comprising: Applying the composition according to any one of claims 1 to 4 to the electronic component; and Drying, curing and / or sintering the composition. A manufacturing method comprising:
14. 1. A method for providing electromagnetic interference (EMI) shielding protection to an electronic component, comprising: Applying the composition according to any one of claims 1 to 4 to the electronic component; and drying, curing and / or sintering the composition The method includes:
15. 1. A method for preparing a conductive network comprising the steps of: Applying the composition according to any one of claims 1 to 4 in a predetermined pattern to a suitable substrate, and then drying, curing and / or sintering the composition The method includes:
16. 20. A conductive network for electromagnetic interference (EMI) shielding protection for an electronic package produced by the method of claim 15.
17. 1x10 -3 20. The conductive network of claim 16 having a volume resistivity of no more than ohm-cm.
Citation Information
Patent Citations
Laminate, conductive base material using this laminate, and its manufacturing method
JP2011076866A
Conductive paste
JP2011187194A
Heat curable conductive paste composition
JP2013114837A
Method for producing silver microparticle, silver microparticle produced by the method for producing silver microparticle, and conductive paste containing the silver microparticle
JP2013159805A
Metallic paste and printing pattern formed using the same
JP2014049380A