Ion-exchanged glass with non-error function compressive stress profile and method for providing same
A three-step process for ion exchange glass enhances compressive stress and layer depth beyond conventional limits, addressing brittleness issues and improving damage resistance.
Patent Information
- Application Number
- JP2023078518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2012-02-29
- Filing Date
- 2023-05-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2033-02-27
AI Technical Summary
Existing ion exchange glass technologies are limited by the brittleness limit, which restricts the combination of high compressive stress and deep layer depth, leading to potential brittle behavior under aggressive conditions.
A three-step process involving ion exchange, heat treatment, and reion exchange to create a compressive stress profile that deviates from the conventional complementary error function, allowing higher surface compression and deeper layer depth while maintaining stress balance.
The method achieves a higher combination of compressive stress and layer depth below the brittle limit, enhancing damage resistance and passing handling tests, such as drop ball and ring-on-ring strength tests.
Smart Images

Figure 0007569883000009 
Figure 0007569883000010 
Figure 0007569883000011
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority under 35 U.S.C. §119 to U.S. Provisional Application No. 61 / 604,654, filed February 29, 2012, the contents of which are relied upon and incorporated by reference in their entirety herein. [Technical field]
[0002] The present invention relates to ion-exchanged glasses with non-error function compressive stress profiles and methods for providing same. [Background technology]
[0003] Chemical strengthening of glass (also called ion exchange (IOX)) involves the exchange of smaller cations (e.g., monovalent alkali metal cations, e.g., Li) in the glass at temperatures below the strain point of the glass. + and Na + ) and in an external medium, such as a molten salt bath, there are larger monovalent cations (e.g., K + ) exchange. The ion exchange process is used to impart a compressive stress profile that extends from the surface of the glass to a specific depth that follows a complementary error function. High compressive stress results in high strength in bending, as long as the depth of the compressive layer (depth of layer or "DOL") contains the flaw.
[0004] The stored compressive stress from both sides of the glass is balanced by stored tension, the allowable limits of which are determined by the brittleness limit for a given glass thickness. The limits of compressive stress and depth of layer are determined by various allowable combinations that follow a complementary error function and remain below the brittleness limit. The stored compressive stress is represented by the area under the complementary error function from the surface to the depth of layer. Summary of the Invention [Means for solving the problem]
[0005] The present disclosure provides glasses with compressive stress profiles that allow for higher surface compression and greater depth of layer (DOL) at a given level of stored tension than would be acceptable in glasses with stress profiles that follow a complementary error function. In some instances, there is a buried layer or a local maximum of increasing compression within the depth of layer that can redirect the crack system. These compressive stress profiles are achieved by a three-step process that includes a first ion-exchange step to create a compressive stress and depth of layer that follows a complementary error function, a heat treatment below the strain point of the glass to partially relieve the stress in the glass and allow the larger alkali ions to diffuse to greater depths, and a short re-ion exchange to re-establish the high compressive stress at the surface.
[0006] Accordingly, one aspect of the disclosure is to provide a glass having a surface and a thickness t, the glass including a first region under compressive stress extending from the surface to a depth of layer DOL in the glass, where the compressive stress CS has a maximum value CS1 at the surface and varies with distance d from the surface by a function other than the complementary error function, and a second region under tensile stress CT extending from the depth of layer into the glass.
[0007] A second aspect of the present disclosure is to provide an ion-exchanged glass having a surface and a thickness t. The glass includes a first layer under compressive stress CS extending to a depth of layer DOL within the glass. The first region includes a first segment in which the compressive stress CS varies according to a first function and a second segment in which the compressive stress CS varies according to a second function, where the first function is different from the second function.
[0008] A third aspect of the present disclosure is to provide a method of providing a glass having an in-layer compressive stress extending from a surface of the glass to a layer depth within the glass, the method including the steps of creating a first compressive stress and a first layer depth by ion exchanging the glass with a salt including a first cation, where the first compressive stress varies with distance within the glass according to a complementary error function, relaxing the stress within the glass to allow the first cation to diffuse deeper into the glass, and creating a second compressive stress at the surface by re-ion exchanging the glass with a salt including a first cation, where the compressive stress varies with distance according to a function other than the complementary error function.
[0009] These and other aspects, advantages, and salient features will become apparent from the following detailed description, the accompanying drawings, and the appended claims. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional schematic diagram of an ion-exchanged flat glass article. [Diagram 2] Plot of stress in ion-exchanged glass where the compressive stress follows the complementary error function. [Diagram 3] 11 is a schematic plot comparing example compressive stress profiles that do not follow the complementary error function with compressive stress profiles that follow the complementary error function. [Figure 4] 1 is a plot of the brittle limit CTlimit as a function of thickness t for conventional tempered glass having a compressive stress profile that follows the complementary error function. [Diagram 5] Plots of compressive stress versus thickness for 1) a glass sample ion-exchanged in KNO salt at 410°C for 8 hours; 2) a glass sample heat treated at 500°C for 90 minutes; and 3) a glass sample re-ion-exchanged in KNO salt at 410°C for 5 minutes. [Figure 6]Plots of compressive stress versus thickness for 1) a glass sample ion-exchanged in KNO3 salt at 410°C for 8 hours; 2) a glass sample heat treated at 500°C for 90 minutes; and 3) a glass sample re-ion-exchanged in KNO3 salt at 410°C for 30 minutes. [Figure 7] Plots of compressive stress versus thickness for 1) a glass sample ion-exchanged in KNO3 salt at 410°C for 8 hours; 2) a glass sample heat treated at 500°C for 90 minutes; and 3) a glass sample re-ion-exchanged in KNO3 salt at 410°C for 60 minutes. [Figure 8] Plots of compressive stress versus thickness for 1) a glass sample ion-exchanged in KNO3 salt at 410°C for 16 hours; 2) a glass sample heat treated at 500°C for 90 minutes; and 3) a glass sample re-ion-exchanged in KNO3 salt at 410°C for 60 minutes. [Figure 9] 13 is a plot of a modeled example of the compressive stress profile of ion-exchanged glass. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the following description, like reference characters refer to like or corresponding parts throughout the several figures shown in the drawings. It should also be understood that terms such as "upper", "lower", "outer", "inner" and the like are words of convenience and should not be construed as limiting terms, unless otherwise stated. Furthermore, whenever a group is described as comprising at least one of a group of elements and combinations thereof, it will be understood that the group can comprise, consist essentially of, or consist of any number of those elements listed, either individually or in combination with each other. Similarly, whenever a group is described as consisting of at least one of a group of elements and combinations thereof, it will be understood that the group can consist of any number of those elements listed, either individually or in combination with each other. Unless otherwise stated, a range of values includes both the lower and upper limits of the range, if any, as well as any range therebetween. As used herein, the singular form means "at least one" or "one or more" unless otherwise stated.
[0012] Referring generally to the drawings, and in particular to Figure 1, it will be understood that the figures are for purposes of illustrating particular embodiments and are not intended to limit the scope of the disclosure or the appended claims thereto. The drawings are not necessarily to scale, and certain features and particular views of the drawings may be shown exaggerated in scale or schematic for clarity and conciseness.
[0013] Chemical strengthening of glass, also called ion exchange (IOX), involves the addition of smaller cations (e.g., monovalent alkali metal cations, e.g., Li) to the glass at temperatures below the strain point of the glass. + and Na + ) and larger monovalent cations (e.g., K +) with ions. The ion exchange process is used to impart a compressive stress profile that extends from the surface of the glass to a specific depth that follows a complementary error function. High compressive stresses result in high strength in bending, as long as the flaw is contained within the depth of the compressive layer (depth of layer, or "DOL"). The stored compressive stresses from both surfaces of the glass are balanced by stored tension, the allowable limits of which are determined by the brittleness limit for a given glass thickness.
[0014] A cross-sectional schematic of an ion-exchanged planar glass article is shown in FIG. 1. The glass article 100 has a thickness t, a first surface 110, and a second surface 112. In some embodiments, the glass article 100 has a thickness t ranging from 0.05 mm to about 4 mm. Although the embodiment shown in FIG. 1 depicts the glass article 100 as a flat, planar sheet or plate, the glass article 100 may have other configurations, such as three-dimensional shapes or non-planar configurations. The glass article 100 has a first compressed layer 120 that extends from the first surface 110 into the bulk of the glass article 100 to a layer depth d1. In the embodiment shown in FIG. 1, the glass article 100 also has a second compressed layer 122 that extends from the second surface 112 to a second layer depth d2. The glass article 100 also has a central region 130 that extends from d1 to d2. The central region 130 is under tensile tension or central tension (CT) that balances or counteracts the compressive stresses in the first and second compressive layers 120, 122. The depths d1, d2 of the first and second compressive layers 120, 122 protect the glass article 100 from the propagation of scratches caused by sharp impacts to the first and second surfaces 110, 112 of the glass article 100, while the compressive stresses minimize the likelihood of scratches penetrating the depths d1, d2 of the first and second compressive layers 120, 122.
[0015] The limits of compressive stress and depth of layer are typically determined by various allowable combinations that follow a complementary error function and remain below the brittle limit. The stored compressive stress is represented by the area under the complementary error function from the surface to the depth of layer. As used herein, the terms "depth of layer" and "DOL" refer to the zero stress point where the surface compressive layer first transitions into tension. FIG. 2 is a plot of the stress of an ion-exchanged glass in the first compressive layer 120, where the compressive stress follows a complementary error function 200. The compressive stress has a maximum value at the surface of the glass (depth=0 μm) and decreases at a constant rate through the first compressive layer 120 until it reaches the depth of layer DOL where the compressive stress transitions into tension and the total stress equals zero.
[0016] A deep compressive layer provides damage resistance, i.e., the ability to maintain strength when more violent contact with the glass results in greater flaw depth. While it may be desirable to achieve both high compressive stress and deep compressive layer depth, the limit is set by the transition to brittle behavior when the stored energy exceeds a safe limit, referred to herein as the "brittle limit." The stored compressive stress is represented by the area A under the complementary error function 200 from the surface to the layer depth. The stored compressive stress from both surfaces is balanced by the stored central tension CT, the allowable limit of which is set by the brittle limit for a given glass thickness. The limit of compressive stress and layer depth is set by various allowable combinations that follow the complementary error function 200 and remain below the brittle limit.
[0017] As described herein, chemically strengthened - i.e., ion-exchanged - glasses are provided that are damage resistant for applications such as, but not limited to, cover glass for portable and stationary electronic devices, architectural and automotive glazing / windows, and glass containers, which have a first region under compressive stress (e.g., first and second compressive layers 120, 122, etc., of FIG. 1) extending from the surface of the glass to a depth of layer DOL, and a second region under tensile stress or central tension CT (e.g., central region 130, etc., of FIG. 1) extending from the depth of layer into a central or interior region of the glass.
[0018] The compressive stress CS has a maximum compressive stress CS1 at its surface and a compressive stress that varies with distance d from the surface according to a function different (i.e., other than) than the complementary error function. Examples of such compressive stress functions 310, 320 of possible compressive stress profiles in glasses described herein are shown diagrammatically in Figure 3 and compared with the complementary error function. With particular reference to the compressive stress function 320, the region 120 (Figure 1) includes a first segment 120a, in which the compressive stress function 320 is a first complementary error function, and a second segment 120b, located between the first segment 120a and the central region 130, in which the compressive stress follows a second function different from the first complementary error function.
[0019] As used herein, the terms "error function" and "Erf" refer to the function that is twice the integral of the normalized Gaussian function between 0 and x / σ√2, and "complementary error function" and "Erfc" is equal to 1 minus the error function, i.e., Erfc(x) = 1 -Erf(x).
[0020] The first segment 120a is at a depth d from the first surface 110. 120a, creating a surface compression or compressive stress CS of the glass 100. In some embodiments, the compressive stress is at least about 400 MPa, in other embodiments at least about 600 MPa, and in still other embodiments at least about 800 MPa. The depth of layer DOL of each of the first and second compressive layers 120, 122 is at least about 50 μm, and in some embodiments at least about 100 μm.
[0021] The function of the second segment 120b may include a second complementary error function, a spread tail, or the like. 120b and the depth of layer DOL. Each of the compressive stress functions 310, 320 in Figure 3 has at least one inflection point, where the compressive stress reaches a local maximum CS2 and / or a local minimum CS3 below the surface 110 of the glass. In some embodiments, the first compressive layer 120 can include three or more segments, where each segment has a compressive stress that follows a function other than the function that characterizes an adjacent segment.
[0022] The stored compressive stresses at both major surfaces (110, 112 in FIG. 1) are balanced by the stored tension in the central region of the glass (130), the allowable limits of which are determined by the brittleness limit for a given glass thickness. Brittleness limit and brittleness are described in U.S. Patent No. 8,075,999, filed Aug. 7, 2009 by Kristen L. Barefoot et al., entitled "Strengthened Glass Articles and Method of Making," which claims priority to U.S. Provisional Patent Application No. 61 / 087,324, filed Aug. 8, 2008, the contents of which are incorporated herein by reference in their entirety. As described in U.S. Patent No. 8,075,999, brittle or brittle behavior is characterized by at least one of the following: fracture of the strengthened glass article (e.g., plate or sheet) into multiple small pieces (e.g., 1 mm); the number of fragments formed per unit area of the glass article; multiple cracks branching from an initial crack in the glass article; and violent ejection of at least one fragment a certain distance (e.g., about 5 cm, or about 2 inches) from the original location; and any combination of the aforementioned fracture (size and density), crack, and ejection behavior. The terms "brittle behavior" and "brittleness" refer to those modes of violent or forceful fragmentation in a strengthened glass article that does not have any external durables, such as coatings, adhesive layers, or the like. Although coatings, adhesive layers, and the like can be used with the strengthened glass described herein, such external durables are not used in identifying the brittle or brittle behavior of the glass article.
[0023] The limits of compressive stress CS and depth of layer DOL are determined by various allowable combinations that follow the complementary error function and remain below the brittle limit. Figure 4 shows the brittle limit CT as a function of thickness t for conventional tempered glass with a compressive stress profile that follows the complementary error function as taught by U.S. Pat. No. 8,075,999. limit4 is a plot of the glass article being brittle above the line shown in FIG. 4. The central tension, CT, is given by the following equation:
[0024]
number
[0025] can be determined from the compressive stress CS, the depth of layer DOL, and the thickness t of the glass by using the formula: limit is the following formula:
[0026]
number
[0027] where CT limit , the glass thickness t is expressed in millimeters (mm), where t≦1 mm, and ln(t) is the natural logarithm (base e) of the thickness t.
[0028] Therefore, to keep conventionally strengthened glass with a complementary error function compressive stress profile below the brittle limit, a CS and DOL as shown in Equation 3 below are required.
[0029]
number
[0030] The glasses and methods described herein provide a compressive stress profile that allows for a combination of higher surface compressive stress and greater layer depth than would otherwise be acceptable when using a complementary error function profile. As shown in Equation 3, CT limitis still calculated from the traditional complementary error function profile triangular approximation, but the central tension CT of the glass described herein is calculated as CT limit It can exceed.
[0031]
number
[0032] The glasses described herein may include or consist of any glass that has been chemically strengthened by ion exchange. In some embodiments, the glass is an alkali aluminosilicate glass.
[0033] In one embodiment, the alkali aluminosilicate glass comprises about 64 mol% to about 68 mol% SiO2; about 12 mol% to about 16 mol% Na2O; about 8 mol% to about 12 mol% Al2O3; 0 mol% to about 3 mol% B2O3; about 2 mol% to about 5 mol% K2O; about 4 mol% to about 6 mol% MgO; and 0 mol% to about 5 mol% CaO, in which case the alkali aluminosilicate glass comprises about 64 mol% to about 68 mol% SiO2; about 12 mol% to about 16 mol% Na2O; about 8 mol% to about 12 mol% Al2O3; 0 mol% to about 3 mol% B2O3; about 2 mol% to about 5 mol% K2O; In this case, 66 mol%≦SiO2+B2O3+CaO≦69 mol%; Na2O+K2O+B2O3+MgO+CaO+SrO>10 mol%; 5 mol%≦MgO+CaO+SrO≦8 mol%; (Na2O+B2O3)-Al2O3≧2 mol%; 2 mol%≦Na2O-Al2O3≦6 mol%; and 4 mol%≦(Na2O+K2O)-Al2O3≦10 mol%. Such glasses are described in U.S. Pat. No. 7,666,511, filed Jul. 27, 2007 by Adam J. Ellison et al. and entitled "Down-Drawable, Chemically Strengthened Glass for Cover Plate," which claims priority to U.S. Provisional Patent Application No. 60 / 930,808, filed May 18, 2007, the contents of which are incorporated herein by reference in their entirety.
[0034] In another embodiment, the alkali aluminosilicate glass comprises at least one of alumina and boron oxide, and at least one of alkali metal oxides and alkaline earth metal oxides, where −15 mol%≦(R2O+R′O-Al2O3-ZrO2)-B2O3≦4 mol%, where R is one of Li, Na, K, Rb, and Cs, and R′ is one of Mg, Ca, Sr, and Ba. In some embodiments, the alkali aluminosilicate glass includes about 62 mol% to about 70 mol% SiO2; 0 mol% to about 18 mol% Al2O3; 0 mol% to about 10 mol% B2O3; 0 mol% to about 15 mol% Li2O; 0 mol% to about 20 mol% Na2O; 0 mol% to about 18 mol% K2O; 0 mol% to about 17 mol% MgO; 0 mol% to about 18 mol% CaO; and 0 mol% to about 5 mol% ZrO2. The glass is described in U.S. patent application Ser. No. 12 / 277,573, filed Nov. 25, 2008 by Matthew J. Dejneka et al. and entitled "Glasses Having Improved Toughness And Scratch Resistance," which claims priority to U.S. Provisional Patent Application Ser. No. 61 / 004,677, filed Nov. 29, 2008, the contents of which are incorporated herein by reference in their entirety.
[0035] In another embodiment, the alkali aluminosilicate glass comprises about 60 mol% to about 70 mol% SiO2; about 6 mol% to about 14 mol% Al2O3; 0 mol% to about 15 mol% B2O3; 0 mol% to about 15 mol% Li2O; 0 mol% to about 20 mol% Na2O; 0 mol% to about 10 mol% K2O; 0 mol% to about 8 mol% MgO; 0 mol% to about 10 mol% CaO; 0 mol% to about 5 mol% ZrO2; 0 mol% to about 1 mol% SnO2; 0 mol% to about 1 mol% CeO2; less than about 50 ppm As2O3; and less than about 50 ppm Sb2O3, where 12 mol%≦Li2O+Na2O+K2O≦20 mol% and 0 mol%≦MgO+CaO≦10 mol%. Such glasses are described in U.S. patent application Ser. No. 12 / 392,577, filed Feb. 25, 2009 by Sinue Gomez et al. and entitled "Fining Agents for Silicate Glasses," which claims priority to U.S. Provisional Patent Application Ser. No. 61 / 067,130, filed Feb. 26, 2008, the contents of which are incorporated herein by reference in their entirety.
[0036] In another embodiment, the alkali aluminosilicate glass comprises SiO and NaO, where the glass is cooled to a temperature T at which the glass has a viscosity of 35 kpoise. 35kp where the temperature T at which zircon breaks down to form ZrO2 and SiO2 breakdown is T 35kpIn some embodiments, the alkali aluminosilicate glass comprises about 61 mol% to about 75 mol% SiO2; about 7 mol% to about 15 mol% Al2O3; 0 mol% to about 12 mol% B2O3; about 9 mol% to about 21 mol% Na2O; 0 mol% to about 4 mol% K2O; 0 mol% to about 7 mol% MgO; and 0 mol% to about 3 mol% CaO. The glass is described in U.S. Patent Application Serial No. 12 / 856,840, entitled "Zircon Compatible Glasses for Down Draw," filed August 10, 2010 by Matthew J. Dejneka et al., which claims priority to U.S. Provisional Patent Application Serial No. 61 / 235,762, filed August 29, 2009, the contents of which are incorporated herein by reference in their entirety.
[0037] In another embodiment, the alkali aluminosilicate glass comprises at least 50 mol% SiO2 and at least one modifier selected from the group consisting of alkali metal oxides and alkaline earth metal oxides, where [(Al2O3 (mol %) + B2O3 (mol %)) / (ΣAlkali metal modifier (mol %))]>1. In some embodiments, the alkali aluminosilicate glass comprises 50 mol% to about 72 mol% SiO2; about 9 mol% to about 17 mol% Al2O3; about 2 mol% to about 12 mol% B2O3; about 8 mol% to about 16 mol% Na2O; and 0 mol% to about 4 mol% K2O. The glass is described in U.S. patent application Ser. No. 12 / 858,490, filed Aug. 18, 2010 by Kristen L. Barefoot et al. and entitled "Crack And Scratch Resistant Glass and Enclosures Made Therefrom," which claims priority to U.S. Provisional Patent Application Ser. No. 61 / 235,767, filed Aug. 21, 2009, the contents of which are incorporated herein by reference in their entirety.
[0038] In another embodiment, the alkali aluminosilicate glass comprises SiO, AlO, PO, and at least one alkali metal oxide (R0), where 0.75≦[(P0(mol%)+R0(mol%)) / M0(mol%)]≦1.2, where M0=AlO+B0. In some embodiments, the alkali aluminosilicate glass comprises about 40 mol% to about 70 mol% SiO; 0 mol% to about 28 mol% B2O3; 0 mol% to about 28 mol% Al2O3; about 1 mol% to about 14 mol% P2O5; and about 12 mol% to about 16 mol% R2O, and in certain embodiments, about 40 mol% to about 64 mol% SiO2; 0 mol% to about 8 mol% B2O3; about 16 mol% to about 28 mol% Al2O3; about 2 mol% to about 12% P2O5; and about 12 mol% to about 16 mol% R2O. The glass is described in U.S. patent application Ser. No. 13 / 305,271, filed Nov. 28, 2011 by Dana C. Bookbinder et al. and entitled "Ion Exchangeable Glass with Deep Compressive Layer and High Damage Threshold," which claims priority to U.S. Provisional Patent Application Ser. No. 61 / 417,941, filed Nov. 30, 2010, the contents of which are incorporated herein by reference in their entirety.
[0039] In yet another embodiment, the alkali aluminosilicate glass comprises at least about 4 mol % P2O5, where (M2O3 (mol %) / R X O (mol%) < 1, M2O3 = Al2O3 + B2O3, R XO is the sum of monovalent and divalent cation oxides present in the alkali aluminosilicate glass. In some embodiments, the monovalent and divalent cation oxides are selected from the group consisting of Li2O, Na2O, KO, Rb2O, Cs2O, MgO, CaO, SrO, BaO, and ZnO. In some embodiments, the glass contains 0 mol% B2O3. The glass is described in U.S. Provisional Patent Application No. 61 / 560,434, filed November 16, 2011 by Timothy M. Gross and entitled "Ion Exchangeable Glass with High Crack Initiation Threshold," the contents of which are incorporated herein by reference in their entirety.
[0040] In yet another embodiment, the alkali aluminosilicate glass comprises at least about 50 mol% SiO2 and at least about 11 mol% Na2O and has a compressive stress of at least about 900 MPa. In some embodiments, the glass further comprises Al2O3 and at least one of B2O3, K2O, MgO, and ZnO, where -340+27.1·Al2O3-28.7·B2O3+15.6·Na2O-61.4·K2O+8.1·(MgO+ZnO)≧0 mol%. In certain embodiments, the glass comprises about 7 mol% to about 26 mol% Al2O3; 0 mol% to about 9 mol% B2O3; about 11 mol% to about 25 mol% Na2O; 0 mol% to about 2.5 mol% K2O; 0 mol% to about 8.5 mol% MgO; and 0 mol% to about 1.5 mol% CaO. The glass is described in U.S. Provisional Patent Application No. 61 / 503,734, filed July 1, 2011 by Matthew J. Dejneka et al. and entitled "Ion Exchangeable Glass with High Compressive Stress," the contents of which are incorporated herein by reference in their entirety.
[0041] In some embodiments, the alkali aluminosilicate glasses described above are substantially free (i.e., contain 0 mol %) of at least one of lithium, boron, barium, strontium, bismuth, antimony, and arsenic.
[0042] In some embodiments, the alkali aluminosilicate glasses described above are downdrawable by processes known in the art, such as slot draw, fusion draw, redraw, and the like, and have a liquidus viscosity of at least 130 kilopoise.
[0043] Also provided is a method for providing a glass, such as the glasses described above, having a compressive stress profile that does not follow a complementary error function. The glass is first ion-exchanged with an ion-exchange medium. The ion-exchange medium may be a molten salt bath, gel, paste, or the like, and includes a salt that includes a first cation. The first cation displaces smaller second cations in the glass to a first depth of layer, creating a first compressive stress within the first depth of layer. The first compressive stress varies with distance into the glass according to a complementary error function. This process can be modified to fix the starting compressive stress and depth of layer at any desired level, and the brittle limit CT limit There is no need to be bound by
[0044] After ion exchange, the surface compressive stress is relieved and the first ions diffuse deeper into the glass to a second depth deeper than the first depth. In some embodiments, this step includes heating the glass below the strain point of the glass. Heating the ion-exchanged glass to this temperature results in a compressive stress maximum at a depth below the surface, i.e., a compressive stress maximum that is "buried" below the surface of the glass.
[0045] After the step of relieving the surface compressive stress of the glass, the glass is again ion-exchanged to re-establish the surface compressive stress. As with the first ion-exchange step, the ion-exchange is carried out by contacting the glass with a medium, which may be a molten salt bath, gel, paste, or the like, and which contains a salt containing a first cation to create a second surface compressive stress in the glass. In some embodiments, the second ion-exchange is carried out for a shorter period of time than the first ion-exchange.
[0046] The resulting compressive stress profile (i.e., change in compressive stress C) after the second ion exchange of the glass may vary according to a function other than (and different from) the complementary error function, and may take the form of the function shown in the accompanying figures previously described above.
[0047] The glasses and methods described herein achieve a higher combination of CS and DOL while remaining below the brittle limit. In cases where an increase and maximum in embedded compressive stress is achieved, reorientation of the crack system may result. Higher compressive stress may also allow the glass to pass handling tests, ball drop tests, and as-built ring-on-ring strength tests. A greater layer depth also provides damage resistance, i.e., the ability to maintain strength when more violent contact results in greater scratch depth. EXAMPLES
[0048] The following examples illustrate features and advantages of the glasses and methods described herein, and are not intended to limit the scope of the disclosure or the appended claims thereto.
[0049] Four examples of glasses with the following nominal compositions were prepared and ion-exchanged according to the methods described herein to achieve stress profiles that do not follow a single complementary error function. Stress measurements and depth profiles were made using interferometry on 650 μm diameter rods of ion-exchanged glass. The method was limited to measuring stress within the first 5-10 μm of the rod. Corrections for surface compression were made using FSM measurements on 1.3 mm thick flat glass samples.
[0050] The method consists of three steps. The first step is to ion exchange the glass to have a standard complementary error function stress profile. Step 1 of the ion exchange for the samples shown in Figures 4-6 was an immersion treatment in a KNO3 salt bath at 410°C for 8 hours, which resulted in a typical complementary error function profile for each sample with a DOL of 44 microns and a CS of 595 MPa. This treatment resulted in a depth of layer (DOL) of about 44 μm and a compressive stress (CS) of about 595 MPa, however step 1 can be modified to fix the starting CS and DOL at any desired level, as well as a central tension CT determined by brittleness testing. limit You don't need to be bound by.
[0051] In step 2, the ion-exchanged glass sample was heat treated below the strain point of the glass for a desired time to promote potassium diffusion to expand the depth of the DOL while simultaneously relieving the surface compressive stress of the sample. This step resulted in a maximum of embedded compressive stress below the surface of the glass rather than at the surface. The sample shown in Figures 5-7 was heat treated at 500°C for 90 minutes in a N2 atmosphere, which resulted in an expansion of the DOL beyond that achieved in step 1. The selection of heat treatment temperature and time will depend on the rate of stress relaxation and rate of diffusion for a given glass composition at a given temperature.
[0052] In step 3, a second ion exchange for a shorter time re-establishes the surface compressive stress. In Figure 5, a second ion exchange at 410 °C for 5 min resulted in a spike of CS at the surface and a buried region of increased CS by overlaying the profiles from steps 2 and 3. Step 3 also resulted in a buried compressive layer with a total DOL of about 64 μm and a CS of about 684 MPa.
[0053] In Figure 6, a second ion exchange at 410°C for 30 min resulted in a higher CS at the surface and a shoulder appeared from the overlay of the profiles from steps 2 and 3. Step 3 also resulted in a buried compression layer with a total DOL of about 59 microns and a CS of about 744 MPa.
[0054] In Figure 7, a second ion exchange at 410°C for 60 minutes resulted in a profile with a spike of surface CS extending deeper into the glass. Step 3 also resulted in a buried compression layer with a total DOL of about 55 microns and a CS of about 749 MPa.
[0055] The glass sample shown in FIG. 8 was ion-exchanged in KNO3 salt at 450° C. for 16 hours in step 1, resulting in a typical complementary error function profile. In step 2, the glass sample was heat-treated at 500° C. for 90 minutes to relieve compressive stress at the surface and promote potassium ion diffusion to deeper depths, resulting in a deeper compressive layer depth. In step 3, the sample was re-ion-exchanged in KNO3 salt at 410° C. for 60 minutes to re-establish high surface compression. Step 3 also resulted in a buried compressive layer with a total DOL of about 90 μm and a CS of about 740 MPa.
[0056] A modeled example of the compressive stress profile for flat glass is shown in Figure 9. The total stress A, expressed as a function of depth L, A(L), can be written as:
[0057]
number
[0058] The term A1 is the peak compressive stress after the first ion exchange step, not considering the contribution of the stress relaxation effect, CT1 is the compressive stress after the first ion exchange step and the subsequent relaxation step, and b1 and Erf(L / b1) are the depth of the ion exchanged layer and the error function of the stress profile associated with the first ion exchange step, respectively. The term b2 is the depth of the stress relaxation after the first ion exchange step. A2 is the peak compressive stress after the stress relaxation step after the first ion exchange step. The terms b3 and CT2 are the depth of the ion exchanged layer and the central tension adjustment after the second ion exchange step, respectively.
[0059] The central tension CT1 after the first ion exchange and subsequent relaxation step can be calculated using equation (1) as follows:
[0060]
number
[0061] where the compressive stress CS1 is the peak value or maximum of the compressive stress "embedded" (i.e., located below the surface of the glass) in DOL2 of the compressive layer (X in FIG. 9). After the second ion-exchange step, the central tension decreases to a second value CT2, CS1 and DOL1 decrease to CS1-1 and DOL1-1, respectively, and the maximum compressive stress CS2 is achieved at the surface (thickness=0).
[0062]
number
[0063] In some embodiments, the total tensile stress CT = CT1 + CT2 is the brittle limit CT limit (Equation (3)). The total tensile stress CT is obtained by combining equations (6) and (7).
[0064]
number
[0065] An embodiment of the disclosure is a glass having a surface and a thickness t, the glass including a first region under compressive stress extending in the glass from the surface to a depth of layer DOL, where the compressive stress CS has a maximum value CS1 at the surface and varies with distance d from the surface according to a function other than a complementary error function, and a second region under tensile stress CT extending from the depth of layer into the glass.
[0066] As another aspect of the present disclosure, the first region may be a glass including: a. a first segment extending from the surface to a first depth d1, the depth d1 being less than the depth of layer DOL, and the compressive stress Cs varying according to a first function; and b. a second segment extending from the first depth d1 to the depth of layer DOL, the compressive stress Cs varying according to a second function, the first function being different from the second function. Another aspect of the present disclosure may be a glass in which the first function is a first complementary error function.
[0067] In another aspect of the present disclosure, the second function may be a second complementary error function or a diffusion tail.
[0068] Another embodiment of the present disclosure may be a glass in which the compressive stress has a maximum CS2 in the second segment. Another embodiment of the present disclosure may be a glass in which CS1>CS2. Another embodiment of the present disclosure may be glass in which the tensile stress CT expressed in MPa is equal to or greater than −36.71n(t)(MPa)+48.7(MPa). In another aspect of the present disclosure, the glass may be an alkali aluminosilicate glass.
[0069] Another embodiment of the present disclosure may be a glass having a maximum compressive stress CS1 of at least about 400 MPa.
[0070] Yet another aspect of the present disclosure is a method of providing a glass having a compressive stress in a layer extending from a surface of the glass to a layer depth, the method comprising: creating a first compressive stress and a first layer depth by ion exchanging the glass with a salt comprising a first cation, wherein the first compressive stress varies with distance within the glass according to a complementary error function; heating the glass below a strain point of the glass to relieve stress in the glass and cause the first cation to diffuse deeper into the glass; and creating a second compressive stress at the surface by re-ion exchanging the glass with a salt comprising the first cation, wherein the second compressive stress varies with distance according to a function other than the complementary error function.
[0071] Although exemplary embodiments have been described in detail for purposes of illustration, the foregoing description should not be deemed a limitation on the scope of the disclosure or the appended claims. Thus, various modifications, adaptations, and substitutions may occur to those skilled in the art without departing from the spirit and scope of the disclosure or the appended claims. [Explanation of symbols]
[0072] 100 Glass items 110 First surface 112 Second surface 120 First Compression Layer 122 Second Compression Layer 130 Central area 200 Complementary Error Function 120a First Segment 120b Second Segment 310 Compressive Stress Function 320 Compressive Stress Function
Claims
1. A glass having a surface and a thickness t in the range of 0.05 mm to 1.3 mm, A first region under compressive stress extending from the surface to a depth of layer DOL in the glass, the compressive stress CS having a maximum value CS 1 and varies with distance d from the surface, said compressive stress CS having a maximum compressive stress CS 1 of at least 400 MPa, and said depth of layer DOL being at least 50 μm; a second region under tensile stress CT extending from said layer depth into said glass, wherein a value CT C determined by trigonometric approximation for said second region is equal to [(CS 1 ·DOL) / (t−2·DOL)], CT C being expressed in MPa and being greater than −37.6ln(t)(MPa)+48.7(MPa); Including, the second region further has an achieved central tension CT A , where CT A is expressed in MPa and is less than or equal to −37.6ln(t)(MPa)+48.7(MPa); The first region is a. a first segment extending from the surface to a first depth d1, the depth d1 being less than the depth of layer DOL, the compressive stress CS varying in the first segment according to a first function, the first function being a first complementary error function; b. a second segment extending from the first depth d1 to the depth of layer DOL, in which the compressive stress CS varies according to a second function, the second function being different from the first function; Including, Glass.
2. The glass of claim 1, wherein the second function is a second complementary error function.
3. The glass of claim 1, wherein the glass is an alkali aluminosilicate glass having an alkali metal oxide, the alkali metal being Na or K.
4. The glass of claim 1, wherein the glass is ion-exchanged.
5. The glass of claim 1, wherein the glass is non-brittle.
Citation Information
Patent Citations
Glass with a compression surface for consumer use
JP2011527661A
Tempered glass articles and methods for manufacturing the same
JP2011530470A
Variable temperature / continuous ion exchange process
WO2011149812A1