High strength thick hot rolled steel sheet with excellent elongation ratio and its manufacturing method

By controlling steel composition and hot rolling and cooling conditions, the method achieves uniform microstructure and improved durability in high-strength thick hot-rolled steel sheets, addressing non-uniformity and crack propagation issues in existing technologies.

JP7569928B2Active Publication Date: 2024-10-18POHANG IRON & STEEL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023516788
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-25
Filing Date
2021-09-16
Publication Date
2024-10-18
Estimated Expiration
2041-09-16

AI Technical Summary

Technical Problem

Existing methods for manufacturing high-strength thick hot-rolled steel sheets face challenges in achieving uniform microstructure distribution in the thickness direction, leading to non-uniform stress concentration, increased crack propagation, and reduced durability due to segregation and non-uniformity of microstructure, especially in thicker materials.

Method used

A method involving controlled steel composition (C: 0.05~0.15%, Si: 0.01~1.0%, Mn: 1.0~2.0%, Sol.Al: 0.01~0.1%, Cr: 0.005~1.0%, P: 0.001~0.02%, S: 0.001~0.01%, N: 0.001~0.01%, Nb: 0.005~0.07%, Ti: 0.005~0.11%) and specific hot rolling and cooling conditions to ensure a uniform microstructure, including reheating to 1200 to 1350°C, finish hot rolling at controlled temperatures, and cooling rates between 450 to 550°C with air or water cooling.

Benefits of technology

The method results in high-strength thick hot-rolled steel sheets with tensile strength of 590 MPa or more and elongation ratio of 30% or more, ensuring uniform microstructure and improved durability by minimizing segregation and non-uniformity, with a El×TS×0.5Hv max /ΔH value of 140,000 or more.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569928000005
    Figure 0007569928000005
  • Figure 0007569928000006
    Figure 0007569928000006
  • Figure 0007569928000007
    Figure 0007569928000007
Patent Text Reader

Abstract

The present invention provides a high-strength, thick, hot-rolled steel sheet having an excellent elongation ratio and a method for manufacturing the same. The high-strength, thick, hot-rolled steel sheet contains, by weight %, 0.05-0.15% C, 0.01-1.0% Si, 1.0-2.0% Mn, 0.01-0.1% Sol.Al, 0.005-1.0% Cr, 0.001-0.02% P, 0.001-0.01% S, 0.001-0.01% N, 0.001-0.01% Nb, 0.005-0.07% Ti, and the remainder being iron and inevitable impurities, and satisfies the following [Relational Formula 1], and by area %, 25-50% polygonal ferrite, 30-50% bainitic ferrite + acicular ferrite, and 20% or less bainite. 2 The total area fraction of carbides and pearlite structures with a diameter of 0.5 μm or more observed within the steel sheet is less than 5%, and the fine structure contains less than 5% of MA phase (Martensitic-austenitic constituents).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a manufacturing method for a high-strength hot-rolled steel sheet having a thickness of 10 to 14 mm, which is mainly used for structural components such as wheel discs, wheel rims, members, and frames of commercial vehicles. More specifically, the present invention relates to a high-strength thick hot-rolled steel sheet having an excellent tensile strength of 590 MPa or more and an elongation rate of 30% or more, and therefore, no cracks are generated during molding of parts such as wheel discs, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, plate materials with a thickness of 13 to 20 mm and a tensile strength of 440 MPa or more have been mainly used for structural members of commercial vehicles and heavy equipment, but in recent years, as part of efforts to reduce weight by using high-strength, thin steel materials, a technology has been developed that uses high-strength steel materials with a tensile strength of 590 MPa or more and a thickness of 10 to 15 mm. However, when manufacturing such high-strength thick steel materials using a hot rolling process, it is difficult to ensure a uniform microstructure in the thickness direction when utilizing a transformed structure. As a result, it is difficult to ensure stable ductility and yield strength, cracks are likely to occur during the manufacturing of parts, and local stress concentration occurs during use, resulting in a problem of reduced durability life.

[0003] In relation to this, a technique has been proposed in which conventional steel materials are subjected to normal hot rolling in the austenite region, then coiled at high temperature to make the ferrite phase the base structure, and fine precipitates are formed to ensure strength and ductility (Patent Document 1), and a technique in which rolling is performed so as not to form coarse pearlite structures, and then the coiling temperature is cooled through two cooling steps to a temperature at which the bainite phase is formed before coiling (Patent Document 2).In addition, a technique has been proposed in which Ti, Nb, etc. are used to reduce the austenite grains by a large reduction of 40% or more in the non-recrystallized region during hot rolling to refine the austenite grains (Patent Document 3).

[0004] However, although the alloy elements such as Si, Mn, Al, Mo, and Cr mainly used in the above technology to manufacture thick high-strength steel are effective in improving strength, excessive addition of the alloy elements leads to segregation and uneven microstructure, deteriorating formability. In addition, fine cracks generated on the shear surface are easily propagated in a fatigue environment, causing damage to the part. In particular, as the thickness increases, the unevenness of the microstructure between the surface and deeper layers increases, increasing local stress concentration, and the propagation speed of cracks in a fatigue environment also increases, deteriorating durability.

[0005] In addition, in order to refine the crystal grains of thick steel sheets and obtain the effect of precipitation strengthening, it is effective to utilize precipitate-forming elements such as Ti, Nb, and V. However, unless the steel sheet is coiled at a high temperature of 500 to 700°C, at which precipitates are likely to form, or the cooling rate of the steel sheet is not controlled during cooling after hot rolling, coarse carbides are formed in the center of the thickness of the thick steel sheet, deteriorating the quality of the sheared surface.

[0006] When the coiling temperature is cooled to a temperature at which the bainite phase is formed to prevent the formation of coarse pearlite structures, the two-stage cooling control method is restricted by the length of the ROT section, but the smaller the unit weight required by the client, the more of a limit there is to how effective the method can be over the entire length of the coil. In addition, controlling the cooling rate value during primary cooling to a level of 70°C / sec places a heavy load on the equipment, which directly leads to reduced productivity. Furthermore, applying a large reduction of 40% in the unrecrystallized region during hot rolling deteriorates the shape quality of the rolled sheet and places a load on the equipment, making it difficult to actually apply the method. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 2002-322541 [Patent Document 2] Korean Patent Publication No. 10-2020-0062422 [Patent Document 3] Japanese Patent Publication No. 1997-143570 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention aims to provide a thick hot-rolled steel sheet having excellent strength and ductility and a constant hardness distribution in the thickness direction by controlling the steel composition, hot rolling and cooling conditions to ensure a uniform distribution of microstructure in the thickness direction of the steel material, and a manufacturing method thereof.

[0009] The object of the present invention is not limited to the above. The object of the present invention can be understood from the overall content of this specification, and a person having ordinary knowledge in the technical field to which the present invention belongs will have no difficulty in understanding further object of the present invention. [Means for solving the problem]

[0010] One aspect of the present invention is a steel sheet containing, by weight%, 0.05-0.15% C, 0.01-1.0% Si, 1.0-2.0% Mn, 0.01-0.1% Sol.Al, 0.005-1.0% Cr, 0.001-0.02% P, 0.001-0.01% S, 0.001-0.01% N, 0.005-0.07% Nb, 0.005-0.11% Ti, with the remainder being iron and unavoidable impurities, and satisfying the following [Relational Formula 1], and by area%, 25-50% polygonal ferrite, 30-50% bainitic ferrite + acicular ferrite, 20% or less bainite, and 2 The present invention relates to a high-strength thick hot-rolled steel sheet having a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more, and a fine structure including less than 5% of the total area fraction of carbides and pearlite structures with diameters of 0.5 μm or more observed in the steel sheet, and less than 5% of MA phase (Martensitic-austenitic constituents).

[0011] [Equation 1] 0.3≦R≦1.0 R=[C]*+0.7×[Mn]+8.5×[P]+7.5×[S]-0.9×[Si]-1.5×[Nb] [C]*=[C]-[C]×Q Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) In the above formula (1), C, Mn, P, S, Si, Nb, and Ti are the weight percent of the alloying elements.

[0012] The above hot-rolled steel sheets are El×TS×0.5Hv max / ΔH value can be 140,000 or more.

[0013] Another aspect of the present invention relates to a method for producing a high-strength thick hot-rolled steel sheet having a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation of 30% or more, the method including the steps of: reheating a steel slab having the above-mentioned composition and satisfying the following [Relational Formula 1] to 1200 to 1350°C; finish hot rolling the reheated steel slab in a temperature range satisfying the following [Relational Formula 2]; cooling the finish hot-rolled steel sheet to a temperature in the range of 450 to 550°C at a cooling rate that satisfies the following [Relational Formula 3], and then coiling the steel sheet at a temperature in the range of 400 to 550°C; and air-cooling or water-cooling the coiled steel sheet to a temperature in the range of room temperature to 200°C.

[0014] [Equation 1] 0.3≦R≦1.0 R=[C]*+0.7×[Mn]+8.5×[P]+7.5×[S]-0.9×[Si]-1.5×[Nb] [C]*=[C]-[C]×Q Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) In the above formula 1, C, Mn, P, S, Si, Nb, and Ti are the weight percent of the alloying elements.

[0015] [Equation 2] Tn-70≦FDT≦Tn Tn=750+92×[C]+70×[Mn]+45×[Cr]+647×[Nb]+515×[Ti]-50×[Si]-2.4×(t-5) In the above formula 2, C, Mn, Cr, Nb, Ti, and Si are the weight percent of the alloying elements. FDT in the above formula 2 is the temperature of the hot-rolled sheet at the end of hot rolling (℃) In the above formula 2, t is the thickness of the final rolled plate material (mm).

[0016] [Equation 3] CR Min ≦CR*≦60 CR Min =65-157×[C]-25.2×[Si]-14.1×[Mn]-27.3×[Cr]+61×[Ti]+448×[Nb]+1.4×(t-5) In the above formula 3, C, Si, Mn, Cr, Ti, and Nb are the weight percent of the alloying elements. CR* in the above formula 3 is the cooling rate (℃ / sec) when cooling the plate material after hot rolling.

[0017] After the air or water cooling, the method may further include pickling and oiling the steel sheet. Effect of the Invention

[0018] The present invention having the above-mentioned configuration has polygonal ferrite: 25 to 50 area %, bainitic ferrite and acicular ferrite: 30 to 50 area %, bainite: 20 area % or less, and a unit area (1 cm 2 The total area fraction of carbides and pearlite structures with a diameter of 0.5 μm or more observed in the steel sheet is less than 5 area %, and the MA phase (Martensitic-austenitic constituents): less than 5 area %. The steel sheet has a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more. max It is possible to provide high-strength, thick, hot-rolled steel sheet that satisfies a / ΔH value of 140,000 or more. [Brief description of the drawings]

[0019] [Figure 1] 1 is a photograph showing cross-sectional microstructures according to thickness (surface layer and ¼t) of steel sheets of Example 3 and Comparative Example 9 in the examples of the present invention. [Diagram 2] FIG. 2 is a diagram showing hardness distribution in a thickness cross section of Example 3 and Comparative Example 3 in the examples of the present invention. [Diagram 3] FIG. 2 is a diagram showing the distribution of El×TS×0.5Hvmax / ΔH values ​​for the elongation levels in the examples of the present invention and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will now be described. The inventors investigated the distribution of microstructures in the thickness direction and detailed changes in material properties depending on the composition, hot rolling and cooling conditions for thick rolled steel materials having various components with different microstructures, and from the results, sought a method for imparting excellent strength and ductility to thick hot rolled steel sheets. In particular, the inventors derived the following Relational Formulas 1 to 3, and when a thick high strength steel sheet with a thickness of 10 to 14 mm is manufactured based on these Relational Formulas, uniformity of the microstructure is ensured in the thickness direction, and the hardness distribution is constant in the thickness direction, and the hardness is increased by El×TS×0.5Hv. max It has been confirmed that the / ΔH value satisfies 140,000 or more, and the present invention is presented.

[0021] The high strength thick hot rolled steel sheet of the present invention contains, by weight %, C: 0.05-0.15%, Si: 0.01-1.0%, Mn: 1.0-2.0%, Sol.Al: 0.01-0.1%, Cr: 0.005-1.0%, P: 0.001-0.02%, S: 0.001-0.01%, N: 0.001-0.01%, Nb: 0.005-0.07%, Ti: 0.005-0.11%, with the remainder being iron and unavoidable impurities, and satisfies the following [Relational Formula 1], and the microstructure of the steel has, by area %, 25-50% polygonal ferrite, 30-50% bainitic ferrite + acicular ferrite, and 20% or less bainite, and a surface area (1 cm 2 The total area fraction of carbides and pearlite structures with diameters of 0.5 μm or more observed in the steel sheet is less than 5%, and the total area fraction of MA phase (Martensitic-austenitic constituents) is less than 5%.

[0022] The compositional components of the steel of the present invention and the reasons for limiting the content of these components will be explained below, with "%" used herein meaning "% by weight."

[0023] C: 0.05~0.15% The above C is the most economical and effective element for strengthening steel, and when the amount of addition is increased, the effect of precipitation strengthening or the fraction of bainite phase increases, and the tensile strength increases. In addition, when the thickness of the hot-rolled steel sheet increases, the cooling rate at the center of the thickness during cooling after hot rolling slows down, and when the C content is large, coarse carbides and pearlite are likely to be formed. Therefore, if the content is less than 0.05%, it is difficult to obtain a sufficient strengthening effect, and if it exceeds 0.15%, there is a problem that coarse carbides, pearlite phase, and band structure are formed at the center of the thickness, which deteriorates the formability and durability, and further deteriorates the weldability. Therefore, in the present invention, it is preferable to limit the C content to 0.05 to 0.15%, and more preferably to limit it to the range of 0.06 to 0.12%.

[0024] Silicon: 0.01 to 1.0% The Si has the effect of deoxidizing molten steel and solid solution strengthening, and is advantageous in delaying the formation of coarse carbides to improve formability. However, if the content is less than 0.01%, the effect of solid solution strengthening is small, and the effect of delaying the formation of carbides is also small, making it difficult to improve formability. On the other hand, if the content exceeds 1.0%, the phase transformation temperature increases, and coarse grains are likely to be formed in the surface layer due to local ferrite region rolling during low-temperature hot rolling of extremely thick materials, and red scale is formed on the surface of the steel sheet, which not only significantly deteriorates the quality of the steel sheet surface, but also reduces ductility and weldability. Therefore, in the present invention, the Si content is preferably limited to the range of 0.01 to 1.0%, and more preferably limited to the range of 0.1 to 0.9%.

[0025] Mn: 1.0-2.0% The Mn, like Si, is an effective element for solid solution strengthening of steel, and increases the hardening ability of steel to facilitate the formation of bainite phase during cooling after hot rolling. However, if the content is less than 1.0%, the above effect of addition cannot be obtained, and if it exceeds 2.0%, the hardening ability increases significantly, making martensite phase transformation more likely to occur, and the formation of pearlite is promoted during high-temperature coiling. In addition, when a slab is cast in a continuous casting process, segregation areas develop significantly in the thickness center, and during cooling after hot rolling, a microstructure is formed non-uniformly in the thickness direction, resulting in deterioration of formability and durability. Therefore, in the present invention, the Mn content is preferably limited to the range of 1.0 to 2.0%, and more preferably to the range of 1.1 to 2.0%.

[0026] Cr: 0.005~1.0% The Cr content strengthens the steel through solid solution and retards the ferrite phase transformation during cooling to aid in the formation of bainite. However, if the Cr content is less than 0.005%, the effect of the addition is not obtained, and if it exceeds 1.0%, the ferrite transformation is excessively retarded, and the elongation rate decreases due to the formation of martensite phase. In addition, similar to Mn, segregation areas develop significantly in the thickness center, making the microstructure non-uniform in the thickness direction and deteriorating formability and durability. Therefore, in the present invention, the Cr content is preferably limited to the range of 0.005 to 1.0%, and more preferably to the range of 0.1 to 0.9%.

[0027] P: 0.001~0.02% The P element, like Si, simultaneously has the effects of strengthening the solid solution and promoting ferrite transformation. However, controlling the P content to less than 0.001% requires high manufacturing costs, which is economically disadvantageous and insufficient for obtaining strength. On the other hand, if the P content exceeds 0.02%, embrittlement occurs due to grain boundary segregation, fine cracks are likely to occur during forming, and formability and durability are significantly deteriorated. Therefore, in the present invention, it is preferable to limit the P content to the range of 0.001 to 0.02%.

[0028] S: 0.001~0.01% The above-mentioned S is an impurity present in steel, and if its content exceeds 0.01%, it bonds with Mn and the like to form nonmetallic inclusions, which tend to cause fine cracks during cutting of the steel, resulting in a problem of greatly reducing formability and durability. On the other hand, in order to control the S content to less than 0.001%, it takes a lot of time during steelmaking operations, and there is a possibility that productivity will decrease. Therefore, in the present invention, it is preferable to limit the S content to 0.001 to 0.01%.

[0029] Sol.Al: 0.01~0.1% The above-mentioned Sol.Al is a component added mainly for deoxidation, and if its content is less than 0.01%, the effect of its addition is insufficient, and if it exceeds 0.1%, it combines with nitrogen to form AlN, which makes it easy for corner cracks to occur in the slab during continuous casting and easy for defects to occur due to the formation of inclusions. Therefore, in the present invention, it is preferable to limit the content of Sol.Al to 0.01 to 0.1%.

[0030] N: 0.001~0.01% The above-mentioned N, together with C, is a typical solid solution strengthening element, and forms coarse precipitates together with Ti, Al, etc. In general, the effect of solid solution strengthening of N is superior to that of carbon, but there is a problem that the toughness is greatly reduced as the amount of N in steel increases. In addition, in order to control the content to less than 0.001%, it takes a lot of time during steelmaking operation, and the productivity decreases. Therefore, in consideration of this point, in the present invention, it is preferable to limit the N content to 0.001 to 0.01%.

[0031] Ti: 0.005~0.11% The Ti is a typical precipitation strengthening element, and forms coarse TiN in steel due to its strong affinity with N. TiN has the effect of suppressing the growth of crystal grains during the heating process for hot rolling. In addition, Ti that reacts with nitrogen and remains is dissolved in steel and combines with carbon to form TiC precipitates, making it a useful component for improving the strength of steel. If the Ti content is less than 0.005%, the above effect cannot be obtained, and if the Ti content exceeds 0.11%, there is a problem that the generation of coarse TiN and the coarsening of the precipitates cause local stress concentration during forming, making it easy for cracks to occur. Therefore, in the present invention, it is preferable to limit the Ti content to 0.005 to 0.11%, and it is more advantageous to limit it to 0.01 to 0.1%.

[0032] Nb: 0.005~0.07% The above-mentioned Nb, together with Ti, is a typical precipitation strengthening element, and since it precipitates during hot rolling and has the effect of refining crystal grains by delaying recrystallization, it is effective in improving the strength and impact toughness of steel. If the Nb content is less than 0.005%, the above effect cannot be obtained, and if the Nb content exceeds 0.07%, there is a problem that the formability and durability are deteriorated because elongated crystal grains and coarse composite precipitates are formed due to excessive delay in recrystallization during hot rolling. Therefore, in the present invention, the Nb content is preferably limited to 0.005 to 0.07%, and more preferably limited to 0.01 to 0.07%.

[0033] Equation 1 The present invention is characterized in that the contents of C, Mn, P, S, Si, Nb and Ti are controlled so that the R value defined by the following [Relation 1] falls within the range of 0.3 to 1.0.

[0034] The reason for setting this [Relationship 1] in the present invention is to suppress the formation of segregation, coarse carbides, and non-uniform pearlite structure in the thickness direction of the rolled plate by minimizing the segregation of C, Mn, P, S, etc. and MnS formation that occurs during the solidification of steel and cooling of the slab in the continuous casting process, thereby improving the uniformity of the microstructure. If the R value defined by the above [Relationship 1] is less than 0.3, the fraction of segregation, coarse carbides, and non-uniform pearlite structure in the thickness direction of the rolled plate is rapidly reduced, but there is a problem that the strength level proposed in the present invention cannot be ensured. If it exceeds 1.0, there is a problem that excessive pearlite structure is formed in the center of the microstructure of the rolled plate, or unnecessary segregation and coarse carbides are formed, thereby increasing the non-uniformity of the microstructure in the thickness direction.

[0035] [Equation 1] 0.3≦R≦1.0 R=[C]*+0.7×[Mn]+8.5×[P]+7.5×[S]-0.9×[Si]-1.5×[Nb] [C]*=[C]-[C]×Q Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) In the above formula (1), C, Mn, P, S, Si, Nb, and Ti are the weight percent of the alloying elements.

[0036] The remaining component of the present invention is iron (Fe). However, in normal manufacturing processes, unintended impurities may be inevitably mixed in from the raw materials or the surrounding environment, and it is not possible to exclude them. These impurities are known to anyone skilled in normal manufacturing processes, so the full content of them will not be mentioned in this specification.

[0037] In addition, the high strength thick hot rolled steel sheet of the present invention has, in terms of area percentage, polygonal ferrite: 25 to 50%, bainitic ferrite + acicular ferrite: 30 to 50%, bainite: 20% or less, and 2The microstructure of the steel includes less than 5% of the total area fraction of carbides and pearlite structures with diameters of 0.5 μm or more observed in the steel sheet, and less than 5% of MA phase (Martensitic-austenitic constituents).

[0038] In the present invention, if the fraction of polygonal ferrite, which is the above-mentioned high-temperature ferrite structure, is less than 25%, there is a problem in that sufficient ductility cannot be ensured, and if it exceeds 50%, there is a problem in that an appropriate fraction of low-temperature phases such as bainitic ferrite cannot be ensured, and the strength and durability are deteriorated due to the coarsening of the microstructure and the increase in the fraction of grain boundary carbides caused by the relatively slow cooling rate.

[0039] In the present invention, the total fraction of bainitic ferrite and acicular ferrite is limited to the range of 30-50%, but if the content exceeds 50%, sufficient polygonal ferrite structure cannot be secured, resulting in deterioration of ductility. Above all, in order to control the cooling rate and coiling temperature to secure bainitic ferrite and the like exceeding 50% for a thick material having a thickness of 10-14 mm, considering the length of the cooling equipment and the ROT section, there is a large restriction in terms of equipment, which may directly lead to a decrease in productivity. On the other hand, if the total fraction is less than 30%, polygonal ferrite and pearlite structures are unnecessarily formed, or the fraction of low-temperature phases such as bainite and martensite increases sharply, which also causes problems such as deterioration of strength, ductility, and durability.

[0040] In addition, in the present invention, the bainite fraction is limited to 20% or less. If the bainite fraction exceeds 20%, the polygonal ferrite fraction in the structure is rapidly reduced, which may cause a problem of unnecessary deterioration of ductility.

[0041] On the other hand, in the present invention, the unit area (1 cm 2The reason for limiting the total area fraction of carbides and pearlite structures with diameters of 0.5 μm or more observed in the steel sheet to less than 5%, and the martensitic-austenitic constituents (MA phases) to less than 5%, is to suppress the fraction of the MA phase, which locally increases the deformation rate due to excessive carbon concentration, and instead form an appropriate proportion of bainite and bainitic ferrite to induce uniform deformation behavior in the thickness direction, thereby improving ductility and durability.

[0042] Hot-rolled steel sheets with a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more, having the above-mentioned steel composition and microstructure, form a uniform structure in the thickness direction, and have El×TS×0.5Hv regarding elongation rate, strength, and material uniformity. max / ΔH value can be 140,000 or more.

[0043] Next, the method for producing a high strength hot rolled steel sheet according to the present invention will be described in detail.

[0044] In the present invention, the appropriate strength, ductility and material uniformity of the steel cannot be ensured unless the compositional components of the steel satisfy the following [Relationship 1] and the manufacturing process of the steel simultaneously satisfies the following [Relationship 2] and [Relationship 3]. This can be effectively achieved by minimizing the segregation of C, Mn, P, S, etc. and the formation of MnS that occurs during the solidification of the steel and the cooling of the slab in the continuous casting process.

[0045] The delay in recrystallization during hot rolling refines the structure during phase transformation and promotes ferrite phase transformation, which contributes to ensuring uniform yield strength and formability in the thickness direction. In addition, the amount of untransformed phase decreases, reducing the fraction of coarse MA and martensite phases, and the coarse carbides and pearlite structures in the center of the thickness where the cooling rate is relatively slow decrease, eliminating the non-uniform structure of the hot-rolled steel sheet.

[0046] However, in the normal level of hot rolling, it is difficult to make the microstructure of the thickness center of a thick material of 10 to 14 mm uniform, and if hot rolling is performed at an excessively low temperature in order to obtain the effect of delaying recrystallization in the thickness center, the deformed structure develops strongly from just below the surface layer of the rolled plate to the t / 4 position, and rather the unevenness of the microstructure phase with the thickness center increases, making it easier for fine cracks to occur in the uneven areas during forming and reducing ductility. Therefore, as shown in the following [Relationship 2], the finish hot rolling end temperature is controlled between Tn temperature, which is the temperature at which the delay of recrystallization begins, and Tn-70 according to the thick material, and in Tn, the above effect cannot be obtained unless the total reduction amount is given to 10 to 60% in the finish hot rolling end temperature section. If the total reduction is less than 10%, it is difficult to obtain the effect of retarding recrystallization, and therefore uneven coarse grains tend to form, whereas if the total reduction exceeds 60%, an excessively elongated microstructure is formed. If the microstructure is formed along the grain boundaries of carbides, cracks tend to occur along the grain boundaries during forming. In addition, the number of fine precipitates is reduced, and the effect of precipitation strengthening is also reduced.

[0047] Furthermore, since the cooling rate at the center of the thickness during cooling after hot rolling is slower than that at the surface layer of the thickness of the rolled sheet, coarse ferrite phases and coarse carbides are formed, which may result in a non-uniform microstructure. Therefore, when the rolled sheet is cooled immediately after hot rolling, a specific cooling rate (CR min ) must be cooled faster than the end of cooling temperature (CT). In addition, the cooling end temperature (CT) is limited to 400 to 550°C, which not only suppresses the formation of coarse ferrite phases and coarse carbides, but also minimizes the formation of MA phases and martensite phases.

[0048] The manufacturing method of such a high-strength thick hot-rolled steel sheet of the present invention includes the steps of reheating a steel slab having the above compositional components and satisfying the following [Relationship 1] to 1200 to 1350°C; finish hot rolling the reheated steel slab in a temperature range satisfying the following [Relationship 2]; cooling the finish hot-rolled steel sheet to a temperature in the range of 450 to 550°C at a cooling rate satisfying the following [Relationship 3], and then coiling the steel sheet at a temperature in the range of 400 to 550°C; and air-cooling or water-cooling the coiled steel sheet to a temperature in the range of room temperature to 200°C.

[0049] First, in the present invention, a steel slab that satisfies the above compositional components and the above [Relational Formula 1] is reheated to 1200 to 1350°C.

[0050] At this time, if the reheating temperature is less than 1200°C, the precipitates are not sufficiently redissolved, so that the formation of precipitates is reduced in the process after hot rolling, and coarse TiN remains. On the other hand, if the reheating temperature exceeds 1350°C, the strength may decrease due to abnormal grain growth of austenite grains. In consideration of this, in the present invention, it is preferable to limit the reheating temperature to the range of 1200 to 1350°C.

[0051] Next, in the present invention, the reheated steel slab is finish hot rolled in a temperature range that satisfies the following [Relationship 2].

[0052] In the present invention, the temperature at which hot rolling is started is preferably 1150°C or lower, and the finish hot rolling temperature is set to satisfy the following [Relationship 2], taking into consideration the microstructure of the steel. If hot rolling is started at a temperature higher than 1150°C, the temperature of the hot-rolled steel sheet will increase, causing the crystal grains to become coarse, which may deteriorate the surface quality of the hot-rolled steel sheet.

[0053] In particular, in the present invention, if rolling is terminated at a temperature higher than Tn, which is the temperature proposed in the following [Relationship 2], the microstructure of the steel becomes coarse and non-uniform. Also, if rolling is terminated at a temperature lower than Tn-70, in a thick high-strength steel having a steel plate thickness of 10 to 14 mm, the ferrite phase transformation is promoted in the surface layer where the temperature is relatively low, and the fine ferrite phase fraction increases, but the shape of the elongated crystal grains may become large, which may cause cracks to propagate quickly. Also, a non-uniform microstructure may remain in the center of the thickness, which may be detrimental to durability.

[0054] In the present invention, the above effect cannot be obtained unless the reduction is 10 to 60% within the above finish hot rolling temperature range. If the reduction is less than 10%, it is difficult to obtain the effect of retarding recrystallization, and non-uniform coarse grains are likely to be formed. On the other hand, if the reduction exceeds 60%, an excessively elongated microstructure is formed, but if it is formed along the grain boundaries of carbides in the microstructure, cracks are likely to occur along the grain boundaries during forming. In addition, fine precipitates are also reduced, and the effect of precipitation strengthening is also reduced.

[0055] [Equation 2] Tn-70≦FDT≦Tn Tn=750+92×[C]+70×[Mn]+45×[Cr]+647×[Nb]+515×[Ti]-50×[Si]-2.4×(t-5) In the above formula 2, C, Mn, Cr, Nb, Ti, and Si are the weight percent of the alloying elements. FDT in the above formula 2 is the temperature of the hot-rolled sheet at the end of hot rolling (℃) In the above formula 2, t is the thickness of the final rolled plate material (mm).

[0056] Next, in the present invention, the finish hot rolled steel sheet is cooled to a temperature in the range of 450 to 550°C at a cooling rate that satisfies the following [Relationship 3], and then the cooled steel sheet is coiled at a temperature in the range of 400 to 550°C.

[0057] The temperature range from FDT, the temperature immediately after hot rolling, to CT, the cooling end temperature, corresponds to the temperature range in which ferrite phase transformation occurs during cooling. Since the cooling rate at the center of the thickness is slower than that at the surface layer of the rolled plate, coarse ferrite phase and coarse carbide are formed at the center of the thickness, resulting in a non-uniform microstructure. Therefore, in order to prevent this, a specific cooling rate (CR min ) in this temperature range. If the average cooling rate of the surface layer of the hot-rolled steel sheet (the region from the steel sheet surface to the thickness direction of 1 to 2 mm) is higher than 60°C / sec, the difference in cooling rate between the surface layer and the deeper layer is too large, and the difference in hardness between the surface layer and the deeper layer increases significantly, which may deteriorate formability and durability. In addition, in terms of equipment, there are disadvantages in that the equipment load due to extremely strong cooling at all stages is high and it is difficult to realize in a slab with a small unit weight. Therefore, as shown in the following [Relationship 3], cooling must be performed to satisfy the cooling rate set in consideration of the steel components.

[0058] Furthermore, in the present invention, if the coiling temperature exceeds 550°C, pearlite phase is formed in the band structure or a large amount of coarse carbides is formed, resulting in insufficient formability and durability of the steel, whereas if it is less than 400°C, martensite phase and MA phase are formed in excess, resulting in poor formability and durability. Therefore, in the present invention, it is preferable to limit the coiling temperature to 450 to 550°C.

[0059] [Equation 3] CR Min ≦CR*≦60 CR Min =65-157×[C]-25.2×[Si]-14.1×[Mn]-27.3×[Cr]+61×[Ti]+448×[Nb]+1.4×(t-5) In the above formula 3, C, Si, Mn, Cr, Ti, and Nb are the weight percent of the alloying elements. CR* in the above formula 3 is the cooling rate (℃ / sec) when cooling the plate material after hot rolling.

[0060] In the present invention, the coiled hot-rolled steel sheet is air-cooled or water-cooled to a temperature in the range of room temperature to 200°C.

[0061] Air cooling of a steel sheet means cooling in air at room temperature at a cooling rate of 0.001 to 10°C / hour. In this case, even if the cooling rate exceeds 10°C / hour, water cooling may be performed since it is possible to suppress transformation of a part of the untransformed phase in the steel into the MA phase as long as the coiling temperature and cooling conditions are satisfied. Here, water cooling means cooling by inserting the coil into a water bath at room temperature. In addition, in order to control the cooling rate to less than 0.001°C / hour, separate heating and heat retention equipment are required, which is economically disadvantageous.

[0062] In the present invention, after the air or water cooling, the steel sheet can be pickled and oiled to produce a PO (pickled and oiled) steel sheet.

[0063] The high strength thick hot rolled steel sheet of the present invention manufactured by the above-mentioned manufacturing process and having a thickness of 10 to 14 mm has, in terms of area percentage, polygonal ferrite: 25 to 50%, bainitic ferrite + acicular ferrite: 30 to 50%, bainite: 20% or less, and unit area (1 cm 2 The steel has a microstructure containing less than 5% of the total area fraction of carbides and pearlite structures with diameters of 0.5 μm or more observed in the steel sheet, and less than 5% of MA phase (Martensitic-austenitic constituents), and can exhibit a tensile strength of 590 MPa or more and an elongation rate of 30% or more.

[0064] In addition, the hot-rolled steel sheet of the present invention has El × TS × 0.5Hv max / ΔH value can be 140,000 or more. EXAMPLES

[0065] The present invention will now be described in more detail with reference to examples.

[0066] (Example) The compositions of steel slabs having the component compositions of the present invention as shown in Table 1 below were prepared. Then, for each of the prepared steel slabs, hot-rolled steel sheets were produced using the manufacturing process conditions shown in Table 2 below, such as the rolling thickness, finish hot rolling temperature (FDT), coiling temperature (CT), reduction (%) applied in the temperature range below Tn and above Tn-70, which is the non-recrystallization temperature region, and cooling rate (CR) up to the coiling temperature, which is the cooling end temperature after finish hot rolling. Meanwhile, the cooling rate of the steel sheet after coiling, which is not shown in Table 2, was kept constant at 1°C / hour.

[0067] The microstructural phase fractions of the surface layer (1 mm below the surface) and center (2 / t) of the hot-rolled steel sheets were measured and are shown in Table 3 below. Meanwhile, the area fraction of the MA phase was measured by etching using the Lepera etching method, and analyzed at 1000x magnification using an optical microscope and image analyzer. The phase fractions of martensite (M), polygonal ferrite (PF), bainitic ferrite (BF), acicular ferrite (AF), bainite (B) and pearlite (P) were measured by etching using a Nital etching solution, and analyzed at 3000x and 5000x magnification using a scanning electron microscope (SEM).

[0068] The mechanical properties and hardness of the hot-rolled steel sheets produced above were measured, and the results are shown in Table 4 below. Here, YS, TS, YR, and El mean 0.2% off-set yield strength, tensile strength, yield ratio, and elongation at break, and are the results of tests performed on JIS No. 5 standard test pieces that were parallel to the rolling direction and sampled.

[0069] Meanwhile, the hardness was measured using a Micro-Vickers tester, measuring the Vickers hardness value in the thickness direction at 0.5 mm intervals from the surface layer (1 mm directly below the surface) to 1 / 2t thickness, with a load of 500 g applied. Here, the maximum Vickers hardness value measured is defined as Hmax, the minimum hardness value as Hmin, and ΔHv means Hmax-Hmin.

[0070] [Table 1]

[0071] [Table 2]

[0072] [Table 3] *In Table 3, P is the ratio of pearlite to unit area (1 cm 2 ) and the total fraction of carbides with a diameter of 0.5 μm or more observed within the

[0073] [Table 4] *In Table 4, A* is El × TS × 0.5Hv max / ΔH

[0074] As shown in Tables 1-4 above, Invention Examples 1-7, which satisfy all of the component ranges, manufacturing conditions, and Relational Formulas 1-3 proposed in the present invention, have the targeted microstructure and material properties.

[0075] In contrast, in Comparative Example 1, the C content is outside the range proposed by the present invention, and the [Relationship 1] considering segregation exceeds the range of the present invention. In this case, excessive pearlite structure is formed in the center and surface layers of the microstructure, which results in insufficient ductility and large hardness variation through the thickness.

[0076] In Comparative Example 2, the Si content does not fall within the range of the present invention and does not satisfy [Relationship 1], and it can be confirmed that the MA phase fraction is high in both the surface layer and the deep layer. This is because the phase transformation temperature rises due to the excessive addition of Si, ferrite phase is formed in the surface layer during hot rolling, and rolling is performed in the two-phase region, and some of the untransformed austenite phase is transformed into the MA phase, resulting in a decrease in the elongation rate.

[0077] Comparative Example 3-4 is a case where the Mn content is outside the range of the Mn content proposed in the present invention and does not satisfy [Relationship 1]. Specifically, Comparative Example 3 is a case where the Mn content is too high, and the pearlite structure is excessively formed, and elongated MnS inclusions are also observed. In particular, when the hardness is measured in the thickness direction, a locally high hardness difference is observed, and the ductility is also insufficient. And Comparative Example 4 has a low Mn content, and although segregation in the thickness direction of the rolled plate, coarse carbides, and non-uniform pearlite structure are not formed, the yield strength and tensile strength are insufficient, and the results are outside the scope of the present invention.

[0078] In Comparative Examples 5 and 6, the compositional components of the steels satisfy the range of the present invention, but the range of the FDT does not satisfy the range of the present invention. Comparative Example 5 resulted in the formation of coarse ferrite (polygonal ferrite) and did not satisfy the target strength, whereas Comparative Example 6 resulted in the formation of a large amount of coarse ferrite (polygonal ferrite) that was elongated by rolling in the two-phase region, which increased the heterogeneity of the structure and also deteriorated the strength.

[0079] Comparative Examples 7-8 are cases that do not satisfy the coiling temperature standard proposed in the present invention. Specifically, Comparative Example 7 is a case where the coiling temperature is higher than the range proposed in the present invention, and pearlite structures are locally formed in the structure, and in particular, pearlite band structures are observed in the thickness center portion. As a result, a locally high hardness difference is observed when hardness is measured in the thickness direction. And Comparative Example 8 is a case where the coiling temperature is lower than the range proposed in the present invention, and it can be confirmed that the elongation rate is reduced due to the formation of excessive martensite in the structure.

[0080] In Comparative Example 9, the cooling rate after hot rolling was slower than the range proposed in the present invention. It was confirmed that the fraction of coarse ferrite (polygonal ferrite) in the structure was high, resulting in a decrease in strength, and that pearlite and coarse carbides were formed in the center of the thickness, causing hardness variations.

[0081] 1 is a photograph showing the cross-sectional microstructures according to the thickness (surface layer and 1 / 4t) of the steel sheets of Example 3 and Comparative Example 9 in the examples of the present invention. It can be seen that Example 3 has a more homogeneous structure than Comparative Example 9.

[0082] 2 is a diagram showing the distribution of hardness values ​​in the thickness cross section of Example 3 and Comparative Example 3 in the examples of the present invention. It can be seen that Example 3 has smaller hardness variation for each thickness than Comparative Example 3.

[0083] FIG. 3 shows the relationship between the El×TS×0.5Hv and the elongation levels of the invention examples and comparative examples in the examples of the present invention. max FIG. 1 shows the distribution of / ΔH values.

[0084] As described above, the detailed description of the present invention has been given of the preferred embodiment of the present invention, but it goes without saying that a person having ordinary skill in the art to which the present invention pertains can make various modifications within the scope of the present invention. Therefore, the scope of the present invention should not be limited to the described embodiment, but should be determined by the claims below as well as equivalents thereto.

Claims

1. In weight percent, C: 0.05-0.15%, Si: 0.01-1.0%, Mn: 1.0-2 .. 0%, Sol. Al: 0.01-0.1%, Cr: 0.005-1.0%, P: 0.0 01-0.02%, S: 0.001-0.01%, N: 0.001-0.01%, Nb: 0.005 to 0.07%, Ti: 0.005 to 0.11%, the remainder being iron and unavoidable impurities, and satisfying the following [Relationship 1]: By area percentage, polygonal ferrite: 25-50%, bainitic ferrite + acicular ferrite Ferrite: 30-50%, Bainite: 20% or less, Unit area (1 cm 2 ) observed in The total area fraction of carbides and pearlite structures with a diameter of 0.5 μm or more: less than 5%, and MA phase (Martensitic-austenitic constitutions) : A high-strength thick hot-rolled steel plate having a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more, and having a fine structure containing less than 5%. [Relationship 1] 0.3≦R≦1.0 R=[C]*+0.7×[Mn]+8.5×[P]+7.5×[S]-0.9×[Si ]−1.5×[Nb] [C]*=[C]-[C]×Q Q=([Nb] / 93+[Ti] / 48) / ([C] / 12) In the above formula (1), C, Mn, P, S, Si, Nb, and Ti are the weight percentages of the alloy elements.

2. The hot-rolled steel sheet has a thickness of El×TS×0.5Hv max / ΔH value is 140,000 or more The high-strength thick hot-rolled steel sheet according to claim 1, having a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more.

3. In weight percent, C: 0.05-0.15%, Si: 0.01-1.0%, Mn: 1.0-2 .. 0%, Sol. Al: 0.01-0.1%, Cr: 0.005-1.0%, P: 0.0 01-0.02%, S: 0.001-0.01%, N: 0.001-0.01%, Nb: a step of reheating a steel slab containing 0.005-0.07%, Ti: 0.005-0.11%, the remainder being iron and unavoidable impurities, and satisfying the following [Relationship 1] to 1200-1350°C; The reheated steel slab is finish hot-rolled in a temperature range that satisfies the following [Relationship 2]. a step of: The finish hot-rolled steel sheet is heated to a temperature in the range of 450 to 550° C. by the following [Relationship 3] and then coiling at a temperature in the range of 400 to 550°C; and cooling the coiled steel sheet by air or water to a temperature in the range of room temperature to 200° C.; The air-cooled or water-cooled hot-rolled steel sheet has a microstructure including, in area percentages, 25 to 50% polygonal ferrite, 30 to 50% bainitic ferrite + acicular ferrite, 20% or less bainite, less than 5% total area fraction of carbides and pearlite structures with diameters of 0.5 μm or more observed within a unit area (1 cm 2 ), and less than 5% MA phase (martensitic-austenitic constituents), and the El×TS×0.5Hv max / ΔH value is 140,000 or more. [Relationship 1] 0.3≦R≦1.0 R=[C]*+0.7×[Mn]+8.5×[P]+7.5×[S]-0.9×[Si ]−1.5×[Nb] [C]*=[C]-[C]×Q Q=([Nb] / 93+[Ti] / 48) / ([C] / 12) In the above Relational Formula 1, C, Mn, P, S, Si, Nb, and Ti are the weight percentages of the alloy elements. [Relationship 2] Tn-70≦FDT≦Tn Tn=750+92×[C]+70×[Mn]+45×[Cr]+647×[Nb]+ 515×[Ti]-50×[Si]-2.4×(t-5) In the above-mentioned relational formula 2, C, Mn, Cr, Nb, Ti, and Si are the weight percentages of the alloy elements. FDT in the above Relational Formula 2 is the temperature (°C) of the hot-rolled sheet at the end of hot rolling. In the above Relational Formula 2, t is the thickness (mm) of the final rolled plate material. [Relationship 3] CR Min ≦CR*≦60 CR Min =65-157×[C]-25.2×[Si]-14.1×[Mn]-27 .. 3×[Cr]+61×[Ti]+448×[Nb]+1.4×(t-5) In the above-mentioned relational expression 3, C, Si, Mn, Cr, Ti, and Nb are the weight percentages of the alloy elements. CR* in the above-mentioned Relational Formula 3 is the cooling rate (°C / sec) when cooling the plate material rolled after hot rolling.

4. 4. The method according to claim 3, further comprising pickling and oiling the steel sheet after the air or water cooling. A method for manufacturing a high-strength thick hot-rolled steel sheet having a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more.

5. The method according to claim 3, wherein the reduction amount is controlled to 10 to 60% within the range of the finish hot rolling temperature. A method for manufacturing a high-strength thick hot-rolled steel sheet having a thickness of 10 to 14 mm, a tensile strength of 590 MPa or more, and an elongation rate of 30% or more.

Citation Information

Patent Citations

  • Controlled rolling and cooling process for Cr-containing economic X70 pipeline hot-rolled steel coil plate

    CN103042039A

  • Production of high tensile strength steel plate having extremely fine structure

    JP1997143570A

  • High strength and low yield ratio hot rolled steel sheet for pipe and its production

    JP1998176239A

  • Manufacture of hot rolled high tensile strength steel plate

    JP1998298645A

  • High formability high tensile hot rolled steel sheet having excellent material uniformity, production method therefor and working method therefor

    JP2002322541A