THERMAL RECORDING LAMINATE AND METHOD FOR PRODUCING THERMAL RECORDING LAMINATE

The heat-sensitive recording laminate addresses durability issues by incorporating specific compounds and a thermoplastic resin overcoat, achieving improved resistance to alcohol, oils, and scratches, along with enhanced adhesion and transparency.

JP7569949B1Active Publication Date: 2024-10-18TOKYO PRINTING INC MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024007134
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-22
Publication Date
2024-10-18
Estimated Expiration
2044-01-22

AI Technical Summary

Technical Problem

Existing thermosensitive recording materials lack adequate alcohol resistance, oil resistance, scratch resistance, and transparency, with insufficient curing agents or crosslinking agents in protective layers leading to poor durability and performance.

Method used

A heat-sensitive recording laminate comprising a thermosensitive coloring layer with specific compounds, an aqueous coating layer, and an overcoat layer containing a thermoplastic resin and polyisocyanate, enhancing adhesion and durability.

Benefits of technology

The laminate provides improved water resistance, low residual solvent, stain resistance, transparency, and enhanced resistance to alcohol, scratches, and oils, with better adhesion and abrasion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569949000001
    Figure 0007569949000001
  • Figure 0007569949000002
    Figure 0007569949000002
  • Figure 0007569949000003
    Figure 0007569949000003
Patent Text Reader

Abstract

An object of the present invention is to provide a laminate which has not only water resistance but also little residual solvent, is resistant to blocking, and has background smear resistance, transparency, color density, adhesion, alcohol resistance, scratch resistance before and after color development, head resistance, abrasion resistance, and oil resistance. [Solution] A thermal recording laminate having a thermal coloring layer on one side of a plastic film substrate, the thermal coloring layer comprising a leuco dye, at least one color developer selected from the compounds represented by general formulas (1) to (4), and a thermal coloring agent containing an aqueous resin, an alcohol, and water, an aqueous coating layer on the thermal coloring layer, the aqueous coating layer comprising an aqueous coating agent containing a water-soluble resin and water, and an overcoat layer on the aqueous coating layer, the overcoat layer comprising an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermosensitive recording laminate and a method for producing the thermosensitive recording laminate. [Background technology]

[0002] Generally, a thermal recording medium is prepared by coating a support such as paper, synthetic paper, film, or plastic with a coating liquid containing a colorless or light-colored electron-donating leuco dye (hereinafter also referred to as "leuco dye") and an electron-accepting developer (hereinafter also referred to as "developer") such as a phenolic compound, and the coating liquid develops color through an instantaneous chemical reaction caused by heating with a thermal head, hot stamp, heat pen, laser light, etc., to obtain a recorded image. Thermal recording media are widely used as recording media for facsimiles, computer terminal printers, automatic ticket vending machines, measurement recorders, receipts from supermarkets and convenience stores, etc.

[0003] It has the advantage of being able to record in a short amount of time using relatively simple equipment and being inexpensive, so in recent years it has been rapidly adopted in the food packaging field for foods, boxed lunches, prepared dishes, etc., because it can contribute to improving image reliability, reducing the need for conventional labels, improving design, and reducing the cost of packaging materials. There is a demand for label-less printing, transparency, water resistance, oil resistance, alcohol resistance, scratch resistance, and no color change at low temperatures (resistance to scumming).

[0004] Patent Document 1 discloses a thermal recording medium having a thermal recording layer on a plastic film, the thermal recording layer containing a leuco dye and a urea-urethane compound as a color developer, and a protective layer as the outermost layer on the thermal recording layer, the protective layer containing an acrylic resin and a polyolefin resin. However, the protective layer uses an aqueous emulsion of an acrylic resin and a polyolefin resin in combination, and it is clear from the comparative example that the aqueous emulsion of an acrylic resin alone has excellent print running properties (head resistance), but only a certain degree of water resistance and slight coating defects (a certain degree of transparency), but the alcohol resistance may be poor. Since no hardener or crosslinking agent is used in the protective layer, the oil resistance may be poor. In addition, there is no description or suggestion about smear resistance, blocking, residual solvent, adhesion, scratch resistance, and abrasion resistance.

[0005] Patent Document 2 discloses a thermosensitive recording medium having a support, a thermosensitive recording layer on the support, which contains a color developer that is an N,N'-diaryl urea derivative and a styrene-acrylic resin, and a protective layer on the thermosensitive recording layer (Example 6). The protective layer is made of a water-soluble styrene-acrylic resin and an oxazoline group-containing polymer as a curing agent, and is water-resistant. As for ethanol resistance, the change in image density before and after immersion in ethanol after printing on the thermosensitive recording medium with a laser marker to form an image was evaluated, but the alcohol resistance of the thermosensitive recording medium itself was not evaluated, and may be inferior. Furthermore, there is no mention or suggestion of background smear resistance, blocking, residual solvent, adhesion, scratch resistance, head resistance, abrasion resistance, or oil resistance. As for transparency, it is described that the support is preferably a transparent film, and that there is no problem if the haze (turbidity) is about 10% or less, but this is only the transparency of the support, not the transparency of the thermosensitive recording medium itself, and there is no mention or suggestion of the transparency of the thermosensitive recording medium.

[0006] Patent Document 3 discloses a thermosensitive recording medium having a thermosensitive recording layer on a partial area of ​​a support and a thermosensitive recording layer forming liquid containing a leuco dye, a color developer having a specific solubility, and a solvent, and further has a protective layer on the thermosensitive recording layer (Examples 21 to 28). The protective layer uses an acrylic resin emulsion and has water resistance. It also has excellent background uniformity (few coating unevenness = adhesion) and background density (coloring density). However, since no hardener or crosslinking agent is used in the protective layer, it may have poor oil resistance. Furthermore, it may also have poor alcohol resistance. Furthermore, there is no description or suggestion about smear resistance, blocking, transparency, residual solvent, scratch resistance, head resistance, and abrasion resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-199054 A [Patent Document 2] JP 2022-146283 A [Patent Document 3] JP 2022-151636 A Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, an object of the present invention is to provide a laminate which has not only water resistance but also little residual solvent, is resistant to blocking, and has background smear resistance, transparency, color density, adhesion, alcohol resistance, scratch resistance before and after color development, head resistance, abrasion resistance, and oil resistance. [Means for solving the problem]

[0009] As a result of intensive research, the inventors have found that the above-mentioned object can be achieved by forming a thermal recording laminate having, on one side of a plastic film substrate, a thermal coloring layer comprising a thermal coloring agent containing a leuco dye, at least one color developer selected from specific compounds, an aqueous resin, an alcohol, and water, an aqueous coating layer on the thermal coloring layer comprising an aqueous coating agent containing a water-soluble resin and water, and an overcoat layer on the aqueous coating layer comprising an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent, and have thus completed the present invention.

[0010] That is, according to the present invention, there are provided a thermosensitive recording laminate, an overcoat set for use in the thermosensitive recording laminate, and a method for producing the thermosensitive recording laminate, which are shown below. (1) A thermosensitive coloring layer on one side of a plastic film substrate, the thermosensitive coloring layer comprising a leuco dye, at least one color developer selected from the group consisting of a compound represented by the following general formula (1), a compound represented by the following general formula (2), a compound represented by the following general formula (3), and a compound represented by the following general formula (4), a thermosensitive coloring agent containing a water-soluble resin, alcohol, and water, and an aqueous coating layer on the thermosensitive coloring layer, the aqueous coating agent containing a water-soluble resin and water. a thermal recording laminate having an overcoat layer on the aqueous coating layer, the overcoat layer being made of an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent;

[0011] [ka] (R 1 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, each of which may be the same or different, and R 2are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, which may be the same or different; Z 1 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group.

[0012] [ka] (R 3 is an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkyloxyalkyl group having 3 to 12 carbon atoms, a polyoxyalkylenealkyl group having 3 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, an alkylsulfanyl group having 1 to 12 carbon atoms, an aralkylsulfanyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 14 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an aralkylsulfonyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 15 carbon atoms, a phenyl group, an aralkylsulfonylamino group having 7 to 12 carbon atoms, an arylsulfonylamino group having 6 to 15 carbon atoms, an acyl group having 2 to 10 carbon atoms, an acylamino group having 2 to 10 carbon atoms, an (acyl having 2 to 10 carbon atoms)oxycarbonylamino group, an (alkyl having 1 to 12 carbon atoms)oxycarbonylamino group, an aralkyloxycarbonylamino group, an (aralkyl having 7 to 12 carbon atoms)oxycarbonylamino group, or an (aryl having 6 to 15 carbon atoms)oxycarbonylamino group, 3 may be bonded to each other to form an aromatic or non-aromatic ring together with the carbon atom to which they are bonded, R 4 , R 5 is a hydrogen atom or a methyl group; a, b, and c are independently an integer of 0 to 4; a+c is an integer of 0 to 5; n is 0 or 1; Y is a divalent organic group; Z 2 is a sulfonyloxy group or a sulfonyl group.

[0013] [ka] (R 6is a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom; R 7 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, l and m are 0 or 1, and Z 3 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group.

[0014] [ka] (R 8 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, each of which may be the same or different, and R 9 is a methyl group, d is an integer of 0 to 4, and Z 4 and Z 5 are sulfonyloxy groups, sulfonyl groups, or sulfonamide groups, and may be the same or different.

[0015] (2) A thermosensitive coloring layer on one side of a plastic film substrate, the thermosensitive coloring layer comprising a thermosensitive coloring agent containing a leuco dye, a compound represented by the following general formula (5), a water-soluble resin, an alcohol, and water, and an aqueous coating layer on the thermosensitive coloring layer, the aqueous coating layer comprising a water-soluble resin and water, a thermal recording laminate having an overcoat layer on the aqueous coating layer, the overcoat layer being made of an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent;

[0016] [ka] (R 10 are linear, branched or alicyclic alkyl groups having 1 to 12 carbon atoms, unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms, or aralkyl groups having 7 to 12 carbon atoms substituted with a halogen atom, or unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms, or aryl groups having 6 to 12 carbon atoms substituted with a halogen atom, and may be the same or different.

[0017] (3) The thermal recording laminate according to (1) or (2), wherein the aqueous resin is a water-soluble resin or an aqueous emulsion resin. (4) The thermosensitive recording laminate according to any one of (1) to (3), wherein the thermoplastic resin is an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, or a fiber-based resin. (5) An overcoat set for use in the thermal recording laminate according to any one of (1) to (3), a coating agent A containing a thermoplastic resin and an organic solvent; and a curing agent B containing a polyisocyanate and an organic solvent. (6) preparing a plastic film substrate; a gravure printing process for forming a thermosensitive coloring layer on one side of the plastic film substrate, the thermosensitive coloring layer being made of a thermosensitive coloring agent containing a leuco dye, a color developer, an aqueous resin, alcohol, and water; a coating step of forming an aqueous coating layer on the thermosensitive coloring layer using an aqueous coating agent containing a water-soluble resin and water; a coating step of forming an overcoat layer on the aqueous coating layer using an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent, A method for producing a thermal recording laminate, wherein the developer is at least one of a compound represented by the following general formula (1), a compound represented by the following general formula (2), a compound represented by the following general formula (3), and a compound represented by the following general formula (4):

[0018] [ka] (R 1 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, each of which may be the same or different, and R 2 are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, which may be the same or different; Z 1 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group.

[0019] [ka] (R 3is an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkyloxyalkyl group having 3 to 12 carbon atoms, a polyoxyalkylenealkyl group having 3 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, an alkylsulfanyl group having 1 to 12 carbon atoms, an aralkylsulfanyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 14 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an aralkylsulfonyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 15 carbon atoms, a phenyl group, an aralkylsulfonylamino group having 7 to 12 carbon atoms, an arylsulfonylamino group having 6 to 15 carbon atoms, an acyl group having 2 to 10 carbon atoms, an acylamino group having 2 to 10 carbon atoms, an (acyl having 2 to 10 carbon atoms)oxycarbonylamino group, an (alkyl having 1 to 12 carbon atoms)oxycarbonylamino group, an aralkyloxycarbonylamino group, an (aralkyl having 7 to 12 carbon atoms)oxycarbonylamino group, or an (aryl having 6 to 15 carbon atoms)oxycarbonylamino group, 3 may be bonded to each other to form an aromatic or non-aromatic ring together with the carbon atom to which they are bonded, R 4 , R 5 is a hydrogen atom or a methyl group; a, b, and c are independently an integer of 0 to 4; a+c is an integer of 0 to 5; n is 0 or 1; Y is a divalent organic group; Z 2 is a sulfonyloxy group or a sulfonyl group.

[0020] [ka] (R 6 is a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom; R 7is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, l and m are 0 or 1, and Z 3 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group.

[0021] [ka] (R 8 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, each of which may be the same or different, and R 9 is a methyl group, d is an integer of 0 to 4, and Z 4 and Z 5 are sulfonyloxy groups, sulfonyl groups, or sulfonamide groups, and may be the same or different.

[0022] (7) preparing a plastic film substrate; a gravure printing process for forming a thermosensitive coloring layer on one side of the plastic film substrate, the thermosensitive coloring layer being made of a thermosensitive coloring agent containing a leuco dye, a color developer, an aqueous resin, alcohol, and water; a coating step of forming an aqueous coating layer on the thermosensitive coloring layer using an aqueous coating agent containing a water-soluble resin and water; a coating step of forming an overcoat layer on the aqueous coating layer using an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent, A method for producing a thermal recording laminate, wherein the developer is a compound represented by the following general formula (5):

[0023] [ka] (R 10 are linear, branched or alicyclic alkyl groups having 1 to 12 carbon atoms, unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms, or aralkyl groups having 7 to 12 carbon atoms substituted with a halogen atom, or unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms, or aryl groups having 6 to 12 carbon atoms substituted with a halogen atom, and may be the same or different.

[0024] (8) The method for producing a thermal recording laminate according to (6) or (7), wherein the aqueous resin is a water-soluble resin or an aqueous emulsion resin. (9) The method for producing a thermosensitive recording laminate according to any one of (6) to (8), wherein the thermoplastic resin is an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, or a fiber-based resin. (10) A method for producing a thermosensitive recording laminate according to any one of (6) to (9), further comprising a coating step of forming an anchor coat layer between the plastic film substrate and the thermosensitive color developing layer using an anchor coat agent. (11) A method for producing a thermosensitive recording laminate according to any one of (6) to (10), further comprising a laminating step or a coating step of forming a seal layer on the plastic film substrate on the side opposite to the thermosensitive color developing layer. (12) A method for producing a thermosensitive recording laminate according to any one of (6) to (11), further comprising a gravure printing step of forming a design layer on the plastic film substrate or on the surface of the plastic film substrate opposite to the thermosensitive color developing layer. (13) A method for producing a thermosensitive recording laminate according to any one of (6) to (12), further comprising a gravure printing step for forming a colored ink layer. It is. Effect of the Invention

[0025] According to the present invention, it is possible to provide a laminate which has not only water resistance but also a small amount of residual solvent, is resistant to blocking, and has background smear resistance, transparency, color density, adhesion, alcohol resistance, scratch resistance before and after color development, head resistance, abrasion resistance, and oil resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, an embodiment of the present invention will be described in detail. Note that this embodiment is merely one embodiment of the present invention, and the present invention is not limited to this embodiment. Various modifications are possible without departing from the gist of the present invention.

[0027] The thermal recording laminate of the present invention preferably has, on one side of a plastic film substrate, a thermal color developing layer comprising a leuco dye, at least one color developer selected from the group consisting of a compound represented by the following general formula (1), a compound represented by the following general formula (2), a compound represented by the following general formula (3), and a compound represented by the following general formula (4), and a thermal color developing agent containing an aqueous resin, an alcohol, and water; an aqueous coating layer on the thermal color developing layer comprising an aqueous coating agent containing a water-soluble resin and water; and an overcoat layer on the aqueous coating layer comprising an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent.

[0028] The heat-sensitive color former of the present invention preferably contains a compound represented by the general formula (1). The compound represented by the general formula (1) is as follows.

[0029] [ka]

[0030] R 1represents a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms and substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms and substituted with a halogen atom, and may be the same or different.

[0031] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a 2-ethylhexyl group, and a lauryl group.

[0032] Examples of the aralkyl group include benzyl group, 1-phenylethyl group, 2-phenylethyl group, 3-phenylpropyl group, p-methylbenzyl group, m-methylbenzyl group, m-ethylbenzyl group, p-ethylbenzyl group, p-isopropylbenzyl group, pt-butylbenzyl group, p-methoxybenzyl group, m-methoxybenzyl group, o-methoxybenzyl group, m,p-di-methoxybenzyl group, p-ethoxy-m-methoxybenzyl group, p-phenylmethylbenzyl group, p-cumylbenzyl group, p-phenylbenzyl group, o-phenylbenzyl group, m-phenylbenzyl group, p-tolylbenzyl group, m-tolylbenzyl group, o-tolylbenzyl group, and p-chlorobenzyl group, and the like.

[0033] Examples of the aryl group include unsubstituted aryl groups or aryl groups substituted with an alkyl group, an alkoxy group, an aralkyl group, an aryl group, or a halogen atom, such as a phenyl group, a p-tolyl group, an m-tolyl group, an o-tolyl group, a 2,5-dimethylphenyl group, a 2,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a 2,3-dimethylphenyl group, a 3,4-dimethylphenyl group, a mesitylene group, a p-ethylphenyl group, a p-isopropylphenyl group, a p-butylphenyl group, a p-methoxyphenyl group, a 3,4-dimethoxyphenyl group, a p-ethoxyphenyl group, a p-chlorophenyl group, a 1-naphthyl group, a 2-naphthyl group, or a t-butylated naphthyl group.

[0034] R 2 are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, and may be the same or different. R 2 may be the same or different and are the 3rd, 4th or 5th positions. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. Of these, a hydrogen atom is more preferable.

[0035] Z 1 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group. Among them, a compound containing a sulfonyloxy group represented by the following general formula (5) is more preferable. R 10 The position of -SO2-O- may be the same or different and is the 3-position, 4-position or 5-position, more preferably the 3-position.

[0036] It is more preferable that the heat-sensitive color former of the present invention contains a compound represented by the general formula (5). The compound represented by the general formula (5) is as follows.

[0037] [ka]

[0038] R 10 represents a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms and substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms and substituted with a halogen atom, and may be the same or different.

[0039] R 10 As the R 1 Among them, a phenyl group, a p-tolyl group, a m-tolyl group, an o-tolyl group, a mesitylene group, a 2-naphthyl group, a methyl group, an ethyl group, a benzyl group, a p-ethylbenzyl group, a p-methoxybenzyl group, and the like are more preferable.

[0040] More particularly, N,N'-di-[3-(p-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(o-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(benzenesulfonyloxy)phenyl]urea, N,N'-di-[(3-benzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(mesitylenesulfonyloxy)phenyl]urea, N,N'-di-[3-(4-ethylbenzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(2-naphthalenesulfonyloxy)phenyl]urea, N,N'-di-[3-(p-methoxybenzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(benzylsulf [p-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(ethanesulfonyloxy)phenyl]urea, N,N'-di-[3-(p-toluenesulfonyloxy)-4-methyl-phenyl]urea, N,N'-di-[4-(p-toluenesulfonyloxy)phenyl]urea, N,N'-di-[4-(benzenesulfonyloxy)phenyl]urea, N,N'-di-[4-(ethanesulfonyloxy)phenyl]urea, N,N'-di-[2-(p-toluenesulfonyloxy)]phenylurea, and the like.

[0041] The thermosensitive color former of the present invention preferably contains a compound represented by formula (2). The compound represented by formula (2) is as follows.

[0042] [ka]

[0043] R 3is an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkyloxyalkyl group having 3 to 12 carbon atoms, a polyoxyalkylenealkyl group having 3 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, an alkylsulfanyl group having 1 to 12 carbon atoms, an aralkylsulfanyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 14 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an aralkylsulfonyl group having 7 to 12 carbon atoms, an aryl group having 6 to 15 carbon atoms, and (aryl)oxycarbonylamino groups.

[0044] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, and a lauryl group.

[0045] Examples of the alkenyl group include a vinyl group, an allyl group, a propenyl group, and a butenyl group.

[0046] Examples of the alkyloxyalkyl group include C2H5O-C2H4-, C3H7O-C3H6-, and the like.

[0047] The polyoxyalkylene alkyl group may be O-(C2H4O)n-C2H4- (n=1 to 3), HO-(C3H6O) n -C3H6- (n = 1 to 3), etc.

[0048] Examples of the aralkyl group include a benzyl group, a p-methylbenzyl group, a p-isopropylbenzyl group, a p-butylbenzyl group, a p-chlorobenzyl group, a p-methoxybenzyl group, a m-methoxybenzyl group, a m,p-dimethoxybenzyl group, a phenethyl group, an α-phenethyl group, and a phenylpropyl group.

[0049] Examples of the aryl group include a phenyl group, a tolyl group, a p-ethylphenyl group, a p-xylyl group, a m-xylyl group, a 1,2,3-trimethylphenyl group, a mesitylene group, a 1,2,4-trimethylphenyl group (pseudocumene group), a 1-naphthyl group, a 2-naphthyl group, a biphenyl group, and a dimethylbiphenyl group.

[0050] Examples of the alkylsulfanyl group include a methylsulfanyl group and a butylsulfanyl group.

[0051] Examples of the aralkylsulfanyl group include a benzylsulfanyl group, a 1-phenylethylsulfanyl group, a 2-phenylethylsulfanyl group, a 1-phenylpropylsulfanyl group, a 2-phenylpropylsulfanyl group, a 1-phenylbutylsulfanyl group, a 2-phenylbutylsulfanyl group, a 1-naphthylmethylsulfanyl group, a 2-naphthylmethylsulfanyl group, a (1-naphthyl)ethylsulfanyl group, and a (2-naphthyl)ethylsulfanyl group.

[0052] The arylsulfanyl group includes a phenylsulfanyl group.

[0053] Examples of the alkylsulfonyl group include a methanesulfonyl group, an ethanesulfonyl group, a propanesulfonyl group, and a butanesulfonyl group.

[0054] Examples of the aralkylsulfonyl group include a benzylsulfonyl group.

[0055] Examples of the arylsulfonyl group include a benzenesulfonyl group, a toluenesulfonyl group, a 2-p-xylylenesulfonyl group, a mesitylenesulfonyl group, a 2,4,6-triisopropylbenzenesulfonyl group, a 1-naphthalenesulfonyl group, a 2-naphthalenesulfonyl group, and a 4-biphenylsulfonyl group.

[0056] Examples of the aralkylsulfonylamino group include a benzylsulfonylamino group.

[0057] Examples of the arylsulfonylamino group include a benzenesulfonylamino group and a toluenesulfonylamino group.

[0058] Examples of the acyl group include an acetyl group, a propionyl group, an acryloyl group, a methacryloyl group, a benzoyl group, a toluoyl group, and a 2-naphthoyl group.

[0059] Examples of the acylamino group include an acetylamino group, a propionylamino group, a benzoylamino group, and a toluoylamino group.

[0060] Examples of the (acyl having 2 to 10 carbon atoms)oxycarbonylamino group include an acetyloxycarbonylamino group, a propionyloxycarbonylamino group, a benzoyloxycarbonylamino group, and a toluoyloxycarbonylamino group.

[0061] Examples of the (alkyl having 1 to 12 carbon atoms)oxycarbonylamino group include a methoxycarbonylamino group and a butoxycarbonylamino group.

[0062] Examples of the aralkyloxycarbonylamino group include a benzyloxycarbonylamino group, a p-methoxybenzyloxycarbonylamino group, and a p-nitrobenzyloxycarbonylamino group.

[0063] Examples of the (aralkyl having 7 to 12 carbon atoms)aralkyloxycarbonylamino group include a phenethyloxycarbonylamino group, a 3-phenylpropyloxycarbonylamino group, a 4-phenylbutyloxycarbonylamino group, a (1-naphthyl)methyloxycarbonylamino group, and a (2-naphthyl)methyloxycarbonylamino group.

[0064] Examples of the (aryl having 6 to 15 carbon atoms)oxycarbonylamino group include a phenoxycarbonylamino group and a tolyloxycarbonylamino group.

[0065] Two adjacent R in the general formula (2) 3 may be bonded together to form an aromatic or non-aromatic ring together with the carbon atom to which they are attached, preferably an aromatic ring, e.g., R 3 may form a naphthalene ring together with the aromatic ring to which it is bonded.

[0066] Of these, alkyl groups having 1 to 4 carbon atoms are more preferred.

[0067] R 4 , R 5 is preferably a hydrogen atom or a methyl group.

[0068] a, b, and c are independently an integer of 0 to 4, and a+c is an integer of 0 to 5. a and b are more preferably 0, and c is preferably 0 or 1.

[0069] n is preferably 0 or 1, and more preferably 0.

[0070] Y is preferably a divalent organic group, and examples thereof include a divalent organic group obtained by removing two hydrogen atoms from a saturated or unsaturated aliphatic hydrocarbon or alicyclic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from an aliphatic hydrocarbon or alicyclic hydrocarbon linked by a linking group containing a hetero element, a divalent organic group obtained by removing two hydrogen atoms from a monocyclic aromatic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from a polycyclic aromatic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a single bond, a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group formed by removing two hydrogen atoms from a saturated or unsaturated aliphatic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group containing a hetero element, and a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group formed by removing two hydrogen atoms from an aromatic hydrocarbon.

[0071] Examples of the divalent organic group obtained by removing two hydrogen atoms from the saturated or unsaturated aliphatic hydrocarbon or alicyclic hydrocarbon include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a hexamethylene group, an octamethylene group, an isopropylidene group, a cyclohexanediyl group, a vinylene group, a propenylene group, and a 1-butenylene group.

[0072] Examples of divalent organic groups obtained by removing two hydrogen atoms from an aliphatic hydrocarbon or alicyclic hydrocarbon linked by a linking group containing a hetero element such as -O-, -S-, -SO2-, -C(=O)- include -C2H4OC2H4-, -C2H4OC2H4OC2H4-, -C2H4SC2H4-, -C2H4-SO2-C2H4-, -C2H4COC2H4-, etc.

[0073] Examples of divalent organic groups obtained by removing two hydrogen atoms from a monocyclic aromatic hydrocarbon include benzene, toluene, xylene, mesitylene, benzyl, and ethylbenzene.

[0074] Examples of the divalent organic group obtained by removing two hydrogen atoms from a polycyclic aromatic hydrocarbon such as naphthalene or a substituted naphthalene include a naphthalenediyl group, a 2,6-naphthalenediyl group, a 1,8-naphthalenediyl group, and a 2,3-naphthalenediyl group.

[0075] Examples of the divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by single bonds, such as biphenyl and substituted biphenyl, include a biphenyldiyl group.

[0076] Examples of the divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group obtained by removing two hydrogen atoms from the saturated or unsaturated aliphatic hydrocarbon include diphenylmethane and 2,2-diphenylpropane.

[0077] Examples of the divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group containing a hetero element include diphenyl ether, diphenoxyethane, di(phenoxyethyl) ether, diphenyl sulfide, and diphenyl sulfone.

[0078] More preferred examples of Y include divalent organic groups obtained by removing two hydrogen atoms from a monocyclic or polycyclic aromatic hydrocarbon, such as a phenylene group, a 1,3-phenylene group, a 1,4-phenylene group, a 1,2-phenylene group, a biphenyl group, a 4,4'-biphenyl group, a 3,4'-biphenyl group, a 3,3'-biphenyl group, an oxydiphenyl group, a 4,4'-oxydiphenyl group, a 3,4'-oxydiphenyl group, or a 3,3'-oxydiphenyl group; divalent organic groups obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by single bonds; and divalent organic groups obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group containing a hetero element.

[0079] Z 2are sulfonyloxy groups or sulfonyl groups, which may be the same or different, and are more preferably sulfonyloxy groups, and further preferably the same.

[0080] More specifically, 1,3-bis-(3-[3-phenylureido]phenyloxysulfonyl)benzene, 1,3-bis-(3-[3-{m-tolyl}ureido]phenyloxysulfonyl)benzene, 1,3-bis-(4-[3-{m-tolyl}ureido]phenyloxysulfonyl)benzene, 4,4'-bis-(3-[3-{m-tolyl}ureido]phenyloxysulfonyl)biphenyl, 4,4'-bis-(3-[3-{m-tolyl}ureido]phenyloxysulfonyl)biphenyl, 4,4'-bis-(3-[3-phenylureido]phenyloxysulfonyl)diphenyl ether, 4,4'-bis-(3-[3-phenylureido]phenyloxysulfonyl)biphenyl, 1,3-bis-(3-[3-{p-tolyl}ureido]phenyloxysulfonyl)benzene, 1,3-bis-(3-[3-{1-naphthyl}ureido]phenyloxysulfonyl)benzene, and the like.

[0081] The thermosensitive color former of the present invention preferably contains a compound represented by the general formula (3). The compound represented by the general formula (3) is as follows.

[0082] [ka]

[0083] R 6 is a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom.

[0084] R 6 As the R 1 Among them, a phenyl group substituted with a linear or branched alkyl group having 1 to 12 carbon atoms, an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms, a benzyl group, and the like are more preferred.

[0085] R 7 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms. Examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group, and among these, a methyl group is more preferable.

[0086] Each of l and m is preferably 0 or 1, and more preferably 0.

[0087] Z 3 is preferably a sulfonyloxy group, a sulfonyl group, or a sulfonamide group, and more preferably a sulfonyloxy group or a sulfonamide group.

[0088] More specifically, examples thereof include N-[2-(3-phenylureido)phenyl]benzenesulfonamide, N-benzyl-N'-3-(p-toluenesulfonyloxyphenyl)urea, 3-[(4-methylbenzenesulfonyl)methyl]-1-phenylurea, 3-[4-(octane-1-sulfonyl)phenyl]-1-phenylurea, 1-(benzenesulfonyl)-3-phenylurea, and 1-(4-methylphenylsulfonyl)-3-phenylurea.

[0089] The thermosensitive color former of the present invention preferably contains a compound represented by the general formula (4). The compound represented by the general formula (4) is as follows.

[0090] [ka]

[0091] R 8 represents a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms and substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms and substituted with a halogen atom, and may be the same or different.

[0092] R 8 As the R 1 Among them, a phenyl group, a p-tolyl group, a m-tolyl group, an o-tolyl group, a mesitylene group, a 2-naphthyl group, a methyl group, an ethyl group, a benzyl group, a p-ethylbenzyl group, a p-methoxybenzyl group, and the like are more preferable.

[0093] R 9 is preferably a methyl group, and R in the benzene ring of the general formula (4) is preferably a methyl group. 9 The position is 3rd, 4th or 5th.

[0094] d is an integer of 0 to 4, and is more preferably 0.

[0095] Z 4 and Z 5 is preferably a sulfonyloxy group, a sulfonyl group or a sulfonamide group, more preferably a sulfonyloxy group or a sulfonyl group, and -Z in the benzene ring of the general formula (4) is 5 The -position is the 3rd, 4th or 5th position, more preferably the 3rd position.

[0096] More specifically, examples thereof include Np-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea, N-benzyl-N'-3-(p-toluenesulfonyloxy)phenylurea, and the like.

[0097] At least one of the color developers represented by the general formulae (1) to (5) is preferably contained in the thermosensitive color former in an amount of 1 to 70% by mass, more preferably 5 to 50% by mass, and even more preferably 10 to 40% by mass. If the amount of at least one of the compounds represented by the general formulae (1) to (5) is less than 1% by mass, the color developing effect is difficult to achieve, whereas if it exceeds 70% by mass, the dispersion stability of the thermosensitive color former itself may be poor, and there is a risk of causing a decrease in heat resistance or solvent resistance during printing.

[0098] The heat-sensitive color former of the present invention preferably contains a leuco dye. As the leuco dye, any of those known in the field of conventional pressure-sensitive or heat-sensitive recording materials can be used, and there is no particular limitation, but triarylmethane compounds, fluoran compounds, fluorene compounds, divinyl compounds, diphenylmethane compounds, thiazine compounds, spiro compounds, etc. are preferred. These leuco dyes can be used alone or in combination of two or more.

[0099] Examples of the triarylmethane compounds include 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide and 3,3-bis(p-dimethylaminophenyl)phthalide.

[0100] Examples of the fluoran-based compounds include 3-diethylamino-6-methylfluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-(o,p-dimethylanilino)fluoran, 3-diethylamino-6-methyl-7-chlorofluoran, 3-diethylamino-6-methyl-7-(m-trifluoromethylanilino)fluoran, 3-diethylamino-6-methyl-7-(o-chloroanilino)fluoran, 3-diethylamino-6-methyl-7-(p-chloroanilino)fluoran, 3-diethylamino-6-methyl-7-(o-chloroanilino)fluoran, 3-Diethylamino-6-methyl-7-(o-fluoroanilino)fluoran, 3-Diethylamino-6-methyl-7-(m-methylanilino)fluoran, 3-Diethylamino-6-methyl-7-n-octylanilinofluoran, 3-Diethylamino-6-methyl-7-n-octylaminofluoran, 3-Diethylamino-6-methyl-7-benzylaminofluoran, 3-Diethylamino-6-methyl-7-dibenzylaminofluoran, 3-Diethylamino-6-methyl-7-(3-methylphenylamino)fluoran, 3-Diethylamino-6-chlor ... Fluoro-7-methylfluoran, 3-diethylamino-6-chloro-7-anilinofluoran, 3-diethylamino-6-chloro-7-p-methylanilinofluoran, 3-diethylamino-6-ethoxyethyl-7-anilinofluoran, 3-diethylamino-7-methylfluoran, 3-diethylamino-7-octylaminofluoran, 3-diethylamino-7-benzylaminofluoran, 3-diethylamino-7-chlorofluoran, 3-diethylamino-7-bromofluoran, 3-diethylamino-7-phenoxyfluoran, 3-diethylamino-7-phenoxyfluoran, Ethylamino-7-phenylfluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-diethylamino-7-(o-chloroanilino)fluoran, 3-diethylamino-7-(p-chloroanilino)fluoran, 3-diethylamino-7-(o-fluoroanilino)fluoran, 3-diethylamino-7-(4-nitroanilino)fluoran, 3-diethylamino-7-(3,4-dichloroanilino)fluoran, 3-diethylamino-benzo[a]fluoran, 3-diethylamino-benzo[c]fluoran,3-Diethylamino-7,8-dibenzofluoran, 3-Dibutylamino-6-methyl-fluoran, 3-Dibutylamino-6-methyl-7-anilinofluoran, 3-Dibutylamino-6-methyl-7-(o,p-dimethylanilino)fluoran, 3-Dibutylamino-6-methyl-7-(o-chloroanilino)fluoran, 3-Dibutylamino-6-methyl-7-(p-chloroanilino)fluoran, 3-Dibutylamino-6-methyl-7-(o-fluoroanilino)fluoran, 3-Dibutylamino-6-methyl-7-(m-trifluoran p-methylanilino)fluoran, 3-dibutylamino-6-methyl-7-chlorofluoran, 3-dibutylamino-6-ethoxyethyl-7-anilinofluoran, 3-dibutylamino-6-chloro-7-anilinofluoran, 3-dibutylamino-6-methyl-7-p-methylanilinofluoran, 3-dibutylamino-7-(o-chloroanilino)fluoran, 3-dibutylamino-7-(o-fluoroanilino)fluoran, 3-di-n-pentylamino-6-methyl-7-anilinofluoran, 3-di-n-pentylamino-6-methyl -7-(p-chloroanilino)fluoran, 3-di-n-pentylamino-7-(m-trifluoromethylanilino)fluoran, 3-di-n-pentylamino-6-chloro-7-anilinofluoran, 3-di-n-pentylamino-7-(p-chloroanilino)fluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 3-(N-methyl-N-propylamino)-6-methyl-7-anilinofluoran, 3-(N-methyl-N-cyclohexylamino)-6-methyl-7- Anilinofluoran, 3-(N-methyl-N-isoamylamino)-7-phenoxyfluoran, 3-(N-ethyl-N-cyclohexylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-hexylamino)-6-methyl-7-(p-chloroanilino)fluoran, 3-(N-ethyl-N-tolyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isoamylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isoamylamino)-6-chloro-7-anilinofluoran,3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isobutylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-ethoxypropylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-tolyl)amino-6-methyl-7-phenethylaminofluoran, 3-(N-ethyl-Nn-hexylamino)-7-(o-chloroanilino)fluoran, 3-(N-ethyl-Np-tolylamino)-7-(N-phenyl-N-methylamino)fluoran ethylamino)fluoran, 3-(N-methyl-N-isoamylamino)-7,8-benzofluoran, 3-cyclohexylamino-6-chlorofluoran, 3-pyrrolidino-6-chlorofluoran, 3-pyrrolidino-7-dibenzylaminofluoran, 2-(4-oxahexyl)-3-dimethylamino-6-methyl-7-anilinofluoran, 2-(4-oxahexyl)-3-diethylamino-6-methyl-7-anilinofluoran, 2-(4-oxahexyl)-3-dipropylamino-6-methyl-7-anilinofluoran, 2-Methyl-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 2-Methoxy-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 2-Chloro-3-methyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 2-Chloro-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 2-Nitro-6-p-(p-diethylaminophenyl)aminoanilinofluoran, 2-Amino-6-p-(p-diethylaminophenyl)aminoanilinofluoran, 2-Diethylaminophenyl 2-phenyl-6-methyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 2-benzyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 2-hydroxy-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 3-methyl-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 3-diethylamino-6-p-(p-diethylaminophenyl)aminoanilinofluoran,Examples of the fluoran include 3-diethylamino-6-p-(p-dibutylaminophenyl)aminoanilinofluoran, 2,4-dimethyl-6-[(4-dimethylamino)anilino]-fluoran, and 3,6-dimethoxyfluoran.

[0101] Examples of the fluorene-based compounds include 3,6,6'-tris(dimethylamino)spiro[fluorene-9,3'-phthalide], 3,6,6'-tris(diethylamino)spiro[fluorene-9,3'-phthalide], and the like.

[0102] Examples of the divinyl compounds include 3,3-bis-[2-(p-dimethylaminophenyl)-2-(p-methoxyphenyl)ethenyl]-4,5,6,7-tetrabromophthalide, 3,3-bis-[2-(p-dimethylaminophenyl)-2-(p-methoxyphenyl)ethenyl]-4,5,6,7-tetrachlorophthalide, 3,3-bis-[1,1-bis(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrabromophthalide, and 3,3-bis-[1-(4-methoxyphenyl)-1-(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide.

[0103] Examples of the diphenylmethane compound include 4,4'-bisdimethylaminobenzhydrin benzyl ether, N-halophenylleucoauramine, and N-2,4,5-trichlorophenylleucoauramine.

[0104] Examples of the thiazine compounds include benzoyl leuco methylene blue and p-nitrobenzoyl leuco methylene blue.

[0105] Examples of the spiro compounds include 3-methyl-spiro-dinaphthopyran, 3-ethyl-spiro-dinaphthopyran, 3,3'-dichloro-spiro-dinaphthopyran, 3-benzyl-spiro-dinaphthopyran, 3-methylnaphtho-(3-methoxybenzo)-spiropyran, and 3-propyl-spiro-dibenzopyran.

[0106] Other examples include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-octyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-cyclohexylethylamino-2-methoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, and 3-(1-ethyl-2-methylindol-3-yl)-3-(4-diethylamino-2-n-hexyloxyphenyl). )-4-azaphthalide, 3-(1-ethyl-2-methylindol-3-yl)-3-(4-diethylamino)-2-methylphenyl-4-azaphthalide, 3-(2-methyl-1-n-octyl indol-3-yl)-3-(4-diethylamino-2-ethoxyphenyl)-4-azaphthalide, 3,3-bis(1-ethyl-2-methylindol-3-yl)phthalide, 3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide, 3,3-bis(1,2-dimethylindol-3-yl)-5-dimethylaminophthalide, 3,3-bis (1,2-dimethylindol-3-yl)-6-dimethylaminophthalide, 3,3-bis(9-ethylcarbazol-3-yl)-5-dimethylaminophthalide, 3,3-bis(2-phenylindol-3-yl)-5-dimethylaminophthalide, 3-(p-dimethylaminophenyl)-3-(1,2-dimethylindol-3-yl)phthalide, 3-(p-dimethylaminophenyl)-3-(2-methylindol-3-yl)phthalide, 3-(p-dimethylaminophenyl)-3-(2-phenylindol-3-yl)phthalide, 3-(p-dimethylaminophenyl)-3-(2-phenylindol-3-yl)phthalide, methylaminophenyl)-3-(1-methylpyrrol-2-yl)-6-dimethylaminophthalide, 3-(p-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)phthalide, 3,6-bis(diethylamino)fluoran-γ-(3'-nitro)anilinolactam, 3,6-bis(diethylamino)fluoran-γ-(4'-nitro)anilinolactam, 1,1-bis-[2',2',2'',2''-tetrakis-(p-dimethylaminophenyl)-ethenyl]-2,2-dinitrileethane, 1,1-bis-[2',2',2'',2''-tetrakis-(p-dimethylaminophenyl)-ethenyl]-2-β-naphthoylethane, 1,1-bis-[2',2',2'',2''-tetrakis-(p-dimethylaminophenyl)-ethenyl]-2,2-diacetylethane, bis-[2,2,2',2'-tetrakis-(p-dimethylaminophenyl)-ethenyl]-methylmalonic acid dimethyl ester, 2,2-bis{4-[6'-(N-cyclohexyl-N-methylamino)-3'-methylspiro[phthalido-3,9'-xanthene]-2'-ylamino]phenyl}propane, etc.,

[0107] The leuco dye is preferably contained in the thermosensitive color former in an amount of 1 to 20% by mass, more preferably 3 to 15% by mass, and even more preferably 5 to 10% by mass. If the amount of the leuco dye is less than 1% by mass, the coloring effect is difficult to achieve, and if it exceeds 20% by mass, the dispersibility of the thermosensitive color former itself is poor, so that the cohesive force of the thermosensitive coloring layer film cannot be obtained and there is a risk of poor adhesion to the plastic film substrate. The content ratio of the developer and the leuco dye contained in the thermosensitive color former is preferably developer / leuco dye=7 / 1 to 0.5 / 1, more preferably 5 / 1 to 1 / 1, and even more preferably 4 / 1 to 2 / 1. When the content ratio is within the above range, the thermosensitive color former has excellent thermosensitive color development properties.

[0108] It is preferable that the thermal color former of the present invention contains an aqueous resin. As the aqueous resin, any conventionally known resin can be used as long as it is soluble or dispersible in an aqueous medium. The aqueous medium refers to a medium containing water or a hydrophilic solvent as a component. Among them, a water-soluble resin or an aqueous emulsion resin is more preferable.

[0109] The water-soluble resin has a water-soluble substituent such as an ionic group such as a sulfonyl group or a carboxyl group, or a hydroxyl group in the molecule, and dissolves in water. For example, water-soluble polyacrylamide, water-soluble acrylic resin, water-soluble polyester resin, polyvinyl alcohol, polyvinyl formal, polyvinyl butyral, or other polyvinyl alcohol resin, water-soluble nylon resin, water-soluble alkyd resin, water-soluble melamine resin, water-soluble urea resin, water-soluble phenol resin, water-soluble epoxy resin, water-soluble polybutadiene resin, water-soluble urethane resin, water-soluble acrylic / styrene resin, water-soluble vinyl acetate / acrylic copolymer resin, water-soluble styrene / maleic acid copolymer resin, water-soluble fluorine resin, water-soluble polyisocyanate resin, polystyrene resin, polyvinylpyrrolidone, polyethylene oxide, polyvinyl acetate, carboxymethylcellulose, water-soluble polyether resin, and copolymers thereof, as well as natural polymer compounds such as starch, gelatin, casein, gum arabic, chitosan, dextran, and guar gum. Among them, water-soluble acrylic resin and water-soluble polyester resin are more preferable. In particular, water-soluble polyester resin is even more preferable.

[0110] The aqueous emulsion resin refers to a state in which resin particles are dispersed in an aqueous medium or the like, and it does not matter whether the resin particles are solid or liquid. Examples of resin particles include polyamides, polyimides, low-density polyethylene, high-density polyethylene, poly(meth)acrylic acid esters, polystyrenes such as polystyrene and its derivatives, polyvinyl chloride, phenolic resins, melamine resins, urea resins, epoxy resins, polybutadiene resins, polycarbonates, alkyd resins, fluororesins, vinyl acetate resins, polyisocyanate resins, chlorinated polyolefin resins, and copolymers thereof. Among these, polystyrenes such as poly(meth)acrylic acid esters, polystyrene and its derivatives are more preferred. In particular, polystyrenes are more preferred, and it is preferred to contain acidic monomer units such as acrylic acid units and methacrylic acid units.

[0111] The aqueous resin is preferably contained in the thermosensitive color former in an amount of 1 to 50% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 30% by mass. If the amount of the aqueous resin is less than 1% by mass, the dispersibility of the thermosensitive color former itself is poor, so that the cohesive force of the thermosensitive color former coating film may not be obtained or there may be a risk of poor adhesion to the plastic film substrate, whereas if the amount of the aqueous resin is more than 50% by mass, there may be a risk of a decrease in print density or poor flowability.

[0112] The heat-sensitive color former of the present invention preferably contains alcohol. Examples of alcohol include methanol, ethanol, propyl alcohol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol, tert-butanol, ethylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,4-pentanediol, 2,5-hexanediol, 1,6-hexanediol, triethylene glycol, 1-methyl-1,3-butylene glycol, 2-methyl-1,3-butylene glycol, 2,4-diethyl-1,5-pentanediol, 2,2-diethyl-1,3-propanediol, tripropylene glycol, 1,2-propylene glycol, 2-methyl-1,5-pentanediol, 2-methyl-1,4-pentanediol ... Preferred are hexanediol, 2-methyl-2,4-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,6-hexanediol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and among these, methanol, ethanol, propyl alcohol, isopropyl alcohol, normal propyl alcohol, and propylene glycol monomethyl ether are more preferred.

[0113] The alcohol is preferably contained in the thermosensitive color developer in an amount of 1 to 50% by mass, more preferably 2 to 40% by mass, and even more preferably 5 to 20% by mass. If the amount of the alcohol is less than 1% by mass, the colorant may be difficult to dry and may be less suitable for high-speed printing, whereas if the amount of the alcohol is more than 50% by mass, the colorant may have a lower print density and poor flowability.

[0114] In the heat-sensitive color former of the present invention, a sensitizer can be used as required, and any of the conventionally known sensitizers can be used. For example, fatty acid amides such as stearic acid amide, bisstearic acid amide, N-hydroxymethylstearic acid amide, N-stearylstearic acid amide, ethylene bisstearic acid amide, methylene bisstearic acid amide, methylolstearic acid amide, and palmitic acid amide, p-toluenesulfonamide, stearic acid, calcium, zinc, aluminum, and other fatty acid metal salts such as behenic acid and palmitic acid, N-stearyl urea, benzyl-2-naphthyl ether, 4-benzylbiphenyl, 2,2'-bis(4-methoxyphenoxy)diethyl ether, α,α'-diphenoxyxylene, bis(4-methoxyphenyl)ether, p-benzylbiphenyl, diphenyl sulfone, benzyl benzyloxybenzoate, 2-benzyloxynaphthalene, 1,2-bis(m-tolyloxy)ethane, 1,2-bis(p- tolyloxy)ethane, 1,2-bis(phenoxy)ethane, 1,2-bis(3-methylphenoxy)ethane, 1,3-bis(phenoxy)propane, dibenzyl oxalate, p-methylbenzyl oxalate, bis(4-methylbenzyl)oxalate, bis(4-chlorobenzyl)oxalate, diphenyl adipate, dimethyl terephthalate, dibenzyl terephthalate, phenyl benzenesulfonate, bis(4 -allyloxyphenyl)sulfone, 1,2-diphenoxyethane, 4-acetylacetophenone, m-terphenyl, 1-hydroxy-2-naphthoic acid, acetoacetic anilides, fatty acid anilides, and the like can be mentioned, and among these, 1,2-bis(3-methylphenoxy)ethane, 1,2-bis(m-tolyloxy)ethane, 1,2-bis(p-tolyloxy)ethane, and 1,2-bis(phenoxy)ethane are more preferable.

[0115] It is preferable that the heat-sensitive color former of the present invention contains water. The water is not particularly limited, and tap water, well water, distilled water, ion-exchanged water, pure water, etc. can be used. Among them, it is more preferable to use distilled water, ion-exchanged water, and pure water.

[0116] The water content is the balance of the above-mentioned components.

[0117] The heat-sensitive color former of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, pigment dispersants, antistatic agents, slipping agents, plasticizers, tackifiers, curing agents, silane coupling agents, waxes, etc. Any known and commonly used ones may be appropriately selected within the range that does not impair the properties as a heat-sensitive color former.

[0118] Examples of the coloring material include inorganic or organic pigments such as amorphous silica, amorphous calcium silicate, heavy calcium carbonate, light calcium carbonate, kaolin, calcined kaolin, diatomaceous earth, talc, titanium dioxide, zinc oxide, aluminum hydroxide, magnesium hydroxide, barium sulfate, colloidal silica, polystyrene powder, nylon powder, urea-formalin resin filler, styrene-methacrylic acid copolymer, styrene-butadiene copolymer, and hollow plastic pigment.

[0119] The thermosensitive color former of the present invention is preferably used in gravure printing, and may be applied as is, but may also be diluted with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) to adjust the viscosity to a desired level depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0120] The dilution solvent may be any solvent capable of adjusting the viscosity of the ink composition, and examples of the dilution solvent include organic solvents and water. Commercially available solvents are also usable, and are not particularly limited. Commercially available solvents include WA734 solvent (alcohol-based water-based solvent), WA735 solvent (alcohol-based water-based solvent), WA736 solvent (alcohol-based solvent), TA50 solvent (alcohol-based solvent), and TA52 solvent (alcohol-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0121] The thermal recording laminate of the present invention preferably has a thermal color developing layer made of the above-mentioned thermal color developing agent.

[0122] The thickness of the thermosensitive coloring layer is preferably 0.1 to 5 μm, and more preferably 0.2 to 3 μm. If the thickness of the thermosensitive coloring layer is less than 0.1 μm, the color density after printing may be insufficient, and if it exceeds 5 μm, blocking may occur.

[0123] The thermosensitive recording laminate of the present invention preferably has an aqueous coating layer made of an aqueous coating agent on the thermosensitive color developing layer.

[0124] The aqueous coating agent preferably contains a water-soluble resin and water.

[0125] The water-soluble resin used in the water-based coating agent may be the same as that used in the heat-sensitive color former. Among them, polyvinyl alcohols are more preferable. These water-soluble resins may be used alone or in combination of two or more.

[0126] The water-soluble resin is preferably contained in the aqueous coating agent in an amount of 1 to 50% by mass, and more preferably 2 to 30% by mass. If the amount of the water-soluble resin is less than 1% by mass, the film-forming properties of the aqueous coating layer are poor, whereas if it exceeds 50% by mass, the ink fluidity is poor and manufacturability is poor.

[0127] The water is not particularly limited, and tap water, well water, distilled water, ion-exchanged water, pure water, etc. can be used. In addition, the ink may contain a solvent that is usually used in gravure ink. For example, aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, cyclohexane, methylcyclohexane, and ethylcyclohexane, alcohol solvents such as methanol, ethanol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol, and tert-butanol, ester solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, and tert-butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ... Examples of the glycol ether solvents include glycol ether solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and esterified products thereof. As the esterified products, acetates are mainly selected, for example, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, and methyl ethyl ketone are more preferable. These can be used alone or in combination of two or more.

[0128] The water content in the aqueous coating agent is preferably within the range of 1 to 50% by mass. If it is less than 1% by mass, wetting during printing will be poor, and if it exceeds 50% by mass, the viscosity will increase and manufacturing suitability will be poor.

[0129] The aqueous coating agent of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, curing agents, silane coupling agents, waxes, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties of the aqueous coating agent.

[0130] The aqueous coating agent of the present invention is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0131] The dilution solvent may be any solvent that can adjust the viscosity of the aqueous coating agent, and examples of the dilution solvent include organic solvents and water. Commercially available solvents are also available, and are not particularly limited. Commercially available solvents include WA734 solvent (alcohol-based solvent), WA735 solvent (alcohol-based solvent), WA736 solvent (alcohol-based solvent), TA50 solvent (alcohol-based solvent), and TA52 solvent (alcohol-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0132] The thickness of the aqueous coating layer is preferably 0.01 to 2 μm, more preferably 0.05 to 1.4 μm, and even more preferably 0.1 to 1.2 μm. If the thickness of the aqueous coating layer is less than 0.01 μm, the film-forming properties of the aqueous coating layer are poor, and if it exceeds 2 μm, it may be difficult to dry and may be poorly suited for high-speed printing.

[0133] The heat-sensitive recording laminate of the present invention preferably further has an overcoat layer made of an overcoat agent on the aqueous coating layer.

[0134] The overcoat agent preferably contains a thermoplastic resin, a polyisocyanate, and an organic solvent.

[0135] The thermoplastic resin is preferably an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, or a fiber-based resin. Of these, an acrylic resin, a polyurethane resin, or a vinyl chloride-vinyl acetate copolymer is more preferable. These may be used alone or in combination of two or more kinds.

[0136] The overcoat agent preferably contains the thermoplastic resin in an amount of 1 to 50% by mass, and more preferably 2 to 45% by mass. If the amount of the thermoplastic resin is less than 1% by mass, the overcoat layer will have poor film-forming properties and will not be able to effectively protect the thermosensitive color developing layer. If the amount of the thermoplastic resin is more than 50% by mass, blocking may occur.

[0137] Examples of the polyisocyanate include alicyclic diisocyanates such as isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, and methylcyclohexylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexaethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, diisocyanate dimer diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, butane-1,4-diisocyanate, and pentane-1,5-diisocyanate. Examples of the isocyanate include aliphatic diisocyanates such as xylylene diisocyanate (XDI) and their trimethylolpropane trimers, tolylene diisocyanate (TDI), α,α,α',α'-tetramethylxylylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, and tetraalkyldiphenylmethane diisocyanate, as well as modified versions thereof. Among these, alicyclic diisocyanates, aliphatic diisocyanates and araliphatic diisocyanates are more preferred. These may be used alone or in combination of two or more.

[0138] The polyisocyanate is preferably contained in the overcoat agent in an amount of 1 to 50% by mass, more preferably 2 to 45% by mass. If the amount of the polyisocyanate is less than 1% by mass, it is difficult to obtain a crosslinking effect, and if it exceeds 50% by mass, blocking may occur.

[0139] The content ratio of the thermoplastic resin and the polyisocyanate contained in the overcoat coating agent is preferably 100 / 1 to 100 / 50, more preferably 100 / 5 to 100 / 40, and even more preferably 100 / 15 to 100 / 35, based on 100% solids of the thermoplastic resin contained in the overcoat coating agent, and the solids of the polyisocyanate, i.e., thermoplastic resin / polyisocyanate. When the content ratio is within the above range, the coating agent has excellent alcohol resistance, scratch resistance, water resistance, and oil resistance.

[0140] As the organic solvent, solvents that are usually used for gravure inks can be used, for example, aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, cyclohexane, methylcyclohexane and ethylcyclohexane, alcohol solvents such as methanol, ethanol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol and tert-butanol, ester solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate and tert-butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ... Examples of the glycol ether solvents include glycol ether solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and esterified products thereof. As the esterified products, acetates are mainly selected, for example, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, and methyl ethyl ketone are more preferable. These can be used alone or in combination of two or more.

[0141] The organic solvent content in the overcoat agent is preferably within the range of 45 to 90% by mass, and more preferably within the range of 60 to 80% by mass. If it is less than 45% by mass, the solid content will be high, the flowability will be poor, and the manufacturability of the overcoat agent will be poor, and if it exceeds 90% by mass, the viscosity will be low, and there is a risk that a beautiful printing effect will not be obtained.

[0142] The overcoat agent of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, silane coupling agents, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties of the overcoat agent.

[0143] The overcoat agent of the present invention is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0144] The dilution solvent may be any solvent that can adjust the viscosity of the overcoat agent, and may be any organic solvent. Commercially available solvents may also be used, and are not particularly limited. Commercially available solvents include TS32 solvent (ester solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-containing solvent), SL9155 solvent (non-toluene-containing solvent), CN104 solvent (non-toluene-containing solvent), AC372 solvent (non-toluene-containing solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0145] The thickness of the overcoat layer is preferably 0.05 to 5 μm, and more preferably 0.1 to 3 μm. If the thickness of the overcoat layer is less than 0.05 μm, the protective effect of the aqueous coating layer is insufficient, and if it exceeds 5 μm, blocking may occur.

[0146] The thermosensitive recording laminate of the present invention can be used to produce a print by developing the thermosensitive color developing layer using a thermal printer (for example, TH-M2 / PP, manufactured by Okura Engineering Co., Ltd.) or the like. The color density was measured by developing the thermal recording laminate with a heat sealer (manufactured by Tester Sangyo Co., Ltd.) and measuring the L * a * b * It can be evaluated by the L value measured by the method specified in the color space (CIE1976). The lower the L value, the higher the blackness and the better the color is judged to be. Reflection densitometers, spectrodensitometers, spectrophotometers, etc. can be used to measure color density. For example, a portable spectrodensitometer eXact 2 (manufactured by X-Rite) can be used.

[0147] The thermosensitive recording laminate of the present invention may have an anchor coat layer between the plastic film substrate and the thermosensitive color developing layer.

[0148] The anchor coat layer is made of an anchor coat agent, and a resin can be used for the anchor coat agent. Examples of the resin include starches such as oxidized starch, esterified starch, and etherified starch, cellulose resins such as methyl cellulose, carboxy cellulose, methoxy cellulose, methoxy cellulose, and hydroxyethyl cellulose, casein, gelatin, polyvinyl alcohols such as fully (or partially) saponified polyvinyl alcohol, carboxy modified polyvinyl alcohol, acetoacetyl modified polyvinyl alcohol, silicon modified polyvinyl alcohol, amide modified polyvinyl alcohol, sulfonic acid modified polyvinyl alcohol, and butyral modified polyvinyl alcohol, styrene-maleic anhydride copolymer latex, styrene-butadiene copolymer latex, vinyl acetate resin latex, urethane resin latex, and acrylic resin latex. These can be used alone or in combination of two or more.

[0149] The anchor coating agent can use the same organic solvent as the aqueous coating agent and the overcoat agent. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, methyl ethyl ketone, etc. can be used alone or in combination of two or more.

[0150] The anchor coating agent of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, system curing agents, silane coupling agents, waxes, etc. Any known and commonly used agent may be appropriately selected within a range that does not impair the properties of the anchor coating agent. Commercially available agents may also be used, and there are no particular limitations. Commercially available agents include LG-OX Anchor Agent D (manufactured by Tokyo Ink Co., Ltd.).

[0151] The anchor coating agent of the present invention is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0152] The dilution solvent may be any solvent that can adjust the viscosity of the anchor coating agent, and may be any organic solvent. Commercially available solvents may also be used, and are not particularly limited. Commercially available solvents include TS32 solvent (ester solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-containing solvent), SL9155 solvent (non-toluene-containing solvent), CN104 solvent (non-toluene-containing solvent), AC372 solvent (non-toluene-containing solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0153] The thickness of the anchor coat layer is preferably 0.05 to 3 μm, and more preferably 0.1 to 2 μm. If the thickness of the anchor coat layer is less than 0.05 μm, the coating amount may be small and the plastic film substrate may not be covered, and if the thickness exceeds 3 μm, blocking may occur.

[0154] The plastic film substrate is preferably at least one selected from plastic films or sheets and laminates thereof. For example, polyester films such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate, polyolefin films such as polyethylene, polypropylene, and ethylene-vinyl acetate, polystyrene films, alcohol-based films such as ethylene-vinyl alcohol and polyvinyl alcohol, polyamide films or barrier polyamide films with a barrier layer disposed between them, polycarbonate films, polyacrylonitrile films, polyimide films, cellophane, moisture-proof cellophane, transparent vapor-deposited polyester films or transparent vapor-deposited polyamide films in which a vapor-deposited layer of alumina or silica is provided on a PET film or polyamide film, various coating films coated with polyvinylidene chloride resin, polyvinyl alcohol resin, polyacrylic acid resin, etc., co-extruded films of PET and nylon, and polylactic acid films can be mentioned. These may be either stretched or unstretched, and one or more types may be laminated. Appropriate ones can be selected in consideration of mechanical strength and dimensional stability. In addition, in order to improve the adhesion of the anchor coat layer or the laminate layer, the surface may be subjected to corona treatment, low-temperature plasma treatment, frame treatment, solvent treatment, coating treatment, etc., or may be previously subjected to a coating treatment. Among them, PET film, polypropylene film, polyamide film, coating film, transparent vapor-deposited polyester film or transparent vapor-deposited polyamide film, co-extrusion film, etc. are preferred. The thickness of the plastic film substrate is not particularly limited as long as it is within a range that does not interfere with printability, winding suitability, etc., but is preferably 5 to 300 μm, more preferably 6 to 250 μm. In addition, the anchor coat agent may be printed on the plastic film substrate in advance to be used as the plastic film substrate.

[0155] The thermosensitive coloring layer, the aqueous coating layer, the overcoat layer and the anchor coating layer are preferably formed on one side of the plastic film substrate by gravure printing. In particular, it is more preferable to form them by gravure printing using a multicolor gravure printer. Since they can be formed by gravure printing, each layer can be formed on the entire surface, but each layer can also be easily formed on a part.

[0156] The thermosensitive recording laminate of the present invention may have a sealing layer on the surface of the plastic film substrate opposite to the thermosensitive color developing layer.

[0157] The sealing layer may be a layer formed by laminating a laminate having heat sealability or a known sealant film (dry lamination, non-solvent lamination, wet lamination), resin coating by extrusion lamination (extrusion lamination, co-extrusion lamination, PE sandwich lamination), lamination by heat (thermal lamination), or a layer formed by coating a heat sealing agent or a hot melt agent. Also, a layer formed by coating an adhesive or a pressure sensitive adhesive may be used.

[0158] The thickness of the sealing layer is not particularly limited, but is preferably 2 to 200 μm for a sealant film, 1 to 100 μm for a resin coating by extrusion lamination, 0.01 to 30 μm for a coating of a heat sealing agent, and 1 to 50 μm for a coating of a hot melt adhesive.

[0159] Examples of the sealant film include polyolefin films such as polyethylene, polypropylene, ethylene-vinyl acetate, and copolymers thereof, co-extruded films and colored films thereof, polystyrene films, polyacrylonitrile films, and ethylene-vinyl alcohol resin films. These films may be stretched or unstretched, and one or more types may be laminated.

[0160] When an adhesive is used in the dry lamination method, non-solvent lamination method, wet lamination method, extrusion lamination method, etc., a commercially available adhesive may be used, for example, a two-liquid or one-liquid type urethane resin adhesive, an acrylic type, an epoxy type, a polyester type, a polyethyleneimine type, a polybutadiene type, an aqueous urethane type, an isocyanate type, an organic titanium type, a starch type water-soluble adhesive, or an aqueous adhesive such as a vinyl acetate emulsion. A known application method can be used as a method for applying the adhesive to form a sealant layer, for example, a roll coater, a reverse roll coater, a gravure offset coater, a gravure coater, a microgravure coater, a knife coater, a bar coater, a wire bar coater, a die coater, a dip coater, etc. can be used. The thickness of the adhesive is not particularly limited, but is preferably in the range of about 0.001 to 10 μm, and particularly preferably in the range of 0.01 to 5 μm.

[0161] Resins that can be used for resin coating by the extrusion lamination method include thermoplastic resins such as polyethylene resins such as LDPE, LLDPE, and HDPE, polypropylene resin, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl methacrylate copolymer, ethylene-propylene copolymer, methylpentene polymer, acid-modified polyolefin resins obtained by modifying polyethylene or polypropylene with maleic acid, fumaric acid, or the like, polystyrene resin, and polybutylene terephthalate resin, and these resins can be used alone or in combination of two or more kinds.

[0162] Examples of the resin of the heat sealant include thermoplastic resins such as vinylidene chloride, shellacs, rosins, rosin-modified maleic acid resins, rosin-modified phenolic resins, nitrocellulose, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, polyamide resins, vinyl chloride-vinyl acetate copolymers, polyester resins, ketone resins, butyral resins, chlorinated polypropylene resins, chlorinated polyethylene resins, chlorinated ethylene vinyl acetate resins, ethylene vinyl acetate resins, (meth)acrylic resins, urethane resins, ethylene-vinyl alcohol resins, styrene-maleic acid resins, casein, and alkyd resins, which may be used alone or in combination of two or more. Examples include types in which these resins are dissolved in a solvent, or types dispersed in water such as acrylic emulsions, urethane emulsions, ethylene-vinyl alcohol emulsions, polyethylene emulsions, polypropylene emulsions, and ethylene vinyl acetate emulsions.

[0163] The thermal recording laminate of the present invention may have a design layer on the plastic film substrate or on the surface of the plastic film substrate opposite to the thermal coloring layer. It may further have a color ink layer. The order in which the design layer and the color ink layer are formed does not matter. The design layer may be formed over the entire surface or a part of the surface, and may be a halftone dot. The pattern layer is a layer formed using a color printing ink composition typically used in gravure printing, and is a layer on which a pattern, letters, etc. are printed. The colored ink layer is a layer formed using a white ink composition typically used in gravure printing, and is a layer used to provide contrast with the pattern layer, etc., by using solid or halftone dots, to make the layer more visible.

[0164] The thermosensitive recording laminate of the present invention is preferably used for packaging, food preservation, retort, microwave oven, agriculture, civil engineering, fishing, automobile interior / exterior, marine, daily necessities, building interior / exterior, housing equipment, medical / medical equipment, pharmaceutical, home appliances, furniture, stationery / office supplies, sales promotion, commercial, electrical / electronic industry, industrial materials, etc. Among these, it is more preferably used for packaging, retort, and microwave oven.

[0165] The overcoat set of the present invention is an overcoat set for use with a thermal recording laminate, and preferably comprises a coating agent A containing a thermoplastic resin and an organic solvent, and a curing agent B containing a polyisocyanate and an organic solvent.

[0166] In particular, it is more preferable to use the overcoat set to provide a thermosensitive color-developing layer on one side of the plastic film substrate constituting the thermosensitive recording laminate, and an overcoat layer on the aqueous coating layer provided on the thermosensitive color-developing layer.

[0167] The thermoplastic resin contained in the coating agent A is preferably an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, or a fiber-based resin. Among them, an acrylic resin, a polyurethane resin, or a vinyl chloride-vinyl acetate copolymer is more preferable. These can be used alone or in combination of two or more kinds.

[0168] The thermoplastic resin is preferably contained in an amount of 1 to 50% by mass, and more preferably 2 to 45% by mass, in coating agent A. If the amount of the thermoplastic resin is less than 1% by mass, the film-forming property of the overcoat layer is poor and the protective effect of the thermosensitive color developing layer is difficult to exhibit, whereas if the amount exceeds 50% by mass, blocking may occur.

[0169] As the organic solvent, solvents that are usually used for gravure inks can be used, for example, aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, cyclohexane, methylcyclohexane and ethylcyclohexane, alcohol solvents such as methanol, ethanol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol and tert-butanol, ester solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate and tert-butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ... Examples of the glycol ether solvents include glycol ether solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and esterified products thereof. As the esterified products, acetates are mainly selected, for example, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, and methyl ethyl ketone are more preferable. These can be used alone or in combination of two or more.

[0170] The organic solvent is preferably in the range of 45 to 90% by mass, and more preferably in the range of 60 to 80% by mass, in the coating agent A. If it is less than 45% by mass, the solid content is high, the flowability is poor, and the manufacturing suitability of the coating agent A is poor, whereas if it exceeds 90% by mass, the viscosity is low, and there is a risk that a beautiful printing effect cannot be obtained.

[0171] Coating agent A of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, silane coupling agents, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties as a coating agent.

[0172] The polyisocyanate contained in the curing agent B may be, for example, isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexylene diisocyanate, or other alicyclic diisocyanates, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexaethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, dimer diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, butane-1,4-diisocyanate, Examples of the diisocyanates include aliphatic diisocyanates such as pentane-1,5-diisocyanate and xylylene diisocyanate (XDI) and their trimethylolpropane trimers, aromatic diisocyanates such as tolylene diisocyanate (TDI), α,α,α',α'-tetramethylxylylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, and tetraalkyldiphenylmethane diisocyanate, and their modified products. Among these, alicyclic diisocyanates, aliphatic diisocyanates and araliphatic diisocyanates are more preferred. These may be used alone or in combination of two or more.

[0173] The polyisocyanate is preferably contained in an amount of 1 to 50% by mass, and more preferably 2 to 45% by mass, in the curing agent B. If the amount of the polyisocyanate is less than 1% by mass, it is difficult to obtain a crosslinking effect, and if it exceeds 50% by mass, blocking may occur.

[0174] As the organic solvent contained in the curing agent B, the same organic solvent as that in the coating agent A can be used.

[0175] The organic solvent in the curing agent is preferably in the range of 45 to 90% by mass, more preferably in the range of 60 to 80% by mass. If it is less than 45% by mass, the solid content is high, the flowability is poor, and the manufacturability of the overcoat agent is poor, whereas if it exceeds 90% by mass, the viscosity is low, and there is a risk that a beautiful printing effect cannot be obtained.

[0176] The curing agent B of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, silane coupling agents, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties as a curing agent.

[0177] The overcoat set of the present invention uses both the coating agent A and the hardener B. That is, they are used as a two-liquid mixture. The content ratio of the thermoplastic resin and the polyisocyanate contained in the two-liquid mixture is preferably 100 / 1 to 100 / 50, more preferably 100 / 5 to 100 / 40, and even more preferably 100 / 15 to 100 / 35, relative to 100% of the solid content of the thermoplastic resin contained in the two-liquid mixture, that is, the solid content of the polyisocyanate, thermoplastic resin / polyisocyanate. When the content ratio is within the above range, the composition has excellent alcohol resistance, scratch resistance, oil resistance, water resistance, and solvent resistance. The content ratio of the coating agent A and the curing agent B is preferably mixed so as to be the content ratio of the thermoplastic resin and the polyisocyanate, and is preferably coating agent A / curing agent B=100 / 1 to 100 / 30, and more preferably 100 / 5 to 100 / 15. By using the coating agent A and the curing agent B in two liquids within the above ranges, the product has excellent alcohol resistance, scratch resistance, oil resistance, water resistance, and solvent resistance.

[0178] The two-liquid mixture can be produced by mixing or dispersing the coating agent A and the curing agent B by a known method. In particular, it is more preferable to mix or disperse them at a printing factory or the like. Mixing or dispersing can be easily performed by manual stirring, but various stirrers or dispersers such as a dissolver, paint shaker, and homomixer can also be used. These devices may be used alone or in combination of two or more types.

[0179] The two-liquid mixture is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it tends to swim, and if it is more than 40 seconds, transferability during printing becomes poor.

[0180] The dilution solvent may be any solvent that can adjust the viscosity of the two-liquid mixture, and may be any organic solvent. Commercially available solvents may also be used, and are not particularly limited. Commercially available solvents include TS32 solvent (ester solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-containing solvent), SL9155 solvent (non-toluene-containing solvent), CN104 solvent (non-toluene-containing solvent), AC372 solvent (non-toluene-containing solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0181] The coating agent A can be produced by a known method by uniformly dissolving or dispersing the thermoplastic resin and various additives in the organic solvent. For dissolving or dispersing, various stirrers or dispersers such as a dissolver, a roll mill, a ball mill, a bead mill, a sand mill, an attritor, a paint shaker, an agitator, a Henschel mixer, a colloid mill, a pearl mill, an ultrasonic homogenizer, a wet jet mill, a kneader, or a homomixer can be used. These devices may be used alone or in combination of two or more. If air bubbles or coarse particles are contained in the ink composition, they are preferably removed using a known filter or centrifuge, since they deteriorate the printability and the quality of the printed matter.

[0182] The viscosity of the coating agent A is not particularly limited as long as it does not interfere with printing. In consideration of the manufacturability and handling of the coating agent used in gravure printing, it is preferable that the viscosity is 10 to 1,000 mPa·s at 25°C. If the viscosity is less than 10 mPa·s, the viscosity is too low and the pigment tends to settle, and if it is more than 1,000 mPa·s, the fluidity is poor, causing problems during ink production and making it difficult to fill the container. In this case, it can be measured using a commercially available viscometer such as a Brookfield viscometer, a cone-plate viscometer, or a B-type viscometer.

[0183] The coating agent A is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it tends to swim, and if it is more than 40 seconds, transferability during printing becomes poor.

[0184] The curing agent B can be produced by a known method by uniformly dissolving or dispersing polyisocyanate, various additives, etc., in the organic solvent. For dissolving or dispersing, various stirrers or dispersers such as a dissolver, a roll mill, a ball mill, a bead mill, a sand mill, an attritor, a paint shaker, an agitator, a Henschel mixer, a colloid mill, a pearl mill, an ultrasonic homogenizer, a wet jet mill, a kneader, a homomixer, etc., can be used. These devices may be used alone or in combination of two or more. If air bubbles or coarse particles are contained in the curing agent, they are preferably removed using a known filter or centrifuge, etc., since they deteriorate the printability and the quality of the printed matter.

[0185] A method for producing a thermal recording laminate includes the steps of preparing a plastic film substrate, a gravure printing step of forming a thermal coloring layer on one side of the plastic film substrate, the thermal coloring layer being made of a thermal coloring agent containing a leuco dye, a color developer, an aqueous resin, an alcohol, and water, a coating step of forming an aqueous coating layer on the thermal coloring layer being made of an aqueous coating agent containing a water-soluble resin and water, and a coating step of forming an overcoat layer on the aqueous coating layer being made of an overcoat agent containing a thermoplastic resin, a polyisocyanate, and an organic solvent, in which the color developer is preferably at least one of the compounds represented by the following general formula (1), the compounds represented by the following general formula (2), the compounds represented by the following general formula (3), and the compounds represented by the following general formula (4). Among these, it is more preferable that the color developer is a compound represented by the following general formula (5).

[0186] The heat-sensitive color former of the present invention preferably contains a compound represented by the general formula (1). The compound represented by the general formula (1) is as follows.

[0187] [ka]

[0188] R 1represents a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms and substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms and substituted with a halogen atom, and may be the same or different.

[0189] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a 2-ethylhexyl group, and a lauryl group.

[0190] Examples of the aralkyl group include benzyl group, 1-phenylethyl group, 2-phenylethyl group, 3-phenylpropyl group, p-methylbenzyl group, m-methylbenzyl group, m-ethylbenzyl group, p-ethylbenzyl group, p-isopropylbenzyl group, pt-butylbenzyl group, p-methoxybenzyl group, m-methoxybenzyl group, o-methoxybenzyl group, m,p-di-methoxybenzyl group, p-ethoxy-m-methoxybenzyl group, p-phenylmethylbenzyl group, p-cumylbenzyl group, p-phenylbenzyl group, o-phenylbenzyl group, m-phenylbenzyl group, p-tolylbenzyl group, m-tolylbenzyl group, o-tolylbenzyl group, and p-chlorobenzyl group, and the like.

[0191] Examples of the aryl group include unsubstituted aryl groups or aryl groups substituted with an alkyl group, an alkoxy group, an aralkyl group, an aryl group, or a halogen atom, such as a phenyl group, a p-tolyl group, an m-tolyl group, an o-tolyl group, a 2,5-dimethylphenyl group, a 2,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a 2,3-dimethylphenyl group, a 3,4-dimethylphenyl group, a mesitylene group, a p-ethylphenyl group, a p-isopropylphenyl group, a p-butylphenyl group, a p-methoxyphenyl group, a 3,4-dimethoxyphenyl group, a p-ethoxyphenyl group, a p-chlorophenyl group, a 1-naphthyl group, a 2-naphthyl group, or a t-butylated naphthyl group.

[0192] R 2 are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, and may be the same or different. R 2 may be the same or different and are the 3rd, 4th or 5th positions. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. Of these, a hydrogen atom is more preferable.

[0193] Z 1 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group. Among them, a compound containing a sulfonyloxy group represented by the following general formula (5) is more preferable. R 10 The position of -SO2-O- may be the same or different and is the 3-position, 4-position or 5-position, more preferably the 3-position.

[0194] It is more preferable that the heat-sensitive color former of the present invention contains a compound represented by the general formula (5). The compound represented by the general formula (5) is as follows.

[0195] [ka]

[0196] R 10 represents a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms and substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms and substituted with a halogen atom, and may be the same or different.

[0197] R 10 As the R 1 Among them, a phenyl group, a p-tolyl group, a m-tolyl group, an o-tolyl group, a mesitylene group, a 2-naphthyl group, a methyl group, an ethyl group, a benzyl group, a p-ethylbenzyl group, a p-methoxybenzyl group, and the like are more preferable.

[0198] More specifically, N,N'-di-[3-(p-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(o-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(benzenesulfonyloxy)phenyl]urea, N,N'-di-[(3-benzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(mesitylenesulfonyloxy)phenyl]urea, N,N'-di-[3-(4-ethylbenzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(2-naphthalenesulfonyloxy)phenyl]urea, N,N'-di-[3-(p-methoxybenzyloxy)phenyl]urea,

[0113] N,N'-di-[3-(benzylsulfonyloxy)phenyl]urea, N,N'-di-[3-(ethanesulfonyloxy)phenyl]urea, N,N'-di-[3-(p-toluenesulfonyloxy)-4-methyl-phenyl]urea, N,N'-di-[4-(p-toluenesulfonyloxy)phenyl]urea, N,N'-di-[4-(benzenesulfonyloxy)phenyl]urea, N,N'-di-[4-(ethanesulfonyloxy)phenyl]urea, N,N'-di-[2-(p-toluenesulfonyloxy)]phenylurea, and the like.

[0199] The thermosensitive color former of the present invention preferably contains a compound represented by formula (2). The compound represented by formula (2) is as follows.

[0200] [ka]

[0201] R 3 is an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkyloxyalkyl group having 3 to 12 carbon atoms, a polyoxyalkylenealkyl group having 3 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, an alkylsulfanyl group having 1 to 12 carbon atoms, an aralkylsulfanyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 14 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an aralkylsulfonyl group having 7 to 12 carbon atoms, an aryl group having 6 to 15 carbon atoms, and (aryl)oxycarbonylamino groups.

[0202] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, and a lauryl group.

[0203] Examples of the alkenyl group include a vinyl group, an allyl group, a propenyl group, and a butenyl group.

[0204] Examples of the alkyloxyalkyl group include C2H5O-C2H4-, C3H7O-C3H6-, and the like.

[0205] The polyoxyalkylene alkyl group may be O-(C2H4O)n-C2H4- (n=1 to 3), HO-(C3H6O) n -C3H6- (n = 1 to 3), etc.

[0206] Examples of the aralkyl group include a benzyl group, a p-methylbenzyl group, a p-isopropylbenzyl group, a p-butylbenzyl group, a p-chlorobenzyl group, a p-methoxybenzyl group, a m-methoxybenzyl group, a m,p-dimethoxybenzyl group, a phenethyl group, an α-phenethyl group, and a phenylpropyl group.

[0207] Examples of the aryl group include a phenyl group, a tolyl group, a p-ethylphenyl group, a p-xylyl group, a m-xylyl group, a 1,2,3-trimethylphenyl group, a mesitylene group, a 1,2,4-trimethylphenyl group (pseudocumene group), a 1-naphthyl group, a 2-naphthyl group, a biphenyl group, and a dimethylbiphenyl group.

[0208] Examples of the alkylsulfanyl group include a methylsulfanyl group and a butylsulfanyl group.

[0209] Examples of the aralkylsulfanyl group include a benzylsulfanyl group, a 1-phenylethylsulfanyl group, a 2-phenylethylsulfanyl group, a 1-phenylpropylsulfanyl group, a 2-phenylpropylsulfanyl group, a 1-phenylbutylsulfanyl group, a 2-phenylbutylsulfanyl group, a 1-naphthylmethylsulfanyl group, a 2-naphthylmethylsulfanyl group, a (1-naphthyl)ethylsulfanyl group, and a (2-naphthyl)ethylsulfanyl group.

[0210] The arylsulfanyl group includes a phenylsulfanyl group.

[0211] Examples of the alkylsulfonyl group include a methanesulfonyl group, an ethanesulfonyl group, a propanesulfonyl group, and a butanesulfonyl group.

[0212] Examples of the aralkylsulfonyl group include a benzylsulfonyl group.

[0213] Examples of the arylsulfonyl group include a benzenesulfonyl group, a toluenesulfonyl group, a 2-p-xylylenesulfonyl group, a mesitylenesulfonyl group, a 2,4,6-triisopropylbenzenesulfonyl group, a 1-naphthalenesulfonyl group, a 2-naphthalenesulfonyl group, and a 4-biphenylsulfonyl group.

[0214] Examples of the aralkylsulfonylamino group include a benzylsulfonylamino group.

[0215] Examples of the arylsulfonylamino group include a benzenesulfonylamino group and a toluenesulfonylamino group.

[0216] Examples of the acyl group include an acetyl group, a propionyl group, an acryloyl group, a methacryloyl group, a benzoyl group, a toluoyl group, and a 2-naphthoyl group.

[0217] Examples of the acylamino group include an acetylamino group, a propionylamino group, a benzoylamino group, and a toluoylamino group.

[0218] Examples of the (acyl having 2 to 10 carbon atoms)oxycarbonylamino group include an acetyloxycarbonylamino group, a propionyloxycarbonylamino group, a benzoyloxycarbonylamino group, and a toluoyloxycarbonylamino group.

[0219] Examples of the (alkyl having 1 to 12 carbon atoms)oxycarbonylamino group include a methoxycarbonylamino group and a butoxycarbonylamino group.

[0220] Examples of the aralkyloxycarbonylamino group include a benzyloxycarbonylamino group.

[0221] Examples of the (aralkyl having 7 to 12 carbon atoms)aralkyloxycarbonylamino group include a phenethyloxycarbonylamino group, a 3-phenylpropyloxycarbonylamino group, a 4-phenylbutyloxycarbonylamino group, a (1-naphthyl)methyloxycarbonylamino group, and a (2-naphthyl)methyloxycarbonylamino group.

[0222] Examples of the (aryl having 6 to 15 carbon atoms)oxycarbonylamino group include a phenoxycarbonylamino group and a tolyloxycarbonylamino group.

[0223] Two adjacent R in the general formula (2) 3 may be bonded together to form an aromatic or non-aromatic ring together with the carbon atom to which they are attached, preferably an aromatic ring, e.g., R 3 may form a naphthalene ring together with the aromatic ring to which it is bonded.

[0224] Of these, alkyl groups having 1 to 4 carbon atoms are more preferred.

[0225] R 4 , R 5 is preferably a hydrogen atom or a methyl group.

[0226] a, b, and c are independently an integer of 0 to 4, and a+c is an integer of 0 to 5. a and b are more preferably 0, and c is preferably 0 or 1.

[0227] n is preferably 0 or 1, and more preferably 0.

[0228] Y is preferably a divalent organic group, and examples thereof include a divalent organic group obtained by removing two hydrogen atoms from a saturated or unsaturated aliphatic hydrocarbon or alicyclic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from an aliphatic hydrocarbon or alicyclic hydrocarbon linked by a linking group containing a hetero element, a divalent organic group obtained by removing two hydrogen atoms from a monocyclic aromatic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from a polycyclic aromatic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a single bond, a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group formed by removing two hydrogen atoms from a saturated or unsaturated aliphatic hydrocarbon, a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group containing a hetero element, and a divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group formed by removing two hydrogen atoms from an aromatic hydrocarbon.

[0229] Examples of the divalent organic group obtained by removing two hydrogen atoms from the saturated or unsaturated aliphatic hydrocarbon or alicyclic hydrocarbon include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a hexamethylene group, an octamethylene group, an isopropylidene group, a cyclohexanediyl group, a vinylene group, a propenylene group, and a 1-butenylene group.

[0230] Examples of divalent organic groups obtained by removing two hydrogen atoms from an aliphatic hydrocarbon or alicyclic hydrocarbon linked by a linking group containing a hetero element such as -O-, -S-, -SO2-, -C(=O)- include -C2H4OC2H4-, -C2H4OC2H4OC2H4-, -C2H4SC2H4-, -C2H4-SO2-C2H4-, -C2H4COC2H4-, etc.

[0231] Examples of divalent organic groups obtained by removing two hydrogen atoms from a monocyclic aromatic hydrocarbon include benzene, toluene, xylene, mesitylene, benzyl, and ethylbenzene.

[0232] Examples of the divalent organic group obtained by removing two hydrogen atoms from a polycyclic aromatic hydrocarbon such as naphthalene or a substituted naphthalene include a naphthalenediyl group, a 2,6-naphthalenediyl group, a 1,8-naphthalenediyl group, and a 2,3-naphthalenediyl group.

[0233] Examples of the divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by single bonds, such as biphenyl and substituted biphenyl, include a biphenyldiyl group.

[0234] Examples of the divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group obtained by removing two hydrogen atoms from the saturated or unsaturated aliphatic hydrocarbon include diphenylmethane and 2,2-diphenylpropane.

[0235] Examples of the divalent organic group obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group containing a hetero element include diphenyl ether, diphenoxyethane, di(phenoxyethyl) ether, diphenyl sulfide, and diphenyl sulfone.

[0236] More preferred examples of Y include divalent organic groups obtained by removing two hydrogen atoms from a monocyclic or polycyclic aromatic hydrocarbon, such as a phenylene group, a 1,3-phenylene group, a 1,4-phenylene group, a 1,2-phenylene group, a biphenyl group, a 4,4'-biphenyl group, a 3,4'-biphenyl group, a 3,3'-biphenyl group, an oxydiphenyl group, a 4,4'-oxydiphenyl group, a 3,4'-oxydiphenyl group, or a 3,3'-oxydiphenyl group; divalent organic groups obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by single bonds; and divalent organic groups obtained by removing two hydrogen atoms from a plurality of aromatic hydrocarbons linked by a linking group containing a hetero element.

[0237] Z 2are sulfonyloxy groups or sulfonyl groups, which may be the same or different, and are more preferably sulfonyloxy groups, and further preferably the same.

[0238] More specifically, 1,3-bis-(3-[3-phenylureido]phenyloxysulfonyl)benzene, 1,3-bis-(3-[3-{m-tolyl}ureido]phenyloxysulfonyl)benzene, 1,3-bis-(4-[3-{m-tolyl}ureido]phenyloxysulfonyl)benzene, 4,4'-bis-(3-[3-{m-tolyl}ureido]phenyloxysulfonyl)biphenyl, 4,4'-bis-(3-[3-{m-tolyl}ureido]phenyloxysulfonyl)biphenyl, 4,4'-bis-(3-[3-phenylureido]phenyloxysulfonyl)diphenyl ether, 4,4'-bis-(3-[3-phenylureido]phenyloxysulfonyl)biphenyl, 1,3-bis-(3-[3-{p-tolyl}ureido]phenyloxysulfonyl)benzene, 1,3-bis-(3-[3-{1-naphthyl}ureido]phenyloxysulfonyl)benzene, and the like.

[0239] The thermosensitive color former of the present invention preferably contains a compound represented by the general formula (3). The compound represented by the general formula (3) is as follows.

[0240] [ka]

[0241] R 6 is a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom.

[0242] R 6 As the R 1 Among them, a phenyl group substituted with a linear or branched alkyl group having 1 to 12 carbon atoms, an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms, a benzyl group, and the like are more preferred.

[0243] R 7 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms. Examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group, and among these, a methyl group is more preferable.

[0244] Each of l and m is preferably 0 or 1, and more preferably 0.

[0245] Z 3 is preferably a sulfonyloxy group, a sulfonyl group, or a sulfonamide group, and more preferably a sulfonyloxy group or a sulfonamide group.

[0246] More specifically, examples thereof include N-[2-(3-phenylureido)phenyl]benzenesulfonamide, N-benzyl-N'-3-(p-toluenesulfonyloxyphenyl)urea, 3-[(4-methylbenzenesulfonyl)methyl]-1-phenylurea, 3-[4-(octane-1-sulfonyl)phenyl]-1-phenylurea, 1-(benzenesulfonyl)-3-phenylurea, and 1-(4-methylphenylsulfonyl)-3-phenylurea.

[0247] The thermosensitive color former of the present invention preferably contains a compound represented by the general formula (4). The compound represented by the general formula (4) is as follows.

[0248] [ka]

[0249] R 8 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms and substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms and substituted with a halogen atom, each of which may be the same or different,

[0250] R 8 As the R 1 Among them, a phenyl group, a p-tolyl group, a m-tolyl group, an o-tolyl group, a mesitylene group, a 2-naphthyl group, a methyl group, an ethyl group, a benzyl group, a p-ethylbenzyl group, a p-methoxybenzyl group, and the like are more preferable.

[0251] R 9 is preferably a methyl group, and R in the benzene ring of the general formula (4) is preferably a methyl group. 9 The position is 3rd, 4th or 5th.

[0252] d is an integer of 0 to 4, and is more preferably 0.

[0253] Z 4 and Z 5 is preferably a sulfonyloxy group, a sulfonyl group or a sulfonamide group, more preferably a sulfonyloxy group or a sulfonyl group, and -Z in the benzene ring of the general formula (4) is 5 The -position is the 3rd, 4th or 5th position, more preferably the 3rd position.

[0254] More specifically, examples thereof include Np-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea, N-benzyl-N'-3-(p-toluenesulfonyloxy)phenylurea, and the like.

[0255] At least one of the color developers represented by the general formulae (1) to (5) is preferably contained in the thermosensitive color former in an amount of 1 to 70% by mass, more preferably 5 to 50% by mass, and even more preferably 10 to 40% by mass. If the amount of at least one of the compounds represented by the general formulae (1) to (5) is less than 1% by mass, the color developing effect is difficult to achieve, whereas if it exceeds 70% by mass, the dispersion stability of the thermosensitive color former itself may be poor, and there is a risk of causing a decrease in heat resistance or solvent resistance during printing.

[0256] The heat-sensitive color former of the present invention preferably contains a leuco dye. As the leuco dye, any of those known in the field of conventional pressure-sensitive or heat-sensitive recording materials can be used, and there is no particular limitation, but triarylmethane compounds, fluoran compounds, fluorene compounds, divinyl compounds, diphenylmethane compounds, thiazine compounds, spiro compounds, etc. are preferred. These leuco dyes can be used alone or in combination of two or more.

[0257] Examples of the triarylmethane compounds include 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide and 3,3-bis(p-dimethylaminophenyl)phthalide.

[0258] Examples of the fluoran-based compounds include 3-diethylamino-6-methylfluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-(o,p-dimethylanilino)fluoran, 3-diethylamino-6-methyl-7-chlorofluoran, 3-diethylamino-6-methyl-7-(m-trifluoromethylanilino)fluoran, 3-diethylamino-6-methyl-7-(o-chloroanilino)fluoran, 3-diethylamino-6-methyl-7-(p-chloroanilino)fluoran, 3-diethylamino-6-methyl-7-(o-chloroanilino)fluoran, 3-Diethylamino-6-methyl-7-(o-fluoroanilino)fluoran, 3-Diethylamino-6-methyl-7-(m-methylanilino)fluoran, 3-Diethylamino-6-methyl-7-n-octylanilinofluoran, 3-Diethylamino-6-methyl-7-n-octylaminofluoran, 3-Diethylamino-6-methyl-7-benzylaminofluoran, 3-Diethylamino-6-methyl-7-dibenzylaminofluoran, 3-Diethylamino-6-methyl-7-(3-methylphenylamino)fluoran, 3-Diethylamino-6-chlor ... Fluoro-7-methylfluoran, 3-diethylamino-6-chloro-7-anilinofluoran, 3-diethylamino-6-chloro-7-p-methylanilinofluoran, 3-diethylamino-6-ethoxyethyl-7-anilinofluoran, 3-diethylamino-7-methylfluoran, 3-diethylamino-7-octylaminofluoran, 3-diethylamino-7-benzylaminofluoran, 3-diethylamino-7-chlorofluoran, 3-diethylamino-7-bromofluoran, 3-diethylamino-7-phenoxyfluoran, 3-diethylamino-7-phenoxyfluoran, Ethylamino-7-phenylfluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-diethylamino-7-(o-chloroanilino)fluoran, 3-diethylamino-7-(p-chloroanilino)fluoran, 3-diethylamino-7-(o-fluoroanilino)fluoran, 3-diethylamino-7-(4-nitroanilino)fluoran, 3-diethylamino-7-(3,4-dichloroanilino)fluoran, 3-diethylamino-benzo[a]fluoran, 3-diethylamino-benzo[c]fluoran,3-Diethylamino-7,8-dibenzofluoran, 3-Dibutylamino-6-methyl-fluoran, 3-Dibutylamino-6-methyl-7-anilinofluoran, 3-Dibutylamino-6-methyl-7-(o,p-dimethylanilino)fluoran, 3-Dibutylamino-6-methyl-7-(o-chloroanilino)fluoran, 3-Dibutylamino-6-methyl-7-(p-chloroanilino)fluoran, 3-Dibutylamino-6-methyl-7-(o-fluoroanilino)fluoran, 3-Dibutylamino-6-methyl-7-(m-trifluoran p-methylanilino)fluoran, 3-dibutylamino-6-methyl-7-chlorofluoran, 3-dibutylamino-6-ethoxyethyl-7-anilinofluoran, 3-dibutylamino-6-chloro-7-anilinofluoran, 3-dibutylamino-6-methyl-7-p-methylanilinofluoran, 3-dibutylamino-7-(o-chloroanilino)fluoran, 3-dibutylamino-7-(o-fluoroanilino)fluoran, 3-di-n-pentylamino-6-methyl-7-anilinofluoran, 3-di-n-pentylamino-6-methyl -7-(p-chloroanilino)fluoran, 3-di-n-pentylamino-7-(m-trifluoromethylanilino)fluoran, 3-di-n-pentylamino-6-chloro-7-anilinofluoran, 3-di-n-pentylamino-7-(p-chloroanilino)fluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 3-(N-methyl-N-propylamino)-6-methyl-7-anilinofluoran, 3-(N-methyl-N-cyclohexylamino)-6-methyl-7- Anilinofluoran, 3-(N-methyl-N-isoamylamino)-7-phenoxyfluoran, 3-(N-ethyl-N-cyclohexylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-hexylamino)-6-methyl-7-(p-chloroanilino)fluoran, 3-(N-ethyl-N-tolyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isoamylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isoamylamino)-6-chloro-7-anilinofluoran,3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isobutylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-ethoxypropylamino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-tolyl)amino-6-methyl-7-phenethylaminofluoran, 3-(N-ethyl-Nn-hexylamino)-7-(o-chloroanilino)fluoran, 3-(N-ethyl-Np-tolylamino)-7-(N-phenyl-N-methylamino)fluoran ethylamino)fluoran, 3-(N-methyl-N-isoamylamino)-7,8-benzofluoran, 3-cyclohexylamino-6-chlorofluoran, 3-pyrrolidino-6-chlorofluoran, 3-pyrrolidino-7-dibenzylaminofluoran, 2-(4-oxahexyl)-3-dimethylamino-6-methyl-7-anilinofluoran, 2-(4-oxahexyl)-3-diethylamino-6-methyl-7-anilinofluoran, 2-(4-oxahexyl)-3-dipropylamino-6-methyl-7-anilinofluoran, 2-Methyl-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 2-Methoxy-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 2-Chloro-3-methyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 2-Chloro-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 2-Nitro-6-p-(p-diethylaminophenyl)aminoanilinofluoran, 2-Amino-6-p-(p-diethylaminophenyl)aminoanilinofluoran, 2-Diethylaminophenyl 2-phenyl-6-methyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 2-benzyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 2-hydroxy-6-p-(p-phenylaminophenyl)aminoanilinofluoran, 3-methyl-6-p-(p-dimethylaminophenyl)aminoanilinofluoran, 3-diethylamino-6-p-(p-diethylaminophenyl)aminoanilinofluoran,Examples of the fluoran include 3-diethylamino-6-p-(p-dibutylaminophenyl)aminoanilinofluoran, 2,4-dimethyl-6-[(4-dimethylamino)anilino]-fluoran, and 3,6-dimethoxyfluoran.

[0259] Examples of the fluorene-based compounds include 3,6,6'-tris(dimethylamino)spiro[fluorene-9,3'-phthalide], 3,6,6'-tris(diethylamino)spiro[fluorene-9,3'-phthalide], and the like.

[0260] Examples of the divinyl compounds include 3,3-bis-[2-(p-dimethylaminophenyl)-2-(p-methoxyphenyl)ethenyl]-4,5,6,7-tetrabromophthalide, 3,3-bis-[2-(p-dimethylaminophenyl)-2-(p-methoxyphenyl)ethenyl]-4,5,6,7-tetrachlorophthalide, 3,3-bis-[1,1-bis(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrabromophthalide, and 3,3-bis-[1-(4-methoxyphenyl)-1-(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide.

[0261] Examples of the diphenylmethane compound include 4,4'-bisdimethylaminobenzhydrin benzyl ether, N-halophenylleucoauramine, and N-2,4,5-trichlorophenylleucoauramine.

[0262] Examples of the thiazine compounds include benzoyl leuco methylene blue and p-nitrobenzoyl leuco methylene blue.

[0263] Examples of the spiro compounds include 3-methyl-spiro-dinaphthopyran, 3-ethyl-spiro-dinaphthopyran, 3,3'-dichloro-spiro-dinaphthopyran, 3-benzyl-spiro-dinaphthopyran, 3-methylnaphtho-(3-methoxybenzo)-spiropyran, and 3-propyl-spiro-dibenzopyran.

[0264] Other examples include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-octyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-cyclohexylethylamino-2-methoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, and 3-(1-ethyl-2-methylindol-3-yl)-3-(4-diethylamino-2-n-hexyloxyphenyl). )-4-azaphthalide, 3-(1-ethyl-2-methylindol-3-yl)-3-(4-diethylamino)-2-methylphenyl-4-azaphthalide, 3-(2-methyl-1-n-octyl indol-3-yl)-3-(4-diethylamino-2-ethoxyphenyl)-4-azaphthalide, 3,3-bis(1-ethyl-2-methylindol-3-yl)phthalide, 3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide, 3,3-bis(1,2-dimethylindol-3-yl)-5-dimethylaminophthalide, 3,3-bis (1,2-dimethylindol-3-yl)-6-dimethylaminophthalide, 3,3-bis(9-ethylcarbazol-3-yl)-5-dimethylaminophthalide, 3,3-bis(2-phenylindol-3-yl)-5-dimethylaminophthalide, 3-(p-dimethylaminophenyl)-3-(1,2-dimethylindol-3-yl)phthalide, 3-(p-dimethylaminophenyl)-3-(2-methylindol-3-yl)phthalide, 3-(p-dimethylaminophenyl)-3-(2-phenylindol-3-yl)phthalide, 3-(p-dimethylaminophenyl)-3-(2-phenylindol-3-yl)phthalide, methylaminophenyl)-3-(1-methylpyrrol-2-yl)-6-dimethylaminophthalide, 3-(p-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)phthalide, 3,6-bis(diethylamino)fluoran-γ-(3'-nitro)anilinolactam, 3,6-bis(diethylamino)fluoran-γ-(4'-nitro)anilinolactam, 1,1-bis-[2',2',2'',2''-tetrakis-(p-dimethylaminophenyl)-ethenyl]-2,2-dinitrileethane, 1,1-bis-[2',2',2'',2''-tetrakis-(p-dimethylaminophenyl)-ethenyl]-2-β-naphthoylethane, 1,1-bis-[2',2',2'',2''-tetrakis-(p-dimethylaminophenyl)-ethenyl]-2,2-diacetylethane, bis-[2,2,2',2'-tetrakis-(p-dimethylaminophenyl)-ethenyl]-methylmalonic acid dimethyl ester, 2,2-bis{4-[6'-(N-cyclohexyl-N-methylamino)-3'-methylspiro[phthalido-3,9'-xanthene]-2'-ylamino]phenyl}propane, etc.,

[0265] The leuco dye is preferably contained in the thermosensitive color former in an amount of 1 to 20% by mass, more preferably 3 to 15% by mass, and even more preferably 5 to 10% by mass. If the amount of the leuco dye is less than 1% by mass, the coloring effect is difficult to achieve, and if it exceeds 20% by mass, the dispersibility of the thermosensitive color former itself is poor, so that the cohesive force of the thermosensitive coloring layer film cannot be obtained and there is a risk of poor adhesion to the plastic film substrate. The content ratio of the developer and the leuco dye contained in the thermosensitive color former is preferably developer / leuco dye=7 / 1 to 0.5 / 1, more preferably 5 / 1 to 1 / 1, and even more preferably 4 / 1 to 2 / 1. When the content ratio is within the above range, the thermosensitive color former has excellent thermosensitive color development properties.

[0266] It is preferable that the thermal color former of the present invention contains an aqueous resin. As the aqueous resin, any conventionally known resin can be used as long as it is soluble or dispersible in an aqueous medium. The aqueous medium refers to a medium containing water or a hydrophilic solvent as a component. Among them, a water-soluble resin or an aqueous emulsion resin is more preferable.

[0267] The water-soluble resin has a water-soluble substituent such as an ionic group such as a sulfonyl group or a carboxyl group, or a hydroxyl group in the molecule, and dissolves in water. For example, water-soluble polyacrylamide, water-soluble acrylic resin, water-soluble polyester resin, polyvinyl alcohol, polyvinyl formal, polyvinyl butyral, or other polyvinyl alcohol resin, water-soluble nylon resin, water-soluble alkyd resin, water-soluble melamine resin, water-soluble urea resin, water-soluble phenol resin, water-soluble epoxy resin, water-soluble polybutadiene resin, water-soluble urethane resin, water-soluble acrylic / styrene resin, water-soluble vinyl acetate / acrylic copolymer resin, water-soluble styrene / maleic acid copolymer resin, water-soluble fluorine resin, water-soluble polyisocyanate resin, polystyrene resin, polyvinylpyrrolidone, polyethylene oxide, polyvinyl acetate, carboxymethylcellulose, water-soluble polyether resin, and copolymers thereof, as well as natural polymer compounds such as starch, gelatin, casein, gum arabic, chitosan, dextran, and guar gum. Among them, water-soluble acrylic resin and water-soluble polyester resin are more preferable. In particular, water-soluble polyester resin is even more preferable.

[0268] The aqueous emulsion resin refers to a state in which resin particles are dispersed in an aqueous medium or the like, and it does not matter whether the resin particles are solid or liquid. Examples of resin particles include polyamides, polyimides, low-density polyethylene, high-density polyethylene, poly(meth)acrylic acid esters, polystyrenes such as polystyrene and its derivatives, polyvinyl chloride, phenolic resins, melamine resins, urea resins, epoxy resins, polybutadiene resins, polycarbonates, alkyd resins, fluororesins, vinyl acetate resins, polyisocyanate resins, chlorinated polyolefin resins, and copolymers thereof. Among these, polystyrenes such as poly(meth)acrylic acid esters, polystyrene and its derivatives are more preferred. In particular, polystyrenes are more preferred, and it is preferred to contain acidic monomer units such as acrylic acid units and methacrylic acid units.

[0269] The aqueous resin is preferably contained in the thermosensitive color former in an amount of 1 to 50% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 30% by mass. If the amount of the aqueous resin is less than 1% by mass, the dispersibility of the thermosensitive color former itself is poor, so that the cohesive force of the thermosensitive color former coating film may not be obtained or there may be a risk of poor adhesion to the plastic film substrate, whereas if the amount of the aqueous resin is more than 50% by mass, there may be a risk of a decrease in print density or poor flowability.

[0270] The heat-sensitive color former of the present invention preferably contains alcohol. Examples of alcohol include methanol, ethanol, propyl alcohol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol, tert-butanol, ethylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,4-pentanediol, 2,5-hexanediol, 1,6-hexanediol, triethylene glycol, 1-methyl-1,3-butylene glycol, 2-methyl-1,3-butylene glycol, 2,4-diethyl-1,5-pentanediol, 2,2-diethyl-1,3-propanediol, tripropylene glycol, 1,2-propylene glycol, 2-methyl-1,5-pentanediol, 2-methyl-1,4-pentanediol ... Preferred are hexanediol, 2-methyl-2,4-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,6-hexanediol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and among these, methanol, ethanol, propyl alcohol, isopropyl alcohol, normal propyl alcohol, and propylene glycol monomethyl ether are more preferred.

[0271] The alcohol is preferably contained in the thermosensitive color developer in an amount of 1 to 50% by mass, more preferably 2 to 40% by mass, and even more preferably 5 to 20% by mass. If the amount of the alcohol is less than 1% by mass, the colorant may be difficult to dry and may be less suitable for high-speed printing, whereas if the amount of the alcohol is more than 50% by mass, the colorant may have a lower print density and poor flowability.

[0272] In the heat-sensitive color former of the present invention, a sensitizer can be used as required, and any of the conventionally known sensitizers can be used. For example, fatty acid amides such as stearic acid amide, bisstearic acid amide, N-hydroxymethylstearic acid amide, N-stearylstearic acid amide, ethylene bisstearic acid amide, methylene bisstearic acid amide, methylolstearic acid amide, and palmitic acid amide, p-toluenesulfonamide, stearic acid, calcium, zinc, aluminum, and other fatty acid metal salts such as behenic acid and palmitic acid, N-stearyl urea, benzyl-2-naphthyl ether, 4-benzylbiphenyl, 2,2'-bis(4-methoxyphenoxy)diethyl ether, α,α'-diphenoxyxylene, bis(4-methoxyphenyl)ether, p-benzylbiphenyl, diphenyl sulfone, benzyl benzyloxybenzoate, 2-benzyloxynaphthalene, 1,2-bis(p- Examples of the bis(4-aryloxy)ethane include 1,2-bis(phenoxy)ethane, 1,2-bis(3-methylphenoxy)ethane, 1,3-bis(phenoxy)propane, dibenzyl oxalate, p-methylbenzyl oxalate, bis(4-methylbenzyl)oxalate, bis(4-chlorobenzyl)oxalate, diphenyl adipate, dimethyl terephthalate, dibenzyl terephthalate, phenyl benzenesulfonate, bis(4-allyloxyphenyl)sulfone, 1,2-diphenoxyethane, 4-acetylacetophenone, m-terphenyl, 1-hydroxy-2-naphthoic acid, acetoacetic anilides, and fatty acid anilides. Among these, 1,2-bis(3-methylphenoxy)ethane, 1,2-bis(p-tolyloxy)ethane, and 1,2-bis(phenoxy)ethane are more preferred.

[0273] It is preferable that the heat-sensitive color former of the present invention contains water. The water is not particularly limited, and tap water, well water, distilled water, ion-exchanged water, pure water, etc. can be used. Among them, it is more preferable to use distilled water, ion-exchanged water, and pure water.

[0274] The water content is the balance of the above-mentioned components.

[0275] The heat-sensitive color former of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, pigment dispersants, antistatic agents, slipping agents, plasticizers, tackifiers, curing agents, silane coupling agents, waxes, etc. Any known and commonly used ones may be appropriately selected within the range that does not impair the properties as a heat-sensitive color former.

[0276] Examples of the coloring material include inorganic or organic pigments such as amorphous silica, amorphous calcium silicate, heavy calcium carbonate, light calcium carbonate, kaolin, calcined kaolin, diatomaceous earth, talc, titanium dioxide, zinc oxide, aluminum hydroxide, magnesium hydroxide, barium sulfate, colloidal silica, polystyrene powder, nylon powder, urea-formalin resin filler, styrene-methacrylic acid copolymer, styrene-butadiene copolymer, and hollow plastic pigment.

[0277] The method for producing a thermosensitive recording laminate of the present invention preferably includes a gravure printing step of forming a thermosensitive coloring layer made of the thermosensitive color former. The thermosensitive color former can be used as is in the gravure printing step, but depending on the coating conditions and coating effect, a step of diluting the thermosensitive color former with a diluting solvent using a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) may be included, and the thermosensitive color former can be used after adjusting to a desired viscosity. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it tends to swim, and if it is more than 40 seconds, transferability during printing becomes poor.

[0278] The dilution solvent may be any solvent capable of adjusting the viscosity of the ink composition, and examples of the dilution solvent include organic solvents and water. Commercially available solvents are also usable, and are not particularly limited. Commercially available solvents include WA734 solvent (alcohol-based water-based solvent), WA735 solvent (alcohol-based water-based solvent), WA736 solvent (alcohol-based solvent), TA50 solvent (alcohol-based solvent), and TA52 solvent (alcohol-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0279] The thickness of the thermosensitive coloring layer is preferably 0.1 to 5 μm, and more preferably 0.2 to 3 μm. If the thickness of the thermosensitive coloring layer is less than 0.1 μm, the color density after printing may be insufficient, and if it exceeds 5 μm, blocking may occur.

[0280] The method for producing a thermosensitive recording laminate of the present invention preferably includes a coating step of forming an aqueous coating layer on the thermosensitive color developing layer using an aqueous coating agent.

[0281] The aqueous coating agent preferably contains a water-soluble resin and water.

[0282] The water-soluble resin used in the water-based coating agent may be the same as that used in the heat-sensitive color former. Among them, polyvinyl alcohols are more preferable. These water-soluble resins may be used alone or in combination of two or more.

[0283] The water-soluble resin is preferably contained in the aqueous coating agent in an amount of 1 to 50% by mass, and more preferably 2 to 30% by mass. If the amount of the water-soluble resin is less than 1% by mass, the film-forming properties of the aqueous coating layer are poor, whereas if it exceeds 50% by mass, the ink fluidity is poor and manufacturability is poor.

[0284] The water is not particularly limited, and tap water, well water, distilled water, ion-exchanged water, pure water, etc. can be used. In addition, the ink may contain a solvent that is usually used in gravure ink. For example, aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, cyclohexane, methylcyclohexane, and ethylcyclohexane, alcohol solvents such as methanol, ethanol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol, and tert-butanol, ester solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, and tert-butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ... Examples of the glycol ether solvents include glycol ether solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and esterified products thereof. As the esterified products, acetates are mainly selected, for example, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, and methyl ethyl ketone are more preferable. These can be used alone or in combination of two or more.

[0285] The water content in the aqueous coating agent is preferably within the range of 1 to 50% by mass. If it is less than 1% by mass, wetting during printing will be poor, and if it exceeds 50% by mass, the viscosity will increase and manufacturing suitability will be poor.

[0286] The aqueous coating agent of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, curing agents, silane coupling agents, waxes, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties of the aqueous coating agent.

[0287] The aqueous coating agent of the present invention can be used as is in the gravure printing process, but depending on the coating conditions and coating effect, a process of diluting it with a diluting solvent using a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) may be included, and it can be used after adjusting to a desired viscosity. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0288] The dilution solvent may be any solvent that can adjust the viscosity of the aqueous coating agent, and examples of the dilution solvent include organic solvents and water. Commercially available solvents are also available, and are not particularly limited. Commercially available solvents include WA734 solvent (alcohol-based solvent), WA735 solvent (alcohol-based solvent), WA736 solvent (alcohol-based solvent), TA50 solvent (alcohol-based solvent), and TA52 solvent (alcohol-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0289] The thickness of the aqueous coating layer is preferably 0.01 to 2 μm, more preferably 0.05 to 1.4 μm, and even more preferably 0.1 to 1.2 μm. If the thickness of the aqueous coating layer is less than 0.01 μm, the film-forming properties of the aqueous coating layer are poor, and if it exceeds 2 μm, it may be difficult to dry and may be poorly suited for high-speed printing.

[0290] The method for producing a thermal recording laminate of the present invention preferably further comprises a coating step of forming an overcoat layer made of an overcoat agent on the aqueous coating layer.

[0291] The overcoat agent preferably contains a thermoplastic resin, a polyisocyanate, and an organic solvent.

[0292] The thermoplastic resin is preferably an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, or a fiber-based resin. Of these, an acrylic resin, a polyurethane resin, or a vinyl chloride-vinyl acetate copolymer is more preferable. These may be used alone or in combination of two or more kinds.

[0293] The overcoat agent preferably contains the thermoplastic resin in an amount of 1 to 50% by mass, and more preferably 2 to 45% by mass. If the amount of the thermoplastic resin is less than 1% by mass, the overcoat layer will have poor film-forming properties and will not be able to effectively protect the thermosensitive color developing layer. If the amount of the thermoplastic resin is more than 50% by mass, blocking may occur.

[0294] Examples of the polyisocyanate include alicyclic diisocyanates such as isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, and methylcyclohexylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexaethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, diisocyanate dimer diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, butane-1,4-diisocyanate, and pentane-1,5-diisocyanate. Examples of the isocyanate include aliphatic diisocyanates such as xylylene diisocyanate (XDI) and their trimethylolpropane trimers, tolylene diisocyanate (TDI), α,α,α',α'-tetramethylxylylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, and tetraalkyldiphenylmethane diisocyanate, as well as modified versions thereof. Among these, alicyclic diisocyanates, aliphatic diisocyanates and araliphatic diisocyanates are more preferred. These may be used alone or in combination of two or more.

[0295] The polyisocyanate is preferably contained in the overcoat agent in an amount of 1 to 50% by mass, more preferably 2 to 45% by mass. If the amount of the polyisocyanate is less than 1% by mass, it is difficult to obtain a crosslinking effect, and if it exceeds 50% by mass, blocking may occur.

[0296] The content ratio of the thermoplastic resin and the polyisocyanate contained in the overcoat coating agent is preferably 100 / 1 to 100 / 50, more preferably 100 / 5 to 100 / 40, and even more preferably 100 / 15 to 100 / 35, based on 100% solids of the thermoplastic resin contained in the overcoat coating agent, and the solids of the polyisocyanate, i.e., thermoplastic resin / polyisocyanate. When the content ratio is within the above range, the coating agent has excellent alcohol resistance, scratch resistance, water resistance, and oil resistance.

[0297] As the organic solvent, solvents that are usually used for gravure inks can be used, for example, aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, cyclohexane, methylcyclohexane and ethylcyclohexane, alcohol solvents such as methanol, ethanol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol and tert-butanol, ester solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate and tert-butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ... Examples of the glycol ether solvents include glycol ether solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and esterified products thereof. As the esterified products, acetates are mainly selected, for example, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, and methyl ethyl ketone are more preferable. These can be used alone or in combination of two or more.

[0298] The organic solvent content in the overcoat agent is preferably within the range of 45 to 90% by mass, and more preferably within the range of 60 to 80% by mass. If it is less than 45% by mass, the solid content will be high, the flowability will be poor, and the manufacturability of the overcoat agent will be poor, and if it exceeds 90% by mass, the viscosity will be low, and there is a risk that a beautiful printing effect will not be obtained.

[0299] The overcoat agent of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, silane coupling agents, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties of the overcoat agent.

[0300] The overcoat agent of the present invention can be used as is in the gravure printing process, but depending on the coating conditions and coating effect, a process of diluting it with a diluting solvent using a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) may be included, and it can be used after adjusting to a desired viscosity. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0301] The dilution solvent may be any solvent that can adjust the viscosity of the ink composition, and may be any organic solvent. Commercially available solvents may be used, and are not particularly limited. Commercially available solvents include TS32 solvent (ester solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-containing solvent), SL9155 solvent (non-toluene-containing solvent), CN104 solvent (non-toluene-containing solvent), AC372 solvent (non-toluene-containing solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0302] The thickness of the overcoat layer is preferably 0.05 to 5 μm, and more preferably 0.1 to 3 μm. If the thickness of the overcoat layer is less than 0.05 μm, the protective effect of the aqueous coating layer is insufficient, and if it exceeds 5 μm, blocking may occur.

[0303] The thermosensitive recording laminate produced by the thermosensitive recording laminate manufacturing method of the present invention can be used to produce printed matter by coloring the thermosensitive color-developing layer using a thermal printer (e.g., TH-M2 / PP, manufactured by Okura Engineering Co., Ltd.). The color density was measured by developing the thermal recording laminate with a heat sealer (manufactured by Tester Sangyo Co., Ltd.) and measuring the L * a * b * It can be evaluated by the L value measured by the method specified in the color space (CIE1976). The lower the L value, the higher the blackness and the better the color is judged to be. Reflection densitometers, spectrodensitometers, spectrophotometers, etc. can be used to measure color density. For example, a portable spectrodensitometer eXact 2 (manufactured by X-Rite) can be used.

[0304] The method for producing a thermosensitive recording laminate of the present invention may further include a coating step of forming an anchor coat layer between the plastic film substrate and the thermosensitive color developing layer using an anchor coat agent.

[0305] Resins can be used in the anchor coating agent. Examples of resins include starches such as oxidized starch, esterified starch, and etherified starch; cellulose resins such as methyl cellulose, carboxy cellulose, methoxy cellulose, methoxy cellulose, and hydroxyethyl cellulose; casein, gelatin, polyvinyl alcohols such as fully (or partially) saponified polyvinyl alcohol, carboxy modified polyvinyl alcohol, acetoacetyl modified polyvinyl alcohol, silicon modified polyvinyl alcohol, amide modified polyvinyl alcohol, sulfonic acid modified polyvinyl alcohol, and butyral modified polyvinyl alcohol; styrene-maleic anhydride copolymer latex, styrene-butadiene copolymer latex, vinyl acetate resin latex, urethane resin latex, and acrylic resin latex. These can be used alone or in combination of two or more.

[0306] The anchor coating agent can use the same organic solvent as the aqueous coating agent and the overcoat agent. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, methyl ethyl ketone, etc. can be used alone or in combination of two or more.

[0307] The anchor coating agent of the present invention may contain, as necessary, coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, system curing agents, silane coupling agents, waxes, etc. Any known and commonly used agent may be appropriately selected within a range that does not impair the properties of the anchor coating agent. Commercially available agents may also be used, and there are no particular limitations. Commercially available agents include LG-OX Anchor Agent D (manufactured by Tokyo Ink Co., Ltd.).

[0308] The anchor coating agent of the present invention can be used as is in the gravure printing process, but depending on the coating conditions and coating effect, a process of diluting it with a diluting solvent using a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) may be included, and it can be used after adjusting to the desired viscosity. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.

[0309] The dilution solvent may be any solvent that can adjust the viscosity of the anchor coating agent, and may be any organic solvent. Commercially available solvents may also be used, and are not particularly limited. Commercially available solvents include TS32 solvent (ester solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-containing solvent), SL9155 solvent (non-toluene-containing solvent), CN104 solvent (non-toluene-containing solvent), AC372 solvent (non-toluene-containing solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0310] The thickness of the anchor coat layer is preferably 0.05 to 3 μm, and more preferably 0.1 to 2 μm. If the thickness of the anchor coat layer is less than 0.05 μm, the coating amount may be small and the plastic film substrate may not be covered, and if the thickness exceeds 3 μm, blocking may occur.

[0311] The step of preparing the plastic film substrate is preferably a step of preparing at least one selected from plastic films or sheets and laminates thereof. For example, polyester films such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate, polyolefin films such as polyethylene, polypropylene, and ethylene-vinyl acetate, alcohol-based films such as polystyrene films, ethylene-vinyl alcohol, and polyvinyl alcohol, polyamide films or barrier polyamide films with a barrier layer disposed between them, polycarbonate films, polyacrylonitrile films, polyimide films, cellophane, moisture-proof cellophane, transparent vapor-deposited polyester films or transparent vapor-deposited polyamide films in which a vapor-deposited layer of alumina or silica is provided on a PET film or polyamide film, various coating films coated with polyvinylidene chloride resin, polyvinyl alcohol resin, polyacrylic acid resin, etc., co-extruded films of PET and nylon, and polylactic acid films can be mentioned. These may be either stretched or unstretched, and may be a step of preparing one or more laminates of one type or two or more types. An appropriate one can be selected in consideration of mechanical strength, dimensional stability, etc. In addition, in order to improve the adhesion of the anchor coat layer or the laminate layer, the surface may be subjected to corona treatment, low-temperature plasma treatment, frame treatment, solvent treatment, coating treatment, etc., or may be prepared by selecting a pre-treated one. Among them, it is preferable to prepare a PET film, a polypropylene film, a polyamide film, a coating film, a transparent vapor-deposited polyester film or a transparent vapor-deposited polyamide film, a co-extruded film, etc. The thickness of the plastic film substrate is not particularly limited as long as it is within a range that does not interfere with printability, winding suitability, etc., but is preferably 5 to 300 μm, more preferably 6 to 250 μm.

[0312] It is preferable that the step is a gravure printing step of forming a thermosensitive coloring layer made of the thermosensitive coloring agent on one side of the plastic film substrate, and the coating step of forming an aqueous coating layer made of the aqueous coating agent on the thermosensitive coloring layer and the coating step of forming an overcoat layer made of the overcoat agent on the aqueous coating layer are not particularly limited, but are more preferable to be gravure printing steps. Furthermore, it is more preferable that the coating step of forming an anchor coat layer made of an anchor coat agent is also a gravure printing step. This allows the film to be produced by a gravure printing step using a multicolor gravure printer. Since it can be produced by a gravure printing step, each layer can be formed on the entire surface, but each layer can also be easily formed partially.

[0313] The method for producing a thermosensitive recording laminate of the present invention may further include a laminating step or a coating step of forming a seal layer on the surface of the plastic film substrate opposite to the thermosensitive color developing layer.

[0314] The process for forming the seal layer includes lamination processes such as lamination of a laminate provided with heat sealability or a known sealant film (dry lamination, non-solvent lamination, wet lamination), resin coating by extrusion lamination (extrusion lamination, co-extrusion lamination, PE sandwich lamination), and lamination by heat (thermal lamination), and application processes of heat seal agents or hot melt agents. Also includes application processes of adhesives or pressure sensitive adhesives.

[0315] The thickness of the sealing layer is not particularly limited, but is preferably 2 to 200 μm for a sealant film, 1 to 100 μm for a resin coating by extrusion lamination, 0.01 to 30 μm for a coating of a heat sealing agent, and 1 to 50 μm for a coating of a hot melt adhesive.

[0316] Examples of the sealant film include polyolefin films such as polyethylene, polypropylene, ethylene-vinyl acetate, and copolymers thereof, co-extruded films and colored films thereof, polystyrene films, polyacrylonitrile films, and ethylene-vinyl alcohol resin films. These films may be stretched or unstretched, and one or more types may be laminated.

[0317] When an adhesive is used in the lamination process such as the dry lamination method, the non-solvent lamination method, the wet lamination method, or the extrusion lamination method, a commercially available adhesive may be used, and examples of such adhesives include two-liquid or one-liquid type urethane resin adhesives, acrylic, epoxy, polyester, polyethyleneimine, polybutadiene, water-based urethane, isocyanate, organic titanium, and starch-based water-soluble adhesives, and aqueous adhesives such as vinyl acetate emulsion. As the adhesive coating process for forming a sealant layer, a known coating process can be used, and for example, a roll coater, a reverse roll coater, a gravure offset coater, a gravure coater, a microgravure coater, a knife coater, a bar coater, a wire bar coater, a die coater, and a dip coater can be used. There is no particular limitation on the thickness of the adhesive, but it is preferably in the range of about 0.001 to 10 μm, and particularly preferably in the range of 0.01 to 5 μm.

[0318] Resins that can be used for the resin coating by the extrusion lamination process include thermoplastic resins such as polyethylene resins such as LDPE, LLDPE, and HDPE, polypropylene resin, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl methacrylate copolymer, ethylene-propylene copolymer, methylpentene polymer, acid-modified polyolefin resins obtained by modifying polyethylene or polypropylene with maleic acid, fumaric acid, or the like, polystyrene resin, and polybutylene terephthalate resin, and these resins can be used alone or in combination of two or more kinds.

[0319] Examples of the resin of the heat sealant include thermoplastic resins such as vinylidene chloride, shellacs, rosins, rosin-modified maleic acid resins, rosin-modified phenolic resins, nitrocellulose, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, polyamide resins, vinyl chloride-vinyl acetate copolymers, polyester resins, ketone resins, butyral resins, chlorinated polypropylene resins, chlorinated polyethylene resins, chlorinated ethylene vinyl acetate resins, ethylene vinyl acetate resins, (meth)acrylic resins, urethane resins, ethylene-vinyl alcohol resins, styrene-maleic acid resins, casein, and alkyd resins, which can be used alone or in combination of two or more. Examples include types in which these resins are dissolved in a solvent, or types dispersed in water, such as acrylic emulsions, urethane emulsions, ethylene-vinyl alcohol emulsions, polyethylene emulsions, polypropylene emulsions, and ethylene vinyl acetate emulsions.

[0320] The method for producing a thermosensitive recording laminate of the present invention may include a gravure printing step of forming a design layer on the plastic film substrate or on the surface of the plastic film substrate opposite to the thermosensitive coloring layer. It may further include a gravure printing step of forming a color ink layer. The order of the steps of forming the design layer and the color ink layer does not matter. In addition, the design layer may be formed on the entire surface or on a part of the surface, and may be formed by halftone dots. The pattern layer is a layer formed using a color printing ink composition typically used in gravure printing, and is a layer on which a pattern, letters, etc. are printed. The colored ink layer is a layer formed using a white ink composition typically used in gravure printing, and is a layer used to provide contrast with the pattern layer, etc., by using solid or halftone dots, to make the layer more visible.

[0321] The packaging body according to the embodiment of the present invention is preferably made using the laminate, and may be a packaging bag, a label, or a lid material (collectively referred to as the "packaging body").

[0322] The laminate to be the packaging bag may have a structure such as plastic film substrate / thermosensitive coloring layer / aqueous coating layer / overcoat layer, plastic film substrate / anchor coating layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, seal layer / DL / plastic film substrate / thermosensitive coloring layer / aqueous coating layer / overcoat layer, seal layer / DL / design layer / colored ink layer / plastic film substrate / thermosensitive coloring layer / aqueous coating layer / overcoat layer, seal layer / DL / design layer / plastic film substrate / colored ink layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, seal layer / DL / design layer / plastic film substrate / anchor coating layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, etc. The packaging bag may be in any of the well-known forms such as two-sided seal, three-sided seal, four-sided seal, pillow seal, standing pouch, envelope seal, gusset, and melt-cut seal.

[0323] The label can also be made by forming an adhesive layer or a pressure-sensitive adhesive layer on the plastic film substrate on the other side of the substrate on which the thermosensitive coloring layer is formed, and then forming a release layer. The adhesive layer or the pressure-sensitive adhesive layer may be any material that adheres to the plastic film substrate and the release layer, such as a rubber-based adhesive material or an acrylic resin-based adhesive material, and allows the release layer to be easily peeled off. The release layer may be any material, such as a polyethylene film, a polyester film, or paper (release paper). The laminate that becomes the label may have a configuration such as adhesive layer / plastic film substrate / thermosensitive coloring layer / aqueous coating layer / overcoat layer, hot melt layer / plastic film substrate / thermosensitive coloring layer / aqueous coating layer / overcoat layer, adhesive layer / design layer / colored ink layer / plastic film substrate / thermosensitive coloring layer / aqueous coating layer / overcoat layer, adhesive layer / design layer / plastic film substrate / colored ink layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, adhesive layer / design layer / plastic film substrate / anchor coat layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, adhesive layer / design layer / plastic film substrate / anchor coat layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, etc.

[0324] The lid material may be in any known form such as a cover, a lid, or a cap. The configuration of the laminate that serves as the lid material may be sealing layer / DL / plastic film base material / thermosensitive coloring layer / aqueous coating layer / overcoat layer, sealing layer / DL / pattern layer / colored ink layer / plastic film base material / thermosensitive coloring layer / aqueous coating layer / overcoat layer, sealing layer / DL / pattern layer / plastic film base material / colored ink layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, sealing layer / DL / pattern layer / plastic film base material / anchor coat layer / thermosensitive coloring layer / aqueous coating layer / overcoat layer, etc.

[0325] Furthermore, it is preferable that the container is sealed by being tightly attached to the container. The sealing with the container may be performed manually, or a machine such as an automatic sealing device may be used. These methods may be appropriately selected depending on the type, shape, size, and quantity of the food, the container to be sealed, the equipment, the environment, etc., and may be performed by a method using heat sealing (thermal pressure sealing), surface sealing, pasting or adhesion with an adhesive, etc. It is more preferable that the container is a cylindrical container with a bottom. In this case, it is preferable that a lid cover the opening of the cylindrical container with a bottom to seal it, and it is more preferable that the sealing is performed by heat sealing. Examples of the resin used for the container include thermoplastic resins such as polyethylene, polypropylene, polyethylene terephthalate, polyvinyl chloride, polystyrene, and polyacrylonitrile. EXAMPLES

[0326] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" means "parts by mass" and "%" means "% by weight."

[0327] [Preparation of thermosensitive color former] Production Example 1 (Preparation of Color Developer Dispersion) 30 parts of N,N'-di(3-(p-toluenesulfonyl)oxy)phenylurea, 30 parts of an aqueous resin (Hiros M-141, aqueous acrylic emulsion resin, manufactured by Seiko PMC Corporation), 20 parts of methanol, and 20 parts of water were added and mixed / dispersed to prepare agent A 1. Similarly, agents A 2 to A 10 were prepared in the same manner as agent A 1, according to the formulations in Table 1.

[0328] [Table 1]

[0329] Production example 21 (leuco dye dispersion) 30 parts of leuco dye (3-dibutylamino-6-methyl-7-anilinofluoran, Yamamoto Chemical Industry Co., Ltd.), 40 parts of water-based resin (Pluscoat RZ-570, water-soluble polyester resin, GOO Chemical Industry Co., Ltd.), 15 parts of isopropyl alcohol, and 15 parts of water were added and stirred to prepare Agent B 1. Similarly, Agents B 2 to B 5 were prepared in the same manner as Agent B 1, according to the formulation in Table 2.

[0330] [Table 2]

[0331] The materials used were as follows: JONCRYL PDX7741, water-based acrylic emulsion resin, manufactured by BASF JONCRYL PDX7779, water-based acrylic emulsion resin, manufactured by BASF JONCRYL PDX7326, water-based acrylic emulsion resin, manufactured by BASF JONCRYL HPD-96J, water-soluble acrylic resin, manufactured by BASF JONCRYL HPD-196, water-soluble acrylic resin, manufactured by BASF JONCRYL PDX7356, water-based acrylic emulsion resin, manufactured by BASF 1,3-bis-(3-[3-phenylureido]phenyloxysulfonyl)benzene, developer N-[2-(3-phenylureido)phenyl]benzenesulfonamide, developer Np-Toluenesulfonyl-N'-3-(p-Toluenesulfonyloxy)phenylurea, Developer

[0332] Production Example 31 (Preparation of Thermosensitive Color Forming Agent) Next, 70 parts of Agent A 1 and 30 parts of Agent B 1 were stirred together to prepare Thermosensitive Color Former 1. Similarly, Thermosensitive Color Formers 2 to 14 were prepared in the same manner as Thermosensitive Color Former 1 according to the formulations in Tables 3 and 4.

[0333] [Table 3]

[0334] [Table 4]

[0335] Production Example 51 (Preparation of Water-Based Coating Agent) Aqueous coating agent 1 was prepared by adding 30 parts of a 10% aqueous polyvinyl alcohol solution (manufactured by Nippon Vinyl Acetate & Poval Co., Ltd.), 20 parts of isopropyl alcohol, and 50 parts of water and stirring.

[0336] [Table 5]

[0337] [Preparation of overcoat agent] Manufacturing Example 81 Coating agent 1 of Production Example 61 was prepared by stirring 40 parts of an acrylic resin solution (LG-OX anchor agent A, solid content 18%, manufactured by Tokyo Ink Co., Ltd.) and 10 parts of n-propyl acetate. Furthermore, 25 parts of trimethylolpropane trimer of xylylene diisocyanate and 25 parts of ethyl acetate were stirred to prepare a curing agent 1 of Production Example 71. The coating agent 1 and the curing agent 1 were mixed in a ratio of coating agent 1:curing agent 1=100:8 immediately before the gravure printing described below, to prepare an overcoating agent 1 of Production Example 81. Similarly, according to the formulations in Table 6, coating agents 2 to 8 were prepared in the same manner as coating agent 1. Similarly, curing agent 2 was prepared in the same manner as curing agent 1 according to the formulation in Table 7. Similarly, according to the formulations in Table 8, overcoat agents 2 to 9 were prepared in the same manner as overcoat agent 1. Note that overcoat agent 7 is similar to protective liquid 1 in Comparative Example 4 of Patent Document 1. Overcoat agent 8 is similar to protective liquid 1 in Example 6 of Patent Document 2. Overcoat agent 9 is similar to protective liquid 1 in Example 21 of Patent Document 3.

[0338] [Table 6]

[0339] [Table 7]

[0340] [Table 8]

[0341] The materials used were as follows: LG-FK R Medium A: Vinyl chloride copolymer solution, solid content 18%, manufactured by Tokyo Ink Co., Ltd. LAMREK R Medium: Urethane resin solution, solid content 15%, manufactured by Tokyo Ink Co., Ltd. ASN1004K: Acrylic resin emulsion, solid content 18%, manufactured by Mitsui Chemicals, Inc. NeoCryl A-1125: Acrylic resin emulsion, 19.5% solids, DSM Coating Resin Hexamethylene diisocyanate TMP trimer: Trimethylolpropane trimer of hexamethylene diisocyanate Curing agent 3: Oxazoline group-containing polymer, Epocross WS-300, manufactured by Nippon Shokubai Co., Ltd.

[0342] [Laminated body production] <Example 1> Using a five-color gravure printing machine, one side of a 12 μm-thick double-treated PET film (E-5202, abbreviated as double-treated PET, manufactured by Toyobo Co., Ltd.) was printed with a thermosensitive color former 1 to a thickness of 2 μm in the first unit, a water-based coating agent 1 to a thickness of 1 μm in the second unit, and an overcoat agent 1 to a thickness of 1 μm in the third unit, and then wound up to produce a laminate 1. At this time, the thermosensitive color former 1 was diluted with WA734 (non-toluene-based solvent, manufactured by Tokyo Ink Co., Ltd.), the water-based coating agent 1 with water, and the overcoat agent 1 with SL9170 (non-toluene-based solvent, manufactured by Tokyo Ink Co., Ltd.), and the viscosity was adjusted to 17 seconds using a Zahn cup No. 3. As a result, a laminate 1 of double-treated PET / thermosensitive color former 1 / water-based coating agent 1 / overcoat agent 1 was obtained.

[0343] Similarly, as shown in Tables 9 and 10, laminates 2 to 27 (Examples 2 to 27) were obtained.

[0344] The plastic film substrates used were as follows: AL-deposited PET film, Tetolite PC, thickness 12 μm, manufactured by Oike Kogyo Co., Ltd., abbreviation: AL-deposited PET (printed on the deposited surface) Transparent vapor-deposited PET film, Barrierox 1011HG-CR, thickness 12 μm, manufactured by Toray Advanced Film Co., Ltd., abbreviation: transparent vapor-deposited PET (printed on the vapor-deposited surface) OPP film, OPU-2, thickness 20μm, manufactured by Mitsui Chemicals Tocello Co., Ltd., abbreviation: OPP Both-treated nylon film, ONMB, thickness 15μm, manufactured by Unitika Ltd., abbreviation: both-treated NY

[0345] <Example 28> In addition, using a gravure printing machine, LG-OX anchor agent D (manufactured by Tokyo Ink Co., Ltd.) was printed to a film thickness of 1 μm on one side of a 12 μm-thick double-treated PET film (E-5202, manufactured by Toyobo Co., Ltd.) by a first unit, and the film was wound up to obtain a plastic film substrate (abbreviation: PET anchor). At this time, LG-OX anchor agent D was diluted with SL9170 (non-toluene-based solvent, manufactured by Tokyo Ink Co., Ltd.) and adjusted to a viscosity of 17 seconds using Zahn cup No. 3. On the anchor agent-printed surface of this plastic film substrate (PET anchor), a thermal color former 1, a water-based coating agent 1, and an overcoat agent 1 were printed in the same manner as in Example 1, and the film was wound up to obtain a laminate 28.

[0346] [Table 9]

[0347] [Table 10]

[0348] <Comparative Examples 1 to 5> A laminate 31 (Comparative Example 1) was obtained in the same manner as in Example 1, except that the aqueous coating agent was not printed. Also, a laminate 32 (Comparative Example 2) was obtained in the same manner as in Example 1, except that the overcoat agent was not printed. Laminates 33 to 35 (Comparative Examples 3 to 5) were obtained in the same manner as in Comparative Example 1, except that the overcoat agent was replaced with overcoat agents 7 to 9. However, water was used as the dilution solvent. Laminate 33 is similar to Comparative Example 4 in Patent Document 1. Laminate 34 is similar to Example 6 in Patent Document 2. Laminate 35 is similar to Example 21 in Patent Document 3.

[0349] [Table 11]

[0350] The laminate was evaluated for smear resistance, blocking, transparency, residual solvent, color density, adhesion, alcohol resistance, scratch resistance (before printing), head resistance, abrasion resistance, scratch resistance (after printing), water resistance, and oil resistance, and the results are shown in Tables 9 to 11.

[0351] <Stain resistance> The laminate was evaluated for the degree of black dullness of the coating layer (thermosensitive coloring layer, aqueous coating layer, overcoat layer, hereinafter collectively referred to as "coating layer") surface immediately after preparation. Visual evaluation was performed by five observers. Coating layers that were not blackened (little black dullness) were judged as good. The background stain resistance was rated on a four-point scale: ◎: All five observers judged that there was no black dullness, ○: Three observers judged that there was no black dullness, △: Three or more observers judged that there was a slight black dullness (no practical problem), ×: All five observers judged that there was a black color.

[0352] <Blocking> Immediately after the laminate was produced, two pieces were cut into pieces measuring 3 cm x 3 cm, and these were stacked with the coating layer surface facing the plastic film substrate surface, and then subjected to a pressure of 5 N / cm at 50°C for 24 hours. 2After applying a load of 1000 mm, the overlapping portion of the coating layer surface and the plastic film substrate surface was peeled off, and the peeling state and peeling resistance were evaluated. Those that peeled off without resistance and did not peel off were judged to be good. Blocking was evaluated on a two-level scale: ◯: peeled off without resistance and no peeling, ×: resistance was high during peeling and peeling was observed.

[0353] <Transparency> The laminate was cut into three pieces of 2cm x 3cm immediately after production, and the haze value of the coating layer surface was measured using HAZE GARD II (manufactured by Toyo Seiki Seisakusho Co., Ltd.) and the average value was evaluated as transparency. A low haze value was judged to be good. Transparency was evaluated on a three-level scale: ○: haze value less than 45, △: haze value between 45 and 70, ×: haze value 70 or more.

[0354] <Residual Solvent> After the laminate was prepared, 24 hours were allowed to stand at room temperature, and then 0.1 m 2 The test pieces were cut into pieces of 0.01 mg / m2, placed in a vial, and preheated at 80°C for 30 minutes. The headspace was analyzed using a gas chromatograph mass spectrometer (HS-20, detector: TCD type, manufactured by Shimadzu Corporation) to quantify the residual solvent. Those with a small amount of residual solvent were considered good. 2 Less than 5-10mg / m 2 Less than 10 mg / m 2 The evaluation was done on a three-point scale.

[0355] <Color Density> After preparation, the laminate was stored in a 40°C thermostatic chamber for 24 hours, and then sealed in a heat sealer (manufactured by Tester Sangyo Co., Ltd.) at 150°C and a printing pressure of 2 kgf / cm. 2 The L value when coloring was allowed to occur under conditions of 0.5 seconds of printing pressure was measured using a portable spectrodensitometer eXact 2 (manufactured by X-Rite) and used as the color density. A lower L value (higher blackness) was deemed good. Color density was evaluated using three levels: ○: L value less than 20, △: L value between 20 and 40, ×: L value 40 or more.

[0356] <Adhesion> After the laminate was prepared, it was stored in a 40°C thermostatic chamber for 24 hours, and then an adhesive tape (18 mm, manufactured by Nichiban Co., Ltd.) was attached to the coating surface and quickly peeled off at an angle of 90 degrees. The peeling state of the coating surface was visually observed and the adhesion was evaluated. The adhesion was judged to be good when the coating surface did not peel off. The adhesion was evaluated in two stages: ○: no peeling at all, ×: some peeling.

[0357] <Alcohol resistance> The laminate was stored in a 40°C thermostatic chamber for 24 hours after preparation, and the coating surface was rubbed with a cotton swab containing disinfectant ethanol (80% ethanol aqueous solution) to visually observe the peeling state of the coating surface and evaluate the alcohol resistance. The coating surface was judged to have good alcohol resistance when it did not peel off. The alcohol resistance was evaluated in two stages: ○: no peeling at all, ×: some peeling.

[0358] <Scratch resistance (before printing)> The laminate was stored in a 40°C thermostatic chamber for 24 hours after preparation, and the coating surface was rubbed 10 times with a metal spatula to evaluate the peeling state of the coating layer. Visual evaluation was performed by five observers. Coatings that did not peel were judged as good. Scratch resistance was rated on a four-point scale: ◎: All five observers judged there was no peeling, ○: Three observers judged there was no peeling, △: Three or more observers judged there was slight peeling (no practical problem), ×: All five observers judged there was peeling.

[0359] <Head resistance> The laminate was stored in a 40°C thermostatic chamber for 24 hours after preparation, and then printed matter was produced by coloring with a thermal printer (TH-M2 / PP, manufactured by Okura Engineering Co., Ltd.) at a pulse width of 1.4 ms. The degree of rubbing in the heating part (head part) was visually observed and evaluated. The printed part was judged to be good when the degree of rubbing in the printed part was small. The evaluation was made on a three-level scale: ○: no rubbing in the printed part, △: slight rubbing was observed, ×: rubbing was clearly visible.

[0360] <Abrasion resistance> Under the same conditions as the evaluation of <head resistance> above, the printed portion of the laminate was rubbed with a dry cotton cloth (Kanakin No. 3) under a load of 400 g, and the change in the printed portion was visually observed to evaluate the rub resistance. Those that showed no change in the printed portion were judged to be good. Rub resistance was evaluated on a four-point scale: ○: no change in the printed portion even after rubbing 50 times or more, △: slight scratches on the printed portion after rubbing 50 times (no practical problem), ×: the printed portion disappeared after rubbing 20 to 50 times, and XX: the printed portion disappeared in less than 20 times.

[0361] <Scratch resistance (after printing)> Under the same conditions as the head resistance evaluation described above, the printed area of ​​the laminate was rubbed 10 times with a metal spatula to evaluate the peeling state of the coating layer on the printed area. Visual evaluation was performed by five observers. The coating layer on the printed area was judged to be good if it was not peeled off. Scratch resistance was rated on a four-point scale: ◎: All five observers judged there was no peeling, ○: Three observers judged there was no peeling, △: Three or more observers judged there was slight peeling (no practical problem), ×: All five observers judged there was peeling.

[0362] <Water resistance> Under the same conditions as the evaluation of <head resistance>, the printed portion of the laminate was rubbed with a cotton swab containing water, and the presence or absence of decolorization was visually observed and evaluated. The printed portion was judged to be good when the degree of decolorization was small. The water resistance was evaluated in three stages: ○: no decolorization of the printed portion, △: slight decolorization (no practical problem), ×: complete decolorization.

[0363] <Oil resistance> Under the same conditions as the evaluation of head resistance, the printed portion of the laminate was rubbed with a cotton swab soaked in lubricant (New Highness-G, Nissei Co., Ltd.) and visually observed for the presence or absence of discoloration. The printed portion was judged to be good if it had little discoloration. The oil resistance was evaluated in three stages: ○: no discoloration of the printed portion, △: slight discoloration (no practical problem), ×: complete discoloration.

[0364] From Tables 9 to 11, it is clear that the laminates of Examples 1 to 28 have good smear resistance, blocking, transparency, residual solvent, color density, adhesion, alcohol resistance, scratch resistance (before printing), head resistance, abrasion resistance, scratch resistance (after printing), water resistance, and oil resistance. On the other hand, the laminate of Comparative Example 1, which does not have an aqueous coating layer, is clearly inferior in smear resistance, color density, and alcohol resistance, while the laminate of Comparative Example 2, which does not have an overcoat layer, is clearly inferior in scratch resistance, head resistance, abrasion resistance, and water resistance. The laminate of Comparative Example 3, which is similar to Reference 1, is clearly inferior in transparency, alcohol resistance, water resistance, and oil resistance. The laminate of Comparative Example 4, which is similar to Reference 2, is clearly inferior in alcohol resistance. The laminate of Comparative Example 5, which is similar to Reference 3, is clearly inferior in alcohol resistance and oil resistance.

Claims

1. a thermosensitive color developing layer on one surface of a plastic film substrate, the thermosensitive color developing layer comprising a leuco dye, at least one color developer selected from the group consisting of a compound represented by the following general formula (1), a compound represented by the following general formula (2), a compound represented by the following general formula (3), and a compound represented by the following general formula (4), and a thermosensitive color developing agent containing an aqueous resin, an alcohol, and water; an aqueous coating layer formed on the thermosensitive coloring layer and made of an aqueous coating agent containing a water-soluble resin and water; A thermal recording laminate characterized by having an overcoat layer on the aqueous coating layer, the overcoat layer being made of an overcoat agent containing one or more of acrylic resin, polyurethane resin, vinyl chloride-vinyl acetate copolymer and fiber-based resin, polyisocyanate and an organic solvent. 【Chemistry 1】 (R 1 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, which may be the same or different, R 2 are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, which may be the same or different; Z 1 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group. 【Chemistry 2】 (R 3 represents an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkyloxyalkyl group having 3 to 12 carbon atoms, a polyoxyalkylenealkyl group having 3 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, an alkylsulfanyl group having 1 to 12 carbon atoms, an aralkylsulfanyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 14 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an aralkylsulfonyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 15 carbon atoms, a phenyl group, an aralkylsulfonylamino group having 7 to 12 carbon atoms, an arylsulfonylamino group having 6 to 15 carbon atoms, an acyl group having 2 to 10 carbon atoms, an acylamino group having 2 to 10 carbon atoms, an (acyl having 2 to 10 carbon atoms)oxycarbonylamino group, an (alkyl having 1 to 12 carbon atoms)oxycarbonylamino group, an aralkyloxycarbonylamino group, an (aralkyl having 7 to 12 carbon atoms)oxycarbonylamino group, or an (aryl having 6 to 15 carbon atoms)oxycarbonylamino group, 3 may be bonded to each other to form an aromatic or non-aromatic ring together with the carbon atom to which they are bonded; R 4 , R 5 is a hydrogen atom or a methyl group; a, b, and c are independently an integer of 0 to 4; a+c is an integer of 0 to 5; n is 0 or 1; Y is a divalent organic group; Z 2 is a sulfonyloxy group or a sulfonyl group. 【Chemistry 3】 (R 6 is a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom; R 7 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, l and m are 0 or 1, and Z 3 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group. 【Chemistry 4】 (R 8 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, which may be the same or different, R 9 is a methyl group, d is an integer from 0 to 4, Z 4 and Z 5 are sulfonyloxy groups, sulfonyl groups, or sulfonamide groups, and may be the same or different.

2. A thermosensitive coloring layer formed on one surface of a plastic film substrate, the thermosensitive coloring layer being composed of a thermosensitive coloring agent containing a leuco dye, a compound represented by the following general formula (5), an aqueous resin, an alcohol, and water, an aqueous coating layer formed on the thermosensitive coloring layer and made of an aqueous coating agent containing a water-soluble resin and water; A thermal recording laminate characterized by having an overcoat layer on the aqueous coating layer, the overcoat layer being made of an overcoat agent containing one or more of acrylic resin, polyurethane resin, vinyl chloride-vinyl acetate copolymer and fiber-based resin, polyisocyanate and an organic solvent. 【Chemistry 5】 (R 10 are linear, branched or alicyclic alkyl groups having 1 to 12 carbon atoms, unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms or aralkyl groups having 7 to 12 carbon atoms substituted with a halogen atom, or unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms or aryl groups having 6 to 12 carbon atoms substituted with a halogen atom, and may be the same or different.

3. 3. The heat-sensitive recording laminate according to claim 1, wherein the aqueous resin comprises at least one of a water-soluble acrylic resin, an aqueous acrylic emulsion resin, and a water-soluble polyester resin.

4. An overcoat set for use in the thermal recording laminate according to claim 1 or 2, a coating agent A containing one or more of an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, and a fiber-based resin, and an organic solvent; and a curing agent B containing a polyisocyanate and an organic solvent.

5. An overcoat set for use in the thermal recording laminate according to claim 3, comprising: a coating agent A containing one or more of an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, and a fiber-based resin, and an organic solvent; and a curing agent B containing a polyisocyanate and an organic solvent.

6. Providing a plastic film substrate; a gravure printing process for forming a thermosensitive coloring layer on one side of the plastic film substrate, the thermosensitive coloring layer being made of a thermosensitive coloring agent containing a leuco dye, a color developer, an aqueous resin, alcohol, and water; a coating step of forming an aqueous coating layer on the thermosensitive coloring layer using an aqueous coating agent containing a water-soluble resin and water; a coating step of forming an overcoat layer on the aqueous coating layer, the overcoat layer being provided with an overcoat agent containing one or more of an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, and a fiber-based resin, a polyisocyanate, and an organic solvent, A method for producing a thermal recording laminate, characterized in that the developer is at least one of a compound represented by the following general formula (1), a compound represented by the following general formula (2), a compound represented by the following general formula (3), and a compound represented by the following general formula (4). 【Chemistry 6】 (R 1 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, which may be the same or different, R 2 are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, which may be the same or different; Z 1 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group. 【Chemistry 7】 (R 3 represents an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkyloxyalkyl group having 3 to 12 carbon atoms, a polyoxyalkylenealkyl group having 3 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, an alkylsulfanyl group having 1 to 12 carbon atoms, an aralkylsulfanyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 14 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an aralkylsulfonyl group having 7 to 12 carbon atoms, an arylsulfanyl group having 6 to 15 carbon atoms, a phenyl group, an aralkylsulfonylamino group having 7 to 12 carbon atoms, an arylsulfonylamino group having 6 to 15 carbon atoms, an acyl group having 2 to 10 carbon atoms, an acylamino group having 2 to 10 carbon atoms, an (acyl having 2 to 10 carbon atoms)oxycarbonylamino group, an (alkyl having 1 to 12 carbon atoms)oxycarbonylamino group, an aralkyloxycarbonylamino group, an (aralkyl having 7 to 12 carbon atoms)oxycarbonylamino group, or an (aryl having 6 to 15 carbon atoms)oxycarbonylamino group, 3 may be bonded to each other to form an aromatic or non-aromatic ring together with the carbon atom to which they are bonded; R 4 , R 5 is a hydrogen atom or a methyl group; a, b, and c are independently an integer of 0 to 4; a+c is an integer of 0 to 5; n is 0 or 1; Y is a divalent organic group; Z 2 is a sulfonyloxy group or a sulfonyl group. 【Chemistry 8】 (R 6 is a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom; R 7 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, l and m are 0 or 1, and Z 3 is a sulfonyloxy group, a sulfonyl group, or a sulfonamide group. 【Chemistry 9】 (R 8 are a linear, branched or alicyclic alkyl group having 1 to 12 carbon atoms, an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms substituted with a halogen atom, or an unsubstituted or alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms substituted with a halogen atom, which may be the same or different, R 9 is a methyl group, d is an integer from 0 to 4, Z 4 and Z 5 are sulfonyloxy groups, sulfonyl groups, or sulfonamide groups, and may be the same or different.

7. Providing a plastic film substrate; a gravure printing process for forming a thermosensitive coloring layer on one side of the plastic film substrate, the thermosensitive coloring layer being made of a thermosensitive coloring agent containing a leuco dye, a color developer, an aqueous resin, alcohol, and water; a coating step of forming an aqueous coating layer on the thermosensitive coloring layer using an aqueous coating agent containing a water-soluble resin and water; a coating step of forming an overcoat layer on the aqueous coating layer, the overcoat layer being provided with an overcoat agent containing one or more of an acrylic resin, a polyurethane resin, a vinyl chloride-vinyl acetate copolymer, and a fiber-based resin, a polyisocyanate, and an organic solvent, The method for producing a thermal recording laminate, wherein the developer is a compound represented by the following general formula (5): 【Chemistry 10】 (R 10 are linear, branched or alicyclic alkyl groups having 1 to 12 carbon atoms, unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms or aralkyl groups having 7 to 12 carbon atoms substituted with a halogen atom, or unsubstituted or alkyl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryl groups having 6 to 12 carbon atoms or aryl groups having 6 to 12 carbon atoms substituted with a halogen atom, and may be the same or different.

8. 8. The method for producing a thermal recording laminate according to claim 6, wherein the aqueous resin comprises at least one of a water-soluble acrylic resin, an aqueous acrylic emulsion resin, and a water-soluble polyester resin.

Citation Information

Patent Citations

  • Heat sensitive recording material

    JP2013199054A

  • Heat-sensitive recording medium

    JP2014030993A

  • Thermosensitive recording layer forming liquid, thermosensitive recording medium and method for manufacturing the same, and image recording method

    JP2022146283A

  • Thermosensitive recording layer forming liquid, thermosensitive recording medium and production method therefor, and image recording method

    JP2022151636A