Adhesive tape for dicing and method for manufacturing semiconductor chips
The adhesive tape for dicing semiconductor materials, with a silicone resin layer enhanced by a crosslinking agent and platinum catalyst, addresses adhesive strength and residue issues, ensuring secure chip separation and reduced scattering.
Patent Information
- Application Number
- JP2021565363
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-11-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-11-09
AI Technical Summary
Existing adhesive tapes for dicing semiconductor materials face issues with insufficient adhesive strength when applied over coating materials, leading to scattered semiconductor chips, and high adhesive strength results in adhesive residue on the chips after separation.
An adhesive tape with a silicone resin layer composed of a specific ratio of silicone gum and silicone resin, containing a crosslinking agent and a photosensitive platinum catalyst, which is activated by light to enhance adhesive strength and reduce tack force, preventing chip scattering and residue.
The adhesive tape provides strong adhesion to coated semiconductor elements, prevents scattering during dicing, and minimizes adhesive residue on separated chips, ensuring effective chip pickup and manufacturing efficiency.
Smart Images

Figure 0007571050000013 
Figure 0007571050000014 
Figure 0007571050000015
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive tape for dicing used for dicing a semiconductor material that is a raw material for semiconductor chips, and a method for manufacturing semiconductor chips using the adhesive tape for dicing. [Background technology]
[0002] 2. Description of the Related Art Conventionally, adhesive tapes having an adhesive layer made of an acrylic resin have been known as adhesive tapes for dicing used for producing semiconductor chips having LEDs (Light Emitting Diodes) and the like (see Patent Document 1). Furthermore, as a dicing pressure-sensitive adhesive tape used for producing a semiconductor chip having an LED or the like, a pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer made of a silicone resin is known (see Patent Documents 2 and 3). Furthermore, a known method for producing semiconductor chips using an adhesive tape for dicing involves attaching an adhesive tape to the substrate side of a semiconductor element substrate having a plurality of semiconductor elements formed on the substrate, and cutting the semiconductor element substrate with a dicer (see Patent Document 4). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-38408 A [Patent Document 2] JP 2015-050216 A [Patent Document 3] JP 2016-122812 A [Patent Document 4] JP 2005-93503 A Summary of the Invention [Problem to be solved by the invention]
[0004] Recently, a technique has been proposed for producing individual semiconductor chips by dicing, in which an adhesive tape is attached to a semiconductor material having multiple semiconductor elements covered with a coating material such as sealing resin or phosphor, and then dicing is performed, which is a technique compatible with the so-called wafer-level CSP (chip-scale package) process. In this way, when an adhesive tape is applied to a semiconductor material in which a semiconductor element is covered with a covering material, the adhesive strength may be insufficient and the semiconductor chips separated by dicing may fly apart depending on the configuration of the adhesive layer in the adhesive tape, the material of the covering material, etc. Also, if the ball tack or adhesive strength of the adhesive layer is designed to be high in order to suppress the scattering of the semiconductor chips, when the obtained semiconductor chip is peeled off from the adhesive tape, the adhesive may remain attached to the semiconductor chip, resulting in so-called glue residue.
[0005] The present invention aims to provide an adhesive tape for dicing that has good adhesive strength and tackiness to a semiconductor material having a plurality of semiconductor elements covered with a coating material, and that suppresses adhesive residue on the semiconductor chips when the semiconductor chips that have been diced into individual pieces are peeled off, and a method for manufacturing semiconductor chips using the same. [Means for solving the problem]
[0006] With this objective in mind, the present inventors have conducted extensive research into the adhesive layer of a dicing adhesive tape, and have discovered that if the adhesive layer is composed of an adhesive composition obtained by adding (3) a photosensitive platinum (Pt) catalyst to a specific resin composition containing at least (1) a silicone-based resin containing a silicone gum made of an organopolysiloxane containing silicon-bonded alkenyl groups, and (2) a crosslinker having a silicon-bonded hydrogen atom (SiH group), and the mixing ratio of the silicone gum to the silicone resin in the silicone-based resin and the content of silicon-bonded alkenyl groups in the entire silicone-based resin are within predetermined ranges, the adhesive layer will have good adhesion to a semiconductor material having a plurality of semiconductor elements covered with a coating material, and will be less likely to leave adhesive residue on the semiconductor chips when the semiconductor chips are separated by dicing, which has led to the present invention. That is, it was found that the following effects can be achieved by forming the adhesive layer of the dicing adhesive tape from an adhesive composition in which a silicone gum and a silicone resin are mixed at a predetermined ratio, and a crosslinking agent and a photosensitive platinum (Pt) catalyst are added to a silicone resin having a predetermined amount of silicon-bonded alkenyl groups. First, it was found that when dividing a semiconductor material having a plurality of semiconductor elements covered with a coating material into a plurality of semiconductor chips, the adhesive layer is formed from an adhesive composition containing a silicone resin in which a silicone gum and a silicone resin are mixed at an appropriate ratio, and the good tack and adhesive strength provided by the ratio prevents the individual semiconductor chips from scattering during dicing. On the other hand, when the semiconductor chips separated by dicing are peeled off from the dicing adhesive tape, the photosensitive platinum (Pt) catalyst in the adhesive composition is activated by irradiating the adhesive layer with light such as ultraviolet light, and the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl group of the silicone gum in the silicone resin and the silicon-bonded hydrogen atom (SiH group) of the crosslinking agent is promoted, and the crosslinking density increases, so that the cohesive force of the adhesive composition becomes larger than that before the light irradiation. As a result, the tack force of the adhesive layer is appropriately reduced, and the failure mode in the holding power test becomes "interface peeling" or "not falling" in the holding power test. It has been found that this improves the pick-up property of the semiconductor chip from the dicing adhesive tape and suppresses adhesive residue on the semiconductor chip.
[0007] The dicing pressure-sensitive adhesive tape of the present invention comprises a substrate and a pressure-sensitive adhesive layer laminated on the substrate, and is used when dividing a semiconductor material having a plurality of semiconductor elements covered with a coating material into a plurality of semiconductor chips, the pressure-sensitive adhesive layer being composed of a silicone-based resin in which a silicone gum (G) and a silicone resin (R) are mixed, an organopolysiloxane having at least two silicon-bonded hydrogen atoms (SiH groups) in one molecule as a crosslinking agent for the silicone-based resin, and a pressure-sensitive adhesive composition containing a photosensitive platinum (Pt) catalyst, the mixture ratio ((G) / (R)) of the silicone gum (G) to the silicone resin (R) in the entire silicone-based resin being in the range of 35.0 / 65.0 to 50.0 / 50.0 by mass, the silicone gum (G) being a silicone gum (G) composed of an organopolysiloxane containing a silicon-bonded alkenyl group. alk The content of the silicon-bonded alkenyl groups in the entire silicone resin is 1.8×10 -6 mol / g or more 1.0×10 -5 The adhesive tape for dicing is characterized in that its molecular weight is in the range of mol / g or less. Here, the semiconductor element may be used by being attached from the side of the covering material to the semiconductor material sealed with the covering material made of silicone resin. The pressure-sensitive adhesive layer has a silicon-bonded alkenyl group content of 3.0×10 -6 mol / g or more 1.0×10 -5 mol / g or less. The pressure-sensitive adhesive layer can also be characterized in that the molar ratio (SiH group / silicon-bonded alkenyl group) of the content (total amount) of silicon-bonded hydrogen atoms (SiH groups) in the crosslinking agent contained in the pressure-sensitive adhesive composition to the content (total amount) of silicon-bonded alkenyl groups in the entire silicone resin contained in the pressure-sensitive adhesive composition is in the range of 2.0 or more and 10.0 or less. The pressure-sensitive adhesive layer may be characterized in that the content of the photosensitive platinum (Pt) catalyst in the pressure-sensitive adhesive composition is in the range of 0.10 parts by mass or more and 3.00 parts by mass or less in terms of solid content per 100 parts by mass of the total solid content of the silicone-based resin. The adhesive properties conforming to JIS Z 0237 (2009) can also be characterized in that they satisfy all of the following conditions (a) to (c). (a) The adhesive strength before light irradiation to the BA-SUS test plate is in the range of 2.7 N / 10 mm or more and 4.1 N / 10 mm or less. (b) In an inclined ball tack test (inclination angle 30°, temperature 23°C, relative humidity 50% RH), the ball number value before light exposure is BN0 and the ball number value after light exposure is BN1, so that BN0 > BN1. (c) In a holding power test after light irradiation (temperature 40°C, relative humidity 33% RH, leaving time 2880 minutes), the destruction phenomenon when dropped is interfacial peeling between the adhesive layer and the BA-SUS test plate, or the sample does not drop during the holding power test.
[0008] From another perspective, a method for manufacturing a semiconductor chip to which the present invention is applied is a method for manufacturing a semiconductor chip, comprising: an attachment step of attaching the above-mentioned dicing adhesive tape to a semiconductor element substrate, on which a plurality of semiconductor elements sealed with a sealing resin made of silicone resin are formed, from the sealing resin side; a cutting step of cutting the semiconductor element substrate to which the dicing adhesive tape is attached, into a plurality of semiconductor chips; an irradiation step of irradiating light to the dicing adhesive tape of the semiconductor element substrate; and a peeling step of peeling the dicing adhesive tape from the plurality of semiconductor chips. Effect of the Invention
[0009] According to the present invention, it is possible to provide an adhesive tape for dicing that has good adhesive strength and tackiness for a semiconductor material having a plurality of semiconductor elements covered with a covering material before light irradiation, and that has good pick-up properties for the semiconductor chips when the individual semiconductor chips are peeled off by dicing after light irradiation, and that leaves little adhesive residue on the semiconductor chips, as well as a method for manufacturing semiconductor chips using the same. [Brief description of the drawings]
[0010] [Figure 1] 1 is a diagram showing an example of a configuration of an adhesive tape for dicing to which the present embodiment is applied. [Diagram 2] 1(a) to 1(e) are diagrams showing a method for manufacturing a semiconductor chip using the adhesive tape of the present embodiment. [Diagram 3] 1 is a schematic diagram showing the relationship between the crosslink density of a silicone-based resin in a pressure-sensitive adhesive layer and the results (drop time) of a holding power test of a pressure-sensitive adhesive tape 1. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. [Adhesive tape composition] 1 is a diagram showing an example of the configuration of a dicing adhesive tape 1 (hereinafter simply referred to as adhesive tape 1) to which the present embodiment is applied. The adhesive tape 1 of the present embodiment is used, for example, in dicing a semiconductor material that is the source of a semiconductor chip in a manufacturing process of a semiconductor chip having a semiconductor element such as an LED (Light Emitting Diode) or a power semiconductor.
[0012] As shown in FIG. 1, an adhesive tape 1 has a structure in which an adhesive layer 3 is laminated on a substrate 2. Although not shown in the drawings, the pressure-sensitive adhesive tape 1 may have an anchor coat layer between the substrate 2 and the pressure-sensitive adhesive layer 3, if necessary, for enhancing adhesion between the substrate 2 and the pressure-sensitive adhesive layer 3. The surface of the substrate 2 (the surface opposite to the surface facing the pressure-sensitive adhesive layer 3) may be subjected to a surface treatment. Furthermore, the surface of the pressure-sensitive adhesive layer 3 (the surface opposite to the surface facing the substrate 2) may have a release liner.
[0013] <Base material> The base material 2 of the present embodiment is made of a material that transmits light such as ultraviolet light. The material of the base material 2 is not particularly limited as long as it is capable of transmitting light such as ultraviolet light, and for example, plastics that can transmit light such as ultraviolet light can be used. Note that, here, being capable of transmitting light such as ultraviolet light does not mean that the transmittance of light such as ultraviolet light is 100%, but it is sufficient that light can be transmitted to a degree that can promote the addition reaction between the silicone resin and the crosslinking agent by a photosensitive platinum (Pt) catalyst contained in the adhesive layer 3, which will be described later.
[0014] Specifically, resin films such as polyethylene terephthalate, polyethylene naphthalate, polyphenylene sulfide, biaxially oriented polypropylene, aliphatic polyimide (transparent polyimide), polycycloolefin, fluorine-based resin, polyolefin resin, etc. may be used as the material of the base material 2. Depending on the application, the base material 2 may be, for example, a composite film laminated with polyethylene terephthalate and a polyolefin resin film, a composite film laminated with a resin film on the composite film, or a resin film multilayered by coextrusion. Among these, it is preferable to use a material containing polyethylene terephthalate as a main component for the base material 2.
[0015] <Adhesive layer> The adhesive layer 3 of this embodiment is composed of an adhesive composition containing a silicone resin which is a mixture of silicone gum (G) and silicone resin (R), a crosslinker for the silicone resin having at least two silicon-bonded hydrogen atoms (SiH groups) per molecule, and a photosensitive platinum (Pt) catalyst. Silicone-based resins are classified as "silicone gums (G) made of organopolysiloxanes containing silicon-bonded alkenyl groups." alk The adhesive layer 3 is made of a mixed resin in which a "silicone gum (G) containing a silicone gum (G)" and a "silicone resin (R) made of organopolysiloxane" are blended in a predetermined ratio. Each component contained in the adhesive composition constituting the adhesive layer 3 will be described below in order.
[0016] (Silicone resin) The silicone resin of the present embodiment is a silicone gum (G) made of an organopolysiloxane containing a silicon atom-bonded alkenyl group. alk It is composed of a mixed resin in which a "silicone gum (G) containing an organopolysiloxane" and a "silicone resin (R) composed of organopolysiloxane" are blended in a ratio of 35.0 / 65.0 to 50.0 / 50.0. In other words, it is composed of a mixed resin in which the blend ratio ((G) / (R)) of the silicone gum (G) and the silicone resin (R) is blended in a mass ratio of 35.0 / 65.0 to 50.0 / 50.0. In addition, the silicone resin has a silicon-bonded alkenyl group content of 1.8×10 -6 mol / g or more 1.0×10 -5 mol / g or less, and more preferably 3.0×10 -6 mol / g or more 1.0×10 -5 The silicone resin is configured so that the content is within the range of mol / g or less. Here, "mol / g" means "the amount of substance per 1 g of solid content of the entire silicone resin."
[0017] The content of silicon-bonded alkenyl groups in the entire silicone resin is 1.8 x 10 -6If it is less than mol / g, when the adhesive tape 1 is irradiated with light such as ultraviolet light, the crosslinking density is not sufficiently improved by the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl groups of the silicone gum and the silicon-bonded hydrogen atoms (SiH groups) of the crosslinking agent, making it difficult for the adhesive to harden and difficult to improve the cohesive force. In this case, the desired tack strength reduction and the destruction mode in the holding strength test are not obtained, and after the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, when the obtained semiconductor chips or the like are peeled off from the adhesive tape 1, the pickup ability of the individualized semiconductor chips may be deteriorated or adhesive residue may be easily generated on the semiconductor chips or the like. On the other hand, when the content of silicon-bonded alkenyl groups in the entire silicone resin is 1.0×10 -5 If it exceeds mol / g, when a release liner that has been release-treated with, for example, fluoroalkyl-modified silicone is provided in the pressure-sensitive adhesive tape 1, the release force of the release liner to the pressure-sensitive adhesive layer 3 may become large. In addition, the storage stability of the pressure-sensitive adhesive tape 1 against light may be deteriorated.
[0018] The content of silicon-bonded alkenyl groups in the entire silicone resin relative to the non-volatile components of the silicone resin is as follows: 1 It can be calculated by measuring H-NMR (nuclear magnetic resonance) spectrum and determining the resonance signal area (integral value) of the alkenyl group. Details will be described later.
[0019] The silicone resin of the present embodiment may contain a silicone gum (G0) made of an organopolysiloxane that does not contain silicon-bonded alkenyl groups, so long as the "mixing ratio ((G) / (R)) of the silicone gum (G) to the silicone resin (R)" and the "content of silicon-bonded alkenyl groups" are within the above-mentioned ranges. In other words, the silicone gum (G) may contain a "silicone gum (G0) made of an organopolysiloxane that contains silicon-bonded alkenyl groups." alk )" alone or in a mixture of two or more of them, or "silicone gum (G) made of organopolysiloxane containing silicon-bonded alkenyl groups" alk)" and "silicone gum (G0) consisting of organopolysiloxane containing no silicon-bonded alkenyl groups" or a mixture of two or more of these.
[0020] Hereinafter, the term "silicone gum (G) made of organopolysiloxane containing silicon-bonded alkenyl groups contained in silicone resins" will be used. alk ), "Silicone gum (G0) composed of organopolysiloxane containing no silicon-bonded alkenyl groups," and "Silicone resin (R) composed of organopolysiloxane containing no silicon-bonded alkenyl groups" will be explained in more detail below. In the following description, the silicone gum (G alk ) with a silicone gum (G alk ), or simply silicone gum (G alk ). Similarly, silicone gum (G0) made of organopolysiloxane that does not contain silicon-bonded alkenyl groups may be written as silicone gum (G0) that does not contain silicon-bonded alkenyl groups, or simply as silicone gum (G0). Furthermore, silicone resin (R) made of organopolysiloxane may be written simply as silicone resin (R).
[0021] (Silicone gum made of organopolysiloxane containing silicon-bonded alkenyl groups (G alk )) In the present embodiment, the silicone gum (G alk ) is not particularly limited as long as it is one that is generally used as an addition reaction type silicone resin, that is, one that contains, on average, at least two silicon-bonded alkenyl groups per molecule. Specifically, silicone gum (G alk ) has a silicon-bonded alkenyl group content of 1.0 × 10 -6mol / g or more 1.0×10 -1 In the present embodiment, from the viewpoint of controlling the adhesive properties of the adhesive layer 3 or from the viewpoint of ease of availability when using a commercially available product, the content of silicon-bonded alkenyl groups is in the range of 1.7×10 -6 mol / g or more 1.0×10 -2 It is preferable to use silicone gum having a molecular weight of 1000 mol / g or less. alk ) is a silicone-based resin obtained by mixing the above-mentioned silicone gum (G) and silicone resin (R), and the alkenyl group content in the entire silicone-based resin is 1.8 × 10 -6 mol / g or more 1.0×10 -5 One type may be used alone, or two or more types may be used in combination so that the content is within the range of mol / g or less.
[0022] Silicone gum (G alk Examples of the molecular structure of the organopolysiloxane containing a silicon-bonded alkenyl group constituting the (1) include a straight-chain structure in which the main chain portion is composed of repeated diorganosiloxane units, a structure containing a branched chain as part of the molecular structure, a branched-chain structure, and a cyclic structure. Among these, organopolysiloxanes having a straight-chain structure are preferred from the viewpoint of the mechanical strength and physical properties of the adhesive after irradiation with light such as ultraviolet light.
[0023] Silicone gum (G) consisting of organopolysiloxane containing silicon-bonded alkenyl groups alk The silicone gum (G) may be either oil-like or rubber-like, but is preferably rubber-like. When it is oil-like, it is preferable to use silicone gum (G) made of organopolysiloxane. alk The viscosity of the adhesive layer 3 is preferably 1,000 mPa·s or more at 25°C. If the viscosity is less than 1,000 mPa·s, the adhesive may not exhibit the desired adhesive properties before and after irradiation with light such as ultraviolet light, and the adhesive layer 3 may have poor adhesion to the substrate 2. When the adhesive layer 3 is in the form of raw rubber, the silicone gum (G) made of organopolysiloxane is preferably used. alkWhen silicone gum (G) is dissolved in toluene to a concentration of 30% by mass, the viscosity at 25°C is preferably 100,000 mPa·s or less. If the viscosity exceeds 100,000 mPa·s, stirring during preparation of the adhesive composition may become difficult. alk The viscosity of the above mixture can be measured using a B-type rotational viscometer (using a BM type rotor, the same applies below).
[0024] Silicone gum (G) consisting of organopolysiloxane containing silicon-bonded alkenyl groups alk ) may be, for example, those represented by the following general formula (1) or general formula (2), but is not limited thereto.
[0025] [ka]
[0026] [ka]
[0027] In the above general formula (1) and general formula (2), R 1 are each independently a monovalent hydrocarbon group having no aliphatic unsaturated bond, and X is an alkenyl-containing organic group. a is an integer of 0 to 3, m is an integer of 0 or more, and n is an integer of 100 or more, with the proviso that a and m are not simultaneously 0, and m is an integer of 2 or more only when a is 0. m+n is the content of the silicone gum (G) comprising the organopolysiloxane. alk ) at 25°C is 1,000 mPa s or more.
[0028] R 1is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 7 carbon atoms, and having no aliphatic unsaturated bonds. Examples include alkyl groups such as methyl, ethyl, propyl, and butyl groups; cycloalkyl groups such as cyclohexyl groups; and aryl groups such as phenyl and tolyl groups, with methyl and phenyl groups being particularly preferred.
[0029] X is preferably an alkenyl-containing organic group having 2 to 10 carbon atoms. Examples include vinyl, allyl, hexenyl, octenyl, acryloylpropyl, acryloylmethyl, methacryloylpropyl, acryloxypropyl, acryloxymethyl, methacryloxypropyl, methacryloxymethyl, cyclohexenylethyl, and vinyloxypropyl. Among them, lower alkenyl groups such as vinyl and allyl are preferred, and from an industrial viewpoint, vinyl is particularly preferred. The bonding position of the alkenyl group is not particularly limited, and may be a molecular chain terminal, a molecular chain side chain, or both a molecular chain terminal and a molecular chain side chain.
[0030] The number of alkenyl groups cannot be generalized as the appropriate range varies depending on the content of silicone resin (R) made of organopolysiloxane contained in the silicone-based pressure-sensitive adhesive, the type and amount of crosslinking agent added, and the balance with other added components, but for example, it is usually preferable that the number is in the range of 0.1 to 3.0 per 100 organo groups of the organopolysiloxane. Within this ratio range, it is preferable to adjust the molecular weight so that the viscosity falls within the above-mentioned range, and to adjust so that the number of alkenyl groups per molecule of organopolysiloxane is at least 2 on average. If the number of alkenyl groups is less than 0.1 per 100 organo groups of the organopolysiloxane, when the pressure-sensitive adhesive tape 1 is irradiated with light such as ultraviolet light, the silicone gum (G alkThe crosslinking density is not sufficiently improved by the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl group of the crosslinker 1 and the silicon-bonded hydrogen atom (SiH group) of the crosslinker for the silicone resin, so that the adhesive is difficult to cure and the cohesive force is difficult to improve. In this case, the desired tack strength is not reduced and the destruction mode in the holding strength test is not obtained, and after the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, when the obtained semiconductor chip or the like is peeled off from the adhesive tape 1, the pickup property of the individualized semiconductor chip may be deteriorated and adhesive residue may be easily generated on the semiconductor chip or the like. On the other hand, if the number of alkenyl groups exceeds 3.0 per 100 organo groups of the organopolysiloxane, when a release liner that has been subjected to a release treatment with, for example, fluoroalkyl-modified silicone is provided in the adhesive tape 1, the peeling force of the release liner from the adhesive layer 3 may be large.
[0031] Such silicone gums containing silicon-bonded alkenyl groups (G alk Specific examples of the above include dimethylpolysiloxanes capped with dimethylvinylsiloxy groups at both molecular chain ends, dimethylsiloxane-methylvinylsiloxane copolymers capped with dimethylvinylsiloxy groups at both molecular chain ends, dimethylsiloxane-methylphenylsiloxane copolymers capped with dimethylvinylsiloxy groups at both molecular chain ends, methylphenylpolysiloxanes capped with dimethylvinylsiloxy groups at both molecular chain ends, and dimethylsiloxane-methylvinylsiloxane copolymers capped with trimethylsiloxy groups at both molecular chain ends. copolymers, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain ends with trimethylsiloxy groups, dimethylsiloxane-methylhexenylsiloxane copolymers capped at both molecular chain ends with trimethylsiloxy groups, dimethylsiloxane-methylhexenylsiloxane copolymers capped at both molecular chain ends with dimethylvinylsiloxy groups, and dimethylsiloxane-methylhexenylsiloxane copolymers capped at both molecular chain ends with dimethylhexenylsiloxy groups.
[0032] (Silicone gum (G0) made of organopolysiloxane containing no silicon-bonded alkenyl groups) In the present embodiment, the silicone gum (G0) made of an organopolysiloxane that does not contain silicon-bonded alkenyl groups is not particularly limited as long as it is one that is generally used as a peroxide-curable silicone resin, that is, one that does not contain silicon-bonded alkenyl groups. Examples of the molecular structure of the organopolysiloxane constituting such silicone gum (G0) include a straight-chain structure in which the main chain portion is composed of repeating diorganosiloxane units, a structure containing a branched chain as part of the molecular structure, a branched-chain structure, and a cyclic structure.
[0033] The silicone gum (G0) made of organopolysiloxane not containing silicon-bonded alkenyl groups may be either oil-like or raw rubber-like, but is preferably raw rubber-like. When it is oil-like, the viscosity of the silicone gum (G0) made of organopolysiloxane is preferably 1,000 mPa·s or more at 25°C. If the viscosity is less than 1,000 mPa·s, the adhesive may not exhibit the desired adhesive properties before and after irradiation with light such as ultraviolet light, or the adhesive layer 3 and the substrate 2 may have poor adhesion. When it is raw rubber-like, the viscosity of the silicone gum (G0) made of organopolysiloxane when dissolved in toluene to a concentration of 30% by mass is preferably 100,000 mPa·s or less at 25°C. If the viscosity exceeds 100,000 mPa·s, stirring may become difficult when preparing the adhesive composition. The viscosity of the silicone gum (G0) made of organopolysiloxane can be measured using a B-type rotational viscometer.
[0034] Examples of silicone gums (G0) made of organopolysiloxanes that do not contain silicon-bonded alkenyl groups include those represented by the following general formula (3) or general formula (4), but are not limited to these.
[0035] [ka]
[0036] [ka]
[0037] Here, in the above general formula (3) and general formula (4), R 4 are each independently a monovalent hydrocarbon group free of aliphatic unsaturated bonds, and t is an integer of 100 or greater such that the viscosity of the silicone gum (G0) made from the diorganopolysiloxane at 25°C is 1,000 mPa s or greater.
[0038] R 4 is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 7 carbon atoms, and having no aliphatic unsaturated bonds. Examples include alkyl groups such as methyl, ethyl, propyl, and butyl groups; cycloalkyl groups such as cyclohexyl groups; and aryl groups such as phenyl and tolyl groups, with a methyl group being particularly preferred.
[0039] (Silicone resin(R) made from organopolysiloxane) The silicone resin (R) made of organopolysiloxane in this embodiment is R 2 3SiO 0.5 It is an organopolysiloxane having units (M units) and SiO2 units (Q units), and is generally used in silicone-based adhesives and is called MQ resin. The silicone resin (R) made of this organopolysiloxane basically does not have an alkenyl group in the molecule, and conventionally known silicone resins can be used. 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and 1 The organopolysiloxane constituting the silicone resin (R) is R 2 3SiO 0.5 units and SiO2 units, R 2 3SiO 0.5 It is preferable that the molar ratio of R units / SiO2 units is in the range of 0.5 to 1.7. 2 3SiO 0.5If the molar ratio of R to SiO2 units is less than 0.5, the adhesive strength and tackiness of the resulting adhesive layer 3 may decrease. 2 3SiO 0.5 If the molar ratio of the unit / SiO2 unit exceeds 1.7, the adhesive strength and holding power of the obtained adhesive layer 3 may decrease. The organopolysiloxane constituting the silicone resin (R) may have an OH group. In that case, the content of the OH group is preferably 4.0 mass% or less with respect to the total mass of the organopolysiloxane. If the content of the OH group exceeds 4.0 mass%, the curing property of the adhesive may decrease.
[0040] The organopolysiloxane may be used in combination of two or more kinds. In addition, the organopolysiloxane may contain R 2 SiO 1.5 Units (T units) and / or R 2 It may have 2SiO units (D units).
[0041] Silicone gum (G) made of organopolysiloxane containing silicon-bonded alkenyl groups alk )," "silicone gum (G0) made of organopolysiloxane that does not contain silicon-bonded alkenyl groups," and "silicone resin (R) made of organopolysiloxane" can usually be used simply by mixing them together. alk In the case where the silicone gum (G0) made of an organopolysiloxane not containing a silicon-bonded alkenyl group contains an organopolysiloxane represented by the above general formula (4), the silicone gum (G1) may be an organopolysiloxane represented by the above general formula (5) as long as the characteristics of the present invention are not impaired. alk Alternatively, the silicone gum (G0) may be reacted with the silicone resin (R) or with the silicone gum (G0) and the silicone resin (R) in advance to obtain a (partial) condensation reaction product.
[0042] (Mixing ratio of silicone gum (G) to silicone resin (R) in the entire silicone resin ((G) / (R))) In the entire silicone-based resin contained in the pressure-sensitive adhesive layer 3 of this embodiment, the mixture ratio ((G) / (R)) of the silicone gum (G) to the silicone resin (R) is in the range of 35.0 / 65.0 to 50.0 / 50.0 in terms of mass ratio. When two or more types of silicone gums (G) are used in combination, the total amount of each silicone gum (G) is regarded as the mass of the silicone gum (G) in the entire silicone-based resin. For example, alk When silicone gum (G0) is used in combination with silicone gum (G), the mass of silicone gum (G) in the entire silicone resin is alk ) and the mass of the silicone gum (G0). Similarly, when two or more types of silicone resin (R) are used in combination, the total amount of each silicone resin is considered to be the mass of the silicone resin (R) in the entire silicone resin.
[0043] In the entire silicone-based resin contained in the adhesive layer 3 of this embodiment, if the mixture ratio ((G) / (R)) of the silicone gum (G) and the silicone resin (R) is less than the lower limit of the above range, when the adhesive tape 1 is irradiated with light such as ultraviolet light, the contribution of the crosslinking density improvement due to the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl group of the silicone gum (G) and the silicon-bonded hydrogen atom (SiH group) of the crosslinking agent for the silicone-based resin becomes insufficient, the adhesive is difficult to harden, and the cohesive force is difficult to improve. In this case, the desired tack strength reduction and the destruction mode in the holding strength test are not obtained, and after the adhesive tape 1 is used for dicing a semiconductor element substrate, etc., when the obtained semiconductor chip, etc. is peeled off from the adhesive tape 1, the pickup property of the individualized semiconductor chip may be deteriorated, or adhesive residue may be easily generated on the semiconductor chip, etc.
[0044] On the other hand, in the entire silicone-based resin contained in the adhesive layer 3 of this embodiment, if the mixture ratio ((G) / (R)) of the silicone gum (G) and the silicone resin (R) exceeds the upper limit of the above range, when the adhesive is not cured before irradiation with ultraviolet light or the like, and a semiconductor element substrate or the like is diced, the vibration of the dicing is easily transmitted to the adhesive layer 3, and the vibration amplitude increases, and for example, the semiconductor element substrate may be displaced from the reference position. As a result, chipping may occur in the individualized semiconductor chips, or the size of each individual semiconductor chip may vary. In addition, the adhesive force and tack force of the adhesive layer 3 may decrease. In this case, when the adhesive tape 1 is used for dicing a semiconductor element substrate or a fluorescent substrate, which will be described later, the semiconductor chips, which are cut pieces, may fly off.
[0045] In contrast, by setting the mixture ratio ((G) / (R)) of the silicone gum (G) and the silicone resin (R) in the entire silicone resin contained in the adhesive layer 3 of this embodiment within the above-mentioned range, the following effects can be achieved. That is, before irradiation with light such as ultraviolet light, it is possible to impart to the uncured adhesive layer 3 appropriate adhesive strength and tackiness that will not cause the scattering of cut pieces such as semiconductor chips during dicing. On the other hand, after irradiation with light such as ultraviolet light, the silicone resin of the adhesive layer 3 has a silicon atom-bonded alkenyl group content of 1.8×10 in the entire silicone resin as described above. -6 mol / g or more 1.0×10 -5Since the composition is configured to be in the range of mol / g or less, the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl group of the silicone gum (G) and the silicon-bonded hydrogen atom (SiH group) of the crosslinking agent for the silicone resin proceeds sufficiently. As a result, the curing of the adhesive layer 3 proceeds, the crosslinking density increases, and the cohesive force improves, so that the desired reduction in tack force and the destruction mode in the holding force test can be obtained. As a result, after the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, good pick-up properties can be realized when the obtained semiconductor chip or the like is peeled off from the adhesive tape 1, and it is possible to suppress adhesive residue on the semiconductor chip or the like.
[0046] The silicone-based resin obtained by mixing the silicone gum (G) and silicone resin (R) of the present invention may be prepared by mixing and preparing an appropriate combination of the commercially available materials exemplified below. Here, the term "a suitable combination and mixing" refers to a silicone-based resin in which the content of silicon-bonded alkenyl groups in the entire silicone-based resin of the pressure-sensitive adhesive layer 3 is 1.8×10 -6 mol / g or more 1.0×10 -5 The term "compounds prepared by appropriately combining and mixing individual materials so that the silicone gum (G) and silicone resin (R) have a mixing ratio ((G) / (R)) of 35.0 / 65.0 to 50.0 / 50.0" means "a mixture prepared by appropriately combining and mixing individual materials so that the silicone gum (G) and silicone resin (R) have a mixing ratio ((G) / (R)) of 35.0 / 65.0 to 50.0 / 50.0." Examples of individual commercially available materials for appropriately combining and mixing include the following materials (1) to (4).
[0047] Silicone-based resins containing silicon-bonded alkenyl groups include (1) silicone gum (G alk (2) Silicone gum (G) and silicone resin (R) are mixed in a specific ratio to create a commercially available addition reaction type silicone adhesive. alkExamples of silicone resins that do not contain silicon-bonded alkenyl groups include (3) commercially available peroxide-curing silicone adhesives in which silicone gum (G0) and silicone resin (R) are mixed in a specified ratio, and (4) commercially available silicone resin (R) alone. In the present invention, when these commercially available individual materials are appropriately combined and mixed to prepare the mixture, it is preferable to contain at least the addition reaction type silicone release agent (2), and more preferably to further contain the addition reaction type silicone adhesive (1) in addition to this.
[0048] As described above, the silicone resin containing silicon-bonded alkenyl groups includes (1) silicone gum (G alk (2) Silicone gum (G) and silicone resin (R) are mixed in a specific ratio to create a commercially available addition reaction type silicone adhesive. alk A commercially available addition reaction type silicone release agent containing 1,4-dichlorophenylsilane (TPA) as a main component can be used. Specific examples of commercially available materials are given below.
[0049] (1) Addition reaction type silicone adhesive The commercially available addition reaction type silicone adhesive is not particularly limited as long as it is generally used as a silicone adhesive for silicone adhesive tapes.Specific examples of the commercially available silicone adhesive include KR-3700, KR-3701, X-40-3237-1, X-40-3240, X-40-3291-1, X-40-3229, X-40-3270, and X-40-3306 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., and TSR1512, TSR1516, and XR37-B9204 (all trade names) manufactured by Momentive Performance Materials, Inc. For example, SD4580, SD4584, SD4585, SD4560, SD4564, SD4565, SD4570, SD4574, SD4575, SD4600PFC, SD4593, and DC7651ADHESIVE (all trade names) manufactured by Dow Toray Co., Ltd., types that do not include a platinum (Pt) catalyst and a crosslinking agent, which will be described later, can be used. Note that types that include a crosslinking agent can also be used, but if the content of silicon-bonded hydrogen atoms (SiH groups) contained in the added crosslinking agent is unknown, the content can be determined by the method described later. 1 It can be determined by analysis such as H-NMR (nuclear magnetic resonance) spectroscopy.
[0050] (2) Addition reaction type silicone release agent The commercially available addition reaction type silicone release agent is not particularly limited as long as it is generally used as a release treatment agent for silicone release films for adhesive tapes. Specifically, for example, LTC750A, LTC310, LTC300B (all trade names) manufactured by Dow-Toray Co., Ltd., KS3600, KS778 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., TPR6710, TPR6700 (all trade names) manufactured by Momentive Performance Materials, Inc., etc. can be used. In this case, either a type without a crosslinking agent or a type with a crosslinking agent may be used, and the content of silicon-bonded hydrogen atoms (SiH groups) possessed by the crosslinking agent may be, 1 It can be determined by analysis such as H-NMR (nuclear magnetic resonance) spectroscopy.
[0051] If the mixing ratio of the silicone gum (G) and the silicone resin (R) in the commercially available addition reaction type silicone pressure sensitive adhesive is unknown, the mixing ratio is 29 It can be determined from the peak area ratio of D units to Q units (silicone gum:silicone resin = D units:Q units) measured by Si-NMR (nuclear magnetic resonance) spectroscopy. It can also be determined from the ratio of the respective peak areas measured by gel permeation chromatography (GPC).
[0052] As the silicone resin that does not contain silicon-bonded alkenyl groups, a commercially available peroxide-curing silicone adhesive in which silicone gum (G0) and silicone resin (R) are mixed in a specific ratio, or a commercially available silicone resin (R) alone can be used. Specific examples of commercially available materials are given below.
[0053] (3) Peroxide-curing silicone adhesive The commercially available peroxide curing silicone adhesive is not particularly limited as long as it is generally used as a silicone adhesive for silicone adhesive tapes.Specific examples include KR-100 and KR-101-10 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., YR3340, YR3286, PSA610-SM, XR37-B6722, and YF3897 (all trade names) manufactured by Momentive Performance Materials, and SH4280, SH4282, SE4200, BY24-717, BY24-715, and Q2-7735 (all trade names) manufactured by Dow Toray Co., Ltd.
[0054] (4) Silicone resin Specific examples of commercially available silicone resins (R) alone include YF3800, XF3905, YF3057, YF3807, YF3802, YF3897, XC96-723, and 2D SILANOL FLUID (all trade names) manufactured by Momentive Performance Materials.
[0055] When the mixing ratio of the silicone gum (G) and the silicone resin (R) in the commercially available peroxide-curing silicone-based pressure-sensitive adhesive is unknown, the mixing ratio can be determined as follows, as described above: 29 It can be determined from the peak area ratio of D units to Q units (silicone gum:silicone resin = D units:Q units) measured by Si-NMR (nuclear magnetic resonance) spectroscopy. It can also be determined from the ratio of the respective peak areas measured by gel permeation chromatography (GPC).
[0056] As described above, the content of silicon-bonded alkenyl groups in the entire silicone resin of the pressure-sensitive adhesive layer 3 is 1.8×10 -6 mol / g or more 1.0×10 -5 The silicone gum (G) and silicone resin (R) may be appropriately combined and mixed so that the silicone gum (G) and silicone resin (R) have a mixing ratio ((G) / (R)) of 35.0 / 65.0 to 50.0 / 50.0. When using these commercially available silicone resins, specifically, a silicone resin obtained by adding an addition reaction type silicone release agent to an addition reaction type silicone adhesive, or a silicone resin obtained by further adding a peroxide curing type silicone adhesive and / or silicone resin (R) to the above may be used as the main component of the adhesive composition constituting the adhesive layer 3. In the description of this embodiment, "as a main component" means that the content is 75 parts by mass or more, preferably 90 parts by mass or more, and more preferably 95 parts by mass or more, based on 100 parts by mass of the solid content of the pressure-sensitive adhesive composition.
[0057] (Crosslinking agent) The crosslinking agent in this embodiment exhibits a function as a crosslinking agent for the silicone-based adhesive by irradiating the adhesive layer 3 with light such as ultraviolet light. That is, the crosslinking agent in this embodiment crosslinks the silicone gum (G) contained in the silicone-based resin when the photosensitive platinum (Pt) catalyst in the silicone-based adhesive is activated by irradiating the adhesive layer 3 with light such as ultraviolet light. alk) to cause an addition reaction with the silicon-bonded alkenyl groups in the adhesive layer 3, thereby crosslinking the adhesive layer 3. The crosslinking agent crosslinks the silicone resin, hardening the adhesive layer 3 and increasing the crosslink density, so that the cohesive strength of the adhesive layer 3 increases compared to before it was irradiated with light such as ultraviolet light. As the crosslinking agent, an organopolysiloxane (organohydrogenpolysiloxane) having at least two, preferably three or more, silicon-bonded hydrogen atoms (SiH groups) in one molecule is used. In the following description, the organopolysiloxane having silicon-bonded hydrogen atoms (SiH groups) may be simply referred to as organohydrogenpolysiloxane.
[0058] The molecular structure of the organohydrogenpolysiloxane used as the crosslinking agent may be, for example, linear, partially branched linear, branched, or network. The organohydrogenpolysiloxane preferably has a viscosity at 25°C in the range of 1 mPa·s to 5,000 mPa·s. The viscosity can be measured using a B-type rotational viscometer.
[0059] The organohydrogenpolysiloxane used as the crosslinking agent may be any known organohydrogenpolysiloxane, including, but not limited to, those represented by the following general formula (5) or (6).
[0060] [ka]
[0061] [ka]
[0062] Here, in the general formula (5) and the general formula (6), R 3is a monovalent hydrocarbon group having 1 to 10 carbon atoms, b is 0 or 1, and p and q are integers such that the viscosity of the organohydrogenpolysiloxane at 25°C is 1 mPa·s or more and 5,000 mPa·s or less. r is an integer of 2 or more, s is an integer of 0 or more, and r+s≧3, preferably 8≧r+s≧3. The organohydrogenpolysiloxane may be a mixture of two or more types.
[0063] R 3 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 7 carbon atoms. Examples include alkyl groups such as methyl, ethyl, propyl, and butyl groups; cycloalkyl groups such as cyclohexyl groups; aryl groups such as phenyl and tolyl groups, and alkenyl groups such as vinyl and allyl groups, with a methyl or phenyl group being particularly preferred.
[0064] The content of organohydrogenpolysiloxane used as a crosslinking agent in the adhesive layer 3 of the present embodiment is silicone gum (G alk ) and the content of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane, and so cannot be generalized; however, it is usually preferable that the molar ratio of the content (total amount) of silicon-bonded hydrogen atoms (SiH groups) in the crosslinking agent contained in the pressure-sensitive adhesive composition to the content (total amount) of silicon-bonded alkenyl groups in the silicone resin contained in the pressure-sensitive adhesive composition constituting pressure-sensitive adhesive layer 3 is in the range of 2.0 or more and 10.0 or less.
[0065] If the content of organohydrogenpolysiloxane is less than the lower limit, when the adhesive tape 1 is irradiated with light such as ultraviolet light, the crosslinking density is not sufficiently improved by the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl group of the silicone gum and the silicon-bonded hydrogen atom (SiH group) of the crosslinking agent, making it difficult for the adhesive to harden and difficult to improve the cohesive force. In this case, the desired tack strength reduction and the destruction mode in the holding strength test are not obtained, and after the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, when the obtained semiconductor chip or the like is peeled off from the adhesive tape 1, the pickup ability of the individualized semiconductor chip may be deteriorated, or adhesive residue may be easily generated on the semiconductor chip or the like.
[0066] On the other hand, if the content of organohydrogenpolysiloxane exceeds the upper limit, the unreacted organohydrogenpolysiloxane may contaminate the semiconductor chip. Also, silicon-bonded hydrogen atoms (SiH groups) in the unreacted organohydrogenpolysiloxane may react with oxygen or moisture in the air to convert to SiOH, increasing the adhesive strength of the adhesive layer 3 to the adherend, which may result in poor pick-up properties of the individual semiconductor chips.
[0067] The content of the crosslinking agent in the pressure-sensitive adhesive layer 3 of the present embodiment may be adjusted so that the molar ratio of the content (total amount) of silicon-bonded hydrogen atoms (SiH groups) in the entire crosslinking agent to the content (total amount) of silicon-bonded alkenyl groups in the entire silicone-based resin in the pressure-sensitive adhesive layer 3 falls within the above-mentioned range. The content of the crosslinking agent that satisfies this range varies depending on the number of silicon-bonded hydrogen atoms (SiH groups) possessed by the crosslinking agent, but for example, the crosslinking agent may be added in an amount ranging from 0.20 parts by mass to 20.00 parts by mass in terms of solid content per 100 parts by mass of the entire silicone-based resin contained in the pressure-sensitive adhesive composition that constitutes the pressure-sensitive adhesive layer 3.
[0068] By setting the content of the crosslinking agent relative to the silicone resin in the adhesive layer 3 within the above-mentioned range, when peeling off the semiconductor chip from the dicing adhesive tape, the photosensitive platinum (Pt) catalyst in the silicone adhesive is activated by irradiating the adhesive layer 3 with light such as ultraviolet light, and the silicone gum (G) in the silicone resin is activated. alk The crosslinking reaction (addition reaction) between the silicon-bonded alkenyl groups of the crosslinker 1 and the silicon-bonded hydrogen atoms (SiH groups) of the crosslinking agent for the silicone resin is promoted, increasing the crosslink density and increasing the cohesive strength of the adhesive compared to before irradiation with light such as ultraviolet light. As a result, the tack strength of the adhesive layer 3 is appropriately reduced, achieving good pick-up properties when peeling a semiconductor chip or the like from the adhesive tape 1 and making it possible to suppress adhesive residue on the semiconductor chip or the like.
[0069] The crosslinking agent is not particularly limited, and may be any of those generally used as crosslinking agents for addition reaction type silicone adhesives, i.e., organopolysiloxanes (organohydrogenpolysiloxanes) having at least two silicon-bonded hydrogen atoms (SiH groups) in one molecule. Specific examples include X-92-122 (trade name) manufactured by Shin-Etsu Chemical Co., Ltd., and BY24-741 (trade name) manufactured by Dow-Toray Co., Ltd. If the content of silicon-bonded hydrogen atoms (SiH groups) contained in these crosslinking agents is unknown, the content may be determined as described below. 1 It can be determined by analysis such as H-NMR (nuclear magnetic resonance) spectroscopy.
[0070] (Photosensitive platinum (Pt) catalyst) The photosensitive platinum (Pt) catalyst is used to promote curing by addition reaction (hydrosilylation) between the silicone resin constituting the adhesive layer 3 and the crosslinking agent by irradiation with light such as ultraviolet light. alk The wavelength of light that can be used to promote curing by addition reaction between the silicon-bonded alkenyl groups in the crosslinking agent and the silicon-bonded hydrogen atoms (SiH groups) in the crosslinking agent is preferably in the range of 240 nm or more and 400 nm or less. As the photosensitive platinum (Pt) catalyst, it is preferable to use a photosensitive cyclopentadienyl platinum (IV) compound because of its good photosensitivity and reaction rate.
[0071] The photoactive cyclopentadienyl platinum (IV) compound is not particularly limited, but examples thereof include (cyclopentadienyl)dimethyltrimethylsilylmethylplatinum, (cyclopentadienyl)diethyltrimethylsilylmethylplatinum, (cyclopentadienyl)dipropyltrimethylsilylmethylplatinum, (cyclopentadienyl)diisopropyltrimethylsilylmethylplatinum, (cyclopentadienyl)diallyltrimethylsilylmethylplatinum, (cyclopentadienyl)dibenzyltrimethylsilylmethylplatinum, (cyclopentadienyl)dimethyltrimethylsilylmethylplatinum, (cyclopentadienyl)dimethyltrimethylsilylmethylplatinum, (cyclopentadienyl)diisopropyltrimethylsilylmethylplatinum, (cyclopentadienyl)diphenyl ... triethylsilylmethylplatinum, (cyclopentadienyl)dimethyltripropylsilylmethylplatinum, (cyclopentadienyl)dimethyltriisopropylsilylmethylplatinum, (cyclopentadienyl)dimethyltriphenylsilylmethylplatinum, (cyclopentadienyl)dimethyldimethylphenylsilylmethylplatinum, (cyclopentadienyl)dimethylmethyldiphenylsilylmethylplatinum, (cyclopentadienyl)dimethyldimethyl(trimethylsiloxy)silylmethylplatinum, (cyclopentadienyl)dimethyldimethyl(dimethylvinylsiloxy) Silylmethylplatinum, [(1'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [(2'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-methyl-3-(1'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-methyl-3-(2'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [(4'-biphenyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-(4'-biphenyl)-3-methylcyclopentadienyl]trimethylsilylmethylplatinum, [(9' [1-methyl-3-(9'-phenanthryl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-(2'-anthracenyl)-3-methylcyclopentadienyl]trimethylsilylmethylplatinum, [(2'-anthracenyl)cyclopentadienyl]trimethylsilylmethylplatinum, [(1'-pyrenyl)cyclopentadienyl]trimethylsilylmethylplatinum, and [1-methyl-3-(1'-pyrenyl)cyclopentadienyl]trimethylsilylmethylplatinum.
[0072] The cyclopentadienyl ring in the above-mentioned compounds may be substituted with methyl, chloro, fluoro, trimethylsilyl, triethylsilyl, dimethylphenylsilyl, methyldiphenylsilyl, triphenylsilyl, phenyl, fluorophenyl, chlorophenyl, methoxy, naphthyl, biphenyl, anthracenyl, pyrenyl, 2-benzoylnaphthalene, thioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, anthraquinone, 1-chloroanthraquinone, acetophenone, benzophenone, 9,10-dimethylanthracene, 9,10-dichloroanthracene, and a cyclopentadienyl ring substituted with one or more groups selected from among these. In the above compounds, the cyclopentadienyl ring may be substituted with a η5-fluorenyl group.
[0073] The cyclopentadienyl ring in the above-mentioned compound is preferably unsubstituted, substituted with one or more aromatic organic groups, substituted with one or more aliphatic organic groups, or substituted with one or more aromatic organic groups and one or more aliphatic organic groups.The organic group substituted on the cyclopentadienyl ring is preferably naphthyl, biphenyl, anthracenyl, phenanthryl, or pyrenyl.
[0074] The content of the photosensitive platinum (Pt) catalyst in the adhesive layer 3 of the present embodiment is determined by irradiating the silicone gum (G) in the silicone adhesive with light such as ultraviolet light. alkThe catalyst is not particularly limited as long as it can promote the addition reaction between the silicon-bonded alkenyl group of the silicone gum and the silicon-bonded hydrogen atom (SiH group) of the crosslinking agent. The content of the photosensitive platinum (Pt) catalyst in the adhesive layer 3 of the present embodiment is preferably in the range of 0.10 parts by mass or more and 3.00 parts by mass or less in terms of solid content, for example, relative to 100 parts by mass of the total solid content of the silicone resin in the adhesive composition constituting the adhesive layer 3. If the content of the photosensitive platinum (Pt) catalyst is less than 0.10 parts by mass, when the adhesive tape 1 is irradiated with light such as ultraviolet light, the crosslinking reaction (addition reaction) between the silicon-bonded alkenyl group of the silicone gum and the silicon-bonded hydrogen atom (SiH group) of the crosslinking agent does not proceed sufficiently, the improvement of the crosslinking density becomes insufficient, the adhesive is difficult to cure, and the cohesive force is difficult to improve. In this case, the desired tack strength reduction or failure mode in the holding strength test is not obtained, and after the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, the pick-up properties of the individualized semiconductor chips may be poor and adhesive residue may be easily left on the semiconductor chips when the resulting semiconductor chips are peeled off from the adhesive tape 1. On the other hand, when the content of the photosensitive platinum (Pt) catalyst exceeds 3.00 parts by mass, the above-mentioned crosslinking reaction (addition reaction) proceeds sufficiently, so that even if the content is, for example, 10.0 parts by mass, there is no particular problem in terms of the properties of the adhesive tape 1, but it is not preferable from the viewpoint of economy.
[0075] (Other ingredients) The silicone-based adhesive layer of the present embodiment is made of an adhesive composition containing a silicone-based resin, which is a mixture of silicone gum (G) and silicone resin (R), an organopolysiloxane having at least two silicon-bonded hydrogen atoms (SiH groups) in one molecule as a crosslinking agent for the silicone-based resin, and a photosensitive platinum (Pt) catalyst, but may contain other components within a range that does not impair the effects of the present invention. Examples of other components include a cohesive strength improver, a reinforcing filler, and a release control agent.
[0076] (Cohesion enhancer) The cohesive strength improver is used as necessary to improve the cohesive strength of the pressure-sensitive adhesive layer 3. The cohesive strength improver is not particularly limited, but for example, a multifunctional thiol is used. Examples of the cohesive strength improver made of a multifunctional thiol include Karenz (registered trademark) MT-PE1 and Karenz MT-NR1 manufactured by Showa Denko K.K.
[0077] However, since polyfunctional thiols are not compatible with the silicone resin in the adhesive composition constituting the adhesive layer 3, it is necessary to use a compatibilizer between the silicone resin and the polyfunctional thiol in order to use the polyfunctional thiol as a cohesive strength improver. The compatibilizer is not particularly limited, but examples thereof include KBM-802 and KBM-803 (both trade names) manufactured by Shin-Etsu Chemical Co., Ltd., which are silane coupling agents having a mercapto group, and SH6062 (trade name) manufactured by Dow Toray Co., Ltd. When a cohesive strength improver is used in the pressure-sensitive adhesive layer 3, the amount of the cohesive strength improver added is preferably in the range of 6 parts by mass or less in terms of solid content per 100 parts by mass of the total solid content of the silicone-based resin. If the amount of the cohesive strength improver added exceeds 6 parts by mass in terms of solid content per 100 parts by mass of the total solid content of the silicone-based resin, there is a risk of phase separation between the silicone-based resin and the polyfunctional thiol that is the cohesive strength improver, even if a compatibilizer is added.
[0078] (Reinforcing filler) The reinforcing filler is used as necessary to improve the strength of the pressure-sensitive adhesive layer 3. The reinforcing filler is not particularly limited, but examples thereof include Aerosil (registered trademark) 130, Aerosil 200, and Aerosil 300 manufactured by Nippon Aerosil Co., Ltd., Reolosil (registered trademark) QS-102 and Reolosil QS-30 manufactured by Tokuyama Corporation, Carplex (registered trademark) 80 manufactured by DSL. Japan Co., Ltd., and Hi-Sil (registered trademark)-233-D manufactured by PPG.
[0079] (peeling control agent) The release control agent is used as necessary to further reduce the adhesive strength of the pressure-sensitive adhesive layer 3 after irradiation with light such as ultraviolet light. The release control agent is not particularly limited, but examples thereof include light release additives such as silicone oil. However, if a large amount of release control agent is added, there is a risk of contamination of the adherend surface due to bleed-out, so it is preferable to add the agent within an acceptable range for the contamination level of the adherend surface.
[0080] <Adhesive layer thickness> The thickness of the adhesive layer 3 is preferably in the range of 10 μm to 100 μm, more preferably in the range of 20 μm to 40 μm. When the thickness of the adhesive layer 3 is less than 10 μm, the thickness of the silicone-based adhesive contained in the adhesive layer 3 becomes thin, and the adhesive strength of the adhesive tape 1 is likely to decrease. On the other hand, when the thickness of the adhesive layer 3 is thicker than 100 μm, the adhesive layer 3 may easily cause cohesive failure. After the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, when the obtained semiconductor chip or the like is peeled off from the adhesive tape 1, adhesive residue may easily occur on the semiconductor chip or the like. In addition, when dicing a semiconductor element substrate or the like, the vibration of dicing is easily transmitted to the adhesive layer 3, and the vibration amplitude becomes large, and for example, the semiconductor element substrate may be displaced from the reference position. As a result, chipping may occur in the individualized semiconductor chips, and size deviations may occur for each individual semiconductor chip.
[0081] <Anchor coat layer> As described above, in the adhesive tape 1 of the present embodiment, an anchor coat layer suited to the type of substrate 2 may be provided between the substrate 2 and the adhesive layer 3, or a surface treatment such as a corona treatment may be performed, depending on the manufacturing conditions of the adhesive tape 1 and the use conditions of the manufactured adhesive tape 1. This makes it possible to improve the adhesion between the substrate 2 and the adhesive layer 3.
[0082] <Surface treatment> The surface of the substrate 2 (the surface opposite to the surface facing the pressure-sensitive adhesive layer 3) may be subjected to a surface treatment such as a release property improving treatment. The treating agent used for the surface treatment of the substrate 2 is not particularly limited, but examples of the treating agent that can be used include non-silicone release treating agents such as long-chain alkyl vinyl monomer polymers, fluoroalkyl vinyl monomer polymers, polyvinyl alcohol carbamates, and aminoalkyd resins. Examples of such non-silicone release treating agents include P-LOIL (registered trademark) 1050 and P-LOIL 1200 manufactured by Lion Specialty Chemicals Co., Ltd.
[0083] <Release liner> Furthermore, a release liner may be provided on the surface of the adhesive layer 3 (the surface opposite to the surface facing the substrate 2) as necessary. The release liner may be a film of paper, polyethylene, polypropylene, polyethylene terephthalate, or the like, which has been subjected to a release treatment to enhance releasability from the silicone-based adhesive contained in the adhesive layer 3. There is no particular limitation on the material used for the release treatment of the release liner, but examples of materials that may be used include fluoroalkyl-modified silicone, long-chain alkyl vinyl monomer polymer, amino alkyd resin, and the like.
[0084] <Adhesive tape thickness> The overall thickness of the adhesive tape 1 having the structure described above is preferably in the range of 20 μm or more and 200 μm or less. If the thickness of the adhesive tape 1 is less than 20 μm, when the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, it may become difficult to peel off the formed semiconductor chips or the like from the adhesive tape 1. On the other hand, if the thickness of the adhesive tape 1 exceeds 200 μm, it becomes difficult for the adhesive tape 1 to conform to the irregularities formed on the attachment surface of the semiconductor element substrate when the adhesive tape 1 is attached to the semiconductor element substrate. In this case, the adhesion area between the adhesive tape 1 and the semiconductor element substrate or the like becomes small, and there is a risk that the semiconductor chips or the like may easily fly off during dicing.
[0085] [Adhesive tape manufacturing method] Next, a method for producing the adhesive tape 1 of the present embodiment will be described. Note that the method for producing the adhesive tape 1 described below is just one example, and the method for producing the adhesive tape 1 is not limited thereto.
[0086] When manufacturing the adhesive tape 1, first, the above-mentioned silicone adhesive, crosslinking agent, photosensitive platinum (Pt) catalyst, and other components are dissolved in a general-purpose organic solvent such as toluene or ethyl acetate to obtain an adhesive solution. Then, this adhesive solution is applied to a predetermined thickness using a comma coater or the like on the surface of the substrate 2, which has been subjected to a surface treatment or an anchor coat layer formation as necessary. Next, the base material 2 coated with the adhesive solution is heated in a drying oven to dry the adhesive solution and form the adhesive layer 3. Conditions for heating and drying may be those disclosed in, for example, JP 2012-107125 A. Specifically, for example, the adhesive solution for the adhesive layer 3 is coated on the base material 2, and the temperature is increased stepwise from 40 to 90° C. in the first half zone of the drying oven to perform initial drying, and then the adhesive solution is heated and dried for 1 to 5 minutes in the temperature range of 120 to 200° C. in the second half zone of the drying oven, and then wound into a roll-shaped raw material. Through the above steps, an adhesive tape 1 having an adhesive layer 3 laminated on a substrate 2 is obtained, as shown in FIG.
[0087] [How to use adhesive tape] The adhesive tape 1 of the present embodiment is used for dicing semiconductor material that is the source of semiconductor chips in the manufacturing process of semiconductor chips having semiconductor elements such as LEDs (Light Emitting Diodes) and power semiconductors.
[0088] Specifically, the adhesive tape 1 is used to obtain individual semiconductor chips by dicing a semiconductor element substrate having a plurality of semiconductor elements, such as LED elements and power semiconductor elements, formed on a substrate made of resin, ceramic, etc. Here, in a semiconductor element substrate having a plurality of semiconductor elements formed on a substrate, a sealing resin, which is an example of a covering material, may be provided to cover the semiconductor elements in order to protect the semiconductor elements from external environments such as temperature and humidity. The pressure-sensitive adhesive tape 1 of the present embodiment can be preferably used in dicing of a semiconductor element substrate provided with a sealing resin.
[0089] As a method for obtaining a plurality of semiconductor chips by cutting a semiconductor element substrate provided with a sealing resin, for example, the following method has been conventionally known. First, an adhesive tape for dicing is attached to the substrate side of the semiconductor element substrate, and the semiconductor element substrate is cut from the side on which the semiconductor elements are formed using a dicer or the like. Then, each semiconductor chip formed by cutting is peeled off from the adhesive tape to obtain a plurality of semiconductor chips.
[0090] However, when a dicing adhesive tape is attached to the substrate side of the semiconductor element substrate in this manner and the semiconductor element substrate is cut, problems arise such as the occurrence of chipping on the cut surface (the substrate side surface of the semiconductor chip) (so-called sagging) and the cut surface becoming rough. Therefore, in recent years, in order to solve such problems, a method has been proposed in which a dicing adhesive tape is attached to the semiconductor element substrate not only on the substrate side, but also on the side on which the semiconductor elements are formed, i.e., the sealing resin side that seals the semiconductor elements, to cut the semiconductor element substrate.
[0091] Here, epoxy resins, which have excellent electrical properties and heat resistance, have traditionally been used as sealing resins for semiconductor elements such as LEDs and power semiconductors. However, epoxy resins have the problem that they are prone to discoloration when used in high-output LEDs or power semiconductors, when used in short-wavelength LEDs, or depending on the environment in which the semiconductor chip is used.
[0092] In contrast, silicone resins are less likely to discolor due to heat or light compared to epoxy resins, and so in recent years, silicone resins are often used as sealing resins for semiconductor elements such as LEDs and power semiconductors. More specifically, silicone resins containing both or either of a methyl group and a phenyl group as functional groups, i.e., silicone resins containing a methyl group, silicone resins containing a phenyl group, and silicone resins containing both a methyl group and a phenyl group, are often used.
[0093] By using silicone resin as the sealing resin for semiconductor elements, discoloration of the sealing resin due to heat or light can be suppressed. In addition, silicone resin has a high light transmittance of 88% or more (wavelength 400 to 800 nm), and the refractive index can be adjusted in the range of 1.41 to 1.57. Therefore, when the semiconductor element is an LED, by using a silicone resin with a higher refractive index as the sealing resin, the light emitted from the LED can be efficiently taken out of the package. Among the above-mentioned silicone resins, by using a silicone resin containing a phenyl group, the refractive index of the sealing material can be made higher than when a silicone resin containing a methyl group is used, and therefore the efficiency of the emitted light can be further improved.
[0094] Examples of silicone resins containing methyl groups include, but are not limited to, KER-2300, KER-2460, KER-2500N, KER-2600, KER-2700, KER-2900, and X-32-2528 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., IVS4312, IVS4312, XE14-C2042, IVS4542, IVS4546, IVS4622, IVS4632, IVS4742, IVS4752, IVS4752, IVSG3445, IVSG0810, IVSG5778, XE13-C2479, and IVSM4500 (all trade names) manufactured by Momentive Performance Materials, Inc., and OE-6351, OE-6336, and OE-6301 (all trade names) manufactured by Dow Toray Co., Ltd. The silicone resin containing a methyl group and a phenyl group is not particularly limited, but examples thereof include KER-6075, KER-6150, and KER-6020 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd. Examples of silicone resins containing phenyl groups include, but are not limited to, KER-6110, KER-6000, KER-6200, ASP-1111, ASP-1060, ASP-1120, and ASP-1050P (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., XE14-C2508 (trade name) manufactured by Momentive Performance Materials, Inc., and OE-6520, OE-6550, OE-6631, OE-6636, OE-6635, and OE-6630 (all trade names) manufactured by Dow Toray Industries, Inc.
[0095] Conventionally, as an adhesive tape for dicing used for cutting semiconductor elements, for example, an adhesive tape having an adhesive layer made of an acrylic resin-based adhesive has been used. However, when such conventional adhesive tape is applied to the side of the semiconductor element substrate on which the semiconductor elements are formed (the sealing resin side) and the semiconductor element substrate is diced, problems may arise, such as semiconductor chips scattering during dicing, if the adhesive strength between the sealing resin and the adhesive tape is insufficient.
[0096] In particular, the silicone resin has a high releasability compared to, for example, epoxy resins conventionally used as sealing resins. Therefore, when a semiconductor element substrate using silicone resin as sealing resin is attached with, for example, an adhesive tape whose adhesive layer is made of an acrylic resin-based adhesive, the adhesive strength between the silicone resin sealing resin and the adhesive tape is likely to be reduced. As a result, problems such as scattering of semiconductor chips are more likely to occur when dicing the semiconductor element substrate.
[0097] In contrast, as described above, the adhesive layer 3 of the adhesive tape 1 of the present embodiment is made of an adhesive composition containing a silicone-based resin obtained by mixing silicone gum (G) and silicone resin (R) at an appropriate ratio, and therefore, even when the adhesive tape is attached to the sealing resin side of the semiconductor element substrate when dicing the semiconductor element substrate, the adhesive layer 3 can maintain good adhesive strength and tackiness to the sealing resin of the semiconductor element substrate. Furthermore, compared to conventional adhesive tapes, the occurrence of scattering of semiconductor chips can be suppressed when dicing the semiconductor element substrate. On the other hand, since the adhesive composition constituting the adhesive layer 3 contains a photosensitive platinum (Pt) catalyst and a crosslinking agent in addition to the above-mentioned silicone-based resin, the photosensitive platinum (Pt) catalyst in the silicone-based resin is activated by irradiation with light such as ultraviolet light, and the silicone gum (G) in the silicone-based resin is formed. alk The crosslinking reaction (addition reaction) between the silicon-bonded alkenyl groups of the crosslinking agent for the silicone resin and the silicon-bonded hydrogen atoms (SiH groups) of the crosslinking agent for the silicone resin is promoted, increasing the crosslinking density, and the cohesive strength of the adhesive becomes stronger than before irradiation with light such as ultraviolet light. As a result, the tack strength of the adhesive layer 3 is appropriately reduced, and the failure mode in the holding strength test becomes "interface peeling" or "no drop" in the holding strength test. This makes it possible to achieve good pick-up properties when peeling a semiconductor chip or the like from the adhesive tape 1, and to suppress adhesive residue on the semiconductor chip or the like.
[0098] A detailed description will now be given of a method for using the adhesive tape 1 of the present embodiment, and a method for manufacturing a semiconductor chip using the adhesive tape 1 of the present embodiment. Figures 2(a) to (e) are diagrams showing a method for manufacturing a semiconductor chip using the adhesive tape 1 of the present embodiment. Here, an example will be described in which a semiconductor chip having an LED element as a semiconductor element is manufactured using the adhesive tape 1. The method described below is an example of a method of using the adhesive tape 1 and a method of manufacturing a semiconductor chip using the adhesive tape 1, and is not limited to the following method.
[0099] In this embodiment, first, a plurality of semiconductor elements 102 are mounted on a substrate 101 made of, for example, a resin material or ceramic, to fabricate a semiconductor element substrate 100. The semiconductor elements 102 are, for example, LED elements, and although not shown, are configured by laminating a plurality of semiconductor layers including, for example, a light-emitting layer that emits light when current is applied, and an electrode is formed on the upper portion. Next, the multiple semiconductor elements formed on the substrate 101 of the semiconductor element substrate 100 are sealed with sealing resin 103 made of silicone-based resin (sealing process). In this example, the multiple semiconductor elements 102 are collectively sealed with the sealing resin 103, but each semiconductor element 102 may be individually sealed with the sealing resin 103.
[0100] Next, as shown in FIG. 2(a), the adhesive tape 1 and the semiconductor element substrate 100 are attached together so that the adhesive layer 3 of the adhesive tape 1 faces the sealing resin 103 of the semiconductor element substrate 100 (attaching step). 2(b) and (c), in a state where the adhesive tape 1 and the semiconductor element substrate 100 are attached to each other, the semiconductor element substrate 100 is cut along the intended cutting line X by a dicer or the like (cutting step). In this example, the semiconductor element substrate 100 to which the adhesive tape 1 is attached is cut from the substrate 101 side. Also, in this example, a so-called full cut is performed in which the semiconductor element substrate 100 is entirely cut in the thickness direction, as shown in FIG. 2(c).
[0101] 2(d), the adhesive tape 1 attached to the semiconductor element substrate 100 is irradiated with ultraviolet light from the base material 2 side (irradiation step). As described above, the base material 2 is made of a material that transmits ultraviolet light and other light. Therefore, by irradiating the adhesive tape 1 with ultraviolet light from the base material 2 side, the ultraviolet light passes through the base material 2 and is irradiated onto the adhesive layer 3. In the pressure-sensitive adhesive tape 1 of this embodiment, the pressure-sensitive adhesive layer 3 has a photosensitive platinum (Pt) catalyst, and thus the photosensitive platinum (Pt) catalyst is activated by irradiating the pressure-sensitive adhesive layer 3 with light such as ultraviolet light, which promotes an addition reaction between the silicone resin containing silicon-bonded alkenyl groups and the crosslinking agent in the pressure-sensitive adhesive layer 3. This increases the crosslink density, i.e., the cohesive force, in the pressure-sensitive adhesive layer 3 compared to before irradiation with light such as ultraviolet light, and decreases the tackiness of the pressure-sensitive adhesive layer 3.
[0102] Next, the semiconductor chips 200 formed by cutting the semiconductor element substrate 100 are peeled off (picked up) from the adhesive tape 1 to obtain the individual semiconductor chips 200 as shown in FIG. 2(e) (peeling process).
[0103] As described above, in the adhesive tape 1 of the present embodiment, the adhesive layer 3 contains a silicone-based resin in which the silicone gum (G) and the silicone resin (R) are mixed at an appropriate ratio. This allows the adhesive tape 1 to maintain good adhesive strength and tack strength with respect to the semiconductor element substrate 100 when the adhesive tape 1 is used for dicing. In particular, in recent years, silicone resin with high releasability is often used as the sealing resin 103 that seals the semiconductor element 102. In contrast, the adhesive tape 1 of the present embodiment has the above-mentioned configuration and therefore has good adhesive strength and tackiness even with respect to the sealing resin 103 made of silicone resin. As a result, when the adhesive tape 1 of the present embodiment is used for dicing the semiconductor element substrate 100, it is possible to prevent the semiconductor chips 200 from scattering.
[0104] Furthermore, the adhesive composition containing a silicone-based resin that constitutes the adhesive layer 3 of the adhesive tape 1 of this embodiment has good adhesion to the sealing resin 103 as described above, while also having high releasability. That is, the adhesive tape 1 of the present embodiment contains a photosensitive platinum (Pt) catalyst that promotes an addition reaction between a silicone resin containing a silicon-bonded alkenyl group in the adhesive layer 3 and a crosslinking agent by irradiation with light such as ultraviolet light. After the cutting step, the adhesive layer 3 is irradiated with light such as ultraviolet light through the substrate 2 before the peeling step, whereby the photosensitive platinum (Pt) catalyst is activated, and an addition reaction between a silicone resin containing a silicon-bonded alkenyl group in the adhesive layer 3 and a crosslinking agent is promoted, so that the crosslinking density in the adhesive layer 3 is increased compared to before irradiation with light such as ultraviolet light, that is, the cohesive force is increased, and the tackiness of the adhesive layer 3 can be reduced. As a result, when the semiconductor chip 200 obtained by dicing the semiconductor element substrate 100 is peeled off (picked up) from the adhesive tape 1 in the peeling step, the occurrence of so-called glue residue in which the adhesive adheres to the semiconductor chip 200 can be suppressed. In addition, good pick-up properties can be realized when peeling off the semiconductor chip 200 from the adhesive tape 1.
[0105] In the above, a method has been described in which adhesive tape 1 is attached from the sealing resin side to a semiconductor element substrate having a plurality of semiconductor elements formed thereon, and dicing is performed to obtain individual semiconductor chips. However, the use of adhesive tape 1 in the present embodiment is not limited to this. The adhesive tape 1 of the present embodiment may be used, for example, in the manufacture of chip-scale packaged LEDs, to obtain individual chip-scale packaged LEDs by dicing a semiconductor material in which a plurality of LED elements are covered with a phosphor as an example of a covering material. The phosphor is a material in which a fluorescent material is dispersed in a resin material, ceramic, or the like.
[0106] In recent years, as chip-scale packaged LEDs become smaller, the individual chip-scale packaged LEDs tend to fly apart during dicing. By using the pressure-sensitive adhesive tape 1 of the present embodiment having the above-described configuration, it is possible to maintain good adhesion between the phosphor and the pressure-sensitive adhesive layer 3, and to prevent the individual chip-scale packaged LEDs from flying apart. In addition, after dicing, the adhesive layer 3 can be irradiated with light such as ultraviolet light to reduce the tackiness, making it easier to peel the individual chip-scale package LEDs from the adhesive tape 1 and suppressing the occurrence of glue residue on the peeled chip-scale package LEDs. EXAMPLES
[0107] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0108] In order to prepare various pressure-sensitive adhesive compositions used in the Examples and Comparative Examples, the following silicone-based resins (a) to (h) were used as the main components of the pressure-sensitive adhesive compositions, and the following organopolysiloxanes (organohydrogenpolysiloxanes) (m) and (n) having silicon-bonded hydrogen atoms (SiH) were used as crosslinking agents.
[0109] The silicone resins (a) to (c) are silicone gums (G) each containing a silicon-bonded alkenyl group. alk ) and silicone resin (R), and the mixture ratio and the content of silicon-bonded alkenyl groups differ from each other. alk ) uses a dimethylsiloxane-methylvinylsiloxane copolymer with a weight-average molecular weight (Mw) of about 500,000 and both ends of the molecular chain are blocked with dimethylvinylsiloxy groups. The silicone resin (R) uses a R 2 3SiO 0.5 An organopolysiloxane (MQ resin) having units (M units) and SiO2 units (Q units) was used.
[0110] The silicone resins (d) and (e) are both silicone gums (G) containing silicon-bonded alkenyl groups. alk ) and the content of silicon-bonded alkenyl groups differs from each other. alk) is a dimethylsiloxane-methylhexenylsiloxane copolymer with a weight-average molecular weight (Mw) of about 300,000, both ends of which are blocked with dimethylhexenylsiloxy groups, and silicone gum (G) of silicone resin (e) is used. alk ) was a dimethylsiloxane polymer capped at both ends of the molecular chain with dimethylvinylsiloxy groups and having a weight-average molecular weight (Mw) of approximately 200,000.
[0111] Furthermore, silicone resins (f) and (g) are mixtures of silicone gum (G0) and silicone resin (R) that do not contain silicon-bonded alkenyl groups, and the mixture ratios are different from each other. The silicone gum (G0) uses a dimethylsiloxane polymer with a weight average molecular weight (Mw) of about 500,000, and the silicone resin (R) uses a dimethylsiloxane polymer with a weight average molecular weight (Mw) of about 5,000. 2 3SiO 0.5 An organopolysiloxane (MQ resin) having units (M units) and SiO2 units (Q units) was used.
[0112] Furthermore, the silicone resin (h) is a single silicone resin (R), and the silicone resin (R) contains an R having a weight average molecular weight (Mw) of about 5,000. 2 3SiO 0.5 An organopolysiloxane (MQ resin) having units (M units) and SiO2 units (Q units) was used.
[0113] Silicone resin (a) Silicone gum (G alk ) and silicone resin(R) (G alk ) / (R)=40.0 mass% / 60.0 mass% Alkenyl group (vinyl group) content: 2.0 x 10 -6 mol / g
[0114] Silicone resin (b) Silicone gum (G alk ) and silicone resin(R) (G alk) / (R)=35.0 mass% / 65.0 mass% Alkenyl group (vinyl group) content: 1.8 x 10 -6 mol / g
[0115] Silicone resin (c) Silicone gum (G alk ) and silicone resin(R) (G alk ) / (R)=50.0 mass% / 50.0 mass% Alkenyl group (vinyl group) content: 2.5 x 10 -6 mol / g
[0116] Silicone resin (d) Silicone gum (G alk ) Single Alkenyl group (hexenyl group) content: 2.0 x 10 -4 mol / g
[0117] Silicone resin (e) Silicone gum (G alk ) Single Alkenyl group (vinyl group) content: 2.7 x 10 -3 mol / g
[0118] Silicone resin (f) A mixture of silicone gum (G0) and silicone resin (R) (G0) / (R)=40.0 mass% / 60.0 mass% No alkenyl groups
[0119] Silicone resin (g) A mixture of silicone gum (G0) and silicone resin (R) (G0) / (R)=60.0 mass% / 40.0 mass% No alkenyl groups
[0120] Silicone resin (h) Silicone Resin(R) alone No alkenyl groups
[0121] Crosslinking agent (m) Organohydrogenpolysiloxane SiH group content: 2.0×10 -2 mol / g
[0122] Crosslinking agent (n) Organohydrogenpolysiloxane SiH group content: 2.4×10 -3 mol / g
[0123] The alkenyl group content of the silicone resin and the SiH group content of the crosslinking agent used above were determined based on the results of a 500 MHz 1 The quantification was carried out by measuring the H-NMR (nuclear magnetic resonance) spectrum. Specifically, the non-volatile components of the silicone resin were thoroughly dissolved in deuterated chloroform containing dimethyl sulfoxide as an internal standard sample, and the NMR spectrum was measured using a JEOL Ltd. NMR device "JNM·ECA500" (product name). 1 H-NMR (nuclear magnetic resonance) spectrum was measured. Next, the resonance signal area (integral value) of the internal standard sample dimethyl sulfoxide and the resonance signal area (integral value) of the alkenyl group in the measured spectrum were calculated, and the content of the alkenyl group per 1 g (solid content) of the silicone resin was calculated from the ratio. The SiH group content of the crosslinking agent was also calculated in the same manner. 1 The H-NMR spectrum was measured, and the resonance signal area (integral value) of the internal standard sample dimethyl sulfoxide and the resonance signal area (integral value) of the SiH group in the measured spectrum were calculated, and the content of the SiH group per 1 g (solid content) of the crosslinking agent was calculated from the ratio. Note that when the crosslinking agent is added to the silicone resin from the beginning, the content of the SiH group per 1 g (solid content) of the crosslinking agent was calculated from the ratio. 1 The contents of alkenyl groups and SiH groups can be calculated simultaneously from the H-NMR spectrum.
[0124] 1. Preparation of Adhesive Tape Example 1 <Preparation of silicone resin solution> Silicone-based resin (a) and silicone-based resin (d) were mixed so that the mass ratio (a) / (d) was 96.85 / 3.15 to prepare silicone-based resin (S1), which was then diluted with toluene and stirred to prepare a silicone-based resin (S1) solution (solid content concentration 30 mass%). This silicone-based resin (S1) had a silicone gum (G) and silicone resin (R) mixing ratio ((G) / (R)) of 41.9 / 58.1 and an alkenyl group content of 8.2×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (a). alk )" and "Silicone gum (G) of silicone resin (d) alk The total mass of silicone resin (R) is the amount of silicone resin (R) in silicone-based resin (a).
[0125] <Preparation of crosslinker solution> Next, crosslinker (C1) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 8.82 / 91.18, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C1) solution (solid content concentration: 20 mass%). This crosslinker (C1) had a SiH group content of 4.0×10 -3 The mass ratio was mol / g.
[0126] <Preparation of adhesive solution> Next, 3.50 parts by mass of the crosslinker (C1) solution (0.70 parts by mass in solid content equivalent, molar ratio of SiH group / alkenyl group = 3.4) was mixed with 333.00 parts by mass of the silicone resin (S1) solution (100 parts by mass in solid content equivalent) using a disper, and the mixture was stirred and mixed uniformly. Next, 5.13 parts by mass (0.77 parts by mass in solid content equivalent) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disper, and the mixture was stirred and mixed uniformly to prepare an adhesive solution for coating.
[0127] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 20 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.
[0128] Example 2 <Preparation of silicone resin solution> Silicone resin (b), silicone resin (d), and silicone resin (h) were mixed in a mass ratio (b) / (d) / (h) of 97.30 / 0.95 / 1.75 to prepare silicone resin (S2), which was then diluted with toluene and stirred to prepare a silicone resin (S2) solution (solid content concentration 30 mass%). This silicone resin (S2) had a silicone gum (G) and silicone resin (R) mixing ratio ((G) / (R)) of 35.0 / 65.0 and an alkenyl group content of 3.6×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (b). alk )" and "Silicone gum (G) of silicone resin (d) alk The total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (b)" and "silicone resin (R) of silicone resin (h)."
[0129] <Preparation of crosslinker solution> Next, crosslinker (C2) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 2.83 / 97.17, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C2) solution (solid content concentration: 20 mass%). This crosslinker (C2) had a SiH group content of 2.9×10 -3 The mass ratio was mol / g.
[0130] <Preparation of adhesive solution> Next, 3.30 parts by mass of the crosslinker (C2) solution (0.66 parts by mass in solid content equivalent, molar ratio of SiH group / alkenyl group = 5.3) was mixed with 333.00 parts by mass of the silicone resin (S2) solution (100 parts by mass in solid content equivalent) using a disperser, and stirred and mixed uniformly. Next, 5.20 parts by mass (0.78 parts by mass in solid content equivalent) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disperser, and stirred and mixed uniformly to prepare an adhesive solution for coating.
[0131] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 12 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 10 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 22 μm after drying was obtained.
[0132] Example 3 <Preparation of silicone resin solution> Silicone-based resin (c), silicone-based resin (d), and silicone-based resin (h) were mixed in a mass ratio (c) / (d) / (h) of 92.66 / 3.63 / 3.71 to prepare silicone-based resin (S3), which was then diluted with toluene and stirred to prepare a silicone-based resin (S3) solution (solid content concentration 30 mass%). This silicone-based resin (S3) has a mixture ratio ((G) / (R)) of silicone gum (G) and silicone resin (R) of 50.0 / 50.0 and an alkenyl group content of 9.6×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (c). alk)" and "Silicone gum (G) of silicone resin (d) alk The total mass of silicone resin (R) is the sum of the silicone resin (R) in silicone-based resin (c) and the silicone resin (R) in silicone-based resin (h).
[0133] <Preparation of crosslinker solution> Next, crosslinker (C3) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 10.43 / 89.57, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C3) solution (solid content concentration: 20 mass%). This crosslinker (C3) had a SiH group content of 4.2×10 -3 The mass ratio was mol / g.
[0134] <Preparation of adhesive solution> Next, 3.45 parts by mass of the crosslinker (C3) solution (0.69 parts by mass in solid content, molar ratio of SiH group / alkenyl group = 3.0) was mixed with 333.00 parts by mass of the silicone resin (S3) solution (100 parts by mass in solid content), and the mixture was stirred and mixed uniformly. Next, 4.93 parts by mass (0.74 parts by mass in solid content) of a solution of the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC diluted with toluene to a solid content concentration of 15% by mass was mixed with the mixture using a disperser, and the mixture was stirred and mixed uniformly to prepare an adhesive solution for coating.
[0135] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 50 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 40 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 90 μm after drying was obtained.
[0136] Example 4 <Preparation of silicone resin solution> Silicone resin (a) and silicone resin (d) were mixed so that the mass ratio (a) / (d) was 98.08 / 1.92 to prepare silicone resin (S4), which was then diluted with toluene and stirred to prepare a silicone resin (S4) solution (solid content concentration 30 mass%). This silicone resin (S4) had a silicone gum (G) / silicone resin (R) mixture ratio ((G) / (R)) of 41.2 / 58.8 and an alkenyl group content of 5.8×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (a). alk )" and "Silicone gum (G) of silicone resin (d) alk The total mass of silicone resin (R) is the amount of silicone resin (R) in silicone-based resin (a).
[0137] <Preparation of crosslinker solution> Next, crosslinker (C4) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 10.43 / 89.57, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C4) solution (solid content concentration: 20 mass%). This crosslinker (C4) had a SiH group content of 4.2×10 -3 The mass ratio was mol / g.
[0138] <Preparation of adhesive solution> Next, 333.00 parts by mass (100 parts by mass in terms of solid content) of the above silicone resin (S4) solution was mixed with 1.80 parts by mass (0.36 parts by mass in terms of solid content, molar ratio of SiH group / alkenyl group = 2.6) of the crosslinker (C4) solution using a disperser, and stirred and mixed uniformly. Next, 5.20 parts by mass (0.78 parts by mass in terms of solid content) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disperser, and stirred and mixed uniformly to prepare an adhesive solution for coating.
[0139] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 20 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.
[0140] Example 5 A crosslinker (C5) solution was prepared as described below. In preparing the adhesive solution, the crosslinker was changed from the crosslinker (C4) solution to the crosslinker (C5) solution, and the amount of the crosslinker (C5) solution was changed to 8.30 parts by mass (1.66 parts by mass in terms of solid content, molar ratio of SiH group / alkenyl group=8.0). Except for this, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained in the same manner as in Example 4.
[0141] <Preparation of crosslinker solution> Crosslinker (C5) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 2.28 / 97.72. The resulting mixture was diluted with toluene and stirred to prepare a crosslinker (C5) solution (solid concentration: 20 mass%). This crosslinker (C5) had a SiH group content of 2.8×10 -3 The mass ratio was mol / g.
[0142] Example 6 A crosslinker (C6) solution was prepared as described below. In preparing the adhesive solution, the crosslinker was changed from the crosslinker (C4) solution to the crosslinker (C6) solution, the amount of the crosslinker (C6) solution was changed to 3.45 parts by mass (0.69 parts by mass in terms of solid content, molar ratio of SiH group / alkenyl group=4.0), and the amount of the photosensitive platinum (Pt) catalyst solution was changed to 1.93 parts by mass (0.29 parts by mass in terms of solid content). An adhesive tape 1 having a total thickness of 58 μm after drying was obtained in the same manner as in Example 4.
[0143] <Preparation of crosslinker solution> Crosslinker (C6) was prepared by mixing crosslinker (m) and crosslinker (n) at a mass ratio (m) / (n) of 5.50 / 94.50, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C6) solution (solid content concentration: 20 mass%). This crosslinker (C6) had a SiH group content of 3.4×10 -3 It was mol / g.
[0144] Example 7 Adhesive tape 1 having a total thickness of 58 μm after drying was obtained in the same manner as in Example 6, except that the amount of photosensitive platinum (Pt) catalyst solution used in preparing the adhesive solution was changed to 19.60 parts by mass (2.94 parts by mass in solid content equivalent).
[0145] Example 8 A silicone-based resin (S5) solution was prepared as described below. In preparing the adhesive solution, the amount of the crosslinker (C6) solution was changed to 2.85 parts by mass (0.57 parts by mass in terms of solid content, molar ratio of SiH groups / alkenyl groups=3.7), the amount of the photosensitive platinum (Pt) catalyst solution was changed to 4.40 parts by mass (0.66 parts by mass in terms of solid content), and the thickness of the adhesive layer 3 after drying was changed to 30 μm. Except for this, an adhesive tape 1 having a total thickness after drying of 68 μm was obtained in the same manner as in Example 6.
[0146] <Preparation of silicone resin solution> Silicone-based resin (a), silicone-based resin (d), and silicone-based resin (f) were mixed in a mass ratio (a) / (d) / (f) of 81.99 / 1.61 / 16.40 to prepare silicone-based resin (S5), which was then diluted and stirred with toluene to prepare a silicone-based resin (S5) solution (solid content concentration 30 mass%). This silicone-based resin (S5) had a silicone gum (G) / silicone resin (R) mixture ratio ((G) / (R)) of 49.2 / 50.8 and an alkenyl group content of 5.3×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (a). alk )" and "Silicone gum (G) of silicone resin (d) alkThe total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (a)" and "silicone gum (G0) of silicone resin (f)." The total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (a)" and "silicone resin (R) of silicone resin (f)."
[0147] Example 9 <Preparation of silicone resin solution> Silicone-based resin (a), silicone-based resin (d), silicone-based resin (f), and silicone-based resin (h) were mixed in a mass ratio (a) / (d) / (f) / (h) of 66.49 / 0.26 / 26.60 / 6.65 to prepare silicone-based resin (S6), which was then diluted and stirred with toluene to prepare a silicone-based resin (S6) solution (solid content concentration 30 mass%). This silicone-based resin (S6) has a silicone gum (G) and silicone resin (R) mixing ratio ((G) / (R)) of 37.5 / 62.5 and an alkenyl group content of 1.9×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (a). alk )" and "Silicone gum (G) of silicone resin (d) alk The total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (a)," "silicone resin (R) of silicone resin (f)," and "silicone resin (R) of silicone resin (h)."
[0148] <Preparation of crosslinker solution> Next, crosslinker (C7) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 1.15 / 98.85, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C7) solution (solid content concentration: 20 mass%). This crosslinker (C7) had a SiH group content of 2.6×10 -3 The mass ratio was mol / g.
[0149] <Preparation of adhesive solution> Next, 333.00 parts by mass (100 parts by mass in terms of solid content) of the above silicone resin (S6) solution was mixed with 2.20 parts by mass (0.44 parts by mass in terms of solid content, molar ratio of SiH group / alkenyl group = 6.2) of the crosslinker (C7) solution using a disperser, and stirred and mixed uniformly. Next, 3.53 parts by mass (0.53 parts by mass in terms of solid content) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disperser, and stirred and mixed uniformly to prepare an adhesive solution for coating.
[0150] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 30 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 68 μm after drying was obtained.
[0151] Example 10 <Preparation of silicone resin solution> Silicone-based resin (c), silicone-based resin (d), and silicone-based resin (f) were mixed in a mass ratio (c) / (d) / (f) of 71.18 / 0.35 / 28.47 to produce silicone-based resin (S7), which was then diluted and stirred with toluene to prepare a silicone-based resin (S7) solution (solid content concentration 30 mass%). This silicone-based resin (S7) has a silicone gum (G) and silicone resin (R) mixing ratio ((G) / (R)) of 47.3 / 52.7 and an alkenyl group content of 2.5×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (c). alk )" and "Silicone gum (G) of silicone resin (d) alkThe total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone-based resin (c)" and "silicone resin (R) of silicone-based resin (f)."
[0152] <Preparation of crosslinker solution> Next, crosslinker (C8) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 1.44 / 98.56, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C8) solution (solid concentration: 20 mass%). This crosslinker (C8) had a SiH group content of 2.7×10 -3 It was mol / g.
[0153] <Preparation of adhesive solution> Next, 333.00 parts by mass (100 parts by mass in terms of solid content) of the above silicone resin (S7) solution was mixed with 2.35 parts by mass (0.47 parts by mass in terms of solid content, molar ratio of SiH group / alkenyl group = 5.1) of the crosslinker (C8) solution using a disperser, and the mixture was stirred and mixed uniformly. Next, 3.80 parts by mass (0.57 parts by mass in terms of solid content) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disperser, and the mixture was stirred and mixed uniformly to prepare an adhesive solution for coating.
[0154] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 30 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 68 μm after drying was obtained.
[0155] Comparative Example 1 A silicone-based resin (S8) solution was prepared as described below, and in preparing the adhesive solution, the silicone-based resin was changed from the silicone-based resin (S4) solution to a silicone-based resin (S8) solution, no crosslinking agent was added, and the thickness of the adhesive layer 3 after drying was set to 35 μm. Except for this, an adhesive tape 1 having a total thickness after drying of 73 μm was obtained in the same manner as in Example 4.
[0156] <Preparation of silicone resin solution> Silicone resin (a) and silicone resin (e) were mixed at a mass ratio (a) / (e) of 99.75 / 0.25 to prepare silicone resin (S8), which was then diluted with toluene and stirred to prepare a silicone resin (S8) solution (solid content concentration 30 mass%). This silicone resin (S8) had a silicone gum (G) / silicone resin (R) mixture ratio ((G) / (R)) of 40.1 / 59.9 and an alkenyl group content of 8.7×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (a). alk )" and "Silicone gum (G) of silicone resin (e) alk The total mass of silicone resin (R) is the amount of silicone resin (R) in silicone-based resin (a).
[0157] Comparative Example 2 In preparing the adhesive solution, 5.88 parts by mass (1.47 parts by mass equivalent to solid content) of a solution of platinum (Pt) metal catalyst "NC-25" (product name, solid content concentration 25 mass%) manufactured by Dow-Toray Industries, Inc. was used instead of 1.93 parts by mass of a solution of the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum(IV)" manufactured by Sigma-Aldrich Japan LLC, and the thickness of the adhesive layer 3 after drying was set to 20 μm. An adhesive tape 1 having a total thickness after drying of 58 μm was obtained in the same manner as in Example 6, except that the thickness of the adhesive layer 3 after drying was set to 20 μm.
[0158] Comparative Example 3 <Preparation of silicone resin solution> Silicone-based resin (d), silicone-based resin (f), and silicone-based resin (h) were mixed so that the mass ratio (d) / (f) / (h) was 0.18 / 90.75 / 9.07 to prepare a silicone-based resin (S9), which was then diluted with toluene and stirred to prepare a silicone-based resin (S9) solution (solid content concentration 30 mass%). This silicone-based resin (S9) had a silicone gum (G) and silicone resin (R) mixture ratio ((G) / (R)) of 36.5 / 63.5 and an alkenyl group content of 3.6×10 -7 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (d). alk The total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (f)" and "silicone gum (G0) of silicone resin (f)." Additionally, the total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (f)" and "silicone resin (R) of silicone resin (h)."
[0159] <Preparation of crosslinker solution> Next, crosslinker (C9) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 0.58 / 99.42, and the resulting mixture was diluted with toluene and stirred to prepare a crosslinker solution (solid concentration: 20 mass%). This crosslinker (C9) had a SiH group content of 2.5×10 -3 It was mol / g.
[0160] <Preparation of adhesive solution> Next, 3.00 parts by mass of the crosslinking agent (C9) solution (0.60 parts by mass in solid content equivalent, molar ratio of SiH group / alkenyl group = 42.4) was mixed with 333.00 parts by mass of the silicone resin (S9) solution (100 parts by mass in solid content equivalent) using a disperser, and stirred and mixed uniformly. Next, 4.87 parts by mass (0.73 parts by mass in solid content equivalent) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disperser, and stirred and mixed uniformly to prepare an adhesive solution for coating.
[0161] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 30 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 68 μm after drying was obtained.
[0162] Comparative Example 4 <Preparation of silicone resin solution> Silicone resin (d) and silicone resin (g) were mixed so that the mass ratio (d) / (g) was 5.56 / 94.44 to prepare a silicone resin (S10), which was then diluted with toluene and stirred to prepare a silicone resin (S10) solution (solid content concentration 30 mass%). This silicone resin (S10) had a silicone gum (G) and silicone resin (R) mixing ratio ((G) / (R)) of 62.2 / 37.8 and an alkenyl group content of 1.1×10 -5 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (d). alk )" and "Silicone gum (G0) of silicone resin (g)." The total mass of silicone resin (R) is the amount of silicone resin (R) in silicone resin (g).
[0163] <Preparation of crosslinker solution> Next, crosslinker (C10) was prepared by mixing crosslinker (m) and crosslinker (n) so that the mass ratio (m) / (n) was 14.88 / 85.12, and the resulting mixture was diluted and stirred with toluene to prepare a crosslinker (C10) solution (solid content concentration: 20 mass%). This crosslinker (C10) had a SiH group content of 5.0×10 -3 The mass ratio was mol / g.
[0164] <Preparation of adhesive solution> Next, 3.65 parts by mass of the crosslinker (C10) solution (0.73 parts by mass in solid content equivalent, molar ratio of SiH group / alkenyl group = 3.3) was mixed with 333.00 parts by mass of the silicone resin (S10) solution (100 parts by mass in solid content equivalent) using a disperser, and the mixture was stirred and mixed uniformly. Next, 5.07 parts by mass (0.76 parts by mass in solid content equivalent) of a solution obtained by diluting the photosensitive platinum (Pt) catalyst "trimethyl(methylcyclopentadienyl)platinum (IV)" manufactured by Sigma-Aldrich Japan LLC with toluene to a solid content concentration of 15% by mass was mixed with a disperser, and the mixture was stirred and mixed uniformly to prepare an adhesive solution for coating.
[0165] Next, this adhesive solution was applied onto a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm. The adhesive solution applied onto the substrate 2 was initially dried in stages at a temperature of 40 to 90° C. in the first half of a drying furnace, and was further dried by heating for 3 minutes in a zone in the second half of the drying furnace where the maximum temperature of the heat treatment was 120° C., to form an adhesive layer 3 having a thickness of 40 μm after drying. Next, a release liner that had been subjected to a release treatment with fluoroalkyl-modified silicone was attached to the adhesive layer 3. As a result, an adhesive tape 1 having a total thickness of 78 μm after drying was obtained.
[0166] Comparative Example 5 A silicone-based resin (S11) solution was prepared as described below. In preparing the adhesive solution, the amount of the photosensitive platinum (Pt) catalyst solution was changed to 5.07 parts by mass (0.76 parts by mass in terms of solid content), and the thickness of the adhesive layer 3 after drying was changed to 20 μm. Except for this, an adhesive tape 1 having a total thickness after drying of 58 μm was obtained in the same manner as in Example 2.
[0167] <Preparation of silicone resin solution> Silicone-based resin (b), silicone-based resin (d), and silicone-based resin (h) were mixed in a mass ratio (b) / (d) / (h) of 91.76 / 0.90 / 7.34 to prepare a silicone-based resin (S11), which was then diluted with toluene and stirred to prepare a silicone-based resin (S11) solution (solid content concentration 30 mass%). This silicone-based resin (S11) had a silicone gum (G) and silicone resin (R) mixing ratio ((G) / (R)) of 33.0 / 67.0 and an alkenyl group content of 3.4×10 -6 The total mass of the silicone gum (G) was calculated by dividing the total mass of the silicone gum (G) by the total mass of the silicone gum (G) of the silicone resin (b). alk )" and "Silicone gum (G) of silicone resin (d) alk The total mass of silicone resin (R) is the sum of "silicone resin (R) of silicone resin (b)" and "silicone resin (R) of silicone resin (h)."
[0168] The layer configurations and compositions of the pressure-sensitive adhesive layer 3 in the pressure-sensitive adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5 are shown in Tables 1 to 3.
[0169] [Table 1]
[0170] [Table 2]
[0171] [Table 3]
[0172] 2. Evaluation method Next, a method for evaluating the pressure-sensitive adhesive tape 1 will be described. (1) Adhesion test (before UV exposure) For the adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5, an adhesive strength test (peel adhesive strength test) to BA-SUS was carried out in accordance with the method described in the test method for adhesive tapes and adhesive sheets (JIS Z 0237 (2009)). Specifically, the adhesive tape 1 with the release liner removed was attached to a bright annealed (BA) treated stainless steel plate (SUS304) with a surface roughness (Ra) of 50±25 nm, and pressure-bonded by moving a roller weighing 2000 g back and forth once at a speed of 5 mm / s. After leaving it for 20 to 40 minutes, the tape was peeled off in a 180° direction against the stainless steel plate at a speed of 5 mm / s using a tensile tester, and the adhesive strength to the polished SUS plate was measured. The adhesive strength test was performed on the adhesive tape 1 before it was irradiated with ultraviolet (UV) rays. As a result of the adhesive strength test, taking into consideration the fixing force when the adhesive tape 1 is used for dicing semiconductor materials, the adhesive strength is preferably 2.4 N / 10 mm or more, and from the viewpoint of picking up semiconductor chips and the like that are individualized by dicing, the adhesive strength is preferably 5.5 N / 10 mm or less. More preferably, the adhesive strength is 2.7 N / 10 mm or more and 4.1 N / 10 mm or less.
[0173] (2) Ball tack test (2-1) Measurement of initial ball tack (before UV irradiation) For the adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5 before UV irradiation, a ball tack test was performed in accordance with the method described in the Test Method for Adhesive Tapes and Adhesive Sheets (JIS Z 0237 (2009)).
[0174] (2-2) Measurement of ball tack after UV irradiation Each of the adhesive tapes produced in Examples 1 to 10 and Comparative Examples 1 to 5 was irradiated with UV light from the substrate side and left to stand for 20 to 40 minutes under conditions of a temperature of 23°C and a humidity of 50±5% RH. Then, the release liner of each adhesive tape 1 was peeled off, and a ball tack test was performed in the same manner as for the initial ball tack, in accordance with the method described in Test methods for adhesive tapes and adhesive sheets (JIS Z 0237 (2009)). UV irradiation is performed using a high-pressure mercury lamp, with an integrated dose of 1200 mJ / cm2 of ultraviolet light with a wavelength of 365 nm. 2 The cumulative light dose was adjusted to 3000 mJ / cm 2 The ball tack was also measured in the same way when the integrated light dose was 1200 mJ / cm 2 Since there was no difference between the case where the integrated light amount was 1200 mJ / cm2, 2 The evaluation was carried out as follows.
[0175] As a result of the ball tack test, it is preferable that the ball tack (ball No.) after UV irradiation is lower than the initial ball tack (ball No.) when the pick-up property of semiconductor chips, etc., which are individualized by dicing is taken into consideration. In other words, when the ball number value before UV irradiation is BN0 and the ball number value after UV irradiation is BN1, it is preferable that the relationship of BN0>BN1 is satisfied. This relationship means that the crosslinking reaction of the pressure-sensitive adhesive layer 3 is promoted by UV irradiation, and the cohesive force is increased compared to before UV irradiation.
[0176] (3) Retention strength test (3-1) Measurement of initial retention strength (before UV irradiation) For the adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5 before UV irradiation, a holding power test was carried out in accordance with the method described in the Test Method for Adhesive Tapes and Adhesive Sheets (JIS Z 0237 (2009)). Specifically, the release liner of each adhesive tape 1 was peeled off, and the adhesive layer 3 was attached to a stainless steel plate (SUS304) polished with waterproof abrasive paper, and held under conditions of a temperature of 40°C and a humidity of 33% RH with a specified weight attached, and the time elapsed until the adhesive tape 1 peeled off from the stainless steel plate and fell (fall time (min)) was measured. Furthermore, the failure mode (whether the failure mode between the adhesive layer 3 and the stainless steel plate was interfacial peeling or cohesive failure) when the adhesive tape 1 was peeled off from the stainless steel plate was observed. The measurement of the fall time in the holding power test was carried out up to 2880 minutes. The results of the holding power test shown in Tables 4 to 6 described later show the fall time (min) and the failure mode of the adhesive tape 1.
[0177] (3-2) Measurement of retention strength after UV irradiation The pressure-sensitive adhesive tape 1 was irradiated with UV under the same conditions as those described above for measuring the ball tack after UV irradiation, and after leaving it for a while, a holding power test was carried out in the same manner as for the initial holding power.
[0178] (3-3) Relationship between retention force and failure mode Here, we will explain the relationship between the holding power and the failure mode of the pressure-sensitive adhesive tape 1. Figure 3 is a schematic diagram showing the relationship between the crosslink density of the silicone resin in the pressure-sensitive adhesive layer 3 and the results of the holding power test of the pressure-sensitive adhesive tape 1 (drop time). As shown in Figure 3, in the adhesive tape 1, as the crosslink density of the silicone-based resin in the adhesive layer 3 increases, the failure mode of the adhesive tape 1 against a stainless steel plate in a holding power test changes from [cohesive failure of the adhesive layer 3 (drop)] → [holding (not dropping)] → [interfacial peeling between the adhesive layer 3 and the stainless steel plate (drop)].
[0179] Furthermore, as shown in FIG. 3, in the region where the failure mode of the pressure-sensitive adhesive tape 1 is cohesive failure, the holding power (drop time) of the pressure-sensitive adhesive tape 1 increases as the crosslink density of the silicone resin in the pressure-sensitive adhesive layer 3 increases. 3, in the region where the failure mode of the adhesive tape 1 is interfacial peeling, the holding power (drop time) of the adhesive tape 1 decreases as the crosslink density of the silicone-based resin in the adhesive layer 3 increases. This is presumably because as the crosslink density of the silicone-based resin increases, the cohesive strength of the adhesive layer 3 increases, decreasing the adhesive strength of the adhesive tape 1, and as a result, the adhesive tape becomes more likely to peel off from the stainless steel plate and fall.
[0180] As a result of the holding power test, it is preferable that the destruction mode at least after UV irradiation is holding or interfacial peeling, it is more preferable that the destruction mode at least after UV irradiation is interfacial peeling, and it is even more preferable that the destruction modes at both the initial stage (before UV irradiation) and after UV irradiation are interfacial peeling. Furthermore, when the destruction modes at both the initial stage (before UV irradiation) and after UV irradiation are interfacial peeling, it is preferable that the drop time is as long as possible or that the adhesive tape 1 does not fall at all at the initial stage (before UV irradiation) from the viewpoint of the fixing force when the adhesive tape 1 is used for dicing semiconductor materials, and it is preferable that the drop time is shorter than that at the initial stage (before UV irradiation) from the viewpoint of the pick-up property of semiconductor chips and the like that are individualized by dicing after UV irradiation. In this case, after the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, when the resulting semiconductor chip or the like is peeled off from the adhesive tape 1, UV irradiation of the adhesive tape 1 makes it less likely that glue will remain on the semiconductor chip or the like.
[0181] (4) Silicone resin adhesive residue test For the pressure-sensitive adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5, a test for adhesive residue on a silicone resin was carried out. First, a mixture was prepared by mixing components A and B of a methyl-containing silicone resin for LED devices (KER-2500N (product name) manufactured by Shin-Etsu Chemical Co., Ltd.) at a mixing ratio of 1:1. This mixture was applied to a stainless steel plate and cured by heating at 100°C for 1 hour and then at 150°C for 2 hours to prepare silicone test piece A. Similarly, a mixture was prepared by mixing components A and B of a phenyl-containing silicone resin (KER-6110 (product name) manufactured by Shin-Etsu Chemical Co., Ltd.), which is a silicone resin for LED devices, in a mixing ratio of 3:7. This mixture was applied to a stainless steel plate and cured by heating at 100°C for 2 hours and then at 150°C for 5 hours to prepare silicone test piece B.
[0182] Next, the release liner of the adhesive tape 1 was peeled off, and the adhesive layer 3 was attached to each of the silicone test pieces A and B, and pressed by moving a roller having a mass of 2000 g back and forth once at a speed of 5 mm / s. Next, similarly to the conditions described in the measurement of ball tack after UV irradiation, the adhesive tape 1 was irradiated with UV from the substrate 2 side, and then left for 120 hours in an environment of a temperature of 40°C and a humidity of 90% RH. Thereafter, the adhesive tape 1 was returned to room temperature, and peeled off in a 90° direction from the silicone test pieces A and B at a speed of 800 mm / s to 1200 mm / s, and the adhesive residue on the silicone test pieces A and B was visually confirmed.
[0183] (5) Epoxy resin adhesive residue test For the pressure-sensitive adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5, an adhesive residue test for epoxy resin was carried out. The adhesive layer 3 of the adhesive tape 1 from which the release liner had been peeled off was attached to an epoxy test piece made of an epoxy resin plate (NL-EG-23 (trade name) manufactured by Nikko Chemical Industry Co., Ltd.) in which a glass cloth substrate was impregnated with epoxy resin, and a roller having a mass of 2000 g was moved back and forth once at a speed of 5 mm / s to press the adhesive layer 3. Then, similar to the conditions described in the measurement of ball tack after UV irradiation, the adhesive tape 1 was irradiated with UV from the substrate 2 side, and then left for 120 hours in an environment of a temperature of 40°C and a humidity of 90% RH. Thereafter, the adhesive tape 1 was returned to room temperature, and the adhesive tape 1 was peeled off in a 90° direction relative to the epoxy test piece at a speed of 800 mm / s to 1200 mm / s, and the adhesive residue on the epoxy test piece was visually confirmed.
[0184] The silicone resin adhesive residue test and epoxy resin adhesive residue test were evaluated according to the following criteria. A rating of A or B was considered a pass. A: No adhesive residue on 100% of the unit area of the test piece B: Adhesive residue is observed in less than 2% of the unit area of the test piece. C: Adhesive residue is observed in the range of 2% to less than 5% per unit area of the test piece. D: Adhesive residue is observed over 5% or more of the unit area of the test piece, or adhesive residue is observed on the edge of the test piece.
[0185] (6) Dicing test The pressure-sensitive adhesive tapes 1 produced in Examples 1 to 10 and Comparative Examples 1 to 5 were subjected to a dicing test. Specifically, first, epoxy resin for molding (Hitachi Chemical Co., Ltd. CEL-400ZHF40-W75G (product name)) was placed in a mold and the sealing pressure was 50 kgf / cm 2 (491N / cm 2 ), the sealing material was heated and cured at 150°C for 300 seconds with a thickness of 0.3 mm to prepare a disk-shaped (diameter 200 mm (8 inches)) dicing test piece. Next, the adhesive layer 3 of the adhesive tape 1 from which the release liner had been peeled off was attached to a dicing ring, and the portion protruding from the ring was cut off, and then further attached to a fluorine-based release film (SS1A (product name) manufactured by Nippa Corporation, thickness 75 μm). Next, a roller with a mass of 2000 g was moved back and forth to pressure-bond the adhesive tape 1 and the ring portion. Next, the fluorine-based release film was peeled off, and a dicing test piece was attached to the adhesive layer 3 in the center portion of the ring and pressure-bonded.
[0186] Furthermore, using a dicing device manufactured by Tokyo Seimitsu Co., Ltd. (A-WD-100A (product name)) and a dicing blade manufactured by Disco Corporation, the dicing test piece was cut into chips of 10 mm x 10 mm together with the adhesive tape 1. At this time, the number of scattered chips was counted, and the fixing force in the dicing test was evaluated. Next, the adhesive tape 1 attached to the chips diced into 10 mm x 10 mm pieces was irradiated with UV under the same conditions as those described in the measurement of ball tack after UV irradiation. After that, the individual chips were picked up from the adhesive tape 1, and the presence or absence of adhesive residue on the chips was visually confirmed to evaluate the adhesive residue in the dicing test. In addition, the number of chips that failed to be picked up when the chips were picked up was counted to evaluate the pick-up ability in the dicing test.
[0187] The fixing strength in the dicing test was evaluated according to the following criteria, with a rating of A or B being considered a pass. A: The number of chips scattered is 0 out of 100, and no chipping is observed. B: The number of chips scattered is 1 out of 100, and no chipping is observed. C: The number of chips scattered is 2 out of 100, and no chipping is observed. D: 3 or more chips are scattered out of 100, or chips are chipped.
[0188] The adhesive residue in the dicing test was evaluated according to the following criteria, with a rating of A being a pass. A: No glue residue is visible on the chip. D: Glue residue is visible on the tip, or adhesive strings are visible on the side of the tip.
[0189] The pickup property in the dicing test was evaluated according to the following criteria, with a rating of A or B being considered a pass. A: The number of chips that failed to be picked up was 0 out of 100 B: The number of chips that failed to be picked up was 1 out of 100 C: The number of chips that failed to be picked up was 2 out of 100 D: The number of chips that failed to be picked up was 3 or more out of 100
[0190] 3. Test Results The evaluation results for the pressure-sensitive adhesive tapes 1 of Examples 1 to 10 and Comparative Examples 1 to 5 are shown in Tables 4 to 6.
[0191] [Table 4]
[0192] [Table 5]
[0193] [Table 6]
[0194] As shown in Tables 4 and 5, it was confirmed that the adhesive tapes 1 of Examples 1 to 10, in which the adhesive layer satisfies the requirements of the present invention, gave favorable results in all of the adhesive strength tests, ball tack tests, holding strength tests, silicone resin adhesive residue tests, epoxy resin adhesive residue tests, and dicing tests (fixing strength, adhesive residue, and pick-up properties).
[0195] Among them, the content of silicon-bonded alkenyl groups in the entire silicone resin is 3.0×10 -6 mol / g or more 1.0×10 -5 The pressure-sensitive adhesive tapes 1 of Examples 1 to 8, in which the content of silicon-bonded alkenyl groups in the entire silicone resin is in the range of 1.9 × 10 -6 mol / g, 2.5×10 -6 In comparison with the pressure-sensitive adhesive tapes 1 of Examples 9 and 10, which have a viscosity of 100 mol / g, the evaluation results in the silicone resin adhesive residue test and the epoxy resin adhesive residue test were generally good.
[0196] This confirmed that the adhesive tapes 1 of Examples 1 to 10 are useful as adhesive tapes for dicing semiconductor materials, more specifically, as dicing adhesive tapes that are attached to the sealing resin side of a semiconductor element substrate and used for dicing.
[0197] In contrast, as shown in Table 6, it was confirmed that the adhesive tapes 1 of Comparative Examples 1 to 5, in which the adhesive layer 3 does not satisfy the requirements of the present invention, had test results inferior to those of Examples 1 to 10 in the silicone resin adhesive residue test, the epoxy resin adhesive residue test, and the dicing test (fixing strength, adhesive residue, and pick-up ability).
[0198] Specifically, in the adhesive tape 1 of Comparative Example 1 in which the adhesive layer 3 does not contain a crosslinking agent, crosslinking of the silicone resin does not occur even when UV irradiation is applied, so no change was observed in the results of the ball tack test and the holding power test before and after UV irradiation, and no increase in the cohesive force of the adhesive layer 3 due to UV irradiation was observed. Therefore, in the adhesive residue test against silicone resin and the adhesive residue test against epoxy resin for confirming practical use, a lot of adhesive residue was observed. Also, in the dicing test, the pick-up ability of the chip of the dicing test piece was poor, and adhesive residue was observed on the chip.
[0199] In addition, in the adhesive tape 1 of Comparative Example 2 in which the adhesive layer 3 does not contain a photosensitive platinum (Pt) catalyst but contains a normal platinum (Pt) catalyst, an addition reaction has already proceeded between the silicon-bonded alkenyl group of the silicone resin in the adhesive layer 3 and the SiH group of the crosslinking agent by the platinum (Pt) catalyst at the stage before UV irradiation, i.e., in the heating and drying process for applying the adhesive layer 3 to the substrate 2, and the adhesive layer 3 has become too hard due to crosslinking and hardening, so that in the dicing test, the fixing force of the dicing test piece is somewhat low and a somewhat large amount of chips are scattered during dicing. Since the adhesive layer 3 does not contain a photosensitive platinum (Pt) catalyst, the cohesive force does not increase even when UV irradiation is applied, and no change was observed in the results of the ball tack test and the holding power test before and after UV irradiation, but since the cohesive force of the adhesive layer 3 is high, no adhesive residue was observed in the silicone resin adhesive residue test and the epoxy resin adhesive residue test. Also, in the dicing test, no adhesive residue was observed for the chips that did not scatter.
[0200] Furthermore, in the adhesive tape 1 of Comparative Example 3, in which the content of silicon-bonded alkenyl groups in the silicone resin in the adhesive layer 3 is less than the lower limit of the requirements of the present invention, no change was observed in the results of the ball tack test and the holding power test before and after UV irradiation, and the effect of increasing the cohesive force of the adhesive layer 3 by UV irradiation was insufficient, and the cohesive force itself was also small. Therefore, many adhesive residues were observed in the silicone resin adhesive residue test and the epoxy resin adhesive residue test. Also, in the dicing test, the pick-up ability of the chip of the dicing test piece was poor, and adhesive residues were observed on the chip.
[0201] Furthermore, in the pressure-sensitive adhesive tape 1 of Comparative Example 4, in which the mixture ratio ((G) / (R)) of the silicone gum (G) and the silicone resin (R) in the silicone resin in the pressure-sensitive adhesive layer 3 exceeds the upper limit of the requirements of the present invention, the ratio of the silicone gum (G) in the pressure-sensitive adhesive layer 3 is high, and in the dicing test, the vibration of dicing is easily transmitted to the pressure-sensitive adhesive layer 3, the vibration amplitude becomes large, and chips are observed in the individualized semiconductor chips. In addition, since the adhesive strength is also low, the fixing strength of the dicing test piece is low, and many chips are scattered during dicing. In addition, since the content of silicon atom-bonded alkenyl groups in the silicone resin in the pressure-sensitive adhesive layer 3 exceeds the upper limit of the present embodiment, when the pressure-sensitive adhesive tape 1 is subjected to a test, the release liner is difficult to peel off from the pressure-sensitive adhesive layer 3, and the workability is poor compared to other pressure-sensitive adhesive tapes 1. In addition, since the effect of increasing the cohesive force of the pressure-sensitive adhesive layer 3 by UV irradiation was sufficient, no adhesive residue was observed in the silicone resin adhesive residue test and the epoxy resin adhesive residue test. In addition, in the dicing test, no adhesive residue was observed on the chips that did not shatter.
[0202] Furthermore, in the adhesive tape 1 of Comparative Example 5, in which the mixture ratio ((G) / (R)) of the silicone gum (G) and the silicone resin (R) is less than the lower limit of the requirements of the present invention, the proportion of the silicone resin (R) having no silicon-bonded alkenyl groups in the adhesive layer 3 is high, and the effect of increasing the cohesive strength of the adhesive layer 3 by UV irradiation cannot be said to be sufficient, and in the adhesive residue test for silicone resin and the adhesive residue test for epoxy resin, a somewhat large amount of adhesive residue thought to be due to uncrosslinked components of the silicone resin (R) was observed. Also in the dicing test, the pick-up ability of the chips of the dicing test piece was poor, and a large amount of adhesive residue was observed on the chips. [Explanation of symbols]
[0203] 1...adhesive tape, 2...base material, 3...adhesive layer, 100...semiconductor element substrate, 101...substrate, 102...semiconductor element, 103...encapsulating resin, 200...semiconductor chip
Claims
1. A dicing adhesive tape comprising a substrate and an adhesive layer laminated on the substrate, the adhesive tape being used when dividing a semiconductor material having a plurality of semiconductor elements covered with a covering material into a plurality of semiconductor chips, The pressure-sensitive adhesive layer is The adhesive composition comprises a silicone resin which is a mixture of a silicone gum (G) and a silicone resin (R), an organopolysiloxane having at least two silicon-bonded hydrogen atoms (SiH groups) in one molecule as a crosslinking agent for the silicone resin, and a photosensitive platinum (Pt) catalyst; a mixing ratio ((G) / (R)) of the silicone gum (G) to the silicone resin (R) in the entire silicone-based resin is in the range of 35.0 / 65.0 to 50.0 / 50.0 in terms of mass ratio; The silicone gum (G) is a silicone gum (G) made of an organopolysiloxane containing a silicon atom-bonded alkenyl group. alk ), The content of the silicon-bonded alkenyl group in the entire silicone resin is 1.8×10 -6 mol / g or more 1.0×10 -5 mol / g or less.
2. 2. The adhesive tape for dicing according to claim 1, wherein the adhesive tape is attached to the semiconductor material in which the plurality of semiconductor elements are sealed with the covering material made of silicone resin from the covering material side.
3. The pressure-sensitive adhesive layer has a silicon atom-bonded alkenyl group content of 3.0×10 in the entire silicone resin. -6 mol / g or more 1.0×10 -5 3. The adhesive tape for dicing according to claim 1, wherein the viscosity is in the range of 0.1 mol / g or less.
4. 4. The pressure-sensitive adhesive tape for dicing according to claim 1, wherein the pressure-sensitive adhesive layer has a molar ratio (SiH group / silicon-bonded alkenyl group) of the content (total amount) of the silicon-bonded hydrogen atoms (SiH groups) in the crosslinking agent contained in the pressure-sensitive adhesive composition to the content (total amount) of the silicon-bonded alkenyl groups in the entire silicone-based resin contained in the pressure-sensitive adhesive composition, in the range of 2.0 to 10.
0.
5. 5. The dicing adhesive tape according to claim 1, wherein the content of the photosensitive platinum (Pt) catalyst in the adhesive composition of the adhesive layer is in the range of 0.10 parts by mass or more and 3.00 parts by mass or less in terms of solid content per 100 parts by mass of the total solid content of the silicone-based resin.
6. The adhesive tape for dicing according to any one of claims 1 to 5, characterized in that it satisfies all of the following conditions (a) to (c) in terms of adhesive properties in accordance with JIS Z 0237 (2009): (a) The adhesive strength to a BA-SUS test plate before light irradiation is in the range of 2.7 N / 10 mm or more and 4.1 N / 10 mm or less. (b) In an inclined ball tack test (inclination angle 30°, temperature 23°C, relative humidity 50% RH), the ball number value before light exposure is BN0 and the ball number value after light exposure is BN1, and the relationship of BN0 > BN1 is satisfied. (c) In a holding power test after light irradiation (temperature 40°C, relative humidity 33% RH, leaving time 2880 minutes), the destruction phenomenon when dropped is interfacial peeling between the pressure-sensitive adhesive layer and the BA-SUS test plate, or the sample does not drop in the holding power test.
7. a bonding step of bonding the pressure-sensitive adhesive tape for dicing according to claim 1 to a semiconductor element substrate having a plurality of semiconductor elements formed thereon and sealed with a sealing resin made of a silicone resin, from the sealing resin side; a cutting step of cutting the semiconductor element substrate to which the dicing adhesive tape is attached into a plurality of semiconductor chips; an irradiation step of irradiating the adhesive tape for dicing the semiconductor element substrate with light; a peeling step of peeling off the adhesive tape for dicing from the plurality of semiconductor chips; A method for manufacturing a semiconductor chip comprising the steps of:
Citation Information
Patent Citations
Dicing method
JP2005093503A
Adhesive tape for dicing / die bonding
JP2007150065A
Adhesive tape for fixing semiconductor wafer, method for manufacturing semiconductor chip and adhesive tape with adhesive film
JP2013038408A
Adhesive tape for dicing and method of manufacturing semiconductor chip
JP2015050216A
Adhesive tape for dicing and method of manufacturing semiconductor chip
JP2016122812A