Water-based adhesive for balls

A water-based adhesive with rubber latex and minimal inorganic filler enhances adhesive strength and softness in hollow balls by accelerating vulcanization, addressing the durability and feel issues of conventional adhesives.

JP7571401B2Active Publication Date: 2024-10-23SUMITOMO RUBBER INDUSTRIES LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020114554
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-02
Publication Date
2024-10-23
Estimated Expiration
2040-07-02

AI Technical Summary

Technical Problem

Existing water-based adhesives for bonding hollow ball cores lack sufficient adhesive strength and can impair the ball's feel due to increased viscosity and hardness, failing to meet the durability and softness requirements of tennis balls and similar sports equipment.

Method used

A water-based adhesive comprising rubber latex, a sulfenamide vulcanization accelerator, and minimal inorganic filler (0.1% by mass or less) is applied to the half cores, allowing for a vulcanization reaction acceleration and maintaining fluidity, ensuring strong adhesion and a soft impact feel.

Benefits of technology

The adhesive achieves high adhesive strength equivalent to conventional adhesives with fillers while maintaining the ball's softness and repulsion performance, suitable for various hardness variations in hollow balls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571401000005
    Figure 0007571401000005
  • Figure 0007571401000006
    Figure 0007571401000006
  • Figure 0007571401000001
    Figure 0007571401000001
Patent Text Reader

Abstract

To provide an aqueous adhesive for a ball excellent in adhesive strength.SOLUTION: An aqueous adhesive for a ball contains a rubber latex as a main component. A content of an inorganic filler of the aqueous adhesive is 0.1 mass% or less in terms of solid content. A manufacturing method of the aqueous adhesive includes: a step of preparing a dispersion medium; a step of putting an additive into the dispersion medium and then adjusting a pH to 8.0 to 12.0 to obtain slurry; and a step of adding the slurry to the rubber latex and mixing thereof. The ball 2 has a hollow core 4 obtained by cross-linking a rubber composition including a vulcanizer. The core 4 includes two hemispherical half cores. The two half cores are bonded using the aqueous adhesive for a ball.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to water-based adhesives, particularly to water-based adhesives used in the manufacture of balls. [Background technology]

[0002] Hollow balls filled with gas are widely used in various sports and training. One such hollow ball is the tennis ball. A tennis ball has a hollow core. The outer surface of this core is covered with two dumbbell-shaped pieces of melton (felt). An adhesive is used to bond the melton to the outer surface of the core.

[0003] Usually, the hollow core is formed by bonding two hemispherical half cores together. An adhesive is also used to bond the two half cores together. Each half core is formed by crosslinking a rubber composition. From the viewpoint of affinity with the rubber composition constituting the half core and adhesive strength, a solvent-based adhesive in which a rubber component, a vulcanizing agent, a vulcanization accelerator, etc. are dissolved in an organic solvent has been used to bond the two half cores together.

[0004] In recent years, water-based adhesives have been considered as an alternative to solvent-based adhesives, from the viewpoint of reducing the impact on the environment and the burden on workers. For example, Japanese Patent Application Laid-Open Nos. 57-179265 and 57-179266 disclose adhesives for melton seams that are based on depolymerized natural rubber latex or synthetic rubber latex. Japanese Patent Application Laid-Open No. 58-98372 proposes an adhesive for melton dumbbells that contains rubber latex and a high-temperature decomposition type vulcanizing agent.

[0005] JP 2007-167 A discloses a method for producing a tennis ball in which an adhesive layer between the core and the felt portion is formed using an aqueous composition containing a metal salt of polyacrylic acid.JP 2000-309766 A proposes an adhesive for tennis ball covers in which a thiuram accelerator and a sulfenimide accelerator are blended with natural rubber latex. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 57-179265 [Patent Document 2] Japanese Unexamined Patent Publication No. 57-179266 [Patent Document 3] Japanese Patent Application Publication No. 58-98372 [Patent Document 4] JP 2007-167 A [Patent Document 5] JP 2000-309766 A Summary of the Invention [Problem to be solved by the invention]

[0007] In playing tennis and the like, the ball is hit repeatedly. If the adhesive strength used to bond the half cores together is weak, there is a risk of breakage due to repeated hits. A ball with weak adhesive strength between the half cores has poor durability. To manufacture a ball with excellent durability, a water-based adhesive with high adhesive strength is required. Patent documents 1-5 all propose water-based adhesives for bonding Melton (felt) to the outer peripheral surface of the core. According to the knowledge of the present inventors, the water-based adhesives in Patent documents 1-5 do not have the adhesive strength required for the core of a hollow ball.

[0008] In tennis, there is a demand for balls that offer a softer feel when hit to meet the needs of a wide range of players. Furthermore, in recent years, new sports that use hollow balls have been developed around the world, and as a result, a wide variety of hollow ball hardness options are now required.

[0009] Conventionally, in order to improve the adhesive strength of adhesives using rubber latex, a technique of compounding additives such as fillers and vulcanizing agents has been known. However, the incorporation of these additives causes the adhesive itself to thicken, which leads to a problem of reduced fluidity. In addition, after curing, the adhesive layer containing these additives becomes too hard, which may impair the hitting feel of the ball.

[0010] An aqueous adhesive that has high adhesive strength and does not impair the hitting feel of the ball has not yet been proposed. An object of the present invention is to provide an aqueous adhesive for balls that has excellent adhesive strength. [Means for solving the problem]

[0011] In playing tennis and the like, a ball with high resilience performance is advantageous. In order to improve resilience performance, a vulcanizing agent, a vulcanization accelerator, an inorganic filler, and the like are compounded in the rubber composition of the core or half core. The vulcanizing agent and the vulcanization accelerator contribute to accelerating the vulcanization reaction of the rubber component. The inorganic filler contributes to improving reinforcement. Among the inorganic fillers, metal oxides such as zinc oxide can also contribute to accelerating the vulcanization reaction. As a result of intensive research, the present inventors have found that the vulcanization reaction accelerating component in the half core can migrate to the aqueous adhesive applied to the half core, and have completed the present invention.

[0012] That is, the aqueous adhesive for balls according to the present invention contains rubber latex as a main component and has an inorganic filler content of 0.1 mass % or less calculated as solid content. Preferably, the rubber latex is natural rubber latex and / or synthetic rubber latex.

[0013] Preferably, the sulfur content of the aqueous adhesive is equal to or greater than 0.5 mass % and equal to or less than 18.0 mass % in terms of solid content.

[0014] Preferably, the aqueous adhesive further comprises a sulfenamide vulcanization accelerator. Preferably, the sulfenamide vulcanization accelerator is represented by the general formula R 1 -SN(-R 2 )-R 3 This compound is represented by the formula: 1 , R 2 and R 3 are each independently a hydrogen atom or a linear, branched or cyclic alkyl group having 3 to 20 carbon atoms, an alkyl ether group, an alkylphenyl group, a nitrogen-containing heterocyclic group, a sulfur-containing heterocyclic group or a nitrogen- and sulfur-containing heterocyclic group. The amount of this sulfenamide vulcanization accelerator is preferably 0.01% by mass or more and 5.0% by mass or less in terms of solid content.

[0015] Preferably, the inorganic filler is one or more selected from the group consisting of silica, carbon black, calcium carbonate, calcium hydroxide, mica, magnesium hydroxide, diatomaceous earth, titanium oxide, zinc oxide, bismuth oxide, barium sulfate, talc, magnesium carbonate, and alumina.

[0016] Preferably, the viscosity of this aqueous adhesive is 20 cps or more and 20,000 cps or less, as measured with a Brookfield type rotational viscometer at 23±1° C. Preferably, the pH of this aqueous adhesive is 7.0 or more and 12.0 or less.

[0017] The method for producing this water-based adhesive is as follows: (1) A step of preparing a dispersion medium by adding a dispersant to water; (2) A step of adding and mixing additives to be blended into the rubber latex into a dispersion medium, and then adjusting the pH of the dispersion medium to 8.0 or more and 12.0 or less to obtain a slurry of the additives; and (3) A step of adding and mixing the obtained additive slurry into rubber latex. Contains:

[0018] The ball according to the present invention has a hollow core formed by crosslinking a rubber composition containing a vulcanizing agent. The core is made up of two hemispherical half cores. The two half cores are bonded together using any of the water-based adhesives described above. Effect of the Invention

[0019] The amount of inorganic filler contained in the aqueous adhesive according to the present invention is 0.1% by mass or less. This aqueous adhesive does not cause an increase in viscosity due to the inorganic filler. This aqueous adhesive has excellent fluidity and can be applied uniformly to the bonding surfaces in a short time. This aqueous adhesive provides sufficient adhesion between the bonding surfaces.

[0020] When this aqueous adhesive is used to bond a half core made of a rubber composition, the vulcanization reaction accelerating component in the half core migrates to the applied aqueous adhesive. The vulcanization reaction of the aqueous adhesive is accelerated by the vulcanization reaction accelerating component migrated from the half core. This results in an adhesive strength equivalent to that of conventional adhesives containing inorganic fillers. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a partially cutaway cross-sectional view of a ball according to one embodiment of the present invention. [Diagram 2] 2(a) and 2(b) are cross-sectional views showing a process for forming the core of the ball in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the present invention will be described in detail based on preferred embodiments with reference to the drawings as appropriate.

[0023] FIG. 1 shows a ball 2 according to one embodiment of the present invention. This ball 2 is a tennis ball 2. As shown in the figure, the tennis ball 2 has a hollow core 4, two felt sections 6 covering the core 4, and a seam section 8 located in the gap between the two felt sections 6. The thickness of the core 4 is usually about 3 mm to 4 mm. The inside of the core 4 is filled with compressed gas. The two felt sections 6 are attached to the surface of the core 4 with an adhesive.

[0024] FIG. 2 is a cross-sectional view for explaining a process for forming the core 4 of the tennis ball 2 of FIG. 1. As shown in FIG. 2(a), in the process for forming the core 4, first, an unvulcanized rubber composition is heated and pressurized to prepare two half cores 20. Each half core 20 is in the shape of a hemispherical shell and has an annular edge portion 21. Next, the water-based adhesive according to the present invention is applied to the edge portion 21 of each half core 20, and sodium chloride and sodium nitrite tablets and water are poured into one half core 20. Thereafter, as shown in FIG. 2(b), the two half cores 20 are bonded together at their edge portions 21. A sphere consisting of the two half cores 20 is put into a predetermined mold and heated and pressurized to form a hollow core 4.

[0025] The main component of the water-based adhesive according to the present invention is rubber latex. When the adhesive applied to the edge portion 21 is heated and pressurized in the process of forming the core 4, the volatile components (mainly water) in the adhesive are removed and the vulcanization reaction of the rubber component derived from the rubber latex proceeds. The adhesive hardens due to the vulcanization reaction of the rubber component, and the two half cores 20 are joined together to form the hollow core 4.

[0026] The inorganic filler contained in the aqueous adhesive according to the present invention is 0.1 mass % or less in terms of solid content. The viscosity of this aqueous adhesive is low. This aqueous adhesive can be applied uniformly to the edge portion 21 in a short time. Furthermore, this aqueous adhesive can flow into minute gaps present in each edge portion 21 after the half cores 20 are bonded together and before it hardens. This improves the adhesion between the half cores 20.

[0027] The rubber composition constituting the half core 20 contains a base rubber, a vulcanizing agent, a vulcanization accelerator, an inorganic filler, and the like. Usually, the half core 20 is formed under conditions that result in semi-vulcanization. Therefore, the formed half core 20 may contain unreacted vulcanizing agents, and the like. In addition, metal oxides such as zinc oxide, which are inorganic fillers, also function as vulcanizing agents. According to the findings of the present inventors, in the process of forming the core 4, vulcanization reaction accelerating components such as unreacted vulcanizing agents contained in the half core 20 act on or transfer to the aqueous adhesive applied to the edge portion 21. This promotes the vulcanization reaction of the aqueous adhesive, improving the adhesive strength after curing. The aqueous adhesive according to the present invention achieves adhesive strength equivalent to that of conventional adhesives containing a predetermined amount of filler, even though it does not contain inorganic filler or contains a small amount of inorganic filler of 0.1 mass % or less in terms of solid content. Furthermore, the aqueous adhesive according to the present invention has an appropriate hardness after curing. This aqueous adhesive does not impair the hitting feeling of the resulting ball 2. This water-based adhesive is suitable for producing a ball 2 that has a soft feel when hit.

[0028] From the viewpoint of fluidity and hardness after curing, the amount of inorganic filler contained in this aqueous adhesive is preferably less than 0.1 mass%. The smaller the amount of inorganic filler, the more preferable, and the lower limit is not particularly limited. An aqueous adhesive that does not contain inorganic filler is particularly preferable.

[0029] When the aqueous adhesive contains an inorganic filler, the type is not particularly limited. Preferably, it is one or more selected from the group consisting of silica, carbon black, calcium carbonate, calcium hydroxide, mica, magnesium hydroxide, diatomaceous earth, titanium oxide, zinc oxide, bismuth oxide, barium sulfate, talc, magnesium carbonate, and alumina. More preferably, it is a metal oxide such as titanium oxide, zinc oxide, or bismuth oxide, and particularly preferably, it is zinc oxide.

[0030] As long as the effects of the present invention can be obtained, the type of rubber latex contained in the aqueous adhesive is not particularly limited. In this specification, rubber latex means an emulsion in which a rubber component is dispersed in the form of fine particles in water or an aqueous solution. Natural rubber latex and / or synthetic rubber latex are preferably used.

[0031] Examples of the synthetic rubber in the synthetic rubber latex include styrene-butadiene rubber, acrylonitrile-butadiene rubber, chloroprene rubber, butadiene rubber, isoprene rubber, butyl rubber, ethylene-propylene rubber, or modified products thereof. Examples of modified products include rubber modified with functional groups such as carboxyl groups, amine groups, and hydroxyl groups. From the viewpoint of adhesive strength, one or more selected from the group consisting of natural rubber latex, styrene-butadiene rubber, butadiene rubber, and isoprene rubber are preferred, and one or more selected including at least natural rubber latex are more preferred, with natural rubber latex being particularly preferred. From the viewpoints of fluidity and adhesion, a more preferred natural rubber latex is depolymerized natural rubber latex.

[0032] The solid content concentration of the rubber latex is preferably 80% by mass or less, more preferably 70% by mass or less, from the viewpoint of mixability with a slurry of various additives described later. From the viewpoint of adhesive strength, the solid content concentration of the rubber latex is preferably 20% by mass or more, more preferably 30% by mass or more. The solid content concentration of the rubber latex is determined in accordance with the method described in JIS K6387-2 "Rubber latex-Part 2: Determination of total solid content".

[0033] Preferably, the aqueous adhesive contains a vulcanization accelerator. A preferred vulcanization accelerator is a sulfenamide vulcanization accelerator. The sulfenamide vulcanization accelerator acts as a reaction retarder in the early stage of the vulcanization reaction of rubber, and acts as a reaction accelerator after a certain time has passed. The sulfenamide vulcanization accelerator can contribute to maintaining the fluidity of the half cores 20 in the early stage of adhesion and to a high curing speed after a certain time has passed.

[0034] A suitable example of the sulfenamide vulcanization accelerator is represented by the general formula R 1 -SN(-R 2 )-R 3 In this general formula, R 1 , R 2 and R 3 are each independently a hydrogen atom or a linear, branched or cyclic alkyl group having 3 to 20 carbon atoms, an alkyl ether group, an alkylphenyl group, a nitrogen-containing heterocyclic group, a sulfur-containing heterocyclic group, or a nitrogen- and sulfur-containing heterocyclic group.

[0035] Specific examples of such compounds include N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazole sulfenamide, N,N'-dicyclohexyl-2-benzothiazolyl sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N-diisopropyl-2-benzothiazole sulfenamide, N-ethyl-2-benzothiazole sulfenamide, etc. One or more selected from the group consisting of N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazole sulfenamide, and N-oxydiethylene-2-benzothiazole sulfenamide are more preferred.

[0036] The amount of the sulfenamide vulcanization accelerator contained in the aqueous adhesive is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and particularly preferably 0.1 mass% or more, calculated as solid content. The amount of the sulfenamide vulcanization accelerator is preferably 5.0 mass% or less, more preferably 2.0 mass% or less, and particularly preferably 1.0 mass% or less, calculated as solid content.

[0037] As long as the effect of the present invention is not impaired, the aqueous adhesive may contain other vulcanization accelerators in place of or together with the sulfenamide vulcanization accelerator. Since the effect of the present invention is remarkable, it is preferable to use the sulfenamide vulcanization accelerator in combination. Examples of vulcanization accelerators that can be used in combination include guanidine vulcanization accelerators, thiazole vulcanization accelerators, thiuram vulcanization accelerators, thiourea vulcanization accelerators, dithiocarbamate vulcanization accelerators, morpholine vulcanization accelerators, aldehyde-amine vulcanization accelerators, aldehyde-ammonia vulcanization accelerators, imidazoline vulcanization accelerators, and xanthate vulcanization accelerators.

[0038] When the sulfenamide-based vulcanization accelerator is used in combination with other vulcanization accelerators, the proportion of the sulfenamide-based vulcanization accelerator in the total vulcanization accelerators is preferably 80 mass% or more, more preferably 90 mass% or more, and particularly preferably 95 mass% or more.

[0039] This aqueous adhesive may contain a vulcanizing agent as necessary. Suitable vulcanizing agents include, for example, sulfur such as powdered sulfur, insoluble sulfur, precipitated sulfur, and colloidal sulfur; and sulfur compounds such as morpholine disulfide and alkylphenol disulfide. The amount of the vulcanizing agent in the aqueous adhesive is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and particularly preferably 1.0% by mass or more, calculated as solid content. The amount of the vulcanizing agent is preferably 40.0% by mass or less, more preferably 30.0% by mass or less, and particularly preferably 20.0% by mass or less, calculated as solid content.

[0040] As long as the effects of the present invention are not impaired, the aqueous adhesive may further contain various additives such as a vulcanization accelerator, an antiaging agent, an antioxidant, a light stabilizer, a softener, a processing aid, and a colorant.

[0041] The concentration of the total solid content (solid content concentration) contained in the aqueous adhesive is not particularly limited. From the viewpoint of adhesive strength, the solid content concentration is preferably 3.0 mass% or more, more preferably 5.0 mass% or more, even more preferably 10 mass% or more, and particularly preferably 15 mass% or more. From the viewpoint of fluidity, the solid content concentration is preferably 70 mass% or less, more preferably 60 mass% or less, and particularly preferably 50 mass% or less.

[0042] Preferably, the aqueous adhesive contains sulfur. The sulfur may be sulfur as an element or may be a sulfur atom constituting a sulfur compound. The sulfur may be derived from a vulcanizing agent or a vulcanization accelerator. The sulfur contained in the aqueous adhesive may contribute to the formation of a crosslinked structure. From the viewpoint of improving adhesive strength, the sulfur content in the aqueous adhesive is preferably 0.5 mass% or more, more preferably 1.5 mass% or more, and particularly preferably 2.0 mass% or more, calculated as solid content. The sulfur content is preferably 18.0 mass% or less, more preferably 10.0 mass% and particularly preferably 7.0 mass%. In the present specification, the sulfur content in the aqueous adhesive is the amount of sulfur element measured in accordance with the oxygen flask combustion method described in the 17th revised Japanese Pharmacopoeia, General Test Methods.

[0043] From the viewpoint of adhesion to the adhesive surface, the viscosity of the aqueous adhesive is preferably 20 cps or more, more preferably 50 cps or more, and particularly preferably 100 cps or more. From the viewpoint of application and flowability, the viscosity of the aqueous adhesive is preferably 20,000 cps or less, more preferably 10,000 cps or less, even more preferably 6,000 cps or less, and particularly preferably 2,000 cps or less. The viscosity of this aqueous adhesive is measured using a Brookfield type rotational viscometer at a measurement temperature of 23±1° C. Details of the measurement method will be described later in the examples.

[0044] From the viewpoint of latex stability, the pH of the aqueous adhesive is preferably adjusted to 7.0 to 12.0, more preferably 7.5 to 11.5, and particularly preferably 8.0 to 10.5. The method for measuring the pH will be described later in the Examples.

[0045] The method for producing the water-based adhesive according to the present invention comprises the steps of: (1) A step of adjusting a dispersion medium by adding a dispersant to water; (2) adding and mixing additives to be blended into the rubber latex into the dispersion medium, and then adjusting the pH of the dispersion medium to 8.0 or more and 12.0 or less to obtain a slurry of the additives; and (3) adding and mixing the resulting additive slurry into the rubber latex; Contains:

[0046] The additives to be blended in the rubber latex are not particularly limited, and may be appropriately selected from vulcanizing agents, vulcanization accelerators, inorganic fillers, antioxidants, antioxidants, light stabilizers, softeners, processing aids, colorants, etc. Two or more additives may be used in combination. As described above, the aqueous adhesive according to the present invention does not need to blend an inorganic filler as an additive. When an inorganic filler is blended, the amount is adjusted to be 0.1 mass% or less in terms of solid content.

[0047] The dispersion medium is used to prepare a slurry of the additive. A dispersant is used to improve the dispersion stability of the additive in the slurry. The type of dispersant is not particularly limited, and is appropriately selected from anionic, nonionic, and cationic surfactants depending on the type of additive and the concentration of the slurry. Examples of anionic surfactants include alkylsulfonates having 8 to 20 carbon atoms, alkylaryl sulfates, sodium naphthalenesulfonate-formaldehyde condensates, and alkali metal salts of rosin acid. Examples of nonionic surfactants include aromatic polyglycol ethers, polyvinyl alcohols, polyoxyethylene alkyl ethers, and polyoxyethylene monostearate. Examples of cationic surfactants include dilauryl dimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, and dodecyl trimethyl ammonium chloride. Anionic or nonionic surfactants are preferred. Two or more surfactants may be used in combination.

[0048] From the viewpoint of the stability of the slurry, the concentration of the dispersant in the dispersion medium is preferably 0.5% by mass or more, more preferably 1.0% by mass or more. From the viewpoint of the adhesive strength of the obtained adhesive, the concentration of the dispersant in the dispersion medium is preferably 20% by mass or less, more preferably 15% by mass or less.

[0049] From the viewpoint of dispersion stability of the latex, the production method preferably further includes a step of adjusting the pH of the dispersion medium to 8.0 or more and 12.0 or less before adding the additive. For example, the dispersion medium may be prepared by dissolving the dispersant in purified water, and then adding ammonia water or the like until a predetermined pH is obtained.

[0050] In this manufacturing method, additives are added to a dispersion medium so as to have a predetermined solid content concentration, and the pH is adjusted to 8.0 to 12.0, and then the mixture is uniformly mixed in a ball mill or the like to obtain an additive slurry. The obtained additive slurry is added to rubber latex and mixed uniformly to produce the aqueous adhesive of the present invention.

[0051] In this manufacturing method, when two or more kinds of additives are blended, a slurry may be prepared for each additive and then a predetermined amount of each slurry may be added to the rubber latex, or a slurry containing two or more kinds of additives in a predetermined composition may be prepared and then this slurry may be added to the rubber latex. This manufacturing method may further include a step of blending the slurry of each additive with the rubber latex and then adding a diluent such as water to adjust the solid content concentration.

[0052] Below, we will explain in detail a preferred rubber composition for core 4 (half core 20) of tennis ball 2 in this embodiment, but the rubber composition of core 4 (half core 20) can be changed within the scope of the present invention.

[0053] Examples of the base rubber of the rubber composition of the core 4 include natural rubber, polybutadiene, polyisoprene, styrene-butadiene copolymer, acrylonitrile-butadiene copolymer, polychloroprene, ethylene-propylene copolymer, ethylene-propylene-diene copolymer, isobutylene-isoprene copolymer, and acrylic rubber. More preferred base rubbers are natural rubber and polybutadiene. Two or more types of base rubbers may be used in combination.

[0054] The rubber composition of the core 4 contains a vulcanizing agent and a vulcanization accelerator. The vulcanizing agent and the vulcanization accelerator described above in relation to the water-based adhesive can be appropriately selected and used. Two or more types of vulcanizing agents or vulcanization accelerators may be used in combination.

[0055] The amounts of vulcanizing agent and vulcanization accelerator in the rubber composition of the core 4 are appropriately adjusted depending on the type. From the viewpoint of resilience performance, the amount of vulcanizing agent is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, per 100 parts by mass of the base rubber. The amount of vulcanizing agent is preferably 5.0 parts by mass or less. From the viewpoint of resilience performance, the amount of vulcanization accelerator is preferably 1.0 part by mass or more, more preferably 2.0 parts by mass or more, per 100 parts by mass of the base rubber. The amount of vulcanization accelerator is preferably 6.0 parts by mass or less.

[0056] The rubber composition of the core 4 may further contain a filler. Suitable fillers include metal oxides such as zinc oxide and titanium oxide, talc, kaolin clay, graphite, graphene, bentonite, halloysite, montmorillonite, mica, beidellite, saponite, hectorite, nontronite, vermiculite, illite, allophane, carbon fiber, carbon nanotubes, carbon black, silica, calcium carbonate, magnesium carbonate, barium sulfate, etc. Two or more of these fillers may be used in combination.

[0057] The amount of filler in the rubber composition of the core 4 is adjusted appropriately depending on the type of filler, but from the viewpoints of resilience performance and durability, the amount is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and particularly preferably 15 parts by mass or more, per 100 parts by mass of the base rubber. From the viewpoint of shot feeling, the amount is preferably 120 parts by mass or less, more preferably 100 parts by mass or less, and particularly preferably 80 parts by mass or less.

[0058] The rubber composition of the core 4 may further contain additives such as a vulcanization aid, an antiaging agent, an antioxidant, a light stabilizer, a softener, a processing aid, and a colorant, as long as the effects of the present invention are not impaired.

[0059] As long as the object of the present invention is achieved, the method for producing the rubber composition is not particularly limited. For example, the rubber composition may be produced by heating and pressurizing a kneaded mixture obtained by adding a base rubber and appropriately selected additives to a known kneading machine such as a Banbury mixer, a kneader, or a roll and kneading the mixture. The kneading conditions and vulcanization conditions are selected depending on the compounding of the rubber composition. The kneading temperature is preferably 50°C or higher and 180°C or lower. The vulcanization temperature is preferably 140°C or higher and 180°C or lower. The vulcanization time is preferably 2 minutes or higher and 60 minutes or lower.

[0060] There are no particular limitations on the method for producing tennis ball 2 having core 4 obtained using this rubber composition. For example, felt portion 6, which has been cut into a dumbbell shape in advance, has an adhesive applied to its back surface, and has seam glue applied to its cross section, is bonded to the surface of core 4 to obtain tennis ball 2. Before bonding felt portion 6, adhesive may be applied to the surface of core 4. Any known adhesive may be appropriately selected and used for bonding felt portion 6 and for the seam glue. EXAMPLES

[0061] The effects of the present invention will be clarified by the following examples, but the present invention should not be construed as being limited based on the description of these examples.

[0062] [Example 1] First, 1.6 parts by mass of sodium naphthalenesulfonate-formaldehyde condensate (BASF's product name "Tamol NN9104") and 0.6 parts by mass of aromatic polyglycol ether (LANXCESS's product name "Emulvin WA") were dissolved in 100 parts by mass of purified water, and the pH was adjusted to 8.0 to 12.0 with commercially available ammonia water (28% by mass) to prepare a dispersion medium. Next, the above-mentioned dispersion medium was added to sulfur (Sanshin Chemical's product name "Sunfel EX") and vulcanization accelerator CBS (Sanshin Chemical's product name "Suncerer CM"), respectively, and stirred for 8 hours or more with a ball mill, and then the pH was adjusted to 8.0 to 12.0 with the above-mentioned ammonia water to obtain a slurry of sulfur (containing 20% ​​oil) (solid concentration 40% by mass) and a slurry of vulcanization accelerator CBS (solid concentration 20% by mass). Finally, 6 parts by mass of the sulfur slurry and 3 parts by mass of the vulcanization accelerator CBS slurry were added to 100 parts by mass of natural rubber latex (HYTEX-HA, solid content concentration 60% by mass) and mixed uniformly to produce the aqueous adhesive of Example 1.

[0063] [Comparative Example 1] In Comparative Example 1, a titanium oxide slurry (solid concentration 40% by mass) and a zinc oxide slurry (solid concentration 40% by mass) were prepared in the same manner as the sulfur (containing 20% ​​oil) slurry (solid concentration 40% by mass) and the vulcanization accelerator CBS slurry (solid concentration 20% by mass) described above in Example 1. Next, 38 parts by mass of the titanium oxide slurry, 8 parts by mass of the zinc oxide slurry, 2 parts by mass of the sulfur slurry, and 2 parts by mass of the vulcanization accelerator CBS slurry were added to 100 parts by mass of natural rubber latex (HYTEX-HA, solid concentration 60% by mass) and mixed uniformly to produce the aqueous adhesive of Comparative Example 1.

[0064] [Examples 2-6 and Comparative Example 2] The aqueous adhesives of Examples 2-6 and Comparative Example 2 were produced in the same manner as in Example 1, except that the amounts of latex and each slurry were changed to those shown in Table 1-2 below.

[0065] [Table 1]

[0066] [Table 2]

[0067] Details of the compounds listed in Table 1-2 are as follows: The numbers in parentheses in the left column of Table 1-2 indicate the solid content concentration. Natural rubber: HYTEX-HA (Nomura Trading Co., Ltd.) (solids concentration 60% by mass) SB rubber: Styrene-butadiene rubber latex manufactured by JSR Corporation (solid content concentration 50% by mass) Titanium oxide: Ishihara Sangyo Kaisha, Ltd. product name "A220" Zinc oxide: Product name "Zinc oxide type 2" manufactured by Seido Chemical Co., Ltd. Sulfur: Insoluble sulfur manufactured by Sanshin Chemical Industry Co., Ltd., product name "Sanfer EX", contains 20% oil CBS: Sanshin Chemical Co., Ltd. vulcanization accelerator, N-cyclohexyl-2-benzothiazole sulfenamide, product name "Suncerer CM" TBBS: Vulcanization accelerator manufactured by Sanshin Chemical Industry Co., Ltd., N-(t-butyl)-2-benzothiazole sulfenamide, trade name "Suncerer NS" MBS: Sanshin Chemical Co., Ltd. vulcanization accelerator, N-oxodiethylene-2-benzothiazole sulfenamide, product name "Suncerer NOB"

[0068] [Viscosity measurement] The viscosity of the water-based adhesives of Examples 1-6 and Comparative Examples 1-2 was measured using a Brookfield rotational viscometer (TVC-10 viscometer, rotor No. 2, manufactured by Toki Sangyo Co., Ltd.) in accordance with the description of JIS Z8803 "Method of measuring viscosity of liquids." The average value of three measurements taken at a temperature of 23±1°C and a rotation speed of 20 rpm is shown below in Table 3-4 as the viscosity (cps).

[0069] [pH measurement] Using a pH meter (TPX-999 manufactured by Toko Chemical Laboratory), the pH of the aqueous adhesives of Examples 1-6 and Comparative Examples 1-2 was measured at a temperature of 23° C. The average value of three measurements for each was shown as pH in Tables 3-4 below.

[0070] [Adhesive strength] (Preparation of test core) 100 parts by mass of natural rubber (trade name "SMR CV60" of Astlett Rubber Co.), 15 parts by mass of carbon black (trade name "N330" of Cabot Japan Co.), 4 parts by mass of silica (trade name "Nipsil VN3" of Tosoh Silica Corporation), 30 parts by mass of kaolin clay (trade name "ECKALITE 120" of Imerys Co.), 17 parts by mass of magnesium carbonate (trade name "Kinsei" of Konoshima Chemical Co., Ltd.), and 5 parts by mass of zinc oxide (trade name "Zinc Oxide Type 2" of Seido Chemical Co., Ltd.) were charged into a Banbury mixer and kneaded at 90° C. for 5 minutes. 0.5 parts by mass of salicylic acid (trade name of Tokyo Chemical Industry Co., Ltd.), 2.3 parts by mass of 1,3-diphenylguanidine (trade name "Suncerer D" of Sanshin Chemical Co., Ltd.), and 3.5 parts by mass of sulfur (the above-mentioned trade name "Sunfel EX") were added to the kneaded product and kneaded at 50° C. for 3 minutes using an open roll to obtain a rubber composition.

[0071] The obtained rubber composition was poured into a mold and pressed at 140°C for 4 minutes to form two half cores. The edges of each half core were treated with sandpaper (#100), and then the water-based adhesive of Example 1 was applied to the edges and dried at room temperature for 2 hours or more. Then, 0.5 ml of water was poured into one half core, and the half core was attached to the other half core, and heated at 150°C for 6 minutes to produce a test core 1. Similarly, test cores 2-6 and comparative test cores 1-2 were produced using the water-based adhesives of Examples 2-6 and Comparative Example 1-2.

[0072] (Tensile test) Three JIS No. 3 dumbbell pieces (2 mm thick) were cut out as test pieces from each of the test core 1-6 and the comparative test core 1-2. Each test piece was cut out so that the adhesive surfaces of the two half cores were located in the center of the dumbbell piece.

[0073] A tensile test was performed on each test piece using a tensile tester (Shimadzu Corporation, product name "Autograph AGS-X") at a tensile speed of 500 mm / min, and the cross section of the test piece after breakage was observed. Adhesive strength was evaluated by judging three test pieces each as "good" if they had substrate failure (failure at a surface other than the adhesive surface) and "bad" if they had interface failure (failure at any edge) or cohesive failure (failure at the adhesive layer). The number of test pieces judged as "good" is shown in Table 3-4 below. The higher the number, the higher the evaluation. Adhesive strength was evaluated as follows: A: three out of three pieces were "good", B: two out of three pieces were "good", and C: one out of three pieces were "good".

[0074] [Ball feel] In the same manner as described above for the evaluation of adhesive strength, test cores were prepared using the aqueous adhesives of Examples 1-6 and Comparative Examples 1-2. Tennis balls were produced by attaching two felt pieces with seam glue applied to their cross sections to the surface of each core.

[0075] After manufacturing, each tennis ball was left to stand for 24 hours under atmospheric pressure, at a temperature of 20°C and a relative humidity of 60%, and then 50 players hit each ball with a tennis racket and asked about the feel of the ball when hit. Based on the number of players who answered that the ball felt "soft and good when hit," the following ranking was made. The results are shown in Table 3-4 below. A: More than 40 people B:30-39 people C: 20 people or less

[0076] [Table 3]

[0077] [Table 4]

[0078] As shown in Table 3, the viscosity of Example 1 is lower than that of Comparative Example 1, which has the same composition other than the inorganic filler and the same pH. Furthermore, as shown in Tables 3-4, the aqueous adhesive of the Example, which does not contain any inorganic filler or contains only a small amount of inorganic filler, has an adhesive strength equivalent to that of the aqueous adhesive of the Comparative Example, which contains a large amount of inorganic filler. Furthermore, the aqueous adhesive of the Example does not inhibit the soft hitting feeling. From these evaluation results, the superiority of the present invention is clear. [Industrial Applicability]

[0079] The water-based adhesive described above can be applied to the production of various balls obtained by using the rubber composition. [Explanation of symbols]

[0080] 2. Ball 4. Core 6 Felt section 8. Seam part 20. Half core 21 Edge section

Claims

1. A water-based adhesive to be applied to a portion of a ball that is formed from a rubber composition that contains a vulcanizing agent, a vulcanization accelerator, and an inorganic filler, comprising: The rubber latex is contained as a main component, and the content of an inorganic filler is 0.1% by mass or less in terms of solid content, The composition further contains a sulfenamide vulcanization accelerator, and the amount of the sulfenamide vulcanization accelerator is 0.01% by mass or more and 5.0% by mass or less in terms of solid content, The sulfur content is 0.5% by mass or more and 18.0% by mass or less in terms of solid content, An aqueous adhesive for balls, having a viscosity of 20 cps or more and 20,000 cps or less, as measured at 23±1° C. using a Brookfield rotational viscometer.

2. 2. The water-based adhesive of claim 1, wherein the rubber latex is a natural rubber latex and / or a synthetic rubber latex.

3. The sulfenamide vulcanization accelerator is represented by the general formula R 1 -S-N (-R 2 )-R 3 This compound is represented by the formula: 1 , R 2 and R 3 are each independently a hydrogen atom, a linear, branched or cyclic alkyl group having 3 to 20 carbon atoms, an alkyl ether group, an alkylphenyl group, a nitrogen-containing heterocyclic group, a sulfur-containing heterocyclic group, or a nitrogen- and sulfur-containing heterocyclic group. The aqueous adhesive according to claim 1 or 2.

4. The aqueous adhesive according to any one of claims 1 to 3, wherein the inorganic filler is one or more selected from the group consisting of silica, carbon black, calcium carbonate, calcium hydroxide, mica, magnesium hydroxide, diatomaceous earth, titanium oxide, zinc oxide, bismuth oxide, barium sulfate, talc, magnesium carbonate, and alumina.

5. 5. The aqueous adhesive according to claim 1, having a pH of 7.0 or more and 12.0 or less.

6. A step of preparing a dispersion medium by adding a dispersant to water; a step of adding and mixing additives to be blended in the rubber latex into the dispersion medium, and then adjusting the pH of the mixture to 8.0 or more and 12.0 or less to obtain a slurry of the additives; The method for producing the water-based adhesive according to any one of claims 1 to 5, further comprising the step of adding the slurry of additives obtained in the above step to the rubber latex and mixing the same.

7. The rubber composition includes a vulcanizing agent, a vulcanization accelerator, and an inorganic filler. The rubber composition is crosslinked to form a hollow core. The core is composed of two hemispherical half cores, A ball, wherein the two half cores are attached together using the water-based adhesive according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Adhesive for tennis ball melt seaming

    JP1982179265A

  • Adhesive for tennis ball

    JP1982179266A

  • Adhesive for tennis ball melton dumbbell

    JP1983098372A

  • Rubber composition

    JP1985099149A

  • Adhesive and tackifier

    JP1997249863A