Composite fibers and composite blended fibers, woven and knitted fabrics, and clothing containing the same
The composite fiber, with specific molecular weight and cross-sectional design, addresses the challenge of achieving stretchability, abrasion resistance, and a worsted appearance, offering a soft texture and natural appearance for fabrics and clothing.
Patent Information
- Application Number
- JP2022506132
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-25
- Filing Date
- 2022-01-07
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-01-07
AI Technical Summary
Existing composite fibers fail to simultaneously achieve stretchability, abrasion resistance, and a worsted appearance similar to wool, with issues such as peeling, whitening, and insufficient stretch performance in side-by-side and eccentric core-sheath types, and heathered feel not replicated in eccentric core-sheath fibers.
A composite fiber composed of polyester thermoplastic resins A and B with specific molecular weight differences, thickness ratios, and cross-sectional coverage, along with controlled crimp development, achieves high sensitivity and a delicate worsted texture.
The composite fiber exhibits excellent stretch performance, abrasion resistance, and a soft texture with a natural appearance, suitable for woven and knitted fabrics and clothing, providing a delicate worsted texture and deep natural appearance.
Smart Images

Figure 0007571783000003 
Figure 0007571783000004 
Figure 0007571783000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite fiber, and a woven / knitted fabric and a garment containing the same, and in particular to a composite fiber having high sensitivity such as a delicate worsted texture and a deep, natural appearance and functionality such as stretchability, and to a composite mixed fiber, a woven / knitted fabric and a garment containing the same. [Background technology]
[0002] There has been a demand for worsted fabrics that reproduce the fluffy soft texture and high resilience of wool materials, such as firmness and stiffness. In particular, in recent years, there has been a demand for fabrics that reduce the sense of restriction on the wearer when used in clothing and that have the ability to follow movements, that is, fabrics that have the same worsted appearance as wool materials and also have excellent stretch performance.
[0003] Furthermore, woven and knitted fabrics made of natural fibers such as wool generate a large amount of fiber waste during use, washing, etc. In particular, fiber waste that falls off from the fibers during washing can cause various problems such as increased waste, a burden on wastewater treatment, and a burden on the maintenance of washing machines, etc.
[0004] To date, as a fabric having a worsted texture, for example, a worsted texture fabric made of composite fibers that has been subjected to thick-and-thin processing to imitate the scale-like structure formed on the surface of wool fibers, as disclosed in Patent Document 1, has been proposed.
[0005] On the other hand, eccentric sheath-core composite fibers, such as those disclosed in Patent Document 2, are known as fibers used in stretchable fabrics. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-328248 A [Patent Document 2] International Publication No. 2018 / 110523 Summary of the Invention [Problem to be solved by the invention]
[0007] One of the means for suppressing fiber shedding is to obtain a worsted-like fabric using long fibers. However, in the technology disclosed in Patent Document 1, when the composite fiber is a side-by-side type, friction or impact causes peeling at the interface, resulting in partial white streak-like whitening and fluffing, which reduces the quality of the fabric. Furthermore, since cracks during alkali treatment occur only on one side of the surface, there is a problem that the delicate worsted texture is not fully expressed. Patent Document 1 also describes a case where the composite fiber is a conventional eccentric core-sheath type, but since the high shrinkage component is covered by the low shrinkage component, there is also a problem that sufficient stretch performance is not exhibited compared to the side-by-side type. In other words, it has not been possible to simultaneously satisfy stretchability, abrasion resistance, and a worsted-like appearance.
[0008] Patent Document 2 discloses an invention relating to a fabric with an excellent uniform and smooth appearance, which is the exact opposite of heathered or worsted texture. Therefore, it does not have the heathered texture of natural wool. In addition, a method of blending with a component having a different dyeability is disclosed as a means of obtaining a heathered texture, but this results in a large change in heathered pitch due to twisting the yarn.
[0009] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a composite fiber which satisfies both the characteristics of stretch performance and abrasion resistance, and which exhibits a delicate worsted texture closer to wool, a deep natural appearance and high sensitivity, and a composite blended fiber, a woven or knitted fabric and a garment containing the same. [Means for solving the problem]
[0010] The conjugated fiber of the present invention is made of a polyester-based thermoplastic resin A and a polyester-based thermoplastic resin B, and satisfies the following requirements (1) to (4). (1) Weight average molecular weight M of the polyester thermoplastic resin A Aand the weight average molecular weight M of the polyester thermoplastic resin B B Difference from (M A -M B ) is between 2000 and 15000. (2) In the composite fiber, the apparent thickness ratio (D thick / D thin ) is 1.05 to 3.00. (3) In the cross section of the composite fiber, the polyester-based thermoplastic resin B covers the polyester-based thermoplastic resin A, and the minimum value t of the thickness t of the polyester-based thermoplastic resin B is min and the fiber diameter D of the composite fiber (t min / D) is 0.01 to 0.10 (4) In the cross section of the composite fiber, the thickness t is 1.00t min ≦t≦1.05t min The perimeter C of the part that satisfies t is the circumference C of the entire composite fiber, t ≧0.33C.
[0011] According to a preferred embodiment of the conjugate fiber of the present invention, the conjugate fiber has a hysteresis loss rate during elongation recovery at a maximum load of 0.5 cN / dtex of 0 to 70%.
[0012] According to a preferred embodiment of the composite fiber of the present invention, the composite fiber has a thickness-slenderness ratio LR1 (L2 / L1) of the thickness length (L1) to the thin portion length (L2) in the fiber axis direction at a measurement load of 0.00166 cN / dtex of 0.90 to 1.40, and the ratio (LR2 / LR1) of the thickness-slenderness ratio LR2 at a measurement load of 0.11 cN / dtex to the thickness-slenderness ratio LR1 at a measurement load of 0.00166 cN / dtex is 1.20 to 2.10.
[0013] According to a preferred embodiment of the composite fiber of the present invention, at least the apparent thickness of the composite fiber is a thick fiber diameter (D thick ) has cracks on the surface of the composite fiber.
[0014] In addition, the composite mixed fiber of the present invention is obtained by further combining at least one other type of yarn with the composite fiber of the present invention.
[0015] The woven or knitted fabric of the present invention at least partially contains the composite fiber or the composite mixed fiber.
[0016] Furthermore, the garment of the present invention at least partially comprises the composite fiber or the composite mixed fiber, or the woven or knitted fabric. Effect of the Invention
[0017] According to the present invention, a composite fiber having a fluffy soft feel and high resilience such as firmness and stiffness can be obtained. In particular, the composite fiber of the present invention has excellent stretchability and abrasion resistance, and can be made into composite mixed fibers and woven and knitted fabrics that have a delicate worsted texture closer to natural wool, a deep natural appearance, and a high sense of aesthetics, and can be made into outerwear items for women and men's clothing, such as jackets, suits, and bottoms. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of the state in which polyester thermoplastic resin A and polyester thermoplastic resin B exist in the conjugate fiber of the present invention. [Diagram 2] FIG. 2 is a perspective view illustrating one embodiment of the surface of a composite fiber of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of a drawing apparatus used in producing the composite fiber of the present invention. [Figure 4] FIG. 4 is a schematic diagram of a final distribution plate according to Example 1 of the composite fiber of the present invention. [Diagram 5] FIG. 5 is a schematic diagram of a final distribution plate according to Comparative Example 3 of the composite fiber of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The conjugated fiber of the present invention contains a polyester-based thermoplastic resin A and a polyester-based thermoplastic resin B, and satisfies the following requirements (1) to (4). (1) Weight average molecular weight M of the polyester thermoplastic resin A A and the weight average molecular weight M of the polyester thermoplastic resin B B Difference from (M A -M B ) is between 2000 and 15000. (2) In the composite fiber, the apparent thickness ratio (D thick / D thin ) is 1.05 to 3.00. (3) In the cross section of the composite fiber, the polyester-based thermoplastic resin B covers the polyester-based thermoplastic resin A, and the minimum value t of the thickness t of the polyester-based thermoplastic resin B is min and the fiber diameter D of the composite fiber (t min / D) is 0.01 to 0.10. (4) In the cross section of the composite fiber, the thickness t is 1.00t min ≦t≦1.05t min The perimeter C of the part that satisfies t is the circumference C of the entire composite fiber, t ≧0.33C.
[0020] The present invention will be described in detail below, but the present invention is not limited to the scope of the following description as long as it does not deviate from the gist of the present invention.
[0021] [Polyester-based thermoplastic resin A, Polyester-based thermoplastic resin B] The conjugate fiber of the present invention contains a polyester-based thermoplastic resin A and a polyester-based thermoplastic resin B.
[0022] Specific examples of the polyester resin used in the conjugate fiber of the present invention include polyethylene terephthalate resins whose main repeating unit is ethylene terephthalate, polytrimethylene terephthalate resins whose main repeating unit is trimethylene terephthalate, and polybutylene terephthalate resins whose main repeating unit is butylene terephthalate. More preferably, the main repeating unit of both polyester thermoplastic resin A and polyester thermoplastic resin B is ethylene terephthalate.
[0023] The polyethylene terephthalate resin, polytrimethylene terephthalate resin, and polybutylene terephthalate resin may have a small amount (usually less than 30 mol%) of copolymerization component as necessary. If the copolymerization component of the polyester thermoplastic resin A is 8 mol% or less, it is easy to reduce the hysteresis loss to 70% or less, which is preferable. Furthermore, by making the copolymerization component 8 mol% or less, the molecular orientation in the composite fiber can be maintained even after dyeing processing, and dimensional stability is improved. In addition, preferably, the copolymerization component of both the polyester thermoplastic resin A and the polyester thermoplastic resin B is 5 mol% or less, and more preferably, neither the polyester thermoplastic resin A nor the polyester thermoplastic resin B contains a copolymerization component.
[0024] The polyester-based thermoplastic resin A and the polyester-based thermoplastic resin B in the present invention may contain, as necessary, one or more of a micropore-forming agent, a cationic dyeable agent, a coloring inhibitor, a heat stabilizer, a flame retardant, a fluorescent brightening agent, a matting agent, a colorant, an antistatic agent, a moisture absorbent, an antibacterial agent, inorganic fine particles, etc., within the scope not impairing the object of the present invention.
[0025] The composite fiber of the present invention has a weight average molecular weight M A and the weight average molecular weight M of polyester thermoplastic resin B B Difference from (M A -M B(hereinafter, sometimes simply referred to as "difference in weight-average molecular weight") is 2000 to 15000. By making the difference in weight-average molecular weight 2000 or more, preferably 5000 or more, a composite fiber with higher resilience and stretchability can be obtained. On the other hand, by making the difference in weight-average molecular weight 15000 or less, preferably 13000 or less, the strength of the raw yarn can be improved and stable spinning can be performed.
[0026] In addition, the weight average molecular weight M of the polyester thermoplastic resin A A The range of the weight average molecular weight M of the polyester thermoplastic resin B is preferably 20,000 to 28,000. B The range of the value of is preferably 12000 to 20000. When each of the values is within this range, the functionality and durability of the composite fiber are improved, and the process stability when spinning the composite fiber is also improved.
[0027] In the present invention, the weight average molecular weight is determined by dissolving 2.0 mg of composite fiber in 2.5 cm of tetrahydrofuran. 3 A measurement solution is prepared by completely dissolving the material in polystyrene, and a gel permeation chromatography test is performed using polystyrene as the standard substance, and the value obtained is expressed as an integer value. For example, the "TOSO GMHHR-H(S)HT" manufactured by Tosoh Corporation is used as the gel permeation chromatography (GPC) tester.
[0028] [Composite fiber] In the conjugated fiber of the present invention, polyester thermoplastic resin B covers polyester thermoplastic resin A. That is, as illustrated in Fig. 1, in a cross section substantially perpendicular to the fiber axis of the conjugated fiber, polyester thermoplastic resin A and polyester thermoplastic resin B are present in a bonded state without being substantially separated, and polyester thermoplastic resin B covers polyester thermoplastic resin A on the fiber surface, thus providing a conjugated cross section. In addition, either short fibers or long fibers may be used, but long fibers are preferred from the viewpoint of fiber waste.
[0029] At this time, in the cross section of the composite fiber, the minimum thickness t of the polyester thermoplastic resin B covering the polyester thermoplastic resin A is t min and the fiber diameter D of the composite fiber (t min / D) is 0.01 to 0.10. If it is less than 0.01, the fabric quality and abrasion resistance will decrease due to fuzz, etc. Preferably, it is 0.02 or more. If it exceeds 0.10, it will be difficult to obtain sufficient crimp development and stretch performance. Preferably, it is 0.08 or less.
[0030] In addition, in the cross section of the composite fiber of the present invention, the thickness t is 1.00t min ≦t≦1.05t min The perimeter C of the part that satisfies t is the circumference of the entire composite fiber, C t ≧0.33C. By doing so, the area (S A ) and the area of polyester thermoplastic resin B (S B ) ratio is the same as that of conventional eccentric core-sheath composite fibers, the centers of gravity of the regions where the resins are present are farther apart, so that the resulting crimped fibers can form finer spirals and exhibit good crimp. Furthermore, in order to obtain crimp suitable for woven and knitted fabrics with worsted texture, t It is more preferable to set the temperature to ≧0.40C. In principle, t <Cとなるが、C t ≦0.70C is preferred.
[0031] Furthermore, the composite fiber of the present invention has an apparent thickness-thinness ratio (D thick / D thin In the present invention, the apparent thick-thin ratio (D thick / D thin ) is the fiber diameter (D) of the part of the composite fiber bundle whose width in the direction perpendicular to the fiber axis direction is relatively thicker than the average value at a load of 0.11 cN / dtex. thick ) and the fiber diameter of the part that is relatively thinner than the average (D thin The apparent thickness ratio (D thick / Dthin If the value of t is less than 1.05, the woven or knitted fabric will not have a worsted appearance like that of a natural fiber woven or knitted fabric. It is preferably 1.25 or more, and more preferably 1.40 or more. If the value of t exceeds 3.00, the appearance will deviate from the natural appearance and will not be favorable, so it is preferably 2.00 or less. Specific methods for measuring the thickness t, fiber diameter D, thick-thin ratio, circumference C, etc. are as described in the Examples.
[0032] By simultaneously satisfying the above-mentioned requirements (1) to (4), the present invention can simultaneously achieve a worsted texture and a natural appearance, as well as abrasion resistance, which is an issue with side-by-side type conjugate fibers, and stretchability, which is an issue with general eccentric core-sheath types.
[0033] The cross-sectional shape of the composite fiber is not particularly limited, and may be a circle, an ellipse, a triangle, or the like. However, a circle is more preferable because it allows a composite fiber that satisfies the requirements (1) to (4) to be spun stably.
[0034] In the composite fiber of the present invention, the area (S A ) and the area of polyester thermoplastic resin B (S B ) and S A :S B However, when the ratio is preferably 70:30 to 30:70, and more preferably 60:40 to 40:60, the physical properties are improved. A >S B It is preferable that:
[0035] Next, the composite fiber of the present invention preferably has a hysteresis loss rate of 0 to 70%, more preferably 40 to 70%, when the composite fiber is stretched and recovered at a maximum load of 0.5 cN / dtex. If the hysteresis loss rate is 70% or less, the garment made of the woven or knitted fabric using the composite fiber of the present invention has sufficient recovery even when stretched in accordance with the movement of the body, and the strain on the garment is small, so this is preferable. Furthermore, if the hysteresis loss rate is 40% or more, this is even more preferable because the garment does not tighten excessively after stretching. Note that the hysteresis loss rate is 0% or more due to the measurement method.
[0036] The composite fiber of the present invention preferably has a thickness-thinness ratio LR1 (L2 / L1) of the thick length (L1) to the thin length (L2) in the fiber axis direction at a measurement load of 0.00166 cN / dtex (1.5 mg / Denier) of 0.90 to 1.40. By setting the measurement load to 0.00166 cN / dtex (1.5 mg / Denier), slack can be mainly eliminated when measuring the composite fiber of the present invention. In the composite fiber of the present invention, the thin parts where the orientation is relatively advanced usually become light in color, and the thick parts where the orientation is not advanced become dark in color due to dyeing processing. By setting LR1 to 0.90 to 1.40, it is possible to obtain an appearance with excellent worsted-like light and dark mottled patterns when dyeing a woven or knitted fabric. Increasing LR1 can increase the number of light-colored parts, and decreasing LR1 can increase the number of dark-colored parts. Since the worsted tone can be emphasized by having slightly more light colors than dark colors, LR1 is preferably 1.00 or more, and more preferably 1.10 or more.
[0037] However, in order to obtain a better worsted texture in a composite fiber with stretch performance, in addition to the above-mentioned LR1 being 0.90 to 1.40, it is preferable that the ratio (LR2 / LR1) of the thickness-thin ratio LR2 at a measurement load of 0.11 cN / dtex (0.10 g / Denier) to the thickness-thin ratio LR1 at a measurement load of 0.00166 cN / dtex (1.5 mg / Denier) is 1.20 to 2.10. Here, LR2 is the ratio (L4 / L3) of the thickness length (L3) to the thin length (L4) in the fiber axis direction of the composite fiber at a measurement load of 0.11 cN / dtex. Worsted texture woven and knitted fabrics such as wool woven and knitted fabrics do not have stretchability even when used, so there is little change in appearance. On the other hand, in fabrics having stretchability and worsted texture, there have been cases where the appearance was poor when used, but according to the study by the present inventors, it was found that this was due to the change in appearance caused by stretching. By setting the range of the present invention as described above, excessive changes in the balance of light and dark shades when the woven or knitted fabric is stretched can be suppressed, and a natural appearance can be imparted. The reason for setting the measurement load at 0.11 cN / dtex (0.10 g / Denier) is to correspond to the stress assumed when a garment made of a woven or knitted fabric using the composite fiber of the present invention is stretched in accordance with the movement of the body. The composite fiber of the present invention exhibits coil-shaped crimp due to the shrinkage difference between the polyester thermoplastic resin A and the polyester thermoplastic resin B by the heat treatment of the dyeing process, and this crimp is actively exhibited in the details where the structure difference is large. Furthermore, when the LR2 / LR1 is 1.20 to 2.10, the crimp in the details is stretched, and the stretchability is also excellent. By making the LR2 / LR1 ratio 1.20 or more, more preferably 1.30 or more, and even more preferably 1.40 or more, the fabric will have excellent stretchability, and by making it 2.10 or less, more preferably 2.00 or less, and even more preferably 1.90 or less, the fine details ratio during elongation will be maintained, resulting in an appearance with excellent worsted-like shading and flecks. The values of the thick length and fine details length mentioned above are values measured by the method described in the Examples.
[0038] Next, the composite fiber of the present invention has at least a thick fiber diameter (D thick) on the surface of the composite fiber. More preferably, the cracks are formed in a direction substantially perpendicular to the longitudinal direction of the composite fiber. Even more preferably, the depth of the cracks in the direction substantially perpendicular to the composite fiber varies in the circumferential direction of the fiber. The depth of the cracks is preferably 0.5 to 5.0 μm. In this way, the woven or knitted fabric using the composite fiber can be given a more delicate worsted texture and a deep, natural appearance.
[0039] Here, the depth of the crack is measured at the deepest point of the crack. The direction substantially perpendicular to the longitudinal direction of the composite fiber means that the crack is formed along the circumference substantially perpendicular to the longitudinal direction of the composite fiber, as illustrated in FIG. 2. The length of the crack in the circumferential direction of the composite fiber is not particularly limited, but it is more preferable that the length is 1 / 2 or more of the length of the outer circumference of the composite fiber, because the composite fiber can have a natural worsted appearance when made into a woven or knitted fabric, as when natural fibers are used. In the present invention, the depth and length of the crack are observed using an electron microscope, and the average value of 10 cracks measured in one composite fiber is used. The specific measurement method is as described in the Examples.
[0040] The average fiber diameter D of the composite fiber in the present invention ave The average fiber diameter D is preferably 10 μm to 30 μm. By setting the diameter in this range, it is possible to obtain a woven or knitted fabric having firmness, elasticity, stretchability, and a soft feel closer to that of natural wool materials. ave is a value calculated from the fineness of the composite fiber.
[0041] The conjugate fiber of the present invention may also preferably take the form of flat yarn, crimped yarn, air-jet textured yarn, air entangled yarn, twisted yarn, or the like, depending on the desired purpose.
[0042] [Combined composite fibers, woven and knitted fabrics, and clothing] The composite mixed fiber of the present invention is a composite fiber of the present invention further mixed with at least one other yarn. The woven or knitted fabric of the present invention contains at least a part of the composite fiber and / or composite mixed fiber of the present invention. In this way, as described above, it is possible to obtain an appearance with a natural worsted texture like that when natural fibers are used. The woven or knitted fabric of the present invention can be composed of only the composite fiber or the composite mixed fiber, but it is preferable to compose the woven or knitted fabric in the form of a mixed yarn, composite false twist yarn, or double-twisted yarn with other yarns, since a more natural worsted texture and a heathered feel can be obtained. In the present invention, the other yarn is not particularly limited as long as it is different from the composite fiber of the present invention, but it is preferable that the other yarn is made of a polyester resin, since it has good crimp and mechanical properties and has excellent dimensional stability against changes in humidity and temperature. Specific examples of polyester resins include polyethylene terephthalate resins whose main repeating unit is ethylene terephthalate, polytrimethylene terephthalate resins whose main repeating unit is trimethylene terephthalate, and polybutylene terephthalate resins whose main repeating unit is butylene terephthalate. The polyethylene terephthalate resins or polybutylene terephthalate resins may contain a small amount (usually less than 30 mol%) of a copolymerization component as necessary.
[0043] In addition, it is preferable that the other yarns combined with the composite fiber of the present invention have a yarn length difference from the composite fiber of the present invention after dyeing processing, since this will result in better swelling. Methods for obtaining the yarn length difference include physically adjusting the supply amount of each fiber during the combination, blending a fiber with a lower shrinkage characteristic than the composite fiber of the present invention, and combining by false twisting. The yarn length difference is preferably 10% or more so that the swelling can be easily felt, and is preferably 30% or less in consideration of the physical properties of the woven or knitted fabric. A specific method for measuring the yarn length difference is as described in the examples.
[0044] Furthermore, the apparent thickness ratio (D thick / D thinIt is more preferable that the thickness ratio of the composite fiber of the present invention and the out-of-phase flecks can be expressed, and the worsted texture becomes more natural, when the thickness ratio is 1.05 to 3.00.
[0045] In the woven or knitted fabric of the present invention, the proportion of the composite fiber and / or composite mixed fiber of the present invention used is preferably 30% by mass or more, more preferably 40% by mass or more, based on the mass of the woven or knitted fabric. In a preferred embodiment, all of the fibers constituting the woven or knitted fabric are made of the composite fiber and / or composite mixed fiber of the present invention.
[0046] The fabric structure of the woven or knitted fabric of the present invention is a woven or knitted fabric. The weave structure is selected from plain weave, twill weave, satin weave, and their variations according to the texture and design. Furthermore, a multi-layer weave structure such as a double weave may be used. The knit structure may be selected according to the desired texture and design, and examples of weft knitting include plain weave, elastic weave, pearl weave, tuck knit, floating knit, lace knit, and their variations, while examples of warp knitting include single Denbigh knit, single Van Dyke knit, single cord knit, Berlin knit, Dangle Denbigh knit, Atlas knit, cord knit, half tricot knit, satin knit, sharkskin knit, and their variations. Among these, in order to have a delicate worsted texture and a deep natural appearance, relatively simple weave structures such as plain weave or its variations, twill weave or its variations, and satin weave are more preferable.
[0047] The clothing of the present invention at least partially contains the composite fiber or composite mixed fiber, or the woven or knitted fabric of the present invention. In this way, the clothing can be made to exhibit the delicate worsted texture, deep natural appearance, and high sensibility that the composite fiber or composite mixed fiber, or the woven or knitted fabric of the present invention possess. The clothing of the present invention includes items in the field of outerwear worn as women's and men's clothing, particularly jackets, suits, bottoms, and parts thereof, such as front and back panels, collars, sleeves, chest pockets, and side pockets.
[0048] In addition, after sewing, the garment of the present invention is preferably subjected to a post-treatment of washing, air blowing, or air suction, which allows fiber debris attached to the cut portions of the fabric and the surface of the fabric to be removed in advance, and further reduces the amount of fiber debris generated during washing, etc.
[0049] In the woven / knitted fabric or clothing of the present invention, fiber waste generated during washing can be evaluated by carrying out a washing test on the woven / knitted fabric or clothing, collecting the fiber waste using a collection bag (filter) attached to the drain hose of the washing machine. If there is any influence of fiber waste from washing performed before the evaluation, the washing machine is washed in advance. There is no particular limitation on the washing method, but for example, there is a method in which the washing is performed according to ISO 6330 (2012) without putting the laundry or detergent in the washing machine, and the washing machine is washed. When washing the washing machine, the rinsing and spin-drying processes are each performed at least once without putting the laundry or detergent in the washing machine. The conditions are set to be the same as the washing conditions to be evaluated.
[0050] In this case, a standard type C washing machine as specified in ISO 6330 (2012) is used. The washing is carried out using the 4N method for the standard type C washing machine as specified in ISO 6330 (2012). The fiber waste discharged from the washing machine drain is collected by attaching a collector to the washing machine's drain hose. In this evaluation, a "nylon screen" NY10-HC (purchased from Fluoro Industries Co., Ltd., catalog value: mesh size 10μm) is used. If it is difficult to obtain a "nylon screen" NY10-HC (manufactured by Fluoro Industries Co., Ltd., catalog value: mesh size 10μm), an equivalent product with a mesh size within the range of 10μm ±2μm is used.
[0051] The method for evaluating the amount of fiber waste generated during the washing of woven or knitted fabrics or clothing is to place one piece of the textile product to be evaluated in a washing machine with the collector attached, and wash using the washing machine and washing conditions described above. However, no detergent or load cloth is used. After washing, the weight of the fiber waste attached to the collector is measured. Note that one piece of textile product means one piece, regardless of shape, size, or weight.
[0052] The fiber waste collected by the collector is suction filtered using a filter whose weight has been measured after it has been completely dried. In this evaluation, a polycarbonate membrane (K040A047A, manufactured by Advantec Toyo Co., Ltd.) is used. The filter and fiber waste after filtration are dried at 105°C for 1 hour and their weights are measured. The difference in weight from the weight before filtration is taken as the amount of fiber waste. The conditions for completely drying and weight measurement are heating at 105°C for 1 hour, followed by temperature and humidity adjustment at 20°C and 65% RH, and then weight measurement.
[0053] The woven / knitted fabrics and clothing of the present invention can achieve a fiber waste amount collected after this test of 150 (mg / textile product) or less, and in a preferred embodiment, 100 (mg / textile product) or less.
[0054] [Method of manufacturing composite fibers and woven and knitted fabrics] Next, an example of a preferred method for producing the composite fiber, the composite mixed fiber, and the woven or knitted fabric of the present invention will be described.
[0055] The composite fiber of the present invention can be produced by winding the discharged thermoplastic resin as an undrawn yarn or a semi-drawn yarn, followed by thick and thin drawing. In particular, the composite fiber obtained by winding the semi-drawn yarn and then drawing it is preferable because the difference in orientation between polyester-based thermoplastic resin A and polyester-based thermoplastic resin B gives the composite fiber excellent stretchability when woven or knitted and dyed, and because polyester resin A is highly oriented, the composite fiber has excellent resistance to embrittlement due to alkali reduction.
[0056] [Spinning process] In the method for producing the composite fiber of the present invention, first, polyester-based thermoplastic resin A and polyester-based thermoplastic resin B are each melted, extruded from a spinneret, and wound up as an undrawn yarn or a semi-drawn yarn at a spinning speed preferably of 1400 m / min to 3800 m / min.
[0057] In the present invention, it is preferable to convert semi-drawn yarn into the composite textured yarn of the present invention, since it is easy to reduce the hysteresis loss to 70% or less. Since semi-drawn yarn has a higher crystallization rate than undrawn yarn, plastic deformation due to load can be suppressed.
[0058] The spinning temperature was determined by the melting points (T mA , T mB ) is preferably +20°C to +50°C. mA , T mB ) +20°C or higher, it is possible to prevent the molten polyester-based thermoplastic resin A and the polyester-based thermoplastic resin B from solidifying and clogging the piping of the spinning machine. mA , T mB )+50° C. or less, thermal degradation of the molten polyester-based thermoplastic resin A and the molten polyester-based thermoplastic resin B can be suppressed.
[0059] The spinneret used in the method for producing the composite fiber of the present invention may have any known internal structure as long as it is capable of spinning with stable quality and operation.
[0060] Here, in the cross section of the conjugated fiber of the present invention, as described above, the polyester-based thermoplastic resin A is completely covered with the polyester-based thermoplastic resin B. By forming the conjugated fiber in such a cross section, it is possible to suppress the bending of the discharge line caused by the difference in flow speed between two types of thermoplastic resins discharged from the spinneret, which is an issue during the production of conjugated fibers.
[0061] In the conjugate fiber of the present invention, the thickness t of the polyester thermoplastic resin B covering the polyester thermoplastic resin A is the minimum value t min The thickness t of the cross section of the composite fiber is 1.00t min ≦t≦1.05t min The perimeter C of the part that satisfies tIt is preferable to precisely control the temperature and the amount of the fiber, and a spinning method using a distribution plate, as exemplified in JP-A-2011-174215, JP-A-2011-208313, and JP-A-2012-136804, is preferably used. By using such a distribution plate, min can be within the ranges described above, and t min The exposure of the polyester thermoplastic resin A that occurs as a result of the excessively small t can be suppressed, and the whitening phenomenon and fuzzing of the woven or knitted fabric can be suppressed. min In the method using such a distribution plate, the cross-sectional form of the single yarn can be controlled by the arrangement of distribution holes in the final distribution plate, which is the most downstream of the multiple distribution plates.
[0062] [Stretching process] Next, the yarn produced through the above spinning process is stretched using a stretching device as exemplified in FIG. 3 at a stretch ratio not exceeding the natural stretch ratio of the yarn to form a stretched yarn. This process makes it possible to obtain a desired thick and thin yarn (thick and thin yarn). For example, a semi-stretched yarn obtained by conjugate spinning at a spinning speed of 2600 m / min is pin-stretched at a stretch ratio of 1.5, a hot pin temperature of 70° C., a set temperature of 150° C., and a yarn speed of 300 m / min to obtain a yarn with an apparent thick-thin ratio of 1.05 to 3.00. It is also preferable to stretch the yarn in a range of the natural stretch ratio from the lower limit×1.2 to the upper limit×0.8. By making the conjugate fiber stretched within the above range, it becomes easy to adjust the ratio (LR2 / LR1) of the thick-thin ratio LR1 of the above-mentioned conjugate fiber to the thick-thin ratio LR2 under a load of 0.11 cN / dtex in the dyeing process described later or the like within the range of the present invention. In cases where the heat shrinkage after the drawing step significantly affects subsequent steps, it is desirable to carry out some kind of heat setting after the drawing step in order to suppress the heat shrinkage. It is also preferable to carry out false twisting by a conventional method at this time. This drawn yarn can also be used as the conjugate fiber of the present invention.
[0063] In addition, the drawn composite fiber may be mixed with other yarns before or after winding to form a composite mixed fiber. The mixing method is not particularly limited, and general methods such as interlace mixing and taslan mixing can be used without any problem, and heat setting, false twist processing, and twisting processing can also be performed after mixing.
[0064] [Woven and knitted fabric formation process] The composite fibers obtained in the drawing process are woven or knitted. In the case of woven fabrics, they are woven using air jet looms, water jet looms, rapier looms, projectile looms, shuttle looms, etc. In the case of knitted fabrics, they are knitted using weft knitting machines such as flat knitting machines, old fashion knitting machines, circular knitting machines, computer jacquard knitting machines, sock knitting machines, and tube knitting machines, and warp knitting machines such as tricot knitting machines, raschel knitting machines, air jet looms, and Milanese knitting machines.
[0065] [Alkaline weight reduction process] Furthermore, the woven or knitted fabric obtained in the above-mentioned woven or knitted fabric forming process is subjected to an alkali weight loss treatment as necessary so that the alkali weight loss rate is 5% or more, more preferably 10 to 15%. This process can make the composite fiber have cracks all over its surface. In addition, a continuous weight loss process is preferable to avoid embrittlement due to selective weight loss.
[0066] [Dyeing process] Furthermore, if necessary, before and / or after the above-mentioned alkali weight reduction process, or simultaneously, conventional scouring, relaxation treatment, intermediate heat setting, dyeing processing, and finishing heat setting may be performed (in the present invention, these processes may be collectively referred to as the "dyeing process"). In order to obtain the ratio (LR2 / LR1) of the thickness-thinness ratio LR1 of the composite fiber to the thickness-thinness ratio LR2 at a load of 0.11 cN / dtex, which is a preferred embodiment of the present invention, the feed and tension of each process are appropriately controlled. For example, in the axial direction of the composite fiber of the present invention, in equipment such as a roll to roll system that can control the feed amount, it is desirable to control the overfeed amount within 10%, and in the case of a batch-type liquid flow dyeing machine, it is desirable to control the liquid amount and flow rate so that excessive tension is not applied to the proceeding method. Dyeing is performed using a disperse dye or a cationic dye in a dyeing solution preferably at 110 to 130°C, depending on the dyeability of the thermoplastic resin constituting the composite fiber or other yarns to be combined. EXAMPLES
[0067] Next, the present invention will be specifically described based on examples. However, the present invention is not limited to these examples. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was performed based on the above-mentioned method.
[0068] [Measurement method] (1) Measurement of weight average molecular weight of thermoplastic resin The gel permeation chromatography (GPC) test machine used was a "TOSO GMHHR-H(S)HT" manufactured by Tosoh Corporation.
[0069] (2) Average fiber diameter D ave Measurement Composite fibers were extracted from the woven and knitted fabrics after dyeing, and the fineness and number of filaments were measured according to JIS L1013 (2010) 8.3.1B and JIS L1013 (2010) 8.4, respectively, and the single-yarn fineness was obtained by dividing the fineness by the number of filaments. The average fiber diameter was calculated from the obtained single-yarn fineness according to the following formula.
[0070]
number
[0071] ρ: Density (g / m 3 ) For polyethylene terephthalate, 1.38 x 10 6 g / m 3 .
[0072] (3) Measurement of fiber diameter D, thickness t of polyester-based thermoplastic resin B covering polyester-based thermoplastic resin A, and fiber circumference C A multifilament made of composite fiber was embedded in an embedding agent such as epoxy resin at 10 consecutive points at 1 cm intervals in the fiber axis direction to prepare a sample, and an image of each sample was taken at a magnification where 10 or more fibers could be observed with a transmission electron microscope (TEM). At this time, metal staining was applied to clarify the contrast of the joint between the polyester thermoplastic resin A and the polyester thermoplastic resin B. The image analysis software "WinROOF2015" manufactured by Mitani Shoji Co., Ltd. was used to measure the fiber diameter D from all single yarns in the observed image, and the perimeter C and the thickness t of the polyester thermoplastic resin B were measured. Ten sets of the obtained fiber diameter D, perimeter C, and thickness t were prepared, and the average was used to determine the fiber diameter D with three significant digits, and the perimeter C and thickness t with two significant digits, which were the fiber diameter D, perimeter C, and thickness t of the present invention.
[0073] (4) Hysteresis loss rate Composite fibers were extracted from the woven and knitted fabrics after the dyeing process (finishing heat setting), and in accordance with the constant speed elongation conditions shown in JISL1013 (2010) 8.5.1 standard time test, the sample was elongated with a Tensilon tensile tester from an initial load of 0.1 cN / dtex to a maximum stress of 0.5 cN / dtex at a tensile speed of 20 cm / min with a sample length of 20 cm, and then returned to the original test length position at the same speed, and a hysteresis curve was drawn with the horizontal axis representing elongation and the vertical axis representing stress. The hysteresis loss was calculated from the area (A1) enclosed by the curve at elongation, the curve at recovery, and the horizontal axis, and the area (A2) enclosed by the curve at elongation, a straight line drawn perpendicular to the horizontal axis from the end point of the curve, and the horizontal axis (axis of elongation) according to the following formula. The hysteresis loss rate was calculated to one decimal place by rounding off the first decimal place. Hysteresis loss (%) = (A1 / A2) × 100.
[0074] (5) Apparent Thickness Ratio (D thick / D thin ) Measurement Composite fibers are removed from the woven or knitted fabric after the dyeing process (finishing heat setting), and both ends of the composite fiber are fixed under a load of 0.11 cN / dtex. In an image of the side of the fixed sample taken at 200x magnification using a digital microscope "VHX2000" manufactured by Keyence Corporation, the diameter of the fiber bundle is measured continuously at 500 points at 1.0 mm intervals in the fiber axis direction. The fiber diameter of the thick part (D thick ) and detailed fiber diameter (D thin ) was determined by defining parts thinner than the average of all measured data as details, and parts thicker than the average of all measured data as thick parts. The boundary between a detail and a thick part was determined as the third point in a row where the thickness was 1.05 times or more thicker than the detail, and the boundary between a thick part and a detail was determined as the third point in a row where the thickness was within 1.05 times the thickness of the detail. The apparent thick / thin ratio was calculated by rounding off three decimal places to two decimal places.
[0075] (6) Fiber thickness along the fiber axis (L thick ) and detail length (L thin ) Measurement A composite fiber is removed from the woven or knitted fabric after the dyeing process (finishing heat setting), and both ends of the composite fiber are fixed under a specified load. In an image of the side of the fixed sample taken at 200x magnification using a digital microscope "VHX2000" manufactured by Keyence Corporation, the diameter of the fiber bundle is continuously measured at 1.0mm intervals, and the thick and thin portions that alternate in the fiber axis direction are continuously measured at 50 points each. After measuring at 50 points, the measurement direction is reversed and the thick and thin portions are continuously measured at 50 points on the same part in the same way, and the average of 100 points each is calculated as L. thick , L thin The distinction between thick and fine parts was made in accordance with (5) above. Measurement results were rounded off to two decimal places.
[0076] (7) Check for the presence and depth of cracks The area identified as the thick part in (5) above was observed using a scanning electron microscope "S-3400N" manufactured by Hitachi, Ltd. The composite fiber was pulled out of the woven or knitted fabric after the final heat setting without applying external force, and the presence or absence of cracks was confirmed. If cracks were present, the side surface in the direction approximately perpendicular to the cracks was observed at a magnification of 2000 times. The deepest depth and length of the crack were measured, and the average value of 10 cracks measured within one composite fiber was taken as the crack depth.
[0077] (8) Yarn length difference A yarn of about 5 cm in length was taken out from the woven / knitted fabric after finishing heat setting in an environment of 20°C and 65 RH% for more than 24 hours, and carefully disassembled into single yarns one by one so as not to stretch the fiber itself. The disassembled single yarn was placed on a scale plate coated with glycerin, and the fiber length was measured under a load of 0.11 cN / dtex. The average length of the single yarn group with relatively short fiber length was La, and the average length of the single yarn group with relatively long fiber length was Lb, and calculated using the following formula. All single yarns that make up the composite blended fiber were classified into one of the single yarn groups according to their fiber length. The test was performed 20 times, and the average value was rounded to one decimal place according to Rule B (rounding method) of JIS Z 8401 (2019). ·Thread length difference (%)={(Lb-La) / La}×100.
[0078] (9) Stretchability of woven and knitted fabrics made from composite fibers and composite blended fibers The elongation in the direction along the composite fiber of the present invention was measured according to JIS L1096 (2010) 8.16.1B. When the composite fiber of the present invention was used in both the warp and weft directions, the elongation in each direction was measured, and the average value was used as the result.
[0079] (10) Evaluation of the texture, worsted feel, and heathered feel of woven and knitted fabrics made from composite fibers and composite blended fibers The woven and knitted fabric samples formed using the composite fiber of the present invention were evaluated by 10 healthy adults (5 men and 5 women) who evaluated the texture of the woven and knitted fabrics (especially the fluffy feel and surface feel) by touch and the worsted texture and flecked feel by visual inspection on a 5-point scale of very good (5 points), good (4 points), average (3 points), not very good (2 points), and poor (1 point). The average values of each examiner were rounded off to the nearest whole number.
[0080] (11) Fiber waste from textile products Using the C-type standard washing machine described in ISO 6330 (2012), the washing machine was rinsed and drained twice without any laundry using the "AQW-V700E 7kg" (manufactured by Aqua Co., Ltd.) according to the ISO 6330 (2012) C4N method. Specifically, the washing course was set to thorough, the water volume was 40L, the washing time was 15 minutes, the washing was performed twice, and the spin-drying time was 7 minutes. The washing water temperature was 40°C, and the rinsing water temperature was room temperature. Next, a collection bag manufactured using "nylon screen NY10-HC" (manufactured by Fluoro Industries Co., Ltd., catalog value: mesh size 10μm) with a mesh size of 11.3μm (actual measurement value) was attached to the drain hose of the washing machine. After that, one textile product to be evaluated was placed in the washing machine and washed under the washing conditions of the ISO 6330 C4N method. However, no detergent or load cloth was used. After washing, the fiber waste attached to the "nylon screen" was filtered by suction using a polycarbonate membrane ("K040A047A" manufactured by Advantec Toyo Co., Ltd.) whose weight had been measured in advance. The polycarbonate membrane and fiber waste after filtration were dried at 105°C for 1 hour and weighed. The difference from the weight before filtration was taken as the amount of fiber waste generated. The weight was calculated by rounding off the third decimal place to two decimal places.
[0081] [Example 1] The polyester thermoplastic resin A was polyethylene terephthalate having a weight average molecular weight of 25,000, and the polyester thermoplastic resin B was polyethylene terephthalate having a weight average molecular weight of 15,000. The resins were fed into a conjugate fiber spinneret having 12 discharge holes so that the spinning temperature was 290° C. and the mass conjugation ratio of the polyester thermoplastic resin A to the polyester thermoplastic resin B was 50:50. In the spinning of this Example 1, the distribution holes in the final distribution plate installed at the most downstream of the multiple distribution plates were arranged as shown in FIG. 4, thereby forming an eccentric core-sheath type (FIG. 1) composite cross section in which the polyester thermoplastic resin A is contained in the polyester thermoplastic resin B, and the mass conjugation ratio of the polyester thermoplastic resin A to the polyester thermoplastic resin B is 50:50. The yarn discharged from the spinneret was cooled by an air-cooling device, oil was applied, and then the yarn was wound up by a winder at a speed of 2600 m / min, and stably wound up as a semi-drawn yarn with a total fineness of 100 dtex and 12 filaments.
[0082] The semi-drawn yarn was then fed to a drawing device at a speed of 300 m / min, and pin-drawn using the drawing device shown in FIG. 3 at a draw ratio of 1.50, a hot pin temperature of 70° C., and a set temperature of 150° C. to obtain an apparent thickness-thinness ratio (D thick / D thin A drawn yarn having a t of 1.40 was obtained. thin / D) is 0.020, C t The relationship between and C is C t =0.40C(C t / C=0.40). A :S B The ratio was 50:50.
[0083] Next, a twist of 1200 T / m was imparted to drawn yarn obtained by a conventional method and used as the warp and weft to produce a 1 / 3 twill fabric with a warp density of 115 threads / 2.54 cm and a weft density of 105 threads / 2.54 cm.
[0084] The fabric was then scoured, intermediate heat set, and alkali weight reduction (weight reduction rate 10%).Then, the fabric was dyed with the disperse dye "Dystar Navy Blue S-GL" at a concentration of 1.0 owf% at 130°C for 30 minutes, and then finished by heat setting at 160°C.The results are shown in Table 1.
[0085] [Example 2] In the stretching process, the stretching ratio in the stretching device is set to 1.30 times, and the apparent thick-thin ratio (D thick / D thin Except for obtaining a drawn yarn with a stretch ratio of 1.25, a composite fiber and a woven fabric were obtained in the same manner as in Example 1. The results are shown in Table 1.
[0086] [Example 3] In the stretching process, the stretching ratio in the stretching device is set to 1.40 times, and the apparent thick-thin ratio (D thick / D thin Except for obtaining a drawn yarn having a viscosity of 1.30, a composite fiber and a woven fabric were obtained in the same manner as in Example 1. The results are shown in Table 1.
[0087] [Comparative Example 1] Conjugated fibers and woven fabrics were obtained in the same manner as in Example 1, except that polyethylene terephthalate having a weight average molecular weight of 15,000 was used as both polyester-based thermoplastic resin A and polyester-based thermoplastic resin B. The results are shown in Table 1.
[0088] [Comparative Example 2] A composite fiber and a woven fabric were obtained in the same manner as in Example 1, except that the spinneret used in Example 1 was replaced from a distributor type spinneret to a type of spinneret described in JP-A-09-157941, and a side-by-side type composite fiber consisting of a polyester-based thermoplastic resin A and a polyester-based thermoplastic resin B was obtained. The obtained woven fabric was of poor quality, and was inferior in texture, combed texture, and heathered feel. The results are shown in Table 1.
[0089] [Comparative Example 3] In Example 1, the minimum value t of the thickness t of the polyester thermoplastic resin B covering the polyester thermoplastic resin A minThe arrangement of the distribution holes of the final distribution plate of the spinneret used was changed from that shown in FIG. 4 to that shown in FIG. 5 so that the value of (t min Except for using sheath-core composite fibers having a fiber length of 0.20, composite fibers and woven fabrics were obtained in the same manner as in Example 1. The results are shown in Table 1.
[0090] [Comparative Example 4] In the stretching process, the stretching ratio in the stretching device is set to 1.90 times, and the apparent thick-thin ratio (D thick / D thin A composite fiber and a woven fabric were obtained in the same manner as in Example 1, except that a drawn yarn with a fiber diameter of 1.00 (i.e., a yarn having neither bulging parts (thick parts) of the composite fibers nor bundled parts (fine parts) of the composite fibers and having a uniform fiber diameter) was obtained. The results are shown in Table 1.
[0091] [Example 4] The drawn yarn produced in Example 1 was further subjected to an apparent thickness ratio (D thick / D thin A woven fabric was obtained in the same manner as in Example 1, except that polyethylene terephthalate fiber (74 dtex-48 f) having a density of 1.15 was interlaced and mixed with an interlace nozzle to a concentration of 42 mass% to form a composite mixed fiber, and the warp density was 82 threads / inch and the weft density was 75 threads / inch. The results are shown in Table 1.
[0092] [Example 5] A composite fiber was produced in the same manner as in Example 1, except that the spinning speed was set to 1400 m / min and undrawn yarn was used. However, partial fusion occurred during the drawing setting process, so the setting temperature was changed to 120°C to obtain a composite fiber and woven fabric without fusion. The obtained woven fabric had a low elongation rate, but was excellent in texture and worsted feel. The results are shown in Table 1.
[0093] [Example 6] A composite fiber and a woven fabric were obtained in the same manner as in claim 1, except that a polyester having a weight average molecular weight of 20,000 was used in which 10 mol % of isophthalic acid (IPA) was copolymerized with respect to the acid component as the polyester-based thermoplastic resin A. The results are shown in Table 1.
[0094] [Table 1] [Explanation of symbols]
[0095] 1: Polyester thermoplastic resin A 2: Polyester-based thermoplastic resin B 3: Composite fiber 4: Crack 5: Semi-oriented yarn 6: Guide 7: First feed roller 8: Hot Pin 9: Second feed roller 10:Heater 11: 3rd feed roller 12: Composite fiber with thick-thin ratio 13: Winding section 14: Among the distribution holes in the final distribution plate, a distribution hole of polyester-based thermoplastic resin A 15: Among the distribution holes in the final distribution plate, a distribution hole for polyester-based thermoplastic resin B 16: Thickness t of polyester thermoplastic resin B covering polyester thermoplastic resin A
Claims
1. A composite fiber containing a polyester-based thermoplastic resin A and a polyester-based thermoplastic resin B, and satisfying the following requirements. (1) Weight average molecular weight M of the polyester thermoplastic resin A A and the weight average molecular weight M of the polyester thermoplastic resin B B Difference from (M A -M B ) is between 2,000 and 15,000. (2) In the composite fiber, the apparent thickness-thinness ratio (D thick / D thin ) is 1.05 to 3.
00. (3) In the cross section of the composite fiber, the polyester-based thermoplastic resin B covers the polyester-based thermoplastic resin A, and the minimum value t of the thickness t of the polyester-based thermoplastic resin B is min and the fiber diameter D of the composite fiber (t min / D) is 0.01 to 0.
10. (4) In the cross section of the composite fiber, the thickness t is 1.00t min ≦t≦1.05t min The perimeter C of the part that satisfies t With respect to the perimeter C of the entire composite fiber, t ≧0.33C.
2. The conjugate fiber according to claim 1, wherein the conjugate fiber has a hysteresis loss rate during elongation recovery at a maximum load of 0.5 cN / dtex of 0 to 70%.
3. 3. The composite fiber according to claim 1, wherein a thickness-thinness ratio LR1 (L2 / L1) of a thick length (L1) to a thin length (L2) in the fiber axis direction at a measurement load of 0.00166 cN / dtex is 0.90 to 1.40, and a ratio (LR2 / LR1) of a thickness-thinness ratio LR2 at a measurement load of 0.11 cN / dtex to a thickness-thinness ratio LR1 at a measurement load of 0.00166 cN / dtex is 1.20 to 2.
10.
4. At least the apparent thickness of the composite fiber is a thick fiber diameter (D thick 4. The composite fiber according to claim 1, wherein the composite fiber has a surface having cracks in a portion having the above-mentioned cross-sectional area.
5. A composite mixed fiber in which the composite fiber according to any one of claims 1 to 4 is further mixed with at least one other type of yarn.
6. A woven or knitted fabric comprising at least a part of the conjugate fiber according to any one of claims 1 to 4.
7. A woven or knitted fabric comprising at least a part of the composite mixed fiber according to claim 5.
8. A garment comprising at least a portion of the composite fiber according to any one of claims 1 to 4.
9. A garment comprising at least a portion of the composite mixed fiber according to claim 5.
10. A garment comprising at least a part of the woven or knitted fabric according to claim 6 or 7.
Citation Information
Patent Citations
Uneven yarn
JP1997228181A
Polyester thick and thin multifilament yarn, method for producing the same and woven knitted product
JP2003239153A
Worsted-like cloth and method for producing the same
JP2003328248A
Latently crimpable polyester conjugate fiber
JP2004218156A
Polyester conjugate filament thick-fine yarn fabric and method for production thereof
WO2003093547A1