Ultrahigh-temperature dust collection bag material and preparation method thereof
Through the preparation method of modified polyphenylene sulfide, modified nanomontmorillonite grafting and melt spinning treatment, the problem of oxidation of polyphenylene sulfide fibers in high temperature environment is solved, and the toughness and thermal stability of the material are improved. , suitable for high-temperature flue gas filtration, extending service life.
Patent Information
- Application Number
- CN202411350491.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The existing polyphenylene sulfide fibers are prone to oxidation in high-temperature environments, resulting in thermal strength loss, shortening service life, and cannot meet the strength requirements of high-temperature flue gas filter materials.
Through the preparation method of modified polyphenylene sulfide, nanomontmorillonium was organically treated with γ-aminopropyltriethoxysilane, and was combined with phenylagenic anhydride and 4,4'-diaminodiphenylsulfide. The ether reaction forms modified nanomontmorillonium, grafted onto the polyphenylene sulfide molecular chain, improves its toughness and thermal stability, and forms an ultra-high temperature dust removal bag material through melt spinning and stretching treatment.
It significantly improves the high-temperature toughness and mechanical properties of polyphenylene sulfide, extends the service life, enhances the thermal stability and chemical corrosion resistance of the material, and is suitable for high-temperature flue gas filtration.
Smart Images

Figure BDA0005062218960000111 
Figure BDA0005062218960000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filter materials, and in particular to an ultra-high temperature dust removal bag material and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the enhancement of people's environmental awareness, the prevention and control of air pollution, especially the filtration of high-temperature smoke from industries such as waste incineration, metallurgy, and steel, has received more attention. The industrial exhaust gas emitted by industries such as thermal power generation, steel, and waste incineration is not only high in temperature, but also contains a variety of corrosive oxidizing gases such as SO X 、NO X , HCl, dioxanes, etc., general chemical fiber filter media have poor filtering effects and short service life. Polyphenylene sulfide, the full name of polyphenylene sulfide (PPS for short), is a highly crystalline aromatic sulfur polymer. PPS is a rigid main chain formed by alternating benzene rings and sulfur atoms. The large number of benzene rings on the main chain gives the PPS macromolecule good rigidity, and the sulfur atoms make the PPS macromolecule have a certain flexibility. The presence of large π bonds in the structure makes the performance of PPS very stable. The limiting oxygen index of PPS is greater than 43, and its combustion performance reaches UL94V-1 level. It has good thermal stability, excellent chemical corrosion resistance and electrical insulation. PPS has become one of the preferred filter materials for high-temperature flue gas and special heat medium filtration such as flue gas dust removal in coal-fired power plants and exhaust gas filtration in urban waste incineration plants.
[0003] Although PPS fiber is currently recognized as the most suitable material for dust removal bags, from the inherent physical properties of PPS, and due to the presence of sulfur bonds on the PPS macromolecular chain, the sulfur in the molecular structure exists in a divalent state. Due to the instability of sulfur's outermost electrons, it has multiple valences and is easy to lose electrons and combine with oxygen. This makes PPS fiber prone to oxidation in a high-temperature environment with a high oxygen content, causing a serious loss of thermal strength, resulting in degradation due to oxidation and breakage of macromolecules, greatly reducing the overall performance of the material. When polyphenylene sulfide fiber is used as high-temperature flue gas filter material in power plants, steel mills, etc., the high-temperature flue gas contains 7-8% oxygen, and the maximum oxygen content reaches 14%. The temperature of the high-temperature flue gas is generally 160-180°C, and may reach more than 200°C instantly. In such a long-term strong oxidizing atmosphere, polyphenylene sulfide undergoes sulfur bond oxidation, and the filter material ages; the fiber strength is reduced, and its products are more brittle, less tough, and lack rigidity and strength. They cannot meet the requirements for strength loss in the exhaust gas treatment process of power plants, cement plants, waste incineration plants and other enterprises, and the service life of the filter bag is significantly shortened, thereby reducing the scope of use and service life of the dust bag. Summary of the invention
[0004] The purpose of the present invention is to provide an ultra-high temperature dust removal bag material and a preparation method thereof to solve the following technical problems:
[0005] Due to the inherent physical properties of existing PPS fibers, the mechanical properties and high temperature resistance under oxygen-containing conditions of the material are poor, which greatly reduces the service life of the material.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing an ultra-high temperature dust removal bag material comprises the following steps:
[0008] A1: extruding and granulating the modified polyphenylene sulfide through a twin-screw extruder to obtain a masterbatch;
[0009] A2: Melt spinning, stretching and heat setting the masterbatch to obtain ultra-high temperature dust removal bag material;
[0010] The preparation method of modified polyphenylene sulfide comprises the following steps:
[0011] S1: In a nitrogen atmosphere, polyphenylene sulfide and dichloromethane are added to a reaction kettle, and the reaction is allowed to stand at room temperature for 12-18 hours, and the temperature is controlled at 0-5°C. Anhydrous aluminum chloride and acetyl chloride are added, and the reaction is allowed to react at room temperature for 1-3 hours, and the temperature is controlled at 35-45°C, and the reaction is kept warm for 2-4 hours. An icy hydrochloric acid solution is added to terminate the reaction, and the reaction is performed by suction filtration, washing with a sodium hydroxide solution, washing with water, washing with ethanol, and drying to obtain component 1;
[0012] S2: Add component 1 and anhydrous toluene into a reaction kettle and disperse them evenly, add modified nano-montmorillonite, acetic acid and 4A molecular sieve, control the temperature at 90-100°C, keep the reaction for 9-15h, filter, wash, extract with ethanol Soxhlet and dry to obtain component 2;
[0013] S3: Add component 2 and deionized water into the reaction kettle and disperse them evenly, control the temperature at 90-100°C, adjust the pH to 4-5, add dibutyltin dilaurate, keep the reaction warm for 12-24 hours, filter and dry to obtain modified polyphenylene sulfide.
[0014] As a further solution of the present invention: polyphenylene sulfide is pretreated before preparing modified polyphenylene sulfide: polyphenylene sulfide is dried in a vacuum drum dryer at 140°C and a vacuum degree of -0.08 to -0.085 MPa to control the water content of PPS to below 28 ppm.
[0015] As a further solution of the present invention: the hydrochloric acid ice water solution in S1 is obtained by mixing hydrochloric acid and ice water in a volume ratio of 1:1; the addition ratio of polyphenylene sulfide, dichloromethane, anhydrous aluminum chloride, acetyl chloride, and hydrochloric acid ice water solution is 10g: 50-100mL: 15-18g: 5-10mL: 50-100mL.
[0016] As a further solution of the present invention: the addition ratio of component 1, anhydrous toluene, modified nano-montmorillonite, acetic acid, and 4A molecular sieve in S2 is 10g:150-200mL:0.8-1.5g:1-2mL:3-5g.
[0017] As a further solution of the present invention: the addition ratio of component 2, deionized water and dibutyltin dilaurate in S3 is 10g: 100-200g: 1-5g.
[0018] As a further solution of the present invention: the preparation method of modified nano-montmorillonite comprises the following steps:
[0019] B1: Add methanol, distilled water and γ-aminopropyltriethoxysilane to a reaction bottle and disperse them evenly, add glacial acetic acid to adjust the pH to 4-5, control the temperature to 50-60°C, keep warm for 1-3h under stirring, add nano-montmorillonite, control the temperature to 70-80°C, keep warm for 1-3h under stirring, wash with water and dry to obtain organic montmorillonite;
[0020] B2: Add the organic montmorillonite, pyromellitic anhydride and N,N-dimethylformamide into the reaction kettle and disperse them evenly, control the temperature at 45-55°C, keep the temperature and stir for 3-6 hours, filter and dry to obtain the anhydride montmorillonite;
[0021] B3: In a nitrogen atmosphere, 4,4'-diaminodiphenyl sulfide and N,N-dimethylformamide were added into a reaction kettle and dispersed evenly, and anhydride-treated montmorillonite was added. The mixture was reacted at room temperature for 3-6 hours, filtered, washed with water, and dried to obtain modified nano-montmorillonite.
[0022] As a further solution of the present invention: the addition ratio of methanol, distilled water, γ-aminopropyltriethoxysilane and nano-montmorillonite in B1 is 20-40 mL: 80-160 mL: 4-6 g: 10 g.
[0023] As a further solution of the present invention: the addition ratio of the organized montmorillonite, pyromellitic anhydride and N,N-dimethylformamide in B2 is 10 g: 20-50 g: 100-200 mL.
[0024] As a further embodiment of the present invention: in B3, the addition ratio of 4,4'-diaminodiphenyl sulfide, N,N-dimethylformamide and anhydride-treated montmorillonite is 4.5-7.5 g: 100-200 mL: 10 g.
[0025] As a further solution of the present invention: in A1, the melt temperature during extrusion by the twin-screw extruder is 300-310°C and the screw speed is 180-210rpm; in A2, the spinning speed of the melt spinning is 500-600m / min; in A2, the stretching multiple is 3-4.5 and the stretching temperature is 75-105°C during the stretching process; and in A2, the heat setting temperature is 185-210°C.
[0026] An ultra-high temperature dust removal bag material, made by any one of the above preparation methods.
[0027] Beneficial effects of the present invention:
[0028] (1) The present invention firstly uses γ-aminopropyltriethoxysilane to carry out organic treatment on nano-montmorillonite, and the Si element in the silane coupling agent effectively increases the Si element in the montmorillonite, thereby improving the thermal stability of the montmorillonite; and the montmorillonite modified by the organic silane coupling agent with active groups not only improves the lipophilicity of the material, but also increases the reaction activity of the material; the present invention continues to use the anhydride group on one side of the pyromellitic anhydride to open the ring and react with the amino group between the organic montmorillonite layers, so that the anhydride groups are indirectly branched in the montmorillonite layers, which not only effectively increases the spacing between the montmorillonite, but also makes the surface of the material rougher, thereby improving its subsequent composite with polyphenylene sulfide; finally, the present invention uses the anhydride groups in the anhydride montmorillonite to react with 4,4'-diaminodiphenyl sulfide to obtain modified nano-montmorillonite; the modified nano-montmorillonite prepared in the present invention is indirectly branched with carboxyl groups, amino groups, thioether groups and organic silicon molecular chains in the montmorillonite layers.
[0029] The present application utilizes anhydrous aluminum trichloride as a Lewis acid to complex with acetyl chloride to provide acyl cations, which attack the benzene ring to cause a Friede-Crafts reaction, connect the ketone carbonyl group to the benzene ring of polyphenylene sulfide, and the generated aromatic ketone is complexed with aluminum chloride and released in ice-water decomposition to obtain component one; the present application grafts and dopes the amino groups between modified nano-montmorillonite layers onto the polyphenylene sulfide molecular chain through chemical reaction, thereby effectively solving the problem of shortened life of polyphenylene sulfide filter material due to aerodynamic damage and mechanical damage during use, and effectively improving the toughness and strength of polyphenylene sulfide at high temperatures.
[0030] The modified nano-montmorillonite grafted on the polyphenylene sulfide molecular chain of the present application introduces a stable and flexible SiO chain on the polyphenylene sulfide molecular chain, which is beneficial to the improvement of the toughness of the polymer matrix on the one hand; and after the grafting modification, the polarity of the polymer surface is increased, which is beneficial to the composite with some reinforcing phases with similar polarity or with coupling groups, solving the problem of compatibility between the two phases; on the other hand, the modified montmorillonite prepared in the present application is uniformly dispersed on the polyphenylene sulfide molecular chain, and when subjected to axial tensile force, the polyphenylene sulfide produces slippage and thus increases toughness.
[0031] The present invention improves the crystal morphology of polyphenylene sulfide, improves the strength of the material, improves the spinnability of the polymer, increases the crystallization rate and crystallinity, and improves the fiber axial orientation of the polyphenylene sulfide macromolecules; the sulfide structure grafted on the modified montmorillonite prepared in the present invention has the effect of a chain terminator for the polyphenylene sulfide macromolecules and also has the effect of a hydrogen peroxide decomposer; the montmorillonite can prevent oxygen from penetrating, and the barrier effect of the montmorillonite can prevent some low-molecular degradation products from escaping from the system, thereby delaying the progress of thermal oxidative degradation and effectively improving the thermal oxidation resistance of the polyphenylene sulfide.
[0032] (2) The present application subjects the linear fiber-grade modified polyphenylene sulfide resin after melt spinning to stretching and heat setting treatment. The stretching treatment causes the macromolecular chains to be arranged in an orderly manner. This ordered arrangement effect causes the modified montmorillonite to be grafted with polyphenylene sulfide through the molecular chains and to be oriented along the axial direction of the fiber, thereby promoting the improvement of the fiber's crystal structure and making the fiber more stable. Moreover, under the action of stretching and heat setting, more crystal nuclei are generated in the fiber system, and the crystal nuclei form a physically cross-linked network structure with each other, thereby increasing the density of the primary fiber and the degree of crystallinity, so that the fiber has excellent mechanical properties, excellent thermal stability, flame retardancy and chemical corrosion resistance. DETAILED DESCRIPTION
[0033] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Embodiment 1 The preparation method of modified nano-montmorillonite comprises the following steps:
[0035] B1: Add 20 mL of methanol, 80 mL of distilled water, and 4 g of γ-aminopropyltriethoxysilane into a reaction bottle and disperse them evenly. Add glacial acetic acid to adjust the pH to 4. Control the temperature to 50°C and keep it warm for 1 h under stirring. Add 10 g of nano-montmorillonite and control the temperature to 70°C. Keep it warm for 1 h under stirring. Wash with water and dry to obtain organic montmorillonite.
[0036] B2: 10 g of organic montmorillonite, 20 g of pyromellitic anhydride, and 100 mL of N,N-dimethylformamide were added into a reaction kettle and dispersed evenly. The temperature was controlled at 45°C, stirred for 3 h, filtered, and dried to obtain anhydride montmorillonite.
[0037] B3: In a nitrogen atmosphere, 4.5 g of 4,4'-diaminodiphenyl sulfide and 100 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly. 10 g of anhydride montmorillonite was added and reacted at room temperature for 3 h. The mixture was filtered, washed with water, and dried to obtain modified nano-montmorillonite.
[0038] Embodiment 2 The preparation method of modified nano-montmorillonite comprises the following steps:
[0039] B1: Add 30 mL of methanol, 120 mL of distilled water, and 5 g of γ-aminopropyltriethoxysilane into a reaction bottle and disperse them evenly. Add glacial acetic acid to adjust the pH to 4, control the temperature to 55°C, and keep the temperature under stirring for 2 h. Add 10 g of nano-montmorillonite, control the temperature to 75°C, and keep the temperature under stirring for 2 h. Wash with water and dry to obtain organic montmorillonite.
[0040] B2: 10 g of organic montmorillonite, 35 g of pyromellitic anhydride, and 150 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly. The temperature was controlled at 50°C, stirred for 4.5 hours, filtered, and dried to obtain anhydride montmorillonite.
[0041] B3: In a nitrogen atmosphere, 6 g of 4,4'-diaminodiphenyl sulfide and 150 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly. 10 g of anhydride montmorillonite was added and reacted at room temperature for 4.5 h. The mixture was filtered, washed with water, and dried to obtain modified nano-montmorillonite.
[0042] Example 3 The preparation method of modified nano-montmorillonite comprises the following steps:
[0043] B1: Add 40 mL of methanol, 160 mL of distilled water, and 6 g of γ-aminopropyltriethoxysilane into a reaction bottle and disperse them evenly. Add glacial acetic acid to adjust the pH to 5, control the temperature to 60°C, and keep the temperature for 3 h under stirring. Add 10 g of nano-montmorillonite, control the temperature to 80°C, and keep the temperature for 3 h under stirring. Wash with water and dry to obtain organic montmorillonite.
[0044] B2: 10 g of organic montmorillonite, 50 g of pyromellitic anhydride, and 200 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly. The temperature was controlled at 55°C, stirred for 6 hours, filtered, and dried to obtain anhydride montmorillonite.
[0045] B3: In a nitrogen atmosphere, 7.5 g of 4,4'-diaminodiphenyl sulfide and 200 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly. 10 g of anhydride montmorillonite was added and reacted at room temperature for 6 h. The mixture was filtered, washed with water, and dried to obtain modified nano-montmorillonite.
[0046] Embodiment 4 The preparation method of modified polyphenylene sulfide comprises the following steps:
[0047] S1: drying polyphenylene sulfide in a vacuum drum dryer at 140° C. and a vacuum degree of -0.08 MPa for 14 h to obtain pretreated polyphenylene sulfide;
[0048] S2: In a nitrogen atmosphere, 10 g of pretreated polyphenylene sulfide (Fortron fiber-type polyphenylene sulfide produced by Japan Polyplastics Group, Tm = 285°C) and 50 mL of dichloromethane were added to a reactor, and allowed to stand at room temperature for 12 h. The temperature was controlled at 0°C, 15 g of anhydrous aluminum chloride and 5 mL of acetyl chloride were added, and the reaction was carried out at room temperature for 1 h. The temperature was controlled at 35°C and the reaction was kept warm for 2 h. 50 mL of hydrochloric acid and 50 mL of ice water were mixed and added to the reactor to stop the reaction. The mixture was filtered, washed with 5% sodium hydroxide aqueous solution, washed with water, washed with ethanol, and dried to obtain component 1;
[0049] S3: 10 g of component 1 and 150 mL of anhydrous toluene were added to a reaction kettle and dispersed evenly, 0.8 g of the modified nano-montmorillonite prepared in Example 1 was added, 1 mL of acetic acid and 3 g of 4A molecular sieve were added, the temperature was controlled at 90° C., the reaction was kept warm for 9 h, and the mixture was filtered, washed, extracted with ethanol Soxhlet, and dried to obtain component 2;
[0050] S4: Add 10g of component 2 and 100g of deionized water into a reactor and disperse them evenly. Control the temperature at 90°C. Add 1mol / L hydrochloric acid aqueous solution to adjust the pH to 4. Add 2g of dibutyltin dilaurate. Keep the temperature for 18h. Filter and dry to obtain modified polyphenylene sulfide.
[0051] Embodiment 5 The preparation method of modified polyphenylene sulfide comprises the following steps:
[0052] S1: drying polyphenylene sulfide in a vacuum drum dryer at 140° C. and a vacuum degree of -0.08 MPa for 14 h to obtain pretreated polyphenylene sulfide;
[0053] S2: In a nitrogen atmosphere, 10 g of pretreated polyphenylene sulfide (Fortron fiber-type polyphenylene sulfide produced by Japan Polyplastics Group, Tm = 285°C) and 70 mL of dichloromethane were added to a reactor, and allowed to stand at room temperature for 15 h. The temperature was controlled at 0°C, 15 g of anhydrous aluminum chloride and 7 mL of acetyl chloride were added, and the reaction was carried out at room temperature for 2 h. The temperature was controlled at 40°C and the reaction was kept warm for 3 h. 50 mL of hydrochloric acid and 50 mL of ice water were mixed and added to the reactor to stop the reaction. The mixture was filtered, washed with 5% sodium hydroxide aqueous solution, washed with water, washed with ethanol, and dried to obtain component 1;
[0054] S3: 10 g of component 1 and 200 mL of anhydrous toluene were added to a reaction kettle and dispersed evenly, 1.2 g of the modified nano-montmorillonite prepared in Example 2 was added, 1.5 mL of acetic acid and 4 g of 4A molecular sieve were added, the temperature was controlled at 95° C., the reaction was kept warm for 12 h, and the mixture was filtered, washed, extracted with ethanol Soxhlet, and dried to obtain component 2;
[0055] S4: Add 10g of component 2 and 100g of deionized water into a reactor and disperse them evenly. Control the temperature at 90°C. Add 1mol / L hydrochloric acid aqueous solution to adjust the pH to 4. Add 2g of dibutyltin dilaurate. Keep the temperature for 18h. Filter and dry to obtain modified polyphenylene sulfide.
[0056] Embodiment 6 The preparation method of modified polyphenylene sulfide comprises the following steps:
[0057] S1: drying polyphenylene sulfide in a vacuum drum dryer at 140° C. and a vacuum degree of -0.08 MPa for 14 h to obtain pretreated polyphenylene sulfide;
[0058] S2: In a nitrogen atmosphere, 10 g of pretreated polyphenylene sulfide (Fortron fiber-type polyphenylene sulfide produced by Japan Polyplastics Group, Tm = 285 ° C) and 100 mL of dichloromethane were added to a reactor, and allowed to stand at room temperature for 18 h. The temperature was controlled at 5 ° C. 18 g of anhydrous aluminum chloride and 10 mL of acetyl chloride were added, and the reaction was carried out at room temperature for 3 h. The temperature was controlled at 45 ° C. The reaction was kept warm for 4 h. 50 mL of hydrochloric acid and 50 mL of ice water were mixed and added to the reactor to stop the reaction. The mixture was filtered, washed with 5% sodium hydroxide aqueous solution, washed with water, washed with ethanol, and dried to obtain component 1;
[0059] S3: 10 g of component 1 and 200 mL of anhydrous toluene were added to a reaction kettle and dispersed evenly, 1.5 g of the modified nano-montmorillonite prepared in Example 3 was added, 2 mL of acetic acid and 5 g of 4A molecular sieve were added, the temperature was controlled at 100° C., the reaction was kept warm for 15 h, and the mixture was filtered, washed, extracted with ethanol Soxhlet, and dried to obtain component 2;
[0060] S4: Add 10g of component 2 and 100g of deionized water into a reactor and disperse them evenly. Control the temperature at 90°C. Add 1mol / L hydrochloric acid aqueous solution to adjust the pH to 4. Add 2g of dibutyltin dilaurate. Keep the temperature for 18h. Filter and dry to obtain modified polyphenylene sulfide.
[0061] Embodiment 7 A method for preparing an ultra-high temperature dust removal bag material comprises the following steps:
[0062] A1: The modified polyphenylene sulfide prepared in Example 4 was extruded and granulated through a twin-screw extruder, with the melt temperature of the modified polyphenylene sulfide being 300° C. and the screw speed being 180 rpm, to obtain a masterbatch;
[0063] A2: The masterbatch was melt-spun at a spinning speed of 500 m / min, stretched (stretching ratio 3.5, stretching temperature 90°C), and heat-set at 185°C to obtain an ultra-high temperature dust bag material.
[0064] Embodiment 8 A method for preparing an ultra-high temperature dust removal bag material comprises the following steps:
[0065] A1: The modified polyphenylene sulfide prepared in Example 5 was extruded and granulated through a twin-screw extruder, with the melt temperature of the modified polyphenylene sulfide being 300° C. and the screw speed being 180 rpm, to obtain a masterbatch;
[0066] A2: The masterbatch was melt-spun at a spinning speed of 500 m / min, stretched (stretching ratio 3.5, stretching temperature 90°C), and heat-set at 185°C to obtain an ultra-high temperature dust bag material.
[0067] Example 9 A method for preparing an ultra-high temperature dust removal bag material comprises the following steps:
[0068] A1: The modified polyphenylene sulfide prepared in Example 6 was extruded and granulated through a twin-screw extruder, with the melt temperature of the modified polyphenylene sulfide being 300° C. and the screw speed being 180 rpm, to obtain a masterbatch;
[0069] A2: The masterbatch was melt-spun at a spinning speed of 500 m / min, stretched (stretching ratio 3.5, stretching temperature 90°C), and heat-set at 185°C to obtain an ultra-high temperature dust bag material.
[0070] Comparative Example 1 The preparation method of modified nano-montmorillonite comprises the following steps:
[0071] Add 30 mL of methanol, 120 mL of distilled water, and 5 g of γ-aminopropyltriethoxysilane into a reaction bottle and disperse them evenly. Add glacial acetic acid to adjust the pH to 4. Control the temperature to 55°C and keep warm for 2 h under stirring. Add 10 g of nano-montmorillonite. Control the temperature to 75°C and keep warm for 2 h under stirring. Wash with water and dry to obtain modified nano-montmorillonite.
[0072] Comparative Example 2 The preparation method of modified polyphenylene sulfide comprises the following steps:
[0073] S1: drying polyphenylene sulfide in a vacuum drum dryer at 140° C. and a vacuum degree of -0.08 MPa for 14 h to obtain pretreated polyphenylene sulfide;
[0074] S2: In a nitrogen atmosphere, 10 g of pretreated polyphenylene sulfide (Fortron fiber-type polyphenylene sulfide produced by Japan Polyplastics Group, Tm = 285°C) and 70 mL of dichloromethane were added to a reactor, and allowed to stand at room temperature for 15 h. The temperature was controlled at 0°C, 15 g of anhydrous aluminum chloride and 7 mL of acetyl chloride were added, and the reaction was carried out at room temperature for 2 h. The temperature was controlled at 40°C and the reaction was kept warm for 3 h. 50 mL of hydrochloric acid and 50 mL of ice water were mixed and added to the reactor to stop the reaction. The mixture was filtered, washed with 5% sodium hydroxide aqueous solution, washed with water, washed with ethanol, and dried to obtain component 1;
[0075] S3: 10 g of component 1 and 200 mL of anhydrous toluene were added to a reaction kettle and dispersed evenly, 1.2 g of the modified nano-montmorillonite prepared in comparative example 1 was added, 1.5 mL of acetic acid and 4 g of 4A molecular sieve were added, the temperature was controlled at 95° C., the reaction was kept warm for 12 h, and the mixture was filtered, washed, extracted with ethanol Soxhlet, and dried to obtain component 2;
[0076] S4: Add 10g of component 2 and 100g of deionized water into a reactor and disperse them evenly. Control the temperature at 90°C. Add 1mol / L hydrochloric acid aqueous solution to adjust the pH to 4. Add 2g of dibutyltin dilaurate. Keep the temperature for 18h. Filter and dry to obtain modified polyphenylene sulfide.
[0077] Comparative Example 3 The preparation method of modified polyphenylene sulfide comprises the following steps:
[0078] S1: drying polyphenylene sulfide in a vacuum drum dryer at 140° C. and a vacuum degree of -0.08 MPa for 14 h to obtain pretreated polyphenylene sulfide;
[0079] S2: 10 g of pretreated polyphenylene sulfide (Fortron fiber-type polyphenylene sulfide produced by Japan Polyplastics Group, Tm = 285°C) and 200 mL of anhydrous toluene were added to a reaction kettle and dispersed evenly, 1.2 g of the modified nano-montmorillonite prepared in Example 2 was added, 1.5 mL of acetic acid and 4 g of 4A molecular sieve were added, the temperature was controlled at 95°C, the reaction was kept warm for 12 h, and suction was filtered, washed, extracted with ethanol Soxhlet, and dried to obtain component 2;
[0080] S3: Add 10g of component 2 and 100g of deionized water into a reactor and disperse them evenly. Control the temperature at 90°C. Add 1mol / L hydrochloric acid aqueous solution to adjust the pH to 4. Add 2g of dibutyltin dilaurate. Keep the temperature for 18h. Filter and dry to obtain modified polyphenylene sulfide.
[0081] Comparative Example 4 A method for preparing an ultra-high temperature dust removal bag material comprises the following steps:
[0082] A1: The modified polyphenylene sulfide prepared in Comparative Example 2 was extruded and pelletized through a twin-screw extruder, with the melt temperature of the modified polyphenylene sulfide being 300° C. and the screw speed being 180 rpm, to obtain a masterbatch;
[0083] A2: The masterbatch was melt-spun at a spinning speed of 500 m / min, stretched (stretching ratio 3.5, stretching temperature 90°C), and heat-set at 185°C to obtain an ultra-high temperature dust bag material.
[0084] Comparative Example 5 A method for preparing an ultra-high temperature dust removal bag material comprises the following steps:
[0085] A1: The modified polyphenylene sulfide prepared in Comparative Example 3 was extruded and granulated through a twin-screw extruder, with the melt temperature of the modified polyphenylene sulfide being 300° C. and the screw speed being 180 rpm, to obtain a masterbatch;
[0086] A2: The masterbatch was melt-spun at a spinning speed of 500 m / min, stretched (stretching ratio 3.5, stretching temperature 90°C), and heat-set at 185°C to obtain an ultra-high temperature dust bag material.
[0087] Performance Testing
[0088] (1) Mechanical properties:
[0089] ① Tested according to GB / T 14344-1993 "Test Method for Breaking Strength and Elongation at Break of Synthetic Filament and Textured Filament"; Test conditions: 23°C, 65RH%; Test method: Use GY(B)021 semi-automatic tensile tester to conduct tensile test on filament, with clamping length of 200mm, pre-tension of 0.05cN / dtex, tensile speed of 165mm / min, test breaking strength and breaking elongation, the test results are shown in Table 1;
[0090] ② The modified polyphenylene sulfide fibers prepared in Examples 7-9 and Comparative Examples 4-5 were treated at a constant temperature of 280° C. for 24 h in an air environment, and then the breaking strength and breaking elongation of the materials were tested according to the above steps. The test results are shown in Table 1;
[0091] Table 1: Statistical table of mechanical properties test data of Examples 7-9 and Comparative Examples 4-5
[0092]
[0093]
[0094] It can be seen from Table 1 that the modified polyphenylene sulfide fiber prepared in the present application has good mechanical properties at room temperature; by adding the modified montmorillonite grafted polyphenylene sulfide prepared in the present application, the modified polyphenylene sulfide material still maintains good mechanical properties after being treated in a high temperature environment, so that the modified polyphenylene sulfide fiber prepared in the present application is used as an ultra-high temperature dust bag material in high-temperature flue gas dust removal filter bags and has the advantages of long service life and good filtration effect.
[0095] (2) Thermal oxidation stability: The oxidation induction temperature of the material was measured by differential scanning calorimetry; the specific steps included: 5 mg of the samples prepared in Examples 7-9 and Comparative Examples 3-4 were placed in aluminum crucibles respectively, and the crucibles were placed in a differential scanning calorimeter DSC test chamber produced by Mettler Company, oxygen was purged into the sample at room temperature for 5 min, the heating rate was controlled at 10°C / min and the oxygen rate was 50 mL / min, the temperature was raised from room temperature to 550°C in an oxygen atmosphere, the instrument was cooled to room temperature, and the oxidation induction temperature was calculated by tangent analysis based on the obtained curve. The test results are shown in Table 2;
[0096] (3) Thermal gravimetric performance: A thermal gravimetric analyzer produced by Mettler was used. 10 mg of the samples prepared in Examples 7-9 and Comparative Examples 3-4 were placed in the instrument. The heating rate was controlled at 10° C. / min from room temperature to 600° C. The mass retention rate was calculated. The test results are shown in Table 2.
[0097] Table 2: Statistical table of thermal oxidation stability test performance test data of Examples 7-9 and Comparative Examples 4-5
[0098] Oxidation induction temperature / ℃ Quality retention rate / ℃ Example 7 501 55.3 Example 8 512 56.1 Example 9 509 54.6 Comparative Example 4 464 40.2 Comparative Example 5 478 44.6
[0099] As can be seen from Table 2, the modified montmorillonite prepared in the present application is added to polyphenylene sulfide to prepare modified polyphenylene sulfide, which effectively improves the material's resistance to thermal oxidative decomposition. The thermal oxidative weight loss temperature of the modified polyphenylene sulfide is effectively improved. At 600°C in air, the mass retention rate is as high as 54% or more. The modified polyphenylene sulfide resin has excellent thermal oxidative resistance.
[0100] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for preparing an ultra-high temperature dust removal bag material, characterized in that: The steps include: A1: extruding and granulating the modified polyphenylene sulfide through a twin-screw extruder to obtain a masterbatch; A2: Melt spinning, stretching and heat setting the masterbatch to obtain ultra-high temperature dust removal bag material; The preparation method of the modified polyphenylene sulfide comprises the following steps: S1: In a nitrogen atmosphere, polyphenylene sulfide and dichloromethane are added to a reaction kettle, and the reaction is allowed to stand at room temperature for 12-18 hours, and the temperature is controlled at 0-5°C. Anhydrous aluminum chloride and acetyl chloride are added, and the reaction is allowed to react at room temperature for 1-3 hours, and the temperature is controlled at 35-45°C, and the reaction is kept warm for 2-4 hours. An icy hydrochloric acid solution is added to terminate the reaction, and the reaction is performed by suction filtration, washing with a sodium hydroxide solution, washing with water, washing with ethanol, and drying to obtain component 1; S2: Add component 1 and anhydrous toluene into a reaction kettle and disperse them evenly, add modified nano-montmorillonite, acetic acid and 4A molecular sieve, control the temperature at 90-100°C, keep the reaction for 9-15h, filter, wash, extract with ethanol Soxhlet and dry to obtain component 2; S3: Add component 2 and deionized water into the reaction kettle and disperse them evenly, control the temperature at 90-100°C, adjust the pH to 4-5, add dibutyltin dilaurate, keep the reaction warm for 12-24 hours, filter and dry to obtain modified polyphenylene sulfide.
2. The method for preparing an ultra-high temperature dust removal bag material according to claim 1, characterized in that: The hydrochloric acid ice water solution in S1 is obtained by mixing hydrochloric acid and ice water in a volume ratio of 1:1; the addition ratio of polyphenylene sulfide, dichloromethane, anhydrous aluminum chloride, acetyl chloride, and hydrochloric acid ice water solution is 10g: 50-100mL: 15-18g: 5-10mL: 50-100mL.
3. The method for preparing an ultra-high temperature dust bag material according to claim 1, characterized in that: The addition ratio of component 1, anhydrous toluene, modified nano-montmorillonite, acetic acid, and 4A molecular sieve in S2 is 10g: 150-200mL: 0.8-1.5g: 1-2mL: 3-5g.
4. The method for preparing an ultra-high temperature dust removal bag material according to claim 1, characterized in that: The addition ratio of component 2, deionized water, and dibutyltin dilaurate in S3 is 10g: 100-200g: 1-5g.
5. The method for preparing an ultra-high temperature dust removal bag material according to claim 1, characterized in that: The preparation method of the modified nano-montmorillonite comprises the following steps: B1: Add methanol, distilled water and γ-aminopropyltriethoxysilane to a reaction bottle and disperse them evenly, add glacial acetic acid to adjust the pH to 4-5, control the temperature to 50-60°C, keep warm for 1-3h under stirring, add nano-montmorillonite, control the temperature to 70-80°C, keep warm for 1-3h under stirring, wash with water and dry to obtain organic montmorillonite; B2: Add the organic montmorillonite, pyromellitic anhydride and N,N-dimethylformamide into the reaction kettle and disperse them evenly, control the temperature at 45-55°C, keep the temperature and stir for 3-6 hours, filter and dry to obtain the anhydride montmorillonite; B3: In a nitrogen atmosphere, 4,4'-diaminodiphenyl sulfide and N,N-dimethylformamide were added into a reaction kettle and dispersed evenly, and anhydride-treated montmorillonite was added. The mixture was reacted at room temperature for 3-6 hours, filtered, washed with water, and dried to obtain modified nano-montmorillonite.
6. The method for preparing an ultra-high temperature dust removal bag material according to claim 5, characterized in that: The addition ratio of methanol, distilled water, γ-aminopropyltriethoxysilane and nano-montmorillonite in B1 is 20-40 mL: 80-160 mL: 4-6 g: 10 g.
7. The method for preparing an ultra-high temperature dust bag material according to claim 5, characterized in that: The addition ratio of the organized montmorillonite, pyromellitic anhydride and N,N-dimethylformamide in B2 is 10g:20-50g:100-200mL.
8. The method for preparing an ultra-high temperature dust removal bag material according to claim 5, characterized in that: The addition ratio of 4,4'-diaminodiphenyl sulfide, N,N-dimethylformamide and anhydride-treated montmorillonite in B3 is 4.5-7.5 g: 100-200 mL: 10 g.
9. The method for preparing an ultra-high temperature dust removal bag material according to claim 1, characterized in that: In A1, the melt temperature during extrusion by the twin-screw extruder is 300-310°C and the screw speed is 180-210rpm; in A2, the spinning speed of melt spinning is 500-600m / min; in A2, the stretching multiple is 3-4.5 and the stretching temperature is 75-105°C during the stretching process; in A2, the heat setting temperature is 185-210°C.
10. An ultra-high temperature dust removal bag material, characterized in that: Prepared by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of nano-particle modified polyphenyl thioether filter material
CN101537280A
Organic silicon grafted and modified polyphenylene sulphide material and preparation method thereof
CN102504256A
Preparation method of antioxidant modified polyphenylene sulfide fiber
CN103225124A
Exfoliated polyphenylene sulfide / montmorillonite nanocomposite and preparation method thereof
CN106832931A
Layered nanoparticle-based polyphenylene sulfide anti-oxidation fiber and preparation method thereof
CN108360085A
Cited By
Polyphenylene sulfide fiber pps filter bag
CN119524532A
A polyphenylene sulfide fiber pps filter bag
CN119524532B