Manufacturing method of biaxially oriented polypropylene film

A biaxially oriented polypropylene film with enhanced rigidity and heat resistance is produced through a controlled stretching process, addressing the challenges of maintaining shape and gas barrier properties in thinner films with reduced wrinkles during heat sealing.

JP7571788B2Active Publication Date: 2024-10-23TOYOBO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022531804
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-25
Filing Date
2021-06-14
Publication Date
2024-10-23
Estimated Expiration
2041-06-14

AI Technical Summary

Technical Problem

Existing biaxially oriented polypropylene films face challenges in achieving both high rigidity and heat resistance while maintaining gas barrier properties and minimizing wrinkles during heat sealing, especially when reduced to thinner thicknesses.

Method used

A biaxially oriented polypropylene film production process involving specific polypropylene resin composition and stretching methods, including longitudinal and width direction stretching with controlled temperatures and cooling, to enhance crystallinity and molecular alignment, resulting in a film with high rigidity and heat resistance up to 150°C and reduced heat shrinkage.

Benefits of technology

The film maintains shape and gas barrier properties even at thinner thicknesses, with minimal wrinkles during heat sealing, offering improved rigidity and reduced thermal shrinkage, suitable for packaging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571788000001
    Figure 0007571788000001
  • Figure 0007571788000002
    Figure 0007571788000002
  • Figure 0007571788000003
    Figure 0007571788000003
Patent Text Reader

Abstract

[Problem] To provide a biaxially-oriented polypropylene film that: has high rigidity; easily maintains a bag shape when used as a packaging bag, even if the film is made thin, while at the same time, being able to maintain gas barrier properties at equivalent thickness to conventional films, even if the film is made thin; and, to make the film into packaging, has few wrinkles in a seal part and the periphery thereof when heat sealed. [Solution] A production method for a biaxially-oriented polypropylene film comprises, in order: a step in which an unstretched sheet is obtained by extruding a polypropylene resin composition containing a polypropylene resin having a mesopentad fraction of at least 97.0%; a step in which the unstretched sheet is stretched in the longitudinal direction; a preheating step in which the longitudinally-stretched film is heated at a preheating temperature of Tm to Tm+25°C; a step in which the preheated, longitudinally-stretched film is stretched by a factor of at least 10 in the width direction at a temperature of Tm–10°C to the preheating temperature; a step in which the film is cooled at the width direction stretching temperature or less when the width direction stretching has finished, and at a temperature of Tm–80°C to Tm–15°C; and a step in which heat fixing is carried out while stretching the film by a factor of 1.03 or more in the width direction at a temperature of Tm–5°C to Tm+20°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biaxially oriented polypropylene film having excellent rigidity and heat resistance. More specifically, the present invention relates to a biaxially oriented polypropylene film that is suitable for use as a packaging bag because it is easy to maintain the shape of the bag when made into a packaging bag and has few wrinkles at the sealed portion when heat sealed. [Background technology]

[0002] Biaxially oriented polypropylene films are used for packaging and industrial applications because they have moisture resistance and the necessary rigidity and heat resistance. In recent years, due to environmental considerations, it has been required to maintain strength even when the volume is reduced (thinning the film thickness), and for this purpose, it is essential to significantly improve the rigidity. As a means of improving the rigidity, there have been techniques to improve the crystallinity and melting point of polypropylene resin by improving the catalyst and process technology during polymerization of the polypropylene resin, and to increase the orientation degree of the film by increasing the stretch ratio during the film production process. However, there is a problem that heat resistance decreases at the same time as increasing the rigidity, and there has been no biaxially oriented polypropylene film with sufficient rigidity and heat resistance to date. In addition, when the rigidity is improved to reduce the volume of the film, there is a problem that the water vapor barrier property decreases and the moisture resistance is impaired, which causes food deterioration.

[0003] In the manufacturing process of biaxially oriented polypropylene film, a method has been proposed in which, after stretching in the width direction, the film is subjected to a first-stage heat treatment while relaxing at a temperature equal to or lower than that at the time of width direction stretching, and then a second-stage heat treatment is performed at the first-stage temperature to the width direction stretching temperature (see, for example, Patent Document 1, etc.), and a method in which further stretching in the longitudinal direction is performed after width direction stretching (see, for example, Patent Documents 2 and 3, etc.). However, although the film described in Patent Document 2 has excellent rigidity, it is prone to wrinkles in the sealed portion after heat sealing, and has poor heat resistance. In addition, the orientation of the film described in Patent Document 1 is low and the rigidity is insufficient. The film described in Patent Document 3 is sequentially biaxially stretched, oriented in the width direction, and then re-stretched in the longitudinal direction, so that the molecular chains are not sufficiently aligned in the longitudinal direction, and the rigidity in the longitudinal direction is low. In addition, since relaxation is performed in the width direction, the orientation in the width direction is low and the rigidity is insufficient. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. WO2016 / 182003 [Patent Document 2] JP 2013-177645 A [Patent Document 3] JP 2001-40111 A Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to solve the above-mentioned problems. That is, the present invention relates to a biaxially oriented polypropylene film that has both film rigidity and heat resistance at a high temperature of 150° C. In detail, the object of the present invention is to provide a biaxially oriented polypropylene film that is highly rigid, and that is easy to maintain the bag shape when made into a packaging bag even when the film is thinned, and at the same time, is capable of maintaining the gas barrier property equivalent to that of a conventional thickness even when the film is thinned, and that has few wrinkles at the sealed portion and its surroundings when heat-sealed to make a package. [Means for solving the problem]

[0006] As a result of extensive research by the inventors to achieve this object, they have found that it is possible to obtain a biaxially oriented polypropylene film which is highly rigid, has excellent heat resistance at temperatures as high as 150°C, easily retains its bag shape when made into a packaging bag, and has little pitch misalignment during printing or wrinkles in the sealed area when heat sealed. That is, the present invention is a method for producing a biaxially oriented polypropylene film, which includes, in order, a step of extruding a polypropylene resin composition containing a polypropylene resin having a mesopentad fraction of 97.0% or more to obtain an unstretched sheet, a step of stretching the unstretched sheet in the longitudinal direction, a preheating step of heating the longitudinally stretched film to a preheating temperature in the range of Tm to Tm+25°C, a step of stretching the preheated longitudinally stretched film at a ratio of 10 times or more in the width direction at a temperature of Tm-10°C or more and not exceeding the preheating temperature, a step of cooling the film at a temperature not exceeding the width direction stretching temperature and at a temperature of Tm-80°C or more and not exceeding Tm-15°C upon completion of the width direction stretching, and a step of heat setting while stretching at a ratio of 1.03 times or more in the width direction at Tm-5°C or more and not exceeding Tm+20°C.

[0007] In this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a crystallization temperature of 105° C. or higher and a melting point of 161° C. or higher.

[0008] In this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a melt flow rate of 4.0 g / 10 min or more.

[0009] Furthermore, in this case, it is preferable that the amount of components having a molecular weight of 100,000 or less in the polypropylene resin constituting the biaxially oriented polypropylene film is 35% by mass or more. Effect of the Invention

[0010] The biaxially oriented polypropylene film of the present invention has high rigidity, can be thinned, and can maintain gas barrier properties equivalent to those of conventional thicknesses, and has few wrinkles at the sealed portion and its surroundings when heat-sealed to form a package. Therefore, it can be suitably used for packages, industrial purposes, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The biaxially oriented polypropylene film of the present invention will be described in more detail below. The biaxially oriented polypropylene film of the present invention is made of a polypropylene resin composition containing a polypropylene resin as a main component. Here, "main component" means that the proportion of the polypropylene resin in the polypropylene resin composition is 90% by mass or more, more preferably 93% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more.

[0012] (Polypropylene resin) The polypropylene resin used in the present invention may be a polypropylene homopolymer or a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms. A propylene homopolymer that does not substantially contain ethylene and / or an α-olefin having 4 or more carbon atoms is preferred. Even if it contains ethylene and / or an α-olefin having 4 or more carbon atoms, the amount of ethylene and / or an α-olefin having 4 or more carbon atoms is preferably 1 mol% or less, more preferably 0.5 mol% or less, even more preferably 0.3 mol% or less, and particularly preferably 0.1 mol% or less. When it is within the above range, the crystallinity is likely to be improved. Examples of the α-olefin component having 4 or more carbon atoms that constitutes such a copolymer include 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene. The polypropylene resin may be a homopolymer of two or more different kinds of polypropylene, a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms, or a mixture of these.

[0013] (stereoregularity) The mesopentad fraction ([mmmm]%), which is an index of stereoregularity of the polypropylene resin used in the present invention, is preferably within the range of 97.0 to 99.9%, more preferably within the range of 97.5 to 99.7%, even more preferably within the range of 98.0 to 99.5%, and particularly preferably within the range of 98.5 to 99.3%. If it is 97.0% or more, the crystallinity of the polypropylene resin is increased, and the melting point, crystallinity, and crystal orientation of the crystals in the film are improved, making it easier to obtain rigidity and heat resistance at high temperatures. If it is 99.9% or less, it is easier to reduce costs in terms of polypropylene production, and the film is less likely to break during production. The mesopentad fraction is measured by the nuclear magnetic resonance method (the so-called NMR method). It is more preferable that the mesopentad fraction is 99.5% or less. The mesopentad fraction is measured by a nuclear magnetic resonance method (the so-called NMR method). In order to set the mesopentad fraction of the polypropylene resin within the above-mentioned range, a method of washing the obtained polypropylene resin powder with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or a co-catalyst, and a method of appropriately selecting the components of the polypropylene resin composition are preferably adopted.

[0014] (Melting temperature) The lower limit of the melting temperature (Tm) measured by DSC of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention is preferably 160 ° C, more preferably 161 ° C, even more preferably 162 ° C, even more preferably 163 ° C, and even more preferably 164 ° C. When Tm is 160 ° C or more, rigidity and heat resistance at high temperatures are easily obtained. The upper limit of Tm is preferably 170 ° C, more preferably 169 ° C, even more preferably 168 ° C, even more preferably 167 ° C, and particularly preferably 166 ° C. When Tm is 170 ° C or less, it is easy to suppress the increase in cost in terms of polypropylene production, and it is difficult to break during film formation. The melting temperature can also be further increased by blending a crystal nucleating agent with the above-mentioned polypropylene resin. Tm is the main endothermic peak temperature associated with melting, which is observed when 1 to 10 mg of a sample is packed into an aluminum pan and set in a differential scanning calorimeter (DSC), melted at 230°C for 5 minutes in a nitrogen atmosphere, cooled to 30°C at a scanning rate of -10°C / min, held for 5 minutes, and then heated again at a scanning rate of 10°C / min.

[0015] (crystallization temperature) The lower limit of the crystallization temperature (Tc) measured by DSC of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention is 105 ° C., preferably 108 ° C., and more preferably 110 ° C. If Tc is 105 ° C. or more, crystallization is likely to proceed during the width direction stretching and the subsequent cooling process, and rigidity and heat resistance at high temperatures are likely to be obtained. The upper limit of Tc is preferably 135 ° C., more preferably 133 ° C., even more preferably 132 ° C., even more preferably 130 ° C., particularly preferably 128 ° C., and most preferably 127 ° C. If Tc is 135 ° C. or less, it is difficult to increase the cost in terms of polypropylene production, and it is difficult to break during film formation. The crystallization temperature can also be further increased by blending a crystal nucleating agent with the above-mentioned polypropylene resin. Tc is the main exothermic peak temperature observed when 1 to 10 mg of a sample is packed into an aluminum pan, set in a DSC, melted at 230°C for 5 minutes in a nitrogen atmosphere, and cooled to 30°C at a scanning rate of -10°C / min.

[0016] (Melt Flow Rate) The melt flow rate (MFR) of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention, when measured in accordance with JIS K 7210 (1995) condition M (230°C, 2.16 kgf), is preferably 4.0 g / 10 min or more and 30 g / 10 min or less, more preferably 4.5 g / 10 min or more and 25 g / 10 min or less, even more preferably 4.8 g / 10 min or more and 22 g / 10 min or less, particularly preferably 5.0 g / 10 min or more and 20 g / 10 min or less, and most preferably 6.0 g / 10 min or more and 20 g / 10 min or less. When the melt flow rate (MFR) of the polypropylene resin is 4.0 g / 10 min or more, a biaxially oriented polypropylene film with low thermal shrinkage is easily obtained. Furthermore, when the melt flow rate (MFR) of the polypropylene resin is 30 g / 10 min or less, the film formability is easily maintained.

[0017] From the viewpoint of film properties, the lower limit of the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene resin constituting the film is preferably 5.0 g / 10 min, more preferably 5.5 g / 10 min, even more preferably 6.0 g / 10 min, particularly preferably 6.3 g / 10 min, and most preferably 6.5 g / 10 min. When the melt flow rate (MFR) of the polypropylene resin is 5.0 g / 10 min or more, the amount of low molecular weight components in the polypropylene resin constituting the film is large. Therefore, by adopting a width direction stretching process in the film production process described below, the oriented crystallization of the polypropylene resin is further promoted and the crystallinity of the film is more likely to be increased. In addition, the entanglement of polypropylene molecular chains in the amorphous portion is reduced, making it easier to increase heat resistance. In order to set the melt flow rate (MFR) of the polypropylene resin within the above range, it is preferable to employ a method of controlling the average molecular weight or molecular weight distribution of the polypropylene resin.

[0018] That is, the lower limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve of the polypropylene resin constituting the film of the present invention is 35 mass%, preferably 38 mass%, more preferably 40 mass%, even more preferably 41 mass%, and particularly preferably 42 mass%. The upper limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is preferably 65% ​​by mass, more preferably 60% by mass, and even more preferably 58% by mass. When the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is 65% by mass or less, the film strength is unlikely to decrease. In this case, if the polypropylene resin contains high molecular weight components with long relaxation times or long-chain branched components, the amount of components with a molecular weight of 100,000 or less contained in the polypropylene resin can be easily adjusted without significantly changing the overall viscosity, making it easier to improve film formability without significantly affecting rigidity or thermal shrinkage.

[0019] (molecular weight distribution) The polypropylene resin used in the present invention has a lower limit of mass average molecular weight (Mw) / number average molecular weight (Mn), which is an index of the breadth of molecular weight distribution, of preferably 3.5, more preferably 4, even more preferably 4.5, and particularly preferably 5. The upper limit of Mw / Mn is preferably 30, more preferably 25, even more preferably 23, particularly preferably 21, and most preferably 20. Mw / Mn can be obtained by gel permeation chromatography (GPC). When Mw / Mn is within the above range, it is easy to increase the amount of components having a molecular weight of 100,000 or less.

[0020] The molecular weight distribution of polypropylene resin can be adjusted by polymerizing components of different molecular weights in a series of plants in multiple stages, blending components of different molecular weights offline in a kneader, polymerizing by blending catalysts with different performance, or using a catalyst that can achieve a desired molecular weight distribution. The shape of the molecular weight distribution obtained by GPC may be a gentle molecular weight distribution with a single peak in a GPC chart with the logarithm (logM) of molecular weight (M) on the horizontal axis and the differential distribution value (weight fraction per logM) on the vertical axis, or a molecular weight distribution with multiple peaks or shoulders.

[0021] (Method for producing biaxially oriented polypropylene film) The biaxially oriented polypropylene film of the present invention is preferably obtained by preparing an unstretched sheet made of a polypropylene resin composition mainly composed of the above-mentioned polypropylene resin, and biaxially stretching the sheet. As the method of biaxial stretching, any of the inflation simultaneous biaxial stretching method, the tenter simultaneous biaxial stretching method, and the tenter sequential biaxial stretching method can be used, but it is preferable to adopt the tenter sequential biaxial stretching method from the viewpoint of film formation stability and thickness uniformity. In particular, it is preferable to stretch in the longitudinal direction and then in the width direction, but a method of stretching in the width direction and then in the longitudinal direction may also be used.

[0022] Next, the method for producing the biaxially oriented polypropylene film of the present invention will be described below, but is not necessarily limited thereto. The biaxially oriented polypropylene film of the present invention may have a layer having another function laminated on at least one side. Lamination may be performed on one or both sides. In that case, the resin composition of the other layer or the central layer may be the polypropylene resin composition described above. It may also be different from the polypropylene resin composition described above. The number of layers to be laminated may be one, two, or three or more layers per side, but one or two layers are preferred from the viewpoint of production. As a lamination method, for example, coextrusion by a feed block method or a multi-manifold method is preferred. In particular, for the purpose of improving the processability of the biaxially oriented polypropylene film, a resin layer having heat sealability can be laminated within a range that does not deteriorate the properties. In addition, in order to impart printability, corona treatment can be performed on one or both sides.

[0023] In the following, an example of a single layer will be described in which a tenter sequential biaxial stretching method is adopted. First, a resin composition containing a polypropylene resin is heated and melted in a single-screw or twin-screw extruder, extruded into a sheet from a T-die, and cooled and solidified by being placed on a cooling roll. In order to promote solidification, it is preferable to further cool the sheet cooled by the cooling roll by immersing it in a water tank.

[0024] The sheet is then stretched in the longitudinal direction between two pairs of heated stretching rolls by increasing the rotation speed of the rear stretching roll, to obtain a uniaxially stretched film.

[0025] The uniaxially stretched film is then preheated, and stretched in the width direction at a specific temperature while holding the film ends in a tenter-type stretching machine to obtain a biaxially stretched film. This width direction stretching step will be described in detail later.

[0026] After the width direction stretching step is completed, the biaxially stretched film is heat-treated at a specific temperature to obtain a biaxially oriented film. In the heat treatment step, the film may be relaxed in the width direction.

[0027] The biaxially oriented polypropylene film thus obtained can be subjected to a corona discharge treatment on at least one side, if necessary, and then wound up on a winder to obtain a film roll.

[0028] Each step will be described in detail below. (Extrusion process) First, a polypropylene resin composition mainly composed of polypropylene resin is heated and melted in a range of 200°C to 300°C in a single-screw or twin-screw extruder, and the sheet-shaped molten polypropylene resin composition is extruded from a T-die and cooled and solidified by contacting it with a metal cooling roll. The obtained unstretched sheet is preferably further put into a water tank. The temperature of the cooling roll, or the cooling roll and water bath, is preferably in the range of 10° C. to Tc, and when it is desired to increase the transparency of the film, it is preferable to cool and solidify the film with a cooling roll having a temperature in the range of 10 to 50° C. If the cooling temperature is 50° C. or less, the transparency of the unstretched sheet is likely to increase, and it is preferably 40° C. or less, and more preferably 30° C. or less. In order to increase the degree of crystal orientation after sequential biaxial stretching, it may be preferable to set the cooling temperature to 40° C. or more, but when a propylene homopolymer having a mesopent fraction of 97.0% or more is used as described above, it is preferable to set the cooling temperature to 40° C. or less in order to easily perform the stretching in the next step and to reduce thickness unevenness, and it is more preferable to set the cooling temperature to 30° C. or less. The thickness of the unstretched sheet is preferably 3500 μm or less in terms of cooling efficiency, more preferably 3000 μm or less, and can be appropriately adjusted depending on the film thickness after sequential biaxial stretching. The thickness of the unstretched sheet can be controlled by the extrusion speed of the polypropylene resin composition and the lip width of the T-die, etc.

[0029] (Longitudinal stretching process) The lower limit of the longitudinal stretching ratio is preferably 3.5 times, more preferably 3.8 times, and particularly preferably 4.2 times. Within the above range, strength is easily increased and thickness unevenness is reduced. The upper limit of the longitudinal stretching ratio is preferably 7.0 times, more preferably 6.0 times, and particularly preferably 7 times. When it is within the above range, the width direction stretching in the width direction stretching step is easy, and the productivity is improved. The lower limit of the longitudinal stretching temperature is preferably Tm-30°C, more preferably Tm-27°C, and even more preferably Tm-25°C. Within this range, the subsequent width direction stretching becomes easy and thickness unevenness is reduced. The upper limit of the longitudinal stretching temperature is preferably Tm-7°C, more preferably Tm-10°C, and even more preferably Tm-12°C. Within this range, the heat shrinkage rate is easily reduced, and there is little deterioration in quality due to difficulty in applying the film to the stretching rolls and increasing surface roughness. The longitudinal stretching may be performed in two or more stages using three or more pairs of stretching rolls.

[0030] (Preheating process) Prior to the width direction stretching step, the uniaxially stretched film after the longitudinal stretching is heated in the range of Tm to Tm+25°C to soften the polypropylene resin composition. By setting the temperature at or above Tm, softening proceeds and stretching in the width direction becomes easier. By setting the temperature at or below Tm+25°C, orientation proceeds during transverse stretching and rigidity is easily developed. The temperature is more preferably Tm+2 to Tm+20°C, and particularly preferably Tm+3 to Tm+15°C. Here, the maximum temperature in the preheating step is defined as the preheating temperature.

[0031] (Width direction stretching process) In the transverse stretching step after the preheating step, a preferred method is as follows.

[0032] In the width direction stretching step, stretching is preferably performed at a temperature of Tm-10° C. or more and the preheating temperature or less. In this case, the start of width direction stretching may be when the preheating temperature is reached, or when the temperature is lowered after reaching the preheating temperature to a temperature lower than the preheating temperature. The lower limit of the temperature in the width direction stretching step is more preferably Tm-9° C., further preferably Tm-7° C., and particularly preferably Tm-5° C. When the width direction stretching temperature is within this range, the rigidity of the obtained biaxially oriented film is easily improved. The upper limit of the temperature in the width direction stretching step is preferably Tm+10° C., more preferably Tm+7° C., and particularly preferably Tm+5° C. When the width direction stretching temperature is within this range, stretching unevenness is unlikely to occur. In the transverse stretching step, a later stretching step of stretching at a lower temperature may be added subsequent to the transverse stretching in the above temperature range. That is, a section (early section) in which the film is stretched at a temperature of Tm-10° C. or more and Tm+10° C. or less may be followed by a section (late section) in which the film is stretched at a temperature lower than that of the early section and at Tm-70° C. or more and Tm-5° C. or less. Providing an early section and a late section makes it easier to increase rigidity. The lower limit of the stretching temperature in the latter section is preferably Tm-65° C., more preferably Tm-60° C., and further preferably Tm-55° C. When the stretching temperature in the latter section is within this range, film formation is likely to be stable.

[0033] The lower limit of the final width direction stretching ratio in the width direction stretching step is preferably 9 times, more preferably 10 times. If it is 9 times or more, the rigidity is easily increased and the film thickness unevenness is easily reduced. The upper limit of the width direction stretching ratio is preferably 20 times, more preferably 17 times, and even more preferably 15 times. If it is 20 times or less, the heat shrinkage rate is easily reduced and the film is less likely to break during stretching. When the latter section is added, the total stretching ratio is set to be within the above range. In this case, the lower limit of the stretching ratio in the former stretching step is preferably 4 times, more preferably 5 times, even more preferably 6 times, and particularly preferably 6.5 times. The upper limit of the stretching ratio at the end of the former section is preferably 15 times, more preferably 14 times, and even more preferably 13 times.

[0034] It is preferable to cool the film immediately after the end of the width direction stretching, i.e., when the final width direction stretching ratio is reached. The cooling temperature at this time is preferably a temperature lower than the width direction stretching temperature and a temperature of Tm-80°C or higher and Tm-15°C or lower, more preferably a temperature of Tm-80°C or higher and Tm-20°C or lower, even more preferably a temperature of Tm-80°C or higher and Tm-30°C or lower, and particularly preferably a temperature of Tm-70°C or higher and Tm-35°C or lower. By adding a cooling step, crystallization occurs and the crystal orientation is fixed, and even if the temperature is then raised to a temperature higher than the melting temperature, the orientation history is maintained, and as a result, the crystal orientation in the film can be increased. The temperature can be gradually lowered from the temperature at the end of the transverse stretching to the temperature at the time of cooling, or can be lowered stepwise or in one step. Lowering the temperature stepwise or in one step is preferred because it is easier to increase the crystal orientation in the film.

[0035] After cooling the film, it is preferable to stretch the film again in the width direction at a high temperature. The lower limit of the stretching temperature is Tm-5°C, preferably Tm, more preferably Tm+5°C, even more preferably Tm+7°C, and particularly preferably Tm+9°C. If the temperature is Tm-5°C or higher, it is easy to increase the rigidity and to reduce the heat shrinkage rate. The upper limit of the stretching temperature is preferably Tm+20° C., more preferably Tm+18° C., and further preferably Tm+16° C. When the temperature is Tm+20° C. or lower, the rigidity is easily increased. The lower limit of the re-stretching ratio at high temperature is 1.03 times, preferably 1.05 times, and more preferably 1.10 times. The upper limit of the re-stretching ratio at high temperature is preferably 2, more preferably 1.7, and further preferably 1.5. If the re-stretching ratio is too large, the heat shrinkage rate may become too large, thickness unevenness may occur, or the film may break.

[0036] In other words, it has been found that by stretching the film in the width direction again at a temperature sufficiently higher than the melting point, rather than immediately relaxing the film at a high temperature after stretching in the width direction as in the conventional method, it is possible to reduce the thermal shrinkage rate while further improving the rigidity. That is, in the step after the first width direction stretching, it is preferable to perform stretching at Tm-5° C. or higher. At Tm-5° C. or higher, the mobility of molecular chains is sufficiently high, and the influence of entanglement of molecular chains is easily eliminated by stretching. As a result, the molecular chains are not easily restrained, so that the molecular orientation is not easily disturbed and crystallization proceeds sufficiently. By cooling the film below a crystallizable temperature after stretching it in the width direction at a high temperature, the crystal orientation is fixed, and a high melting point film with a high degree of crystallization and thick crystalline lamellae can be obtained.

[0037] Even in areas other than the crystalline lamellae, there are few molecular chains restrained by entanglement points, and the distortion of molecular orientation is small, so the film is less likely to shrink even when the crystals begin to melt. Furthermore, as the degree of crystallization improves and the crystalline lamellae become thicker, the melting point tends to be higher, and melting is less likely to occur below the melting point. This makes it easier for the thermal shrinkage rate to decrease. As a result, it is possible to reduce the thermal shrinkage while improving the rigidity.

[0038] In the normal film-making process (extrusion - longitudinal stretching - transverse stretching - heat treatment), in order to eliminate distortion caused by transverse stretching performed at a temperature lower than the melting point, the film is exposed to a high temperature above the melting point in the heat treatment process and relaxed by several to several tens of percent, thereby reducing the heat shrinkage rate. By relaxing the film, it is possible to eliminate the difficulty in crystallization due to the molecular chains being restrained, which contributes to reducing the heat shrinkage rate. However, on the other hand, the rigidity is also reduced due to the decrease in the width-direction orientation of the molecular chains generated in the transverse stretching process, making it difficult to achieve both low heat shrinkage and high rigidity. In addition, there is also the problem that the film turns white if the temperature is too high. In the normal film-making process (extrusion - longitudinal stretching - width stretching - heat treatment), if the temperature in the width stretching step is increased to increase the mobility of the molecular chains and stretch the film so as to leave no distortion, the crystals formed by longitudinal stretching will melt and the crystal orientation will decrease. In the method of the present invention, the film is stretched once in the width direction to achieve sufficient width direction orientation, and then the film, which has sufficient tension even if the fixed crystal orientation is melted by cooling, is stretched again at a high temperature of Tm-5°C or more. Therefore, even when stretched again, the film has sufficient tension and there is little concern about thickness unevenness or film breakage. The stretching ratio at high temperatures should be at least 1.03 times sufficient to disentangle and align the molecular chains, and a stretching ratio of 2 times or less is unlikely to cause thickness unevenness.

[0039] In this way, by using a highly crystalline polypropylene resin with high stereoregularity and a high melting point, and employing the above-mentioned longitudinal stretching process, width direction stretching process, cooling process, and high-temperature stretching process, the molecules of the polypropylene resin are aligned to a significantly high degree in the main orientation direction (which corresponds to the width direction in the above-mentioned width direction stretching process), and therefore, the crystals in the obtained biaxially oriented film have strong crystal orientation and are more likely to produce a large number of crystals with a high melting point.

[0040] In addition, by increasing the low molecular weight component of the polypropylene resin, the entanglement of molecular chains is reduced, the crystallinity of the film is easily increased, and the area other than the crystalline lamellae is reduced. In addition, the heat shrinkage stress of the area other than the crystalline lamellae is weakened, which makes it easier to further reduce the heat shrinkage rate. Considering that in the prior art, when either the rigidity or the thermal shrinkage rate is improved, the other property tends to decrease, the present invention can be said to have a revolutionary effect.

[0041] (Heat treatment process) If necessary, the biaxially stretched film can be heat-treated to further reduce the heat shrinkage. The upper limit of the heat treatment temperature is preferably 183°C, more preferably 180°C, and even more preferably 178°C. By keeping the temperature at 183°C or less, the rigidity is unlikely to decrease, the film surface is not too rough, and the film is unlikely to whiten. The lower limit of the heat treatment temperature is preferably Tm-3°C, more preferably Tm-2°C, and particularly preferably Tm. In order to adjust the thermal shrinkage rate, the film may be relaxed (relaxed) in the width direction during heat treatment, but the upper limit of the relaxation rate is preferably 8%, more preferably 5%, and even more preferably 3%. Within the above range, the rigidity is unlikely to decrease and the film thickness fluctuation is likely to be small. When the rigidity is to be further increased, heat treatment may not be performed.

[0042] (cooling process) After stretching in the width direction, it is preferable to cool the film immediately after stretching again in the width direction at a temperature of Tm-5°C or higher, or immediately after the heat treatment step. The cooling temperature at this time is preferably 10°C or higher and 140°C or lower, more preferably 15°C or higher and 135°C or lower, even more preferably 20°C or higher and 130°C or lower, and particularly preferably 20°C or higher and 125°C or lower. By providing a cooling step, the state of the film can be fixed.

[0043] (film thickness) The thickness of the biaxially oriented polypropylene film of the present invention is set according to each application, but in order to obtain the strength of the film, the lower limit of the film thickness is preferably 2 μm, more preferably 3 μm, even more preferably 4 μm, particularly preferably 8 μm, and most preferably 10 μm. When the film thickness is 2 μm or more, the film is easily rigid. The upper limit of the film thickness is preferably 100 μm, more preferably 80 μm, even more preferably 60 μm, particularly preferably 50 μm, and most preferably 40 μm. When the film thickness is 100 μm or less, the cooling rate of the unstretched sheet during the extrusion process is unlikely to be reduced. The biaxially oriented polypropylene film of the present invention is usually produced as a roll having a width of about 2000 to 12000 mm and a length of about 1000 to 50000 m, and wound into a film roll. It is then slit according to the intended use and provided as a slit roll having a width of about 300 to 2000 mm and a length of about 500 to 5000 m. The biaxially oriented polypropylene film of the present invention can be used to obtain a longer film roll.

[0044] (Thickness uniformity) The lower limit of the thickness uniformity of the biaxially oriented polypropylene film of the present invention is preferably 0%, more preferably 0.1%, even more preferably 0.5%, and particularly preferably 1%. The upper limit of the thickness uniformity is preferably 20%, more preferably 17%, even more preferably 15%, particularly preferably 12%, and most preferably 10%. Within the above range, defects are unlikely to occur during post-processing such as coating and printing, and the film is easy to use in applications requiring precision. The measurement method was as follows: A test piece 40 mm wide was cut out from a steady region where the film properties were stable in the length direction of the film, and the film thickness was measured continuously over 20,000 mm using a film feeder manufactured by Micron Measurement Instruments Co., Ltd. (product number: A90172) and a continuous film thickness measuring instrument manufactured by Anritsu Corporation (product name: K-313A wide-range high-sensitivity electronic micrometer), and the thickness uniformity was calculated using the following formula. Thickness uniformity (%) = [(maximum thickness value - minimum thickness value) / average thickness value] x 100

[0045] (Film characteristics) The biaxially oriented polypropylene film of the present invention is characterized by the following properties. Here, the "longitudinal direction" of the biaxially oriented polypropylene film of the present invention is the direction corresponding to the flow direction in the film manufacturing process, and the "width direction" is the direction perpendicular to the flow direction in the film manufacturing process. For polypropylene films whose flow direction in the film manufacturing process is unknown, wide-angle X-rays are incident perpendicularly to the film surface, and the scattering peaks originating from the (110) plane of the α-type crystals are scanned in the circumferential direction, and the direction with the largest diffraction intensity in the obtained diffraction intensity distribution is defined as the "longitudinal direction" and the direction perpendicular to that is defined as the "width direction."

[0046] It is preferable that the heat shrinkage rate (%) in the width direction at 150° C. and the stress at 5% elongation (MPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae. By satisfying the following formula, the rigidity is higher and the thermal shrinkage rate at high temperatures is smaller, so that the shape of the bag when made into a packaging bag can be more easily maintained, and the film is less likely to deform during processing such as heat sealing at high temperatures, improving the packaging quality. In addition, the film can be made thinner, which contributes to reducing the volume of packaging materials. Stress at 5% elongation in the width direction at 23℃ (MPa) ≧ Heat shrinkage in the width direction at 150℃ (%) × 4.0 + 140 It is more preferable that the heat shrinkage rate (%) in the width direction at 150° C. and the stress at 5% elongation (MPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae. Stress at 5% elongation in the width direction at 23℃ (MPa) ≧ Heat shrinkage in the width direction at 150℃ (%) × 4.0 + 150 It is further preferable that the heat shrinkage rate (%) in the width direction at 150° C. and the stress at 5% elongation (MPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae: Stress at 5% elongation in the width direction at 23℃ (MPa) ≧ Heat shrinkage in the width direction at 150℃ (%) × 4.0 + 160

[0047] (Heat shrinkage rate at 150℃) The upper limit of the heat shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 150° C. is preferably 10%, more preferably 7.0%, even more preferably 6.0%, particularly preferably 5.0%, and most preferably 4.0% or less. The upper limit of the heat shrinkage rate in the transverse direction at 150° C. is preferably 30%, more preferably 20%, even more preferably 16%, and particularly preferably 15% or less. When the heat shrinkage rate in the longitudinal direction is 10% or less and the heat shrinkage rate in the transverse direction is 30% or less, wrinkles are unlikely to occur during heat sealing, and in particular, when the heat shrinkage rate in the longitudinal direction is 8.0% or less and the heat shrinkage rate in the transverse direction is 15% or less at 150°C, distortion when the zipper part is fused to the opening is small, which is preferable. In order to reduce the heat shrinkage rate at 150°C, it is effective to set the lower limit of the amount of components with a molecular weight of 100,000 or less when measuring the gel permeation chromatography (GPC) cumulative curve of the polypropylene resin constituting the film to 35% by mass.

[0048] (Stress at 23℃ 5% elongation) The lower limit of F5 in the width direction of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 140 MPa, more preferably 160 MPa, even more preferably 180 MPa, and particularly preferably 190 MPa. At 140 MPa or more, the film has high rigidity, so that the shape of the bag formed into a packaging bag is easily maintained, and deformation of the film is unlikely to occur during processing such as printing. The upper limit of F5 in the width direction at 23° C. is preferably 300 MPa, more preferably 290 MPa, and further preferably 280 Pa. If it is 280 MPa or less, practical production is easy and the longitudinal-width balance is easily improved. The lower limit of the stress (F5) of the biaxially oriented polypropylene film of the present invention at 23° C. and 5% elongation in the longitudinal direction is preferably 40 Pa, more preferably 42 Pa, even more preferably 46 Pa, and particularly preferably 48 Pa. At 40 MPa or more, the film has high rigidity, so that the shape of the bag when made into a packaging bag is easily maintained, and deformation of the film is unlikely to occur during processing such as printing. The upper limit of F5 in the longitudinal direction at 23° C. is preferably 70 MPa, more preferably 65 MPa, further preferably 62 MPa, and particularly preferably 60 Pa. At 70 MPa or less, practical production becomes easy and the longitudinal-width balance tends to be improved. F5 can be kept within the range by adjusting the stretch ratio and relaxation rate, or by adjusting the temperature during film formation.

[0049] The biaxially oriented polypropylene film of the present invention preferably has the following characteristics and structure. (120℃ heat shrinkage rate) The upper limit of the heat shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 120°C is preferably 2.0%, more preferably 1.5%, even more preferably 1.2%, and particularly preferably 1.0%. If it is 2.0% or less, printing pitch deviation is unlikely to occur when transferring printing ink. The upper limit of the heat shrinkage rate in the transverse direction at 120°C is 10.0% or less, preferably 5.0%, more preferably 3.5%, and particularly preferably 2.5%. If it is 10.0% or less, wrinkles are unlikely to occur during heat sealing. The heat shrinkage rate at 120°C can be kept within the range by adjusting the stretch ratio, stretching temperature and heat setting temperature.

[0050] It is preferable that the heat shrinkage rate (%) in the width direction at 120° C. and the tensile modulus (GPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae. By satisfying the following formula, the rigidity is higher and the thermal shrinkage rate at high temperatures is smaller, so that printing pitch deviation is less likely to occur when the material is made into packaging bags. Tensile modulus (GPa) in the width direction at 23°C ≧ Heat shrinkage rate (%) in the width direction at 120°C × 0.1 + 7.0 It is more preferable that the heat shrinkage rate (%) in the width direction at 120° C. and the tensile modulus (GPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae: Tensile modulus (GPa) in the width direction at 23°C ≥ Heat shrinkage (%) in the width direction at 120°C × 0.1 + 8.0 It is further preferable that the heat shrinkage rate (%) in the width direction at 120° C. and the tensile modulus (GPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae: Tensile modulus (GPa) in the width direction at 23°C ≥ Heat shrinkage (%) in the width direction at 120°C × 0.1 + 9.0

[0051] (23℃ tensile modulus) The lower limit of the tensile modulus in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23 ° C. is preferably 2.0 GPa, more preferably 2.1 GPa, even more preferably 2.2 GPa, even more preferably 2.3 GPa, particularly preferably 2.4 GPa, and most preferably 2.6 GPa. At 2.0 GPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of the tensile modulus in the longitudinal direction is preferably 4.0 GPa, more preferably 3.8 GPa, even more preferably 3.7 GPa, particularly preferably 3.6 GPa, and most preferably 3.5 GPa. At 4.0 GPa or less, practical production is easy and the balance of the properties in the longitudinal direction and the width direction is easily improved. The lower limit of the tensile modulus in the width direction at 23°C of the biaxially oriented polypropylene film of the present invention is preferably 6.0 GPa, more preferably 6.5 GPa, more preferably 6.7 GPa, even more preferably 7.0 GPa, particularly preferably 8.0 GPa, and most preferably 8.5 GPa. At 6.0 GPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of the tensile modulus in the width direction is preferably 15 GPa, more preferably 13 GPa, and even more preferably 12 GPa. At 15 GPa or less, practical production is easy and the balance of the properties in the longitudinal direction and the width direction is easily improved. The tensile modulus can be kept within the range by adjusting the stretch ratio and relaxation rate, or by adjusting the temperature during film formation.

[0052] (23℃ tensile breaking strength) The lower limit of the longitudinal tensile breaking strength of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 90 MPa, more preferably 100 MPa, even more preferably 110 MPa, and particularly preferably 115 MPa. If it is 90 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The upper limit of the longitudinal tensile breaking strength is preferably 200 MPa as a practical value, more preferably 180 MPa, and even more preferably 160 MPa. If it is 200 MPa or less, film breakage and packaging bag breakage are likely to be reduced. The lower limit of the tensile breaking strength in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 400 MPa, more preferably 420 MPa, even more preferably 440 MPa, and particularly preferably 450 MPa. If it is 400 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The upper limit of the tensile breaking strength in the width direction is preferably 650 MPa as a practical value, more preferably 600 MPa, and even more preferably 550 MPa. If it is 650 MPa or less, film breakage and packaging bag breakage are likely to be reduced. The tensile breaking strength can be controlled within the range by adjusting the stretch ratio, stretching temperature and heat setting temperature.

[0053] (23℃ tensile elongation at break) The lower limit of the longitudinal tensile elongation at break of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 180%, more preferably 190%, more preferably 200%, and particularly preferably 210% or more. If it is 180% or more, film breakage and packaging bag breakage are likely to be reduced. The upper limit of the longitudinal tensile elongation at break at 23°C is preferably 300% as a practical value, and more preferably 280%.

[0054] The lower limit of the tensile elongation at break in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 15%, more preferably 20%, and more preferably 30%. If it is 15% or more, the film breakage and the packaging bag breakage are likely to be reduced. The upper limit of the tensile elongation at break in the width direction at 23°C is preferably 60%, more preferably 55%, and even more preferably 50%. If it is 60% or less, the printing pitch deviation is unlikely to occur when transferring the printing ink, and the durability of the packaging bag is likely to be excellent. The tensile elongation at break can be controlled within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.

[0055] (Refractive Index) The lower limit of the refractive index (Nx) in the longitudinal direction of the biaxially oriented polypropylene film of the present invention is preferably 1.4950, more preferably 1.4970, even more preferably 1.4980, particularly preferably 1.4990, and most preferably 1.5000. If it is 1.4950 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Nx) in the longitudinal direction is preferably 1.5100, more preferably 15070, and even more preferably 1.5050. If it is 1.5100 or less, the film is likely to have an excellent balance of properties in the longitudinal direction and the width direction.

[0056] The lower limit of the refractive index (Ny) in the width direction of the biaxially oriented polypropylene film of the present invention is preferably 1.5250, more preferably 1.5253, even more preferably 1.5255, particularly preferably 1.5260, and most preferably 1.5265. If it is 1.5250 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Ny) in the width direction is preferably 1.5280, more preferably 1.5275, and even more preferably 1.5270. If it is 1.5280 or less, the film is likely to have an excellent balance of properties in the longitudinal direction and the width direction.

[0057] The lower limit of the refractive index (Nz) in the thickness direction of the biaxially oriented polypropylene film of the present invention is preferably 1.4960, more preferably 14965, even more preferably 1.4970, particularly preferably 1.4980, and most preferably 1.4990. If it is 1.4960 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Nz) in the thickness direction is preferably 1.5020, more preferably 1.5015, and even more preferably 1.5010. If it is 1.5020 or less, the heat resistance of the film is easily increased. The refractive index can be adjusted within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.

[0058] (△Ny) The lower limit of ΔNy, which is the degree of orientation in the width direction of the biaxially oriented polypropylene film of the present invention, is preferably 0.0240, more preferably 0.0245, even more preferably 0.0247, particularly preferably 0.0250, most preferably 0.0255, and particularly most preferably 0.0260. If it is 0.0240 or more, the rigidity of the film tends to be high. The upper limit of ΔNy is preferably 0.0280 as a practical value, more preferably 0.0277, even more preferably 0.0273, and particularly preferably 0.0270. If it is 0.0280 or less, the thickness unevenness tends to be good. ΔNy can be kept within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature of the film. ΔNy is calculated by the following formula, where Nx, Ny, and Nz are the refractive indices along the length, width, and thickness directions of the film, respectively, and it means the degree of orientation in the width direction in the overall orientation of the film in the length, width, and thickness directions. △Ny=Ny-[(Nx+Nz) / 2]

[0059] (Face orientation coefficient) The lower limit of the plane orientation coefficient (ΔP) of the biaxially oriented polypropylene film of the present invention is preferably 0.0135, more preferably 0.0138, and even more preferably 0.0140. If it is 0.0135 or more, the balance in the plane direction of the film is good, and the thickness unevenness is also good. The upper limit of the plane orientation coefficient (ΔP) is preferably 0.0155 as a practical value, more preferably 0.0152, and even more preferably 0.0150. If it is 0.0155 or less, it is likely to have excellent heat resistance at high temperatures. The plane orientation coefficient (ΔP) can be within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature. The plane orientation coefficient (ΔP) was calculated using the formula: [(Nx+Ny) / 2]-Nz.

[0060] (average refractive index) The lower limit of the average refractive index of the biaxially oriented polypropylene film of the present invention is preferably 1.5080, more preferably 1.5081, even more preferably 1.5082, particularly preferably 1.5083, and most preferably 1.5090. The upper limit of the average refractive index is preferably 1.5150, more preferably 1.5140, even more preferably 1.5135, and particularly preferably 1.5130 as a practical value. If it is 1.5080 or more, wrinkles are unlikely to occur during heat sealing of the film. The average refractive index can be within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature of the film. The average refractive index is calculated by the following formula, where Nx, Ny, and Nz are the refractive indices in the longitudinal, transverse, and thickness directions of the film, respectively. Average refractive index = (Nx + Ny + Nz) / 3

[0061] (Hayes) The upper limit of the haze of the biaxially oriented polypropylene film of the present invention is preferably 5.0%, more preferably 4.5%, even more preferably 4.0%, particularly preferably 3.5%, and most preferably 3.0%. If it is 5.0% or less, it is easy to use in applications where transparency is required. The lower limit of the haze is preferably 0.1% as a practical value, more preferably 0.2%, even more preferably 0.3%, and particularly preferably 0.4%. If it is 0.1% or more, it is easy to manufacture. The haze can be kept within the range by adjusting the cooling roll (CR) temperature, the width direction stretching temperature, the tenter preheating temperature before width direction stretching, the width direction stretching temperature, or the heat setting temperature, or the amount of the component having a molecular weight of 100,000 or less of the polypropylene resin, but it may become large by adding an antiblocking agent or providing a seal layer.

[0062] (Half-width of diffraction peak due to oriented crystals) In the azimuth angle dependence of the scattering peak of the (110) plane of the polypropylene α-type crystals obtained by wide-angle X-ray measurement perpendicular to the film surface of the biaxially oriented polypropylene film of the present invention, the upper limit of the half-width (Wh) of the diffraction peak derived from the oriented crystals in the width direction of the film is preferably 21.0°, more preferably 20.5° or less, more preferably 20.0° or less, particularly preferably 19.5° or less, and most preferably 19.0° or less. When the half-width (Wh) is 21.0° or less, the rigidity of the film is easily increased. In addition, the water vapor permeability is easily reduced. The lower limit of Wh is preferably 15°, more preferably 16°, and even more preferably 17°.

[0063] (X-ray orientation degree) The lower limit of the degree of X-ray orientation of the biaxially oriented polypropylene film of the present invention calculated from Wh by the following formula is preferably 0.883, more preferably 0.886, and even more preferably 0.889. By making it 0.892 or more, the rigidity can be easily increased. X-ray orientation degree=(180-Wh) / 180 The upper limit of the degree of X-ray orientation is preferably 0.917, more preferably 0.911, and further preferably 0.906. By setting it to 0.917 or less, film formation is likely to be stable.

[0064] (Water vapor transmission rate) The water vapor permeability of the biaxially oriented polypropylene film of the present invention is 5.0 g / m2 when converted to a thickness of 20 μm. 2 It is preferable to set the value to 4.6 g / m or less. 2 It is more preferable to set it to 4.3 g / m or less. 2 It is more preferable to set the thickness to 5.0 g / m or less. 2 When the film thickness is less than or equal to ·d, sufficient water vapor barrier properties are obtained even when the film is made thin.

[0065] (Practical properties of film) The practical properties of the biaxially oriented polypropylene film of the present invention will now be described. (Rigidity and water vapor barrier properties) Packaging materials used for packaging foods, beverages, etc. must protect the contents from various distribution processes, storage such as refrigeration, and treatments such as heat sterilization. In addition to functions such as rigidity and heat resistance, they are particularly required to have high barrier properties for the purpose of preserving the quality and volume of the contents. Even when made thin, these properties must be excellent.

[0066] (Wrinkles during heat sealing) To form a bag for packaging food, the contents are filled into a bag that has already been made, and the film is heated to melt and fuse to seal it. In addition, the same process is often used when making a bag while filling it with food. Usually, a sealant film made of polyethylene or polypropylene is laminated on the base film, and the sealant film surfaces are fused together. The heating method is to apply pressure from the base film side with a heating plate to hold down the film and seal it, and the seal width is often about 10 mm. At this time, the base film is also heated, and the shrinkage at that time causes wrinkles. In terms of bag durability, it is better to have fewer wrinkles, and it is also better to have fewer wrinkles to increase purchasing desire. The sealing temperature may be around 120°C, but a higher sealing temperature is required to increase the bag making processing speed, and even in that case, it is preferable that the shrinkage is small. When a zipper is fused to the opening of the bag, sealing at an even higher temperature is required.

[0067] (Print pitch deviation) Packaging films are often basically made up of a laminated film of a printed base film and a sealant film. Bag making machines are used to manufacture bags, and various types of bags are used, including three-sided bags, standing bags, and gusset bags. Print pitch deviation is thought to occur because tension and heat are applied to the film during the printing process, causing the film base material to expand and contract. Eliminating defective products due to print pitch deviation is important in terms of efficient use of resources and increasing purchasing motivation.

[0068] (Film processing) Printing on the biaxially oriented polypropylene film of the present invention can be carried out by letterpress printing, lithographic printing, intaglio printing, stencil printing or transfer printing, depending on the application. Also, it can be used as a laminate with heat sealability by laminating an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of low density polyethylene, linear low density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, or polyester as a sealant film. When gas barrier properties or heat resistance is to be improved, an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of aluminum foil, polyvinylidene chloride, nylon, ethylene-vinyl alcohol copolymer, or polyvinyl alcohol can be provided as an intermediate layer between the biaxially oriented polypropylene film and the sealant film. An adhesive applied by dry lamination or hot melt lamination can be used to laminate the sealant film. To improve the gas barrier properties, aluminum or inorganic oxides can be vapor-deposited on the biaxially oriented polypropylene film, intermediate layer film, or sealant film. Vacuum deposition, sputtering, and ion plating can be used as the vapor deposition method, but vacuum deposition of silica, alumina, or a mixture thereof is particularly preferred.

[0069] The biaxially oriented polypropylene film of the present invention can be made suitable for packaging fresh produce such as vegetables, fruits, flowers, and other plants that require high freshness by containing an anti-fog agent, such as fatty acid esters of polyhydric alcohols, amines of higher fatty acids, amides of higher fatty acids, or ethylene oxide adducts of amines or amides of higher fatty acids, in an amount of 0.2 to 5 mass %.

[0070] In addition, various additives for improving qualities such as slipperiness and antistatic properties, for example, lubricants such as wax and metal soaps for improving productivity, plasticizers, processing aids, heat stabilizers, antioxidants, antistatic agents, ultraviolet absorbers, etc. can also be blended within a range that does not impair the effects of the present invention.

[0071] (Industrial Applicability) Since the biaxially oriented polypropylene film of the present invention has the above-mentioned excellent properties not available in the prior art, it can be preferably used for packaging bags, and the thickness of the film can be made thinner than in the prior art.

[0072] Furthermore, it is also suitable for applications that require high temperatures, such as insulating films for capacitors and motors, backsheets for solar cells, barrier films for inorganic oxides, and base films for transparent conductive films such as ITO, as well as applications that require rigidity, such as separate films. In addition, it is possible to coat or print at high temperatures using coating agents, inks, lamination adhesives, etc. that were previously difficult to use, and this is expected to improve production efficiency. EXAMPLES

[0073] The present invention will be described in detail below with reference to examples. The properties were measured and evaluated by the following methods. (1) Melt flow rate The melt flow rate (MFR) was measured in accordance with JIS K7210 at a temperature of 230° C. and a load of 2.16 kgf.

[0074] (2) Meso-pentad fraction The mesopentad fraction ([mmmm]%) of polypropylene resin is measured as follows: 13 The mesopentad fraction was calculated according to the method described in Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973). 13 C-NMR measurements were performed using a BRUKER AVANCE500 at 110°C after dissolving 200 mg of a sample in a 8:2 mixture of o-dichlorobenzene and deuterated benzene at 135°C.

[0075] (3) Number average molecular weight, weight average molecular weight, amount of components with molecular weights of 100,000 or less, and molecular weight distribution of polypropylene resin The molecular weight was determined by gel permeation chromatography (GPC) using monodisperse polystyrene as the standard in terms of PP. When the baseline was unclear, the baseline was set to the lowest point of the high molecular weight tail of the elution peak closest to the elution peak of the standard substance. The GPC measurement conditions are as follows. Equipment: HLC-8321PC / HT (Tosoh Corporation) Detector: RI Solvent: 1,2,4-trichlorobenzene + dibutylhydroxytoluene (0.05%) Column: TSK gelguard column HHR (30) HT (7.5 mm I.D. x 7.5 cm) x 1 + TSK gel GMHHR-H (20) HT (7.8 mm I.D. x 30 cm) x 3 Flow rate: 1.0mL / min Injection volume: 0.3mL Measurement temperature: 140℃ The number average molecular weight (Mn) and the mass average molecular weight (Mw) are the molecular weights (M i ) number of molecules (N i ) is defined by the following formula: Number average molecular weight: Mn=Σ(N i M i ) / ΣN i Mass average molecular weight: Mw=Σ(N i M i 2 ) / Σ(N i M i ) Here, the molecular weight distribution can be obtained by Mw / Mn. In addition, the proportion of components having a molecular weight of 100,000 or less was determined from the integral curve of the molecular weight distribution obtained by GPC.

[0076] (4) Crystallization temperature (Tc), melting temperature (Tm) Heat measurements were performed under nitrogen atmosphere using a TA Instruments Q1000 differential scanning calorimeter. Approximately 5 mg was cut out from the polypropylene resin pellets and sealed in an aluminum pan for measurement. The temperature was raised to 230°C and held for 5 minutes, then cooled to 30°C at a rate of -10°C / min, and the exothermic peak temperature was taken as the crystallization temperature (Tc). The heat of crystallization (△Hc) was calculated by setting a baseline so that the area of ​​the exothermic peak was smoothly connected from the start of the peak to the end of the peak. The temperature was held at 30°C for 5 minutes, and then raised to 230°C at 10°C / min, and the main endothermic peak temperature was taken as the melting temperature (Tm).

[0077] (5) Film thickness The thickness of the films was measured using a Seiko EM Millitron 1202D.

[0078] (6) Hayes Measurements were performed at 23°C in accordance with JIS K7105 using an NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0079] (7) Tensile test The tensile strength of the film in the longitudinal and transverse directions was measured at 23°C in accordance with JIS K7127. Samples were cut out from the film to a size of 15 mm x 200 mm, and set in a tensile tester (Instron 5965 dual column tabletop tester manufactured by Instron Japan Co., Ltd.) with a chuck width of 100 mm. The tensile test was performed at a tensile speed of 200 mm / min. From the obtained strain-stress curve, the tensile modulus was determined from the slope of the linear portion at the beginning of elongation, and the stress at 5% elongation was determined as F5. The tensile breaking strength and tensile breaking elongation were respectively the strength and elongation at the time when the sample broke.

[0080] (8) Heat shrinkage rate The measurement was performed according to the following method in accordance with JIS Z 1712. The film was cut into pieces of 20 mm width and 200 mm length in both the longitudinal and transverse directions of the film, and was hung in a hot air oven at 120°C or 150°C and heated for 5 minutes. The length after heating was measured, and the thermal shrinkage rate was calculated as the ratio of the shrunken length to the original length.

[0081] (9) Refractive index, △Ny, plane orientation coefficient, average refractive index Measurements were made at a wavelength of 589.3 nm and a temperature of 23°C using an Abbe refractometer manufactured by Atago Co., Ltd. The refractive indices along the longitudinal and width directions of the film were designated Nx and Ny, respectively, and the refractive index along the thickness direction was designated Nz. The degree of orientation in the width direction, ΔNy, was calculated using Nx, Ny, and Nz using the formula Ny-[(Nx+Nz) / 2]. The plane orientation coefficient (ΔP) was calculated using the formula ΔP=[(Nx+Ny) / 2]-Nz. The average refractive index was calculated using the formula Average refractive index=(Nx+Ny+Nz) / 3.

[0082] (10) X-ray half-width, degree of orientation Measurements were performed using an X-ray diffraction device (Rigaku Corporation, SmartLab, with αβγ attachment) in the transmission method. X-rays with a wavelength of 1.5418 Å were used, with an X-ray output of 45 kV and 200 mA. A hybrid multidimensional pixel detector Hypix-3000 was used in 0-dimensional mode as the detector. For the parallel beam method, a solar slit of 2.5°, a longitudinal limiting slit of 10 mm, and an entrance slit width of 1 mm were used as the entrance slit. A parallel slit analyzer of 0.228° was used as the receiving slit. The camera length was 300 mm and the detector integral width was 2 mm. A sample was prepared by stacking films to a thickness of 400 μm. A detector was placed at the diffraction peak position (diffraction angle 2θ = 14.1°) of the (110) plane of the α-crystal of polypropylene resin, and the sample was rotated 360° around the axis of the thickness direction of the film to obtain the azimuth angle dependence of the diffraction intensity of the (110) plane. The measurement was performed with a step interval of 0.5° and a measurement speed of 60° / min. From this azimuth angle dependence, the half-width Wh of the diffraction peak resulting from oriented crystals in the width direction of the film was obtained. In addition, the degree of X-ray orientation was calculated using Wh according to the following formula. X-ray orientation degree=(180-Wh) / 180

[0083] (11) Water vapor permeability 265 Water vapor permeability was measured in accordance with JIS K7129 Method B. Using a water vapor permeability measuring device (PERMATRAN-W3 / 33, manufactured by MOCON), the water vapor permeability was measured under an atmosphere of a temperature of 40°C and a humidity of 90% RH. Since the water vapor permeability is inversely proportional to the film thickness, the thickness of each sample was measured and converted to a value at 20 μm.

[0084] Example 1 The polypropylene resin used was a blend of 80 parts by weight of a propylene homopolymer PP-1 (Sumitomo Chemical Co., Ltd., Sumitomo Noblen FLX80E4) having an MFR of 7.5 g / 10 min, [mmmm] of 98.9%, Tc of 116.2°C, and Tm of 162.5°C, and 20 parts by weight of a propylene homopolymer PP-2 (Sumitomo Chemical Co., Ltd., EL80F5) having an MFR of 11 g / 10 min, [mmmm] of 98.8%, Tc of 116.5°C, and Tm of 161.5°C. The sheet was extruded from a T-die at 250°C, brought into contact with a cooling roll at 20°C, and then placed in a water bath at 20°C. The film was then stretched 4.5 times in the longitudinal direction with two pairs of rolls at 142°C, then both ends were clamped with clips, introduced into a hot air oven, preheated at 170°C, and stretched 10 times in the width direction at 162°C as the first stage. Immediately after stretching in the width direction, the film was cooled at 120°C while still being held by the clips, and then re-stretched 1.2 times in the width direction at 175°C. Finally, the film was cooled at room temperature. The thickness of the film thus obtained was 18.6 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As shown in Table 3, the physical properties of the film obtained were excellent in rigidity and had a low thermal shrinkage rate at high temperatures. The film also had excellent water vapor permeability.

[0085] Example 2 The same procedure as in Example 1 was carried out except that the film was re-stretched by 1.2 times in the width direction at 165°C. The thickness of the obtained film was 18.4 µm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As shown in Table 3, the physical properties of the film were very excellent in rigidity, and a film with low heat shrinkage at high temperatures was obtained. The film also had excellent water vapor permeability.

[0086] Example 3 The same procedure as in Example 1 was repeated except that the film was stretched in the longitudinal direction at 147° C., then stretched 10 times in the width direction at 165° C. as the first stage, and immediately after the width direction stretching, it was cooled at 120° C. while still held by the clips, and then re-stretched 1.2 times in the width direction at 177° C. The thickness of the obtained film was 18.9 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As shown in Table 3, the physical properties of the film obtained were high rigidity and low heat shrinkage at high temperatures. The film also had excellent water vapor permeability.

[0087] Example 4 The same procedure as in Example 3 was repeated except that the film was re-stretched to 1.1 times the width direction at 177° C. The thickness of the obtained film was 20.6 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As shown in Table 3, the physical properties of the film were high rigidity and low heat shrinkage at high temperatures. The film also had excellent water vapor permeability.

[0088] Comparative Example 1 The same procedure as in Example 1 was repeated except that the film was stretched 12 times in the width direction at 162°C as the first stage, and immediately after the width direction stretching, it was cooled at 100°C while still being held by the clips, and then heat-set at 170°C while keeping the width constant. The thickness of the obtained film was 20.8 µm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As shown in Table 3, the physical properties of the film were excellent in water vapor permeability and high rigidity, but poor in heat shrinkage.

[0089] Comparative Example 2 The film was stretched 12 times in the width direction at 162°C as the first stage, and immediately after the stretching in the width direction, the film was not cooled while still held by the clips, but was heat-set at 172°C while keeping the width constant, in the same manner as in Example 1. The thickness of the obtained film was 23.1 µm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. The physical properties of the film were poor in stiffness, as shown in Table 3. The film also had poor water vapor permeability.

[0090] Comparative Example 3 The same procedure as in Example 1 was repeated except that the film was stretched 12 times in the width direction at 168°C as the first stage, and immediately after the width direction stretching, it was cooled at 100°C while still being held by the clips, and then heat-set at 170°C while keeping the width constant. The thickness of the obtained film was 18.7 µm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As shown in Table 3, the physical properties of the film were high in heat shrinkage at high temperatures and poor in rigidity. The film also had poor water vapor permeability.

[0091] Comparative Example 4 As the polypropylene resin, PP-3 (manufactured by Japan Polypropylene Co., Ltd., FL203D) with MFR=3g / 10min, [mmmm]=94.8%, Tc=117.2°C, and Tm=160.6°C was used. The film was extruded into a sheet from a T-die at 250°C, brought into contact with a cooling roll at 20°C, and then placed in a water tank at 20°C. The film was then stretched 4.5 times in the longitudinal direction at 130°C, and in the width direction stretching with a tenter, the preheating temperature was set to 168°C, and 8.2 times stretching was performed at 155°C as the first stage of stretching. Immediately after the width direction stretching, the film was cooled at 120°C while being held by the clip, and then re-stretched 1.2 times in the width direction at 170°C. Finally, the film was cooled at room temperature. The thickness of the obtained film was 18.8 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As shown in Table 3, the physical properties of the film were high in heat shrinkage at high temperatures and poor in rigidity. The film also had poor water vapor permeability.

[0092] [Table 1]

[0093]

Table 2

[0094]

Table 3

Claims

1. A method for producing a biaxially oriented polypropylene film, comprising the steps of: extruding a polypropylene resin composition containing a polypropylene resin having a mesopentad fraction of 97.0% or more to obtain an unstretched sheet; stretching the unstretched sheet in the longitudinal direction; a preheating step of heating the longitudinally stretched film to a preheating temperature in the range of Tm to Tm+25°C; stretching the preheated longitudinally stretched film at a ratio of 10 times or more in the width direction at a temperature of Tm-10°C or more and not exceeding the preheating temperature; cooling the film at a temperature of Tm-80°C or more and not exceeding Tm-15°C at the end of the width direction stretching at a temperature not exceeding the width direction stretching temperature and; and heat setting while stretching at a ratio of 1.03 times or more in the width direction at Tm-5°C or more and not exceeding Tm+20°C.

2. The method for producing a biaxially oriented polypropylene film according to claim 1, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a crystallization temperature of 105°C or higher and a melting point of 160°C or higher.

3. The method for producing a biaxially oriented polypropylene film according to claim 1 or 2, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a melt flow rate of 4.0 g / 10 min or more.

4. The method for producing a biaxially oriented polypropylene film according to any one of claims 1 to 3, wherein the amount of components of the polypropylene resin constituting the biaxially oriented polypropylene film having a molecular weight of 100,000 or less is 35% by mass or more.

Citation Information

Patent Citations

  • Reinforced, biaxially oriented polypropylene film

    JP2001040111A

  • Biaxially oriented polypropylene film and method for producing the same

    JP2013177645A

  • Biaxially oriented polypropylene film for capacitor, metal laminated film, and film capacitor

    WO2016158590A1

  • Polypropylene film, metal membrane layered film, and film capacitor, and method for manufacturing same

    WO2016182003A1