Polarizing plate with adhesive and image display device
The adhesive composition for image display devices addresses durability issues by maintaining minimal transmittance changes and UV protection, ensuring the polarizer's stability under humid conditions, thereby enhancing device performance.
Patent Information
- Application Number
- JP2020125754
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-22
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-07-22
AI Technical Summary
Image display devices with a cover window bonded to a polarizer using an adhesive sheet face durability issues under humid conditions, particularly due to fading and discoloration of the polarizer caused by ultraviolet exposure and high humidity.
A pressure-sensitive adhesive composition is developed with specific transmittance criteria (ΔT and δT) and ultraviolet absorbing properties to minimize polarizer fading, ensuring the adhesive sheet maintains minimal transmittance changes under heat and moisture, thereby enhancing the durability of the image display device.
The adhesive composition ensures the polarizer retains its optical properties and durability under high temperature and humidity conditions, reducing fading and discoloration, thus maintaining image quality and device performance.
Smart Images

Figure 0007572176000002 
Figure 0007572176000003 
Figure 0007572176000004
Abstract
Description
[Technical field]
[0001] The present invention is used in the formation of an image display device. Viscosity Polarizing plate with adhesive 、 And the present invention relates to an image display device. [Background technology]
[0002] Liquid crystal display devices and organic electroluminescence (EL) display devices are widely used as various image display devices such as mobile phones, smartphones, car navigation devices, PC monitors, and televisions. Due to the display principle of liquid crystal display devices, a polarizing plate is arranged on the viewing side surface of the liquid crystal cell. In self-luminous display devices such as organic EL, a circular polarizing plate (a laminate of a polarizing plate and a quarter-wave plate) is arranged on the viewing side surface of the cell to prevent external light from being reflected by the metal electrode (cathode) and being viewed as a mirror surface.
[0003] A front transparent plate (also called a "cover window") such as a transparent resin plate or a glass plate is provided on the viewing side surface of the image display device for the purpose of preventing damage to the image display panel due to impact from the outer surface, etc. The cover window is attached to the polarizing plate arranged on the viewing side surface of the image display panel via an adhesive sheet.
[0004] A polarizing plate generally has a laminated structure in which transparent protective films are bonded to both sides of a polarizer, but from the viewpoint of making image display devices thinner and more flexible, a structure in which the transparent protective films on one or both sides of the polarizer are omitted has been proposed. For example, Patent Document 1 discloses a structure in which a cover window is bonded to a polarizer via an adhesive sheet disposed in contact with the polarizer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2017 / 216886 Summary of the Invention [Problem to be solved by the invention]
[0006] An image display device having a cover window attached by a pressure-sensitive adhesive sheet provided in contact with the viewing side surface of a polarizer is used in various environments, and is required to have high durability even under humid conditions. In view of this problem, an object of the present invention is to provide a pressure-sensitive adhesive sheet disposed adjacent to a polarizer, and a pressure-sensitive adhesive composition used for forming the pressure-sensitive adhesive sheet. [Means for solving the problem]
[0007] One embodiment of the present invention is a pressure-sensitive adhesive composition for forming a pressure-sensitive adhesive sheet that is used to bond a polarizer to a cover window of an image display device and is arranged in contact with the polarizer. When a sample in which the pressure-sensitive adhesive sheet is arranged in contact with the polarizer is subjected to a wet heat test in which the sample is left in an environment at a temperature of 85° C. and a relative humidity of 85% for 100 hours, it is preferable that ΔT1, ΔT2, ΔT3, and ΔT4 all satisfy a range of 1.0 to 1.2, and it is preferable that ΔT1, ΔT2, ΔT3, and ΔT4 all satisfy a range of 0.95 to 1.05.
[0008] ΔT n =(T n '-T0') / (T n -T0) δT n =(T n ' / ΣT i ') / (T n / ΣT i ) In the above formula, n and i are integers from 1 to 4.
[0009] T0 is the 100 μm equivalent transmittance at a wavelength of 380 nm before the moist heat test, T1 is the 100 μm equivalent transmittance at a wavelength of 450 nm before the moist heat test, T2 is the 100 μm equivalent transmittance at a wavelength of 520 nm before the moist heat test, T3 is the 100 μm equivalent transmittance at a wavelength of 580 nm before the moist heat test, and T4 is the 100 μm equivalent transmittance at a wavelength of 660 nm before the moist heat test. T0' is the 100 μm equivalent transmittance at a wavelength of 380 nm after the moist heat test, T1' is the 100 μm equivalent transmittance at a wavelength of 450 nm after the moist heat test, T2' is the 100 μm equivalent transmittance at a wavelength of 520 nm after the moist heat test, T3' is the 100 μm equivalent transmittance at a wavelength of 580 nm after the moist heat test, and T4' is the 100 μm equivalent transmittance at a wavelength of 660 nm after the moist heat test.
[0010] The 100 μm converted transmittance T (%), the total thickness L (μm) of the pressure-sensitive adhesive sheet and the polarizer, and the measured transmittance t (%) are log 10 (T / 100)=(100 / L)×log 10 (t / 100) Satisfy the relationship.
[0011] The pressure-sensitive adhesive composition preferably contains an ultraviolet absorber.
[0012] The pressure-sensitive adhesive composition is used to form a pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet of one embodiment is used to attach a polarizer to a cover window of an image display device, and is disposed in contact with the polarizer.
[0013] One embodiment of the present invention is a polarizing plate with adhesive, in which the above-mentioned adhesive sheet is disposed on the first main surface of a polarizer having a first main surface and a second main surface. The polarizing plate with adhesive may further include an adhesive sheet on the second main surface side of the polarizer. The adhesive sheet disposed on the second main surface side of the polarizer may be in contact with the second main surface of the polarizer, or may be laminated on the second main surface of the polarizer via another layer.
[0014] One embodiment of the present invention is an image display device having, in this order, a second adhesive sheet, a polarizer made of a polyvinyl alcohol-based film containing iodine, a first adhesive sheet, and a cover window on the surface of an image display cell, wherein the first adhesive sheet is the above-mentioned adhesive sheet and is arranged in contact with the polarizer. Effect of the Invention
[0015] An image display device in which the pressure-sensitive adhesive sheet according to the embodiment of the present invention is disposed in contact with the viewing side surface of a polarizer has durability against external ultraviolet rays, and can also exhibit high durability even in a humid environment. [Brief description of the drawings]
[0016] [Figure 1] 1 is a cross-sectional view illustrating an embodiment of an image display device. [Diagram 2] FIG. 1 is a cross-sectional view illustrating one embodiment of a polarizing plate with a pressure-sensitive adhesive. [Diagram 3] FIG. 1 is a cross-sectional view illustrating one embodiment of a polarizing plate with a pressure-sensitive adhesive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] One embodiment of the present invention relates to a pressure-sensitive adhesive sheet to be placed in contact with a viewing side surface of a polarizer in an image display device, and a pressure-sensitive adhesive composition for forming the pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet is used to attach the polarizer to a cover window.
[0018] 1 is a cross-sectional view showing one embodiment of an image display device having a cover window on the viewing side surface. The image display device 100 has a polarizing plate 10 attached to the surface of an image display cell 60 via an adhesive sheet 22, and a cover window 70 attached to the polarizing plate 10 via an adhesive sheet 21 of an embodiment of the present invention.
[0019] The polarizing plate 10 includes a polarizer 11 made of a polyvinyl alcohol-based film containing iodine. An appropriate optical layer 15 may be provided on a second main surface (surface on the image display cell 60 side) of the polarizer 11. A pressure-sensitive adhesive sheet 21 according to an embodiment of the present invention is disposed on a first main surface (surface on the viewing side) of the polarizer 11 in contact with the polarizer 11. By disposing the pressure-sensitive adhesive sheet 21 on the viewing side of the polarizer 11 without any other optical layer therebetween, it is possible to make the image display device thinner and more flexible.
[0020] [Heat and moisture resistance of adhesive sheet (change in transmittance)] The pressure-sensitive adhesive sheet 21 according to the embodiment of the present invention is used for bonding the polarizer 11 and the cover window 70 of the image display device, and is disposed in contact with the polarizer 21. The pressure-sensitive adhesive sheet 21 is formed using a pressure-sensitive adhesive composition described below.
[0021] The adhesive sheet 21 of the embodiment of the present invention is characterized by having small change in transmittance over a wide range of visible light when a sample in which the adhesive sheet is placed in contact with a polarizer is subjected to a moist heat test in which the sample is left in an environment of 85°C temperature and 85% relative humidity for 100 hours.
[0022] The change in transmittance is evaluated based on the 100 μm equivalent transmittance, which is the measured transmittance t (%) of the laminate of the polarizer and the adhesive sheet converted to the transmittance at a thickness of 100 μm. If the total thickness of the adhesive sheet and the polarizer is L (μm) and the measured transmittance is t (%), according to Lambert's law, the 100 μm equivalent transmittance T (%), t (%) and L (μm) satisfy the following relationship. log 10 (T / 100)=(100 / L)×log 10 (t / 100)
[0023] The transmittance change is evaluated using the 100μm equivalent transmittance T0 at a wavelength of 380nm, the 100μm equivalent transmittance T1 at a wavelength of 450nm, the 100μm equivalent transmittance T2 at a wavelength of 520nm, the 100μm equivalent transmittance T3 at a wavelength of 580nm, and the 100μm equivalent transmittance T4 at a wavelength of 660nm. The wavelength of 380nm is in the ultraviolet region, the wavelength of 450nm corresponds to blue light, the wavelength of 520nm corresponds to green light, the wavelength of 580nm corresponds to yellow light, and the wavelength of 660nm corresponds to red light.
[0024] The 100 μm equivalent transmittances of the sample at wavelengths of 380 nm, 450 nm, 520 nm, 580 nm, and 660 nm after subjecting the laminate of the polarizer and the adhesive sheet to a moist heat test in which the laminate is left in an environment at a temperature of 85°C and a relative humidity of 85% for 100 hours are designated as T0', T1, T2', T3', and T4', respectively.
[0025] The change in transmittance before and after the heat and humidity test is mainly due to the fading of the polarizer. In the case of polyvinyl alcohol polarizers that contain iodine, the polyvinyl alcohol polymer chains and polyiodine ions (I3 - and I5 - ) form a complex, and the polymer chains are oriented in a specific direction, which in turn aligns the polyiodine ions, providing polarizing performance. When the polarizer is exposed to a high-temperature, high-humidity environment, the structure of the polyiodine ions changes (for example, I5 - From I3 - The polarizer fades due to the following reasons: (change to 100μm), disturbance in the orientation of polyiodine ions, release of iodine outside the system (e.g. sublimation of I2), etc. If the adhesive sheet placed in contact with the polarizer has ultraviolet absorption properties, the change in transmittance due to the fading of the polarizer is small in the ultraviolet region. Therefore, the 100μm-equivalent transmittance T0 at a wavelength of 380nm of the sample before the moist heat test and the 100μm-equivalent transmittance T0' of the sample after the moist heat test can be used as a standard for evaluating the change in visible light transmittance.
[0026] The change in visible light transmittance is indicated by the index ΔT n =(T n '-T0') / (T n-T0), where n is an integer between 1 and 4, and n=1 is an index of the change in transmittance at a wavelength of 450 nm, n=2 is an index of the change in transmittance at a wavelength of 520 nm, n=3 is an index of the change in transmittance at a wavelength of 580 nm, and n=4 is an index of the change in transmittance at a wavelength of 660 nm.
[0027] For example, the change in transmittance at a wavelength of 450 nm (n=1) can be evaluated by the index ΔT1=(T1'-T0') / (T1-T0). (T1-T0) is the difference in the 100 μm-equivalent transmittance between the wavelengths of 450 nm and 380 nm of the sample before the moist heat test, and (T1'-T0') is the difference in the 100 μm-equivalent transmittance between the wavelengths of 450 nm and 380 nm of the sample after the moist heat test. If the ratio ΔT1 is 1, it means that the transmittance difference between the wavelengths of 450 nm and 380 nm does not change before and after the moist heat test. If ΔT1 is greater than 1, it means that the transmittance difference between the wavelengths of 450 nm and 380 nm has increased after the moist heat test, and if ΔT1 is less than 1, it means that the transmittance difference between the wavelengths of 450 nm and 380 nm has decreased after the moist heat test.
[0028] As described above, when the pressure-sensitive adhesive sheet has ultraviolet absorbing properties, the change in the transmittance at a wavelength of 380 nm before and after the moist heat test is small. When the polarizer fades, the transmittance of visible light increases, so the sample after the moist heat test tends to have a large difference in transmittance with a wavelength of 380 nm. Therefore, ΔT n is generally 1.00 or more, and ΔT n The smaller (closer to 1.00) the smaller the fading of the polarizer.
[0029] For each of n = 1 to 4 (i.e., wavelengths of 450 nm, 520 nm, 580 nm, and 660 nm), ΔT n It is important that ΔT is between 1.0 and 1.2 (especially between 1.00 and 1.20). n The upper limit is more preferably 1.15 or less, further preferably 1.10 or less, particularly preferably 1.05 or less, and may be 1.04 or less.
[0030] ΔT nWhen the ratio is 1.0 to 1.2, deterioration of the polarizer caused by external ultraviolet rays, heating, humidification, etc. is suppressed, and the polarizer has excellent durability. Therefore, the polarizer can be used under various conditions, and can exhibit high durability even under humid conditions in particular.
[0031] ΔT n In order to make ΔT 1.20 or less, for example, the composition of the adhesive can be adjusted. For example, the composition of the base polymer in the adhesive composition can be adjusted. In the case of an acrylic adhesive, it is preferable to reduce the ratio of polar monomers such as nitrogen-containing monomers and hydroxyl-containing monomers in the base polymer. In addition, adding an ultraviolet absorber to the adhesive composition can also reduce ΔT n This is useful for keeping the ratio below 1.20.
[0032] The change in transmittance before and after the heat and humidity test is ΔT n On the other hand, ΔT n Even if the transmittance change rate is large, if the rate of change in transmittance for each wavelength of visible light is constant, the transmitted light hue will not change significantly. n Even if is small, ΔT due to wavelength n If the variation is large, the change in the hue of the transmitted light is large, which may cause deterioration in visibility, such as coloring of the image in the image display device.
[0033] The ratio of the transmittance of a specific wavelength to the transmittance of all visible light is T n / ΣT i where i is an integer between 1 and 4, and ΣT i =T1+T2+T3+T4. For example, T1 / ΣT i is the 100 μm-equivalent transmittance of a wavelength of 450 nm relative to the sum of the 100 μm-equivalent transmittances of wavelengths of 450 nm, 520 nm, 580 nm, and 660 nm.
[0034] Percentage of transmittance of a specific wavelength before the damp heat test T n / ΣT i The ratio of transmittance of a specific wavelength after the heat and humidity test to n ' / ΣTi 'Ratio of δT n =(T n ' / ΣT i ') / (T n / ΣT i ) is an index showing how the ratio of transmittance of a specific wavelength to the total visible light changes, and δT n If n=1, it means that the ratio of the transmittance of a specific wavelength (for example, 450 nm when n=1) to the total visible light does not change before and after the moist heat test.
[0035] When ΔT1 is greater than 1, it means that the ratio of the transmittance at a wavelength of 450 nm increases after the wet heat test, and when ΔT1 is smaller than 1, it means that the ratio of the transmittance at a wavelength of 450 nm decreases after the wet heat test. n The closer to 1.00, the smaller the color change of the transmitted light caused by the fading of the polarizer is.
[0036] For each of n = 1 to 4 (i.e., for wavelengths of 450 nm, 520 nm, 580 nm, and 660 nm), ΔT n is preferably from 0.95 to 1.05, more preferably from 0.97 to 1.03, further preferably from 0.98 to 1.02, and particularly preferably from 0.99 to 1.01.
[0037] δT n When the ratio is 0.95 to 1.05, deterioration of the polarizer caused by external ultraviolet rays, heating, humidification, etc. can be further suppressed, and durability can be further improved. Therefore, the polarizer can be used under various conditions, and can exhibit high durability even under humid conditions in particular.
[0038] δT nIn order to bring ΔT within the range of 0.95 to 1.05, for example, the composition of the adhesive may be adjusted. For example, the composition of the base polymer in the adhesive composition may be adjusted, and in the case of an acrylic adhesive, it is preferable to reduce the ratio of polar monomers such as nitrogen-containing monomers and hydroxyl-containing monomers in the base polymer. In addition, it is also possible to include an ultraviolet absorber in the adhesive composition to reduce ΔT n is useful for keeping the value in the range of 0.95 to 1.05.
[0039] As above, for each of n = 1 to 4, ΔT n The smaller (closer to 1.00), the smaller the change in transmittance before and after the heat and humidity test. n The closer to 1.00, the smaller the color change of the transmitted light. For each of the samples in which a polarizer was attached to the pressure-sensitive adhesive sheet produced using the pressure-sensitive adhesive composition of the present invention, ΔT n is within the above range, and ΔT n is preferably within the above range.
[0040] [Adhesive composition] The adhesive composition constituting the adhesive sheet 21 is such that a sample in which a polarizer is attached to an adhesive sheet produced using the composition has the above-mentioned ΔT n and / or δT n The composition is not particularly limited as long as it has ΔT n and / or δT n In order to set the above range, it is preferable that the pressure-sensitive adhesive composition has ultraviolet shielding properties. For example, the pressure-sensitive adhesive composition contains an ultraviolet absorber, so that the pressure-sensitive adhesive composition can have ultraviolet absorbing properties and can shield ultraviolet rays.
[0041] <Base polymer> A pressure-sensitive adhesive composition generally contains a base polymer, such as an acrylic-based, silicone-based, polyester, polyurethane, polyamide, polyvinyl ether, vinyl acetate / vinyl chloride copolymer, modified polyolefin, epoxy-based, fluorine-based, or rubber-based polymer.
[0042] In particular, acrylic adhesives containing an acrylic polymer as the base polymer are preferred because they have excellent optical transparency and adhesion. In acrylic adhesives, the ratio of polar monomers such as hydroxyl group-containing monomers and nitrogen-containing monomers in the base polymer is reduced, thereby reducing the aforementioned ΔT n In the case of an acrylic pressure sensitive adhesive, the ratio of polar monomers such as nitrogen-containing monomers and hydroxyl-containing monomers in the base polymer can be reduced to 1.20 or less. n can be within the range of 0.95 to 1.05.
[0043] When the amount of the hydroxyl group-containing monomer in the base polymer is large, the hydrophilicity and moisture permeability of the adhesive sheet increase with an increase in the polarity of the polymer, and the polarizer placed in contact with the adhesive sheet is likely to fade under high temperature and high humidity. When the hydrophilicity and moisture permeability of the adhesive sheet are high, moisture from the external environment easily reaches the polarizer, and the orientation of the polymer chain constituting the polarizer is disturbed by moisture, and polyiodine ions are detached from the polymer chain, which is considered to be one of the causes of the fading of the polarizer. In addition, as the amount of the nitrogen-containing monomer in the base polymer increases, the polarizer placed in contact with the adhesive sheet is likely to fade. Since nitrogen atoms are easily coordinated to iodine, when the amount of nitrogen atoms contained in the base polymer of the adhesive sheet increases, the iodine fixed to the polymer chain of the polarizer is coordinated to the nitrogen atoms of the adhesive and detached from the polymer chain, which is considered to be one of the causes of the fading of the polarizer.
[0044] The amount of hydroxyl-containing monomers and nitrogen-containing monomers in the base polymer is small, which suppresses the fading of the polarizer. n and δT n can be within the above range.
[0045] The acrylic base polymer contains an alkyl (meth)acrylate ester as a main constituent monomer component. In this specification, "(meth)acrylic" means acrylic and / or methacrylic. As the alkyl (meth)acrylate ester, an alkyl (meth)acrylate ester having 1 to 20 carbon atoms in the alkyl group is preferably used. The alkyl group in the alkyl (meth)acrylate ester may be branched or may have a cyclic alkyl group (alicyclic alkyl group).
[0046] Specific examples of (meth)acrylic acid alkyl esters having a chain alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, and butyl (meth)acrylate. ) nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, isododecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.
[0047] Specific examples of the (meth)acrylic acid alkyl ester having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring such as isobornyl (meth)acrylate; and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring such as dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate. The (meth)acrylic acid alkyl ester having an alicyclic alkyl group may have a substituent on the ring such as 3,3,5-trimethylcyclohexyl (meth)acrylate.
[0048] The amount of the (meth)acrylic acid alkyl ester relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 60 parts by weight or more, more preferably 70 parts by weight or more, even more preferably 80 parts by weight or more, and may be 85 parts by weight or more, 90 parts by weight or more, or 92 parts by weight or more.
[0049] The acrylic base polymer preferably contains an acrylic monomer having a crosslinkable functional group as a copolymerization monomer component. By having the crosslinkable functional group in the base polymer, the base polymer can be reacted with a crosslinking agent to increase the cohesive strength of the pressure-sensitive adhesive and improve the adhesion reliability.
[0050] Examples of acrylic monomers having crosslinkable functional groups include hydroxyl group-containing monomers and carboxyl group-containing monomers. For example, when an isocyanate-based crosslinking agent is used, a crosslinking structure is introduced by the reaction between a hydroxyl group and an isocyanate group. When an epoxy-based crosslinking agent is used, a crosslinking structure is introduced by the reaction between a carboxyl group and an epoxy group. As described below, from the viewpoint of making the adhesive acid-free, it is preferable to use a hydroxyl group-containing monomer as a copolymerization component of the base polymer and introduce a crosslinking structure by an isocyanate-based crosslinking agent. When the base polymer contains a hydroxyl group-containing monomer as a monomer component, the crosslinking property of the base polymer is enhanced and the opacity of the adhesive in a high temperature and high humidity environment tends to be suppressed, resulting in a highly transparent adhesive.
[0051] Examples of hydroxyl group-containing monomers include (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. Among these, 2-hydroxyethyl acrylate (Tg of homopolymer: -15°C) and 4-hydroxybutyl acrylate (Tg of homopolymer: -32°C) are preferred because they contribute greatly to improving adhesive strength and can suppress clouding of the pressure-sensitive adhesive sheet in a high humidity environment.
[0052] The amount of the hydroxyl group-containing monomer relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 0.1 parts by weight or more, more preferably 0.5 parts by weight or more, and even more preferably 0.8 parts by weight or more, and may be 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more. By increasing the amount of the hydroxyl group-containing monomer, the unreacted functional groups of the crosslinking agent are reduced, so that the degree of crosslinking can be increased with a small amount of crosslinking agent, and the adhesion reliability can be improved.
[0053] On the other hand, if the amount of the hydroxyl group-containing monomer in the base polymer is excessively large, the polarity of the adhesive increases, and the polarizer 11 placed in contact with the adhesive sheet 21 is likely to fade, and this leads to a decrease in ΔT n and Δδ n Therefore, the amount of the hydroxyl group-containing monomer relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 8 parts by weight or less, more preferably 7 parts by weight or less, and may be 6 parts by weight or less, or 5 parts by weight or less.
[0054] The acrylic base polymer may contain monomer components other than those described above. The acrylic base polymer may contain, as monomer components, for example, vinyl ester monomers, aromatic vinyl monomers, epoxy group-containing monomers, vinyl ether monomers, and the like.
[0055] The acrylic base polymer may contain a nitrogen-containing monomer as a monomer component, such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylcarboxylic acid amides, N-vinylcaprolactam, acrylonitrile, and methacrylonitrile.
[0056] As the amount of the nitrogen-containing monomer used increases, the polarizer 11 placed in contact with the adhesive sheet 21 is more likely to fade, and this leads to a decrease in ΔT n and Δδ n The deviation from 1.00 tends to become large. Therefore, the amount of the nitrogen-containing monomer relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 5 parts by weight or less, more preferably 3 parts by weight or less, and may be 1 part by weight or less, 0.5 parts by weight or less, 0.1 parts by weight or less, or 0.05 parts by weight or less. The acrylic base polymer may not contain a nitrogen-containing monomer as a monomer component.
[0057] If the acid component contained in the adhesive sheet migrates to the polarizer, it may promote hydrolysis of polyvinyl alcohol, which may cause the polarizer to deteriorate. Therefore, the adhesive sheet 21 preferably has a low content of organic acid monomers (free organic acids) such as (meth)acrylic acid. In a thermosetting or photosetting polymer, the presence of unreacted residual monomers is inevitable. Therefore, in order to reduce the content of acid monomers in the adhesive sheet, it is preferable to reduce the amount of organic acid monomer components such as (meth)acrylic acid in the monomer components constituting the base polymer. The content of the carboxyl group-containing monomer relative to the total amount of 100 parts by weight of the constituent monomer components of the acrylic base polymer is preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, and even more preferably 0.1 parts by weight or less. It is preferable that the acrylic base polymer does not contain a carboxyl group-containing monomer as a monomer component.
[0058] Suppresses fading of polarizer 11 in high temperature and high humidity environments, and reduces ΔT n and Δδ n To bring the polarity closer to 1.00, the base polymer constituting the pressure-sensitive adhesive sheet 21 arranged in contact with the polarizer 11 preferably has low polarity. To reduce the polarity of the base polymer, it is preferable that the content of polar monomers such as nitrogen-containing monomers, hydroxyl group-containing monomers, and carboxyl group-containing monomers as constituent monomer components is small. The content of the polar monomer relative to 100 parts by weight of the total amount of the constituent monomer components of the acrylic base polymer is preferably 12 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 8 parts by weight or less, and may be 6 parts by weight or less, or 5 parts by weight or less.
[0059] The acrylic base polymer may not contain a polar monomer as a constituent monomer component. However, from the viewpoint of introducing a crosslinking structure by a thermal crosslinking agent such as an isocyanate-based crosslinking agent into the base polymer, it is preferable that the polar monomer such as a hydroxyl group-containing monomer is contained in an amount of 0.1 parts by weight or more. The content of the polar monomer relative to 100 parts by weight of the total amount of the constituent monomer components of the acrylic base polymer is more preferably 0.5 parts by weight or more, further preferably 0.8 parts by weight or more, and may be 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more.
[0060] The monomer components are polymerized by various known methods such as solution polymerization, emulsion polymerization, and bulk polymerization to obtain an acrylic base polymer. From the viewpoint of the balance of properties such as adhesive strength and holding power of the adhesive, and the cost, the solution polymerization method is preferable. As a solvent for solution polymerization, ethyl acetate, toluene, etc. are generally used. The solution concentration is usually about 20 to 80% by weight. As a polymerization initiator, a thermal polymerization initiator such as an azo initiator, a peroxide initiator, or a redox initiator combining a peroxide and a reducing agent (for example, a combination of a persulfate and sodium hydrogen sulfite, or a combination of a peroxide and sodium ascorbate) is preferably used. The amount of the polymerization initiator is not particularly limited, but for example, it is preferably about 0.005 to 5 parts by weight, more preferably about 0.02 to 3 parts by weight, based on 100 parts by weight of the total amount of the monomer components forming the base polymer.
[0061] A chain transfer agent may be used to adjust the molecular weight of the base polymer. The chain transfer agent receives radicals from the growing polymer chain to stop the elongation of the polymer, and the chain transfer agent that has received the radicals attacks the monomer to restart polymerization. Therefore, by using a chain transfer agent, it is possible to suppress an increase in the molecular weight of the base polymer without decreasing the radical concentration in the reaction system. As the chain transfer agent, for example, thiols such as α-thioglycerol, lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol are preferably used.
[0062] The amount of chain transfer agent used is not particularly limited, but if the amount of chain transfer agent used is too large, the molecular weight of base polymer decreases, and the processability and processing dimensional stability of the adhesive sheet before photocuring may decrease.Therefore, the amount of chain transfer agent used is preferably 1 part by weight or less, more preferably 0.3 parts by weight or less, even more preferably 0.15 parts by weight or less, and particularly preferably 0.1 parts by weight or less, based on 100 parts by weight of the total amount of the monomer components constituting the base polymer.
[0063] The weight average molecular weight of the acrylic base polymer is preferably 100,000 to 3,000,000, more preferably 250,000 to 2,000,000, and even more preferably 500,000 to 1,500,000. When a crosslinked structure is introduced into the acrylic base polymer, the molecular weight of the base polymer refers to the molecular weight before the introduction of the crosslinked structure.
[0064] <Cross-linked structure of base polymer> The acrylic base polymer preferably has a crosslinked structure. Methods for introducing a crosslinked structure into a base polymer generally include (1) a method in which a base polymer having a functional group capable of reacting with a crosslinking agent is polymerized, and then a crosslinking agent is added to react the base polymer with the crosslinking agent; and (2) a method in which a photopolymerizable multifunctional compound is included in the polymerization components of the base polymer to introduce a branched structure (crosslinked structure) into the polymer chain.
[0065] In the adhesive composition constituting the adhesive sheet 21 arranged in contact with the polarizer 11, the acrylic base polymer preferably has a crosslinked structure introduced by the above method (1). The adhesive composition constituting the adhesive sheet 21 may contain a photopolymerizable multifunctional compound and a photopolymerization initiator, and may be one in which the crosslinked structure of the above method (2) is introduced by photocuring after bonding the adhesive sheet 21 and the cover window 70 together. That is, the adhesive composition constituting the adhesive sheet 21 preferably has a base polymer with a crosslinked structure caused by a (thermal) crosslinking agent such as an isocyanate-based crosslinking agent, and may further be one in which a crosslinked structure caused by a photopolymerizable multifunctional compound (photocrosslinking agent) can be introduced by photocuring.
[0066] <Adhesive composition> A pressure-sensitive adhesive composition is prepared by mixing an acrylic base polymer with a crosslinking agent, a photopolymerizable multifunctional compound, a photopolymerization initiator, and, if necessary, an oligomer or various additives. The pressure-sensitive adhesive composition preferably has a viscosity (for example, about 0.5 to 20 Pa·s) suitable for application onto a substrate. The viscosity of the pressure-sensitive adhesive composition can be adjusted to an appropriate range by adjusting the molecular weight of the base polymer, the amount of the photopolymerizable multifunctional compound added, and the composition, molecular weight, and amount added of other components (for example, oligomers). A thickening additive or the like may be used for the purpose of viscosity adjustment or the like.
[0067] (UV absorber) The adhesive sheet 21 preferably has ultraviolet absorbing properties. In a polarizing plate in which a transparent protective film is provided on the viewing side surface of the polarizer, the transparent protective film generally has ultraviolet absorbing properties to suppress deterioration of the polarizer due to ultraviolet rays incident from outside the display device. On the other hand, in a configuration in which the adhesive sheet 21 is disposed in contact with the viewing side surface of the polarizer 11, since no transparent protective film is provided on the viewing side of the polarizer, the adhesive sheet 21 is provided with ultraviolet absorbing properties to suppress photodeterioration of the polarizer 11 caused by ultraviolet rays (for example, structural changes in polyiodine ions (I5 - From I3 - It is preferable to prevent color change of the polarizer due to the change to a transparent state or the like.
[0068] In order to impart ultraviolet absorbing properties to the adhesive sheet 21, the adhesive composition preferably contains an ultraviolet absorbing agent. Examples of ultraviolet absorbing agents include benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, triazine-based ultraviolet absorbing agents, salicylate-based ultraviolet absorbing agents, and cyanoacrylate-based ultraviolet absorbing agents. Triazine-based ultraviolet absorbing agents and benzotriazole-based ultraviolet absorbing agents are preferred because they have high ultraviolet absorbing properties, are highly compatible with acrylic polymers, and are easy to use to obtain highly transparent acrylic adhesives. Among these, triazine-based ultraviolet absorbing agents containing a hydroxyl group and benzotriazole-based ultraviolet absorbing agents having one benzotriazole skeleton in one molecule are preferred.
[0069] Commercially available products may be used as the ultraviolet absorber. Commercially available triazine-based ultraviolet absorbers include the reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl and [(alkyloxy)methyl]oxirane (BASF's "TINUVIN 400"), the reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester (BASF's "TINUVIN 405"), (2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (BASF's "TINUVIN 460"), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol (BASF "TINUVIN 577"), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (BASF "TINUVIN 479"), 5,5'-bis(2-ethylhexyloxy)-2,2'-[6-(4-methoxyphenyl)-1,3,5-triazine-2,4-diyl]diphenol (BASF "Tinosorb S"), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (ADEKA "ADK STAB LA-46" and others.
[0070] Commercially available benzotriazole UV absorbers include 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "TINUVIN 928"), 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (BASF's "TINUVIN PS"), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (BASF's "TINUVIN 900"), and 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "TINUVIN 928"), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (BASF "TINUVIN 571"), 2-(2H-benzotriazol-2-yl)-p-cresol (BASF "TINUVIN P"), 2-(2H-benzotriazol-2-yl)-4-6-bis(1-methyl-1-phenylethyl)phenol (BASF "TINUVIN 234"), 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (BASF "TINUVIN 326"), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol (BASF "TINUVIN 328"), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF "TINUVIN 329"), benzenepropanoic acid and 3-(2H-benzotriazol-2-yl)-5-(1,Examples of such compounds include esters of 1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (BASF's "TINUVIN 384-2"), reaction products of methyl-3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate and polyethylene glycol (BASF's "TINUVIN 1 130"), reaction products of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (BASF's "TINUVIN 213"), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole (Sumitomo Chemical's "Sumisorb 250"), etc.
[0071] The content of the ultraviolet absorber in the adhesive composition is about 0.05 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 0.3 to 3 parts by weight, relative to 100 parts by weight of the base polymer. By setting the content of the ultraviolet absorber within the above range, it is possible to suppress a decrease in transparency due to bleeding out of the ultraviolet absorber, while imparting ultraviolet shielding properties to the adhesive sheet 21, thereby improving weather resistance and suppressing photodegradation of the polarizer caused by external ultraviolet rays.
[0072] (Crosslinking agent) As described above, the acrylic base polymer preferably has a crosslinked structure. The crosslinked structure is introduced into the base polymer by adding a crosslinking agent to the adhesive composition and heating it as necessary. In order to distinguish it from the crosslinked structure introduced by the photopolymerizable multifunctional compound, the crosslinking by the isocyanate crosslinking agent or the like may be described as "thermal crosslinking", but the introduction of the crosslinked structure by the crosslinking agent may not be accompanied by heating. By introducing a thermal crosslinked structure into the acrylic base polymer, the cohesiveness of the adhesive sheet is increased, and the adhesiveness tends to be improved.
[0073] Examples of the crosslinking agent include compounds that react with functional groups such as hydroxyl groups contained in the base polymer. Specific examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, and metal chelate-based crosslinking agents. Among these, isocyanate-based crosslinking agents are preferred because they have high reactivity with the hydroxyl groups of the base polymer and are easy to introduce a crosslinked structure.
[0074] As the isocyanate crosslinking agent, a polyisocyanate having two or more isocyanate groups in one molecule is used. Examples of the isocyanate crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; trimethylolpropane / Examples of isocyanate adducts include tolylene diisocyanate trimer adducts (e.g., "Coronate L" manufactured by Tosoh), trimethylolpropane / hexamethylene diisocyanate trimer adducts (e.g., "Coronate HL" manufactured by Tosoh), trimethylolpropane adducts of xylylene diisocyanate (e.g., "Takenate D110N" manufactured by Mitsui Chemicals, and isocyanurate of hexamethylene diisocyanate (e.g., "Coronate HX" manufactured by Tosoh).
[0075] The cohesive strength and adhesive strength of the pressure-sensitive adhesive can be adjusted by adjusting the amount of the crosslinking agent added. The amount of the crosslinking agent added is preferably 0.01 to 1 part by weight, more preferably 0.05 to 0.7 parts by weight, and even more preferably 0.1 to 0.5 parts by weight, relative to 100 parts by weight of the base polymer.
[0076] (Photopolymerizable polyfunctional compound) In order to impart photocurability to the adhesive sheet, the adhesive composition preferably contains a photopolymerizable multifunctional compound. The photopolymerizable multifunctional compound has two or more photopolymerizable functional groups in one molecule. The photopolymerizable functional group may be any of radical polymerizable, cationic polymerizable, and anionic polymerizable, but a radical polymerizable functional group having an unsaturated double bond (ethylenically unsaturated group) is preferable because of its excellent reactivity. As the photopolymerizable multifunctional compound, a multifunctional (meth)acrylate is preferable because of its high compatibility with an acrylic-based polymer, and a multifunctional acrylate is particularly preferable because of its high photoradical reactivity.
[0077] Examples of polyfunctional (meth)acrylates include hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, bisphenol A ethylene oxide modified di(meth)acrylate, bisphenol A propylene oxide modified di(meth)acrylate, alkanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, pentaerythritol di(meth)acrylate, neopentyl glycol di(meth)acrylate, and glycerin di(meth)acrylate. trifunctional (meth)acrylic acid esters such as pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated isocyanuric acid tri(meth)acrylate; tetrafunctional (meth)acrylic acid esters such as ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, and pentaerythritol tetra(meth)acrylate; and penta- or higher functional (meth)acrylic acid esters such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate.
[0078] From the viewpoint of improving the adhesive reliability of the pressure-sensitive adhesive sheet after photocuring, the molecular weight of the photopolymerizable multifunctional compound is preferably 1500 or less, and more preferably 1000 or less. The functional group equivalent (g / eq) of the multifunctional compound is preferably 50 to 500, more preferably 70 to 300, and even more preferably 80 to 200. In order to exhibit appropriate compatibility with the base polymer, the photopolymerizable multifunctional compound is preferably a liquid at room temperature.
[0079] The content of the photopolymerizable multifunctional compound in the adhesive composition is preferably 0.3 to 15 parts by weight, more preferably 0.5 to 10 parts by weight, and even more preferably 1 to 5 parts by weight, based on 100 parts by weight of the acrylic base polymer. When the content of the photopolymerizable multifunctional compound is low, the adhesive reliability of the adhesive sheet after photocuring tends to be insufficient. On the other hand, when the content of the photocurable multifunctional compound is excessively large, the ratio of the base polymer in the adhesive sheet (adhesive composition) before photocuring becomes small, and the processability and processing dimensional stability of the adhesive sheet may decrease. In addition, when the content of the photocurable multifunctional compound is excessively large, the adhesive sheet after photocuring becomes hard, and the adhesive strength and impact resistance of the adhesive sheet 21 at low temperatures may become insufficient.
[0080] (Photopolymerization initiator) The photocurable adhesive composition containing the photopolymerizable polyfunctional compound preferably contains a photopolymerization initiator. Examples of the photopolymerization initiator include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, and acylphosphine oxide-based photopolymerization initiators. The content of the photopolymerization initiator in the adhesive composition is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, based on 100 parts by weight of the base polymer.
[0081] (Oligomer) The pressure-sensitive adhesive composition may contain various oligomers for the purpose of adjusting the adhesive strength and viscosity of the pressure-sensitive adhesive sheet, etc. As the oligomer, for example, one having a weight average molecular weight of about 1000 to 30000 is used. As the oligomer, an acrylic oligomer is preferable because it has excellent compatibility with the acrylic base polymer.
[0082] The acrylic oligomer contains an alkyl (meth)acrylate ester as a main constituent monomer component. Among them, it is preferable to use an alkyl (meth)acrylate ester having a chain alkyl group (chain alkyl (meth)acrylate) and an alkyl (meth)acrylate ester having an alicyclic alkyl group (alicyclic alkyl (meth)acrylate) as the constituent monomer component. Specific examples of the chain alkyl (meth)acrylate and the alicyclic alkyl (meth)acrylate are as exemplified above as the constituent monomers of the acrylic base polymer.
[0083] The glass transition temperature of the acrylic oligomer is preferably 20°C or higher, more preferably 50°C or higher, even more preferably 80°C or higher, and particularly preferably 100°C or higher. The adhesive strength of the pressure-sensitive adhesive sheet tends to be improved by using a low Tg base polymer with a crosslinked structure introduced and a high Tg acrylic oligomer in combination. The upper limit of the glass transition temperature of the acrylic oligomer is not particularly limited, but is generally 200°C or lower, preferably 180°C or lower, and more preferably 160°C or lower. The glass transition temperature of the acrylic oligomer is calculated by the above-mentioned Fox formula.
[0084] Among the exemplified (meth)acrylic acid alkyl esters, methyl methacrylate is preferred as the chain alkyl (meth)acrylate because it has a high glass transition temperature and excellent compatibility with the base polymer. As the alicyclic alkyl (meth)acrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate, cyclohexyl acrylate, and cyclohexyl methacrylate are preferred. That is, the acrylic oligomer preferably contains, as a constituent monomer component, one or more selected from the group consisting of dicyclopentanyl acrylate, dicyclopentanyl methacrylate, cyclohexyl acrylate, and cyclohexyl methacrylate, and methyl methacrylate.
[0085] The amount of the alicyclic alkyl (meth)acrylate relative to the total amount of the monomer components constituting the acrylic oligomer is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and even more preferably 30 to 70% by weight. The amount of the chain alkyl (meth)acrylate relative to the total amount of the monomer components constituting the acrylic oligomer is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and even more preferably 30 to 70% by weight.
[0086] The weight average molecular weight of the acrylic oligomer is preferably from 1000 to 30000, more preferably from 1500 to 10000, and even more preferably from 2000 to 8000. By using an acrylic oligomer having a molecular weight within this range, the adhesive strength and adhesive retention of the pressure-sensitive adhesive sheet tend to be improved.
[0087] The acrylic oligomer can be obtained by polymerizing the above-mentioned monomer components by various polymerization methods. Various polymerization initiators may be used in the polymerization of the acrylic oligomer. In addition, a chain transfer agent may be used for the purpose of adjusting the molecular weight.
[0088] When the pressure-sensitive adhesive composition contains an oligomer component such as an acrylic oligomer, the content is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, relative to 100 parts by weight of the base polymer. When the content of the oligomer in the pressure-sensitive adhesive composition is within the above range, improvement in adhesion can be expected.
[0089] (Silane coupling agent) A silane coupling agent may be added to the pressure-sensitive adhesive composition for the purpose of adjusting adhesive strength, etc. When a silane coupling agent is added to the pressure-sensitive adhesive composition, the amount added is usually about 0.01 to 5.0 parts by weight, and preferably about 0.03 to 2.0 parts by weight, per 100 parts by weight of the base polymer.
[0090] (Antioxidants) The pressure-sensitive adhesive composition may contain an antioxidant. By containing an antioxidant, it is possible to suppress the reaction or deterioration of the curable component caused by heat or light in the storage environment or use environment of the pressure-sensitive adhesive composition or the pressure-sensitive adhesive sheet. Examples of the antioxidant include amine-based antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, and phenol-based antioxidants. Among them, those that act as radical chain inhibitors such as amine-based antioxidants and phenol-based antioxidants are preferred, and phenol-based antioxidants having a hindered phenol structure are particularly preferred.
[0091] Antioxidants having a hindered phenol structure have a group with large steric hindrance, such as a tert-butyl group, bonded to at least one of the carbon atoms adjacent to the carbon atom on the aromatic ring to which the OH group of phenol is bonded. Examples of antioxidants having a hindered phenol structure include dibutylhydroxytoluene (BHT), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (BASF's "Irganox 1010"), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (BASF's "Irganox 1076"), 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-triyl)tri-p-cresol (BASF's "Irganox 1076"). 1330"), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (BASF "Irganox 3114"), tris[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate (BASF "Irganox 3125"), pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (ADEKA "ADEKA STAB AO-60"), 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane (ADEKA "ADEKA STAB AO-80"), 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate (Sumitomo Chemical "Sumilizer GS"), 2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl acrylate (Sumitomo Chemical "Sumilizer GM"), 2,2'-dimethyl-2,2'-(2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diyl)dipropane-1,1'-diyl=bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoate] (Sumitomo Chemical's "Sumilizer GA-80"), 1,3,5-tris(3-hydroxy-4-tert-butyl-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (Cyanox 1790) and the like.
[0092] When the adhesive composition contains an antioxidant, the content of the antioxidant is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, even more preferably 0.1 parts by weight or more, and may be 0.3 parts by weight or more or 0.5 parts by weight or more, based on 100 parts by weight of the acrylic base polymer, from the viewpoint of suppressing undesired curing reaction or deterioration. On the other hand, if the content of the antioxidant is excessively high, it may cause curing inhibition when the adhesive sheet is photocured. Therefore, the content of the antioxidant is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 3 parts by weight or less, based on 100 parts by weight of the acrylic base polymer.
[0093] (Other additives) In addition to the above-exemplified components, the pressure-sensitive adhesive composition may contain additives such as a chain transfer agent, a tackifier, a plasticizer, a softener, an antidegradant, a filler, a colorant, a surfactant, and an antistatic agent.
[0094] [Formation of adhesive sheet] The adhesive composition is applied onto a substrate, and the solvent is dried and removed as necessary to form an adhesive sheet on the substrate. Any suitable substrate is used for forming the adhesive sheet. The substrate may be a release film having a release layer on the surface of a resin film.
[0095] Examples of the resin material of the release film include polyester resins such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, and polyphenylene sulfide resins. Among these, polyester resins such as polyethylene terephthalate are particularly preferred. The thickness of the release film is preferably 10 to 200 μm, and more preferably 25 to 150 μm. Examples of the material of the release layer include silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, and fatty acid amide-based release agents. The thickness of the release layer is generally about 10 to 2000 nm.
[0096] As a method for applying the pressure-sensitive adhesive composition onto a substrate, various methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coater can be used.
[0097] When the pressure-sensitive adhesive composition contains a solvent, it is preferable to dry the solvent after applying the pressure-sensitive adhesive composition onto the substrate. As the drying method, a suitable method can be adopted depending on the purpose. The heating and drying temperature is preferably 40°C to 200°C, more preferably 50°C to 180°C, and particularly preferably 70°C to 170°C. As the drying time, a suitable time can be adopted. The drying time is preferably 5 seconds to 20 minutes, more preferably 5 seconds to 15 minutes, and particularly preferably 10 seconds to 10 minutes.
[0098] After drying the solvent, it is preferable to attach a cover sheet to protect the surface of the pressure-sensitive adhesive sheet. As the cover sheet, it is preferable to use a release film having a release layer on the surface that comes into contact with the pressure-sensitive adhesive sheet, similar to the base film.
[0099] After the adhesive composition is applied onto the substrate, it is heated as necessary to introduce a crosslinked structure into the base polymer. The heating temperature and heating time may be appropriately set depending on the type of crosslinking agent used, and are usually in the range of 20°C to 160°C and about 1 minute to 7 days. The heating for drying the solvent may also serve as the heating for crosslinking. As mentioned above, the introduction of a crosslinked structure does not necessarily have to be accompanied by heating.
[0100] A crosslinking catalyst may be used to promote the formation of a crosslinked structure. For example, the crosslinking catalyst for the isocyanate-based crosslinking agent may be a metal-based crosslinking catalyst (especially a tin-based crosslinking catalyst) such as tetra-n-butyl titanate, tetraisopropyl titanate, nursem ferric, butyltin oxide, dioctyltin dilaurate, or dibutyltin dilaurate.
[0101] By laminating a release film on the surface of the adhesive sheet, an adhesive sheet having release films temporarily attached to both sides is obtained. The substrate or cover sheet used in forming the adhesive sheet may be used as the release film.
[0102] When release films are provided on both sides of the pressure-sensitive adhesive sheet, the thickness of one release film and the thickness of the other release film may be the same or different. The peeling force when peeling the release film temporarily attached to one side from the pressure-sensitive adhesive sheet and the peeling force when peeling the release film temporarily attached to the other side from the pressure-sensitive adhesive sheet may be the same or different.
[0103] The thickness of the adhesive sheet 21 used to attach the polarizer 11 and the cover window 70 is preferably 30 μm or more, more preferably 40 μm or more, and even more preferably 50 μm or more. By increasing the thickness of the adhesive sheet 21, impact resistance tends to increase. Furthermore, when the cover window 70 has a printing step due to decorative printing, the adhesive sheet 21 can be made to have step absorption properties. There is no particular upper limit on the thickness of the adhesive sheet 21, but from the viewpoint of the productivity of the adhesive sheet, etc., it is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less.
[0104] The total light transmittance of the pressure-sensitive adhesive sheet 21 is preferably 85% or more, and more preferably 90% or more. The haze of the pressure-sensitive adhesive sheet is preferably 1.5% or less, and more preferably 1% or less.
[0105] The optical transmittance of the adhesive sheet 21 at a wavelength of 380 nm is preferably 5% or less, more preferably 4% or less, and may be 3% or less. By increasing the ultraviolet shielding property of the adhesive sheet 21, the weather resistance is improved and photodegradation such as yellowing of the polarizer 11 caused by ultraviolet light incident from the outside can be suppressed. As described above, by including an ultraviolet absorbing agent in the adhesive composition, the adhesive sheet 21 can be made ultraviolet absorbing while maintaining the transparency of visible light.
[0106] [Polarizing plate] <Polarizer> The polarizing plate 10 includes a polarizer 11. The polarizer 11 is, for example, a polyvinyl alcohol-based film containing iodine. As a material for the polyvinyl alcohol-based film applied to the polarizer, polyvinyl alcohol or a derivative thereof is used. Examples of the polyvinyl alcohol derivative include polyvinyl formal, polyvinyl acetal, etc., as well as those modified with olefins such as ethylene and propylene, unsaturated carboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, their alkyl esters, acrylamide, etc. Polyvinyl alcohol having a degree of polymerization of about 1000 to 10000 and a degree of saponification of about 80 to 100 mol % is generally used.
[0107] A polarizer is obtained by subjecting a polyvinyl alcohol-based film to iodine dyeing and stretching treatment. The thickness of the polarizer is preferably about 1 to 50 μm. A thin polarizer having a thickness of 10 μm or less can also be used as the polarizer. Examples of the thin polarizer include polarizers described in JP-A-51-069644, JP-A-2000-338329, WO2010 / 100917, Japanese Patent No. 4691205, Japanese Patent No. 4751481, etc. Such a thin polarizer can be obtained, for example, by a manufacturing method including a step of stretching a polyvinyl alcohol-based resin layer and a resin substrate for stretching in a laminate state, and a step of dyeing with iodine.
[0108] <Optical layer> No optical layer is provided on the first main surface (the surface on the viewing side) of the polarizer 11, and as described above, the adhesive sheet 21 is provided in contact with the polarizer 11. The polarizing plate 10 may be composed of only the polarizer 11, or an appropriate optical layer 15 may be disposed on the second main surface (the surface on the image display cell 60 side) of the polarizer 11.
[0109] The optical layer 15 may be a transparent protective film for protecting the polarizer 11, or may have a function such as an optical compensation layer for the purpose of widening the viewing angle, or a quarter-wave plate for constituting a circular polarizing plate together with the polarizer 11. The optical layer 15 may have both a function as a transparent protective film and a function as a retardation plate.
[0110] Examples of materials constituting the optical layer 15 include resin materials having excellent transparency, mechanical strength, and thermal stability. Specific examples of such resin materials include cellulose-based resins such as triacetyl cellulose, polyester-based resins, polyethersulfone-based resins, polysulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, cyclic polyolefin-based resins (norbornene-based resins), polyarylate-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, and mixtures thereof. The optical layer 15 may be a liquid crystal material. For example, the optical layer 15 may be a liquid crystal layer in which liquid crystal molecules are aligned in a predetermined direction.
[0111] The optical layer 15 may be in direct contact with the second main surface of the polarizer 11, or may be attached via an appropriate adhesive layer. The optical layer 15 may be a laminate of two or more layers. For example, the optical layer 15 may be a laminate of two or more films, a laminate in which a liquid crystal layer is provided on a film substrate, or a laminate in which two or more liquid crystal layers are laminated. The optical layer 15 may include an alignment film for aligning liquid crystal molecules in a predetermined direction.
[0112] [Polarizing plate with adhesive] The adhesive sheet 21 may be provided as an adhesive-attached polarizing plate 81 integrally laminated with the polarizing plate 10, as shown in Fig. 2. In the adhesive-attached polarizing plate, the adhesive sheet 21 is disposed in contact with a first main surface of the polarizer 11. In Fig. 2, an optical layer 15 is provided on the second main surface of the polarizer 11, but as described above, the polarizing plate 10 does not need to have an optical layer on the second main surface of the polarizer.
[0113] There is no particular limitation on the method for attaching the adhesive sheet 21 onto the first main surface of the polarizer 11. The adhesive sheet 21, which has been prepared in advance on a base material, may be attached onto the polarizer 11, or the adhesive sheet 21 may be formed using the polarizer 11 as a base material.
[0114] In the polarizing plate 81 with adhesive, a release film 41 is preferably removably attached onto the adhesive sheet 21. The release film has a function of protecting the exposed surface of the adhesive sheet 21 until the adhesive sheet 21 is attached to the cover window 70. The base material used in forming (applying) the adhesive sheet may be used as it is as the release film 41 on the adhesive sheet 21.
[0115] 3, the polarizing plate with adhesive may be a double-sided adhesive polarizing plate having an adhesive sheet 21 in contact with the polarizer 11 on the viewing side surface of the polarizing plate 10, and another adhesive sheet 22 on the other side of the polarizing plate. It is preferable that a release film 42 is removably attached on the adhesive sheet 22.
[0116] 3, a polarizing plate 10 has an optical layer 15 on the second main surface of a polarizer 11, and an adhesive sheet 22 is disposed on the optical layer 15. The adhesive sheet 22 may be laminated on the second main surface of the polarizer 11 in contact with the polarizer 11 without any other layer therebetween.
[0117] In this way, by using a double-sided adhesive polarizing plate in which an adhesive layer has already been applied to both sides of the polarizing plate 10, the process of attaching a separate adhesive sheet to the polarizing plate after bonding the polarizing plate to the surface of the image display cell can be omitted, and the manufacturing process of the image display device can be simplified.
[0118] The adhesive sheet 22 is used to bond the polarizing plate 10 and the image display cell 60 together. The thickness of the adhesive sheet 22 is preferably 3 μm to 30 μm, more preferably 5 μm to 27 μm, and even more preferably 10 μm to 25 μm. As the adhesive sheet 22, various adhesives used to bond a polarizing plate and an image display cell can be used. As the adhesive constituting the adhesive sheet 22, an acrylic adhesive is preferably used.
[0119] When the adhesive polarizing plate, in which the adhesive sheet 21 is arranged in contact with one side of the polarizer 11, is subjected to a wet heat test in which it is left in an environment of a temperature of 85°C and a relative humidity of 85% for 100 hours, it is preferable that all of ΔT1, ΔT2, ΔT3, and ΔT4 satisfy 1.00 to 1.20. ΔT1, ΔT2, ΔT3, and ΔT4 are as defined above. ΔT n is preferably 1.15 or less, more preferably 1.10 or less, particularly preferably 1.05 or less, and may be 1.04 or less for each of n=1 to 4. n The closer the value is to 1.00, the less the polarizer fades and the more excellent the resistance to moisture and heat is.
[0120] When the adhesive polarizing plate, in which the adhesive sheet 21 is arranged in contact with one side of the polarizer 11, is subjected to a wet heat test in which it is left in an environment of a temperature of 85°C and a relative humidity of 85% for 100 hours, it is preferable that all of ΔT1, ΔT2, ΔT3, and ΔT4 satisfy 0.95 to 1.05. ΔT1, ΔT2, ΔT3, and ΔT4 are as defined above. ΔT n is more preferably 0.97 to 1.03, further preferably 0.98 to 1.02, and particularly preferably 0.99 to 1.01 for each of n=1 to 4. n The closer it is to 1.00, the smaller the color change of the transmitted light is.
[0121] The polarizing plate with adhesive, in which the adhesive sheet 21 is arranged in contact with one side of the polarizer 11, has a thickness of ΔT n is within the above range, and ΔT n is preferably in the above range.
[0122] [Image display device] 1, the image display device 100 includes a cover window 70 attached to the viewing side of a polarizing plate 10 via an adhesive sheet 21. An image display cell 60 such as a liquid crystal cell or an organic EL cell is attached to the other surface of the polarizing plate 10 via an adhesive sheet 22. The image display cell 60 may be foldable.
[0123] A transparent plate having appropriate mechanical strength and thickness is used as the cover window 70. For example, a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate is used as such a transparent plate. When the image display cell 60 is foldable, the cover window 70 may also be foldable. The cover window may be a laminate of a plurality of transparent films with an adhesive or a bonding agent interposed therebetween, and may include a touch panel sensor. As the touch panel sensor, any type of touch panel such as a resistive film type, a capacitive type, an optical type, or an ultrasonic type is used.
[0124] There is no particular limitation on the order of bonding the polarizing plate 10 and the cover window 70 with the adhesive sheet 21 and bonding the adhesive sheet 22 and the image display cell 60. As described above, an adhesive-attached polarizing plate in which an adhesive sheet is attached in advance to the surface of the polarizing plate may be used.
[0125] After the polarizing plate 10 and the cover window 70 are bonded together via the adhesive sheet 21, degassing may be performed to remove air bubbles at the bonding interface and near the printing step. As a degassing method, a suitable method such as heating, pressurization, or decompression may be used. For example, bonding may be performed under reduced pressure and heating while suppressing the inclusion of air bubbles, and then heating and pressurization may be performed simultaneously by autoclaving or the like in order to suppress delay bubbles, etc.
[0126] When the adhesive sheet 21 is made of a photocurable adhesive composition, the adhesive composition is photocured after bonding the polarizing plate 10 and the cover window 70. The light irradiation causes a polymerization reaction of the photopolymerizable multifunctional compound, which increases the adhesion reliability of the adhesive sheet.
[0127] The amount of light irradiated during photocuring is not particularly limited as long as the adhesive sheet can be photocured, and for example, the cumulative light amount is 50 to 10,000 mJ / cm 2The adhesive sheet 21 may be irradiated with light from either the polarizing plate 10 side or the cover window 60 side, but from the viewpoint of preventing deterioration of the polarizer 11 due to ultraviolet rays, it is preferable to irradiate the ultraviolet rays from the cover window 10 side. If the adhesive sheet 21 has ultraviolet shielding properties, even when ultraviolet rays are irradiated to photo-cure the adhesive sheet 21, most of the ultraviolet rays are absorbed by the adhesive sheet 21, so that the amount of ultraviolet rays irradiated to the polarizer can be reduced.
[0128] In the image display device 100, the adhesive composition used to form the adhesive sheet 21 disposed in contact with the viewing side of the polarizer 11 has the properties as described above. Therefore, an image display device including the adhesive sheet 21 has excellent durability with little deterioration such as fading or yellowing of the polarizer even when exposed to a high-temperature and high-humidity environment or to external light for a long period of time. EXAMPLES
[0129] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0130] [Examples 1 to 3 and Comparative Examples 1 and 2] <Polymerization of base polymer> In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube, the monomer components (total 100 parts by weight) in the ratio shown in Table 1 and azobisisobutyronitrile (AIBN) as a thermal polymerization initiator were charged together with 233 parts by weight of ethyl acetate, and the mixture was stirred for 1 hour in a nitrogen atmosphere at 23°C, followed by nitrogen substitution. The mixture was then reacted at 56°C for 5 hours, and then at 70°C for 3 hours to prepare an acrylic-based polymer solution.
[0131] In Table 1, the monomers are described by the following abbreviations. BA: Butyl acrylate 2EHA: 2-Ethylhexyl acrylate 4HBA: 4-hydroxybutyl acrylate
[0132] <Preparation of Pressure-Sensitive Adhesive Composition> The following components were added to the acrylic base polymer solution obtained above in the amounts shown in Table 1 per 100 parts by weight of the base polymer, and then mixed uniformly to prepare a pressure-sensitive adhesive composition. Isocyanate crosslinking agent: Trimethylolpropane adduct of xylylene diisocyanate ("Takenate D110N" manufactured by Mitsui Chemicals) UV absorber: 5,5'-bis(2-ethylhexyloxy)-2,2'-[6-(4-methoxyphenyl)-1,3,5-triazine-2,4-diyl]diphenol (BASF "Tinosorb S")
[0133] <Preparation of adhesive sheet> The above photocurable adhesive composition was applied onto a release film (a polyethylene terephthalate film with a silicone-based release layer on one side), heated at 100°C for 3 minutes to remove the solvent, and then another release film was attached to the surface. This laminate was aged in an atmosphere of 25°C for 3 days to promote crosslinking, and an adhesive sheet with release films temporarily attached to both sides was obtained.
[0134] [Preparation of adhesive sheet A] In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube, 97 parts by weight of butyl acrylate and 3 parts by weight of acrylic acid as monomer components, and 0.2 parts by weight of AIBN as a thermal polymerization initiator were added together with 233 parts by weight of ethyl acetate, and the mixture was stirred for 1 hour under a nitrogen atmosphere at 23°C to perform nitrogen substitution. After that, the mixture was reacted for 5 hours at 60°C to obtain a solution of an acrylic base polymer having a weight average molecular weight (Mw) of 1.1 million. To this base polymer solution, 0.8 parts by weight of trimethylolpropane tolylene diisocyanate ("Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd.) as an isocyanate crosslinking agent and 0.1 parts by weight of a silane coupling agent ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.) were added, and the mixture was mixed uniformly to prepare a pressure-sensitive adhesive composition solution.
[0135] The above pressure-sensitive adhesive composition was applied onto a release film so that the thickness after drying would be 20 μm, and after drying for 3 minutes at 100° C. to remove the solvent, another release film was attached to the surface. This laminate was aged in an atmosphere at 50° C. for 2 days to promote crosslinking, and a pressure-sensitive adhesive sheet A with release films temporarily attached to both sides was obtained.
[0136] [evaluation] A polarizer made of a 25 μm-thick stretched polyvinyl alcohol film impregnated with iodine was attached to a first non-alkali glass plate via an adhesive sheet A. A second non-alkali glass plate was attached thereon via the adhesive sheets of the examples and comparative examples to prepare evaluation samples.
[0137] (Weather resistance test) Using an ultraviolet fade meter (U48AU manufactured by Suga Test Instruments), the temperature was 40°C, the relative humidity was 20%, and the radiation intensity (300-700 nm integrated illuminance) was 500±50W / m 2 The weather fade test was carried out by irradiating the second non-alkali glass plate with carbon arc lamp light for 100 hours under the conditions of * 0 and the b of the transmitted light of the sample after the test * Difference from 1 Δb * =b * 1-b * In addition, b * is the chromaticity index b of the CIE1976 color space * The measurement was performed by placing a sample on a backlight.
[0138] (Damp heat test) The transmittance spectrum of the evaluation sample was measured using a visible-ultraviolet spectrophotometer, and the initial transmittances t0, t1, t2, t3, and t4 at wavelengths of 380 nm, 450 nm, 520 nm, 580 nm, and 660 nm were read. The evaluation sample was held in a thermohygrostat at a temperature of 85°C and a relative humidity of 85% for 100 hours to conduct a moist heat test. The transmittance spectrum of the sample before and after the moist heat test was measured, and the transmittances t0', t1', t2', t3', and t4' at wavelengths of 380 nm, 450 nm, 520 nm, 580 nm, and 660 nm were read.
[0139] From the measured transmittance value t, the 100 μm equivalent transmittance T was calculated based on the following formula in accordance with Lambert's law, converting the total thickness L = 125 μm of the polarizer (25 μm) and adhesive sheet (100 μm) into the transmittance at a thickness of 100 μm. log 10 (T / 100)=(100 / L)×log 10 (t / 100)
[0140] T0: 100μm-equivalent transmittance at a wavelength of 380nm before the wet heat test T1: 100μm equivalent transmittance at a wavelength of 450nm before the wet heat test T2: 100μm equivalent transmittance at a wavelength of 520nm before the wet heat test T3: 100μm equivalent transmittance at a wavelength of 580nm before the wet heat test T4: 100μm equivalent transmittance at a wavelength of 660nm before the wet heat test T0': 100μm equivalent transmittance at a wavelength of 380nm after moist heat test T1': 100μm equivalent transmittance at a wavelength of 450nm after moist heat test T2': 100μm equivalent transmittance at a wavelength of 520nm after moist heat test T3': 100μm equivalent transmittance at a wavelength of 580nm after moist heat test T4': 100μm equivalent transmittance at a wavelength of 660nm after moist heat test
[0141] From the 100μm-equivalent transmittances T0 to T4 before the above-mentioned heat and humidity test and the 100μm-equivalent transmittances T0' to T4' after the heat and humidity test, the following ΔT n and δT n (n=1-4) was calculated. ΔTn=(T n '-T0') / (T n -T0) δTn=(T n ' / ΣT i ') / (T n / ΣT i ) where i=1~4
[0142] The adhesive composition of each adhesive sheet and the evaluation results are shown in Table 1. The numerical values in the adhesive composition in Table 1 are the blending amounts (parts by weight). For Comparative Example 2, Δb * Since the temperature exceeded 5%, which meant that the weather resistance was not acceptable, a damp heat test was not performed.
[0143] [Table 1]
[0144] As shown in Table 1, the pressure-sensitive adhesive sheets of Examples 1 to 3 have a Δb * is small and has good weather resistance, and ΔT n and δT n was close to 1.00 for all of n=1 to 4, and the polarizer had little fading and excellent resistance to moisture and heat. [Explanation of symbols]
[0145] 10 Polarizing plate 11 Polarizer 15 Optical layer 21,22 Adhesive sheet 81,82 Polarizing plate with adhesive 60 Image display cells 70 Cover Window 100 Image display device
Claims
1. A polarizing plate with an adhesive comprising: a polarizer having a first principal surface and a second principal surface; and a first adhesive sheet disposed in contact with the first principal surface of the polarizer, the first adhesive sheet is used for bonding to a cover window of an image display device, the first pressure-sensitive adhesive sheet is made of a pressure-sensitive adhesive composition including an acrylic base polymer and 0.05 to 10 parts by weight of an ultraviolet absorber relative to 100 parts by weight of the acrylic base polymer; The acrylic base polymer contains a nitrogen-containing monomer, a hydroxyl group-containing monomer, and a carboxyl group-containing monomer in a total amount of 8 parts by weight or less relative to 100 parts by weight of the total of the monomer components, When subjected to a moist heat test in which the material is left in an environment of 85° C. and 85% relative humidity for 100 hours, the ΔT 1 , ΔT 2 , ΔT 3 and ΔT 4 A polarizing plate with an adhesive, in which all of the above satisfy 1.0 to 1.2: ΔT n = (T n '-T 0 ') / (T n -T 0 ) n is an integer from 1 to 4, T 0 is the 100 μm-equivalent transmittance at a wavelength of 380 nm before the wet heat test, T 1 is the 100 μm-equivalent transmittance at a wavelength of 450 nm before the wet heat test, T 2 is the 100 μm-equivalent transmittance at a wavelength of 520 nm before the wet heat test, T 3 is the 100 μm-equivalent transmittance at a wavelength of 580 nm before the wet heat test, T 4 is the 100 μm-equivalent transmittance at a wavelength of 660 nm before the wet heat test, T 0 ' is the 100 μm equivalent transmittance at a wavelength of 380 nm after the wet heat test, T 1' is the 100 μm equivalent transmittance at a wavelength of 450 nm after the wet heat test, T 2 ' is the 100 μm equivalent transmittance at a wavelength of 520 nm after the wet heat test, T 3 ' is the 100 μm equivalent transmittance at a wavelength of 580 nm after the wet heat test, T 4 ' is the 100 μm equivalent transmittance at a wavelength of 660 nm after the wet heat test, The 100 μm converted transmittance T (%), the total thickness L (μm) of the pressure-sensitive adhesive sheet and the polarizer, and the measured transmittance t (%) are log 10 (T / 100)=(100 / L)×log 10 (t / 100) Satisfy the relationship.
2. An adhesive polarizing plate comprising: a polarizer having a first principal surface and a second principal surface; and a first adhesive sheet disposed in contact with the first principal surface of the polarizer, the first adhesive sheet is used for bonding to a cover window of an image display device, the first pressure-sensitive adhesive sheet is made of a pressure-sensitive adhesive composition including an acrylic base polymer and 0.05 to 10 parts by weight of an ultraviolet absorber relative to 100 parts by weight of the acrylic base polymer; The acrylic base polymer contains a nitrogen-containing monomer, a hydroxyl group-containing monomer, and a carboxyl group-containing monomer in a total amount of 8 parts by weight or less relative to 100 parts by weight of the total of the monomer components, When left in an environment of 85°C and 85% relative humidity for 100 hours, the δT 1 , δT 2 , δT 3 and δT 4 A pressure-sensitive adhesive composition, wherein all of δT n = (T n ' / ΣT i ') / (T n / ΣT i ) n and i are integers from 1 to 4; T 0 is the 100 μm-equivalent transmittance at a wavelength of 380 nm before the wet heat test, T 1 is the 100 μm-equivalent transmittance at a wavelength of 450 nm before the wet heat test, T 2 is the 100 μm-equivalent transmittance at a wavelength of 520 nm before the wet heat test, T 3 is the 100 μm-equivalent transmittance at a wavelength of 580 nm before the wet heat test, T 4 is the 100 μm-equivalent transmittance at a wavelength of 660 nm before the wet heat test, T 0 ' is the 100 μm equivalent transmittance at a wavelength of 380 nm after the wet heat test, T 1 ' is the 100 μm equivalent transmittance at a wavelength of 450 nm after the wet heat test, T 2 ' is the 100 μm equivalent transmittance at a wavelength of 520 nm after the wet heat test, T 3 ' is the 100 μm equivalent transmittance at a wavelength of 580 nm after the wet heat test, T 4 ' is the 100 μm equivalent transmittance at a wavelength of 660 nm after the wet heat test, The 100 μm converted transmittance T (%), the total thickness L (μm) of the pressure-sensitive adhesive sheet and the polarizer, and the measured transmittance t (%) are log 10 (T / 100)=(100 / L)×log 10 (t / 100) Satisfy the relationship.
3. An adhesive-attached polarizing plate as described in claim 1 or 2, wherein the acrylic base polymer contains 0.1 parts by weight or more of hydroxy group-containing monomer per 100 parts by weight of the total of the monomer components.
4. An adhesive-attached polarizing plate as described in claim 3, wherein the acrylic-based polymer has a cross-linked structure formed by an isocyanate-based cross-linking agent.
5. The polarizing plate with adhesive according to any one of claims 1 to 4, further comprising a second adhesive sheet on a second main surface side of the polarizer.
6. The polarizing plate with adhesive according to claim 5 , wherein the second adhesive sheet is laminated in contact with a second main surface of the polarizer.
7. The polarizing plate with adhesive according to claim 5 , wherein the second adhesive sheet is laminated on a second main surface of the polarizer via another layer.
8. An image display device comprising a second adhesive sheet, the adhesive-attached polarizing plate according to any one of claims 1 to 7, and a cover window, in this order, on a surface of an image display cell, The image display device, wherein the first adhesive sheet of the adhesive-attached polarizing plate is attached to the cover window.
Citation Information
Patent Citations
Production of polarizing film
JP1994337311A
Polarization film with adhesive layer on both sides, and image formation apparatus
JP2017003906A
Polarizing plate with adhesive and image display device
JP2019139007A
Optical member and image display device
JP2020064160A
Double-sided pressure-sensitive-adhesive-layer-attached polarizing film, and image display device