Coated copper material stripping treatment method, treatment device, treatment device control unit, and program
The use of sulfuric acid with persulfuric acid to dissolve and electrolyze insulation coatings on copper materials addresses inefficiencies in existing methods, enhancing copper recovery yield and reducing environmental impact.
Patent Information
- Application Number
- JP2024068266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2044-04-19
AI Technical Summary
Existing methods for peeling off insulation coatings from copper materials are inefficient, leading to low peeling rates, high equipment and processing costs, purity loss due to high temperatures, and environmental concerns from chemical stripping solutions, with limited use and increased waste treatment costs.
A method involving the use of a sulfuric acid solution, preferably with persulfuric acid, to dissolve and decompose the coating material, followed by electrolysis to regenerate the solution for reuse, with monitoring of decomposition state through electrical conductivity and redox potential.
Achieves high-purity copper recovery with improved yield and reduced environmental impact by efficiently removing insulation coatings while minimizing energy costs and waste treatment burdens.
Smart Images

Figure 0007572696000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for stripping a coated copper material, a processing device, a processing device control unit, and a program for stripping and removing a coating material from a copper material coated with the coating material. [Background technology]
[0002] Copper wire is widely used in automobiles, home appliances, industrial applications, etc. However, copper is a resource that is expected to run out in about 40 years, and there are concerns that it will run out. In addition, in copper mines, the grade of copper concentrate has been gradually declining in recent years, and it is said that the burden on the mining and smelting processes is increasing. In the automotive industry, there is a sudden movement toward recycling materials and parts used, mainly among European manufacturers, and there is also a demand for copper recovery from copper wire used in windings.
[0003] Copper wires are often covered with resin that has insulating properties, and in copper recovery, it is necessary to peel off the covering material from the copper wire. Currently, the covering material of some copper wires for winding is peeled off by a dry method. In one dry method, the wire is cut with a rotating blade, then crushed with opposing rolling rollers that roll it, and separated based on the difference in specific gravity (Patent Document 1). As another treatment method, Patent Document 2 discloses a recovery method in which a resin-coated copper wire is heat-treated at 250° C. to 380° C. in an air atmosphere, and the thermally denatured insulating coating is mechanically peeled off.
[0004] As for recycling by a wet method, Patent Document 3 discloses a recovery method in which the material is heated at 500°C to 800°C using superheated steam, and then washed with 10 to 35 mass % hydrochloric acid to remove the material, and Patent Document 4 discloses a recovery method in which the material is chemically removed using a stripping solution containing an inorganic alkali, an alkanolamine having 1 to 10 carbon atoms, and water. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5828145 specification [Patent Document 2] Patent No. 6604515 specification [Patent Document 3] Patent No. 6056088 Specification [Patent Document 4] JP 2021-108531 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in Patent Documents 1 and 2, the peeling rate of the coating material is low at about 97% due to contamination with insulating coating components, and recycling requires processing starting from the smelting process. In Patent Document 3, after heating at 500°C to 800°C using superheated steam, the wire is chemically stripped using hydrochloric acid. These conventional techniques require many processing steps due to the high heat treatment temperature and the need for mechanical or chemical removal after heating, resulting in high equipment and processing costs. Furthermore, there is a problem that the purity is impaired by the formation of oxides on the copper wire due to the high temperature heat treatment. Furthermore, Patent Document 4 raises issues such as the cleanliness of the copper wire after stripping, and makes no mention of the state of the solution after stripping, raising concerns about the insulating film removing ability of the stripping / removal solution as the number of uses increases.
[0007] When recovering high-purity copper wire, further issues include the cleanliness of the copper wire after stripping and the yield of the copper wire during stripping. In addition, the challenge in this field is to completely remove the insulating film while reducing energy costs and carbon dioxide emissions during recovery. Chemical removal methods are effective as a method for solving these challenges, but there is also the problem that the number of times the solution can be used is limited because the used solution contains dissolved insulating film components and the peeling and removal ability decreases as the number of times it is used increases. Furthermore, in disposing of the used stripping / removal solution, the following problems can easily be imagined as the number of stripping / removal treatments increases. (1) Increased costs for waste liquid treatment and replacement, and collection and transportation costs (2) Increased wastewater treatment costs due to multiple wastewater treatment processes (3) Increased environmental impact from waste liquid treatment to replacement and regeneration
[0008] The present invention has been made in consideration of the above-mentioned conventional problems, and aims to provide a recovery method, etc., which can recover high-purity copper material from coated copper material with a high yield using only chemical treatment and can autolyze the coating material components dissolved in the used solution. [Means for solving the problem]
[0009] That is, in the first form of the method for stripping a coated copper material, a coating material coated on a copper material is brought into contact with a sulfuric acid solution, the coating material is dissolved in the sulfuric acid solution, and the coating material is stripped and removed from the copper material, and the coating material dissolved in the sulfuric acid solution is decomposed by an electrolytic sulfuric acid solution containing persulfuric acid.
[0010] In another aspect of the invention, in the above aspect of the invention, the concentration of persulfuric acid in the electrolytic sulfuric acid solution is 0.5 g / L or more.
[0011] In another aspect of the invention, in the above aspect of the invention, the sulfuric acid solution in which the coating material has been decomposed is reused for peeling and removing the coated copper material or other coated copper materials.
[0012] In another embodiment of the invention, in the above embodiment of the invention, the sulfuric acid solution brought into contact with the coating material coating the copper material has a persulfuric acid concentration of less than 0.5 g / L, a sulfuric acid concentration of 85.0 mass% or more, and a temperature within the range of 60 to 140°C.
[0013] In another embodiment of the present invention, in the above-mentioned embodiment, the sulfuric acid solution to be brought into contact with the coating material coated on the copper material is an electrolytic sulfuric acid solution having a persulfuric acid concentration of 0.5 g / L or more in a part or all of the peeling and removing process, and the sulfuric acid concentration is 80.0 mass% or more and the temperature is within the range of 60 to 140°C.
[0014] According to another aspect of the invention, in the above aspect of the invention, the electrolytic sulfuric acid solution is electrolyzed at a solution temperature of 20 to 60°C.
[0015] The decomposition state of the coating material is judged by one or both of the electrical conductivity and the oxidation-reduction potential of the sulfuric acid solution.
[0016] When the decomposition state of the coating material reaches a standard, the regeneration is judged to be complete, and the regenerated sulfuric acid solution is used to peel off and remove the coated copper material.
[0017] The invention of the coated copper material peeling and removal treatment device has a sulfuric acid solution contact section that brings the coating material of the coated copper material into contact with a sulfuric acid solution, and a decomposition section that decomposes the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution.
[0018] The invention of another aspect is the invention of the above aspect, wherein the sulfuric acid solution contact portion includes an immersion treatment tank for immersing the coated copper material in a sulfuric acid solution and a material The sulfuric acid solution is discharged into one or both of the discharge and contact tanks for contacting the sulfuric acid solution with the
[0019] In another aspect of the invention, in the above aspect, the decomposition section is provided with an electrolysis section that electrolyzes a sulfuric acid solution.
[0020] In another aspect of the invention, in the above aspect of the invention, a plurality of the sulfuric acid solution contact parts are provided, and one or more of the electrolysis parts are capable of selectively electrolyzing the sulfuric acid solutions in the plurality of the sulfuric acid solution contact parts.
[0021] In another aspect of the invention, in the above aspect, the decomposition section includes a decomposition storage tank and an electrolysis section, and an electrolysis circulation path for circulating a sulfuric acid solution between the decomposition storage tank and the electrolysis section.
[0022] In another aspect of the invention, in the above aspect, a decomposition / regeneration liquid transfer path is provided between the sulfuric acid solution contact section and the decomposition storage tank.
[0023] Another aspect of the invention is the above-mentioned aspect of the invention, comprising a measurement unit that measures the decomposition state of the sulfuric acid solution in the decomposition unit; Electrolysis in the electrolysis section, the circulation path for electrolysis, and the liquid supply path for decomposition and regeneration Control the A control unit is provided. The control unit receives the measurement result of the measurement unit and performs the control based on the measurement result. of Determine the content.
[0024] Another embodiment of the stripping device control unit is provided in a treatment device having a measuring unit for measuring the decomposition state of a coating material in a sulfuric acid solution containing persulfuric acid, a sulfuric acid solution contact unit for dissolving the coating material of the coated copper material by contacting it with the sulfuric acid solution to strip and remove it, a decomposition storage tank for decomposing the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution, a decomposition / regeneration liquid supply path provided between the sulfuric acid solution contact unit and the decomposition storage tank, an electrolysis unit for electrolyzing the sulfuric acid solution, and an electrolysis circulation path for circulating the sulfuric acid solution between the decomposition storage tank and the electrolysis unit, Upon receiving the measurement result from the measuring section, the electrolysis section is controlled to control the electrolysis, the electrolysis circulation path, and the decomposition / regeneration liquid supply path. Control the , receiving the measurement result, and controlling the of Control is exercised in determining the content.
[0025] Another aspect of the program invention is a program executed by a control unit which receives a measurement result from a measurement unit which measures the decomposition state of a coating material in a sulfuric acid solution containing persulfuric acid, and controls a sulfuric acid solution contact unit which dissolves the coating material of the coated copper material by contacting it with the sulfuric acid solution to peel off and remove it, and a decomposition storage tank which decomposes the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution, a liquid feed through a decomposition / regeneration liquid feed path provided between the decomposition storage tank and the sulfuric acid solution contact unit, electrolysis in an electrolysis unit which electrolyzes the sulfuric acid solution, and a liquid feed through an electrolysis circulation path which circulates the sulfuric acid solution between the decomposition storage tank and the electrolysis unit, The program includes a step of sending the sulfuric acid solution in which the coating material has been dissolved in the sulfuric acid solution contact portion to a decomposition storage tank through a decomposition / regeneration liquid sending path; receiving the measurement results; Executing electrolysis by the electrolysis unit and sending the solution through the electrolysis circuit until the measurement result reaches a reference; When the measurement result reaches a reference value, electrolysis by the electrolysis unit is stopped, and the sulfuric acid solution in the decomposition storage tank is sent to the sulfuric acid solution contact unit through the decomposition / regeneration liquid sending path. The control unit executes the process. Effect of the Invention
[0026] According to the present invention, by contacting the coating material of the coated copper material with a sulfuric acid solution, the coating material can be peeled off and removed from the copper material, and a high-purity copper material can be recovered. The dissolved coating material is decomposed by an electrolytic sulfuric acid solution containing persulfuric acid. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an apparatus used in an embodiment of the present invention. [Diagram 2] FIG. 1 is a process flow diagram illustrating an embodiment of a method for stripping and removing an insulating film and a method for regenerating a stripping solution according to the present invention. [Diagram 3] FIG. 11 is a schematic cross-sectional view showing an example of an apparatus used in another embodiment. [Figure 4] 10 is a flowchart showing the procedure of an electrolysis / regeneration step in another embodiment. [Diagram 5] FIG. 13 is a flow diagram illustrating an embodiment in which an electrolytic sulfuric acid solution is used as the solution that is brought into contact with the coating material to strip and remove it. [Figure 6] FIG. 11 is a schematic cross-sectional view showing an example of an apparatus used in another embodiment of the present invention. [Figure 7] This is a process flow when multiple stripping tanks are prepared. [Figure 8] FIG. 11 is a schematic cross-sectional view showing an example of an apparatus used in still another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] (Embodiment 1) FIG. 1 is a schematic cross-sectional view showing an example of an apparatus used in one embodiment of the present invention, and shows a treatment apparatus applicable to a method for stripping a resin coating material coated on a copper material and a method for regenerating a sulfuric acid solution after the stripping.
[0029] Copper materials having a high purity (for example, 99.96% or more) can be preferably used, and examples thereof include wire and plate shapes, but the shape is not limited to a specific one.
[0030] The coating material may be a coating film having a small thickness relative to the surface area of the copper material, and is preferably used, for example, as a material having insulation and heat resistance. Examples of insulating materials include those having a large volume electrical resistivity (10 7 The heat resistance required varies depending on the application, but the preferred application of the present invention is heat resistance class B (130° C.) or higher as specified in JIS standard C4003.
[0031] The coating material may be either a natural resin or a synthetic resin, and may be either a thermoplastic resin or a thermosetting resin, and is not limited to a specific resin. The coating material may be, for example, any of polyimide resin, polyesterimide resin, polyamideimide resin, polyurethane resin, and polyester resin. The coating material is not limited to one type, and may be a plurality of types, for example, a laminate of layers of different materials.
[0032] The coating material may cover the entire copper material, or may cover only a part of the copper material (in the cross-sectional or longitudinal direction). Examples of the coating material include those formed in the form of a film on the surface of the copper material, but the thickness is not limited. In the following embodiment, a copper wire is used as the copper material.
[0033] The treatment device 1 has a treatment tank 5 that contains a sulfuric acid solution, and the treatment tank 5 immerses the resin-coated copper wire 2 in the sulfuric acid solution to peel off the coating material.
[0034] The treatment device 1 also includes an electrolytic sulfuric acid device 6 that electrolyzes a sulfuric acid solution to decompose the peeled material. The treatment tank 5 is one form of the sulfuric acid contact section of the present invention, and corresponds to an immersion contact tank. The electrolytic treatment device 6 constitutes a part of the decomposition section of the present invention, and corresponds to the electrolysis section. In this embodiment, the treatment tank 5 serves as a decomposition storage tank in the decomposition section.
[0035] In the treatment tank 5, stirring means such as an external air pump 4 and an air bubble generator 3 connected thereto may be provided in order to stir the inside of the tank as necessary. An electrolytic sulfuric acid device 6 for regenerating the sulfuric acid solution is connected to the treatment tank 5. A solution inlet path 9A and one end of a solution outlet path 9B are disposed in the treatment tank 5 in a connected state, allowing the solution to be introduced into the treatment tank 5 and the solution to be discharged from the treatment tank 5. The inlet path 9A and the outlet path 9B constitute an electrolytic circulation path.
[0036] The other ends of the solution inlet path 9A and the outlet path 9B are connected to the liquid passage of the electrolytic cell 10, and a circulation pump 8 is provided in the solution outlet path 9B. By operating the circulation pump 8 to send the solution to the electrolytic cell side, the solution is sent to the outlet path 9B, the electrolytic cell 10, the inlet path 9A, and the treatment tank 5, enabling the solution to circulate.
[0037] In the electrolysis cell 10, a solution outlet path 9B is connected to the lower end of the cell, and a solution inlet path 9A is connected to the upper end of the cell, with an anode 10A and a cathode 10B installed in the flow path between them, and a bipolar electrode 10C installed between the anode 10A and the cathode 10B, so that the solution moves from bottom to top in the flow path between the electrodes. A DC power supply 7 for electrolysis is provided between the anode 10A and the cathode 10B.
[0038] In this embodiment, a device having a bipolar electrode has been described, but the present embodiment is not particularly limited to the presence or absence of a bipolar electrode.
[0039] In this embodiment, the device shown in FIG. 1 is used. However, the method of electrolysis is not particularly limited, and is not limited to the device shown in FIG.
[0040] <Flowchart> FIG. 2 is a flow chart showing the steps of the method for peeling and removing resin and the method for decomposing and regenerating a sulfuric acid solution according to the present invention, which will be described below.
[0041] Here, the method mainly includes a stripping process as a first step in which the coating material is stripped and removed from the surface of the copper wire 2 using a sulfuric acid solution, which is an acidic stripping solution, and a stripping solution regeneration process as a second step in which the sulfuric acid solution is electrolyzed to produce peroxodisulfuric acid through electrolysis, and peroxomonosulfuric acid and other oxidants produced by the self-decomposition of peroxodisulfuric acid react with organic matter, which is a component of the coating material, and the organic matter is decomposed into carbon dioxide and water.
[0042] In the initial stripping step (step S1), a sulfuric acid solution is placed in a treatment tank 5. The sulfuric acid solution is preferably adjusted to have a sulfuric acid concentration of 85 mass % or more and a temperature within a range of 60 to 140°C. It is even more preferable to set the lower limit at 90°C and the upper limit at 100°C. The temperature of the sulfuric acid solution can be adjusted by heating it using a heater (not shown) installed in the tank. The copper wire 2 on which a coating material (not shown) is formed is immersed in this sulfuric acid solution to bring the resin coating material into contact with the sulfuric acid solution.
[0043] In addition, if the sulfuric acid concentration of the sulfuric acid solution is increased, the degree of dissociation of sulfuric acid decreases, and as a result, the ion concentration in the solution decreases. In other words, the solution becomes hydrophobic and it becomes possible to dissolve the coating material covering the copper wire. Since it is not possible to take a long time to peel and remove the coating material industrially, it is preferable to set the lower limit of the sulfuric acid concentration in the sulfuric acid solution to 85.0 mass%. However, when electrolyzing the sulfuric acid solution in a later process, it is preferable to set the sulfuric acid concentration to 94.0 mass% or less from the viewpoint of electrolysis efficiency.
[0044] In addition, increasing the temperature of the sulfuric acid solution increases the dissolution rate. For this reason, it is desirable to set the temperature of the sulfuric acid solution and electrolytic sulfuric acid solution that are brought into contact with the insulating coating of the coating material to 60°C or higher. For the same reason, it is desirable to set it to 90°C or higher. On the other hand, if the solution temperature becomes too high, oxides will form on the copper wire, reducing the purity and causing the copper wire to dissolve, resulting in a decrease in recovery yield. For this reason, it is desirable to set the solution temperature to 140°C or lower. Furthermore, for the same reason, it is desirable to set it to 100°C or lower.
[0045] Here, the sulfuric acid solution may be sulfuric acid itself or a sulfate, etc., as long as the sulfuric acid concentration described above can be obtained. As for the solution for peeling and removing the coating material, a sulfuric acid solution containing persulfuric acid can be used as described later, but in this form, the action of persulfuric acid is not required, so a persulfuric acid-free solution or one with a persulfuric acid concentration of less than 0.5 g / L is used.
[0046] When the copper wire 2 covered with the covering material is immersed, air can be sent from an external air pump 4 to the air bubble generator 3 to appropriately agitate the sulfuric acid solution. In the copper wire 2 covered with a covering material, the covering material is gradually peeled off and removed by contact with the sulfuric acid solution, and the covering material dissolves in the sulfuric acid solution.
[0047] Once the coating material has been removed from the copper wire 2, the copper wire 2 undergoes a cleaning and drying process (step S2). In the cleaning and drying process (step S2), the copper wire 2 from which the coating material has been peeled off is taken out of the treatment tank 5, washed with a cleaning solution (not shown), and dried. The cleaned and dried copper wire 2 can be recycled while maintaining its purity and achieving a high recovery rate. For example, the purity of the copper wire can be 99.96% or more, and the recovery rate can be 98% or more. In recycling, for example, a process can be adopted in which recovered copper wire is melted and refined to produce copper wire with high purity.
[0048] The sulfuric acid solution in which the coating material is dissolved is electrolyzed by the electrolytic sulfuric acid device 6 in the electrolytic sulfuric acid solution generating step (step S3). In the electrolytic sulfuric acid solution generating process, the circulation pump 8 is operated to circulate the sulfuric acid solution in the treatment tank 5 through the delivery line 9B, the electrolytic cell 10, the introduction line 9A, and the treatment tank 5. In the delivery line 9B, a cooler (not shown) or the like is provided to adjust the temperature of the sulfuric acid solution to 20 to 60° C. as a desirable electrolysis condition.
[0049] If the solution temperature during electrolysis is less than 20°C, the diffusion rate of ions to the anode surface is slow, and increasing the current density will cause the diamond used in the electrode to wear out. On the other hand, if the temperature during electrolysis is more than 60°C, adverse effects such as the self-decomposition rate of the oxidant increasing and the reduction of the oxidant at the cathode will occur. Therefore, it is desirable to keep the temperature range between 20 and 60°C.
[0050] In the electrolysis cell 10, a voltage is applied between the anode 10A and the cathode 10B by the DC power supply for electrolysis 7 to pass a current, and the sulfuric acid solution flowing through the flow path is electrolyzed by the anode 10A, the cathode 10B, and the bipolar electrode 10C to produce an electrolytic sulfuric acid solution such as peroxodisulfuric acid. The generated electrolytic sulfuric acid solution can be supplied to the treatment tank 5 via the inlet line 9A, and the process can proceed to the sulfuric acid solution regeneration step (step S4). In the regeneration process of the sulfuric acid solution, it is desirable to increase the oxidizing power of the electrolytic sulfuric acid solution supplied to the treatment tank 5 by heating it to 60 to 140°C using a heater installed in the inlet 9A or a heater installed in the treatment tank 5. If the temperature is less than 60°C, the self-decomposition rate of the oxidizing agent is slow, and if the temperature exceeds 140°C, the self-decomposition rate is too fast.
[0051] In the treatment tank 5 where the electrolytic sulfuric acid solution is introduced, peroxodisulfuric acid (SO2O8 2- ) and peroxomonosulfuric acid (HSO5 - The organic matter, which is a component of the coating material dissolved in the sulfuric acid solution, reacts with sulfuric acid (SO2) and hydrogen peroxide (H2O2), breaking it down into carbon dioxide and water, regenerating the sulfuric acid solution. The regenerated sulfuric acid solution can then be used again to peel off and remove the coating material from another copper wire with a resin coating. In addition, when decomposing coating materials, it is desirable for the persulfuric acid concentration to be 0.5 g / L or higher. If the concentration is less than 0.5 g / L, the decomposition efficiency of the coating material is insufficient. On the other hand, since the released persulfuric acid reacts immediately with organic matter, the persulfuric acid concentration can only rise to about 5.0 g / L. In order to exceed 5.0 g / L, a large number of electrolytic cells would be required, which is not practical from a cost perspective.
[0052] The present invention will now be described chemically. The process in which the coating material dissolves in the electrolyzed sulfuric acid solution is a phenomenon in which the hydrophobic insulating coating dissolves and diffuses in the hydrophobic sulfuric acid solution, that is, it is a physical phenomenon, and there is no chemical reaction formula. The chemical reaction formula when sulfuric acid solution is electrolyzed is shown below. From formula (1), when sulfuric acid solution is electrolyzed, hydrogen sulfate ions (HSO4 - ) reacts with peroxodisulfate (SO8 2- ) is produced. Peroxodisulfate is unstable, so it is converted to peroxomonosulfate (HSO5 - ) and hydrogen peroxide (H2O2) (equations (2) and (3)), and there are three types of oxidants in the electrolytic sulfuric acid solution. 2HSO4 - → 2H + + S2O8 2- + 2e - (1) S2O8 2- + H2O → HSO5 - + HSO4 - (2) HSO5 - + H2O → HSO4 - + H2O2(3) Next, the reaction in which the insulating film, which is an organic material, reacts with an oxidizing agent such as peroxodisulfuric acid and decomposes into carbon dioxide and water will be described.
[0053] By generating an electrolytic sulfuric acid solution, the resin is decomposed into sulfate radicals and hydroxyl radicals as shown in formulas (4) to (5). The generated sulfate radicals and hydroxyl radicals completely oxidize and decompose the resin components in the stripping and removal solution as shown in formulas (6) to (7). S2O82- → 2SO4 - (4) 2SO4 - + 2H2O → 2HSO4 - + 2OH· (5) C, H + 2SO4 - · → 2HSO4- + xCO2+ yH2O (6) C, H + 2OH· → xCO2+ yH2O (7)
[0054] [Reduction in decomposition rate of coating materials] The decomposition rate of the insulating coating material decreases with increasing resin concentration in the sulfuric acid solution or electrolytic sulfuric acid solution, and also decreases with decreasing oxidizing agent concentration. When the organic coating material dissolves, the electrical conductivity decreases as the concentration of the insulator organic material increases. Therefore, the organic material concentration can be estimated from the electrical conductivity, and the decomposition rate can be determined. There are methods to directly analyze the organic material concentration, but incorporating such a method into the equipment would be too expensive, so this method makes it easier to determine the concentration. The oxidizing agent reacts with the organic matter and decomposes the organic matter into carbon dioxide and water. Therefore, it is important to balance the oxidizing agent generation rate and the organic matter dissolution rate. If the oxidizing agent generation rate is slower than the organic matter dissolution rate, the organic matter concentration in the sulfuric acid solution or electrolytic sulfuric acid solution will gradually increase, and eventually the organic matter will no longer dissolve. By measuring the redox potential of the solution, the amount (concentration) of the oxidizing agent can be grasped, and the decomposition rate of the coating material can be determined. Therefore, the measurement unit for measuring the decomposition state of the sulfuric acid solution is preferably one that measures either the electrical conductivity or the redox potential of the sulfuric acid solution, or both.
[0055] (Embodiment 2) 3 shows an example of a treatment apparatus 1A in which a measurement unit 11 for measuring electrical conductivity or redox potential is provided in a treatment tank 5. Electrical conductivity can be measured with a conductivity meter, and redox potential can be measured with a redox potentiometer. Note that the same reference numerals are used to designate the same components as those described above, and description thereof will be omitted. As the decomposition proceeds, the electrical conductivity increases, and when it reaches a predetermined reference value, it can be determined that the decomposition has ended. With respect to the oxidation-reduction potential, as the decomposition progresses, the oxidation-reduction potential increases, and when the oxidation-reduction potential reaches a predetermined reference value, it can be determined that the decomposition is complete.
[0056] The measurement results of the measurement unit 11 are received by the control unit 20 and can be used to control the electrolytic cell 10 and the circulation pump 8. Until the measurement results of the measurement unit 11 reach a predetermined standard, the operation of the electrolytic cell 10 and the circulation pump 8 continues, and when the measurement results reach the standard, the regeneration is completed and the operation of the electrolytic cell 10 and the circulation pump 8 can be stopped. At that time, a notification can be given via a display unit or the like, and depending on the device configuration, the sulfuric acid solution in the treatment tank 5 may be moved, for example. In this embodiment, the measurement unit 11 has been described as measuring the electrical conductivity or the redox potential of the sulfuric acid solution, but the present disclosure is not limited to this, and the configuration is not particularly limited as long as it can measure the decomposition state of the coating material in the sulfuric acid solution.
[0057] FIG. 4 is a flow chart showing the electrolytic sulfuric acid solution generating process and regenerating process. Electrolysis is started based on the electrolytic sulfuric acid solution production process, and the process proceeds to the regeneration process (steps s3, 4). Next, measurement is performed by the measuring device 11 (step s5), and the measurement result is received by the control unit 20. The control unit 20 compares the measured value with a predetermined reference value stored in the memory unit and determines whether the measured value has reached the reference value (step s6). If the measured value has not reached the reference value (step s6, No), electrolysis and regeneration are continued (to step s3). If the measured value has reached the reference value (step s6, Yes), regeneration is deemed to be completed, and electrolysis and operation of the circulation pump are stopped. Thereafter, the sulfuric acid solution can be reused if desired.
[0058] (Embodiment 3) Next, a third embodiment in which the coating material coated on the copper wire 2 is stripped and removed with a sulfuric acid solution containing persulfuric acid by using the treatment device 1 will be described with reference to the flow chart of FIG.
[0059] First, the electrolytic sulfuric acid solution generating step (step S10) is carried out. A sulfuric acid solution is contained in the treatment tank 5. In this case, the sulfuric acid solution preferably has a sulfuric acid concentration of 80 mass % or more. The difference between the sulfuric acid solution in the first embodiment and the electrolytic sulfuric acid solution in the second embodiment is the presence or absence of a strong oxidizing agent, and when an oxidizing agent is present, the dissolution rate increases due to its oxidizing power. Therefore, when peeling and removing a coating material with a sulfuric acid solution containing persulfuric acid, it is preferable to set the lower limit of the sulfuric acid concentration to 80 mass% or more. As with the sulfuric acid solution, the dissolution rate increases as the solution temperature is increased, so it is desirable to set the temperature of the electrolytic sulfuric acid solution to 60°C or higher. For the same reason, 90°C or higher is desirable. On the other hand, it is possible to lower the sulfuric acid concentration, which increases the recovery rate of the copper wire.
[0060] In the electrolytic sulfuric acid solution generating process, the circulation pump 8 is operated to circulate the sulfuric acid solution in the treatment tank 5 through the discharge line 9B, the electrolytic cell 10, the introduction line 9A, and the treatment tank 5. In the discharge line 9B, a cooler (not shown) or the like is provided to adjust the temperature of the sulfuric acid solution being sent to a temperature of 20 to 60° C. The temperature of the solution contained in the treatment tank 5 may be adjusted to this temperature.
[0061] In the electrolysis cell 10, a voltage is applied between the anode 10A and the cathode 10B by the DC power supply for electrolysis 7 to pass a current, and the sulfuric acid solution flowing through the flow path is electrolyzed by the anode 10A, the cathode 10B, and the bipolar electrode 10C to produce an electrolytic sulfuric acid solution such as peroxodisulfuric acid.
[0062] The produced electrolytic sulfuric acid solution is supplied to treatment tank 5 via introduction line 9A. When the sulfuric acid solution in the treatment tank 5 is generated as an electrolytic sulfuric acid solution, the process proceeds to a resin peeling step (step S11). Electrolysis by the electrolytic sulfuric acid device 6 is continued even during the resin peeling step. In this embodiment, a device having a bipolar electrode has been described, but the present embodiment is not particularly limited to the presence or absence of a bipolar electrode.
[0063] In this embodiment, the device shown in Fig. 1 is used, but the method of electrolysis is not particularly limited and is not limited to the device shown in Fig. 1. For example, in each of the above embodiments, the treatment tank 5 and the electrolysis cell 10 are prepared, but it is also possible to use a common tank to perform stripping removal and decomposition. However, it is more efficient to perform stripping removal and electrolysis in separate devices (tanks).
[0064] In the peeling and removing process (step S11) of the coating material , covered The copper wire 2 covered with the covering material is immersed in the electrolytic sulfuric acid solution. At this time, the temperature of the electrolytic sulfuric acid solution is preferably heated to 60° C. or higher.
[0065] The electrolyzed sulfuric acid solution comes into contact with the coating material on the copper wire 2, thereby effectively peeling and removing the coating material from the copper wire 2. The electrolytic sulfuric acid solution has a stronger oxidizing power than a sulfuric acid solution that does not contain an oxidizing agent, so it can uniformly and thinly oxidize the copper wire surface, suppressing excessive oxidation, and allowing the coating material to be peeled and removed while maintaining the purity of the copper wire at a high level.
[0066] Furthermore, the stripped material removed from the coated copper wire dissolves in the electrolytic sulfuric acid solution. The copper wire from which the coating material has been peeled off is transferred to a cleaning and drying step as in the above embodiment (copper wire cleaning and drying step; step S12). At the same time, in the electrolytic sulfuric acid solution dissolved therein, the coating site-utilizing components are decomposed by the oxidizing agent in the electrolytic sulfuric acid solution, and the sulfuric acid solution is regenerated (sulfuric acid solution regeneration step; step S13). According to this embodiment, the coating material can be stripped off from the copper wire and the components of the coating material dissolved in the electrolytic sulfuric acid solution can be decomposed at the same time, so that the treatment can be carried out efficiently.
[0067] (Embodiment 4) In each of the above embodiments, the coated copper material was contacted with the sulfuric acid solution by immersing the coated copper material in the sulfuric acid solution, but the coated material can be contacted with the sulfuric acid solution by any suitable method, such as spraying or flowing the sulfuric acid solution. 6 shows a treatment device 1B in which a nozzle 12 for spraying a sulfuric acid solution downward is provided in a treatment tank 5. The treatment tank 5 in this embodiment is the sulfuric acid solution contact section in the present disclosure, and corresponds to a release contact tank. Note that the same reference numerals are used for the same components as in the above embodiment, and the description thereof will be omitted or simplified.
[0068] The copper wire 2 coated with a coating material is placed on a stage 13 below the nozzle 12, and a sulfuric acid solution is sprayed downward from the nozzle 12 to bring the coating material into contact with the sulfuric acid solution. The coating material is peeled off and removed from the copper wire 2, and is transferred from the treatment tank 5A to the decomposition storage tank 14 via the transfer line 15A. The peeled off coating material dissolves in the sulfuric acid solution. This sulfuric acid solution can be electrolyzed in the electrolytic sulfuric acid device 6, decomposed with a sulfuric acid solution containing persulfuric acid solution, and regenerated, as in the above-mentioned embodiment. The regenerated sulfuric acid solution can be sent to the nozzle 12 via the return line 15B by the liquid sending pump 16 and used in the peeling and removing process. The feed line 15A and the return line 15B constitute a decomposition / regeneration liquid feed path.
[0069] (Embodiment 5) In each of the above-mentioned first embodiments, the embodiment having one treatment tank has been described, but the embodiment having a plurality of treatment tanks may also be used. A fifth embodiment will be described with reference to FIG. In this embodiment, there are two treatment tanks, a first treatment tank 5A and a second treatment tank 5B, and one electrolytic sulfuric acid device 6. The first treatment tank 5A and the second treatment tank 5B are each connected to the electrolytic sulfuric acid device 6 via an inlet path and an outlet path, and the first treatment tank 5A and the second treatment tank 5B can be connected to the electrolytic sulfuric acid device 6 by switching the inlet path and the outlet path. The electrolytic sulfuric acid device 6 is provided with an anode, a cathode, a bipolar electrode, and a DC power supply for electrolysis, as in the first embodiment.
[0070] In this embodiment, one treatment tank, for example, the first treatment tank 5A, is used to immerse the copper wire coated with the coating material in a sulfuric acid solution to peel off and remove the coating material (A in FIG. 7). When the decomposition rate of the coating film in the first treatment tank 5A decreases, it is determined that the peeling and removal capacity is insufficient, and the copper wire is removed. The sulfuric acid solution is circulated between the copper wire and the electrolytic sulfuric acid device 6, and electrolytic sulfuric acid is generated in the electrolytic sulfuric acid device 6, whereby the coating film components are decomposed and sulfuric acid is regenerated. Meanwhile, in the other second treatment tank 5B, a sulfuric acid solution is stored in the treatment tank, and another copper wire covered with a coating film is immersed in the sulfuric acid solution to peel off and remove the coating film (FIG. 7B). When the solubility in the second treatment tank 5B decreases in this state, the copper wire is removed, and the coating components are decomposed and sulfuric acid is regenerated while circulating the solution between the second treatment tank 5B and the electrolytic sulfuric acid device 6. In the other first treatment tank 5A, the copper wire covered with the coating film is immersed in the regenerated sulfuric acid solution to peel off the coating film (C in FIG. 7).
[0071] By repeating the above procedure, multiple resins can be continuously treated without interrupting the process. In this embodiment, the description has been given of a system equipped with two treatment tanks, but the number is not particularly limited, and the system may be equipped with two or more electrolytic sulfuric acid devices. In a specific embodiment of the apparatus for carrying out the coating material stripping method, a plurality of tanks for stripping and removing the coating material are prepared, and stripping and removing the coating material in a tank is terminated according to a decrease in the decomposition rate of the coating material in the tank, and the sulfuric acid solution in the tank is electrolyzed. When stripping and removing the coating material is terminated, stripping and removing the coating material in another tank can be continued or started.
[0072] (Embodiment 6) Next, another embodiment will be described with reference to Fig. 8. Note that the same components as those in the above-described embodiments are given the same reference numerals, and the description thereof will be omitted or simplified.
[0073] The treatment device 1C has multiple treatment tanks (treatment tanks 50A, 50B, 50C, 50D) that contain sulfuric acid solution and in which the coated copper material is immersed, and further has a decomposition storage tank 30 that contains the sulfuric acid solution in which the coating resin is dissolved, and an electrolytic sulfuric acid device 6. The treatment tanks 50A, 50B, 50C, and 50D correspond to the sulfuric acid contacting portion of the present disclosure and the immersion contacting tank. A measuring unit 11 is disposed in the decomposition storage tank 30 and is immersed in the sulfuric acid solution to measure the electrical conductivity or the redox potential of the sulfuric acid solution.
[0074] Between the treatment tanks 50A, 50B, 50C, and 50D and the decomposition tank 30, there is a delivery line 29A for sending the sulfuric acid solution treated in the treatment tank to the decomposition tank 30, and an introduction line 29B for sending the sulfuric acid solution regenerated in the decomposition tank 30. The delivery line 29A is provided with a liquid sending pump 32A, and the introduction line 29B is provided with a liquid sending pump 32B. Furthermore, the introduction line 29B is provided with a heating unit 28 for heating the sulfuric acid solution to be sent. The delivery line 29A and the introduction line 29B are branched and connected to the treatment tanks 50A, 50B, 50C, and 50D, respectively. The delivery line 29A and the introduction line 29B constitute the decomposition / regeneration liquid sending line of the present disclosure.
[0075] In addition, between the decomposition storage tank 30 and the electrolytic sulfuric acid device 6, there are provided an inlet line 31A for sending the sulfuric acid solution of the electrolytic sulfuric acid device 6 to the decomposition storage tank 30, and an outlet line 31B for sending the sulfuric acid solution of the decomposition storage tank 30 to the electrolytic sulfuric acid device 6. The inlet line 31B is provided with a circulation pump 33 and a cooling unit 34 for cooling the sulfuric acid solution. In addition, a control unit 20 is provided which receives the measurement results from the measurement unit 11 and controls the operations of the liquid delivery pumps 32A and 32B and the circulation pump 33.
[0076] Next, the operation of the processing device 1C will be described. The treatment tanks 50A, 50B, 50C, and 50D contain sulfuric acid solutions, which are preferably kept at a temperature of 60 to 140°C. In all or some of these treatment baths 50A, 50B, 50C, and 50D, copper wires coated with a coating material are immersed in a sulfuric acid solution, and the coating material is dissolved and peeled off.
[0077] At the beginning of operation, the sulfuric acid solution is stored in the decomposition storage tank 30, and the sulfuric acid solution can be sent to the necessary treatment tanks 50A, 50B, 50C, and 50D through the inlet line 29B by the liquid sending pump 32B. At this time, the sulfuric acid solution can be heated to a desired temperature (for example, 60 to 140° C.) by the heating unit 28. Note that an electromagnetic valve may be provided at each branch of the inlet line 29B, and the control unit 20 may control the opening and closing of the electromagnetic valve to select the treatment tank to which the solution is sent.
[0078] The sulfuric acid solution in which the coating material is dissolved in the treatment tanks 50A, 50B, 50C, and 50D is sent to the decomposition storage tank 30 through the delivery path 29A by the liquid delivery pump 32A. The state of dissolution in the treatment tank may be checked visually, but an appropriate dissolution measurement unit such as a unit for measuring the solution transmittance may also be used, and the result may be received by the control unit 20, which then compares the result with a dissolution reference value to determine whether or not the peeling has been completed. In this case, the control unit 20 can control the opening and closing of the solenoid valves of each branch path and the liquid delivery pump 32A to deliver the liquid.
[0079] When the sulfuric acid solution in which the coating material is dissolved is stored in the decomposition storage tank 30, the circulation pump 33 is operated to circulate the sulfuric acid solution H2SO4 between the decomposition storage tank 30 and the electrolytic sulfuric acid device 6, while electrolysis of the sulfuric acid solution is performed. During circulation, the sulfuric acid solution sent from the decomposition storage tank 30 is cooled (for example, to 20 to 60°C) by the cooling unit 34 provided in the delivery line 31B. Persulfuric acid H2S2O8 is generated from the sulfuric acid solution by electrolysis in the electrolytic sulfuric acid device 6, and is sent to the decomposition storage tank 30 through the introduction line 31A and the heating unit 35. At this time, the persulfuric acid concentration is preferably 0.5 to 5.0 g / L, and the solution is preferably heated to 60 to 140°C by the heating unit 35.
[0080] In the decomposition storage tank 30, the components of the coating material dissolved in the sulfuric acid solution containing persulfuric acid are gradually decomposed by the sulfuric acid solution introduced. By continuing the above-mentioned operation, the concentration of the coating material dissolved in the sulfuric acid solution gradually decreases. The decomposition state of the coating material in the sulfuric acid solution is measured by the measuring unit 11 and transmitted to the control unit 20. The control unit 20 judges whether the measurement result reaches a reference value, and if it does not reach the reference value, continues circulating and electrolyzing the sulfuric acid solution. If the measured value reaches the reference value, it judges that the decomposition is completed, stops the application in the electrolytic processing device 6, and stops the operation of the circulation pump 33. Next, the liquid sending pump 32B is operated to send the sulfuric acid solution in the decomposition storage tank 30 to any or all of the processing tanks 50A, 50B, 50C, and 50D, and reuses it for peeling and removing the coated copper material. The regenerated sulfuric acid solution may be used for other purposes in addition to the same purpose. The reference value in the control unit 20 may be preset and stored in a non-volatile storage unit, or may be acquired from a server or the like via a network, etc. The reference value may be set to a different value depending on the type of coating material, etc.
[0081] In the above embodiment, the peeling and regeneration treatment of the coated copper material is described without specifying the treatment tank, but these treatments may be performed simultaneously in multiple treatment tanks, or sequentially. By performing sequential treatment in multiple treatment tanks, efficient treatment can be performed without waste.
[0082] Although the present invention has been described based on the above embodiment, appropriate modifications can be made without departing from the scope of the present invention. The resin-coated copper wire to be treated in this embodiment is generally referred to as magnet wire, and the resin of the insulating coating that coats the copper wire may be, for example, any of polyimide resin, polyesterimide resin, polyamideimide resin, polyurethane resin, and polyester resin, and is not limited to a specific resin. The resin-coated copper wire may be in any shape, such as a rectangular wire or a round wire, and may be treated not only as a single resin-coated copper wire but also in a state such as being wound around a coil. The present embodiment can be suitably used as a method for peeling and removing an insulating coating from a resin-coated copper wire, which is a copper wire for winding electronic devices used in automobiles, home appliances, industrial applications, and the like, and recovering the copper wire, but the uses of the present embodiment are not limited to these uses. EXAMPLES
[0083] Example 1 The coating film stripping treatment was carried out in a 94.0 mass% sulfuric acid solution at a solution temperature of 100° C. After visually determining whether the treatment was complete, the purity of copper and the remaining rate of copper after the treatment were determined. In order to visually determine the completion of the treatment, a standard chart has been created that shows the surfaces of various magnet wires treated for different times and the results of checking the presence or absence of an insulating coating using an analytical device.
[0084] [Conditions for peeling test pieces] The test pieces were cut to lengths of approximately 150 mm from magnet wires having polyimide insulating coatings with different peeling conditions. ·Copper wire cross-sectional dimensions: 1.47mm x 2.93mm Insulation film cross-sectional dimensions: 1.68mm x 3.14mm Nominal film thickness: 102.5μm [Specifications of the peeling tank] -Volume of treatment tank 5: 25L
[0085] (Examples 2 to 4) The coating film peeling treatment was carried out using an electrolytic sulfuric acid solution. Example 2 was the same as Example 1 except for the use of an electrolytic sulfuric acid solution. In Example 3, the coating film treatment was carried out at 90.0 mass% and a solution temperature of 110°C, and in Example 4, the coating film treatment was carried out at 80.0 mass% and a solution temperature of 120°C. [Production of electrolytic sulfuric acid solution] The treatment conditions for electrolyzing the sulfuric acid solution are shown below. Material of anode 10A and cathode 10B: Diamond electrode (diameter 150 mm) Bipolar electrode 10C material: Diamond electrode (diameter 150mm) ·Current density: 5~30A / dm 2 Electrolysis cell circulation flow rate: 2-3L / min
[0086] Comparative Example 1 The coating treatment was carried out using an alkaline stripping solution containing potassium hydroxide, monoethanolamine, and phosphoric acid as main components at 95° C. The amount of treatment solution was 1 L. The test pieces and other materials used were the same as those used in Example 1.
[0087] [Table 1]
[0088] The oxidizing agent concentration in each test example was determined by taking a portion of the electrolyzed solution, subjecting it to a starch-iodine reaction and neutralizing titration to determine the total oxidizing power (KI value) of the solution. Meanwhile, the solution was titrated with potassium permanganate to measure the amount of hydrogen peroxide in the solution, and this value was subtracted from the KI value to determine the oxidizing power of the solution.
[0089] As Reference Example 1, treatment was performed under the conditions of Example 1 for the same time as Example 2. Although the peeling treatment proceeded, it was found that the insulating film could not be completely removed within the set treatment time, and a longer treatment time was required. It was also found that the peeling and removal of the insulating film could be performed more efficiently in a sulfuric acid solution containing persulfuric acid, as in Example 2-4. In Reference Example 2, the treatment was performed with a sulfuric acid concentration lower than the desired value. Although the peeling treatment proceeded, the treatment could not be completed within the treatment time of 180 minutes, so the treatment was interrupted at the treatment time of 180 minutes. It was found that the treatment efficiency decreased when the sulfuric acid concentration was lower than the desired value. In addition, in Reference Examples 1 and 2, since the peeling and removal of the coating was not completed, the Cu purity and the Cu residual rate were not measured. [Explanation of symbols]
[0090] 1 Processing equipment 1A Processing Equipment 1B Processing equipment 1C Processing Unit 2 copper wire 3. Bubble Generator 4. Air pump 5 Treatment tank 5A First treatment tank 5B Second treatment tank 6 Electrolytic sulfuric acid equipment 7 DC power supply for electrolysis 8 Circulation Pump 9A Inlet path 9B Sending path 10 Electrolysis Cell 10A anode 10B Cathode 10C Bipolar Electrode 11 Measuring part 12 Nozzles 14 Decomposition storage tank 15A feed line 15B Return line 16 Liquid delivery pump 20 Control section 28 Heating section 29A Sending path 29B Introductory path 30 Decomposition storage tank 31A Inlet path 31B Sending path 32A Liquid delivery pump 32B Liquid delivery pump 33 Circulation Pump 34 Cooling section 50A Treatment tank 50B Treatment tank 50C Treatment tank 50D Treatment tank
Claims
1. A method for stripping a coated copper material, comprising contacting a coating material coated on a copper material with a sulfuric acid solution, dissolving the coating material in the sulfuric acid solution and stripping and removing the coating material from the copper material, and decomposing the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution containing persulfuric acid.
2. 2. The method for stripping a coated copper material according to claim 1, wherein the concentration of persulfuric acid in the electrolytic sulfuric acid solution is 0.5 g / L or more.
3. 3. The stripping method according to claim 1, wherein the sulfuric acid solution in which the coating material has been decomposed is reused for stripping and removing the coated copper material or other coated copper materials.
4. The stripping method according to claim 1 or 2, wherein the sulfuric acid solution brought into contact with the coating material coating the copper material has a persulfuric acid concentration of less than 0.5 g / L, a sulfuric acid concentration of 85.0 mass% or more, and a temperature within a range of 60 to 140°C.
5. The sulfuric acid solution to be brought into contact with the coating material coated on the copper material is an electrolytic sulfuric acid solution having a persulfuric acid concentration of 0.5 g / L or more in a part or all of the peeling and removing process, and the sulfuric acid concentration is 80.0 mass% or more and the temperature is within the range of 60 to 140 ° C. The stripping treatment method according to claim 1.
6. 6. The stripping method according to claim 1, wherein the electrolytic sulfuric acid solution is electrolyzed at a solution temperature of 20 to 60°C.
7. 7. The stripping method according to claim 5, wherein the decomposition state of the coating material is judged by one or both of the electric conductivity and the oxidation-reduction potential of the sulfuric acid solution.
8. 8. The stripping method according to claim 7, wherein when the decomposition state of the coating material reaches a standard, the regeneration is judged to be completed, and the regenerated sulfuric acid solution is used for stripping and removing the coated copper material.
9. A peeling and removal treatment device having a sulfuric acid solution contact section that brings a coating material of a coated copper material into contact with a sulfuric acid solution, and a decomposition section that decomposes the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution.
10. 10. The peeling and removal treatment device according to claim 9, wherein the sulfuric acid solution contact section has one or both of an immersion treatment tank for immersing the coated copper material in the sulfuric acid solution and a release contact tank for releasing the sulfuric acid solution onto the coated material and contacting it.
11. The peeling and removal treatment device according to claim 9 or 10, wherein the decomposition section is provided with an electrolysis section that electrolyzes a sulfuric acid solution.
12. The peeling and removal treatment apparatus according to claim 11 , further comprising a plurality of the sulfuric acid solution contact sections, and one or more of the electrolysis sections are capable of selectively electrolyzing the sulfuric acid solutions in the plurality of the sulfuric acid solution contact sections.
13. 11. The peeling and removal treatment device according to claim 9, wherein the decomposition section comprises a decomposition storage tank and an electrolysis section, and an electrolysis circulation path for circulating a sulfuric acid solution between the decomposition storage tank and the electrolysis section is provided.
14. The peeling and removal treatment device according to claim 13, further comprising a decomposition and regeneration liquid feed path between the sulfuric acid solution contact section and the decomposition storage tank.
15. A measurement unit for measuring a decomposition state of the sulfuric acid solution in the decomposition unit; a control unit that controls electrolysis in the electrolysis unit, and liquid delivery through the electrolysis circulation path and the decomposition / regeneration liquid delivery path; The peeling and removal processing apparatus according to claim 14 , wherein the control unit receives a measurement result from the measurement unit and determines the content of the control based on the measurement result.
16. The apparatus is provided in a treatment apparatus having a measuring section for measuring the decomposition state of a coating material in a sulfuric acid solution containing persulfuric acid, a sulfuric acid solution contact section for dissolving the coating material of the coated copper material by contact with the sulfuric acid solution to peel off and remove it, a decomposition storage tank for decomposing the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution, a decomposition / regeneration liquid supply path provided between the sulfuric acid solution contact section and the decomposition storage tank, an electrolysis section for electrolyzing the sulfuric acid solution, and an electrolysis circulation path for circulating the sulfuric acid solution between the decomposition storage tank and the electrolysis section, receiving the measurement result of the measurement unit, and controlling electrolysis of the electrolysis unit, and liquid delivery through the electrolysis circulation path and the decomposition / regeneration liquid delivery path; A processing device control unit receives the measurement results and performs control to determine the content of the control based on the measurement results.
17. A program executed by a control unit that receives a measurement result from a measurement unit that measures the decomposition state of a coating material in a sulfuric acid solution containing persulfuric acid, and controls a sulfuric acid solution contact unit that dissolves the coating material of the coated copper material by contacting it with the sulfuric acid solution to peel off and remove it, and a decomposition storage tank that decomposes the coating material dissolved in the sulfuric acid solution with an electrolytic sulfuric acid solution, a liquid feed through a decomposition / regeneration liquid feed path provided between the decomposition storage tank and the electrolysis unit that electrolyzes the sulfuric acid solution, and a liquid feed through an electrolysis circulation path that circulates the sulfuric acid solution between the decomposition storage tank and the electrolysis unit, The program includes a step of sending the sulfuric acid solution in which the coating material is dissolved in the sulfuric acid solution contact portion to a decomposition storage tank through a decomposition / regeneration liquid sending path; receiving the measurement results; Executing electrolysis by the electrolysis unit and sending the solution through the electrolysis circuit until the measurement result reaches a reference; When the measurement result reaches a reference value, electrolysis by the electrolysis unit is stopped, and the sulfuric acid solution in the decomposition storage tank is sent to the sulfuric acid solution contact unit through the decomposition / regeneration liquid sending path. A program to be executed by the control unit.
Citation Information
Patent Citations
Method for recovering polymer component from waste plastic
JP1999323360A
Method of processing resin covered cable
JP2014069137A
Method for producing copper and copper production device
JP2016180164A
Method for collecting copper from resin-coated copper wire
JP2017061584A
Circuit breaker
JP1983028145A