Adhesive tape

The adhesive tape with a phenoxy resin, acid anhydride, and epoxy resin composition addresses the issue of wire connection reliability in QFN manufacturing, enhancing stability and reducing adhesive residue in semiconductor devices.

JP7572792B2Active Publication Date: 2024-10-24ARISAWA MFG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020064847
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-10-24
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Conventional adhesive tapes used in QFN manufacturing lack sufficient wire connection reliability, especially when PPF lead frames and copper wires are employed, leading to connection failures during the wire bonding process.

Method used

An adhesive tape with an adhesive layer containing phenoxy resin, acid anhydride, and epoxy resin, with specific storage modulus and glass transition temperature ranges, to enhance wire connection reliability.

Benefits of technology

The adhesive tape provides excellent wire connection reliability and minimizes adhesive residue, ensuring stable connections and efficient resin sealing in semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572792000003
    Figure 0007572792000003
  • Figure 0007572792000004
    Figure 0007572792000004
  • Figure 0007572792000001
    Figure 0007572792000001
Patent Text Reader

Abstract

To provide an adhesive tape which is excellent in wire connection reliability after a wire bonding step.SOLUTION: An adhesive tape has an adhesive layer containing a phenoxy resin, an acid anhydride, and an epoxy resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive tape that is primarily used in the manufacture of semiconductor devices. [Background technology]

[0002] In the field of LSI mounting technology, CSP (Chip Size / Scale Package) technology has been attracting attention, and in particular, packages in which lead terminals are incorporated inside the package, such as QFN (Quad Flat Non-leaded package), are advantageous in terms of miniaturization and high integration. A method for manufacturing such QFNs is to arrange multiple QFN semiconductor chips on the die pad in the package pattern area of ​​a lead frame, encapsulate them in a mold cavity with encapsulating resin, and then cut them into individual QFN structures, thereby improving productivity per lead frame area.

[0003] In the above-mentioned manufacturing method of QFN in which multiple semiconductor chips are encapsulated at once, the area clamped by the mold die during resin encapsulation is only the area outside the resin encapsulation area that extends beyond the package pattern area. Therefore, the encapsulation resin easily leaks out to the back side of the lead frame, which can cause connection failures due to burrs caused by the molding resin, or problems such as QFN terminals being covered with resin. For this reason, in the manufacturing method of QFN, it is considered effective to attach a heat-resistant adhesive tape to the back side of the lead frame and use the self-adhesive power (masking) of this adhesive tape to create a sealing effect to prevent resin leakage to the back side of the lead frame during resin encapsulation.

[0004] In such a manufacturing method, a method of laminating an adhesive tape after mounting a semiconductor chip on a lead frame or after performing wire bonding, or a method of laminating an adhesive tape on the back surface (outer pad surface) of a lead frame in an initial stage, and then performing a semiconductor chip mounting process, a wire bonding process, and a sealing process using a sealing resin are adopted. For example, Patent Document 1 proposes a manufacturing method that uses a heat-resistant adhesive tape having an adhesive layer to perform a series of processes such as wire bonding while preventing resin leakage. In addition, Patent Document 2 discloses an adhesive tape for manufacturing electronic components, which includes a substrate and an adhesive layer made of an adhesive composition containing a phenoxy resin, and reports that this can improve adhesive residues on the adhesive tape and leakage of sealing resin during the resin sealing process. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-184801 A [Patent Document 2] Special Publication No. 2012-504698 Summary of the Invention [Problem to be solved by the invention]

[0006] In the manufacture of QFN, after mounting a semiconductor chip on a lead frame, a wire bonding process is performed in which the tip of the terminal part of the lead frame and the electrode pad on the semiconductor chip are electrically connected with a bonding wire. In this case, if the adhesive tape attached to the back surface of the lead frame is not highly elastic, there is a problem that a connection failure occurs between the bonding wire and the lead frame, and the wire connection reliability decreases. In this respect, conventional adhesive tapes cannot be said to have sufficient wire connection reliability, and the decrease in wire connection reliability is particularly noticeable when a PPF (Pre-Plated Lead-Frame) is used as the lead frame and copper is used as the wire.

[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an adhesive tape that has excellent wire connection reliability after a wire bonding process. [Means for solving the problem]

[0008] Means for Solving the Problems The inventors of the present invention conducted intensive research to solve the above-mentioned problems and discovered that an adhesive tape having an adhesive layer containing a phenoxy resin, an acid anhydride, and an epoxy resin can solve the above-mentioned problems, thereby completing the present invention.

[0009] That is, the present invention is as follows. [1] An adhesive tape having an adhesive layer containing a phenoxy resin, an acid anhydride, and an epoxy resin. [2] The pressure-sensitive adhesive tape according to [1] above, wherein the pressure-sensitive adhesive layer has a storage modulus of 50 MPa or less at 150° C. or more and 200° C. or less, and a storage modulus of 3 MPa or more at a temperature higher than 200° C. and 250° C. or less. [3] The pressure-sensitive adhesive tape according to the above-mentioned [1] or [2], wherein the pressure-sensitive adhesive layer has a storage modulus of 3 MPa to 10,000 MPa at a temperature below 150°C. [4] The pressure-sensitive adhesive tape according to any one of the above-mentioned [1] to [3], wherein the phenoxy resin comprises one or more selected from the group consisting of bisphenol A type phenoxy resins, bisphenol F type phenoxy resins, phenoxy resins containing a bisphenol A / F mixed type skeleton, bisphenol S type phenoxy resins, phenoxy resins containing a naphthalene skeleton, phenoxy resins containing a fluorene skeleton, phenoxy resins containing a biphenyl skeleton, phenoxy resins containing an anthracene skeleton, phenoxy resins containing a pyrene skeleton, phenoxy resins containing a xanthene skeleton, phenoxy resins containing an adamantane skeleton, and phenoxy resins containing a dicyclopentadiene skeleton. [5] The pressure-sensitive adhesive tape according to any one of the above [1] to [4], wherein the resin composition constituting the pressure-sensitive adhesive layer has a glass transition temperature (Tg) of 80° C. or higher. [6] The pressure-sensitive adhesive tape according to any one of the above-mentioned [1] to [5], wherein the acid anhydride includes at least one selected from the group consisting of monofunctional acid anhydrides and polyfunctional acid anhydrides. [7] The pressure-sensitive adhesive tape according to any one of the above [1] to [6], wherein the epoxy resin is an epoxy resin having two or more epoxy groups in one molecule. [8] The pressure-sensitive adhesive tape according to any one of the above-mentioned [1] to [7], wherein the pressure-sensitive adhesive layer further contains a curing catalyst. [9] The pressure-sensitive adhesive tape according to any one of the above [1] to [8], which is used in the manufacture of a semiconductor device.

[10] The adhesive tape according to [9] above, wherein the semiconductor device is a QFN package (Quad Flat Non-leaded Package).

[11] The adhesive tape according to the above [9] or

[10] , which is a pre-attachment tape to be attached to a lead frame prior to a wire bonding step. Effect of the Invention

[0010] According to the present invention, it is possible to provide an adhesive tape having excellent wire connection reliability after a wire bonding process. [Brief description of the drawings]

[0011] [Figure 1-1] 1A to 1C are process diagrams illustrating an example of a method for manufacturing a semiconductor device using the pressure-sensitive adhesive tape of the present invention.

[0012] [Figure 1-2] 1A to 1C are process diagrams illustrating an example of a method for manufacturing a semiconductor device using the pressure-sensitive adhesive tape of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist. In this specification, unless otherwise specified, "curing" includes not only full curing but also half curing. In addition, in this specification, "adhesive tape" refers to a tape that does not adhere to an adherend at room temperature (20 to 30°C) but can adhere well to an adherend at a high temperature range (100°C or higher).

[0014] The pressure-sensitive adhesive tape of the present embodiment is a pressure-sensitive adhesive tape having an adhesive layer containing a phenoxy resin, an acid anhydride, and an epoxy resin.

[0015] [Phenoxy resin] The resin contained in the adhesive layer of the adhesive tape of this embodiment is a phenoxy resin, which is used from the viewpoint of increasing the heat resistance of the cured product and increasing the wire connection reliability in a high temperature range. The phenoxy resin is not particularly limited, and examples thereof include a resin obtained by reacting an epihalohydrin with a dihydric phenol compound, or a resin obtained by reacting a divalent epoxy compound with a dihydric phenol compound. Examples of the resin include one or more selected from the group consisting of bisphenol A type phenoxy resin, bisphenol F type phenoxy resin, phenoxy resin containing a bisphenol A / F mixed type skeleton, bisphenol S type phenoxy resin, phenoxy resin containing a naphthalene skeleton, phenoxy resin containing a fluorene skeleton, phenoxy resin containing a biphenyl skeleton, phenoxy resin containing an anthracene skeleton, phenoxy resin containing a pyrene skeleton, phenoxy resin containing a xanthene skeleton, phenoxy resin containing an adamantane skeleton, and phenoxy resin containing a dicyclopentadiene skeleton. Among these, from the viewpoint of adhesive residue, bisphenol A type, bisphenol F type, bisphenol A / F mixed type, bisphenol S type, biphenyl type, and naphthalene type phenoxy resins are preferred, and bisphenol A type, bisphenol A / F mixed type, bisphenol S type, and biphenyl type phenoxy resins are more preferred.

[0016] The weight average molecular weight of the phenoxy resin is not particularly limited, but is preferably 1000 to 200000, more preferably 5000 to 100000, and further preferably 10000 to 50000. When the weight average molecular weight of the phenoxy resin is 1000 to 200000, the adhesive layer tends to be stably formed.

[0017] The glass transition temperature (Tg) of the phenoxy resin is not particularly limited, but is preferably 80° C. or higher, more preferably 100° C. or higher, and even more preferably 120° C. or higher. When the Tg of the phenoxy resin is 80° C. or higher, the wire connection reliability tends to improve.

[0018] The content of the phenoxy resin in the adhesive layer is not particularly limited, but is preferably 30 to 80 parts by mass, more preferably 40 to 70 parts by mass, and even more preferably 50 to 60 parts by mass, relative to 100 parts by mass of the adhesive layer. When the content of the phenoxy resin is 30 parts by mass or more, adhesive transfer tends to be good, and when it is 80 parts by mass or less, wire connection reliability tends to be good.

[0019] [Acid anhydride] The acid anhydride contained in the adhesive layer of the adhesive tape of the present embodiment is not particularly limited, and examples thereof include one or more types selected from the group consisting of monofunctional acid anhydrides and polyfunctional acid anhydrides.

[0020] As the monofunctional acid anhydride, for example, any one or more selected from the group consisting of trimellitic anhydride, phthalic anhydride, maleic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, methylhexahydrophthalic anhydride, and methyltetrahydrophthalic anhydride can be used.

[0021] Examples of polyfunctional acid anhydrides include pyromellitic dianhydride, benzene-1,2,3,4-tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, naphthalene-2,3,6,7-tetracarboxylic dianhydride, naphthalene-1,2,5,6-tetracarboxylic dianhydride, naphthalene-1,2,4,5-tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, naphthalene-1,2,6, Any one or more selected from the group consisting of 7-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,2',3,3'-diphenyltetracarboxylic dianhydride, 2,3,3',4'-diphenyltetracarboxylic dianhydride, and 5-(2,5-dioxotetrahydro-3-furanyl)-3 methyl-3-cyclohexene-1,2-carboxylic dianhydride can be used. Among them, from the viewpoint of stably forming an adhesive layer, trimellitic anhydride, phthalic anhydride, and maleic anhydride are preferred, and trimellitic anhydride is more preferred.

[0022] The content of the acid anhydride contained in the adhesive layer is not particularly limited, but is preferably 10 to 25 parts by mass, more preferably 15 to 20 parts by mass, relative to 100 parts by mass of the adhesive layer. If the content of the acid anhydride is 10 parts by mass or more, the curing of the phenoxy resin, which is the main component, tends to be sufficient, and if it is 25 parts by mass or less, the adhesive residue tends to be good.

[0023] [Epoxy resin] The epoxy resin contained in the adhesive layer of the adhesive tape of this embodiment is not particularly limited as long as it has two or more epoxy groups in one molecule, and for example, any one or more selected from the group consisting of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, novolac type epoxy resin, amine type epoxy resin, biphenyl type epoxy resin, and alicyclic epoxy resin can be used. Among them, from the viewpoint of adhesive residue, novolac type epoxy resin and amine type epoxy resin are preferred, and novolac type epoxy resin is more preferred.

[0024] The content of the epoxy resin in the adhesive layer is not particularly limited, but is preferably 10 to 45 parts by mass, and more preferably 15 to 40 parts by mass, relative to 100 parts by mass of the adhesive layer. If the content of the epoxy resin is 10 parts by mass or more, the curing of the phenoxy resin, which is the main component, tends to be sufficient, and if it is 45 parts by mass or less, the adhesive residue tends to be good.

[0025] From the viewpoint of reactivity, the epoxy resin preferably has an epoxy equivalent of 90 to 300 g / eq, and more preferably 90 to 200 g / eq.

[0026] [Curing catalyst] The adhesive layer of the adhesive tape of this embodiment may further contain a curing catalyst. It is preferable to use a curing catalyst having an active temperature of 120° C. or less. Examples of the curing catalyst include organic peroxides such as benzoyl peroxide, methyl ethyl ketone peroxide, t-butylperoxy-2-ethylhexanoate, cumene hydroperoxide, cyclohexanone peroxide, and dicumyl peroxide; imidazole-based initiators such as 2-methylimidazole, N-benzyl-2-methylimidazole, and 2-undecylimidazole; azo-based initiators such as 2,2'-azobis-(2-methylbutyronitrile) and 2,2'-azobisisobutyronitrile, Lewis acid complexes such as boron trifluoride monoethylamine, polyamines, and melamine resins. Among the above, imidazole-based initiators such as 2-methylimidazole and 2-undecylimidazole are preferable from the viewpoint of contamination by catalyst residues.

[0027] The content of the curing catalyst contained in the adhesive layer is not particularly limited, but is preferably 0.01 to 3 parts by mass, more preferably 0.05 to 2 parts by mass, and even more preferably 0.05 to 1 part by mass, relative to 100 parts by mass of the phenoxy resin. If the content of the curing catalyst is 0.01 parts by mass or more, it tends to be possible to sufficiently initiate the reaction, and if it is 3 parts by mass or less, the risk of contamination of the adherend (glue residue) tends to be lower.

[0028] [Other ingredients] The adhesive layer included in the adhesive tape of the present embodiment may further contain other additives in addition to those described above, etc. Examples of such other additives include various additives such as a release agent, an ultraviolet absorber, a tackifier, a softener, a filler, an antiaging agent, a pigment, a dye, and a silane coupling agent.

[0029] [Adhesive layer] The storage modulus of the adhesive layer of this embodiment is not particularly limited, but is preferably 50 MPa or less, more preferably 30 MPa or less, and even more preferably 20 MPa or less at 150 to 200 ° C. When the storage modulus is 50 MPa or less at 150 to 200 ° C., the adhesiveness to the lead frame, which is the adherend, tends to improve. In addition, the storage modulus is preferably 3 MPa or more, preferably 5 MPa or more, and even more preferably 10 MPa or more at more than 200 ° C. and less than 250 ° C., when the storage modulus is 3 MPa or more at more than 200 ° C. and less than 250 ° C., the deformation of the adhesive tape is suppressed even in the above temperature range, and the wire connection reliability tends to improve. Furthermore, from the viewpoint of handling properties, the storage modulus of the adhesive layer at less than 150° C. is preferably 3 to 10,000 MPa, more preferably 5 to 10,000 MPa, and even more preferably 10 to 10,000 MPa.

[0030] The storage modulus of the adhesive layer can be adjusted, for example, by adjusting the ratio of the phenoxy resin, the epoxy resin, and the acid anhydride added.

[0031] The Tg of the resin composition constituting the adhesive layer of the present embodiment is not particularly limited, but is preferably 80° C. or higher, more preferably 100° C. or higher, and even more preferably 120° C. or higher. When the Tg of the resin composition constituting the resin layer is 80° C. or higher, wire connection reliability tends to be improved.

[0032] [Adhesive tape] The pressure-sensitive adhesive tape of the present embodiment is a pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer containing the specific component described above. Here, the pressure-sensitive adhesive tape may be composed of the pressure-sensitive adhesive layer and a base layer. For example, the resin composition constituting the adhesive layer of this embodiment can be applied onto a substrate (sometimes called a base film, etc.) to form an adhesive layer, thereby making it into an adhesive tape.

[0033] The thickness of the adhesive layer of the adhesive tape of this embodiment is preferably 3 to 40 μm, more preferably 3 to 20 μm. When the thickness of the adhesive layer is 3 μm or more, sufficient sealing property tends to be obtained in the sealing step. On the other hand, when the thickness is 40 μm or less, the adhesive layer is not destroyed even by the clamping pressure of the mold, and the adhesive tape tends to be stably produced. On the other hand, the thickness of the base layer is not particularly limited, but is preferably 5 μm or more from the viewpoint of preventing bending or cracking, and more preferably 10 to 100 μm from the viewpoint of handling properties.

[0034] The material constituting the substrate layer is not particularly limited, and examples thereof include polyethylene terephthalate (PET)-based substrates, polyimide (PI)-based substrates, polyamide (PA)-based substrates, polyethylene naphthalate (PEN)-based substrates, polyphenylene ether sulfide (PPS)-based substrates, etc. Among these, polyimide-based substrates are preferred from the viewpoint of heat resistance, etc. In addition, the substrate can be subjected to a surface modification treatment such as a corona treatment or a plasma treatment. This makes it possible to prevent the physical properties of the substrate from changing over time and to perform various surface modifications, etc.

[0035] The adhesive tape of the present embodiment may have the adhesive layer protected by a release film (separate film) or the like before use. By attaching such a release film, the adhesive strength of the adhesive layer can be maintained. The release film is not particularly limited, and a known one can be used appropriately. Examples of the release film include polyethylene terephthalate film, polypropylene film, polyethylene film, release paper, etc., which have been subjected to a silicone-based release treatment or a fluorine-based release treatment.

[0036] Examples of methods for manufacturing the adhesive tape of this embodiment include a method in which a solution in which the resin composition constituting the adhesive layer is dissolved in an organic solvent is prepared, and the solution is applied onto a substrate and dried, etc., to form an adhesive layer on the substrate.

[0037] Examples of organic solvents include alcohols such as methanol and ethanol; glycols such as ethylene glycol and propylene glycol; glycol monoalkyl ethers such as ethylene glycol monomethyl ether and ethylene glycol monoethyl ether; glycol dialkyl ethers such as ethylene glycol dimethyl ether and ethylene glycol diethyl ether; alkyl esters such as methyl acetate, ethyl acetate, propyl acetate, methyl acetoacetate and methyl acetoacetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene and ethylbenzene; aliphatic hydrocarbons such as hexane, cyclohexane and octane; amides such as dimethylphosphamide, dimethylacetamide and N-methylpyrrolidone; and cyclic ethers such as tetrahydrofuran and dioxane.

[0038] The coating method is not particularly limited, and any known method can be used, such as a die coater, a comma coater, or a gravure coater.

[0039] [Method of manufacturing semiconductor device] The pressure-sensitive adhesive tape of the present embodiment is used by being attached to mask terminal portions when electronic components or semiconductor components are resin-sealed. Fig. 1 is a process diagram of an example of a method for manufacturing a semiconductor device using the adhesive tape of this embodiment. As shown in Fig. 1, the method for manufacturing a semiconductor device of this embodiment includes at least a mounting step of a semiconductor chip 3 and a sealing step with a sealing resin 5. The method for manufacturing a semiconductor device of this embodiment may further include a dicing step of cutting the sealed structure.

[0040] The mounting process is a process of bonding a semiconductor chip 3 onto a die pad of a metal lead frame 2 having an adhesive tape 1 attached to the back side of the lead frame (the lower side of the figure) as shown in Figures 1(a) to (d).

[0041] The lead frame 2 is made of a metal such as copper, on which a QFN terminal pattern is engraved, and the electrical contact portion may be coated (plated) with a material such as silver, nickel, palladium, or gold. When a PPF (Pre-Plated Lead-Frame) is used as the lead frame, the effect of the present invention tends to be more pronounced. The thickness of the lead frame 2 is generally 100 to 300 μm. However, this does not apply to portions that have been partially thinned by etching or the like. It is preferable that the lead frame 2 has an arrangement pattern of individual QFNs arranged in an orderly manner so that it can be easily cut in a subsequent cutting process.

[0042] The adhesive tape 1 is preferably applied at least outside the package pattern area and to an area including the entire outer periphery of the resin sealing area to be resin-sealed. The lead frame 2 usually has guide pin holes near the ends for positioning during resin sealing, and it is preferable to apply the adhesive tape 1 to an area that does not block these holes. In addition, since multiple resin sealing areas are arranged in the longitudinal direction of the lead frame 2, it is preferable to apply the adhesive tape 1 continuously across these multiple areas.

[0043] A semiconductor chip 3, i.e., a silicon wafer chip which is a semiconductor integrated circuit part, is mounted on the lead frame 2 as described above. A fixing area called a die pad is provided on the lead frame 2 to fix the semiconductor chip 3, and various methods such as using conductive paste, adhesive tape, and adhesive are used for bonding (fixing) to the die pad. When using conductive paste or a thermosetting adhesive for die bonding, the die is generally cured at a temperature of about 150 to 200°C for about 30 to 90 minutes. The lead frame on which the semiconductor chip is mounted may be subjected to plasma treatment as shown in Figure 1(c) in order to remove dirt from the die attachment material and improve wire connectivity and adhesion between the mold and frame.

[0044] Generally, this is followed by a wire bonding process in which the tip of the terminal portion of the lead frame and the electrode pad on the semiconductor chip are electrically connected by a bonding wire. As shown in FIG. 1(d), the wire bonding process is a process in which the tip of the terminal portion (inner lead) of the lead frame 2 is electrically connected to the electrode pad on the semiconductor chip 3 by a bonding wire 4. For example, a gold wire or an aluminum wire is used as the bonding wire 4, but when a copper wire is used, the effect of the present invention tends to be more remarkable. In general, the wire is connected by combining vibration energy by ultrasonic waves and pressure bonding energy by applying pressure in a state heated to 150 to 250°C. At that time, the adhesive tape attached to the lead frame 2 can be vacuum-suctioned to securely fix it to the heat block. In the above, the semiconductor chip is mounted face-up and the wire bonding process is performed, but when the semiconductor chip is mounted face-down, a reflow process is appropriately performed.

[0045] The encapsulation step is a step of encapsulating the semiconductor chip side with an encapsulation resin 5 on one side as shown in FIG. 1(e). The encapsulation step is performed to protect the semiconductor chip 3 and the bonding wires 4 mounted on the lead frame 2, and is typically performed in a mold using an encapsulation resin, particularly an epoxy resin. In this case, the encapsulation step is generally performed simultaneously with a plurality of encapsulation resins 5 using a mold consisting of an upper mold and a lower mold having a plurality of cavities. Specifically, for example, the heating temperature during resin encapsulation is 170 to 180° C., and after curing at this temperature for several minutes, post-mold curing is further performed for several hours. Following the encapsulation step, the adhesive tape attached to the lead frame 2 is peeled off as shown in FIG. 1(f). It is preferable to peel off the adhesive tape 1 before the post-mold curing.

[0046] 1(g), the dicing process is a process of cutting the encapsulated structure into individual semiconductor devices 10. In general, the dicing process includes a process of cutting the encapsulating resin 5 at the cutting portion using a rotary cutting blade such as a dicer.

[0047] As described above, the adhesive tape of this embodiment may be adhered to the lead frame before the semiconductor chip mounting process, or after the semiconductor chip mounting process (after wire bonding) and before the sealing process. However, from the viewpoint of making the effects of the present invention more pronounced, it is preferable that the adhesive tape be a pre-attached tape that is adhered to the lead frame before the semiconductor chip mounting process, particularly before the wire bonding process. EXAMPLES

[0048] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples in any way. The evaluation and measurement methods are as follows.

[0049] <Weight average molecular weight> The measurement was performed by gel permeation chromatography (GPC) using standard polystyrene having an average molecular weight of about 500 to about 1 million.

[0050] <Glass transition temperature (Tg)> The measurements were carried out by differential scanning calorimetry (DSC).

[0051] <Storage modulus> A sheet-like sample having a thickness of 100 μm and the same composition as the adhesive layer of the adhesive tape was prepared, and the storage modulus E' was measured using a dynamic viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments). The measurement was performed at a temperature range of -50 to 300°C with a temperature rise rate of 10.0°C / min and a frequency of 1 Hz. The storage moduli E' at 25°C, 100°C, 140°C, 175°C, and 225°C are shown in Tables 1 and 2. In the tables, "Not measurable" means that the adhesive layer was stretched too much and could not be measured.

[0052] <Wire connection reliability> After bonding the adhesive tape to the lead frame under conditions of 240°C x 10 sec x 10 MPa, the semiconductor chip was mounted on the die pad of the lead frame using a die attachment material, and the die attachment material was cured by heating at 160°C for 30 minutes. After that, wire bonding was performed between the electrode part of the mounted semiconductor chip and the electrode part of the lead frame using a φ25μm copper wire (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.). At this time, a wire bonder (manufactured by K&S Co., Ltd.) was used, and wire bonding was performed under the conditions of a stage temperature of 200°C, a current value of 200mA, a time of 30ms, and a load of 100g. After wire bonding, it was visually confirmed whether the wire was accurately inserted. In addition, the wire connection strength was measured by a wire pull test. If the wire was accurately inserted and the wire pull strength was 5 gf or more, it was evaluated as "○". On the other hand, if the wire was accurately inserted but the wire pull strength was less than 5 gf, or if the wire was not accurately inserted, it was evaluated as "×".

[0053] <Glue residue> After the above-mentioned wire bonding process, sealing was performed. The sealing material used was Hitachi Chemical's CEL-9200HF9, and sealing was performed using a transfer molding device at a temperature of 175°C, a pressure of 3MPa, and a time of 90 seconds. The sealing material was then cured at a temperature of 175°C for 6 hours. The tape was then peeled off, and the mold surface and lead frame surface were observed under a microscope to see if there was any glue residue. If there was no glue residue, it was rated as "○", and if there was glue residue, it was rated as "×".

[0054] Specifically, the following components were used in the resin compositions in the examples and comparative examples. [Phenoxy resin] Phenoxy resin A: Bisphenol A / F mixed phenoxy resin (Mitsubishi Chemical Corporation, 1256B40) Phenoxy resin B: Bisphenol S-type phenoxy resin (Mitsubishi Chemical Corporation, YX8100BH30) [Acid anhydride] Trimellitic anhydride (Mitsubishi Gas Chemical Company, Inc.) Phthalic anhydride (JFE Chemical) Polyfunctional acid anhydride: 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-carboxylic acid dianhydride (DIC, B-4400) [Epoxy resin] Epoxy resin C: Phenol novolac type epoxy resin (epoxy equivalent: 210g / eq) Epoxy resin D: Glycidylamine type tetrafunctional epoxy resin (epoxy equivalent: 100g / eq) [Imidazole] 2-Undecylimidazole (Curesol C11Z, manufactured by Shikoku Chemical Industry Co., Ltd.) [Acrylic resin] Acrylic resin E: Butyl acrylate-acrylic acid random copolymer (manufactured by Taisei Fine Chemical Co., Ltd., 1HY-3006Y, Tg: -53°C) [Isocyanate] Isocyanate F: Hexamethylene diisocyanate (Asahi Kasei Corporation, Duranate D201)

[0055] [Example 1] To 100 parts by mass of phenoxy resin A, 75 parts by mass of trimellitic anhydride (manufactured by Mitsubishi Gas Chemical Company, Inc.), 60 parts by mass of phenol novolac type epoxy resin (manufactured by Mitsubishi Chemical Corporation, jER152, epoxy equivalent 210 g / eq), and 0.2 parts by mass of 2-undecylimidazole (manufactured by Shikoku Chemical Industry Co., Ltd., Curesol C11Z) were added and stirred at room temperature to obtain a resin composition. The obtained resin composition was applied to a polyimide film having a thickness of 25 μm using a die coater so that the thickness after drying would be 6 μm, and then dried at 150° C. for 5 minutes to obtain an adhesive tape. Next, the release surface of a release-treated separate film was laminated onto the adhesive layer of the adhesive tape, and the resulting mixture was heated at 100° C. for 100 hours to obtain an adhesive tape with a release film. The obtained adhesive tape was used to evaluate various physical properties, and the evaluation results are shown in Table 1 (the unit of content in the table is "parts by mass" unless otherwise specified).

[0056] [Example 2] to [Example 8] An adhesive tape was manufactured in the same manner as in Example 1, except that the type and content of each component contained in the composition forming the adhesive layer was changed to the type and content shown in Table 1, and each physical property was evaluated.

[0057] [Comparative Example 1] to [Comparative Example 6] An adhesive tape was manufactured in the same manner as in Example 1, except that the type and content of each component contained in the composition forming the adhesive layer was changed to the type and content shown in Table 2, and each physical property was evaluated.

[0058] [Table 1]

[0059] [Table 2]

[0060] As shown in Tables 1 and 2, the pressure-sensitive adhesive tapes of Examples 1 to 8 were excellent in wire connection reliability after the wire bonding step, and also achieved suppression of adhesive residue during the tape peeling step. [Industrial Applicability]

[0061] The pressure-sensitive adhesive tape of the present invention has industrial applicability as a pressure-sensitive adhesive tape used in the production of semiconductor devices.

Claims

1. The adhesive layer includes a phenoxy resin, an acid anhydride, and an epoxy resin. For 100 parts by mass of the adhesive layer, The content of the phenoxy resin is 30 to 80 parts by mass, The content of the acid anhydride is 10 to 25 parts by mass, The adhesive tape has an epoxy resin content of 10 to 45 parts by mass.

2. The pressure-sensitive adhesive tape according to claim 1 , wherein the pressure-sensitive adhesive layer has a storage modulus of 50 MPa or less at 150° C. or more and 200° C. or less, and a storage modulus of 3 MPa or more at a temperature higher than 200° C. and 250° C. or less.

3. The pressure-sensitive adhesive tape according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a storage modulus of 3 MPa to 10,000 MPa at a temperature below 150° C.

4. The pressure-sensitive adhesive tape according to any one of claims 1 to 3, wherein the phenoxy resin comprises at least one selected from the group consisting of bisphenol A type phenoxy resins, bisphenol F type phenoxy resins, phenoxy resins containing a bisphenol A / F mixed type skeleton, bisphenol S type phenoxy resins, phenoxy resins containing a naphthalene skeleton, phenoxy resins containing a fluorene skeleton, phenoxy resins containing a biphenyl skeleton, phenoxy resins containing an anthracene skeleton, phenoxy resins containing a pyrene skeleton, phenoxy resins containing a xanthene skeleton, phenoxy resins containing an adamantane skeleton, and phenoxy resins containing a dicyclopentadiene skeleton.

5. The pressure-sensitive adhesive tape according to any one of claims 1 to 4, wherein the resin composition constituting the pressure-sensitive adhesive layer has a glass transition temperature (Tg) of 80°C or higher.

6. The pressure-sensitive adhesive tape according to any one of claims 1 to 5, wherein the acid anhydride comprises at least one selected from the group consisting of monofunctional acid anhydrides and polyfunctional acid anhydrides.

7. 7. The adhesive tape according to claim 1, wherein the epoxy resin has two or more epoxy groups in one molecule.

8. The adhesive tape according to any one of claims 1 to 7, wherein the adhesive layer further comprises a curing catalyst.

9. The adhesive tape according to any one of claims 1 to 8, which is used in the manufacture of a semiconductor device.

10. 10. The adhesive tape according to claim 9, wherein the semiconductor device is a QFN package (Quad Flat Non-leaded Package).

11. 11. The pressure-sensitive adhesive tape according to claim 9, which is a pre-attachment tape that is attached to a lead frame prior to a wire bonding step.

12. The adhesive tape described in claim 11, which is peelable from the lead frame.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor device

    JP2002184801A

  • Insulation sheet

    JP2011168672A

  • Adhesive tape for electronic component manufacturing

    JP2012504698A

  • Adhesive composition improved in electric reliability at high voltage, and adhesive tape for semiconductor packaging using the same

    JP2014019869A

  • Adhesive film-integrated surface protection tape for use in grinding thin film, and method for manufacturing semiconductor chip

    JP2015218287A