Method for producing rubber composition
By using a nitrogen-containing aromatic compound as a solvent, crosslinked rubber is decomposed at low temperatures to produce liquid hydrocarbons efficiently, addressing the limitations of existing methods in recycling crosslinked rubber.
Patent Information
- Application Number
- JP2020128382
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing methods for recycling crosslinked rubber face challenges in producing liquid hydrocarbons under mild conditions and achieving high decomposition rates, particularly when using solvents like toluene.
Heating crosslinked rubber at 300°C or less in a reaction solvent containing a nitrogen-containing aromatic compound with at least one nitrogen atom, such as nitrobenzene, to facilitate the formation of liquid hydrocarbons through bond cleavage and radical reactions.
This method enables the production of liquid hydrocarbons at a high decomposition rate under mild conditions, reducing energy consumption and enhancing the efficiency of the recycling process.
Smart Images

Figure 0007572807000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a rubber composition. [Background technology]
[0002] From the viewpoints of the environment and resource conservation, the regeneration of crosslinked rubber and its reuse as new crosslinked rubber have been considered. For example, Patent Document 1 discloses a method for efficiently and simply producing reusable liquid hydrocarbons and carbon black from vulcanized rubber waste, in which vulcanized rubber such as vulcanized rubber waste is thermally decomposed in the presence of a hydrogen-donor solvent to produce liquid hydrocarbons and carbon black. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-310076 Summary of the Invention [Problem to be solved by the invention]
[0004] In the method described in Patent Document 1, for example, as described in paragraph number
[0033] , "the reaction was carried out for one hour at a nitrogen gas initial pressure of 20 kg / cm2 and a reaction temperature of 440°C," crosslinked rubber is decomposed under a high-pressure environment. However, from the viewpoint of resource and energy conservation, a method for obtaining liquid hydrocarbons even under mild conditions is desired. In addition, it is believed that non-polar solvents such as toluene and tetralin have good compatibility with vulcanized rubber. Patent Document 1 discloses an invention in which tetralin is used as a decomposition solvent, but there is a need to further improve the decomposition rate.
[0005] An object of the present invention is to provide a method for producing a rubber composition, which can produce liquid hydrocarbons at a high decomposition rate even under mild conditions, and an object of the present invention is to achieve the above object. [Means for solving the problem]
[0006] <1> A method for producing a rubber composition, comprising heating a crosslinked rubber at 300°C or less in a reaction solvent containing a nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of an amino group, a cyano group, and a nitro group, to obtain a rubber composition containing liquid hydrocarbons.
[0007] <2> The nitrogen-containing aromatic compound has an amino group or a nitro group. <1> A method for producing the rubber composition according to claim 1. <3> The nitrogen-containing aromatic compound has a nitro group. <1> or <2> A method for producing the rubber composition according to claim 1. <4> The nitrogen-containing aromatic compound has one nitro group. <1> ~ <3> 13. A method for producing the rubber composition according to claim 12. <5> The nitrogen-containing aromatic compound includes nitrobenzene. <1> ~ <4> 13. A method for producing the rubber composition according to claim 12.
[0008] <6> The crosslinked rubber is heated at 150 to 250° C. <1> ~ <5> 13. A method for producing the rubber composition according to claim 12. <7> The crosslinked rubber is a crosslinked product of a rubber component containing 50 to 100% by mass of a diene rubber. <1> ~ <6> 13. A method for producing the rubber composition according to claim 12. <8> The crosslinked rubber includes a vulcanized rubber. <1> ~ <7> 13. A method for producing the rubber composition according to claim 12. Effect of the Invention
[0009] According to the present invention, there can be provided a method for producing a rubber composition which is capable of producing liquid hydrocarbons at a high decomposition rate even under mild conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Method of manufacturing rubber composition> The method for producing a rubber composition of the present invention includes a step of heating a crosslinked rubber at 300°C or less in a reaction solvent containing a nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of an amino group, a cyano group, and a nitro group to obtain a rubber composition containing liquid hydrocarbons (hereinafter, sometimes referred to as the "decomposition step"). The method for producing a rubber composition of the present invention may include, in addition to the decomposition step, a drying step of drying the reaction product obtained in the decomposition step. The liquid hydrocarbons contained in the rubber composition produced by the production method of the present invention are rubber molecules that constitute the crosslinked rubber, and vary depending on the composition of the crosslinked rubber, but when crosslinked rubber derived from waste tires is used, they usually contain natural rubber, styrene-butadiene copolymer rubber, etc. Note that "liquid" means that the material is in a liquid state at room temperature (25°C) and atmospheric pressure (0.1 MPa), or is easily solubilized in petroleum components (alcohol, diethyl ether, tetrahydrofuran, etc.) to become liquid.
[0011] It is believed that the method for producing a rubber composition of the present invention breaks bonds (carbon-carbon bonds) between carbon atoms derived from rubber molecules constituting the crosslinked rubber, and bonds (e.g., carbon-sulfur bonds) between such carbon atoms and heteroatoms (oxygen atoms, sulfur atoms, etc.) derived from the crosslinking agent, due to the effects of heat and solvent, generating radicals and / or new bonds. It is presumed that the use of the nitrogen-containing aromatic compound as the reaction solvent leads to a radical chain transfer effect, and a higher decomposition rate can be achieved than when a general non-polar solvent such as toluene is used. In addition, according to the present invention, a high decomposition rate can be achieved, and therefore the decomposition reaction can be completed in a short time. The method for producing the rubber composition of the present invention will be described in detail below.
[0012] [Crosslinked rubber] The crosslinked rubber is a crosslinked product of a rubber component, and the rubber component that is the raw material of the crosslinked rubber may be either a diene rubber or a non-diene rubber. The diene rubber may be at least one selected from the group consisting of natural rubber (NR) and synthetic diene rubber. Examples of synthetic diene rubbers include polyisoprene rubber (IR), styrene-butadiene copolymer rubber (SBR), polybutadiene rubber (BR), ethylene-propylene-diene rubber (EPDM), chloroprene rubber (CR), halogenated butyl rubber, and acrylonitrile-butadiene rubber (NBR). Examples of non-diene rubbers include butyl rubber, ethylene propylene rubber, urethane rubber, silicone rubber, and acrylic rubber. These rubber components may be used alone or in combination of two or more.
[0013] Among the above, since rubber products such as tires generally use diene rubber, the rubber component preferably contains 50% by mass or more of diene rubber. In other words, the crosslinked rubber is preferably a crosslinked product of a rubber component containing 50 to 100% by mass of diene rubber. The rubber component more preferably contains 70% by mass or more of diene rubber, and even more preferably contains 90% by mass or more of diene rubber. In addition, the diene rubber is preferably at least one selected from the group consisting of natural rubber, polyisoprene rubber, and styrene-butadiene copolymer rubber.
[0014] The crosslinking agent for the rubber component is not particularly limited, and examples thereof include sulfur-based crosslinking agents, organic peroxide-based crosslinking agents, acid crosslinking agents, polyamine crosslinking agents, resin crosslinking agents, sulfur compound-based crosslinking agents, and oxime-nitrosamine-based crosslinking agents. Since a sulfur-based crosslinking agent (vulcanizing agent) is usually used for the rubber component of a tire or the like, it is preferable that the crosslinked rubber contains a vulcanizate vulcanized with a vulcanizing agent, that is, a vulcanized rubber. When vulcanized rubber is heated at 300°C or less in a reaction solvent containing a nitrogen-containing aromatic compound having at least one nitrogen atom, the carbon-sulfur bonds that mainly constitute the molecular structure of the vulcanized rubber undergo exchange reactions due to bond scission caused by heat and solvent effects, etc., and it is believed that the hydrogen atoms released from the nitrogen-containing aromatic compound having at least one nitrogen atom are attracted to the highly reactive radical species generated by the scission, thereby terminating the radical reaction. The content of vulcanized rubber in the crosslinked rubber is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, and it is particularly preferable that the crosslinked rubber is a vulcanized rubber (the content is 100% by mass).
[0015] (Filler) The crosslinked rubber may contain a filler. Tires generally contain reinforcing fillers such as carbon black and silica in order to improve various functions of the tire, such as durability and abrasion resistance. As the filler, either silica or carbon black may be used alone, or both silica and carbon black may be used.
[0016] The silica is not particularly limited, and may be any type depending on the application, such as general-grade silica, special silica that has been surface-treated with a silane coupling agent, etc. As the silica, it is preferable to use, for example, wet silica. The carbon black is not particularly limited and can be appropriately selected depending on the purpose. For example, FEF, SRF, HAF, ISAF, and SAF grade carbon black are preferable. The content of the filler in the crosslinked rubber is preferably from 40 to 100 parts by mass, and more preferably from 50 to 90 parts by mass, based on 100 parts by mass of the rubber component.
[0017] The crosslinked rubber may be a crosslinked product obtained by crosslinking a rubber composition containing, in addition to the rubber component and the above-mentioned filler, compounding agents commonly used in the rubber industry, such as softeners, stearic acid, antioxidants, zinc oxide, vulcanization accelerators, etc. Tires generally contain vulcanized rubber obtained by vulcanizing rubber compositions containing these compounding agents.
[0018] [Reaction Solvent] The reaction solvent contains a nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of an amino group, a cyano group, and a nitro group. By selecting the nitrogen-containing aromatic compound as the reaction solvent, a higher decomposition rate can be achieved due to the radical chain transfer effect, as compared to the use of general non-polar solvents such as toluene. If the reaction solvent does not contain the nitrogen-containing aromatic compound, a high decomposition rate cannot be achieved. The nitrogen-containing aromatic compound may have at least one of an amino group, a cyano group, and a nitro group, and may have two or more amino groups, two or more cyano groups, and two or more nitro groups.
[0019] Specific examples of the nitrogen-containing aromatic compound include aniline, nitrobenzene, dinitrobenzene, benzonitrile, phthalonitrile, and nitrobenzonitrile.
[0020] From the viewpoint of producing liquid hydrocarbons at a higher decomposition rate, the nitrogen-containing aromatic compound preferably has an amino group or a nitro group, and more preferably contains at least a nitro group. The nitrogen-containing aromatic compound preferably has one nitro group, in other words, the number of nitro groups that the nitrogen-containing aromatic compound has is preferably one. Nitrogen-containing aromatic compounds are used from the viewpoint of producing liquid hydrocarbons at a higher decomposition rate.
[0021] In the present invention, from the viewpoint of producing liquid hydrocarbons at a higher cracking rate, the nitrogen-containing aromatic compound preferably has a structure in which a nitrogen-containing functional group having at least one nitrogen atom selected from the group consisting of an amino group, a cyano group, and a nitro group is bonded to a non-nitrogen-containing aromatic ring. The non-nitrogen-containing aromatic ring and the nitrogen-containing functional group may be bonded directly or via a divalent or higher hydrocarbon group such as an alkylene or alkenylene. From the viewpoint of producing liquid hydrocarbons at a higher cracking rate, the non-nitrogen-containing aromatic ring and the nitrogen-containing functional group are preferably bonded directly. The non-nitrogen-containing aromatic ring is preferably a benzene ring. From the viewpoint of producing liquid hydrocarbons at a higher cracking rate, the nitrogen-containing aromatic compound preferably contains one or more compounds selected from the group consisting of aniline and nitrobenzene, and more preferably contains nitrobenzene.
[0022] The reaction solvent may consist of a nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of a cyano group and a nitro group, or may contain other solvents in addition to the nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of a cyano group and a nitro group. From the viewpoint of increasing the decomposition rate of liquid hydrocarbons, however, it is preferred that the main component of the reaction solvent is a nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of a cyano group and a nitro group. Here, the term "main component" refers to a reaction solvent in which the content of a nitrogen-containing aromatic compound having at least one nitrogen atom selected from the group consisting of a cyano group and a nitro group exceeds 50% by volume. The content of the nitrogen-containing aromatic compound in the reaction solvent is preferably 70% by volume or more, more preferably 90% by volume or more, and may be 100% by volume or more.
[0023] In the decomposition step, the reaction solvent is preferably used in such a range that the ratio (Vs / Wg) of the volume [mL] (Vs) of the reaction solvent to the mass [mg] (Wg) of the crosslinked rubber is preferably 0.001 / 1 to 1 / 1, more preferably 0.005 / 1 to 0.1 / 1. By using the reaction solvent within the above range, the solvolysis reaction is further promoted, sufficient hydrogen atoms are supplied to the crosslinked rubber, recombination of radicals generated by thermal decomposition is suppressed, and the crosslinked rubber can be efficiently decomposed.
[0024] [Reaction conditions for the decomposition process] (temperature) In the decomposition step, the crosslinked rubber and the reaction solvent are heated to a temperature of 300°C or less. By setting the heating temperature at 300°C or less, energy saving is excellent and a decrease in the decomposition rate due to side reactions and the like can be suppressed. The heating temperature in the decomposition step is sometimes referred to as the decomposition temperature. By heating the crosslinked rubber at a lower temperature, the crosslinked rubber can be decomposed by prioritizing the reaction involving the solvent. The heating temperature is preferably 150°C or more, more preferably 155°C or more, and even more preferably 160°C or more, and is preferably 250°C or less, more preferably 240°C or less, even more preferably 230°C or less, even more preferably 220°C or less, and even more preferably 210°C or less.
[0025] (Decomposition time) In the decomposition step, the time for heating the crosslinked rubber (decomposition time) is preferably 30 to 240 minutes, and more preferably 60 to 180 minutes, from the viewpoint of sufficiently advancing the decomposition reaction of the crosslinked rubber.
[0026] (pressure) In the decomposition step, the pressure applied to the crosslinked rubber and the reaction solvent is not particularly limited. From the viewpoint of the reaction rate of the decomposition reaction of the crosslinked rubber and resource and energy saving, the pressure is preferably 0 to 2.0 MPa (G), and more preferably 0.01 to 1.5 MPa (G). The unit "MPa (G)" means that the pressure is a gauge pressure. When the pressure is 2.0 MPa (G) or less, the molecular weight of the liquid hydrocarbon is less likely to decrease, and when the pressure is 0.1 MPa (G) or more, the reaction solvent can easily permeate the crosslinked rubber, making it easier to increase the reaction rate.
[0027] (atmosphere) The reaction atmosphere in the decomposition step at 300° C. or less is not particularly limited, and the reaction may be carried out in a gas atmosphere consisting of an inert gas such as argon gas or nitrogen gas (hereinafter simply referred to as an inert gas atmosphere), a gas atmosphere consisting of air (hereinafter simply referred to as an air atmosphere), or a mixed gas atmosphere of air and an inert gas. When an inert gas is used, two or more kinds of inert gases may be mixed and used. From the viewpoint of performing the decomposition of the crosslinked rubber using lighter equipment and promoting energy saving, the crosslinked rubber is preferably heated in an aerobic environment, i.e., in an oxygen-containing atmosphere, more preferably in an atmosphere of a gas containing air, and further preferably in an air atmosphere.
[0028] [Drying process] The method for producing a rubber composition of the present invention preferably includes a drying step of drying the reaction product (rubber composition containing liquid hydrocarbons) obtained in the decomposition step. The reactants may be subjected to blowing of hot air at, for example, 100 to 150° C. The hot air may be air or an inert gas such as nitrogen gas.
[0029] As described above, a rubber composition containing liquid hydrocarbons is obtained by heating the crosslinked rubber at 300°C or less in a reaction solvent containing a nitrogen-containing aromatic compound having at least one nitrogen atom. The rubber composition generally contains a liquid product containing liquid hydrocarbons obtained by thermal decomposition of the crosslinked rubber, as well as a solid content remaining without decomposition. Furthermore, when waste tires are used as the crosslinked rubber, the solid content also contains the filler since tires usually contain a filler. In the case of isoprene rubber (IR), raw rubber before vulcanization generally has a weight average molecular weight (Mw) of about 1 million and a number average molecular weight (Mn) of about 300,000, and in the case of styrene-butadiene copolymer rubber (SBR), generally, the weight average molecular weight (Mw) is about 300,000 and the number average molecular weight (Mn) is about 120,000. The closer the Mw and Mn of the obtained liquid hydrocarbon are to these values, the closer the molecular chain of the obtained rubber is to the raw rubber. The Mw and Mn of the liquid hydrocarbon can be measured, for example, by gel permeation chromatography (GPC).
[0030] The liquid hydrocarbons produced by the above-mentioned method can be used for regenerating crosslinked rubber. Furthermore, for regenerating crosslinked rubber, not only liquid hydrocarbons alone may be used as a raw material, but also the liquid hydrocarbons may be mixed with the solid matter obtained in the cracking step, that is, the rubber composition obtained in the cracking step may be used as it is as a raw material for regenerated rubber without separating the liquid hydrocarbons from the rubber composition obtained in the cracking step.
[0031] <Recrosslinked rubber> The re-crosslinked rubber of the present invention is a re-crosslinked rubber obtained by re-crosslinking the rubber composition produced by the rubber composition production method of the present invention, and contains liquid hydrocarbons contained in the rubber composition as a rubber component, and the content of the liquid hydrocarbons in the rubber component is 1 to 100 mass %. That is, the re-crosslinked rubber of the present invention is a re-crosslinked product of a rubber composition containing liquid hydrocarbons obtained by thermal decomposition of a crosslinked rubber as a rubber component, and the rubber component contains at least 1 mass % of liquid hydrocarbons, and may be 100 mass %. The content of liquid hydrocarbons in the rubber component may be 20 mass % or more, 30 mass % or more, 60 mass % or more, or 70 mass % or more.
[0032] When the content of the liquid hydrocarbons in the rubber component is less than 100% by mass, the other rubber components used together with the liquid hydrocarbons are not particularly limited. The other rubber components used together with the liquid hydrocarbons are sometimes referred to as pure rubber components. The pure rubber component is the rubber component already mentioned as the raw material for the crosslinked rubber. Among them, at least one selected from the group consisting of natural rubber (NR) and synthetic diene rubber is preferable, and at least one selected from the group consisting of natural rubber, polyisoprene rubber, polybutadiene rubber, and styrene-butadiene copolymer rubber is more preferable.
[0033] The rubber composition serving as the raw material for the re-crosslinked rubber of the present invention may contain, in addition to the rubber component containing the liquid hydrocarbon, a filler, a vulcanizing agent, a vulcanization accelerator, a softener, stearic acid, an antioxidant, zinc oxide, etc. As described above, the rubber composition produced by the rubber composition production method of the present invention contains, in addition to the liquid product containing liquid hydrocarbons obtained by thermal decomposition of the crosslinked rubber, solid components remaining without decomposition, and the solid components may also contain fillers. The rubber composition as the raw material of the re-crosslinked rubber may contain solids remaining without decomposition. By producing the re-crosslinked rubber using the solids remaining without decomposition together with the liquid hydrocarbons obtained by thermal decomposition of the crosslinked rubber, the environmental burden can be further reduced. The conditions for re-crosslinking the rubber composition produced by the method for producing a rubber composition of the present invention are not particularly limited. The re-crosslinked rubber of the present invention may be a re-vulcanized rubber obtained by vulcanizing a rubber component containing a liquid hydrocarbon with a vulcanizing agent.
[0034] <Tires> The tire of the present invention comprises the recrosslinked rubber of the present invention. By forming a tire using a re-crosslinked rubber obtained by re-crosslinking a rubber composition containing liquid hydrocarbons obtained by thermal decomposition of a crosslinked rubber, it is possible to make a tire with a small environmental impact. Depending on the type and components of the tire to be applied, the tire may be obtained by molding an uncrosslinked rubber composition and then crosslinking it, or by first obtaining a semi-crosslinked rubber from an uncrosslinked rubber composition through a preliminary crosslinking step or the like, and then molding the rubber using the semi-crosslinked rubber and then further performing full crosslinking. As the gas to be filled into the tire, in addition to normal air or air with an adjusted oxygen partial pressure, inert gases such as nitrogen, argon, and helium can be used.
[0035] <Rubber industrial products> The rubber industrial products of the present invention are made of the recrosslinked rubber of the present invention. Examples of rubber industrial products include automobile parts other than the above tires, hose tubes, anti-vibration rubbers, conveyor belts, crawlers, cables, sealing materials, ship parts, building materials, etc. By using the re-crosslinked rubber of the present invention to form rubber industrial products, the industrial products can be made to have a small environmental impact. EXAMPLES
[0036] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.
[0037] <Preparing vulcanized rubber> As the vulcanized rubber, the following vulcanized rubber was prepared. Vulcanized rubber (SBR): Vulcanized rubber obtained by vulcanizing styrene-butadiene copolymer rubber.
[0038] <Production of Liquid Hydrocarbons> Example 1 (decomposition process) 0.4g of vulcanized rubber (SBR) cut into small pieces of about 1mm and 5mL of nitrobenzene were put into an autoclave (EYELA, pressure-resistant container, product name "HIP-30L"). The autoclave was sealed and placed in a heating container (EYELA, personal organic synthesis device ChemStation, product name "PPV-CTRL1"), and the contents were heated at 200°C for 2 hours while adjusting the pressure to 0-0.3MPa (G). After heating, the heating container was returned to room temperature (25°C) with cooling water, and the reactants were allowed to reach room temperature. The decomposition reaction was carried out in an air atmosphere.
[0039] (drying process) The reaction product obtained in the decomposition step was dried using a spray-type test tube concentrator (manufactured by EYELA, product name "MGS-3100") under nitrogen flow conditions at 130°C, to obtain the decomposition product organic matter of Example 1.
[0040] [Example 2, Comparative Examples 1 to 4] In the production of liquid hydrocarbons in Example 1, the reaction solvent was changed from nitrobenzene to the solvents shown in Table 1, and the decomposition product organic substances of Example 2 and Comparative Examples 1 to 4 were obtained in the same manner.
[0041] <Analysis of organic matter produced by decomposition> The decomposition organic matter obtained in the examples and comparative examples was dissolved in tetrahydrofuran and analyzed by gel permeation chromatography (GPC). From the analysis results, the solubilization rate and weight average molecular weight (Mw) of the decomposition organic matter were measured. In addition, a calibration curve was created using tetrahydrofuran solutions of pure rubber components with different concentrations. The calibration curve was used to quantify the liquid hydrocarbons in tetrahydrofuran and calculate the decomposition rate.
[0042] The conditions for the GPC measurement are as follows: Column: Tosoh Corporation, manufactured by TSKgel GMHXL Eluent: Tetrahydrofuran ·Flow rate: 1mL / min ·Temperature: 40℃ Detector: RI
[0043] The weight average molecular weight (Mw) obtained in Comparative Example 1 was set as 100.0, and the weight average molecular weights (Mw) of Examples 1 and 2 and Comparative Examples 2 to 4 were indexed. In addition, the decomposition rate obtained in Comparative Example 1 was set as 100.0, and the decomposition rates of Examples 1 and 2 and Comparative Examples 2 to 4 were indexed. The results are shown in Table 1.
[0044] [Table 1]
[0045] As can be seen from Table 1, nitrobenzene and aniline were able to produce liquid hydrocarbons at a higher decomposition rate than the reaction solvent of the comparative example. Although the decomposition rate of aniline was lower than that of nitrobenzene, liquid hydrocarbons with a high molecular weight were produced, which was a good result.
Claims
1. A method for producing a rubber composition, comprising mixing a reaction solvent containing more than 50 volume % of a nitrogen-containing aromatic compound (excluding compounds which are aromatic secondary amine-based antiaging agents) having at least one nitrogen atom selected from the group consisting of an amino group, a cyano group, and a nitro group, with a crosslinked rubber, and heating the resulting mixture at 300°C or less to obtain a rubber composition containing liquid hydrocarbons.
2. 2. The method for producing a rubber composition according to claim 1, wherein the nitrogen-containing aromatic compound (excluding compounds which are aromatic secondary amine-based antioxidants) has an amino group or a nitro group.
3. 3. The method for producing a rubber composition according to claim 1, wherein the nitrogen-containing aromatic compound (excluding compounds which are aromatic secondary amine-based antioxidants) has a nitro group.
4. The method for producing a rubber composition according to any one of claims 1 to 3, wherein the nitrogen-containing aromatic compound (excluding compounds which are aromatic secondary amine-based antioxidants) has one nitro group.
5. The method for producing a rubber composition according to any one of claims 1 to 4, wherein the nitrogen-containing aromatic compound (excluding compounds which are aromatic secondary amine-based antioxidants) contains nitrobenzene.
6. The method for producing a rubber composition according to any one of claims 1 to 5, wherein the crosslinked rubber is heated at 150 to 250°C.
7. The method for producing a rubber composition according to any one of claims 1 to 6, wherein the crosslinked rubber is a crosslinked product of a rubber component containing 50 to 100 mass % of a diene rubber.
8. The method for producing a rubber composition according to any one of claims 1 to 7, wherein the crosslinked rubber includes a vulcanized rubber.
Citation Information
Patent Citations
A method of devulcanizing a rubber vulcanizate
EP3514200A1
JP1975067882A
Production of liquid hydrocarbon and carbon black
JP1995310076A
Reclaimed rubber
JP2000128901A
Method for decomposing vulcanized rubber and decomposed rubber composition
JP2004315766A