Piezoelectric thin film element
The piezoelectric thin film element with controlled oxygen content in aluminum nitride layers addresses the issue of tensile stress, enhancing mechanical strength and piezoelectric properties, thereby improving the yield and performance of microfabricated devices.
Patent Information
- Application Number
- JP2021022666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-16
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2041-02-16
AI Technical Summary
Conventional methods for reducing tensile stress in piezoelectric thin films deteriorate the orientation of the crystal structure of AlN, leading to a decrease in piezoelectric properties and mechanical strength, which is particularly problematic for microfabrication applications.
A piezoelectric thin film element comprising a substrate, a first electrode layer, a piezoelectric thin film made of aluminum nitride with controlled oxygen content between 0.001 and 6 atomic%, and a second electrode layer, where the oxygen concentration varies to balance mechanical strength and piezoelectric properties.
The proposed structure enhances the mechanical strength and piezoelectric properties of the thin film, reducing tensile stress and improving the yield rate by maintaining crystal orientation and reducing dielectric loss.
Smart Images

Figure 0007572871000003 
Figure 0007572871000004 
Figure 0007572871000005
Abstract
Description
[Technical field]
[0001] One aspect of the present invention relates to a piezoelectric thin film element. [Background technology]
[0002] In recent years, MEMS (Micro Electro Mechanical Systems) have been attracting attention. MEMS (Micro Electro Mechanical Systems) are devices in which mechanical components and electronic circuits are integrated on a single substrate by microfabrication technology. MEMS with functions such as sensors, transducers, filters, harvesters, and actuators use piezoelectric thin films. In the manufacture of MEMS using piezoelectric thin films, a lower electrode layer, a piezoelectric thin film, and an upper electrode layer are laminated on a substrate such as silicon or sapphire. MEMS with desired characteristics can be obtained through subsequent post-processing (microfabrication such as patterning, etching, and dicing). By selecting a piezoelectric thin film with excellent piezoelectric characteristics, the characteristics of piezoelectric thin film elements such as MEMS can be improved, and the piezoelectric thin film elements can be made smaller. The piezoelectric characteristics of a piezoelectric thin film are evaluated, for example, based on the positive piezoelectric constant (piezoelectric strain constant) d and the piezoelectric output coefficient g. g is expressed as d / ε0ε r where ε0 is the dielectric constant of a vacuum, and ε r is the relative dielectric constant of the piezoelectric thin film. Increasing d and g improves the characteristics of the piezoelectric thin film element.
[0003] Known examples of piezoelectric compositions that form the piezoelectric thin film include Pb(Zr,Ti)O3 (lead zirconate titanate, abbreviated as PZT), LiNbO3 (lithium niobate), AlN (aluminum nitride), ZnO (zinc oxide), and CdS (cadmium sulfide).
[0004] PZT and LiNbO3 have a perovskite structure. The d of a piezoelectric thin film having a perovskite structure is relatively large. However, when the piezoelectric thin film has a perovskite structure, d tends to decrease as the thickness of the piezoelectric thin film decreases. Therefore, a piezoelectric thin film having a perovskite structure is not suitable for microfabrication. In addition, the ε r Since is relatively large, g of a piezoelectric thin film having a perovskite structure tends to be relatively small.
[0005] On the other hand, AlN, ZnO and CdS have a wurtzite structure. The d of a piezoelectric thin film having a wurtzite structure is smaller than that of a piezoelectric thin film having a perovskite structure. However, the ε r Since is relatively small, a piezoelectric thin film having a wurtzite structure can have a larger g than a piezoelectric thin film having a perovskite structure. Therefore, for piezoelectric thin film elements that require a large g, a piezoelectric composition having a wurtzite structure is a promising material.
[0006] When a piezoelectric thin film containing AlN is formed on the surface of a lower electrode layer made of metal, tensile stress approximately parallel to the surface of the lower electrode layer is likely to occur in the piezoelectric thin film due to the interaction between AlN and the lower electrode layer. The piezoelectric thin film is likely to be destroyed due to this tensile stress (residual stress). For example, when the piezoelectric thin film is mechanically processed (diced, etc.), cracks are likely to be formed in the piezoelectric thin film along a direction approximately perpendicular to the surface of the lower electrode layer due to the tensile stress. Such destruction of the piezoelectric thin film deteriorates the piezoelectric characteristics and insulating properties of the piezoelectric thin film, and the yield rate of the piezoelectric thin film element decreases. Therefore, the tensile stress is reduced (alleviated) and high mechanical strength is required for the piezoelectric thin film element.
[0007] For example, the piezoelectric layer described in Patent Document 1 below has a laminated structure composed of a tensile stress layer and a compressive stress layer. By offsetting the tensile stress in the tensile stress layer with the compressive stress in the compressive stress layer, the mechanical strength of the piezoelectric layer is increased and cracks in the piezoelectric layer are suppressed.
[0008] The piezoelectric thin film described in Patent Document 2 below is composed of AlN crystal, in which a part of the Al in the AlN crystal is replaced with a first element, and a second element having an ionic radius larger than that of Al is added to the AlN crystal. Doping with the first and second elements reduces residual stress in the piezoelectric thin film. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2007 / 063842 Brochure [Patent Document 2] International Publication No. 2016 / 111280 Brochure Summary of the Invention [Problem to be solved by the invention]
[0010] Conventional methods for reducing the tensile stress in the piezoelectric thin film deteriorate the orientation of the AlN crystal structure, which in turn deteriorates the piezoelectric properties of the piezoelectric thin film. Therefore, a new method for reducing the tensile stress is required.
[0011] An object of one aspect of the present invention is to provide a piezoelectric thin film element having a piezoelectric thin film excellent in mechanical strength and piezoelectric characteristics. [Means for solving the problem]
[0012] A piezoelectric thin film element according to one aspect of the present invention comprises a substrate, a first electrode layer laminated on the substrate, a piezoelectric thin film laminated on the first electrode layer, and a second electrode layer laminated on the piezoelectric thin film, wherein the piezoelectric thin film contains aluminum nitride and oxygen, and the average oxygen concentration in the piezoelectric thin film is 0.001 atomic % or more and 6 atomic % or less.
[0013] The piezoelectric thin film may comprise a first piezoelectric layer laminated on a first electrode layer, and a second piezoelectric layer laminated on the first piezoelectric layer and in contact with a second electrode layer, and the concentration of oxygen in the first piezoelectric layer may be lower than the concentration of oxygen in the second piezoelectric layer.
[0014] The ratio of the thickness of the second piezoelectric layer to the thickness of the piezoelectric thin film may be 0.1% or more and 60% or less, and the ratio of the total amount of oxygen in the second piezoelectric layer to the total amount of oxygen in the piezoelectric thin film may be greater than 60% and less than 100%.
[0015] The oxygen concentration in the second piezoelectric layer may increase along a direction substantially perpendicular to the surface of the first electrode layer on which the piezoelectric thin film is laminated and from the first electrode layer toward the second electrode layer.
[0016] The first electrode layer may contain at least one element selected from the group consisting of platinum, iridium, gold, rhodium, palladium, silver, nickel, copper, aluminum, molybdenum, tungsten, vanadium, chromium, niobium, tantalum, ruthenium, zirconium, hafnium, titanium, yttrium, scandium, and magnesium. Effect of the Invention
[0017] According to one aspect of the present invention, there is provided a piezoelectric thin film element having a piezoelectric thin film excellent in mechanical strength and piezoelectric characteristics. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic cross-section of a piezoelectric thin film element according to one embodiment of the present invention, and the cross-section shown in FIG. 1 is approximately perpendicular to the lamination direction of the substrate, the first electrode layer, the piezoelectric thin film, and the second electrode layer. [Diagram 2] FIG. 2 is a perspective view of a unit cell of the crystal structure (wurtzite structure) of aluminum nitride. [Diagram 3] FIG. 3 shows an example of the oxygen concentration distribution in the piezoelectric thin film. [Figure 4] FIG. 4 shows another example of the oxygen concentration distribution in the piezoelectric thin film. [Diagram 5] FIG. 5 shows another example of the oxygen concentration distribution in the piezoelectric thin film. [Figure 6] FIG. 6 shows another example of the oxygen concentration distribution in the piezoelectric thin film. [Figure 7] FIG. 7 shows a profile of the temperature of the substrate in the process of forming the piezoelectric thin film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. The present invention is not limited to the following embodiments. In each drawing, the same or equivalent components are given the same reference numerals. X, Y, and Z shown in FIG. 1 represent three coordinate axes that are mutually orthogonal.
[0020] As shown in FIG. 1, the piezoelectric thin film element 10 according to this embodiment includes a substrate 6, an adhesive layer 5 directly laminated on the surface of the substrate 6, a first electrode layer 4 indirectly laminated on the surface of the substrate 6 via the adhesive layer 5, a piezoelectric thin film 3 directly or indirectly laminated on the surface of the first electrode layer 4, and a second electrode layer 7 directly or indirectly laminated on the surface of the piezoelectric thin film 3. The laminate direction of the substrate 6, the adhesive layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 is substantially parallel to the Z axis. The substrate 6, the adhesive layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may each have a flat shape extending along the XY plane direction (X axis and Y axis). The thickness of the substrate 6, the adhesive layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may each be substantially uniform. The adhesive layer 5 may directly cover a part or the whole of the surface of the substrate 6. The first electrode layer 4 may directly cover a part or the whole of the surface of the adhesive layer 5. The piezoelectric thin film 3 may directly or indirectly cover a part or the whole of the surface of the first electrode layer 4. The second electrode layer 7 may directly or indirectly cover a part or the whole of the surface of the piezoelectric thin film 3. The adhesion layer 5 is not essential for the piezoelectric thin film element 10, and the first electrode layer 4 may be directly laminated on the surface of the substrate 6. When the adhesion layer 5 is not present, the first electrode layer 4 may directly cover a part or the whole of the surface of the substrate 6. The first electrode layer 4 may be rephrased as a lower electrode layer. The second electrode layer 7 may be rephrased as an upper electrode layer. A first intermediate layer (first buffer layer) may be provided between the first electrode layer 4 and the piezoelectric thin film 3. For example, the first intermediate layer may be made of a conductor or a piezoelectric material. The lattice constant of the first intermediate layer in a direction substantially parallel to the surface of the first electrode layer 4 may be equal to or smaller than the lattice constant of the first electrode layer 4 in the same direction, and may be equal to or larger than the lattice constant of the piezoelectric thin film 3 in the same direction. A second intermediate layer (second buffer layer) may be provided between the piezoelectric thin film 3 and the second electrode layer 7. For example, the second intermediate layer may be made of a conductor or a piezoelectric material. The lattice constant of the second intermediate layer in a direction substantially parallel to the surface of the first electrode layer 4 may be equal to or smaller than the lattice constant of the second electrode layer 7 in the same direction, and may be equal to or larger than the lattice constant of the piezoelectric thin film 3 in the same direction.
[0021] The piezoelectric thin film 3 includes crystalline aluminum nitride (AlN). The AlN constituting the piezoelectric thin film 3 may be single crystal or polycrystalline. The crystal structure of AlN is a hexagonal wurtzite structure. FIG. 2 shows a unit cell ucw of the wurtzite structure. The unit cell ucw is a regular hexagonal column. The AlN in the piezoelectric thin film 3 may be columnar crystals extending in the normal direction to the surface of the first electrode layer 4.
[0022] The (001) and (002) planes of AlN in the piezoelectric thin film 3 may be approximately parallel to the surface of the first electrode layer 4 on which the piezoelectric thin film 3 is laminated. In other words, the (001) and (002) planes of AlN in the piezoelectric thin film 3 may be oriented in the normal direction to the surface of the first electrode layer 4. The (001) plane of AlN corresponds to a regular hexagonal crystal plane in the unit cell ucw shown in FIG. 2. When the piezoelectric thin film 3 includes a plurality of AlN crystalline grains, the (001) and (002) planes of some or all of the crystal grains may be approximately parallel to the surface of the first electrode layer 4.
[0023] The crystal orientation in which the piezoelectric properties of AlN are expressed is
[0001] of AlN. Therefore, the (001) and (002) planes of AlN are approximately parallel to the surface of the first electrode layer 4, so that the piezoelectric thin film 3 can have excellent piezoelectric properties. For the same reason, the (001) and (002) planes of the wurtzite structure of aluminum nitride may be approximately parallel to the surface of the piezoelectric thin film 3 that is in contact with the first electrode layer 4. In other words, the (001) and (002) planes of AlN in the piezoelectric thin film 3 may be oriented in the normal direction to the surface of the piezoelectric thin film 3.
[0024] The piezoelectric thin film 3 contains not only AlN but also oxygen (O), and the average concentration of oxygen in the piezoelectric thin film 3 is 0.001 atomic % or more and 6.000 atomic % or less. As a result, the piezoelectric thin film 3 can have high mechanical strength and excellent piezoelectric characteristics. The reasons for this are as follows.
[0025] Since the piezoelectric thin film 3 grows epitaxially on the surface of the crystalline first electrode layer 4, lattice mismatch between the piezoelectric thin film 3 and the first electrode layer 4 is likely to occur. As a result, stress that expands the wurtzite structure in the in-plane direction is likely to occur at the interface between the piezoelectric thin film 3 and the first electrode layer 4. In other words, tensile stress (residual stress) approximately parallel to the surface of the first electrode layer 4 is likely to occur in the piezoelectric thin film 3. If the piezoelectric thin film 3 does not contain oxygen, the tensile stress will likely cause the piezoelectric thin film 3 to break in a direction approximately parallel to the surface of the first electrode layer 4. For example, the tensile stress will likely cause cracks to form in the piezoelectric thin film 3 along a direction approximately perpendicular to the surface of the first electrode layer 4. As a result, the piezoelectric properties and insulating properties of the piezoelectric thin film 3 will deteriorate. However, since the piezoelectric thin film 3 according to this embodiment contains oxygen, the crystal lattice of AlN constituting the piezoelectric thin film 3 contains oxygen atoms. Due to the crystal lattice of AlN containing oxygen atoms, the crystal structure of AlN expands in a direction substantially parallel to the surface of the first electrode layer 4. That is, the lattice constant of AlN increases in a direction substantially parallel to the surface of the first electrode layer 4. As a result, the lattice mismatch between the piezoelectric thin film 3 and the first electrode layer 4 is reduced, the tensile stress in the piezoelectric thin film 3 is reduced (relaxed), and the piezoelectric thin film 3 can have high mechanical strength. That is, the destruction of the piezoelectric thin film 3 caused by the residual stress in the piezoelectric thin film 3 is suppressed. As a result, the piezoelectric characteristics and insulating properties of the piezoelectric thin film 3 are improved. For the same reason as above, the destruction of the piezoelectric thin film 3 during the manufacturing process of the piezoelectric thin film element 10 according to this embodiment is suppressed, and the yield rate of the piezoelectric thin film element 10 is increased. As the average oxygen concentration in the piezoelectric thin film 3 decreases, the crystallinity of AlN and the orientation of AlN improve, and there is a tendency for the piezoelectric characteristics of the piezoelectric thin film 3 to improve. However, if the average oxygen concentration in the piezoelectric thin film 3 is lower than 0.001 atomic %, the amount of oxygen in the piezoelectric thin film 3 is too small, so that the tensile stress in the piezoelectric thin film 3 is not sufficiently reduced, making it difficult for the piezoelectric thin film 3 to have high mechanical strength. As the average oxygen concentration in the piezoelectric thin film 3 increases, the tensile stress in the piezoelectric thin film 3 decreases and the mechanical strength of the piezoelectric thin film 3 tends to increase. However, if the average oxygen concentration in the piezoelectric thin film 3 is higher than 6.000 atomic %, there is too much oxygen in the piezoelectric thin film 3, which deteriorates the crystallinity and orientation of AlN, making it difficult for the piezoelectric thin film 3 to have excellent piezoelectric properties. The dielectric loss tangent (tan δ) of the piezoelectric thin film 3 tends to increase as the average oxygen concentration in the piezoelectric thin film 3 increases. In particular, when the average oxygen concentration in the piezoelectric thin film 3 is higher than 6.000 atomic %, the dielectric loss tangent of the piezoelectric thin film 3 is significantly large. It is preferable that the dielectric loss tangent of the piezoelectric thin film 3 is small. For example, the dielectric loss tangent of the piezoelectric thin film 3 may be 0% or more and 5% or less, 0% or more and 3% or less, 0% or more and 2% or less, or 0% or more and 1% or less. Since the piezoelectric thin film 3 is likely to have high mechanical strength and excellent piezoelectric characteristics, and the dielectric tangent of the piezoelectric thin film 3 is likely to be reduced, the average oxygen concentration in the piezoelectric thin film 3 may be 0.021 atomic % or more and 5.800 atomic % or less.
[0026] The piezoelectric thin film 3 may be composed of a first piezoelectric layer 1 laminated directly on the first electrode layer 4, and a second piezoelectric layer 2 laminated directly on the first piezoelectric layer 1 and in contact with the second electrode layer 7. The oxygen concentration in the first piezoelectric layer 1 may be lower than the oxygen concentration in the second piezoelectric layer 2. The average oxygen concentration in the first piezoelectric layer 1 may be lower than the average oxygen concentration in the second piezoelectric layer 2. The first piezoelectric layer 1 may not contain oxygen. The first piezoelectric layer 1 may contain oxygen. The thickness T1 of the first piezoelectric layer 1 may be approximately uniform. The thickness T2 of the second piezoelectric layer 2 may be approximately uniform. T3 of the piezoelectric thin film 3 is equal to T1 + T2. In the process of forming the piezoelectric thin film 3, after the first piezoelectric layer 1 grows on the surface of the first electrode layer 4, the second piezoelectric layer 2 grows continuously on the first piezoelectric layer 1. Therefore, the crystallinity and orientation of AlN contained in the second piezoelectric layer 2 depend on the crystallinity and orientation of AlN contained in the first piezoelectric layer 1. That is, due to the improvement of the crystallinity of AlN contained in the first piezoelectric layer 1, the crystallinity of AlN contained in the second piezoelectric layer 2 is also improved, and due to the orientation of the (001) plane of AlN contained in the first piezoelectric layer 1, the (001) plane of AlN contained in the second piezoelectric layer 2 is also oriented in the same direction. In addition, with a decrease in the concentration of oxygen in the first piezoelectric layer 1, the crystallinity and orientation of AlN contained in the first piezoelectric layer 1 are improved. For the above reasons, when the concentration of oxygen in the first piezoelectric layer 1 is lower than the concentration of oxygen in the second piezoelectric layer 2, the AlN contained in the second piezoelectric layer 2 inherits the excellent crystallinity and orientation of AlN contained in the first piezoelectric layer 1, and the crystallinity and orientation of AlN in the entire piezoelectric thin film 3 are improved. As a result, the piezoelectric thin film 3 can have excellent piezoelectric characteristics. Furthermore, when the oxygen concentration in second piezoelectric layer 2 is higher than the oxygen concentration in first piezoelectric layer 1, oxygen located near the surface of second piezoelectric layer 2 in contact with second electrode layer 7 tends to bond with elements (metal elements, etc.) constituting second piezoelectric layer 2. As a result, second electrode layer 7 tends to adhere to second piezoelectric layer 2, and peeling of second electrode layer 7 from second piezoelectric layer 2 (piezoelectric thin film 3) is suppressed.
[0027] The ratio (T2 / T3) of the thickness T2 of the second piezoelectric layer 2 to the thickness T3 of the piezoelectric thin film 3 may be 0.1% or more and 60% or less, and the ratio of the total amount of oxygen in the second piezoelectric layer 2 to the total amount of oxygen in the piezoelectric thin film 3 may be more than 60% and 100% or less. The unit of the total amount of oxygen may be moles. The unit of the ratio of the total amount of oxygen in the second piezoelectric layer 2 to the total amount of oxygen in the piezoelectric thin film 3 may be mole % or atomic %. When T2 / T3 is 0.1% or more, the piezoelectric thin film 3 is likely to have a sufficiently high mechanical strength. When T2 / T3 is 60% or less, the piezoelectric thin film 3 is likely to have a sufficiently high mechanical strength without impairing the piezoelectric characteristics of the piezoelectric thin film 3, and the dielectric loss tangent of the piezoelectric thin film 3 is likely to be reduced. When the ratio of the total amount of oxygen in the second piezoelectric layer 2 to the total amount of oxygen in the piezoelectric thin film 3 is greater than 60%, the piezoelectric thin film 3 is likely to have a sufficiently high mechanical strength. Since the piezoelectric thin film 3 is likely to have high mechanical strength and excellent piezoelectric characteristics, T2 / T3 may be 1% or more and 60% or less. Since the piezoelectric thin film 3 is likely to have high mechanical strength and excellent piezoelectric characteristics, the ratio of the total amount of oxygen in the second piezoelectric layer 2 to the total amount of oxygen in the piezoelectric thin film 3 may be more than 60% and 99.9% or less, or 64% or more and 95% or less.
[0028] The thickness T3 of the piezoelectric thin film 3 may be, for example, 100 nm or more and 30,000 nm or less, or 200 nm or more and 2,000 nm or less. The thickness T2 of the second piezoelectric layer 2 may be, for example, (0.001×T3) nm or more and (0.600×T3) nm or less. The thickness T2 of the second piezoelectric layer 2 may be, for example, 10 nm or more and 1,200 nm or less. The thickness T1 of the first piezoelectric layer 1 is equal to T3−T2. The thickness T1 of the first piezoelectric layer 1 may be, for example, 300 nm or more and 990 nm or less.
[0029] The direction that is approximately perpendicular to the surface of the first electrode layer 4 and faces from the first electrode layer 4 to the second electrode layer 7 is represented as the thickness direction D of the piezoelectric thin film 3. The
[0001] (crystal orientation) of AlN contained in the piezoelectric thin film 3 may be approximately parallel to the thickness direction D. Specific examples of the oxygen concentration distribution in the piezoelectric thin film 3 along the thickness direction D are shown in Figures 3, 4, 5, and 6. The horizontal axis shown in each figure indicates the distance d (unit: nm) from the surface of the first electrode layer 4 in the thickness direction D, and corresponds to an arbitrary position in the piezoelectric thin film 3. The vertical axis of the graph shown in each figure indicates the oxygen concentration [O] (unit: atomic %) at the distance d from the surface of the first electrode layer 4.
[0030] The oxygen concentration in the second piezoelectric layer 2 may increase gradually or stepwise along the thickness direction D. That is, the oxygen concentration distribution in the second piezoelectric layer 2 may have an increasing gradient along the thickness direction D. When the oxygen concentration in the second piezoelectric layer 2 increases along the thickness direction D, the tensile stress in the piezoelectric thin film 3 is likely to be reduced, and the piezoelectric thin film 3 is likely to have high mechanical strength.
[0031] As shown in FIG. 3, the concentration distribution of oxygen in the second piezoelectric layer 2 may be represented by a straight line.
[0032] 4, the oxygen concentration distribution in the second piezoelectric layer 2 may be represented by a downwardly convex curve. In the case of the oxygen concentration distribution shown in FIG. 4, oxygen is localized near the surface of the second piezoelectric layer 2 that contacts the second electrode layer 7. As a result, the piezoelectric thin film 3 is likely to have sufficiently high mechanical strength without impairing the piezoelectric characteristics of the piezoelectric thin film 3, and the second electrode layer 7 is likely to adhere to the second piezoelectric layer 2.
[0033] As shown in FIG. 5, the concentration distribution of oxygen in the second piezoelectric layer 2 may be represented by an upwardly convex curve.
[0034] As shown in FIG. 6, the concentration of oxygen in the second piezoelectric layer 2 may be approximately uniform.
[0035] 3, 4, 5, and 6, the oxygen concentration in the first piezoelectric layer 1 may be approximately uniform. When the oxygen concentration in the first piezoelectric layer 1 is approximately uniform, the crystallinity and orientation of AlN in the entire piezoelectric thin film 3 are likely to be improved. However, the oxygen concentration in the first piezoelectric layer 1 may increase along the thickness direction D.
[0036] The average oxygen concentration [O]1 in the first piezoelectric layer 1 may be, for example, 0.000 atomic % or more and 5.000 atomic % or less, or 0.001 atomic % or more and 5.000 atomic % or less. [O]1 may be, for example, a value obtained by dividing the integral of the oxygen concentration distribution in the first piezoelectric layer 1 along the thickness direction D by the thickness T1 of the first piezoelectric layer 1.
[0037] The average oxygen concentration [O]2 in the second piezoelectric layer 2 may be, for example, 2.000 atomic % or more and 6.000 atomic % or less. [O]2 may be, for example, a value obtained by dividing the integral of the oxygen concentration distribution in the second piezoelectric layer 2 along the thickness direction D by the thickness T2 of the second piezoelectric layer 2.
[0038] As described above, the average oxygen concentration [O]3 in the piezoelectric thin film 3 is 0.001 atomic % or more and 6.000 atomic % or less. [O]3 may be, for example, a value obtained by dividing the integral of the oxygen concentration distribution in the piezoelectric thin film 3 along the thickness direction D by the thickness T3 of the piezoelectric thin film 3. [O]3 is equal to the weighted average value of [O]1 and [O]2 based on T1 and T2. In other words, [O]3 is equal to (T1 / T3) × [O]1 + (T2 / T3) × [O]2.
[0039] The first piezoelectric layer 1 and the second piezoelectric layer 2 may be distinguished from each other based on the difference in oxygen concentration. For example, the interface between the first piezoelectric layer 1 and the second piezoelectric layer 2 may be a plane including a bending point or an inflection point of a line showing the oxygen concentration distribution in the piezoelectric thin film 3 along the thickness direction D.
[0040] The oxygen concentration may be approximately uniform throughout the piezoelectric thin film 3. The piezoelectric thin film 3 may not be composed of the first piezoelectric layer 1 and the second piezoelectric layer 2, the oxygen concentration in the piezoelectric thin film 3 may increase continuously along the thickness direction D, and the line showing the oxygen concentration distribution in the piezoelectric thin film 3 along the thickness direction D may not have any bending points or inflection points.
[0041] The piezoelectric thin film 3 may be composed of only Al, N, and O. However, the piezoelectric thin film 3 may further contain other elements in addition to Al, N, and O, as long as the mechanical strength and piezoelectric properties of the piezoelectric thin film 3 are not impaired. For example, the piezoelectric thin film 3 may further contain at least one additive element selected from the group consisting of a monovalent metal element Mm, a divalent metal element Md, a trivalent metal element Mtr, a tetravalent metal element Mt, and a pentavalent metal element Mp. Doping AlN with the additive element distorts the wurtzite structure of AlN or changes the strength of the chemical bonds between atoms in the wurtzite structure. As a result, the piezoelectric properties of the piezoelectric thin film 3 may be improved. The monovalent metal element Mm may be at least one element selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb) and cesium (Cs). The divalent metal element Md may be at least one selected from the group consisting of magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba). The trivalent metal element Mtr may be at least one element selected from the group consisting of Sc (scandium), Y (yttrium), lanthanoids, and In (indium). The tetravalent metal element Mt may be at least one selected from the group consisting of germanium (Ge), titanium (Ti), zirconium (Zr) and hafnium (Hf). The pentavalent metal element Mp may be at least one element selected from the group consisting of Cr (chromium), V (vanadium), Nb (niobium) and Ta (tantalum). The average valence of the additive element contained in the piezoelectric thin film 3 may be three. The total content of monovalent metal element Mm in aluminum nitride may be expressed as [Mm] atomic %. The total content of pentavalent metal element Mp in aluminum nitride may be expressed as [Mp] atomic %. [Mm] / [Mp] may be approximately 1.0. The total content of the divalent metal element Md in the aluminum nitride may be expressed as [Md] atomic %. The total content of the tetravalent metal element Mt in the aluminum nitride may be expressed as [Mt] atomic %. [Md] / [Mt] may be approximately 1.0.
[0042] The substrate 6 may be, for example, a semiconductor substrate (such as a silicon substrate or a gallium arsenide substrate), an optical crystal substrate (such as a sapphire substrate), an insulating substrate (such as a glass substrate or a ceramic substrate), or a metal substrate (such as a stainless steel plate).
[0043] The first electrode layer 4 may contain at least one element (metal Me) selected from the group consisting of Pt (platinum), Ir (iridium), Au (gold), Rh (rhodium), Pd (palladium), Ag (silver), Ni (nickel), Cu (copper), Al (aluminum), Mo (molybdenum), W (tungsten), V (vanadium), Cr (chromium), Nb (niobium), Ta (tantalum), Ru (ruthenium), Zr (zirconium), Hf (hafnium), Ti (titanium), Y (yttrium), Sc (scandium), and Mg (magnesium). The first electrode layer 4 may be made of only one type of metal Me. The first electrode layer 4 may be made of only at least two types of metal Me. In other words, the first electrode layer 4 may be made of only an alloy composed of at least two types of metal Me. The first electrode layer 4 may further contain an element other than the metal Me. The metal Me constituting the first electrode layer 4 may have a crystalline structure. That is, the first electrode layer 4 may be crystalline. For example, when the metal Me is at least one element selected from the group consisting of Pt, Ir, Au, Rh, Pd, Ag, Ni, Cu, and Al, the metal Me is likely to have a face-centered cubic (fcc) structure, and the (111) plane of the fcc structure is likely to be oriented in the normal direction to the surface of the first electrode layer 4. When the metal Me is at least one element selected from the group consisting of Mo, W, V, Cr, Nb, and Ta, the metal Me is likely to have a body-centered cubic (bcc) structure, and the (110) plane of the bcc structure is likely to be oriented in the normal direction to the surface of the first electrode layer 4. When the metal Me is at least one element selected from the group consisting of Ru, Zr, Hf, Ti, Y, Sc, and Mg, the metal Me tends to have a hexagonal close-packed (hcp) structure, and the (001) plane of the hcp structure tends to be oriented in the normal direction to the surface of the first electrode layer 4.
[0044] In a direction substantially parallel to the surface of the first electrode layer 4, the lattice length of the crystal structure of the metal Me may be larger than that of AlN. For example, in a direction substantially parallel to the surface of the first electrode layer 4, the atomic interval in the crystal structure of the metal Me may be larger than that of AlN. Or, in a direction substantially parallel to the surface of the first electrode layer 4, the lattice constant of the crystal structure of the metal Me may be larger than that of AlN. For example, the lattice length in the crystal structure of molybdenum is larger than that of AlN. When the lattice length in the crystal structure of the metal Me is larger than that of AlN in a direction substantially parallel to the surface of the first electrode layer 4, tensile stress is likely to occur in the conventional piezoelectric thin film in a direction substantially parallel to the surface of the first electrode layer 4 due to lattice mismatch between the first electrode layer 4 (metal Me) and the conventional piezoelectric thin film (AlN). However, since the piezoelectric thin film 3 according to this embodiment contains oxygen, the tensile stress in the piezoelectric thin film 3 is reduced, and the piezoelectric thin film 3 can have high mechanical strength.
[0045] The adhesion layer 5 may contain at least one element selected from the group consisting of Al (aluminum), Si (silicon), Ti (titanium), Zn (zinc), Y (yttrium), Zr (zirconium), Cr (chromium), Nb (niobium), Mo (molybdenum), Hf (hafnium), Ta (tantalum), W (tungsten) and Ce (cerium). The adhesion layer 5 may be a metal element, an alloy or a compound (oxide, etc.). The adhesion layer 5 may be composed of another piezoelectric thin film, a polymer or a ceramic. Due to the presence of the adhesion layer 5, the (111) plane of the fcc structure of the first electrode layer 4 is easily oriented in the normal direction to the surface of the first electrode layer 4. Alternatively, due to the presence of the adhesion layer 5, the (110) plane of the bcc structure of the first electrode layer 4 is easily oriented in the normal direction to the surface of the first electrode layer 4. Alternatively, the presence of the adhesion layer 5 makes it easier for the (001) plane of the hcp structure of the first electrode layer 4 to be oriented in the normal direction to the surface of the first electrode layer 4. The adhesion layer 5 also has a function of suppressing peeling of the first electrode layer 4 due to mechanical impact or the like. The adhesion layer 5 may be referred to as an interface layer, a support layer, a buffer layer, or an intermediate layer.
[0046] The second electrode layer 7 may contain at least one element selected from the group consisting of Pt, Ir, Au, Rh, Pd, Ag, Ni, Cu, Al, Mo, W, V, Cr, Nb, Ta, Ru, Zr, Hf, Ti, Y, Sc, and Mg. The second electrode layer 7 may be a simple metal. The second electrode layer 7 may be an alloy containing at least two elements selected from the above group.
[0047] The thickness of the substrate 6 may be, for example, 50 μm or more and 10000 μm or less. The thickness of the adhesion layer 5 may be, for example, 0.003 μm or more and 1 μm or less. The thickness of the first electrode layer 4 may be, for example, 0.01 μm or more and 1 μm or less. The thickness of the second electrode layer 7 may be, for example, 0.01 μm or more and 1 μm or less.
[0048] The adhesion layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may be laminated on the surface of the substrate 6 by a vapor phase growth method such as sputtering. The adhesion layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may be formed by sputtering using at least one type of target. The adhesion layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may be formed by sputtering using multiple targets. The target may contain at least one of the elements constituting each layer or piezoelectric thin film. By selecting and combining targets having a predetermined composition, each layer and each piezoelectric thin film 3 having a desired composition can be formed. For example, the target may be a metal element, an alloy, or an oxide. The composition of the sputtering atmosphere may be a control factor for the composition of each layer and each piezoelectric thin film 3. The input power (power density) given to each target is a control factor for the composition and thickness of each layer and each piezoelectric thin film 3. The total pressure of the sputtering atmosphere, the partial pressure or concentration of the source gas (e.g., nitrogen) in the atmosphere, the duration of sputtering of each target, the temperature of the substrate surface on which the piezoelectric thin film is formed, and the substrate bias are also factors that control the composition and thickness of each layer and piezoelectric thin film 3. By etching (e.g., plasma etching), a piezoelectric thin film having a desired shape or pattern may be formed.
[0049] The sputtering atmosphere (film-forming atmosphere) for forming the piezoelectric thin film 3 contains nitrogen gas (N2) and oxygen gas (O2). The oxygen contained in the piezoelectric thin film 3 originates from the oxygen in the film-forming atmosphere. For example, the film-forming atmosphere may be a mixed gas containing a rare gas (argon, etc.), nitrogen gas, and oxygen gas. The partial pressure of oxygen gas in the film-forming atmosphere is, for example, 5.11×10 -7 The partial pressure of oxygen gas in the film formation atmosphere may be 5.11×10 -7 If the partial pressure of oxygen gas in the film formation atmosphere is too low, the average oxygen concentration in the piezoelectric thin film 3 tends to be lower than 0.001 atomic %.
[0050] The temperature profile of the substrate 6 in the process of forming the piezoelectric thin film 3 is shown in Fig. 7. The horizontal axis of Fig. 7 represents time (unit: seconds), and the vertical axis of Fig. 7 represents the temperature of the substrate 6 (unit: ° C.).
[0051] When forming a piezoelectric thin film 3 having a substantially uniform oxygen concentration, the process of forming the piezoelectric thin film 3 includes a first heating process for raising the temperature of the substrate 6 from the initial temperature T0 to an initial film formation temperature TI, and a first film formation process for maintaining the temperature of the substrate 6 at the initial film formation temperature TI in a film formation atmosphere. The first heating process may be performed before the sputtering of the target containing Al is started. That is, the first film formation process (growth of the piezoelectric thin film 3 in the film formation atmosphere) may be started with the start of sputtering of the target. When forming a piezoelectric thin film 3 having a substantially uniform oxygen concentration, the initial film formation temperature TI is, for example, higher than 300° C. and lower than 400° C., and preferably 350° C. As the initial film formation temperature TI increases, the oxygen concentration in the piezoelectric thin film 3 tends to increase. When the initial film formation temperature TI is lower than 350° C., the average oxygen concentration in the piezoelectric thin film 3 tends to be lower than 0.001 atomic %. When the initial deposition temperature T i is higher than 350° C., the average oxygen concentration in the piezoelectric thin film 3 tends to be higher than 6 atomic %. TOTAL is equal to the duration of the first film formation step (first film formation time ti).
[0052] When forming a piezoelectric thin film 3 consisting of a first piezoelectric layer 1 and a second piezoelectric layer 2, the process of forming the piezoelectric thin film 3 further includes a second temperature increase process following the first temperature increase process and the first film formation process. The second temperature increase process is a process of increasing the temperature of the substrate 6 from the initial film formation temperature TI to the final film formation temperature TF. When forming a piezoelectric thin film 3 consisting of a first piezoelectric layer 1 and a second piezoelectric layer 2, the process of forming the piezoelectric thin film 3 may further include a second film formation process following the above-mentioned second temperature increase process. The second film formation process is a process of maintaining the temperature of the substrate 6 at the final film formation temperature TF in the film formation atmosphere. The first piezoelectric layer 1 may be formed in the first film formation process. The second temperature increase process and the second film formation process may form a second piezoelectric layer 2 having a gradient in the concentration distribution of oxygen. The inventors presume that the second piezoelectric layer 2 having a high oxygen concentration is formed because oxygen in the film formation atmosphere is easily ionized with the temperature increase of the substrate 6 in the second temperature increase process. When forming the piezoelectric thin film 3 consisting of the first piezoelectric layer 1 and the second piezoelectric layer 2, the initial film formation temperature TI may be, for example, 200° C. or more and 300° C. or less. As the initial film formation temperature TI increases, the oxygen concentration in the first piezoelectric layer 1 tends to increase. T ) may be, for example, 1.0° C. / sec or more and 1.9 seconds or less. The final film formation temperature TF may be, for example, 230° C. or more and 350° C. or less. As the final film formation temperature TF increases, the oxygen concentration in the second piezoelectric layer 2 tends to increase. When the final film formation temperature TF is higher than 350° C., the average oxygen concentration in the piezoelectric thin film 3 tends to be higher than 6 atomic %. When forming a piezoelectric thin film 3 consisting of the first piezoelectric layer 1 and the second piezoelectric layer 2, the film formation time t TOTAL is the sum of the first film formation time ti, the time required for the second temperature rise step, and the duration of the second film formation step (second film formation time tf). When forming a piezoelectric thin film 3 consisting of a first piezoelectric layer 1 and a second piezoelectric layer 2, the first film formation time ti can be rephrased as the time from the start of the first film formation step to the start of the second temperature rise step.
[0053] Film forming time t TOTAL The unit of each of the first deposition time ti and the second deposition time tf may be seconds. TOTALAs the time required for the second heating step and the second film formation time tf increase, the thickness T2 of the second piezoelectric layer 2 tends to increase. As the time required for the second heating step and the second film formation time tf increase, the thickness T3 of the piezoelectric thin film 3 tends to increase. As the time required for the second heating step and the second film formation time tf increase, the thickness T1 of the first piezoelectric layer 1 tends to increase.
[0054] The crystal structures of the adhesion layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may be identified by X-ray diffraction (XRD). The composition of each layer and the piezoelectric thin film 3 may be identified by at least one of the following analytical methods: X-ray fluorescence analysis (XRF), X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray analysis (EDX), inductively coupled plasma mass spectrometry (ICP-MS), laser ablation inductively coupled plasma mass spectrometry (LA-ICP-MS), and electron probe microanalyzer (EPMA). The thicknesses of the adhesion layer 5, the first electrode layer 4, the piezoelectric thin film 3, and the second electrode layer 7 may be measured by a scanning electron microscope (SEM) in a cross section of the piezoelectric thin film element 10 parallel to the thickness direction D. The concentration distributions of Al, N, and O in the piezoelectric thin film 3 along the thickness direction D may be measured, for example, by photoelectron spectroscopy (XPS). A cross section of the piezoelectric thin film 3 parallel to the thickness direction D may be observed by SEM, and the concentration distributions of Al, N, and O in the piezoelectric thin film 3 along the thickness direction D may be measured by linear analysis using EDX on the cross section of the piezoelectric thin film 3. Based on the concentration distribution of O in the piezoelectric thin film 3 along the thickness direction D, the thickness T1 of the first piezoelectric layer 1 and the thickness T2 of the second piezoelectric layer 2 may be determined.
[0055] The piezoelectric thin film element according to the present embodiment has a wide variety of applications. For example, the piezoelectric thin film element may be a piezoelectric actuator. The piezoelectric actuator may be used for haptics. That is, the piezoelectric actuator may be used in various devices that require feedback by skin sensation (touch). The device that requires feedback by skin sensation may be a wearable device, a touch pad, a display, or a game controller. The piezoelectric actuator may be used in a head assembly, a head stack assembly, or a hard disk drive. The piezoelectric actuator may be used in a printer head or an inkjet printer device. The piezoelectric actuator may be used in a piezoelectric switch. The piezoelectric thin film element may be a piezoelectric sensor or a piezoelectric transducer. The piezoelectric sensor or the piezoelectric transducer may be used in, for example, a gyro sensor, a pressure sensor, a pulse wave sensor, an ultrasonic sensor, an ultrasonic transducer, or a shock sensor. The ultrasonic transducer may be a piezoelectric micromachined ultrasonic transducer (PMUT). Products using the piezoelectric micromechanical ultrasonic transducer may be, for example, biometric sensors, medical / healthcare sensors (fingerprint sensors, or ultrasonic blood vessel authentication sensors), or ToF (Time of Flight) sensors. The piezoelectric thin film element may be used in a piezoelectric microphone, a filter (SAW filter or BAW filter), a harvester, an oscillator, a resonator, or an acoustic multilayer film. Each of the above-mentioned piezoelectric thin film elements may be a part or the whole of a MEMS.
[0056] The present invention is not limited to the above embodiment. For example, the concentration of oxygen in the first piezoelectric layer 1 may be higher than the concentration of oxygen in the second piezoelectric layer 2. EXAMPLES
[0057] The present invention will be described in detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples.
[0058] Example 1 A wafer made of single crystal Si was used as the substrate. The surface of the substrate was parallel to the (100) plane of Si. The thickness of the substrate was 725 μm. The diameter of the substrate was approximately 8 inches. The thickness of the substrate was uniform.
[0059] A first electrode layer (lower electrode layer) made of Mo was formed directly on the entire surface of the adhesive layer by RF magnetron sputtering in a vacuum chamber. Mo alone was used as the sputtering target. The atmosphere in the vacuum chamber was Ar gas. The input power per unit area of the sputtering target was 0.93 W / cm. 2 The temperature of the substrate during the formation of the first electrode layer was maintained at 600° C. The first electrode layer had a uniform thickness. The first electrode layer had a thickness of 0.2 μm.
[0060] In the process of forming the piezoelectric thin film, the piezoelectric thin film was formed directly on the entire surface of the first electrode layer by RF magnetron sputtering in a vacuum chamber. A single aluminum alloy was used as the sputtering target. The input power per unit area of the sputtering target was 3.72 W / cm. 2 In the piezoelectric thin film formation process, the above-mentioned first heating step and first film formation step were performed. In the case of Example 1, the above-mentioned second heating step and second film formation step were not performed. The film formation atmosphere for the piezoelectric thin film was a mixed gas consisting of Ar, N2, and O2. The total pressure of the film formation atmosphere was 0.4 Pa. The partial pressure of O2 in the film formation atmosphere was 5.11×10 -7 Maintained in Pa.
[0061] Film formation time t TOTAL and the initial film formation temperature TI are shown in the following Table 1. The thickness T3 of the piezoelectric thin film in Example 1 was adjusted to the values shown in the following Tables 1 and 2. The thickness T3 of the piezoelectric thin film was uniform.
[0062] A second electrode layer made of Mo was formed directly on the entire surface of the piezoelectric thin film in the same manner as the first electrode layer. The thickness of the second electrode layer was the same as that of the first electrode. The thickness of the second electrode layer was uniform.
[0063] The laminate produced by the above procedure was composed of a substrate, a first electrode layer directly laminated on the substrate, a piezoelectric thin film directly laminated on the first electrode layer, and a second electrode directly laminated on the piezoelectric thin film. The laminate structure on the substrate was then patterned by photolithography. After patterning, the entire laminate was cut by dicing to obtain a rectangular piezoelectric thin film element of Example 1. The piezoelectric thin film element was composed of a substrate, a first electrode layer directly laminated on the substrate, a piezoelectric thin film directly laminated on the first electrode layer, and a second electrode layer directly laminated on the piezoelectric thin film.
[0064] By the above method, a plurality of piezoelectric thin film elements were produced according to Example 1. The following analyses and measurements were carried out on these piezoelectric thin film elements.
[0065] <Overall composition of piezoelectric thin film> The composition of the entire piezoelectric thin film was analyzed by X-ray fluorescence analysis (XRF method). A wavelength dispersive X-ray fluorescence spectrometer (RIGAKU AZX-400) manufactured by Rigaku Corporation was used for the XRF method. The concentrations (unit: atomic %) of Al, N, and O in the piezoelectric thin film were quantified by the XRF method.
[0066] <Element concentration distribution in the thickness direction D in the piezoelectric thin film> The concentration distributions of Al, N, and O in the piezoelectric thin film along the thickness direction D described above were measured by X-ray photoelectron spectroscopy (XPS). That is, XPS was continuously performed on the surface of the piezoelectric thin film while gradually and uniformly reducing the thickness T3 of the piezoelectric thin film by sputtering the surface of the piezoelectric thin film directly laminated on the first electrode layer. For the XPS method, an X-ray photoelectron spectroscopy device (PHI Quantera IITM) manufactured by ULVAC-PHI, Inc. was used.
[0067] <Crystal structure of piezoelectric thin film> The crystal structure of the piezoelectric thin film formed directly on the first electrode layer was analyzed by X-ray diffraction (XRD). A multipurpose X-ray diffractometer (SmartLab) manufactured by Rigaku Corporation was used for the XRD method. 2θ-θ scan, ω scan, and 2θχ-φ scan were performed on the surface of the piezoelectric thin film formed directly on the first electrode layer using the above-mentioned X-ray diffractometer. The analysis based on the XRD method confirmed that the piezoelectric thin film had a wurtzite structure. The (002) plane of the wurtzite structure was parallel to the surface of the first electrode layer with which the piezoelectric thin film was in contact. The (110) plane of Mo (body-centered cubic structure) constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer with which the piezoelectric thin film was in contact.
[0068] From the above analysis, it was confirmed that the piezoelectric thin film of Example 1 has the following characteristics.
[0069] The piezoelectric thin film of Example 1 was made of crystalline AlN containing oxygen, and the AlN had a wurtzite structure. The (002) plane of the AlN was oriented in the thickness direction D of the piezoelectric thin film (the normal direction to the surface of the first electrode layer). The oxygen concentration in the piezoelectric thin film of Example 1 was uniform in the thickness direction D. The average oxygen concentration [O]3 in the piezoelectric thin film of Example 1 is shown in Table 2 below.
[0070] <Dielectric tangent> The dielectric loss tangent (tan δ) of the piezoelectric thin film of Example 1 was measured. An LCR meter (E4980A) manufactured by Agilent was used to measure tan δ. In measuring tan δ, an electric field of 1 V / μm was applied to the piezoelectric thin film. The areas of the portions of the first electrode layer and the second electrode layer to which the electric field was applied were 600×600 μm 2 The tan δ of Example 1 is shown in Table 2 below.
[0071] <Piezoelectric constant d 33 > Piezoelectric constant d of the piezoelectric thin film of Example 1 33 (Unit: pC / N) was measured. 33 The details of the measurement of the piezoelectric constant d 33(Average value of three measurement points) is shown in Table 2 below. Measurement equipment: Piezotest 33 Meter (PM200) Frequency: 110Hz Clamping pressure: 0.25N
[0072] <Crack rate Rc> 100 samples were prepared by dicing the piezoelectric thin film element in the lamination direction. The dimensions of each sample were uniform, and each sample was a chip-shaped piezoelectric thin film element. The presence or absence of electrical continuity in the piezoelectric thin film of each sample was inspected by applying an electric field of 0.4 V / μm to the piezoelectric thin film of each sample. A commercially available multimeter was used for the electrical continuity inspection. The number n of samples in which electrical continuity was detected in the piezoelectric thin film was counted out of the 100 samples. The crack rate Rc is defined as n%. When the above-mentioned cracks caused by dicing are formed in the piezoelectric thin film of each sample, the cracks function as a conductive path, and therefore electrical continuity in the piezoelectric thin film of each sample is detected. The higher the mechanical strength of the piezoelectric thin film, the more cracks caused by dicing are suppressed, and the lower the crack rate Rc. The crack rate Rc of Example 1 is shown in Table 2 below.
[0073] (Examples 2 to 6) In the process of forming the piezoelectric thin film in each of Examples 2 to 6, the first heating step and the first film-forming step were followed by the above-mentioned second heating step and second film-forming step.
[0074] The deposition time t for each of Examples 2 to 6 TOTAL , initial deposition temperature TI, final deposition temperature TF, first deposition time ti, second deposition time tf, and second heating rate R T is shown in the following Table 1. The thickness T3 of the piezoelectric thin film in each of Examples 2 to 6 was adjusted to the value shown in the following Tables 1 and 2. The thickness T3 of the piezoelectric thin film in each of Examples 2 to 6 was uniform.
[0075] Except for the piezoelectric thin film formation process, the piezoelectric thin film elements of Examples 2 to 6 were fabricated in the same manner as Example 1. Analysis and measurement of the piezoelectric thin film elements of Examples 2 to 6 were carried out in the same manner as Example 1. As a result of the analysis, it was confirmed that the piezoelectric thin film of each of Examples 2 to 6 had the following characteristics.
[0076] The piezoelectric thin film was made of crystalline AlN containing oxygen, and the AlN had a wurtzite structure. The (002) plane of the AlN was oriented in the thickness direction D of the piezoelectric thin film (the normal direction to the surface of the first electrode layer). The piezoelectric thin film consisted of a first piezoelectric layer laminated directly on the first electrode layer, and a second piezoelectric layer laminated directly on the first piezoelectric layer and in contact with the second electrode layer. The oxygen concentration in the first piezoelectric layer was lower than the oxygen concentration in the second piezoelectric layer. The oxygen concentration in the first piezoelectric layer was uniform in the thickness direction D. The oxygen concentration in the second piezoelectric layer gradually increased along the thickness direction D. The thickness T1 of the first piezoelectric layer was uniform. The thickness T2 of the second piezoelectric layer was also uniform.
[0077] The average oxygen concentration [O]3 in the piezoelectric thin films of Examples 2 to 6 is shown in Table 2 below. The average oxygen concentration [O]1 in the first piezoelectric layer in each of Examples 2 to 6 is shown in Table 2 below. The average oxygen concentration [O]2 in the second piezoelectric layer in each of Examples 2 to 6 is shown in Table 2 below. The thickness T1 of the first piezoelectric layer in each of Examples 2 to 6 is shown in Table 2 below. The thickness T2 of the second piezoelectric layer in each of Examples 2 to 6 is shown in Table 2 below. In the following Table 2, T2 / T3 is the ratio of the thickness T2 of the second piezoelectric layer to the thickness T3 of the piezoelectric thin film. T2 / T3 for each of Examples 2 to 6 is shown in the following Table 2. In Table 2 below, R[O]2 means the ratio of the total amount of oxygen in the second piezoelectric layer to the total amount of oxygen in the piezoelectric thin film. R[O]2 is equal to {(T2 / T3)×[O]2} / [O]3. R[O]2 for each of Examples 2 to 6 is shown in Table 2 below. Tan δ and d for each of Examples 2 to 6 33and Rc are shown in Table 2 below.
[0078] (Comparative Examples 1 and 2) The film formation time t TOTAL and the initial film formation temperature TI are shown in Table 1 below. In the cases of Comparative Examples 1 and 2, the above-mentioned second heating step and second film formation step were not performed. The thickness T3 of the piezoelectric thin film in each of Comparative Examples 1 and 2 was adjusted to the values shown in Tables 1 and 2 below. The thickness T3 of the piezoelectric thin film in each of Comparative Examples 1 and 2 was uniform.
[0079] Except for the process of forming the piezoelectric thin film, the piezoelectric thin film elements of Comparative Examples 1 and 2 were fabricated in the same manner as in Example 1. Analysis and measurement of the piezoelectric thin film elements of Comparative Examples 1 and 2 were carried out in the same manner as in Example 1.
[0080] The piezoelectric thin film of Comparative Example 1 did not contain oxygen. The piezoelectric thin film of Comparative Example 1 was composed only of crystalline AlN, and the AlN had a wurtzite structure. The (002) plane of the AlN of Comparative Example 1 was oriented in the thickness direction D of the piezoelectric thin film (the normal direction to the surface of the first electrode layer).
[0081] The piezoelectric thin film of Comparative Example 2 was made of crystalline AlN containing oxygen, and the AlN had a wurtzite structure. The (002) plane of the AlN of Comparative Example 2 was oriented in the thickness direction D of the piezoelectric thin film (the normal direction to the surface of the first electrode layer). The oxygen concentration in the piezoelectric thin film of Comparative Example 2 was uniform in the thickness direction D.
[0082] The average oxygen concentration [O]3 in the piezoelectric thin films of Comparative Examples 1 and 2 is shown in Table 2 below. 33 and Rc are shown in Table 2 below.
[0083] [Table 1]
[0084] [Table 2] [Industrial Applicability]
[0085] For example, the piezoelectric thin film element according to one aspect of the present invention may be used in a microphone, a sensor, a transducer, a filter, a harvester, or an actuator. [Explanation of symbols]
[0086] 1...first piezoelectric layer, 2...second piezoelectric layer, 3...piezoelectric thin film, 4...first electrode layer, 5...adhesion layer, 6...substrate, 7...second electrode layer, 10...piezoelectric thin film element, ucw...unit cell of wurtzite structure.
Claims
1. A substrate; A first electrode layer laminated on the substrate; a piezoelectric thin film laminated on the first electrode layer; A second electrode layer laminated on the piezoelectric thin film; Equipped with the piezoelectric thin film includes aluminum nitride and oxygen; the average oxygen concentration in the piezoelectric thin film is 0.001 atomic % or more and 6 atomic % or less; the piezoelectric thin film includes a first piezoelectric layer laminated on the first electrode layer, and a second piezoelectric layer laminated on the first piezoelectric layer and in contact with the second electrode layer, the concentration of oxygen in the first piezoelectric layer is lower than the concentration of oxygen in the second piezoelectric layer; Piezoelectric thin film element.
2. a ratio of a thickness of the second piezoelectric layer to a thickness of the piezoelectric thin film is 0.1% or more and 60% or less; a ratio of a total amount of oxygen in the second piezoelectric layer to a total amount of oxygen in the piezoelectric thin film is greater than 60% and less than or equal to 100%; 2. The piezoelectric thin film element according to claim 1.
3. the oxygen concentration in the second piezoelectric layer increases along a direction substantially perpendicular to a surface of the first electrode layer on which the piezoelectric thin film is laminated and from the first electrode layer to the second electrode layer; 3. The piezoelectric thin film element according to claim 1 or 2.
4. The first electrode layer contains at least one element selected from the group consisting of platinum, iridium, gold, rhodium, palladium, silver, nickel, copper, aluminum, molybdenum, tungsten, vanadium, chromium, niobium, tantalum, ruthenium, zirconium, hafnium, titanium, yttrium, scandium, and magnesium, 4. The piezoelectric thin film element according to claim 1.
Citation Information
Patent Citations
Ceramic wiring basic material
JP1996162567A
Aluminum nitride thin film-metallic electrode stack, and thin film piezoelectric resonator using it
JP2003198319A
Piezoelectric thin film resonator and manufacturing method of piezoelectric thin film
JP2013128267A
Methods of depositing piezoelectric aln-containing layers, and aln-containing piezoelectric layers
JP2016528385A
Piezoelectric film structure and sensor, and display assembly using them
JP2017538189A