Method for producing at least partially exfoliated clay using an exfoliant comprising a poly(alkylene oxide) (meth)acrylate, a cyclic carbonate, and water

Direct exfoliation of clay minerals in an organic medium using a poly(alkylene oxide)(meth)acrylate and cyclic carbonate mixture addresses the inefficiencies of traditional methods, enabling improved gas barrier and mechanical properties in polymer compositions.

JP7572974B2Active Publication Date: 2024-10-24HENKEL KGAA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021569230
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-20
Filing Date
2020-03-20
Publication Date
2024-10-24
Estimated Expiration
2040-03-20

AI Technical Summary

Technical Problem

Existing methods for exfoliating clay minerals like hectorite require multiple steps, including osmotic swelling in water and subsequent transfer to an organic medium, which can lead to adverse reactions and reduced effectiveness in polymer compositions.

Method used

A method using a release agent comprising a partial ester of poly(alkylene oxide)(meth)acrylate, cyclic carbonate, and a small amount of water directly exfoliates clay minerals in an organic medium, eliminating the need for aqueous swelling and subsequent transfer steps.

Benefits of technology

This approach allows for easy preparation of exfoliated clay suspensions that can be directly used in adhesives and coatings, enhancing gas barrier properties and improving mechanical and thermal properties of polymer compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572974000010
    Figure 0007572974000010
  • Figure 0007572974000011
    Figure 0007572974000011
  • Figure 0007572974000012
    Figure 0007572974000012
Patent Text Reader

Abstract

The present invention relates to a method for preparing at least partially exfoliated clay. The invention further relates to the at least partially exfoliated clay obtainable by such a method, to a suspension comprising such a clay, and to uses of the at least partially exfoliated clay and to uses of the suspension comprising such at least partially exfoliated clay. Furthermore, the invention is also directed to a polymer composition comprising the at least partially exfoliated clay and / or a suspension comprising the at least partially exfoliated clay.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for preparing an at least partially exfoliated phyllosilicate, such as a clay. The present invention also relates to an at least partially exfoliated clay obtainable by such a method, and to a suspension comprising such a clay, as well as to uses of such an at least partially exfoliated clay and to uses of such a suspension comprising an at least partially exfoliated clay. Furthermore, the present invention relates to a polymer composition comprising an at least partially exfoliated clay and / or a suspension comprising an at least partially exfoliated clay. [Background technology]

[0002] Fillers are used in polymer compositions such as sealants, coatings and adhesives to change the physical properties of each formulation.A typical class of fillers is mineral compounds such as silicates.In general, the aspect ratio of filler particles (the ratio of particle size in various dimensions, especially the ratio of the longest diameter to the shortest diameter, or in the case of platelet type particles, often referred to as "aspect ratio", which is the value of the lateral diameter divided by the thickness) is an important factor for improving the properties that fillers impart to polymer compositions, which may include gas and / or fluid barrier function, flame retardancy, and the overall mechanical and thermal properties of polymer compositions.

[0003] The efficiency of the gas barrier effect in terms of correlation between mineral analysis and barrier increases exponentially with particle flatness (i.e., aspect ratio). That is, for the same mineral analysis, the greater the aspect ratio, the better the gas barrier. With regard to gas barrier properties as well as the general dispersibility of the clay particles within the polymer matrix, large aspect ratios of several thousand are advantageous. The aspect ratio of layered clay particles can be maximized by osmotic swelling. Osmotically swollen clay particles / layers are delaminated or exfoliated from each other, which is different from the usual morphology in layering.

[0004] Osmotic swelling occurs in aqueous suspensions and can be facilitated / enhanced by, for example, the introduction of lithium cations, which improves the overall hydration of the clay particle surface. Osmotic swelling of clay minerals results in exfoliated clay particles with relatively large aspect ratios.

[0005] Osmotic swelling usually requires several steps such as treatment with specific chemicals and, in addition, exposure to high shear forces (e.g., stirring at very high frequencies) or, in the case of synthetic hectorite, an initial treatment with water. The transfer of the mixture of exfoliated clays, such as synthetic hectorite, and water to other aqueous or organic preparations has previously required surface modification.

[0006] For example, in US Pat. No. 6,363,636, an exfoliated clay that was first treated with water was then treated with quaternary ammonium salts to achieve surface modification. -D.Kunz,J.Schmid,P.Feicht,J.Erath,A.Fery,J.Breu;ACS Nano,7;No.5(2013)4275-4280; -H.Kalo,MWMoeller,DAKunz,J.Breu;Nanoscale,4(2012)5633-5639; -M. Stoeter, DAKunz, M. Schmid, D. Hirsemann, H. Kalo, B. Putz, J. Senker, J. Breu; J. Am. Chem. Soc., 29 (2013) 1280-1285; and - WO2018 / 033551A1

[0007] Such surface modification treatments also require further steps such as mixing with a solvent or centrifuging, sieving, etc., to transfer the exfoliated clay from an aqueous medium to a solvent-based medium. Only after transferring the medium, the exfoliated clay in the solvent-based medium can be applied to a solvent-based polymer composition, such as a solvent-based adhesive. For example, if the filler used in a solvent-based polyurethane adhesive composition contains a significant amount of water, the isocyanate component will react with the water, create brittle clumps, lack adhesion to surfaces, and exhibit bubble formation due to CO2 generation.

[0008] Furthermore, H. Xia and M. Song, Polym Int 55:229-235 (2006) disclose exfoliating clay layers by direct mixing in trihydroxyl branched polyether polyols. However, this method requires mixing the clay with certain polyether polyols for a relatively long time and at a higher temperature. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] WO2018 / 033551A1 Summary of the Invention [Problem to be solved by the invention]

[0010] The object of the present invention is therefore to provide an alternative exfoliant for the osmotic swelling / exfoliation of various minerals, in particular layered clay minerals such as phyllosilicates, in particular of the hectorite type, which allows a direct and easy preparation of a suspension of said modified minerals in a non-aqueous medium. In other words, instead of exfoliating the hectorite in water and then transferring it to an organic matrix (e.g. a solvent-based preparation), the hectorite can be exfoliated directly in an organic medium. [Means for solving the problem]

[0011] In this regard, the inventors have surprisingly found that the use of a release agent comprising a partial ester of a poly(alkylene oxide) (meth)acrylate, a cyclic carbonate and a very small amount of water allows for at least partial or complete exfoliation of the mineral. The resulting exfoliated clay / mineral suspension can be used directly as an additive in adhesive, sealant and coating compositions, which then exhibit improved gas barrier properties.

[0012] Thus, in a first aspect, the present invention provides a method for preparing an at least partially exfoliated clay, comprising: (1) providing clay; (2) providing a release agent comprising a partial ester of a poly(alkylene oxide) (meth)acrylate, a cyclic carbonate, and water, wherein the water is present in an amount of 10 volume percent or less, based on the volume of the release agent; (3) mixing the clay with the exfoliant; and (4) obtaining an at least partially exfoliated clay The present invention relates to a method comprising the steps of:

[0013] In a further aspect, the present invention relates to an at least partially exfoliated clay obtainable by the preparation process described herein.

[0014] In another aspect, the present invention relates to a suspension comprising an at least partially exfoliated clay as described herein.

[0015] In yet another aspect, the present invention further relates to the use of the at least partially exfoliated clay as described herein.

[0016] In yet another aspect, the present invention relates to the use of a suspension comprising an at least partially exfoliated clay as described herein.

[0017] Finally, the present invention also relates to a polymer composition comprising an at least partially exfoliated clay as described herein and / or a suspension comprising an at least partially exfoliated clay as described herein. [Brief description of the drawings]

[0018] FIG. 1 shows the results of SAXS (small angle X-ray scattering) measurements of a sample according to Example 4. FIG. 2 shows the results of SAXS (small angle X-ray scattering) measurements of a sample based on Example 3. FIG. 3 shows the results of SAXS (small angle X-ray scattering) measurement of a sample according to Example 5. FIG. 4 shows the results of SAXS (small angle X-ray scattering) measurement of a sample based on Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Further preferred embodiments of the invention are set out in the claims.

[0020] As used herein, the terms "a," "an," and "at least one" are equivalent to the term "one or more" and can be used interchangeably.

[0021] As used herein, "one or more" refers to at least one, including one, two, three, four, five, six, seven, eight, nine, or more than nine of the referenced species. Similarly, "at least one" means one or more, i.e., one, two, three, four, five, six, seven, eight, nine, or more. As used herein with respect to any moiety, "at least one" refers to the number of chemically distinct molecules, i.e., the number of different types of the referenced species, but not the total number of molecules.

[0022] When the molecular weight of a polymer or its components is mentioned herein, this refers to the number average molecular weight Mn, unless otherwise specified. The number average molecular weight Mn can be calculated based on end group analysis (OH number according to DIN 53240) or determined by gel permeation chromatography according to DIN 55672-1:2007-08 using THF as eluent. Unless otherwise specified, all given molecular weights are determined by end group analysis. The weight average molecular weight Mw can be determined by GPC as described for Mn.

[0023] All percentages given herein with respect to compositions or preparations relate to % by weight based on the total weight of the respective composition or preparation, unless stated otherwise.

[0024] The method for preparing an at least partially exfoliated clay according to the present invention comprises the following steps:

[0025] In the first step, a clay is provided. In the context of the present invention, any clay characterized by a layered mineral structure can be osmotically swollen and exfoliated in the manner disclosed herein. In various embodiments, the clay is an osmotically swellable clay. In various embodiments, the clay is a natural or synthetic layered silicate mineral. For example, the clay can be a phyllosilicate. In various embodiments, the clay is preferably selected from the group consisting of smectite, montmorillonite, saponite, beidellite, montmorillonite, hectorite, stevensite, vermiculite, kaolinite, halloysite, magadiite, and fluorohectorite. The clay is preferably selected from the group consisting of Ca 2+ , K + , Na + , Li +Such clays may contain naturally occurring cations in the molecular lattice of the clay, such as cations of 20000 to 290000, ...

[0026] In various embodiments, the clay provided in the first step of the method according to the invention is a phyllosilicate.

[0027] In various embodiments, the clay provided in the first step of the process according to the invention is preferably a hectorite.

[0028] In the second step, at least one exfoliant is provided. The term "exfoliant" as used herein refers to a mixture of compounds that osmotically swell clays, such as hectorite, so that 1 nm thick layers of clay are dispersed in the matrix to form a composite structure at the microscale. The osmotic swelling and exfoliation of the clay are thereby dependent on the chemical properties of the exfoliant. In the context of the present invention, the structure of the clay modifier is purposefully selected so that at least partially exfoliated clays can be obtained using the compounds disclosed herein.

[0029] According to the invention, the release agent comprises a partial ester of a poly(alkylene oxide) (meth)acrylate, a cyclic carbonate, and a very small amount of water. Water, preferably demineralized water, is present in an amount of 10% by volume or less, preferably 0.5-10%, more preferably 0.1-5%, even more preferably 0.5-3%, based on the volume of the release agent. Thus, in the context of the present invention, water plays no significant role, neither with regard to the swelling and exfoliation of the clay, nor with regard to the properties, such as polarity and chemical nature, of the matrix in which the clay is contained. The release agent according to the invention can have functional groups, such as hydroxy and / or thiol groups, that allow reaction with a crosslinker, which is incorporated into the polymer network formed upon curing.

[0030] Surprisingly, the inventors have found that by using such a combination of an organic compound and a small amount of water, excellent exfoliation of clay can be achieved.

[0031] The partial ester of a poly(alkylene oxide) (meth)acrylate can be represented as follows: [ka] [During the ceremony, R 1 is hydrogen or methyl, and R 2 ~R 5 are each independently hydrogen or C 1-6 alkyl, preferably each independently hydrogen, methyl or ethyl; L is a single bond or a linear or branched C optionally substituted with reactive groups such as hydroxy, thiol, epoxy, vinyl or (meth)acrylic ester groups. 1-12 Alkylene, C 3-12 Cyclic alkylene, phenylene, C 1-12 a w-valent linking group selected from the residues of polyols, preferably a single bond or a pentaerythritol residue; x is 1 to 5, preferably 1 to 3; y is 1 to 5, preferably 1 to 3; w is 2 to 6, preferably 2 to 4; a and b each independently represent 1 to 50, preferably 1 to 30; c and d each independently represent 0 to 50, preferably 0 to 30; provided that when L is a single bond, x and y are 1, and when L is a w-valent linking group, w is the sum of x and y.

[0032] According to the present invention, the partial ester of a poly(alkylene oxide) (meth)acrylate contains at least one terminal hydroxy group, preferably one or two terminal hydroxy groups.

[0033] In various embodiments, the partial ester of a poly(alkylene oxide) (meth)acrylate is selected from poly(alkylene oxide) mono(meth)acrylate, pentaerythritol poly(alkylene oxide) (meth)acrylate, and combinations thereof, preferably selected from poly(ethylene oxide) mono(meth)acrylate, poly(propylene oxide) mono(meth)acrylate, pentaerythritol poly(ethylene oxide) di(meth)acrylate, and combinations thereof.

[0034] In certain embodiments, the partial ester of poly(alkylene oxide)(meth)acrylate has a number average molecular weight of 150 to 3,000, preferably 200 to 2,000.

[0035] The partial esters of poly(alkylene oxide)(meth)acrylates in the present invention are either commercially available or can be prepared by methods well known in the art.

[0036] Examples of partial esters of poly(alkylene oxide) (meth)acrylates are poly(ethylene glycol) monomethacrylate with Mn of 360, poly(propylene glycol) monoacrylate with Mn of 475, and poly(propylene glycol) monoacrylate with Mn of 375 (all from Sigma-Aldrich).

[0037] In accordance with the present invention, the partial ester of poly(alkylene oxide) (meth)acrylate is present in an amount of 30 to 90 volume percent, preferably 50 to 85 volume percent, based on the volume of the release agent.

[0038] Cyclic carbonates suitable for the present invention are selected from the following compounds, their dimers, and combinations thereof: [ka]

[0039] In formula (I), A is (C(R 6 R 7 )) p where p is 2 or more, preferably 2 or 3, particularly preferably 2; R 6 and R 7 are each independently a hydrogen atom, a saturated or unsaturated, linear or branched or cyclic, aromatic or arylaliphatic, optionally substituted hydrocarbon group having 1 to 12 carbon atoms, or an ether group having 1 to 12 carbon atoms and up to 3 oxygen atoms. 8 X, where R 8 is a divalent aliphatic, alicyclic, aromatic, arylaliphatic or optionally substituted hydrocarbon group, including ether, having 1 to 20 carbon atoms, and X is a hydroxyl, epoxy, carboxylic acid, carboxylic acid ester group. Alternatively, A can be represented by Z, where Z is an unsaturated polymerizable group, preferably a vinyl-, (meth)acrylic-, maleic-, fumaric-, itaconic- or crotonic-ester group.

[0040] The cyclic carbonate may have a number average molecular weight of 50-1,000, preferably 50-500.

[0041] In certain embodiments, the cyclic carbonate is selected from the group consisting of vinylene carbonate, ethylene carbonate, propylene carbonate, glycerol carbonate, 5-ethyl-5-(hydroxymethyl)-1,3-dioxan-2-one, 1,3-dioxan-2-one, 5-((allyloxy)methyl)-5-ethyl-1,3-dioxan-2-one, 1,3-dioxepin-2-one, and combinations thereof, more preferably vinylene carbonate, glycerol carbonate, and combinations thereof.

[0042] The partial esters of poly(alkylene oxide)(meth)acrylates in the present invention are either commercially available or can be prepared by methods well known in the art.

[0043] According to the present invention, the cyclic carbonate is present in an amount of 5 to 60% by volume, preferably 10 to 50% by volume, based on the volume of the release agent.

[0044] In one embodiment, the release agent comprises 30-90% by volume, preferably 50-85% by volume, of a partial ester of a poly(alkylene oxide) (meth)acrylate, 5-60% by volume, preferably 10-50% by volume, of a cyclic carbonate, and 0.1-10% by volume, preferably 0.5-5% by volume, of water (percentages are based on the volume of the release agent).

[0045] In various embodiments, the stripping agent optionally contains one or more additives in the stripping agent, so long as the advantages of the present invention are not impaired. Examples of such additives are ketones, lactones, lactams, nitriles, nitro compounds, carboxamides, urea compounds, sulfoxides, sulfones, ethers, alcohols, primary or secondary amines, carboxylic acids, or primary or secondary amides. The additives may be present in an amount of 0-10% by volume, preferably 0-5% by volume, based on the volume of the stripping agent.

[0046] In order to obtain an at least partially exfoliated clay, in the third step of the method according to the invention, the clay and the exfoliating agent are mixed together. The two components are mixed together in a non-aqueous suspension for a time sufficient for the clay to swell with the exfoliating agent and to exfoliate / disperse in the exfoliating agent. In various embodiments, the mixing of the clay and the exfoliating agent is carried out with additional gentle stirring. In various embodiments, the mixing of the clay and the exfoliating agent is carried out for a period of 1 to 48 hours, preferably 4 to 24 hours.

[0047] The clay provided in the third step of the method according to the invention is provided in the form of a non-aqueous suspension, and the clay may be partially or completely exfoliated in a matrix of the exfoliant. Preferably, the clay is an at least partially exfoliated clay. As used herein, the term "at least partially exfoliated clay" generally refers to clays in which the mineral layers or tactoids are completely or partially separated from each other (i.e., intercalation of the exfoliant molecules and the resulting at least partial exfoliation of the tactoids).

[0048] Methods for preparing non-aqueous suspensions of clay as described herein, in which the clay may be partially or completely exfoliated, are known in the art. For example, non-aqueous clay suspensions can be prepared by subjecting a non-aqueous clay mixture to shear forces, such as by mechanical mixing, to partially and / or completely exfoliate the clay. These methods include, but are not limited to, ultrasonication, megasonication, grinding / crushing, high speed mixing, homogenization, and the like. While such high shear methods can be used in the method of the present invention, they are not required to achieve an exfoliated state, since the clay is spontaneous after being mixed with the exfoliating agent. High shear forces and shock waves, such as those generated in the case of an ultra-turbulent stirrer or ultrasonication, may be beneficial to the method according to the present invention, since they have the potential to penetrate (forming punctures) or disintegrate the mineral platelets, which may have detrimental effects. In various embodiments of the present invention, the clay may include both exfoliated clay layers and non-exfoliated clay particles. In certain embodiments of the present invention, homogenization of the non-aqueous clay suspension is not required.

[0049] In various embodiments of the present invention, in the third step of the process the clay and the exfoliant are mixed at a temperature between 20° C. and 60° C., preferably between 20° C. and 40° C., more preferably at room temperature.

[0050] In various embodiments of the present invention, in the third step of the method the clay and exfoliant are mixed for a period of from 30 minutes to 6 hours, preferably from 30 minutes to 4 hours, more preferably from 1 hour to 2 hours.

[0051] In various embodiments of the present invention, the at least partially exfoliated clay obtained in the third step contains not more than 50%, preferably not more than 20%, more preferably not more than 10%, even more preferably not more than 5% of non-exfoliated clay particles, and in particular no non-exfoliated clay particles, based on the total of exfoliated clay layers and non-exfoliated clay particles as measured by small angle X-ray scattering in the Examples section.

[0052] In various embodiments, the method according to the invention does not include the steps of treating the clay with water, surface modifying the clay, and / or transferring the clay to another solvent system. Thus, the method according to the invention easily transfers the clay from a crude form and partially or completely exfoliates it in an organic matrix in a single transfer step.

[0053] In a further aspect, the present invention relates to an at least partially exfoliated clay obtainable by the above preparation method.

[0054] In yet another aspect, the present invention further relates to a suspension comprising an at least partially exfoliated clay and an exfoliant, as described herein.

[0055] According to certain embodiments, the at least one solvent is selected from the group consisting of methanol, ethanol, acetone, butanone, ethyl acetate and acetonitrile, preferably from the group consisting of ethanol, acetone, butanone and ethyl acetate.In certain other embodiments, the at least one solvent is selected from the group consisting of acetonitrile, acetone, butanone, ethanol, dioxane and ethyl acetate.In various other embodiments, the at least one solvent is selected from the group consisting of acetone, butanone, ethanol, dioxane and ethyl acetate.

[0056] The present invention further relates to the use of the at least partially exfoliated clay as described herein.

[0057] In various embodiments, the at least partially exfoliated clay as described herein is used for the preparation of a polymer composition.

[0058] The exfoliation of clay in the method described herein allows the exfoliated clay particles to be transferred to a polymer matrix in one transfer step. The greater exfoliation of the at least partially exfoliated clay in the polymer matrix generally results in more enhanced properties, such as mechanical properties (e.g., tensile modulus, modulus of rupture), thermal properties (e.g., thermal conductivity), and insulating properties (e.g., gas barrier properties). Therefore, the at least partially exfoliated clay according to the present invention is very useful in the preparation of technically advantageous and superior polymer compositions for various application fields.

[0059] Furthermore, clays that have been at least partially exfoliated according to the present invention may then be used directly or for the modification of other formulations, for example, the clays may occur as a kind of masterbatch formulation and can be added to other formulations to adjust properties such as gas barrier performance.

[0060] According to certain embodiments, the polymer composition is selected from the group consisting of a coating composition, a sealant composition, and an adhesive composition.

[0061] In various embodiments, the transfer of the at least partially exfoliated clay particles into a polymer matrix comprises providing a suspension comprising the at least partially exfoliated clay according to the present invention, whereby said suspension comprising the at least partially exfoliated clay is transferred into a polymer matrix.

[0062] The present invention therefore further relates to the use of a suspension comprising an at least partially exfoliated clay as described herein.

[0063] In various embodiments, a suspension comprising at least a partially exfoliated clay as described herein is used for the preparation of a polymer composition. According to certain embodiments, the polymer composition is selected from the group consisting of a coating composition, a sealant composition and an adhesive composition.

[0064] The present invention is further directed to a polymer composition comprising the at least partially exfoliated clay described herein and / or a suspension comprising the at least partially exfoliated clay described herein.

[0065] According to certain embodiments, the polymer composition is selected from the group consisting of a coating composition, a sealant composition and an adhesive composition.

[0066] In various other embodiments, the at least partially exfoliated clay is present in an amount of from 0.1 to 25 weight percent, preferably from 1 to 10 weight percent, based on the total weight of solids of the polymer composition.

[0067] In a preferred embodiment, the at least partially exfoliated clay or the suspension of the at least partially exfoliated clay described herein can be used as an additive component of an adhesive composition, in particular a polyurethane adhesive composition. The at least partially exfoliated clay described herein can be used as an additive component of a one-component (1-c) or two-component (2-c) polyurethane adhesive composition. A particularly preferred polyurethane (PU) adhesive composition can be a 2-c adhesive composition. These 2-c polyurethane adhesive compositions generally comprise a component (a) and a component (b), where component (a) is a resin component and component (b) is a curing agent or crosslinker component.

[0068] In the separated form, the two components (a) and (b) are storage stable.

[0069] In certain embodiments, the resin component (a) comprises at least one polyol and / or at least one NCO-reactive prepolymer, and the hardener component (b) comprises at least one polyisocyanate. However, in certain other embodiments, the resin component (a) comprises at least one NCO-terminated prepolymer, and the hardener component (b) comprises at least one polyol and / or other compound having at least two NCO-reactive groups. Generally, the latter is preferred.

[0070] In such systems, the at least partially exfoliated clay according to the present invention may be included in the hardener component or the resin component. In a preferred embodiment, the at least partially exfoliated clay may be included in the hardener component.

[0071] To ensure the stability of the formulation, further additives can be incorporated into each component, provided that they do not react with the reactive groups of the other compounds during storage.

[0072] In a preferred embodiment according to the present invention, the resin component (a) comprises at least one NCO-terminated prepolymer.

[0073] Suitable NCO-terminated prepolymers can be prepared by reacting at least one polyol or at least one polyol mixture with at least one polyisocyanate, where the at least one polyisocyanate is used in molar excess.

[0074] The at least one polyol used in the preparation of the NCO-terminated prepolymers can be chosen from a wide range of commercially available products, for example polyether polyols, polyester polyols, oleochemical polyols, aliphatic, cycloaliphatic or aromatic polyols, OH-group-containing polymers or oligomeric compounds such as polycarbonates, polybutadienes, polyacrylates, or mixtures thereof.

[0075] One group of suitable polyols is polyester polyols, which can be prepared by condensing di- or tricarboxylic acids with an excess of di- or trifunctional alcohols. The carboxylic acids can be aliphatic, cycloaliphatic, aromatic or heterocyclic, or mixtures thereof. Examples of suitable acids are aliphatic acids such as adipic acid, sebacic acid, glutaric acid, azelaic acid, suberic acid, undecanedioic acid, dodecanedioic acid, 3,3-dimethylglutaric acid, hexahydrophthalic acid, aromatic acids such as phthalic acid, terephthalic acid, isophthalic acid, unsaturated acids such as maleic acid, fumaric acid, dimer fatty acid, tricarboxylic acids such as citric acid and trimellitic acid. Examples of suitable di- or trifunctional alcohols include, but are not limited to, low molecular weight alcohols such as ethylene glycol, diethylene glycol, neopentyl glycol, hexanediol, butanediol, propylene glycol, glycerol or trimethylolpropane, dipropylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-dicanediol, 1,12-dodecanediol, 1,4-hydroxymethylcyclohexane, 2-methylpropane-1,3-diol, butane-1,2,4-triol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol and polybutylene glycol, as well as glycerol, trimethylolpropane, or mixtures thereof.

[0076] Another group of suitable polyester polyols is based on ε-caprolactone, also called polycaprolactone, or on hydroxycarboxylic acids, such as ω-hydroxycaprolactone. Such polyols contain at least two OH groups, preferably terminal OH groups, or polymers of tetrahydrofuran (THF).

[0077] Another group of polyester polyols useful in the present invention are the so-called oleochemical polyols. Such polyester polyols can be prepared, for example, by complete ring opening of epoxidized triglycerides of a fatty mixture containing at least partially olefinically unsaturated fatty acids and one or more alcohols having 1 to 12 alcohols, followed by partial transesterification of the triglyceride derivatives to give alkyl ester polyols having 1 to 12 carbon atoms in the alkyl group. Another group of such suitable polyols based on natural products are dimer diols, as well as castor oil and their derivatives.

[0078] Another group of polyols are the polyacetals. Polyacetals are understood to be compounds obtained by reacting glycols, such as diethylene glycol or hexanediol or mixtures thereof, with formaldehyde. Polyacetals suitable for the purposes of the present invention can also be obtained by polymerizing cyclic acetals. Another group of polyols are the polycarbonates. Polycarbonates can be obtained, for example, by reacting diols such as propylene glycol, butane-1,4-diol or hexane-1,6-diol, diethylene glycol, triethylene glycol or tetraethylene glycol, or mixtures of two or more thereof, with diaryl carbonates, such as diphenyl carbonate or phosgene.

[0079] Also suitable for use in the present invention are hydroxy-functional polybutadienes known under the tradename Poly-bd®.

[0080] Polycarbonate polyols can be prepared by reacting a diol, such as propylene glycol, 1,4-butanediol or 1,6-hexanediol, diethylene glycol, triethylene glycol or tetraethylene glycol, or mixtures thereof, with a diaryl carbonate, for example diphenyl carbonate or phosgene.

[0081] Other suitable polyol components are polyether polyols, which are reaction products of low molecular weight polyhydric alcohols with alkylene oxides. The alkylene oxides preferably contain 2 to 4 carbon atoms. Suitable reaction products of this type are, for example, the reaction products of ethylene glycol, propylene glycol, isomeric butanediols, hexanediols or 4,4'-dihydroxydiphenylpropane with ethylene oxide, propylene oxide or butylene oxide or mixtures of two or more thereof. Also suitable are the reaction products of polyhydric alcohols such as glycerol, trimethylolethane or trimethylolpropane, pentaerythritol or sugar alcohols or mixtures of two or more thereof with the alkylene oxides mentioned to form polyether polyols. Such polyether polyols are available in different molecular weights, as compositions, as homopolymers or as random or block copolymers. Another group of polyether polyols are polytetramethylene glycols, which can be prepared by polymerization of tetrahydrofuran.

[0082] Also suitable are low molecular weight polyether glycols below 500 g / mol (number average molecular weight Mn).

[0083] Other examples of low molecular weight polyols include low molecular weight diols and triols, for example, C2-C20 diols such as ethylene glycol, propylene glycol, 1,2- or 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,12-dodecanediol, dimeric fatty acid alcohols or higher homologue diols or their isomers. In addition, polyols with three or more functional groups can be used, such as glycerol, trimethylolethane (TME), pentaerythrite and / or trimethylolpropane (TMP), or oligomers of pentaerythrite, TMP or TME, or higher functional alcohols such as diglycerol, triglycerol or sugar alcohols.

[0084] The composition may further comprise a polyol which is a hydroxy-functionalized polymer, for example a hydroxy-functionalized siloxane. An exemplary siloxane which may be used is a hydroxy-functionalized polydimethylsiloxane, especially in liquid form, for example one commercially available under the name Tegomer® H-Si2311 (Evonik, Germany), which has a number-average molecular weight Mn of about 2,200 g / mol. Suitable polydimethylsiloxane (PDMS) polyols are described, for example, in US 6794445 B2. They may be used in amounts of up to 60% by weight, based on the total weight of the polyols used, and usually have low Tg values, for example in the range of -150°C to -100°C.

[0085] The number average molecular weight Mn of the polyol used in the synthesis of the NCO-terminated prepolymer is preferably in the range of 320 to 20,000 g / mol, in particular 330 to 4500 g / mol. The nominal functionality may be in the range of 2 to 4.5. Preferably, the PU prepolymer has a polyether / polyester backbone.

[0086] For the preparation of resin component (a), one or more of the aforementioned polyols can be reacted with at least one polyisocyanate to form an NCO-terminated prepolymer. The at least one polyisocyanate is used in molar excess relative to the hydroxyl groups of all polyols present in the reaction mixture. In certain embodiments, the NCO:OH ratio of the NCO-reactive polyurethane prepolymer is preferably, but not necessarily, 1:1 to 1.8:1, preferably 1:1 to 1.6:1, in particular 1.05:1 to 1.5:1.

[0087] Polyisocyanates suitable for use in preparing the NCO-terminated prepolymers are known in the art and may include monomeric isocyanates containing two or three NCO groups. For example, they include the well-known aliphatic, cycloaliphatic or aromatic monomeric diisocyanates. Preferably, the isocyanates are selected with a molecular weight between 160 g / mol and 500 g / mol, such as aromatic polyisocyanates, e.g., isomers of diphenylmethane diisocyanate (MDI), such as 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 2,2'-diphenylmethane diisocyanate (2,2'-MDI), 2,4'-diphenylmethane diisocyanate (2,4'-MDI); Isomers of phenylene diisocyanates such as 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate; Isomers of toluene diisocyanate (TDI), such as naphthalene-1,5-diisocyanate (NDI), 2,4-TDI and 2,6-TDI; These include m- and p-tetramethylxylene diisocyanate (TMXDI), m- and p-xylene diisocyanate (XDI), 3,3'-dimethyldiphenyl-4,4'-diisocyanate (TODI), toluene diisocyanate, naphthalene, di- and tetraalkyldiphenylmethane diisocyanates, 4,4'-dibenzyl diisocyanate, and combinations thereof.

[0088] Ethylene diisocyanate, dodecane diisocyanate, dimer fatty acid diisocyanate, 4,4'-dibenzyl diisocyanate, 1,6-diisocyanate-2,2,4-trimethylhexane, butane-1,4-diisocyanate, hexane-1,6-diisocyanate (HDI), tetramethoxybutane-1,4-diisocyanate, 1,12-diisocyanate-dodecane, 4,4'-dicyclohexylmethane diisocyanate, 1,3-cyclohexane or 1,4-cyclohexane diisocyanate, 1-methyl-2 Aliphatic and cycloaliphatic isocyanates such as toluene-diisocyanate, 4-diisocyanato-cyclohexane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane (isophorone diisocyanate, IPDI), hydrogenated or partially hydrogenated MDI ([H]12MDI (hydrogenated) or [H]6MDI (partially hydrogenated)), or trimers of HDI, or dimeric or trimeric toluene-diisocyanate, and combinations thereof may also be used.

[0089] It is also possible to include at least partially oligomeric diisocyanates such as allophanates, carbodiimides, isocyanurates, biuret condensation products from diisocyanates, for example from HDI, MDI, IPDI or other isocyanates. Polymeric MDI can also be used. Mixtures of aliphatic or aromatic isocyanates can be used. More preferably, aromatic diisocyanates can be used.

[0090] In certain embodiments, at least one NCO-terminated prepolymer of resin component (a) has a number average molecular weight Mn in the range of 1,500 to 100,000, preferably 2,000 to 50,000 g / mol. Typically, the NCO content of the resulting prepolymer is 5 to 20 wt. % and the nominal average functionality is 2 to 3.

[0091] Examples of suitable NCO-terminated prepolymers are disclosed in EP-A 951493, EP-A 1341832, EP-A 150444, EP-A 1456265 and WO 2005 / 097861.

[0092] Furthermore, the adhesive composition according to the present invention comprises a hardener component (b). Suitable hardener components are known in the art. In the case of a resin component based on NCO-terminated prepolymer, typically, a polyol compound is used in the hardener component. According to a preferred embodiment of the present invention, the hardener component (b) comprises at least one polyol. The polyol may be selected from those disclosed in connection with the prepolymer above.

[0093] Generally, the above is disclosed with reference to NCO-terminated prepolymers, but it is understood that OH-terminated prepolymers can be produced by varying the molar ratios of the reactants described in the prepolymer synthesis. Thus, in such embodiments, the same compounds as above can be used. In yet another embodiment, the polyols disclosed above can be used by themselves or in combination with OH-terminated prepolymers as resin components. In that case, the curing agent will include a polyisocyanate in both cases.

[0094] Furthermore, the adhesive according to the invention may contain other auxiliary materials, which are preferably mixed completely or partially with the resin component. Auxiliaries are substances that are generally added in small amounts to modify the properties of the adhesive, such as viscosity, wetting behavior, stability, reaction rate or shelf life, in the desired direction. Such additives for improving specific properties are, for example, antifoaming agents, wetting agents or surfactants such as stearates, silicone oils and addition products of ethylene oxide or propylene oxide with fatty alcohols; UV-stable antioxidants such as sterically hindered phenols, thioethers, substituted benzotriazoles or HALS types; additional adhesion promoters, for example silanes containing hydrolyzable groups such as hydroxy, (meth)acryloxy, amino or epoxy functional groups (containing methoxy, ethoxy, propoxy or butoxy groups) and flame retardants.

[0095] In order to increase the reactivity of the adhesive with respect to crosslinking, the adhesive may optionally contain a catalyst. Suitable catalysts that may be used according to the invention are, in particular, organometallic and / or amine catalysts. Examples include titanates such as tetrabutyl titanate or tetrapropyl titanate, chelated metals such as dibutyltin dilaurate (DBTL), dibutyltin diacetate, tin octoate, dibutyltin oxide, Zr-acetylacetonate, Ti-acetylacetonate, Fe-acetylacetonate, and amino compounds such as triethylenetetramine, triethylenediamine, diethylaminopropylamine, morpholine, N-methylmorpholine, 1,8-diazabicyclo-[5,4,0]-undecene-7 (DBU), cyclohexylamine, and 2-ethyl-4-methylimidazole. The catalyst is preferably incorporated into the hardener component.

[0096] Another group of additives are tackifying resins. Resins are known in various compositions and types as synthetic or natural resins. Examples of such resins are abietic acid, abietic acid esters, terpene resins, terpene / phenolic resins, poly-α-methylstyrene or aliphatic, aromatic or aromatic / aliphatic hydrocarbon resins or coumarone / indene resins.

[0097] Optionally, the adhesive may contain pigments or fillers. Such additives can be used to modify certain properties of the adhesive. For example, oxides, silicates, sulfates, phosphates or carbonates of Ti, Zr, Al, Fe, Mg, Ca, Ba or Zn, such as natural ground chalk, precipitated chalk, barytes, talcum, mica, carbon black, titanium oxide, iron oxide, aluminum oxide, zinc oxide, zinc sulfate or silicon dioxide. Water-absorbing powders, such as zeolites, may also be present as fillers. The fillers should be present in finely divided form, for example with a size of 1 to 200 μm, in particular up to 50 μm, but they can also be nanoscale pigments.

[0098] The composition may further comprise silicon dioxide. Examples include treated silica, precipitated silica, untreated silica, and particularly pyrogenic or fumed silica.

[0099] The composition may further comprise an additional polymer containing multiple carboxylic acid groups and / or hydroxyl groups. This compound is usually included in the hardener component (b) since it can react with isocyanates. Such components can be selected, for example, from polycarboxylic acid polyhydroxy acid amides, polycarboxylic acid amides, and modified polyhydroxy ureas. Such polymers are known as physical thixotropic agents and are commercially available. They are disclosed, for example, in U.S. Pat. No. 6,420,466 or EP 1048681.

[0100] In principle, various additives and auxiliaries can be included in each component. However, it is useful to select such additives that do not react with other compounds of components (a) or (b). In a particular embodiment, the catalyst is added to component (b).

[0101] Methods for preparing both the resin component (a) and the hardener component (b) are known in the art. The two components are stored separately until use. For use, the resin and hardener components are mixed together in a manner known per se. After mixing the resin component (a) and the hardener component (b), the ratio of isocyanate groups present in the adhesive composition to OH groups present in the adhesive composition is generally in the equivalent range, which is convenient to provide a slight excess of isocyanate groups relative to the moisture present on the surface. The NCO / OH ratio should be 0.90:1 to 1.5:1, in particular 1.0:1 to 1.3:1.

[0102] The polyurethane adhesive of the present invention is liquid at the application temperature. The polyurethane adhesive of the present invention is preferably liquid at room temperature. In various embodiments, the adhesive composition according to the present invention has a viscosity of 500 to 100,000 mPas, in particular 1,000 to 20,000 mPas, at a temperature of 40° C., measured according to DIN ISO 2555 (Brookfield viscometer RVT, spindle number 4, 25° C.; 5 rpm). The adhesives described herein may comprise one or more solvents or may be solvent-free. Suitable solvents are known to those skilled in the art, in particular esters, ketones, halogenated hydrocarbons, alkanes, alkenes and aromatic hydrocarbons. Examples of suitable solvents are methylene chloride, trichloroethylene, toluene, xylene, butyl acetate, amyl acetate, isobutyl acetate, methyl isobutyl ketone, methoxybutyl acetate, cyclohexane, cyclohexanone, dichlorobenzene, diethyl ketone, diisobutyl ketone, acetone, methyl ethyl ketone, dioxane, ethyl acetate, ethylene glycol monobutyl ether, ethylene glycol monoethyl, 2-ethylhexyl acetate, glycol diacetate, heptane, hexane, isobutyl acetate, isooctane, isopropyl acetate, methyl ethyl ketone, tetrahydrofuran or tetrachloroethylene, or a mixture of two or more of the above solvents. In a preferred embodiment, the polyurethane adhesive composition of the present invention is solvent-free.

[0103] The adhesive can be applied to the substrate by any known technique, including, but not limited to, spraying, painting, dip coating, spin coating, printing, and the like.

[0104] Another embodiment of the present invention is therefore a method of using the polyurethane adhesive composition according to the present invention. In various embodiments, such a method comprises the step of applying an adhesive composition to a substrate surface, the adhesive being the polyurethane adhesive composition described above. In the method according to the present invention, the two components (a) and (b) of the adhesive are mixed immediately before application. The adhesive composition is then applied to the substrate surface.

[0105] It is understood that all embodiments disclosed herein with respect to the methods are equally applicable to the disclosed dispersions, compositions and uses, and vice versa.

[0106] The following examples are provided to illustrate the present invention, and as these examples are for illustrative purposes only, the present invention should not be construed as being limited thereto. EXAMPLES

[0107] material: Vinylene carbonate is available from Sigma-Aldrich. Glycerol carbonate is available from Huntsman. Jeffamine M-600 is the trade name for a polyetheramine available from Huntsman having the following structure: [ka] Jeffamine M-2070 is the trade name for a polyetheramine based on polyethylene oxide and polypropylene oxide available from Huntsman. · PPG-triol is a propoxylated glycerol available from Dow under the trade name Voranol CP450. ·PEG-MA is poly(ethylene glycol) monomethacrylate with Mn of 360 available from Sigma-Aldrich. ·PPG-A is poly(propylene glycol) monoacrylate with Mn of 475 available from Sigma-Aldrich. PPG-MA is poly(propylene glycol) monoacrylate with Mn of 375 available from Sigma-Aldrich. PETTEGE-DA is pentaerythritol tetrakis(tetraethylene glycol ether) diacrylate having the following structure: [ka]

[0108] PETTEGE-DA was prepared as follows: 79.7 g (0.1 mol) of pentaerythritol ethoxylate 15 / 4 (EO / OH) available from Sigma-Aldrich was weighed in a 500 ml three-neck flask, then vacuum dried and aerated with dry nitrogen. 200 ml of dichloromethane available from Sigma-Aldrich and 21.3 g (0.21 mol) of triethylamine were added, the mixture was stirred and cooled to 0° C. in an ice bath. 18.1 g (0.2 mol) of acryloyl chloride available from Sigma-Aldrich was added dropwise, and the mixture was stirred at 0° C. for 30 minutes and at room temperature for 30 minutes. The precipitate was then obtained by filtration and washing. The molecular weight of the final product is about 973. The yield is 41.1%.

[0109] Various stripping agents were prepared according to the formulations in Table 1. 2% by weight of untreated hectorite was mixed with each stripping agent for 2 hours at room temperature. No further homogenization was applied. The samples were then visually observed for osmotic swelling and state of stripping according to the following criteria: 1. If collapse of crude hectorite mass is observed 2. If a significant increase in viscosity is observed 3. If the pearlescence effect due to the interference of light is observed, and 4. If a uniform suspension is observed.

[0110] During visual testing, a sample was rated as "Pass" or "P" only if all conditions were observed. If any of the criteria were not observed, the sample was rated as "Fail" or "F." The test results are shown in Table 1.

[0111] In the test results in Table 1, it is clear that all of the examples of the present invention (Examples 1 to 9) exhibited excellent osmotic swelling and complete or near complete exfoliation of the hectorite. However, poor release performance was observed in Comparative Examples (CEx) 1, 6, 7, and 9, which used release agents that did not contain a partial ester of poly(alkylene oxide) (meth)acrylate, a cyclic carbonate, and / or water, in CEx 2 to 5, which used release agents that contained a polyetheramine or a polyether polyol instead of a partial ester of poly(alkylene oxide) (meth)acrylate, and in CEx 8, which used a release agent that contained a large amount of water.

[0112] The clay suspensions were further examined by SAXS (small angle X-ray scattering). The measurements were carried out using a "Double Ganesha AIR" testing machine manufactured by SAXSLAB, Denmark. In the tests, X-rays were generated by a rotating copper anode (MicoMax 007HF, Rigaku Corporation, Japan), which produces a microfocused beam. A position sensitive detector (PILATUS 300K, Dectris) was used at different positions to measure the scattering vector q = 0.001-1 Å. -1 A range of 100 nm to 150 nm was covered. Prior to the measurements, each clay suspension was filled into a 1 mm glass capillary (Hilgenberg, code 4007610). The circularly averaged data were normalized to the incident beam, sample thickness, and measurement time.

[0113] This allowed the interlayer distance of the phyllosilicate platelets to be determined. In each of the Figures 1 to 3 showing the results of the tests of Examples 4, 3 and 5, the peaks representing the initial layer distance of untreated hectorite (non-exfoliated) or of the aggregated platelets of hectorite at 1.8 nm (see dotted line) have completely or almost completely disappeared. If the sample is not exfoliated, a prominent peak can be seen at 1.8 nm (see dotted line), a typical example (CEx.4) is shown in Figure 4.

[0114] Furthermore, the exfoliated hectorite suspension according to the embodiment of the present invention contains an organic matrix having hydroxyl groups and no significant amount of water. When such hectorite suspension is used in polyurethane-based adhesive formulations, such formulations can achieve excellent adhesion and gas barrier properties. This is especially important for laminating adhesives used in flexible packaging.

[0115] [Table 1] The initial disclosure of this specification includes at least the following aspects. [1] A method for preparing an at least partially exfoliated clay, comprising: (1) providing clay; (2) providing a release agent comprising a partial ester of a poly(alkylene oxide) (meth)acrylate, a cyclic carbonate, and water, wherein the water is present in an amount of 10 volume percent or less, based on the volume of the release agent; (3) mixing the clay with the release agent; and (4) obtaining an at least partially exfoliated clay The method includes: [2] The method according to [1], wherein the clay is a natural or synthetic layered silicate mineral, preferably selected from the group consisting of smectite, montmorillonite, saponite, beidellite, montmorillonite, hectorite, stevensite, vermiculite, kaolinite, halloysite, magadiite, fluorohectorite and combinations thereof, more preferably hectorite. [3] The partial ester of poly(alkylene oxide)(meth)acrylate is as follows: TIFF0007572974000006.tif7169 [During the ceremony, R 1 is hydrogen or methyl, and R 2 ~R 5 are each independently hydrogen or C 1-6 alkyl, preferably each independently hydrogen, methyl or ethyl; L is a single bond or a linear or branched C optionally substituted with a hydroxy, thiol, epoxy, vinyl or (meth)acrylic ester group. 1-12 Alkylene, C 3-12 Cyclic alkylene, phenylene, C 1-12 a w-valent linking group selected from the residues of polyols, preferably a single bond or a pentaerythritol residue; x is 1 to 5, preferably 1 to 3; y is 1 to 5, preferably 1 to 3; w is 2 to 6, preferably 2 to 4; a and b each independently represent 1 to 50, preferably 1 to 30; c and d each independently represent 0 to 50, preferably 0 to 30; provided that when L is a single bond, x and y are 1, and when L is a w-valent linking group, w is the sum of x and y. The method according to any one of [1] to [2] above, wherein the formula is [4] The method according to any one of the above [1] to [3], wherein the partial ester of poly(alkylene oxide) (meth)acrylate is selected from poly(alkylene oxide) mono(meth)acrylate, pentaerythritol poly(alkylene oxide) (meth)acrylate, and a combination thereof, preferably selected from poly(ethylene oxide) mono(meth)acrylate, poly(propylene oxide) mono(meth)acrylate, pentaerythritol poly(ethylene oxide) di(meth)acrylate, and a combination thereof. [5] The method according to any one of the above [1] to [4], wherein the partial ester of poly(alkylene oxide) (meth)acrylate has a number average molecular weight of 150 to 3,000, preferably 200 to 2000. [6] The cyclic carbonate is selected from the group consisting of: TIFF0007572974000007.tif2718 [During the ceremony, A is (C(R 6 R 7 )) p 、R 8 It is represented by X or Z, p is 2 or more, preferably 2 or 3, particularly preferably 2; R 6 and R 7 each independently represents a hydrogen atom, a saturated or unsaturated, linear or branched or cyclic, aromatic or arylaliphatic, optionally substituted hydrocarbon group having 1 to 12 carbon atoms, or an ether group having 1 to 12 carbon atoms and up to 3 oxygen atoms; R 8 is a divalent, optionally substituted, aliphatic, alicyclic, aromatic, arylaliphatic, or ether, hydrocarbon group having 1 to 20 carbon atoms; X is a hydroxy, epoxy, carboxylic acid, carboxylate ester group, or Z is an unsaturated polymerizable group, preferably a vinyl-, (meth)acrylic-, maleic-, fumaric-, itaconic- or crotonic-ester group. and a dimer thereof; and a combination thereof. [7] The method according to any one of the above [1] to [6], wherein the cyclic carbonate is selected from the group consisting of vinylene carbonate, ethylene carbonate, propylene carbonate, glycerin carbonate, 5-ethyl-5-(hydroxymethyl)-1,3-dioxan-2-one, 1,3-dioxan-2-one, 5-((allyloxy)methyl)-5-ethyl-1,3-dioxan-2-one, 1,3-dioxepin-2-one, and combinations thereof. [8] The method according to any one of the above [1] to [7], wherein the cyclic carbonate has a number average molecular weight of 50 to 1,000, preferably 50 to 500. [9] The method according to any one of the above [1] to [8], wherein the water is present in an amount of 0.1 to 10% by volume, preferably 0.5 to 5% by volume, based on the volume of the stripping agent.

[10] The method according to any one of the above [1] to [9], wherein the partial ester of poly(alkylene oxide) (meth)acrylate is present in an amount of 30 to 90% by volume, preferably 50 to 85% by volume, based on the volume of the release agent.

[11] The method according to any one of the above [1] to

[10] , wherein the cyclic carbonate is present in an amount of 5 to 60% by volume, preferably 10 to 50% by volume, based on the volume of the release agent.

[12] An at least partially exfoliated clay obtained by the preparation method according to any one of [1] to

[12] above.

[13] A suspension comprising the at least partially exfoliated clay according to

[11] above and an exfoliant.

[14] A polymer composition comprising an at least partially exfoliated clay according to

[12] above or a suspension comprising an at least partially exfoliated clay according to

[13] above.

[15] The polymer composition according to

[14] , wherein the polymer composition is selected from the group consisting of a coating composition, a sealant composition and an adhesive composition.

Claims

1. 1. A method for preparing an at least partially exfoliated clay, comprising: (1) providing a clay; (2) providing a release agent comprising a partial ester of a poly(alkylene oxide) (meth)acrylate, a cyclic carbonate, and water, wherein the water is present in an amount of 5 volume percent or less based on the volume of the release agent; (3) mixing the clay with the release agent; and (4) Obtaining an at least partially exfoliated clay The method includes:

2. 2. The method of claim 1, wherein the clay is a natural or synthetic layered silicate mineral, preferably selected from the group consisting of smectite, montmorillonite, saponite, beidellite, montmorillonite, hectorite, stevensite, vermiculite, kaolinite, halloysite, magadiite, fluorohectorite and combinations thereof, more preferably hectorite.

3. The partial ester of poly(alkylene oxide) (meth)acrylate is 【Chemistry 1】 [During the ceremony, R 1 is hydrogen or methyl; R 2 ~R 5 are each independently hydrogen or C 1-6 alkyl, preferably each independently hydrogen, methyl or ethyl; L is a single bond or a linear or branched C alkyl group optionally substituted with a hydroxy, thiol, epoxy, vinyl or (meth)acrylic ester group. 1-12 Alkylene, C 3-12 Cyclic alkylene, phenylene, C 1-12 a w-valent linking group selected from the residues of polyols, preferably a single bond or a pentaerythritol residue; x is 1 to 5, preferably 1 to 3; y is 1 to 5, preferably 1 to 3; w is 2 to 6, preferably 2 to 4; a and b each independently represent 1 to 50, preferably 1 to 30; c and d each independently represent 0 to 50, preferably 0 to 30; However, when L is a single bond, x and y are 1, and when L is a w-valent linking group, w is the sum of x and y. The method according to claim 1 or 2, wherein

4. 4. The method according to claim 1, wherein the partial ester of poly(alkylene oxide) (meth)acrylate is selected from poly(alkylene oxide) mono(meth)acrylate, pentaerythritol poly(alkylene oxide) (meth)acrylate, and combinations thereof, preferably selected from poly(ethylene oxide) mono(meth)acrylate, poly(propylene oxide) mono(meth)acrylate, pentaerythritol poly(ethylene oxide) di(meth)acrylate, and combinations thereof.

5. The method according to any one of claims 1 to 4, wherein the partial ester of poly(alkylene oxide) (meth)acrylate has a number average molecular weight of 150 to 3,000, preferably 200 to 2000.

6. The cyclic carbonate is selected from the group consisting of: 【Chemistry 2】 [During the ceremony, A is (C(R 6 R 7 )) p , R 8 Represented by X or Z, p is 2 or more, preferably 2 or 3, particularly preferably 2; R 6 and R 7 are each independently a hydrogen atom, a saturated or unsaturated, linear or branched or cyclic, aromatic or arylaliphatic, optionally substituted hydrocarbon group having 1 to 12 carbon atoms, or an ether group having 1 to 12 carbon atoms and up to 3 oxygen atoms; R 8 is a divalent aliphatic, cycloaliphatic, aromatic, arylaliphatic, or ether, optionally substituted, hydrocarbon group having 1 to 20 carbon atoms; X is a hydroxy, epoxy, carboxylic acid, carboxylic acid ester group, or Z is an unsaturated polymerizable group, preferably a vinyl-, (meth)acrylic-, maleic acid-, fumaric acid-, itaconic acid- or crotonic acid-ester group. The method according to any one of claims 1 to 5, wherein the compound is selected from the group consisting of a compound represented by the formula:

7. 7. The method of any one of claims 1 to 6, wherein the cyclic carbonate is selected from the group consisting of vinylene carbonate, ethylene carbonate, propylene carbonate, glyceryl carbonate, 5-ethyl-5-(hydroxymethyl)-1,3-dioxan-2-one, 1,3-dioxan-2-one, 5-((allyloxy)methyl)-5-ethyl-1,3-dioxan-2-one, 1,3-dioxepin-2-one, and combinations thereof.

8. The process according to any one of claims 1 to 7, wherein the cyclic carbonate has a number average molecular weight of 50 to 1,000, preferably 50 to 500.

9. The method of any of claims 1 to 8, wherein the water is present in an amount of 0.5 to 5 volume percent, based on the volume of the stripping agent.

10. The method of any of claims 1 to 9, wherein the partial ester of poly(alkylene oxide) (meth)acrylate is present in an amount of 30 to 90% by volume, preferably 50 to 85% by volume, based on the volume of the release agent.

11. The method according to any of the preceding claims, wherein the cyclic carbonate is present in an amount of from 5 to 60% by volume, preferably from 10 to 50% by volume, based on the volume of the release agent.

12. Method for producing a suspension comprising an at least partially exfoliated clay obtainable by the method according to any one of claims 1 to 11 and an exfoliating agent.

13. A method for the preparation of a polymer composition comprising an at least partially exfoliated clay obtainable by the method according to any of claims 1 to 11 or a suspension obtainable by the method according to claim 12.

14. 14. The method of claim 13, wherein the polymer composition is selected from the group consisting of a coating composition, a sealant composition, and an adhesive composition.

Citation Information

Patent Citations

  • Intercalation formed from n-alkenylamide and / or acrylate-functional pyrrolidone and allylic monomer, oligomer and / or copolymer, released product, and composite material containing them

    JP1999193350A

  • Composition for use in conducting downhole operations in oil and gas wells

    WO2015010011A1

  • Method for preparing a hydrophobically modified clay

    WO2018033551A1