Bonding Wire

A silver-core gold-coated bonding wire with controlled thickness and resistance ratios stabilizes FAB formation and enhances bonding quality by ensuring high sphericity and circularity.

JP7573138B1Active Publication Date: 2024-10-24TATSUTA ELECTRICWIRE & CABLE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024523409
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-01-31
Filing Date
2024-01-29
Publication Date
2024-10-24
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

Bonding wires with a silver core coated with a gold layer face challenges in forming a free air ball (FAB) with high sphericity and achieving a good circular shape for the first joint due to instability during ball bonding.

Method used

A bonding wire with a silver core and a gold coating layer, containing specific ratios of thickness and specific resistance, along with optional palladium, indium, and bismuth, ensures stable FAB formation and circular first joint shape.

Benefits of technology

The bonding wire achieves high sphericity and circularity of the FAB, improving corrosion resistance and bonding strength, while maintaining specific resistance balance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573138000002
    Figure 0007573138000002
  • Figure 0007573138000001
    Figure 0007573138000001
Patent Text Reader

Abstract

The present invention provides a bonding wire that can form a FAB with high sphericity and good shape, in which a coating layer mainly made of Au is provided on the surface of a core material mainly made of Ag. The bonding wire of the present invention is a bonding wire W having a core material 10 mainly made of Ag and a coating layer 12 mainly made of Au provided on the surface of the core material 10, in which the core material 10 contains one or more elements selected from the group consisting of Au, Pd, and In, the ratio of the thickness of the coating layer 12 to the diameter of the core material 10 is 0.0014 or more and 0.0048 or less, and the ratio of the resistivity of the core material 10 to the resistivity of the coating layer 12 is 85% or more and 115% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a bonding wire in which the surface of a bonding wire containing Ag (silver) as a main component is coated with a coating layer containing Au (gold) as a main component. [Background technology]

[0002] Bonding wires used to connect electrodes on semiconductor elements to electrodes on substrates are generally very thin and are made from metal materials that have good conductivity and are easy to process. In particular, bonding wires primarily composed of Au have been widely used due to their chemical stability and ease of handling in air.

[0003] However, bonding wires containing Au as the main component are very expensive because 99% or more of their mass is Au. Therefore, bonding wires containing Ag as the main component instead of Au have been proposed (for example, Patent Documents 1 and 2 listed below).

[0004] Although Ag is cheaper than Au, Ag-based bonding wires are more susceptible to sulfuration of the wire surface, which causes poor bonding to the electrode, compared to Au-based bonding wires. To prevent poor bonding due to Ag sulfuration, bonding wires have been proposed in which the surface of a core material primarily made of Ag is coated with a coating layer primarily made of Au (for example, Patent Documents 3 to 5 listed below). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5616165 [Patent Document 2] Patent No. 5529992 [Patent Document 3] Special table number 2016-517623 [Patent Document 4] International Publication WO2013 / 129253 [Patent Document 5] International Publication WO2021 / 205674 Summary of the Invention [Problem to be solved by the invention]

[0006] When a coating layer primarily made of Au is applied to the surface of a core material primarily made of Ag, it is difficult to consistently form a free air ball (hereafter abbreviated as FAB) with a good shape and high sphericity when ball bonding to an electrode, and it is also difficult to obtain a good circular shape for the first joint formed when the FAB is brought into contact with the electrode and crushed.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a bonding wire having a coating layer mainly composed of Au on the surface of a core material mainly composed of Ag, which can form a FAB with a good shape and high sphericity, and can make the shape of the first joint a good circle. [Means for solving the problem]

[0008] In order to solve the above problems, the bonding wire of the present invention is a bonding wire having a core material containing Ag as a main component and a coating layer containing Au as a main component provided on the surface of the core material, wherein the core material contains one or more elements selected from Au, Pd (palladium), and In (indium), the ratio of the film thickness of the coating layer to the diameter of the core material is 0.0014 or more and 0.0048 or less, and the ratio of the resistivity of the core material to the resistivity of the coating layer is 85% or more and 115% or less. The core material contains Au and Pd, with the Au content being higher than the Pd content. It is something. Another bonding wire of the present invention is a bonding wire having a core material containing Ag as a main component and a coating layer formed on the surface of the core material and containing Au as a main component, The core material contains one or more elements selected from the group consisting of Au, Pd, and In, the ratio of the thickness of the coating layer to the diameter of the core material is 0.0014 or more and 0.0048 or less, the ratio of the resistivity of the core material to the resistivity of the coating layer is 85% or more and 115% or less, and the core material contains 1 mass ppm or more and 50 mass ppm or less of Bi.

[0009] The present invention Other In the bonding wire, the core material may contain at least one of Au and Pd.

[0010] The present invention OtherIn the bonding wire, the core material may contain Au and Pd, with the Au content being greater than the Pd content.

[0012] In the bonding wire according to the present invention, the core material may contain 0.1 mass % to 1.0 mass % of In. [Effects of the Invention]

[0013] The bonding wire of the present invention is a bonding wire having a coating layer mainly composed of Au on the surface of a core material mainly composed of Ag, and can form a FAB with a good shape and high sphericity, and can make the shape of the first joint a good circle. [Brief explanation of the drawings]

[0014] [Figure 1] 1 is a cross-sectional view of a bonding wire according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0015] (1) Composition of bonding wire W A bonding wire W according to one embodiment of the present invention will be described below with reference to the drawings.

[0016] The bonding wire W of this embodiment is a bonding wire for connecting electrodes (e.g., Al alloy electrodes, nickel-palladium-gold coated electrodes, Au coated electrodes, etc.) on a semiconductor element in a semiconductor device (power IC, LSI, transistor, BGA (Ball Grid Array package), QFN (Quad Flat Non-lead package), LED (Light Emitting Diode), etc.) to conductor wiring (electrodes) of a circuit wiring board (lead frame, ceramic substrate, printed circuit board, etc.) 2 by ball bonding. Note that the bonding wire W of this embodiment can be used as a bonding wire in various forms other than semiconductor devices.

[0017] As shown in Figure 1, the bonding wire W of this embodiment comprises a core material 10 mainly composed of Ag and a coating layer 12 mainly composed of Au, and the coating layer 12 covers the entire outer surface of the core material 10 so that there are no exposed portions.

[0018] Specifically, the core material 10 contains 90% by mass or more, preferably 95% by mass or more, of Ag. The Ag constituting the core material 10 may contain impurities such as Fe (iron) that are inevitably present during purification, and it is preferable to produce an Ag alloy constituting the bonding wire W using Ag with a purity of 99.9% by mass or more.

[0019] The core material 10 contains one or more elements selected from the group consisting of Au, Pd, and In in addition to Ag, and the resistivity ρ1 of the core material 10 is adjusted. In other words, the contents of Au, Pd, and In in the core material 10 are adjusted so that the ratio β (=ρ1 / ρ2) of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 is 85% or more and 115% or less, preferably 90% or more and 110% or less.

[0020] For example, the resistivity of the core material 10 and the coating layer 12 can be set to 1.95 μΩ·cm or more and 3.26 μΩ·cm or less, and the resistivity of the coating layer 12 can be set to 2.30 μΩ·cm or more and 2.83 μΩ·cm or less.

[0021] When the resistivity of the coating layer 12 is 2.3 μΩ·cm, the core material 10 contains only one element selected from the group consisting of Au, Pd, and In, and in order to set the ratio β of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 to 85% or more and 115% or less, the core material 10 can contain 1.3 mass% or more and 4.0 mass% or less of Au, 0.7 mass% or more and 2.1 mass% or less of Pd, and 0.2 mass% or more and 0.6 mass% or less of In.

[0022] Furthermore, the bonding wire W has a diameter φ of the core material 10 and a thickness t of the coating layer 12 set so that the ratio α (= t / φ) of the thickness t of the coating layer 12 to the diameter φ of the core material 10 is 0.0014 or more and 0.0048 or less. The diameter of the core material 10 may be various sizes depending on the application of the bonding wire. For example, the diameter (wire diameter) φ of the core material 10 can be 15 μm or more and 150 μm or less. The thickness t of the coating layer 12 is preferably 0.15 μm or more and 0.50 μm or less.

[0023] For the resistivity of the core material 10, three evaluation samples are prepared, and the resistivity of each of the three evaluation samples is measured at room temperature using the four-terminal method, and the average value of the measurement results is defined as the resistivity of the core material 10. For the resistivity of the coating layer 12, three evaluation samples are prepared from bonding wires made with the same alloy composition as the coating layer 12, and the resistivity of each of the three evaluation samples is measured at room temperature using the four-terminal method, just like the core material 10, and the average value of the measurement results is defined as the resistivity of the core material 10.

[0024] The diameter φ of the core material 10 and the thickness t of the coating layer 12 were determined by irradiating X-rays using a fluorescent X-ray thickness meter and converting the intensity of the fluorescent X-rays generated into the thickness of the coating layer.

[0025] The bonding wire W preferably contains Au in the core material 10, and preferably contains Pd together with Au. When the core material 10 contains both Au and Pd, the Au content is preferably greater than the Pd content. When the core material 10 contains both Au and Pd, the total Au and Pd content is preferably 0.6% by mass or more and 3.0% by mass or less.

[0026] The core material 10 may contain 0.1% by mass or more and 1.0% by mass or less of In. When the core material 10 contains 0.1% by mass or more of In, the corrosion resistance of the first bonded portion formed when the FAB is pressed against the electrode and crushed is improved, thereby improving long-term reliability. When the In content of the core material 10 is 1.0% by mass or less, the specific resistance of the wire is maintained within an appropriate range.

[0027] Furthermore, the core material 10 may contain 1 mass ppm or more and 50 mass ppm or less of Bi in addition to one or more elements selected from the group consisting of Au, Pd, and In.

[0028] In the present invention, in addition to the above-mentioned Au, Pd, Bi, and In, one or two elements selected from Ca and Cu may be further contained. If the total content of Ca and Cu is 100 mass ppm or less, the above-mentioned effects achieved by adding Au, Pd, Bi, and In are not impaired, and the strength of the wire can be improved. When Ca and / or Cu are added, the total content of Ca and Cu is preferably 1 mass ppm or more and 100 mass ppm or less, and more preferably 5 mass ppm or more and 85 mass ppm or less.

[0029] The coating layer 12 contains 95% by mass or more, preferably 99% by mass or more, of gold, with gold being the main component. The coating layer 12 may be made of pure gold (gold content of 99.9% or more), or may be made of a gold alloy containing gold and additive elements. The gold alloy constituting the coating layer 12 may contain at least one element selected from the group consisting of Ag, Pd, Bi, Pt (platinum), Ni (nickel), Co (cobalt), and Sb (antimony).

[0030] (2) Manufacturing method of bonding wire W Next, an example of a method for manufacturing the bonding wire W having the above configuration will be described.

[0031] First, an element selected from Au, Pd, and In is added to Ag with a purity of 99.9% by mass or more, and Bi, Ca, and Cu are added as necessary to contain 95% by mass or more of Ag, thereby casting an Ag alloy with a resistivity of 85% to 115% of the resistivity ρ2 of the coating layer 12, and then a rod-shaped ingot of a predetermined diameter is produced by a continuous casting method.

[0032] Next, the rod-shaped ingot is drawn to reduce its diameter to a predetermined diameter of the core material 10. Thereafter, a coating layer 12 containing Au is formed on the entire outer periphery of the core material 10. The coating layer 12 can be formed by known means such as electroplating, electroless plating, or vapor deposition.

[0033] The core material 10 on which the coating layer 12 is formed is then further drawn to reduce its diameter to a predetermined value, thereby obtaining a bonding wire W in which the ratio α of the thickness t of the coating layer 12 to the diameter φ of the core material 10 is 0.0014 or more and 0.0048 or less, and the ratio β of the specific resistance ρ1 of the core material 10 to the specific resistance ρ2 of the coating layer 12 is 85% or more and 115% or less.

[0034] If necessary, heat treatment may be performed on the bonding wire W during or after the wire drawing process. As an example of the heat treatment, continuous annealing treatment may be performed at 300 to 1000°C for 0.1 to 60 seconds in an air atmosphere, a nitrogen gas atmosphere, or a mixed gas atmosphere of 5% hydrogen and 95% nitrogen.

[0035] (3) Effects In the bonding wire W of this embodiment, a coating layer 12 mainly composed of gold is provided on the outer surface of the core material 10, which improves the corrosion resistance of the bonding wire W and provides good bonding strength to metals that constitute electrodes such as Al (aluminum), Au, Ag, and alloys thereof.

[0036] In the bonding wire W, by setting the film thickness t of the coating layer 12 to 0.0014 times or more the wire diameter φ of the core material 10, the corrosion resistance of the bonding wire W is exhibited, ball bonding in the atmosphere becomes possible, and good bonding strength is obtained with respect to the metal constituting the electrode. Furthermore, by setting the film thickness t of the coating layer 12 to 0.0048 times or less the wire diameter φ of the core material 10, the balance of the surface tension of the molten bonding wire W during FAB formation can be well maintained, and a well-shaped FAB with high sphericity can be formed.

[0037] In the bonding wire W, by setting the ratio of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 to be 85% or more and 115% or less, when the tip of the bonding wire W is discharge-heated, the discharged electricity flows uniformly through the tip of the bonding wire W, melting the tip of the bonding wire W from all directions and growing a FAB uniformly. As a result, a well-shaped FAB with high sphericity can be formed, and the shape of the first joint can be made to be a good circle.

[0038] In the bonding wire W, since the core material 10 contains Au, when a FAB is formed at the tip of the bonding wire W by discharge heating or the like, the Au in the coating layer 12 is less likely to diffuse into the core material 10, making it possible to more stably form a FAB with a good shape and high sphericity.

[0039] Since Pd has a higher resistivity than Au, by including Pd in ​​the core material 10 together with Au, the total content of Au and Pd can be reduced while the resistivity of the core material 10, which is primarily composed of Ag, can be made closer to the resistivity of Au. Furthermore, when the core material 10 contains both Au and Pd, the content of Au is higher than that of Pd, making it possible to form a FAB with a good shape and high sphericity, and to make the shape of the first joint a good circle.

[0040] In the bonding wire W, when the core material 10 contains Bi in an amount of 1 mass ppm or more and 50 mass ppm or less, a FAB with a good shape and high sphericity can be stably formed.

[0041] In the bonding wire W, if the core material 10 contains 0.1 mass % or more of In, the corrosion resistance of the first bond formed when the FAB is pressed against the electrode and crushed can be improved, thereby improving long-term reliability. If the In content in the core material 10 is 1.0 mass % or less, the specific resistance of the wire can be maintained within an appropriate range, and a FAB with a good shape and high sphericity can be formed.

[0042] Although the embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, as well as within the scope of the inventions described in the claims and their equivalents. [Example]

[0043] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.

[0044] An Ag alloy having the composition shown in Table 1 below was melted using an Ag raw material with a purity of 99.9% by mass or more, and a rod-shaped ingot was produced by continuous casting. The rod-shaped ingot was then subjected to wiredrawing to reduce the diameter of the core material 10 to 105 μm, and then a coating layer 12 made of an Au alloy having the composition shown in Table 1 below was formed on the outer circumferential surface of the core material 10 by electroplating. The core material 10 with the coating layer 12 formed thereon was then further wiredrawn to reduce the diameter to a wire diameter φ of 20 μm and a coating layer 12 thickness t of approximately 57 nm, and then subjected to continuous annealing (heat treatment) at 400 to 600°C for 0.4 to 0.5 seconds in a mixed gas atmosphere of 5% hydrogen and 95% nitrogen, thereby obtaining bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7.

[0045] In addition, wires consisting only of the core material 10 of the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7, and wires consisting of the same alloy composition as the coating layer 12 of the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7 were produced by the same method as above, except that the outer surface of the core material 10 was not coated with Au.

[0046] Then, for the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7, the diameter φ of the core material 10 and the thickness t of the coating layer 12 were measured using the above-mentioned measurement method, and the ratio α of the thickness t of the coating layer 12 to the diameter φ of the core material 10 was calculated from these measurement results.

[0047] Furthermore, using a wire consisting of only the core material 10 and a wire having the same alloy composition as the coating layer 12, the resistivity ρ1 of the core material 10 and the resistivity ρ2 of the coating layer 12 were measured by the above-mentioned measurement method. From the obtained resistivity ρ1 of the core material 10 and the resistivity ρ2 of the coating layer 12, the ratio β of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 was calculated.

[0048] The diameter φ of the core material 10, the thickness t of the coating layer 12, the ratio α, the specific resistance ρ1 of the core material 10, the specific resistance ρ2 of the coating layer 12, and the ratio β of the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7 are as shown in Table 1 below.

[0049] The resulting bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7 were evaluated in the following items (1) to (4). Specific evaluation methods were as follows. (1)FAB sphericity (formability) Using a wire bonder (Shinkawa Co., Ltd., UTC-5000NeoCu), fabricated fabricated aluminum balls (FABs) measuring 1.9 to 2.1 times the wire diameter were prepared in an ambient atmosphere. To evaluate the sphericity (formability) of the fabricated aluminum balls, 100 fabricated aluminum balls were prepared for each bonding wire used in the examples and comparative examples. They were then visually inspected using a general-purpose electron microscope (JEOL Ltd., JSM-6510LA) to measure the lengths of the fabricated aluminum balls parallel to and perpendicular to the wire. If the average ratio (X / Y) of the fabricated aluminum balls (the length X parallel to the wire and the length Y perpendicular to the wire) was within a range of 100±5%, the balls were judged to have sphericity and were graded "A." If the average value of the ratio (X / Y) was 92% or more but less than 95% or between 105% and 108% or less, the balls were graded "B." If the average value of the ratio (X / Y) was 90% or more but less than 92% or between 108% and 110%, the balls were graded "C." If the average value of the ratio (X / Y) was 90% or more but less than 92% or between 108% and 110%, the balls were visually inspected to be non-circular, the balls were graded "D." (2) Shape stability of the first joint Using the wire bonder described in (1) above, 100 fabricated adhesive layers (FABs) fabricated in an atmospheric gas atmosphere were pressed against electrodes, and bonding was performed so that the diameter of the first bond was 1.4 times the diameter of the fabricated adhesive layer. The center-to-center distance between the center of the first bond and the chamfer diameter of the capillary attached to the wire bonder was measured using a three-dimensional microscope (Olympus STM6 compact measuring microscope). If the center-to-center distance for all 100 fabricated adhesive layers was 2.5 μm or less, the result was rated "A." If the incidence of first bonded layers greater than 2.5 μm and less than 5 μm was less than 20%, the result was rated "B." If the incidence of first bonded layers greater than 2.5 μm and less than 5 μm was 20% or more, the result was rated "C." If even one first bonded layer exceeded 5 μm, the result was deemed unsuitable for fine-pitch applications due to poor circularity, and the result was rated "D." (3) High-temperature storage test (long-term reliability) After bonding in an air atmosphere using the wire bonder used in (1) above, a semiconductor sample was prepared that was sealed with epoxy resin. The semiconductor sample was prepared using a commercially available thermostatic oven and held at 150°C for 1000 hours, after which electrical measurements were performed to evaluate conductivity. Five hundred wires were evaluated, and a defect rate of 1% or less was assigned an "A," a defect rate of more than 1% but less than 3% was assigned a "B," and a defect rate of more than 3% was assigned a "D" due to low resistance. (4) Overall evaluation For the evaluation items (1) to (3) above, if all received an A rating, the rating was "A," if there were one or two A ratings, the rating was "B," if there were no A ratings, the rating was "C," and if there was at least one D rating, the rating was "D."

[0050] [Table 1] The results are shown in Table 1, and Examples 1 to 21 obtained good results in all of the evaluations (1) to (4) above.

[0051] On the other hand, in Comparative Examples 1 to 3, where the ratio α of the thickness t of the coating layer 12 to the diameter φ of the core material 10 was outside the range of 0.0014 to 0.0048, a circular FAB was not formed, and the FAB sphericity and the shape of the first bonded portion deteriorated.Furthermore, in Comparative Examples 4 to 7, where the ratio β of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 was outside the range of 85% to 115%, the shape of the first bonded portion deteriorated. [Explanation of symbols]

[0052] 10...core material, 12...covering layer, W...bonding wire

Claims

1. A bonding wire having a core material containing Ag as a main component and a coating layer containing Au as a main component provided on a surface of the core material, The core material contains one or more elements selected from the group consisting of Au, Pd, and In, a ratio of a thickness of the coating layer to a diameter of the core material is 0.0014 or more and 0.0048 or less; The ratio of the resistivity of the core material to the resistivity of the coating layer is 85% or more and 115% or less, The bonding wire, wherein the core material contains Au and Pd, and the Au content is greater than the Pd content.

2. A bonding wire having a core material containing Ag as a main component and a coating layer containing Au as a main component provided on a surface of the core material, The core material contains one or more elements selected from the group consisting of Au, Pd, and In, a ratio of a thickness of the coating layer to a diameter of the core material is 0.0014 or more and 0.0048 or less; The ratio of the resistivity of the core material to the resistivity of the coating layer is 85% or more and 115% or less, The core material contains Bi in an amount of 1 ppm by mass or more and 50 ppm by mass or less.

3. The bonding wire according to claim 2 , wherein the core material contains at least one of Au and Pd.

4. The bonding wire according to claim 3 , wherein the core material contains Au and Pd, and the Au content is greater than the Pd content.

5. The bonding wire according to any one of claims 1 to 4, wherein the core material contains 0.1 mass% or more and 1.0 mass% or less of In.

Citation Information

Patent Citations

  • Silver wire bonding wire filmed with gold

    JP2001176912A

  • Wire joining structure, bonding wire used in same, and semiconductor device

    WO2021065036A1

  • Prolonging of useful life of vegetable

    JP1980029992A

  • Method and unit for electrostatic latent image development

    JP1981016165A

  • Covered wire for bonding applications

    JP2016517623A