Polishing pad, manufacturing method of polishing pad, and wafer polishing method
The polishing pad with a base resin and optimized pore structure addresses the challenges of liquid management and environmental impact in wafer polishing, achieving cost-effective and energy-efficient semiconductor manufacturing.
Patent Information
- Application Number
- JP2022009205
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-01-25
AI Technical Summary
Existing wafer polishing methods using abrasive-free polishing pads face challenges in managing polishing liquids, requiring separate cleaning processes, increasing manufacturing costs, and posing environmental burdens due to the use of expensive and complex liquid management systems.
A polishing pad with a base resin containing multiple pores and abrasive particles, optimized with specific pore and network thicknesses, allows for the use of inexpensive polishing liquids, simplifies liquid management, and reduces power consumption.
The optimized polishing pad simplifies liquid management, reduces power consumption, and lowers manufacturing costs while minimizing environmental impact by eliminating the need for separate cleaning and liquid reprocessing.
Smart Images

Figure 0007573556000005 
Figure 0007573556000006 
Figure 0007573556000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad, a method for manufacturing a polishing pad, and a method for polishing a wafer. [Background technology]
[0002] A wafer polishing apparatus is known that includes a platen and a carrier. The platen has a first fixed surface that extends in a direction perpendicular to a first axis and is rotated about the first axis. The carrier has a second fixed surface that extends in a direction perpendicular to a second axis that is parallel to the first axis and faces the first fixed surface, and is rotated about the second axis.
[0003] When using this wafer polishing apparatus to polish flat wafers such as Si, SiC, GaN, etc., a polishing pad is fixed to a first fixing surface of a platen, and a wafer is fixed to a second fixing surface of a carrier. Then, the platen and the carrier are rotated while the polishing pad and the wafer are in contact with each other under a predetermined surface pressure in the presence of a polishing liquid. When the polishing liquid contains an agent such as an alkali, the wafer is polished in a chemical mechanical polishing (CMP) process.
[0004] When the polishing pad does not have abrasive particles, such as general nonwoven fabric or hard urethane, the polishing liquid contains abrasive particles. In this case, the polishing liquid needs to be managed and the wafer needs to be cleaned after polishing. In addition, since the polishing liquid is expensive, it is necessary to collect the polishing liquid after polishing and re-adjust it to a specified state before reusing it. Furthermore, when the polishing liquid and cleaning liquid after polishing are discarded, complex processing must be performed so that they do not harm the environment. Therefore, in this case, the manufacturing cost of semiconductor devices increases and the environmental load is large.
[0005] On the other hand, as disclosed in Patent Documents 1 to 3, when the polishing pad is made of a base resin, has a base material with a plurality of pores formed therein, and has abrasive particles held in the base material or the pores, a polishing liquid that does not contain abrasive particles can be used. In this case, if only water is used as the polishing liquid, management of the polishing liquid is not required, and the wafer after polishing is already washed with the polishing liquid, so that a separate cleaning step can be omitted or simplified. In addition, since the polishing liquid is inexpensive, it is not necessarily necessary to recover and reuse the polishing liquid after polishing. Furthermore, when the polishing liquid after polishing is discarded, not much processing is required. Therefore, in this case, it is possible to realize a reduction in the manufacturing cost of semiconductor devices and reduce the environmental load. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 4266579 [Patent Document 2] Patent No. 5511266 [Patent Document 3] Patent No. 6636634 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the wafer polishing process, there is also a strong demand for lower power consumption.
[0008] The present invention has been made in consideration of the above-mentioned conventional situation, and aims to provide a polishing pad that allows easy management of the polishing liquid, omits or simplifies the cleaning process of the wafer after polishing, does not require troublesome disposal of the polishing liquid after polishing, and can realize low power consumption. Another aim of the present invention is to provide a method for manufacturing such a polishing pad. Another aim of the present invention is to provide a method for polishing such a wafer. [Means for solving the problem]
[0009] The polishing pad of the present invention is used in a wafer polishing apparatus including a base plate having a fixing surface extending in a direction perpendicular to an axis and rotated about the axis, and a carrier for holding a flat wafer so as to be rotatable relative to the base plate, A polishing pad fixed to the fixing surface and polishing the wafer under a predetermined surface pressure in the presence of a polishing liquid, The polishing tool has a base material made of a base material resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores; The base resin is polyethersulfone, When any of the pores in the base material is defined as a specific pore and the pores adjacent to the specific pore are defined as adjacent pores, a network is formed between the center of the specific pore and the center of the adjacent pore, the network is made of the base material resin, has a width of 1.89 to 9.88 μm, and the average width is 4.05 to 5.89 μm. 、 In the specific pore, a minor axis which is the shortest inner diameter and a major axis which is the longest inner diameter are defined; The pore diameter, which is a value obtained by multiplying the minor axis, the major axis, pi, and 1 / 4, is 7.01 to 258.72 μm, The average pore size is 19.84 to 67.10 μm. It is characterized by the following.
[0010] The polishing pad of the present invention is made of a base resin, has a base material with a plurality of pores formed therein, and has abrasive particles held in the base material or the pores. Therefore, a polishing liquid that does not contain abrasive particles can be used. Therefore, the polishing liquid is easy to manage, and the cleaning process of the wafer after polishing can be omitted or simplified. In addition, since the polishing liquid is inexpensive, it is not necessarily necessary to recover and reuse the polishing liquid after polishing. Furthermore, when the polishing liquid after polishing is discarded, not much processing is required.
[0011] The inventors have considered that increasing the ratio of pores in the polishing pad is effective in suppressing power consumption. This is because it is believed that increasing the porosity can suppress the contact area ratio between the wafer and the polishing pad, thereby reducing resistance. However, it is presumed that simply increasing the porosity makes the structure of the polishing pad unstable, making it difficult to achieve stable polishing. For this reason, the inventors have obtained an optimal polishing pad by adjusting the ratio of the base resin, the abrasive particles, and the solvent in various ways, and have completed the present invention.
[0012] That is, the base material of the polishing pad has a unique network made of base resin. According to the inventors' tests, in the polishing pad of the present invention, when any pore is a specific pore and the pore adjacent to the specific pore is an adjacent pore, the network has a width of 1.89 to 9.88 μm between the center of the specific pore and the center of the adjacent pore, and the average width is 4.05 to 5.89 μm. In this case, low power consumption can be achieved.
[0013] More specifically, if the network thickness is less than 1.89 μm, the polishing pad structure is likely to become unstable. If the network thickness exceeds 9.88 μm, it is difficult to reduce power consumption. If the average network thickness is less than 4.05 μm, the polishing pad structure is likely to become unstable. If the average network thickness exceeds 5.89 μm, it is difficult to reduce power consumption.
[0014] Therefore, by using the polishing pad of the present invention in the wafer polishing apparatus, the polishing liquid can be easily managed, a separate cleaning process can be omitted or simplified, the polishing liquid after polishing can be easily disposed of, and power consumption can be reduced, which reduces the manufacturing cost of semiconductor devices and reduces the environmental load.
[0015] The method for producing a polishing pad of the present invention includes a first step of preparing a paste containing a base resin, abrasive particles, and a solvent; A second step of forming the paste into a sheet-like molded body; a third step of immersing the molded body in a replacement liquid to replace the solvent in the molded body with the replacement liquid to obtain a replacement body; and a fourth step of removing the replaced liquid from the replaced body to obtain a polishing pad having a base material made of the base material resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores. The base resin is polyethersulfone, The base material has a network between the center of the specific pore and the center of the adjacent pore, the network being made of the base material resin and having a width of 1.89 to 9.88 μm, with the average width being 4.05 to 5.89 μm. 、 In the specific pore, a minor axis which is the shortest inner diameter and a major axis which is the longest inner diameter are defined; The pore diameter, which is a value obtained by multiplying the minor axis, the major axis, pi, and 1 / 4, is 7.01 to 258.72 μm, The average pore size is 19.84 to 67.10 μm. Thus, the ratio of the base resin, the abrasive particles, and the solvent is adjusted in the first step.
[0016] The polishing pad of the present invention can be manufactured by the manufacturing method of the present invention. The inventors confirmed that the polishing pad of the present invention can be manufactured by the manufacturing method of the present invention using N-methyl-2-pyrrolidone as the solvent and water as the substitute liquid.
[0017] The present invention provides a wafer polishing method, which comprises bringing a flat wafer into contact with a flat polishing pad under a predetermined surface pressure in the presence of a polishing liquid, rotating the wafer and the polishing pad relatively around an axis extending in a thickness direction of the wafer, and polishing the wafer, comprising: The polishing pad is made of a base resin and has a base material having a plurality of pores formed therein, and abrasive particles held in the base material or the pores, The base resin is polyethersulfone, The base material has a network between the center of the specific pore and the center of the adjacent pore, the network being made of the base material resin and having a width of 1.89 to 9.88 μm, with the average width being 4.05 to 5.89 μm. 、 In the specific pore, a minor axis which is the shortest inner diameter and a major axis which is the longest inner diameter are defined; The pore diameter, which is a value obtained by multiplying the minor axis, the major axis, pi, and 1 / 4, is 7.01 to 258.72 μm, The average pore size is 19.84 to 67.10 μm. It is characterized by the following.
[0018] The wafer polishing method of the present invention uses the polishing pad of the present invention, and therefore can reduce the manufacturing costs of semiconductor devices and the environmental load. Effect of the Invention
[0019] By using the polishing pad of the present invention, the management of the polishing liquid is easy, a separate cleaning process can be omitted or simplified, the processing of the polishing liquid after polishing is not troublesome, and power consumption can be reduced. The manufacturing method of the present invention can manufacture the polishing pad of the present invention. The wafer polishing method of the present invention can reduce the manufacturing cost of semiconductor devices and reduce the environmental load. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic enlarged cross-sectional view of the polishing pads of Examples 1 to 3 and Comparative Examples 1 and 2. As shown in FIG. [Diagram 2] FIG. 2 is a schematic plan view of an SEM photograph of the polishing surface of each of the polishing pads of Examples 1 to 3 at 2000 magnifications, in which the abrasive particles are omitted and only the pores are shown. [Diagram 3] FIG. 3 is a schematic plan view of an SEM photograph of the polishing surface of the polishing pads of Comparative Examples 1 and 2 at 2000 magnification, in which the abrasive particles are omitted and only the pores are shown. [Figure 4] FIG. 4 is a schematic cross-sectional view of a wafer polishing apparatus used in the wafer polishing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] According to tests conducted by the inventors, when the shortest inner diameter and the longest inner diameter are defined for a specific pore, the pore diameter, which is the product of the shortest diameter, the longest diameter, pi, and 1 / 4, is 7.01 to 258.72 μm, and the average pore diameter is preferably 19.84 to 67.10 μm.
[0022] If the pore diameter defined above is less than 7.01 μm, the structure of the polishing pad is likely to become unstable. If the pore diameter exceeds 258.72 μm, it is difficult to reduce power consumption. If the average value of the pore diameter is less than 19.84 μm, the structure of the polishing pad is likely to become unstable. If the average value of the pore diameter exceeds 67.10 μm, it is difficult to reduce power consumption.
[0023] The base resin used to manufacture the polishing pad is polyethersulfone (PES). )of It is possible to adopt . The researchers have confirmed the effectiveness of this method when the base resin is PES.
[0024] As the solvent used to manufacture the polishing pad, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone (NEP), dimethylformamide, dimethylsulfoxide, acetone, ethyl acetate, methyl ethyl ketone, etc. may be used. These may be used alone or in combination of two or more. The solvent is selected according to the base resin.
[0025] As abrasive particles that can be used to manufacture a polishing pad or that can be contained in a polishing liquid, silica, ceria, alumina, zirconia, titania, diamond, manganese oxide, barium carbonate, chromium oxide, iron oxide, etc. These may be used alone or in a mixture of two or more types.
[0026] The paste used to manufacture the polishing pad may contain alkaline fine particles such as sodium carbonate, piperazine, potassium hydroxide, sodium hydroxide, calcium oxide, potassium carbonate, and magnesium oxide, in addition to the base resin, the abrasive particles, and the solvent. The paste may also contain water repellents such as fluorine-based water repellents, silicon-based water repellents, hydrocarbon-based water repellents, and metal compound-based water repellents. Furthermore, the paste may contain pigments such as inorganic pigments such as titanium dioxide, calcium carbonate, and carbon black, and organic pigments such as azo pigments and polycyclic pigments. These may be used alone or in combination of two or more.
[0027] In the method for manufacturing a polishing pad, when an oil-based solvent is used, a water-based liquid such as tap water can be used as the replacement liquid to replace the solvent.
[0028] When a polishing liquid is used, the polishing liquid may be pure water, may be oil-based, or may contain an acidic or alkaline chemical.
[0029] (Examples and Comparative Examples) Examples 1 to 3 embodying the present invention and Comparative Examples 1 and 2 will be described below.
[0030] First, in the first step, the following base resin, abrasive particles, and solvent were prepared. (Base resin) PES (abrasive particles) Silica (SiO2) (average particle size: 0.3 μm) (solvent) NMP
[0031] These were mixed in the volume percentages shown in Table 1 to obtain pastes for Examples 1 to 3 and Comparative Examples 1 and 2. In Examples 1 to 3 and Comparative Examples 1 and 2, the volume percentages of the base resin and the abrasive particles were made equal, regardless of the amount of solvent added.
[0032] [Table 1]
[0033] In the second step, the pastes obtained in the first step are molded into a sheet-like molded body using a molding device such as a T-die. The molding method is not limited to this as long as it can achieve a uniform thickness to some extent.
[0034] In the third step, each molded body was immersed in tap water as a replacement liquid, and after a predetermined time, each was taken out of the tap water and dried to obtain each solidified body. The surface of each solidified body was ground to a predetermined thickness to obtain a polishing pad 10 with a diameter of 30 cm. Each polishing pad 10 did not have a groove pattern.
[0035] 1, each polishing pad 10 has a base material 12 made of a base resin with a plurality of pores 14 formed therein, and abrasive particles 16 held in the base material 12 or the pores 14. Each pore 14 and each abrasive particle 16 are partially exposed to a polishing surface 10a located on the surface of the polishing pad 10.
[0036] The design specific gravity was calculated and the actual specific gravity was measured. The design specific gravity is the specific gravity when the base resin, abrasive particles, and solvent are mixed in the volume percentage shown in Table 1. The actual specific gravity is the actual specific gravity of each polishing pad 10. Next, the design specific gravity was divided by the actual specific gravity to obtain the ratio value. The design ratio of the resin was divided by that ratio value to obtain the resin ratio. Also, the design ratio of the abrasive particles was divided by that ratio value to obtain the abrasive particle ratio. Then, the resin ratio and the abrasive particle ratio were subtracted from 100 to obtain the porosity (volume %). The porosity of each polishing pad is also shown in Table 1.
[0037] SEM photographs of the polishing surface 10a of the polishing pad 10 of Examples 1 to 3 and Comparative Examples 1 and 2 were taken at 2000 magnifications, and the network thickness (μm) and pore diameter (μm) were measured from each SEM photograph.
[0038] Fig. 2 shows a schematic plan view in which the abrasive particles 16 are omitted from the SEM photographs of the polishing surface 10a of the polishing pad 10 of Examples 1 to 3, and only the pores 14 are shown. Fig. 3 shows a schematic plan view in which the abrasive particles 16 are omitted from the SEM photographs of the polishing surface 10a of the polishing pad 10 of Comparative Examples 1 and 2, and only the pores 14 are shown.
[0039] As shown in Fig. 2 and Fig. 3, in the SEM photograph, an arbitrary pore 14 is designated as a specific pore 14s, and a pore 14 adjacent to the specific pore 14s is designated as an adjacent pore 14n. If the center Os of the specific pore 14s and the center O of another pore 14 are connected by a straight line L, and the straight line L crosses any of the adjacent pores 14n already defined, the pore 14 is not designated as an adjacent pore 14n. In this way, several adjacent pores 14n are defined. There may be a plurality of adjacent pores 14n for a specific pore 14s. Then, the width P between the center Os of the specific pore 14s and the center On of the adjacent pore 14n was measured.
[0040] On the polishing surface 10a of the polishing pad 10 of Examples 1 to 3 and Comparative Examples 1 and 2, 20 specific pores 14s were identified and each was measured for its width P. The maximum, minimum and average width P on the polishing surface 10a of each polishing pad 10 are shown in Table 2.
[0041] [Table 2]
[0042] As shown in Table 2, the polishing surfaces 10a of the polishing pads 10 of Examples 1 to 3 have networks N with a width of 1.89 to 9.88 μm and an average width of 4.05 to 5.89 μm. These networks N are made of a base resin. On the other hand, the polishing pads 10 of Comparative Examples 1 and 2 also have networks N made of a base resin, but each network N has a width of 0.47 to 3.06 μm and an average width of only 1.31 to 1.87 μm.
[0043] In addition, 20 specific pores 14s were identified on the polishing surface 10a of the polishing pads 10 of Examples 1 to 3 and Comparative Examples 1 and 2, and the shortest inner diameter, a (μm), and the longest inner diameter, b (μm), were defined. The shortest inner diameter, a, the longest inner diameter, b, pi, and 1 / 4 were multiplied to determine the pore diameter (μm). The maximum, minimum, and average pore diameters of each polishing pad 10 are shown in Table 3.
[0044] [Table 3]
[0045] As shown in Table 3, the polishing surfaces 10a of the polishing pads 10 in Examples 1 to 3 have pore diameters ranging from 7.01 to 258.72 μm, with an average pore diameter ranging from 19.84 to 67.10 μm. On the other hand, the polishing pads 10 in Comparative Examples 1 and 2 have pore diameters ranging from 1.57 to 26.09 μm, with an average pore diameter ranging from only 8.94 to 11.45 μm.
[0046] As shown in FIG. 4, a wafer polishing apparatus (Engis EJW-380) was prepared for polishing a wafer 1, and the wafer 1 was polished using the polishing pads 10 of Examples 1 to 3 and Comparative Examples 1 and 2. The wafer polishing apparatus includes a plurality of carriers 5, a surface plate 7, a driving device 9, and a polishing liquid supplying device 11. Although only a single carrier 5 is illustrated in FIG. 4, the wafer polishing apparatus has a plurality of carriers 5. Each carrier 5 is in the shape of a horizontal disk. A second fixing surface 5a is recessed on the lower surface of each carrier 5, and the wafer 1 is fixed to the second fixing surface 5a. A carrier rotation shaft 5b is vertically protruded on the upper surface of each carrier 5. Each wafer 1 is a 4H-SiC single crystal having a diameter of 4 inches. The polished surface 1a, which is the Si surface of each wafer 1, faces downward.
[0047] The surface plate 7 is in the shape of a horizontal disk that contains all the carriers 5. A surface plate rotation shaft 7a protrudes vertically from the lower surface of the surface plate 7. The upper surface of the surface plate 7 serves as a first fixing surface 7b. A disk-shaped polishing pad 10 is fixed to the first fixing surface 7b with an adhesive so as to face each wafer 1. The center line O of the polishing pad 10 coincides with the first axis O1.
[0048] The driving device 9 has a main driving device 9a, a sub-driving device 9b, and a pressure device 9c. The main driving device 9a drives the base plate rotation shaft 7a to rotate around the first axis O1 at a predetermined speed. The sub-driving device 9b drives each carrier rotation shaft 5b to rotate around the second axis O2 at a predetermined speed. The pressure device 9c presses each carrier rotation shaft 5b and the sub-driving device 9b toward the base plate 7 with a predetermined load.
[0049] The polishing liquid supplying device 11 is provided above the platen 7. The polishing liquid supplying device 11 provides a polishing liquid 11a between each wafer 1 and the polishing pad 41. In the polishing methods of Examples 1 to 3 and Comparative Examples 1 and 2, the polishing liquid 11a was an aqueous potassium permanganate solution that did not contain abrasive particles.
[0050] In this wafer polishing apparatus, each wafer 1 was polished under the following conditions. Flow rate of polishing liquid 11a: 10 mL / min Load: 30kPa Rotation speed of surface plate 7: 60 rpm Carrier 5 rotation speed: 60 rpm Processing time: 60 minutes
[0051] The surface roughness Sa (nm) and power consumption (W) of the polished wafer 1 were evaluated. The surface roughness Sa was measured using a Nikon BW-D501. The results are shown in Table 4.
[0052] [Table 4]
[0053] From Table 4, it can be seen that the polishing pads 10 of Examples 1 to 3 can reduce the power consumption required to polish the wafer 1 to the same surface roughness Sa, compared to the polishing pads 10 of Comparative Examples 1 and 2. The reason for this is that the base material 12 of the polishing pads 10 of Examples 1 to 3 has a unique network N made of a base material resin. It is believed that in these polishing pads 10, the porosity can be increased by this network N, the contact area ratio between the wafer 1 and the polishing pad 10 can be suppressed, and the resistance can be reduced.
[0054] In addition, the polishing pads 10 of Examples 1 to 3 are made of a base resin, and have a base material 12 with a plurality of pores 14 formed therein, and abrasive particles 16 held in the base material 12 or the pores 14, so that a polishing liquid 11a that does not contain abrasive particles can be used. This makes it easy to manage the polishing liquid 11a, and the cleaning process of the wafer 1 after polishing can be omitted or simplified. In addition, since the polishing liquid 11a is inexpensive, it is not necessarily necessary to collect and reuse the polishing liquid 11a after polishing. Furthermore, when disposing of the polishing liquid 11a after polishing, no significant processing is required.
[0055] Therefore, by using the polishing pad 10 of Examples 1 to 3 in the above-mentioned wafer polishing apparatus, the polishing liquid 11a can be easily managed, a separate cleaning process can be omitted or simplified, the processing of the polishing liquid 11a after polishing is not troublesome, and power consumption can be reduced. Therefore, the manufacturing cost of semiconductor devices can be further reduced, and the environmental load can be reduced.
[0056] Moreover, the manufacturing methods of Examples 1 to 3 can manufacture the polishing pads 10 of Examples 1 to 3. Furthermore, the wafer polishing methods of Examples 1 to 3 can reduce the manufacturing costs of semiconductor devices and reduce the environmental impact.
[0057] In the above, the present invention has been described based on Examples 1 to 3. However, the present invention is not limited to the above Examples 1 to 3, and it goes without saying that the present invention can be modified and applied as appropriate without departing from the spirit of the present invention.
[0058] For example, the polishing pads 10 of Examples 1 to 3 had a base resin of PES and a solvent of NMP, but it is possible to change the base resin to PVDF and the solvent to NMP by adjusting the ratio of the base resin, abrasive particles 16, and solvent in the first step so that the network N made of the base resin has a thickness of 1.89 to 9.88 μm and an average thickness of 4.05 to 5.89 μm. [Industrial Applicability]
[0059] The present invention can be used in semiconductor manufacturing equipment. [Explanation of symbols]
[0060] O1…1st axis center 7b…First fixed surface 7…Fixed plate O2…2nd axis center 5a…Second fixed surface 5…Carrier 1...Wafer 10...Polishing pad 11a...polishing liquid 12...Base material 14…Stoma 16...Abrasive particles N…Network
Claims
1. The present invention is used in a wafer polishing apparatus including a base having a fixing surface extending in a direction perpendicular to an axis and rotated about the axis, and a carrier for holding a flat wafer so as to be rotatable relative to the base, A polishing pad fixed to the fixing surface and polishing the wafer under a predetermined surface pressure in the presence of a polishing liquid, The polishing tool has a base material made of a base material resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores; The base resin is polyethersulfone, When any of the pores in the base material is defined as a specific pore and the pores adjacent to the specific pore are defined as adjacent pores, a network is formed between the center of the specific pore and the center of the adjacent pore, the network being made of the base material resin and having a width of 1.89 to 9.88 μm and an average width of 4.05 to 5.89 μm; In the specific pore, a minor axis which is the shortest inner diameter and a major axis which is the longest inner diameter are defined; a pore diameter, which is a value obtained by multiplying the minor axis, the major axis, pi, and ¼, is 7.01 to 258.72 μm; The polishing pad is characterized in that the average pore size is 19.84 to 67.10 μm.
2. A first step of preparing a paste containing a base resin, abrasive particles, and a solvent; A second step of forming the paste into a sheet-like molded body; a third step of immersing the molded body in a replacement liquid to replace the solvent in the molded body with the replacement liquid to obtain a replacement body; and a fourth step of removing the replaced liquid from the replaced body to obtain a polishing pad having a base material made of the base material resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores. The base resin is polyethersulfone, In the base material, any one of the pores is defined as a specific pore, and the pores adjacent to the specific pore are defined as adjacent pores. Between the center of the specific pore and the center of the adjacent pore, there is a network made of the base material resin, having a width of 1.89 to 9.88 μm, and an average value of the width is 4.05 to 5.89 μm. In the specific pore, a minor axis which is the shortest inner diameter and a major axis which is the longest inner diameter are defined; a pore diameter, which is a value obtained by multiplying the minor axis, the major axis, pi, and ¼, is 7.01 to 258.72 μm; A method for manufacturing a polishing pad, comprising adjusting the ratio of the base resin, the abrasive particles, and the solvent in the first step so that the average pore diameter is 19.84 to 67.10 μm.
3. A wafer polishing method comprising the steps of: bringing a flat wafer into contact with a flat polishing pad under a predetermined surface pressure in the presence of a polishing liquid; rotating the wafer and the polishing pad relative to each other about an axis extending in a thickness direction of the wafer; The polishing pad is made of a base resin and has a base material having a plurality of pores formed therein, and abrasive particles held in the base material or the pores, The base resin is polyethersulfone, In the base material, any one of the pores is defined as a specific pore, and the pores adjacent to the specific pore are defined as adjacent pores. Between the center of the specific pore and the center of the adjacent pore, there is a network made of the base material resin, having a width of 1.89 to 9.88 μm, and an average value of the width is 4.05 to 5.89 μm. In the specific pore, a minor axis which is the shortest inner diameter and a major axis which is the longest inner diameter are defined; a pore diameter, which is a value obtained by multiplying the minor axis, the major axis, pi, and ¼, is 7.01 to 258.72 μm; A wafer polishing method, characterized in that the average pore size is 19.84 to 67.10 μm.
Citation Information
Patent Citations
Production of photo molding material for making stencil
JP1980011266A
Polishing pad for semiconductor substrate and method for polishing semiconductor substrate
JP2004281685A
Method for manufacturing fixed abrasive materials
JP2006519115A