Shutdown Separator
A separator for lithium ion batteries with a high-melting-point substrate and a thermally responsive ethylene-based coating layer addresses thermal runaway by forming a non-porous layer to halt reactions, enhancing safety.
Patent Information
- Application Number
- JP2022558504
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-04-29
AI Technical Summary
Thermal runaway and heat-related safety issues in lithium ion batteries and other lithium-based batteries are a concern, particularly due to their low onset temperature and rapid exothermic nature, necessitating improved electrode separators that can rapidly shut down thermal runaway below 135°C.
A separator for electrochemical cells comprising a porous substrate made of an olefin polymer with a melting point exceeding 130°C and a porous coating layer composed of ethylene-based microparticles with a melting temperature of 80°C to 110°C, which includes a dispersant and optional acid-functional wax, forming a non-porous layer upon heating to prevent further reactions.
The separator effectively shuts down thermal runaway by blocking ion transport when the coating layer melts, preventing further electrochemical reactions and ensuring safety in lithium ion batteries.
Smart Images

Figure 0007573647000004 
Figure 0007573647000005 
Figure 0007573647000006
Abstract
Description
[Background technology]
[0001] Thermal runaway and other heat-related safety problems are known with electrochemical cells such as lithium-ion batteries and other lithium-based batteries. The relatively low onset temperature and rapid exothermic nature of thermal runaway necessitates thermal shutdown of lithium batteries at temperatures well below the melting point of lithium, 179° C., and the rapid vaporization of organic electrolyte solvents around this same temperature range.
[0002] Demand for lithium-based batteries is expanding as they become more energetic and are increasingly used in high power applications such as hybrid electric vehicles (HEVs), etc. As a result, the art has recognized a need for improved electrode separators that can rapidly shut down thermal runaway in electrochemical cells at temperatures below 135° C. Summary of the Invention
[0003] The present disclosure provides an electrochemical cell. In one embodiment, the electrochemical cell includes a separator disposed between an optional anode and an optional cathode. The separator includes (A) a porous substrate and (B) a porous coating layer on the substrate. The porous substrate (A) is comprised of an olefin-based polymer having a melting temperature Tm of greater than 130° C. The porous coating layer (B) has a Tm of 80° C. to 110° C. The porous coating layer (B) is comprised of a plurality of particulates and an optional binder. The particulates have an average particle size of 0.3 micrometers to 1.5 micrometers. The particulates are comprised of (i) an ethylene-based polymer having (a) a density of less than 0.90 g / cc to 0.94 g / cc, (b) a Tm of 90° C. to 120° C., and (c) a melt index of 30 g / 10 min to 600 g / 10 min. The particulates are also comprised of (ii) C 14 ~C 40 The microparticles also include (iii) an optional acid-functional wax. [Brief description of the drawings]
[0004] [Figure 1] FIG. 1 is a schematic diagram of an electrochemical cell according to one embodiment of the present disclosure. [Diagram 2] FIG. 1 is a schematic diagram of an electrochemical cell according to one embodiment of the present disclosure. [Figure 3a] 1 shows scanning electron micrographs (SEM) of the porous coating layers of Examples 1, 2, and 3, respectively. [Figure 3b] 1 shows scanning electron micrographs (SEM) of the porous coating layers of Examples 1, 2, and 3, respectively. [Figure 3c] 1 shows scanning electron micrographs (SEM) of the porous coating layers of Examples 1, 2, and 3, respectively. [Figure 4] 1 is a temperature-time plot illustrating the gas permeability of a separator according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] definition Any reference to the Periodic Table of the Elements is to that published by CRC Press, Inc., 1990-1991. References to element groups in this table are by the new notation for numbering groups.
[0006] For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent U.S. version thereof is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art.
[0007] Numerical ranges disclosed herein include all values, inclusive, between the lower and upper limits, and in the case of ranges containing explicit values (e.g., 1 or 2, or 3-5, or 6, or 7), include every subrange between any two explicit values (e.g., the range 1-7 above includes 1-2, 2-6, 5-7, 3-7, 5-6, etc.).
[0008] Unless otherwise stated, implied from the context, or customary in the art to the contrary, all parts and percentages are by weight and all testing methods are current as of the filing date of this disclosure.
[0009] As used herein, the term "blend" or "polymer blend" refers to a blend of two or more polymers. Such blends may or may not be miscible (not phase separated at the molecular level). Such blends may or may not be phase separated. Such blends may or may not contain one or more domain configurations as determined from transmission electron spectroscopy, light scattering, x-ray scattering, and other methods known in the art.
[0010] The term "composition" refers to a mixture of materials that comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition.
[0011] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional component, step, or procedure, whether or not it is specifically disclosed. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additive, adjuvant, or compound, whether polymeric or not, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes any other component, step, or procedure from the scope of any succeeding description, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not expressly delineated or listed. The term "or" refers to the listed members individually as well as in any combination, unless otherwise stated. The use of the singular includes the use of the plural and vice versa.
[0012] An "ethylene-based polymer" is a polymer that contains greater than 50 weight percent (wt%) polymerized ethylene monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" may be used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylenes) include low density polyethylene (LDPE) and linear polyethylene. Non-limiting examples of linear polyethylene include linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), multi-component ethylene-based copolymer (EPE), ethylene / α-olefin multiblock copolymers (also known as olefin block copolymers (OBC)), substantially linear or linear plastomers / elastomers, and high density polyethylene (HDPE). In general, polyethylene can be produced in gas phase fluidized bed reactors, liquid phase slurry process reactors, or liquid phase solution process reactors using heterogeneous catalyst systems such as Ziegler-Natta catalysts, homogeneous catalyst systems including Group 4 transition metals and ligand structures such as metallocene, nonmetallocene metal centers, heteroaryl, heterovalent aryloxy ethers, phosphinimines, and others. A combination of heterogeneous and / or homogeneous catalysts may also be used in either a single reactor or dual reactor configuration.
[0013] "Ethylene plastomer / elastomer" means a polymer that contains units derived from ethylene and at least one C3-C 10It refers to substantially linear or linear ethylene / α-olefin copolymers containing a homogeneous distribution of short chain branches including units derived from α-olefin comonomers. The ethylene plastomers / elastomers have a density of 0.870 g / cc to 0.917 g / cc. Non-limiting examples of ethylene plastomers / elastomers include AFFINITY™ plastomers and elastomers (available from The Dow Chemical Company), EXACT™ plastomers (available from ExxonMobil Chemical), Tafmer™ (available from Mitsui), Nexlene™ (available from SK Chemicals Co.), and Lucene™ (available from LG Chem Ltd.).
[0014] "High density polyethylene" (or "HDPE") means ethylene homopolymer or at least one C4 to C6 10 Ethylene / α-olefin copolymers containing α-olefin comonomers or C4-C8 α-olefin comonomers and having a density of 0.940 g / cc, or 0.945 g / cc, or 0.950 g / cc, or 0.953 g / cc to 0.955 g / cc, or 0.960 g / cc, or 0.965 g / cc, or 0.970 g / cc, or 0.975 g / cc, or 0.980 g / cc. HDPE can refer to unimodal or multimodal copolymers. "Unimodal ethylene copolymer" refers to an ethylene / C4-C8 copolymer having one distinct peak in gel permeation chromatography (GPC) showing molecular weight distribution. 10 A multimodal ethylene copolymer is an α-olefin copolymer that has at least two clear peaks in the GPC molecular weight distribution of ethylene / C4-C 10It refers to α-olefin copolymers. Multimodality includes copolymers with two peaks (bimodal) as well as copolymers with three or more peaks. Non-limiting examples of HDPE include DOW™ high density polyethylene (HDPE) resins (available from Dow Chemical Company), ELITE™ reinforced polyethylene resins (available from Dow Chemical Company), CONTINUUM™ bimodal polyethylene resins (available from Dow Chemical Company), LUPOLEN™ (available from LyondellBasell), and HDPE products from Borealis, Ineos, and ExxonMobil.
[0015] "Low density polyethylene" (or "LDPE") is a polymer consisting of ethylene homopolymer or at least one C 10 It consists of ethylene / α-olefin copolymers with α-olefins, has a density of less than 0.915 g / cc to 0.940 g / cc, and contains long chain branching with a broad MWD. LDPE is typically produced by high pressure free radical polymerization (tubular reactor or autoclave using a free radical initiator). Non-limiting examples of LDPE include MarFlex™ (Chevron Phillips), LUPOLEN™ (LyondellBasell), and LDPE products from Borealis, Ineos, ExxonMobil, etc.
[0016] "Linear low density polyethylene" (or "LLDPE") means a polyethylene having units derived from ethylene and at least one C3-C 10A linear ethylene / α-olefin copolymer containing a homogeneous distribution of short chain branches with units derived from an α-olefin comonomer. LLDPE is characterized by little, if any, long chain branching, in contrast to conventional LDPE. LLDPE has a density of less than 0.910 g / cc to 0.940 g / cc. Non-limiting examples of LLDPE include TUFLIN™ linear low density polyethylene resins (available from The Dow Chemical Company), DOWLEX™ polyethylene resins (available from The Dow Chemical Company), and MARLEX™ polyethylene (available from Chevron Phillips).
[0017] An "olefin-based polymer" or "polyolefin" is a polymer that contains more than 50 weight percent polymerized olefin monomers (based on the total amount of polymerizable monomers) and may optionally include at least one comonomer. Non-limiting examples of olefin-based polymers include ethylene-based polymers and propylene-based polymers.
[0018] A "polymer" is a compound prepared by polymerizing monomers, whether of the same or different types, that provide multiple and / or repeating "units" or "mer units" that, in polymerized form, make up the polymer. Thus, the term polymer in general encompasses the term homopolymer, which is commonly used to refer to a polymer prepared from only one type of monomer, and the term copolymer, which is commonly used to refer to a polymer prepared from at least two types of monomer. It also encompasses all forms of copolymers, e.g., random, block, etc. The terms "ethylene / α-olefin polymer" and "propylene / α-olefin polymer" refer to the above-mentioned copolymers prepared from polymerizing ethylene or propylene, respectively, with one or more additional polymerizable α-olefin monomers. It should be noted that although polymers are often referred to as "made of" one or more particular monomers, "based on" a particular monomer or monomer type, "containing" a particular monomer content, etc., in this context, the term "monomer" is understood to refer to the polymerized residue of a particular monomer, and not to the unpolymerized species. Generally, polymers are referred to herein in terms of "units" that are the polymerized form of the corresponding monomers.
[0019] A "propylene-based polymer" is a polymer that contains more than 50 weight percent polymerized propylene monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Propylene-based polymers include propylene homopolymers and propylene copolymers (meaning units derived from propylene and one or more comonomers). The terms "propylene-based polymer" and "polypropylene" may be used interchangeably. Non-limiting examples of suitable propylene copolymers include propylene impact copolymers and propylene random copolymers.
[0020] "Ultra-low density polyethylene" (or "ULDPE") and "very low density polyethylene" (or "VLDPE") are defined as polyethylene that is made up of units derived from ethylene and at least one C3-C 10 A linear ethylene / α-olefin copolymer containing a homogeneous distribution of short chain branches including units derived from an α-olefin comonomer. ULDPE and VLDPE each have a density of 0.885 g / cc to 0.915 g / cc. Non-limiting examples of ULDPE and VLDPE include ATTANE™ ultra-low density polyethylene resins (available from The Dow Chemical Company) and FLEXOMER™ very low density polyethylene resins (available from The Dow Chemical Company).
[0021] Test Method Acid value (or acid number) is measured according to ASTM D 1386 / 7. Acid number is a measure of the amount of carboxylic acid present in the final composition. Acid number is the number of milligrams of potassium hydroxide required to neutralize the free carboxylic acid present in one gram of material (e.g., dispersant). The unit of acid number is mg KOH / g.
[0022] Average particle size refers to the volume average particle size as measured using a Malvern Zetasize NanoZS light scattering particle sizer, and results are reported in micrometers (or microns).
[0023] Density is measured according to ASTM D792, Method B. Results are recorded in grams per cubic centimeter (g / cc).
[0024] Differential Scanning Calorimetry (DSC) Differential scanning calorimetry (DSC) may be used to measure the melting, crystallization, and glass transition behavior of polymers over a wide range of temperatures. For example, a TA Instruments Q1000 DSC equipped with an RCS (refrigerated cooling system) and an autosampler is used to perform this analysis. A nitrogen purge gas flow rate of 50 ml / min is used during testing. Each sample is melt pressed into a thin film at approximately 175°C, and the molten sample is then air cooled to room temperature (approximately 25°C). A 3-10 mg, 6 mm diameter specimen is extracted from the cooled polymer, weighed, placed in a light aluminum pan (approximately 50 mg), and crimped shut. Analysis is then performed to determine its thermal properties.
[0025] The thermal behavior of the sample is determined by ramping the sample temperature to generate a heat flow vs. temperature profile. First, the sample is rapidly heated to 180°C and held isothermal for 3 minutes to remove its thermal history. Next, the sample is cooled to -40°C at a cooling rate of 10°C / min and held isothermal at -40°C for 3 minutes. The sample is then heated to 180°C at a heating rate of 10°C / min (this is the "second heat" ramp). A cooling curve and a second heating curve are recorded. The cooling curve is analyzed by setting a baseline endpoint from the onset of crystallization to -20°C. The heating curve is analyzed by setting a baseline endpoint from -20°C to the end of melting. The values determined are the extrapolated melting onset, Tm, and the extrapolated crystallization onset, Tc. The heat of fusion (in Joules per gram) (H f ), and the percent crystallinity of the polyethylene sample calculated using the following equation: percent crystallinity = ((H f ) / 292J / g)×100
[0026] Heat of fusion (H f ) (also known as the enthalpy of fusion) and peak melting temperature are reported from the second heating curve.
[0027] The melting point, Tm, is determined from the DSC heating curve by first drawing a baseline between the onset and end of the melting transition. A tangent line is then drawn to the data on the low temperature side of the melting peak. Where this line intersects the baseline is the extrapolated onset of melting (Tm), as described by Bernhard Wunderlich, The Basis of Thermal Analysis, in Thermal Characterization of Polymeric Materials 92, 277-278 (Edith A. Turi ed., 2d ed. 1997).
[0028] The glass transition temperature, Tg, is determined from the DSC heating curve where half of the sample acquires the heat capacity of a liquid, as described by Bernhard Wunderlich, The Basis of Thermal Analysis, in Thermal Characterization of Polymeric Materials 92, 278-279 (Edith A. Turi ed., 2d ed. 1997). Baselines are drawn below and above the glass transition region and extrapolated through the Tg region. The temperature at which the heat capacity of the sample is halfway between these baselines is the Tg.
[0029] The drop point is measured according to ASTM D3954.
[0030] Gas Permeability. The gas permeability of the separator is measured using a test using a Genuine Gurley™ 4110 automated densometer according to ASTM D-726-58. The coated separator samples were placed in an oven for 30 seconds at different temperatures ranging from room temperature to 120°C. The coated separator samples were removed from the oven and cooled to room temperature. The gas permeability was measured to determine if the porous coating layer had melted. If the porous coating layer had not melted, the gas permeability did not change. If the porous coating layer had melted, the gas permeability changed. The coated separator sample was placed in a tube tester head with an area of 1 square inch. 100 ml of air was passed from one side of the coated separator at 36.26 psi to the other side at 7.25 psi. The time (in seconds) of gas transport for every 100 ml was recorded to evaluate the separator permeability. A higher gas permeability value indicates a longer time for gas transmission / penetration. A lower gas permeability value indicates a shorter time for gas transmission / penetration, which indicates that the pores on the coated separator are blocked.
[0031] Measure the melt index (MI) (I2) in g / 10 min using ASTM D1238 (190° C. / 2.16 kg).
[0032] ASTM D1238 (230° C. / 2.16 kg) is used to measure the melt flow rate (MFR) in g / 10 min.
[0033] Melt viscosity is measured at 177°C using a Brookfield Viscometer model and a Brookfield RV-DV-II-Pro Viscometer spindle 31. The sample is poured into the chamber, which is then inserted into the Brookfield Thermosel and secured in place. The sample chamber has a notch on the bottom that fits into the bottom of the Brookfield Thermosel to ensure that the chamber does not rotate when the spindle is inserted and rotated. The sample (approximately 8-10 grams of resin) is heated to the required temperature until the molten sample is approximately 1 inch below the top of the sample chamber. The viscometer apparatus is lowered, submerging the spindle into the sample chamber. The lowering continues until the viscometer bracket lines up on the Thermosel. The viscometer is turned on and set to operate at a shear rate that results in a torque reading within 40-60 percent of the total torque capacity, based on the rpm output of the viscometer. Readings are taken every minute for 15 minutes or until the value stabilizes, at which point the final reading is recorded.
[0034] Porosity is measured according to ASTM D6583. Detailed Description
[0035] The present disclosure relates to an electrochemical cell. In one embodiment, the electrochemical cell includes a separator. The separator is disposed between an optional anode and an optional cathode. The separator includes (A) a porous substrate and (B) a porous coating layer on the porous substrate. The porous substrate (A) is comprised of an olefin-based polymer having a melting point Tm of greater than 130° C. The porous coating layer (B) has a melting temperature of 80° C. to 110° C., and the porous coating layer is comprised of a plurality of particulates and an optional binder. The particulates have an average particle size of 0.3 micrometers to 1.5 micrometers. The particulates are comprised of (i) an ethylene-based polymer, (ii) a dispersant, and (iii) an optional acid-functional wax. The ethylene-based polymer has (a) a density of 0.90 g / cc to less than 0.94 g / cc, (b) a Tm of 90° C. to 120° C., and (c) a melt index of 30 g / 10 min to 600 g / 10 min. The dispersant is C 14 ~C 40 It is composed of aliphatic fatty acids.
[0036] A. Porous base material The separator includes (A) a porous substrate (interchangeably referred to as a "blank separator"). The porous substrate is composed of an olefin-based polymer having a melting point Tm of greater than 130°C, or greater than 130°C to 160°C. The olefin-based polymer has voids or pores that define a porosity that allows ionic species, such as, for example, lithium ions, to diffuse, permeate, or otherwise transpire through the porous substrate. The pore size of the olefin-based polymer is 1 to 100 micrometers, or 1 micrometer to 50 micrometers, or 1 micrometer to 25 micrometers, or 1 micrometer to 10 micrometers. The olefin-based polymer has a porosity of 30%, or 40% to 50%, or 60%. The porous substrate has a thickness of 0.1 mil, or 0.2 mil, 0.5 mil, or 1.0 mil, or 1.5 mil to 2.0 mil, or 2.5 mil, or 3.0 mil. The porous substrate allows ion transport therethrough. Non-limiting examples of suitable olefin-based polymers include propylene-based polymers having a Tm greater than 130°C and HDPEs having a Tm greater than 130°C.
[0037] Non-limiting examples of commercially available microporous films suitable for use in the present invention include, for example, 1 mil thick CELGARD® 2325 polyethylene film having about 41% void volume, 1 mil thick CELGARD® 2400 polyethylene film having about 35% void volume, and 1 mil thick CELGARD® 2500 polyethylene film having about 45% void volume, each available from Celanese Corporation. Other commercially available porous materials that may be utilized in accordance with the present invention include HIPORE™ polyolefin flat film membranes available from Asahi Kasei Corporation (Tokyo, Japan), such as HIPORE™ 720 microporous high density polyethylene, 1 mil thick, having a void volume of about 37%, HIPORE™ 8416 microporous high density polyethylene, 0.64 mil thick, having a void volume of about 41%, HIPORE™ 9420 microporous high density polyethylene, 1 mil thick, having a void volume of about 41%, and HIPORE™ 6022 microporous high density polyethylene, 1 mil thick, having a void volume of about 50%.
[0038] B. Porous coating layer The separator comprises a porous coating layer (B). The porous coating layer is in direct contact with the porous substrate. The term "in direct contact" as used herein refers to a layer configuration in which a first layer is located immediately adjacent to a second layer, with no intervening layer or structure between the first and second layers. The porous substrate has opposing surface layers. The porous coating layer is in direct contact with one or both surface layers of the porous substrate. In one embodiment, the porous coating layer is in direct contact with and coextensive with one (or both) surface layers of the porous substrate.
[0039] The porous coating layer is comprised of a plurality of particulates and an optional binder. The particulates are comprised of an ethylene-based polymer, (ii) a dispersant, and (iii) an optional acid-functional wax. The porous coating layer is coextensive or substantially coextensive with the surface layer of the porous separator. However, the particulates do not coalesce to form a continuous film, thereby imparting porosity to the coating layer. Micropores exist in the porous coating layer due to the non-coalescing of the particulates. The non-coalescing particulates that cause porosity in the coating layer allow ionic species, such as, for example, lithium ions, to diffuse, permeate, or otherwise transpire through the porous coating layer.
[0040] When the porous coating layer is exposed to a temperature of 80°C or greater than 80°C or between 80°C and 110°C (e.g., as a result of thermal runaway in an electrochemical cell), the ethylene-based polymer particulates begin to soften and / or melt or otherwise coalesce. Upon softening, melting, and particulate coalescence, the particulates form a continuous or substantially continuous, coextensive coating on the porous substrate. Thus, upon melting and / or particulate coalescence, the porous coating layer transforms from a porous layer to a non-porous coating layer. In this manner, the porous coating layer has a melting temperature between 80°C and 110°C. It is understood that the DSC melting temperature Tm is different from the melting temperature of the porous coating layer. The porous coating layer has a thickness that, upon melting and / or particulate coalescence, effectively renders the porous coating layer substantially ion-impermeable, thereby providing a sufficient amount of particulate / polymeric material to prevent or inhibit any further electrochemical reaction. In this manner, the conversion of the porous coating layer to a non-porous and continuous coating layer ceases or otherwise prevents thermal runaway in the electrochemical cell.
[0041] In one embodiment, the porous coating layer has a thickness of from 1 micrometer to 10 micrometers, or from 1 micrometer to 5 micrometers.
[0042] In one embodiment, the porous coating layer has a thickness of from 1 mil to 10 mils, from 1 mil to 5 mils.
[0043] i. Fine particles The porous coating layer is composed of particulates. The particulates are composed of (i) an ethylene-based polymer, (ii) a dispersant, and (iii) optionally an acid-functional wax. The ethylene-based polymer is an ethylene homopolymer or an ethylene / α-olefin copolymer having a density of 0.90 g / cc to less than 0.94 g / cc and a melt index (MI) of 30 g / 10 min to 600 g / 10 min. Non-limiting examples of suitable ethylene-based polymers include LDPE, LLDPE, ULDPE, VLDPE, EPE, substantially linear or linear plastomers / elastomers, and combinations thereof.
[0044] In one embodiment, the microparticles are comprised of an ethylene-based polymer that is a LDPE homopolymer. The LDPE propylene homopolymer has the following characteristics: (i) a density between 0.910 g / cc and 0.930 g / cc, or between 0.915 g / cc and 0.925 g / cc; and / or (ii) an MI of 40 g / 10 min to 70 g / 10 min, or 50 g / 10 min to 60, and / or (iii) having one, some, or all of a Tm of 105°C to 115°C, or 107°C to 113°C; Microparticles composed of LDPE homopolymer (and dispersant, and optional acid functional wax) have the following characteristics: (iv) a density between 0.910 g / cc and 0.930 g / cc, or between 0.915 g / cc and 0.925 g / cc; and / or (v) an MI of 40 g / 10 min to 70 g / 10 min, or 50 g / 10 min to 60, and / or (vi) a melting temperature of 80°C to 110°C, or 90°C to 110°C, and / or (vii) having one, some, or all of the following average particle sizes: 0.3 to 1.5 micrometers, or 0.5 to 1.4 micrometers.
[0045] In one embodiment, the ethylene-based polymer is an ethylene / α-olefin copolymer that is an ethylene / C3-C8 α-olefin comonomer. The ethylene / C3-C8 α-olefin comonomer is an ethylene / C3-C8 α-olefin copolymer that is composed or otherwise consists of ethylene in polymerized form and one copolymerizable C3-C8 α-olefin comonomer. The C3-C8 α-olefin is selected from propylene, butene, hexene, and octene.
[0046] In one embodiment, the ethylene / α-olefin copolymer is an ethylene / propylene copolymer.
[0047] In one embodiment, the ethylene / α-olefin copolymer is an ethylene / C4-C8 α-olefin copolymer. The ethylene / C4-C8 α-olefin comonomer is an ethylene / C4-C8 α-olefin copolymer consisting or otherwise consisting of ethylene in polymerized form and one copolymerizable C4-C8 α-olefin comonomer. The C4-C8 α-olefin comonomer is selected from butene, hexene, and octene. The ethylene / C4-C8 α-olefin comonomer is an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / octene copolymer.
[0048] In one embodiment, the microparticles are composed of an ethylene / α-olefin copolymer, which is an ethylene / C4-C8 α-olefin copolymer.
[0049] In one embodiment, the microparticles are comprised of an ethylene-based polymer that is an ethylene / C4-C8 α-olefin copolymer (and a dispersant, and optionally an acid-functional wax). The ethylene / C4-C8 α-olefin copolymer has the following characteristics: (i) a density between 0.900 g / cc and 0.935 g / cc, or between 0.900 g / cc and 0.910 g / cc, or between 0.925 g / cc and 0.935 g / cc; and / or (ii) an MI of 30 g / 10 min to 600 g / 10 min, or 30 g / 10 min to 40 g / 10 min, or 400 g / 10 min to 600 g / 10 min, and / or (iii) having one, some, or all of a Tm of 90°C to 120°C, or 93°C to 98°C, or 113°C to 118°C; Microparticles composed of ethylene / C4-C8 α-olefin copolymers have the following characteristics: (iv) a density between 0.900 g / cc and 0.935 g / cc, or between 0.900 g / cc and 0.910 g / cc, or between 0.925 g / cc and 0.935 g / cc; and / or (v) an MI of 30 g / 10 min to 600 g / 10 min, or 30 g / 10 min to 40 g / 10 min, or 400 g / 10 min to 600 g / 10 min, and / or (vi) a melting temperature of 80°C to 110°C, or 90°C to 110°C, and / or (vii) having one, some, or all of the following average particle sizes: 0.3 to 1.5 micrometers, or 0.5 to 1.4 micrometers.
[0050] The microparticles also include (ii) a dispersant, and (iii) an optional acid-functionalized wax. The microparticles are formed by a stable aqueous formulation. The stable aqueous formulation is composed of the microparticles (ethylene-based polymer, dispersant, optional acid-functional wax), and (iv) an optional binder (including rheology modifiers and wetting agents), and water, and is applied to a porous substrate. Once applied to the porous substrate, the stable aqueous formulation is dried to form a porous coating layer. As used herein, a "stable aqueous formulation" is an emulsion in which solid particles are uniformly suspended in a continuous water phase. The solid particles of the formulation have a solid content. The "solid content" is the combined weight of (i) the microparticles and the optional binder.
[0051] In one embodiment, the stable aqueous formulation applied to the porous substrate contains, based on the total weight of solids, (i) 50%, or 60%, or 70% to 90%, or 95% by weight of particulates; (ii) 1%, or 2%, or 5% to 15%, or 20%, or 40% by weight of dispersant; (iii) 0%, or 1%, or 5% to 15%, or 20% by weight of acid functionalized wax; and (iv) 0%, or 0.05% to 2%, or 5% by weight of binder.
[0052] Dispersants provide colloidal stability of solids in stable aqueous formulations. Dispersants are long chain fatty acids having 14-40 carbon atoms or 16-36 carbon atoms. Non-limiting examples of long chain fatty acids suitable for dispersants include Unicid™ 350 dispersant behenyl (C 22 ) acids.
[0053] The microparticles optionally include an acid-functionalized wax. When an acid-functionalized wax is present in the microparticles, non-limiting examples of suitable acid-functionalized waxes include acid-functionalized modified polyolefin waxes, maleic anhydride polyolefin copolymers, waxes, and maleic anhydride modified polyethylene waxes. It is understood that the ethylene-based polymers from which the microparticles are made are not waxes, nor are they acid-functionalized waxes.
[0054] In one embodiment, the acid functionalized wax is present in the microparticles, and the acid functionalized wax is a maleic anhydride modified polyethylene wax.
[0055] The porous coating layer optionally includes a binder, which provides adhesion between the particulates and the surface of the porous separator. If a binder is present in the porous coating layer (and the binder is present in the stable aqueous formulation), non-limiting examples of suitable binders include, for example, styrene / butene rubber (SBR) latex and acrylic emulsions, such as, for example, butyl acrylate emulsion.
[0056] In one embodiment, a binder is present in the porous coating layer, the binder being a styrene / butene rubber. The binder also includes a wetting agent and a rheology control agent.
[0057] C. Electrochemical Cell The electrochemical cell includes a separator disposed between an optional anode and an optional cathode, the separator being composed of a porous substrate (as disclosed above) and a porous coating layer on the porous substrate (as disclosed above).
[0058] 1 shows an electrochemical cell 10 having a separator 12, an anode 14 present, and a cathode 16 present. Separator 12 is disposed or otherwise extends between anode 14 and cathode 16. Separator 12 includes a porous substrate 18 and a porous coating layer 20. Porous substrate 18 can be any porous substrate as disclosed above, where porous substrate 18 is comprised of an olefin-based polymer, where the olefin-based polymer has a Tm greater than 130° C.
[0059] Separator 12 also includes a porous coating layer 20. As shown in FIG. 1, porous coating layer 20 is coextensive with and in direct contact with the surface of porous substrate 18. Porous coating layer 20 is composed of (i) a plurality of particulates (ethylene-based polymer, dispersant, optional acid-functional wax as previously disclosed herein), and (iv) optional binder (as previously disclosed herein), hereinafter referred to as "porous coating material." The porous coating material assumes the size and shape of the particulates (and the shape of the binder, if present). The particulates and binder can be any particulates and binder as previously disclosed herein. The microparticles are comprised of an ethylene-based polymer, as previously disclosed herein, having (i) a density of from 0.90 g / cc to less than 0.94 g / cc, (ii) a Tm of from 90° C. to 120° C., (iii) a melt index of from 30 g / 10 min to 600 g / 10 min, and (iv) an average particle size of from 0.5 micrometers to 1.5 micrometers.
[0060] The porous coating material 22 forms a discontinuous layer on the porous substrate 18, causing the "porosity" of the porous coating layer 20, as shown in Figure 1. The electrochemical cell 10 includes an electrolyte, which allows for ion flow or otherwise transport from the cathode 16, through the separator 12 to the anode 14, as shown by flow arrow A in Figure 1.
[0061] Other non-limiting components (not shown) of the electrochemical cell 10 include the negative terminal and the positive terminal of the charge / discharge electrochemical cell 10 .
[0062] Arrow B in Figure 1 indicates the onset of a rapid temperature increase or "thermal runaway" in electrochemical cell 10. The rapid increase in temperature can be the result of an internal short circuit, an external short circuit, overcharging the electrochemical cell, excessive current when charging or discharging the electrochemical cell, material defects within the electrochemical cell, and any combination thereof. In the case of thermal runaway, the temperature can rapidly increase from ambient to 80°C or above 80°C within milliseconds.
[0063] At the onset of thermal runaway, if the temperature rise reaches or exceeds 80° C., the porous coating material 22 will coalesce or otherwise melt to form a continuous layer 24 of coating material along a portion of the porous substrate 18, as shown in FIG. 2. If the separator 18 is exposed to a temperature of 80° C. or higher, the porous coating layer 22 will coalesce to form a non-porous coating layer 24 on the porous substrate. Without being bound to a particular theory, it is believed that the ethylene-based polymer in the microparticles of the porous coating layer begins to soften and melt at temperatures between 80° C. and 110° C., or between 81° C. and 110° C., or between 90° C. and 110° C., or between 90° C. and 100° C. In this temperature range, the softening and melting ethylene-based polymer microparticles will coalesce to block flow through the porous substrate, even if the ethylene-based polymer in the microparticles may not completely melt. In other words, the ethylene-based polymer will begin to soften and melt, and the microparticles will coalesce before the temperature of the separator (and / or the temperature of the porous coating layer) reaches the Tm of the ethylene-based polymer.
[0064] The continuous layer 24 is non-porous. The continuous layer 24 also fills or otherwise occludes the pores in the porous substrate 18. Although Figure 2 shows portions of the porous coating layer 20 as coalescing (as a non-porous, continuous layer 24), it is understood that in the event of severe thermal runaway, the entire porous layer 20 may coalesce into a continuous, non-porous layer that is coextensive or substantially coextensive with the surface of the porous substrate 18.
[0065] The formation of a continuous layer 24 (composed of porous coating material 22) blocks ion transport, thereby abruptly halting thermal runaway as indicated by the labeled "X" in Figure 2. In this manner, the present separator 12 is a thermal shutdown safety device for the electrochemical cell 10.
[0066] In one embodiment, electrochemical cell 10 is a lithium ion battery.
[0067] By way of example, and not by way of limitation, certain embodiments of the present disclosure will now be described in detail in the following examples. EXAMPLES
[0068] The materials used in the examples are provided in Table 1 below.
[0069] [Table 1]
[0070] 1. Dispersion Preparation Process Aqueous dispersion samples were prepared using Dow Inc.'s mechanical dispersion technology. The ethylene-based polymer resin and dispersant were loaded into a specially designed twin-screw extruder (TSE) at a back pressure of about 2 MPa. The ethylene-based polymer resin, dispersant, and acid-functional wax (if present) were melted and blended, followed by injection of KOH solution and a small amount of initial water into the TSE at a temperature of 150°C and a screw rotation of 600 rpm. During this process, a high internal phase emulsion (HIPE) was formed, which was then diluted to 40-60 wt% before the back pressure valve. After the emulsion was cooled to below 100°C, the output was transferred to a vessel for collecting the dispersion of fine particles composed of the ethylene-based polymer resin. The process conditions and ingredients are shown in Table 2 below.
[0071] 2. Preparation of Porous Coating Layer The stable aqueous dispersion of the particulates was then compounded with an SBR binder and other additives to form a liquid coating material. The liquid coating material was applied onto an HDPE porous substrate ("HDPE blank separator") using an automatic film applicator, TQC-020 (Sheen Company), equipped with an HKC-1 rod bar. The coated HDPE porous substrate was transferred to a 60°C oven and allowed to dry for 5 minutes.
[0072] Each dispersion coating formulation (DCF), IE1 to IE5, is 10 to 15 g / m 2 rod bar was used to coat onto each individual and separate porous substrate (blank separator) and dried to form a separator comprised of (i) a porous substrate and (ii) a porous coating layer (porous coating layer having a thickness of 1 mm).
[0073] Each separator (composed of (i) a porous substrate and (ii) a porous coating layer) was characterized by SEM. Figure 3 shows surface SEM images of the porous coating layers: 3(a) IE1 959S-Unicid particulate, 3(b) IE2 8420-Behenic acid particulate, and 3(c) IE3 8402-Unicid particulate.
[0074] Table 2 (below) provides the average particle size of the microparticles in each of IE1-IE5. As shown by the SEM in Figure 3(a), Figure 3(b), and Figure 3(c), each porous coating layer is composed of microparticles (of the porous coating material) having a spherical shape, and the IE1 959S-Unicid microparticles are larger than those of IE2 and IE3. The microparticle material of IE1-IE5 includes SBR latex, a binder for binding to the HDPE separator, a wetting agent for applying a uniform coating on the porous substrate, and a rheology modifier for stabilizing the formulation in dispersion. To print a thin porous coating layer on the porous substrate, the liquid coating contains 16.6 wt% solids based on the total weight of the liquid coating material. The solids of the liquid coating material include an ethylene-based polymer, a dispersant, a binder, a wetting agent, a rheology modifier, and water.
[0075] [Table 2] * Weight percent based on total weight of dispersion
[0076] 3. Solvent resistance test For lithium-ion battery applications, the separator (composed of (i) porous substrate and (ii) porous coating layer) needs to be stable in the electrolyte, otherwise the battery performance will be deteriorated. The electrolyte solvent resistance was evaluated for IE1-IE5. Each DCF of IE1-IE5 was cast into a Petri dish, dried at room temperature, and then dried at a temperature of 90°C to form a dry solid film of the porous coating layer (without the porous substrate) having a thickness of 1 mm. Each film was cut into a dumbbell shape and immersed in a glass vial containing a mixture of electrolyte solvents of ethylene carbonate, propylene carbonate, and ethyl methyl carbonate in a weight ratio of 1:1:1. The glass vial was heated in an oven at 50°C for 2 days, and then the film of the porous coating layer sample was taken out and wiped to obtain the weight. The weight change results of the IE1-IE5 films are listed in Table 3 below. The porous coating layer sample films were made from ethylene-based polymers and SBR that have already been proven to be stable in electrolytes, and each of the IE1-IE5 samples absorbed less than 1 wt.% of the electrolyte solvent, demonstrating that the porous coating layer materials were resistant to the electrolyte solvent.
[0077] [Table 3]
[0078] 4. Thermal response characteristics The DCF for each of IE1 to IE5 is 10 to 15 g / m 2 The separator blanks were then coated on separate and individual HDPE separator blanks using a rod bar. The coated separator blanks were placed in an oven and dried at 60°C for 5 minutes to form separators IE1-IE5 comprised of (i) a porous HDPE substrate and (ii) a porous coating layer containing particulate material IE1-IE5 (hereinafter "separators IE1-IE5"). Each separator IE1-IE5 was heated at different temperatures to evaluate the gas permeation performance of the porous coating layer and the effect of pore closure. The longer the time of gas transport across the separator, the lower the gas permeability of the separator.
[0079] FIG. 4 shows the gas permeability of separators IE1 to IE5 at different temperatures.
[0080] The gas permeability of the coated separators IE1-IE5 was evaluated at temperatures ranging from room temperature to 120°C according to the Gas Permeability Test disclosed above. The baseline HDPE separator blank exhibited gas permeability that did not change significantly as the temperature was increased from room temperature to 120°C. After testing the coated separator samples at different temperatures, gas permeability vs. temperature was plotted to identify the thermally responsive temperature.
[0081] The gas permeability of separator IE1 (particulate material containing 959S-Unicid) drops sharply at about 110°C, indicating that IE1 melts and / or softens at 110°C.
[0082] The gas permeability of separator IE2 drops sharply between 90°C and 100°C, indicating that IE2 melts and / or softens at 90°C or between 90°C and 100°C.
[0083] The gas permeability of IE3 drops sharply at 80°C to 90°C, indicating that IE3 melts and / or softens at 80°C, or at 80°C to 90°C.
[0084] The gas permeability of the separators IE4 to IE5 drops sharply at temperatures between 100°C and 110°C, indicating that IE4 to IE5 melt and / or soften at 100°C, or between 100°C and 110°C.
[0085] These gas permeability results demonstrate that the porous coating layer materials IE1-5 melt and seal the pores of the porous substrate at temperatures between 80°C and 110°C, or between 81°C and 110°C, and particularly at temperatures between 90°C and 110°C, or between 90°C and 100°C. The gas permeability tests demonstrate the effect of pore closure of a porous coating layer constructed from any of the porous coating materials IE1-5. Without being bound to a particular theory, it is believed that the ethylene-based polymer in the microparticles of the porous coating layer begins to soften and melt at temperatures between 80°C and 110°C, or between 81°C and 110°C, or between 90°C and 110°C, and in this temperature range, the softening and melting ethylene-based polymer microparticles coalesce to block flow through the porous substrate, even if the ethylene-based polymer in the microparticles may not completely melt. The gas permeability results demonstrate that a porous coating layer constructed from any of IE1-5 functions as an effective shutdown separator to prevent thermal runaway in an electrochemical cell.
[0086] The present disclosure is not limited to the embodiments and examples contained herein, but is specifically intended to include portions of the embodiments and modified forms of those embodiments, including combinations of elements of different embodiments, within the scope of the following claims. (Aspect) (Aspect 1) 1. An electrochemical cell including a separator disposed between an optional anode and an optional cathode, The separator is (A) a porous substrate composed of an olefin-based polymer having a melting point Tm exceeding 130°C; (B) a porous coating layer on the substrate, the porous coating layer having a melting temperature of 80° C. to 110° C. and comprising a plurality of microparticles and an optional binder, the microparticles having an average particle size of 0.3 micrometers to 1.5 micrometers, the microparticles comprising: (i) An ethylene-based polymer, (a) a density of less than 0.90 g / cc to 0.94 g / cc; (b) Tm of 90°C to 120°C; (c) an ethylene-based polymer having a melt index of 30 g / 10 min to 600 g / 10 min; (ii) a dispersant composed of a C14 to C40 aliphatic fatty acid, and (iii) An electrochemical cell comprising an optional acid-functional wax. (Aspect 2) 2. The electrochemical cell of embodiment 1, wherein the porous substrate is constructed from high density polyethylene. (Aspect 3) The plurality of particles are (a) Density of 0.910g / cc to 0.930g / cc; (b) Tm of 105°C to 115°C; (c) a low-density polyethylene having a melt index of 40 g / 10 min to 70 g / 10 min; (d) The electrochemical cell according to aspect 1 or 2, wherein the fine particles have an average particle size of 0.5 micrometers to 1.4 micrometers. (Aspect 4) The plurality of particles are (a) a density of less than 0.900 g / cc to 0.935 g / cc; (b) a melt index of 30 g / 10 min to 600 g / 10 min; (c) an ethylene / C4-C8 α-olefin copolymer having a Tm of 90°C to 120°C; (d) The electrochemical cell according to aspect 1 or 2, wherein the fine particles have an average particle size of 0.5 micrometers to 1.4 micrometers. (Aspect 5) 5. The electrochemical cell of any one of the preceding claims, wherein the particulate comprises the ethylene-based polymer, the dispersant, and the acid-functional wax. (Aspect 6) 6. The electrochemical cell of embodiment 5, wherein the acid functional wax is a maleic anhydride modified polyethylene wax. (Aspect 7) 7. The electrochemical cell of embodiment 6, wherein the porous coating layer comprises the binder. (Aspect 8) 8. The electrochemical cell of embodiment 7, wherein the binder is a styrene / butene rubber. (Aspect 9) The electrochemical cell of any one of the preceding claims, wherein the porous coating layer has a thickness of from 1 mil to 10 mils. (Aspect 10)
[0023] Exemplary embodiments 1-9 include an electrochemical cell, wherein at least one of the optional anode and the optional cathode is present within the electrochemical cell. (Aspect 11) 11. The electrochemical cell of any one of the preceding aspects, wherein when the separator is exposed to a temperature of 80° C. or greater, the porous coating layer coalesces to form a non-porous coating layer on the porous substrate.
Claims
1. 1. An electrochemical cell including a separator, The separator is (A) a porous substrate composed of an olefin-based polymer having a melting point Tm exceeding 130 ° C; (B) a porous coating layer on the substrate, the porous coating layer having a melting temperature of 80° C. to 110° C. and comprising a plurality of microparticles, the microparticles having an average particle size of 0.3 micrometers to 1.5 micrometers, the microparticles comprising: (i) An ethylene-based polymer, (a) a density of 0.910 g / cc to 0.930 g / cc; (b) a Tm between 105°C and 115°C; (c) a melt index of 40 g / 10 min to 70 g / 10 min; or (a) a density of from 0.900 g / cc to less than 0.935 g / cc; (b) a melt index of 30 g / 10 min to 600 g / 10 min; (c) an ethylene / C4-C8 α-olefin copolymer having a Tm of 90° C. to 120° C.; Ethylene-based polymers, and (ii) an electrochemical cell comprising a dispersant comprised of a C14 to C40 aliphatic fatty acid;
2. 10. The electrochemical cell of claim 1 , wherein the porous substrate is constructed from high density polyethylene.
3. An electrochemical cell as described in claim 1 or 2, wherein the microparticles further comprise (iii) an acid-functional wax.
4. 4. The electrochemical cell of claim 3, wherein said particulate comprises said ethylene-based polymer, said dispersant, and said acid-functional wax.
5. 5. The electrochemical cell of claim 4 wherein the acid functional wax is a maleic anhydride modified polyethylene wax.
6. 6. The electrochemical cell of claim 5, wherein the porous coating layer further comprises a binder.
7. 7. The electrochemical cell of claim 6, wherein the binder is a styrene / butene rubber.
8. 8. The electrochemical cell of claim 1, wherein the porous coating layer has a thickness of from 25.4 μm (1 mil) to 254 μm (10 mils).
9. An electrochemical cell as claimed in any one of claims 1 to 8, wherein the separator is disposed between the anode and the cathode.
10. 10. The electrochemical cell of any one of claims 1 to 9, wherein the porous coating layer coalesces to form a non-porous coating layer on the porous substrate when the separator is exposed to a temperature of 80°C to 110°C.
Citation Information
Patent Citations
Alkaline dry battery
JP1999086881A
Separator for battery
JP2000208122A
Secondary battery separator, secondary battery laminate and wound body including the same, and non-aqueous secondary battery
JP2019192340A
Porous separator and preparation method thereof
KR1020160011531A
Layered polyolefin microporous membrane, separator for batteries, and methods for manufacturing same
WO2017061489A1