Conductive adhesive sheet
A conductive adhesive sheet with scaly and differently shaped fillers ensures high adhesive strength and conductivity, addressing the issues of peeling and reduced adhesion in existing technologies.
Patent Information
- Application Number
- JP2019223696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-11
AI Technical Summary
Conductive adhesive sheets used in electronic devices face issues of decreased conductivity and adhesive strength over time due to the peeling of metal fillers and the need for increased filler content, which compromises adhesion.
A conductive adhesive sheet with an adhesive layer containing a first scaly conductive filler and a second conductive filler of different shape, such as spherical or filamentary particles, maintains high adhesive strength and conductivity by minimizing filler exposure and maximizing contact points.
The sheet maintains excellent conductivity and adhesive strength both initially and over time, suitable for electromagnetic shielding and grounding in electronic equipment.
Smart Images

Figure 0007574534000004 
Figure 0007574534000005 
Figure 0007574534000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive adhesive sheet. [Background technology]
[0002] Due to their ease of handling, conductive adhesive sheets are used for shielding unwanted leakage electromagnetic waves radiated from electrical or electronic devices, shielding harmful spatial electromagnetic waves generated by other electrical or electronic devices, and for grounding to prevent static electricity. However, as electrical or electronic devices have become smaller and thinner in recent years, there has been a demand for the conductive adhesive sheets used in these devices to also be made thinner and smaller.
[0003] As the conductive adhesive sheet, for example, an adhesive sheet has been proposed which has an adhesive layer made of a conductive adhesive having metal filler dispersed in an adhesive substance on a conductive base material (see, for example, Patent Document 1). In addition, a conductive adhesive tape has been proposed having an adhesive layer containing large diameter conductive particles consisting of a group of particles with a particle size range of 15 μm or more and 50 μm or less, and small diameter conductive particles consisting of a group of particles with a particle size range of 1 μm or more and 12 μm or less (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-53102 A [Patent Document 2] Patent No. 6106148 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the pressure-sensitive adhesive sheet described in Patent Document 1 has problems in that, because metal filler is added as conductive particles, peeling occurs easily over time, and the electrical conductivity decreases over time due to a decrease in contact points. Furthermore, since the conductive adhesive tape described in Patent Document 2 uses only two types of spherical conductive fillers, it is necessary to increase the amount of conductive filler to achieve a low resistance value, which results in a problem of reduced adhesive strength. An object of the present invention is to provide a conductive pressure-sensitive adhesive sheet that has excellent electrical conductivity both initially and over time while retaining high adhesive strength. [Means for solving the problem]
[0006] The means for solving the above problems are as follows. <1> A conductive adhesive sheet having an adhesive layer, the pressure-sensitive adhesive layer contains a first conductive filler, a second conductive filler, and a pressure-sensitive adhesive; The first conductive filler has a scale-like shape, the first conductive filler and the second conductive filler have different shapes; The conductive adhesive sheet is characterized in that the content of the first conductive filler is 55 parts by mass or less per 100 parts by mass of the solid content of the adhesive. <2> The first conductive filler is at least one of scaly metal particles, graphite, and scaly particles formed by coating a scaly base material with a metal. <1> The conductive adhesive sheet according to claim 1, <3> The second conductive filler is a spherical or filamentary metal particle. <1> from <2> 10. The conductive adhesive sheet according to claim 9, wherein <4> The mass ratio (A / B) of the content A of the first conductive filler in the pressure-sensitive adhesive layer to the content B of the second conductive filler in the pressure-sensitive adhesive layer is 1 / 1 or more and 1 / 5 or less. <1> from <3> 10. The conductive adhesive sheet according to claim 9, wherein <5> The content of the first conductive filler is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of a solid content of the adhesive. <1> from <4> 10. The conductive adhesive sheet according to claim 9, wherein <6> The content of the second conductive filler is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of a solid content of the adhesive. <1> from <5> 10. The conductive adhesive sheet according to claim 9, wherein <7> The pressure-sensitive adhesive is an acrylic pressure-sensitive adhesive containing a (meth)acrylic polymer. <1> from <6> 10. The conductive adhesive sheet according to claim 9, wherein <8> The above-mentioned having a conductive substrate <1> from <7> 10. The conductive adhesive sheet according to claim 9, wherein <9> A copper foil is attached to one side of a conductive adhesive sheet, which is then cut to a size of 15 mm wide x 100 mm wide, and two tin-plated plates are attached to the other adhesive layer of the conductive adhesive sheet so that the adhesion area is 15 mm x 15 mm, respectively. The resistance change rate [(resistance after 168 hours / initial resistance) x 100] calculated from the initial resistance value measured and the resistance value measured after leaving the test piece at 23°C for 168 hours is 250% or less. <1> from <8> 10. The conductive adhesive sheet according to claim 9, wherein <10> The above-mentioned is used for at least one of electromagnetic shielding and earthing inside and outside electric or electronic equipment. <1> from <9> 10. The conductive adhesive sheet according to claim 9, wherein Effect of the Invention
[0007] According to the present invention, it is possible to provide a conductive pressure-sensitive adhesive sheet that has excellent electrical conductivity both initially and over time while retaining high adhesive strength. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the conductive adhesive sheet of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the conductive adhesive sheet of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing another example of the conductive adhesive sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] (Conductive adhesive sheet) The conductive adhesive sheet of the present invention has an adhesive layer, and the adhesive layer contains a first conductive filler, a second conductive filler, and an adhesive. The conductive adhesive sheet preferably has a conductive substrate and a release liner in addition to the adhesive layer, and may have other layers such as an intermediate layer and an undercoat layer as long as the object of the present invention is not impaired.
[0010] The inventors have conducted extensive research into means for suppressing the increase in electrical resistance over time when metal particles are added to an adhesive layer, and as a result have discovered that by combining a scaly first conductive filler and a second conductive filler having a different shape from the first conductive filler in the adhesive layer, the two types of conductive fillers having different shapes work synergistically, such that less conductive filler comes to the surface of the adhesive layer, thereby not compromising the high adhesive strength, and the two types of conductive fillers come into contact in large amounts inside the adhesive layer, suppressing the decrease in contact points over time, thereby obtaining a conductive adhesive sheet with excellent conductivity both initially and over time, which has led to the present invention.
[0011] The "sheet" in the conductive adhesive sheet of the present invention means a form consisting of only an adhesive layer, or a form having at least one adhesive layer on a conductive substrate or a release liner, and includes all product forms such as individual leaves, rolls, thin plates, or strips (tapes). The "conductive adhesive sheet" may also be referred to as a "conductive adhesive tape" or a "conductive adhesive film", but in the following description, it will be referred to as a "conductive adhesive sheet". Note that the surface of the adhesive layer in the conductive adhesive sheet may be referred to as the "adhesive surface".
[0012] The conductive adhesive sheet of the present invention may be a double-sided adhesive type in which both sides of the sheet are adhesive, or a single-sided adhesive type in which only one side of the sheet is adhesive.
[0013] The double-sided adhesive conductive adhesive sheet may be a so-called substrate-less conductive double-sided adhesive sheet that does not have a conductive substrate such as a metal foil, or may be a so-called substrate-attached conductive double-sided adhesive sheet that has the conductive substrate.
[0014] An example of the substrate-less conductive double-sided pressure-sensitive adhesive sheet is a conductive pressure-sensitive adhesive sheet 10 consisting of only a pressure-sensitive adhesive layer 2, as shown in FIG. An example of the substrate-attached conductive double-sided pressure-sensitive adhesive sheet is a conductive pressure-sensitive adhesive sheet 10 in which pressure-sensitive adhesive layers 2 are formed on both sides of a conductive substrate 1, as shown in FIG.
[0015] An example of a single-sided adhesive conductive adhesive sheet is a conductive adhesive sheet 10 in which an adhesive layer 2 is formed on one side of a conductive substrate 1 such as a metal foil, as shown in Fig. 3. In Figs. 1 to 3, a first conductive filler 3 and a second conductive filler 4 contained in the adhesive layer 2 are shown typically. Although not shown, it is preferable that the adhesive layer 2 has a release liner on the surface thereof in Figs. 1 to 3.
[0016] <Adhesive layer> The pressure-sensitive adhesive layer is a layer that provides an adhesive surface of the conductive pressure-sensitive adhesive sheet and has electrical conductivity (electrical conductivity). When the adhesive surface of the pressure-sensitive adhesive layer is attached to an adherend, electrical conduction is ensured between the adherend, such as a conductor, and the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer contains a first conductive filler, a second conductive filler, and a pressure-sensitive adhesive, and may further contain other components as necessary.
[0017] <<Adhesive>> Examples of the adhesive constituting the adhesive layer include (meth)acrylic adhesives, urethane adhesives, polyester adhesives, synthetic rubber adhesives, natural rubber adhesives, silicone adhesives, etc. Among these, (meth)acrylic adhesives are preferred from the viewpoint of high adhesive strength.
[0018] -(Meth)acrylic adhesive- The (meth)acrylic pressure-sensitive adhesive contains a (meth)acrylic polymer, and preferably contains a tackifier resin and a crosslinking agent, and further contains other components as necessary.
[0019] -(Meth)acrylic polymer- Suitable examples of the (meth)acrylic polymer include acrylic copolymers containing, as a main monomer component, a (meth)acrylate monomer having 1 to 14 carbon atoms. Examples of the (meth)acrylate having 1 to 14 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, (meth)acrylates having an alkyl group with 4 to 12 carbon atoms are preferred, and (meth)acrylates having a linear or branched structure with 4 to 9 carbon atoms are more preferred, and n-butyl acrylate and 2-ethylhexyl acrylate are even more preferred because they provide a conductive adhesive sheet with high adhesive strength.
[0020] The content of the (meth)acrylate having 1 to 14 carbon atoms in the (meth)acrylic polymer is preferably 70% by mass or more and 95% by mass or less, and more preferably 80% by mass or more and 95% by mass or less, of the monomer components constituting the (meth)acrylic polymer.
[0021] As the monomers usable in the production of the acrylic polymer, in addition to the above-mentioned ones, highly polar vinyl monomers can be used as necessary. Examples of the highly polar vinyl monomer include (meth)acrylic monomers having a hydroxyl group, (meth)acrylic monomers having a carboxyl group, and (meth)acrylic monomers having an amide group. These may be used alone or in combination of two or more.
[0022] Examples of vinyl monomers having a hydroxyl group include (meth)acrylic monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate.
[0023] Examples of vinyl monomers having a carboxyl group include (meth)acrylic monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, (meth)acrylic acid dimer, crotonic acid, and ethylene oxide-modified succinic acid acrylate. Among these, it is preferable to use acrylic acid.
[0024] Examples of vinyl having an amide group include (meth)acrylic monomers such as N-vinylpyrrolidone, N-vinylcaprolactam, acryloylmorpholine, acrylamide, and N,N-dimethylacrylamide.
[0025] As the highly polar vinyl monomer, in addition to those mentioned above, vinyl acetate, ethylene oxide modified succinic acid acrylate, 2-acrylamido-2-methylpropanesulfonic acid and other sulfonic acid group-containing monomers can be used.
[0026] The highly polar vinyl monomer is preferably used in a range of 1.5% by mass or more and 20% by mass or less, more preferably 1.5% by mass or more and 10% by mass or less, based on the total amount of monomers used in the production of the acrylic polymer, and even more preferably in a range of 2% by mass or more and 8% by mass or less, since this allows the formation of a pressure-sensitive adhesive layer that is well-balanced in terms of cohesive strength, holding power, and adhesiveness.
[0027] Among the highly polar vinyl monomers, the vinyl monomer having a hydroxyl group is preferably used when the adhesive contains an isocyanate-based crosslinking agent.Specific examples of the vinyl monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate. The vinyl monomer having a hydroxyl group is preferably used in an amount of 0.01% by mass or more and 1.0% by mass or less, and more preferably 0.03% by mass or more and 0.3% by mass or less, based on the total amount of monomers used in the production of the acrylic polymer.
[0028] The acrylic polymer can be produced by polymerizing the monomers by a known polymerization method such as a solution polymerization method, a bulk polymerization method, a suspension polymerization method, or an emulsion polymerization method. Among these, the solution polymerization method or the bulk polymerization method is preferable. In the polymerization, a peroxide-based thermal polymerization initiator such as benzoyl peroxide or lauroyl peroxide, an azo thermal polymerization initiator such as azobisisobutylnitrile, an acetophenone-based photopolymerization initiator, a benzoin ether-based photopolymerization initiator, a benzyl ketal-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, or the like can be used, as necessary.
[0029] The (meth)acrylic polymer obtained by the above method preferably has a weight average molecular weight (Mw) of 500,000 or more and 2,500,000 or less, more preferably 700,000 or more and 2,000,000 or less, and even more preferably 900,000 or more and 1,800,000 or less. The weight average molecular weight is a weight average molecular weight measured by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0030] The molecular weight is measured by the GPC method using a GPC apparatus (HLC-8329GPC) manufactured by Tosoh Corporation under the following measurement conditions, and is expressed as a standard polystyrene equivalent value. [Measurement conditions] Sample concentration: 0.5% by mass (tetrahydrofuran solution) Sample injection volume: 100μL Eluent: THF (tetrahydrofuran) ·Flow rate: 1.0mL / min ·Measurement temperature: 40℃ - Main column: TSKgel GMHHR-H(20) x 2 Guard column: TSKgel HXL-H Detector: Differential refractometer Standard polystyrene molecular weight: 10,000 to 20,000,000 (Tosoh Corporation)
[0031] -Tackifying resin- As the (meth)acrylic pressure sensitive adhesive, it is preferable to use one that contains a tackifier resin in order to improve the adhesion to the adherend and the surface adhesive strength. Examples of the tackifier resin that can be used include rosin-based tackifier resins, polymerizable rosin-based tackifier resins, polymerizable rosin ester-based tackifier resins, rosin phenol-based tackifier resins, stabilized rosin ester-based tackifier resins, disproportionated rosin ester-based tackifier resins, hydrogenated rosin ester-based tackifier resins, terpene-based tackifier resins, terpene phenol-based tackifier resins, petroleum resin-based tackifier resins, and (meth)acrylate-based tackifier resins.
[0032] Among these, as the tackifier resin, it is preferable to use disproportionated rosin ester tackifier resins, polymerizable rosin ester tackifier resins, rosin phenol tackifier resins, hydrogenated rosin ester tackifier resins, (meth)acrylate resins, and terpene phenol resins, either alone or in combination of two or more thereof.
[0033] The tackifier resin preferably has a softening point of 30° C. or more and 180° C. or less, and more preferably has a softening point of 70° C. or more and 140° C. or less in order to form a pressure-sensitive adhesive layer with high adhesive performance. When a (meth)acrylate tackifier resin is used, it is preferable to use one having a glass transition temperature of 30° C. or more and 200° C. or less, and more preferably to use one having a glass transition temperature of 50° C. or more and 160° C. or less.
[0034] The tackifier resin is preferably used in a range of 5 parts by mass or more and 65 parts by mass or less relative to 100 parts by mass of the (meth)acrylic polymer, and more preferably in a range of 8 parts by mass or more and 55 parts by mass or less, since this makes it easier to ensure adhesion to the adherend.
[0035] -Crosslinking agent- The (meth)acrylic adhesive preferably contains a crosslinking agent in order to further improve the cohesive strength of the adhesive layer. The crosslinking agent may be an isocyanate crosslinking agent, an epoxy crosslinking agent, a metal chelate crosslinking agent, an aziridine crosslinking agent, etc. Among them, the crosslinking agent is preferably a type of crosslinking agent that is mixed with the acrylic polymer after production to promote a crosslinking reaction, and it is preferable to use an isocyanate crosslinking agent or an epoxy crosslinking agent that is highly reactive with the acrylic polymer.
[0036] Examples of the isocyanate crosslinking agent include tolylene diisocyanate, naphthylene-1,5-diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and trimethylolpropane-modified tolylene diisocyanate. Among these, trifunctional polyisocyanate compounds are preferred. Examples of trifunctional isocyanate compounds include tolylene diisocyanate or its trimethylolpropane adduct, and triphenylmethane isocyanate.
[0037] As an index of the degree of crosslinking, the gel fraction value obtained by measuring the insoluble portion after immersing the pressure-sensitive adhesive layer in toluene for 24 hours is used. The gel fraction of the pressure-sensitive adhesive layer is preferably 10% by mass or more and 70% by mass or less, more preferably 25% by mass or more and 65% by mass or less, even more preferably 35% by mass or more and 60% by mass or less, and particularly preferably 40% by mass or more and 55% by mass or less.
[0038] The gel fraction refers to a value measured by the following method. The adhesive is applied to a release liner so that the thickness after drying is 50 μm, dried at 100 ° C for 3 minutes, and aged at 40 ° C for 2 days, and cut into a 50 mm square to be used as a sample. Next, the mass (G1) of the above sample before immersion in toluene is measured in advance, and the toluene-insoluble portion of the sample after immersion in a toluene solution at 23 ° C for 24 hours is separated by filtering with a 300 mesh wire net, and the mass (G2) of the residue after drying at 110 ° C for 1 hour is measured, and the gel fraction is calculated according to the following formula. The mass (G3) of the first and second conductive fillers in the sample is calculated from the mass (G1) of the sample and the composition of the adhesive. Gel fraction (mass%)=(G2-G3) / (G1-G3)×100
[0039] <First conductive filler> The first conductive filler is flaky, and examples thereof include flaky metal particles, graphite, and flaky particles formed by coating a flaky base material with a metal.
[0040] The scaly particles are also called thin plate-like particles, flat particles, flake-like particles, and the like. In the present invention, the term "scaly particles" refers to particles having a substantially flat surface and a substantially uniform thickness in the direction perpendicular to the substantially flat surface. The term "scaly particles" refers to particles having a shape in which the thickness is very thin and the length of the substantially flat surface is very long. The length of the substantially flat surface is the diameter of a circle having the same projected area as the projected area of the scale-like particle. The shape of the substantially flat surface is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polygons such as a rectangle, a square, a substantially circle, a substantially ellipse, a substantially triangle, a substantially square, a substantially pentagon, a substantially hexagon, a substantially heptagon, a substantially octagon, etc., and random, indefinite shapes, etc. Among these, a substantially circle or a substantially ellipse is preferable.
[0041] Examples of the flaky metal particles include flaky metal particles made of metals such as nickel, iron, chromium, cobalt, aluminum, antimony, molybdenum, copper, silver, platinum, and gold, and alloys such as solder and stainless steel.
[0042] Examples of graphite include natural graphite, kish graphite, and artificial graphite. The artificial graphite may be anisotropic graphite, isotropic graphite, or a mixture thereof, but isotropic graphite is preferable from the viewpoint of mechanical strength. The graphite may be crystalline or amorphous, or a mixture thereof. The graphite may be a carbon fiber-reinforced carbon composite material (C / C composite) in which graphite is reinforced with carbon fibers.
[0043] Examples of the scaly substrate in the scaly particles formed by coating a scaly substrate with a metal include glass, silica, alumina, mica, and zirconia. The content of the substrate in the scaly particles in which the scaly substrate is metal-coated is preferably 50% by mass or more, more preferably 65% by mass or more, and even more preferably 80% by mass or more. Methods for coating a scaly substrate with a metal include, for example, metal plating. Examples of metals used for metal plating include silver, gold, platinum, palladium, nickel, copper, and aluminum. The content of the metal plating in the scaly particles formed by coating a scaly substrate with a metal is preferably 10% by mass or more and 50% by mass or less, and more preferably 15% by mass or more and 30% by mass or less.
[0044] In the scaly first conductive filler, when the surface with the largest area is taken as the main surface, the average thickness of the main surface is preferably 0.5 μm or more and 6.0 μm or less, and more preferably 1.0 μm or more and 4.0 μm or less. The average particle size of the main surface of the scaly first conductive filler is not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferably 10 μm or more and 200 μm or less, and more preferably 20 μm or more and 100 μm or less. The average particle size refers to the 50% cumulative volume particle size in a volume-based particle size distribution, and is a value measured by a laser diffraction / scattering method, such as a Microtrac MT300II manufactured by Nikkiso Co., Ltd. or a laser diffraction particle size distribution analyzer SALD-3000 manufactured by Shimadzu Corporation. The ratio of the average particle diameter of the main surface of the first conductive filler to the average thickness of the main surface is preferably 10 or more and 100 or less, and more preferably 20 or more and 80 or less. By satisfying the above ranges of average thickness and average particle diameter relative to the main surface, and the ratio of the average particle diameter of the main surface to the average thickness of the main surface, a conductive adhesive sheet can be obtained that has excellent conductivity in the thickness direction of the adhesive sheet (Z-axis direction) as well as in the planar direction (XY direction).
[0045] The content of the first conductive filler is 55 parts by mass or less, preferably 5 parts by mass or more and 50 parts by mass or less, more preferably 10 parts by mass or more and 40 parts by mass or less, and even more preferably 15 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the solid content of the adhesive. By setting the content of the first conductive filler within the above numerical range, it is possible to achieve both high adhesive strength and excellent electrical conductivity both initially and over time.
[0046] <Second conductive filler> The second conductive filler is not particularly limited as long as it has a different shape from the above-mentioned scaly first conductive filler and has conductivity, and can be appropriately selected depending on the purpose, and examples thereof include metals such as nickel, iron, chromium, cobalt, aluminum, antimony, molybdenum, copper, silver, platinum, and gold, solder, and alloys such as stainless steel, etc. These may be used alone or in combination of two or more kinds. Among these, nickel, copper and silver are preferred, and nickel powder produced by the carbonyl method is more preferred. Examples of nickel powder produced by the carbonyl method include Ni123 (spherical) manufactured by Vale and Ni255 (filamentary) manufactured by Vale.
[0047] The shape of the metal particles is not particularly limited and can be appropriately selected depending on the purpose. For example, the shape may be spherical, filamentous (beaded), etc. 、 Among these, from the viewpoints of ensuring adhesive strength and facilitating the formation of conductive paths by the metal particles in the adhesive layer, spherical or filamentary shapes are preferred.
[0048] The particle size of the metal particles is not particularly limited and can be appropriately selected depending on the purpose, but the particle size d40 is preferably 5 μm or more and 30 μm or less, and more preferably 10 μm or more and 20 μm or less. The particle size d70 is preferably 10 μm or more and 50 μm or less, and more preferably 20 μm or more and 40 μm or less. The particle diameter d40 refers to the 40% cumulative volume particle diameter in the volume particle size distribution, and the particle diameter d70 refers to the 70% cumulative volume particle diameter in the volume particle size distribution, and is a value measured by a laser analysis / scattering method. Examples of the measuring device include Microtrac MT3000II manufactured by Nikkiso Co., Ltd. and Laser Diffraction Particle Size Distribution Measuring Instrument SALD-3000 manufactured by Shimadzu Corporation.
[0049] Examples of methods for adjusting the particle diameters d40 and d70 to be within the above-mentioned numerical ranges include a method of pulverizing metal particles with a jet mill and a method of sieving metal particles with a sieve.
[0050] The content of the second conductive filler is preferably 5 parts by mass or more and 50 parts by mass or less, more preferably 10 parts by mass or more and 45 parts by mass or less, and even more preferably 15 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the solid content of the adhesive. By setting the content of the second conductive filler within the above range, it is possible to achieve both high adhesive strength and excellent initial and aging conductivity.
[0051] In the present invention, the mass ratio (A / B) of the content A of the first conductive filler in the pressure-sensitive adhesive layer to the content B of the second conductive filler in the pressure-sensitive adhesive layer is preferably 1 / 1 or more and 1 / 5 or less, more preferably 1 / 1 or more and 1 / 3 or less, and even more preferably 1 / 1 or more and 1 / 2 or less. By setting the mass ratio (A / B) within the above range, it is possible to achieve both high adhesive strength and excellent electrical conductivity both initially and over time.
[0052] An example of a method for dispersing the first and second conductive fillers in the adhesive layer is a method for dispersing the (meth)acrylic polymer, the first and second conductive fillers, a solvent, an additive, and the like, using a dispersion stirrer. Examples of commercially available dispersion stirrers include a dissolver, butterfly mixer, BDM two-shaft mixer, and planetary mixer manufactured by Inoue Seisakusho Co., Ltd. Among these, a dissolver or butterfly mixer that can apply a moderate shear with little increase in viscosity of the adhesive during stirring is preferred.
[0053] <Other ingredients> Other components in the adhesive layer include, for example, additives such as crosslinking agents, antioxidants, ultraviolet absorbers, fillers, polymerization inhibitors, surface conditioners, antistatic agents, defoamers, viscosity modifiers, light stabilizers, weather stabilizers, heat stabilizers, antioxidants, leveling agents, organic pigments, inorganic pigments, pigment dispersants, plasticizers, softeners, flame retardants, metal deactivators, silica beads, organic beads, etc.; inorganic fillers such as silicon oxide, aluminum oxide, titanium oxide, zirconia, antimony pentoxide, etc.
[0054] The conductive adhesive tape of the present invention can be produced, for example, by applying the adhesive to a release liner or a conductive substrate using a roll coater, a die coater, or the like, and drying the applied adhesive. Alternatively, the conductive adhesive tape can be produced by a transfer method in which an adhesive layer formed on a release liner is laminated to a conductive substrate. The double-sided pressure-sensitive adhesive tape can be produced by a transfer method in which the pressure-sensitive adhesive is applied in advance to the surface of a release liner using a roll coater or the like, and then dried to form a pressure-sensitive adhesive layer, and then the pressure-sensitive adhesive layer is bonded to both sides of a conductive substrate.
[0055] When laminating the adhesive layer formed on the release liner and the conductive substrate, it is preferable to perform heat lamination from the viewpoint of imparting excellent adhesion between the conductive substrate and the adhesive layer. The temperature of heat lamination is preferably 60°C to 150°C, more preferably 70°C to 130°C, and even more preferably 80°C to 110°C in terms of adhesion and suppressing shrinkage of the conductive substrate.
[0056] -Release liner- The release liner is not particularly limited and can be appropriately selected depending on the purpose. Examples of the release liner include papers such as kraft paper, glassine paper, and fine paper; resin films such as polyethylene, polypropylene (OPP, CPP), and polyethylene terephthalate; laminated paper in which the above-mentioned papers and resin films are laminated together; and papers in which the above-mentioned papers have been sealed with clay, polyvinyl alcohol, or the like and one or both sides have been treated with a release agent such as a silicone-based resin.
[0057] -Conductive base material- Examples of conductive substrates that can be used in the conductive pressure-sensitive adhesive sheet of the present invention include metal foil substrates and conductive substrates in which a wet-type polyester nonwoven fabric substrate is plated. Examples of the material of the metal foil include gold, silver, copper, aluminum, nickel, iron, tin, and alloys thereof. Among these, a conductive base material containing copper is preferred, and copper foil is more preferred from the viewpoints of conductivity, processability, and cost.
[0058] It is preferable to apply rust prevention treatment to the copper foil. Types of rust prevention treatment include organic rust prevention and inorganic rust prevention, among which inorganic rust prevention by chromate treatment is the most preferable. Examples of commercially available electrolytic copper foil include CF-T9FZ-HS-12 (12 μm: chromate treatment) and CF-T9FZ-HS-9 (9 μm: chromate treatment) manufactured by Fukuda Metal Foil and Powder Co., Ltd. Examples of commercially available rolled copper foil include TCU-H-8-RT (8 μm: organic rust prevention treatment) manufactured by Nippon Foil Co., Ltd. and BAY-64T-DT (35 μm: chromate treatment) manufactured by JX Nippon Mining & Metals Corporation.
[0059] The conductive substrate obtained by plating the wet polyester nonwoven fabric substrate is one that uses electroless metal plating as the plating. Examples of the metal to be plated include copper, nickel, silver, platinum, and aluminum. Among these, copper or nickel is preferred from the viewpoints of conductivity and cost.
[0060] The thickness of the conductive substrate is preferably from 1 μm to 40 μm, more preferably from 3 μm to 35 μm, and even more preferably from 6 μm to 25 μm. The thickness in the above range is preferable because it can be made thin and has excellent processability.
[0061] The conductive adhesive sheet of the present invention may be a so-called substrate-less conductive adhesive sheet that does not have a conductive substrate, or may be a so-called substrate-attached conductive adhesive sheet that has a conductive substrate.
[0062] The substrate-less conductive adhesive sheet is composed only of an adhesive layer, and the average thickness of the adhesive layer is the total thickness of the conductive adhesive sheet. The substrate-less conductive adhesive sheet is formed on a release liner, and is covered with the release liner until use. The average thickness of the substrateless conductive adhesive sheet (average thickness of the adhesive layer) is preferably 30 μm or less, more preferably 5 μm or more and 25 μm or less, and even more preferably 10 μm or more and 20 μm or less. When it is within the above numerical range, it is possible to achieve both excellent adhesiveness and conductivity and a thin shape.
[0063] The total thickness of the conductive adhesive sheet with the substrate is preferably 100 μm or less, more preferably 65 μm or less, and even more preferably 50 μm or less. By being in the above range, the conductive adhesive sheet can be made thinner while ensuring adhesion and conductivity, which can contribute to making portable electronic devices thinner. The total thickness of the conductive adhesive sheet is the thickness of the conductive adhesive sheet itself, not including the release liner.
[0064] The conductive adhesive sheet of the present invention is preferably such that the 180-degree peel adhesion strength at 300 mm / min after the conductive adhesive sheet is pressed against a stainless steel plate (SUS plate) in an environment of a temperature of 23°C and a humidity of 50% RH with a 2 kg roller in one back and forth motion and left to stand for 1 hour is 5 N / 25 mm or more. When the thickness is within the above range, peeling is easily suppressed, and the conductive adhesive sheet can be peeled off in defective products during the manufacturing process.
[0065] The conductive adhesive sheet of the present invention is prepared by attaching copper foil to one side of the conductive adhesive sheet, cutting the sheet to a size of 15 mm wide x 100 mm wide, and attaching two tin-plated plates to the other adhesive layer of the conductive adhesive sheet so that each has an adhesion area of 15 mm x 15 mm. The resistance change rate [(resistance after 168 hours / initial resistance) x 100] calculated from the measured initial resistance value and the resistance value measured after leaving the test piece at 23°C for 168 hours is preferably 250% or less, more preferably 200% or less, and even more preferably 150% or less. When the rate of change in resistance is 250% or less, excellent electrical conductivity can be achieved both initially and over time.
[0066] <Application> The conductive adhesive sheet of the present invention can achieve both high adhesive strength and excellent initial and aging conductivity, and is therefore useful, for example, for shielding electromagnetic waves used in electric or electronic devices, for shielding harmful spatial electromagnetic waves generated by other electric or electronic devices, and for fixing to earth to prevent static electricity. Among these, it is suitable for use in portable electronic devices that are becoming thinner and have strict volume restrictions within the housing, and is particularly suitable for use by attaching it to the built-in components of small electronic terminals. EXAMPLES
[0067] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0068] (Synthesis Example 1 of Acrylic Copolymer) <Acrylic copolymer (1)> In a reaction vessel equipped with a stirrer, a reflux condenser, a thermometer, a dropping funnel, and a nitrogen gas inlet, 92 parts by mass of n-butyl acrylate, 6 parts by mass of acrylic acid, 2 parts by mass of 2-hydroxyethyl acrylate, and 0.2 parts by mass of 2,2'-azobisisobutylnitrile as a polymerization initiator were dissolved in 100 parts by mass of ethyl acetate, and after nitrogen replacement, the mixture was polymerized at 80°C for 8 hours to obtain an acrylic copolymer (1) having a weight average molecular weight of 700,000.
[0069] The weight average molecular weight is a weight average molecular weight measured by gel permeation chromatography (GPC) in terms of standard polystyrene, and was measured by the following method. The molecular weight can be measured by the GPC method using a GPC apparatus (HLC-8329GPC) manufactured by Tosoh Corporation, and is calculated as a polystyrene equivalent value under the following GPC measurement conditions. [Measurement conditions] Sample concentration: 0.5% by mass (tetrahydrofuran solution) Sample injection volume: 100μL Eluent: Tetrahydrofuran (THF) ·Flow rate: 1.0mL / min Column temperature (measurement temperature): 40℃ - Main column: TSKgel GMHHR-H(20) x 2 Guard column: Tosoh Corporation's "TSKgel HXL-H" Detector: Differential refractometer Standard polystyrene molecular weight: 10,000 to 20,000,000 (Tosoh Corporation)
[0070] (Preparation Example 1 of Adhesive) -Preparation of Adhesive A- 100 parts by mass of the acrylic copolymer (1) was mixed with 5 parts by mass of a polymerizable rosin ester-based tackifier resin (D-125, manufactured by Arakawa Chemical Industries, Ltd.) and 15 parts by mass of a petroleum-based tackifier resin (FTR6125, manufactured by Mitsui Chemicals, Inc.), and the mixture was stirred, and then ethyl acetate was added to obtain an adhesive A having a solid content of 40% by mass.
[0071] Example 1 <Production of conductive adhesive composition A> 100 parts by mass (solid content) of the adhesive A was mixed with 30 parts by mass of a first conductive filler (conductive particles obtained by plating glass flake powder with 20% by mass of silver, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 30 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7% by mass, non-volatile content 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition A.
[0072] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition A was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 1.
[0073] Example 2 <Production of Conductive Adhesive Composition B> 100 parts by mass (solid content) of the adhesive A were mixed with 20 parts by mass of a first conductive filler (conductive particles obtained by plating glass flake powder with 20% by mass of silver, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 40 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7% by mass, non-volatile content 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition B.
[0074] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition B was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 2.
[0075] Example 3 <Production of Conductive Adhesive Composition C> 100 parts by mass (solid content) of the adhesive A were mixed with 10 parts by mass of a first conductive filler (conductive particles obtained by plating glass flake powder with 20% by mass of silver, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 50 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7% by mass, non-volatile content 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition C.
[0076] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition C was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated film was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 3.
[0077] Example 4 <Production of Conductive Adhesive Composition D> 100 parts by mass (solid content) of the adhesive A were mixed with 45 parts by mass of a first conductive filler (conductive particles obtained by plating 20% by mass of silver on glass flake powder, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 45 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7% by mass, non-volatile content 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition D.
[0078] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition D was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 4.
[0079] Example 5 <Production of Conductive Adhesive Composition E> 15 parts by mass of a first conductive filler (conductive particles obtained by plating 20% by mass of silver on glass flake powder, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 15 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content of 7% by mass, non-volatile content of 40% by mass) were blended with respect to 100 parts by mass (solid content) of the adhesive A, and the solid content concentration was adjusted to 40% by mass with ethyl acetate, and the mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition E.
[0080] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition E was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated film was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 5.
[0081] Example 6 <Production of conductive adhesive composition F> 100 parts by mass (solid content) of the adhesive A were mixed with 30 parts by mass of a first conductive filler (nickel flake powder, HCA-1, manufactured by Vale, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 12.5 μm), 30 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7 mass%, non-volatile content 40 mass%), and the solid content concentration was adjusted to 40 mass% with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition F.
[0082] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition F was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated film was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 6.
[0083] Example 7 <Production of conductive adhesive composition G> 100 parts by mass (solid content) of the adhesive A were mixed with 30 parts by mass of a first conductive filler (conductive particles obtained by plating glass flake powder with 20% by mass of silver, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 30 parts by mass of a second conductive filler (nickel, Ni123, manufactured by Vale, filament-like, particle diameter d40 = 8.2 nm, particle diameter d70 = 16.6 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7% by mass, non-volatile content 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition G.
[0084] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition G was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 7.
[0085] Example 8 <Production of conductive adhesive composition H> 100 parts by mass (solid content) of the adhesive A were mixed with 30 parts by mass of a first conductive filler (nickel flake powder, HCA-1, manufactured by Vale, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 12.5 μm), 30 parts by mass of a second conductive filler (nickel, Ni123, manufactured by Vale, filament-like, particle diameter d40 = 8.2 nm, particle diameter d70 = 16.6 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7 mass%, non-volatile content 40 mass%), and the solid content concentration was adjusted to 40 mass% with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition H.
[0086] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition H was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 8.
[0087] Example 9 <Production of Conductive Adhesive Composition I> 100 parts by mass (solid content) of the adhesive A were mixed with 10 parts by mass of a first conductive filler (conductive particles obtained by plating 20% by mass of silver on glass flake powder, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 10 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content of 7% by mass, non-volatile content of 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition I.
[0088] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition I was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coating was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce the conductive adhesive sheet of Example 9.
[0089] Comparative Example 1 <Production of Conductive Adhesive Composition J> 100 parts by mass (solid content) of the adhesive A was mixed with 30 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filamentous, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm) and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content 7 mass%, non-volatile content 40 mass%), and the solid content concentration was adjusted to 40 mass% with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition J.
[0090] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition J was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce a conductive adhesive sheet of Comparative Example 1.
[0091] Comparative Example 2 <Production of conductive adhesive composition K> 100 parts by mass (solid content) of the adhesive A was mixed with 30 parts by mass of a first conductive filler (conductive particles formed by plating glass flake powder with 20% by mass of silver, scale-shaped, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm) and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content of 7% by mass, non-volatile content of 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was then mixed with a dispersion stirrer to prepare conductive adhesive composition K.
[0092] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition K was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80°C for 2 minutes and then aged at 40°C for 48 hours to produce a conductive adhesive sheet of Comparative Example 2.
[0093] Comparative Example 3 <Production of conductive adhesive composition L> 100 parts by mass (solid content) of the adhesive A were mixed with 60 parts by mass of a first conductive filler (conductive particles obtained by plating 20% by mass of silver on glass flake powder, scale-like, average thickness of the main surface of 2 μm, average particle diameter of the main surface of 25 μm), 60 parts by mass of a second conductive filler (nickel, Ni255, manufactured by Vale, filament-like, particle diameter d40 = 17.2 nm, particle diameter d70 = 35.4 nm), and 2 parts by mass of Burnock D-40 (manufactured by DIC Corporation, trimethylolpropane adduct of tolylene diisocyanate, isocyanate group content of 7% by mass, non-volatile content of 40% by mass), and the solid content concentration was adjusted to 40% by mass with ethyl acetate. The mixture was mixed with a dispersion stirrer to prepare a conductive adhesive composition L.
[0094] <Preparation of conductive adhesive sheet> The obtained conductive adhesive composition L was coated on a conductive substrate (electrolytic copper foil, average thickness 12 μm) using a comma coater so that the average thickness after drying would be 25 μm, and the coated substrate was dried in a dryer at 80° C. for 2 minutes and then aged at 40° C. for 48 hours to produce a conductive adhesive sheet of Comparative Example 3.
[0095] Next, various properties were evaluated as follows for the obtained conductive adhesive sheets of Examples 1 to 9 and Comparative Examples 1 to 3. The results are shown in Tables 1 to 3.
[0096] <Measurement of the average thickness of conductive adhesive sheets> The average thickness of each conductive adhesive sheet was determined by measuring the thickness of the conductive adhesive sheet at five locations at 100 mm intervals along the length using a dial thickness gauge Type G manufactured by Ozaki Seisakusho Co., Ltd.
[0097] <Method for evaluating adhesive strength> The adhesive strength of the conductive adhesive sheet was determined according to the following procedure in accordance with the 180-degree peel adhesion test method of JIS-Z0237 (2000). The conductive adhesive sheets obtained in the examples and comparative examples were cut to a size of 25 mm width. Next, the adhesive layer on one side of the conductive adhesive sheet was backed with a polyester film having a thickness of 25 μm. Next, under conditions of an environmental temperature of 23°C and humidity of 50% RH, the backed conductive adhesive sheet was attached to a stainless steel plate (SUS plate), and a 2 kg roller was rolled back and forth once on the top surface to press the two together, and then the specimen was left at the above temperature for 1 hour to prepare a test specimen. The test pieces were peeled off at a speed of 300 mm / min under the same temperature and humidity conditions as above using a Tensilon universal tensile tester (RTA100, manufactured by Orientec Co., Ltd.) to measure the 180-degree peel adhesive strength. When the adhesive strength was 5 N / 25 mm or more, it was evaluated as having excellent adhesiveness.
[0098] <Conductivity evaluation method> Copper foil (thickness 12 μm) was attached to one side of the conductive adhesive sheet. The conductive adhesive sheet was cut to a size of 15 mm width × 100 mm width. The other adhesive layer of the cut conductive adhesive sheet was attached to two tin-plated plates so that the attachment area was 15 mm × 15 mm, respectively, to prepare a test piece. In an environment of 23 ° C and 50% RH, a terminal was connected to a position about 100 mm away from the conductive adhesive sheet attachment position on the tin-plated surface, and a current of 10 μA was applied using a resistivity meter (Loresta-GP MCP-T600, manufactured by Mitsubishi Chemical Corporation) to measure the initial resistance value. The prepared test piece was left at 23° C. for 168 hours, and then the resistance was measured in the same manner as above. A test piece was evaluated as having excellent conductivity when the resistance after 168 hours was 100 mΩ or less and the rate of change in resistance (resistance after 168 hours / initial resistance)×100 was 250% or less.
[0099] [Table 1]
[0100] [Table 2]
[0101] [Table 3] [Explanation of symbols]
[0102] 1 Conductive base material 2 Adhesive layer 3. First conductive filler 4 Second conductive filler 10 Conductive adhesive sheet
Claims
1. A conductive adhesive sheet having an adhesive layer, the pressure-sensitive adhesive layer contains a first conductive filler, a second conductive filler, and a pressure-sensitive adhesive; The first conductive filler has a scale-like shape, the second conductive filler is a metal or alloy having a shape other than a flake shape, The content of the first conductive filler is 55 parts by mass or less relative to 100 parts by mass of a solid content of the pressure-sensitive adhesive; The content of the second conductive filler is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of a solid content of the pressure-sensitive adhesive, The first conductive filler has an average particle size of 10 μm or more and 200 μm or less, The particle diameter d40 of the second conductive filler is 5 μm or more and 30 μm or less, and the particle diameter d70 of the second conductive filler is 10 μm or more and 50 μm or less, The conductive adhesive sheet, characterized in that the adhesive contains a (meth)acrylic polymer, a tackifier resin, and a crosslinking agent.
2. The conductive adhesive sheet according to claim 1 , wherein the first conductive filler is at least one of scaly metal particles, graphite, and scaly particles formed by coating a scaly substrate with a metal.
3. The conductive adhesive sheet according to claim 1 , wherein the second conductive filler is a spherical, filamentous, or spike-shaped metal or alloy particle.
4. The conductive adhesive sheet according to any one of claims 1 to 3, wherein the mass ratio (A / B) of the content A of the first conductive filler in the adhesive layer to the content B of the second conductive filler in the adhesive layer is 1 / 1 or more and 1 / 5 or less.
5. The conductive adhesive sheet according to claim 1 , wherein the content of the first conductive filler is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of a solid content of the adhesive.
6. The conductive adhesive sheet according to claim 1 , wherein a ratio of an average particle diameter of the first conductive filler on the main surface to an average thickness of the main surface is 10 or more and 100 or less.
7. The conductive adhesive sheet according to claim 1 , wherein the adhesive is an acrylic adhesive containing a (meth)acrylic polymer.
8. The conductive adhesive sheet according to claim 1 , which comprises a conductive substrate.
9. A conductive adhesive sheet according to any one of claims 1 to 8, wherein a test piece is prepared by attaching copper foil to one side of a conductive adhesive sheet, cutting the sheet to a size of 15 mm wide x 100 mm wide, and attaching two tin-plated plates to the adhesive layer on the other side of the conductive adhesive sheet so that each has an adhesion area of 15 mm x 15 mm. The rate of change in resistance [(resistance after 168 hours / initial resistance) x 100] is calculated from the measured initial resistance value and the resistance value measured after leaving the test piece at 23°C for 168 hours, and is 250% or less.
10. The conductive adhesive sheet according to claim 1 , which is used for at least one of electromagnetic shielding and earthing inside and outside of electric or electronic equipment.
Citation Information
Patent Citations
Leucite porcelain
JP1986006148A
Electrically-conductive pressure-sensitive adhesive composition
JP1986152778A
Manufacture of pressure sensitive conductive sheet
JP1987093811A
Electric conductive adhesive agent
JP1993081923A
Electrically conductive adhesive tape
JP1993117606A