Manufacturing method for insulating circuit board
The method aligns ceramic and metal plates with dummy parts to contain brazing material spread, addressing the issue of poor appearance and etching defects in insulated circuit board manufacturing, ensuring reliable bonding and etching.
Patent Information
- Application Number
- JP2021031572
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-01
AI Technical Summary
The issue of brazing material flowing out during the manufacturing of insulated circuit boards, causing poor appearance and etching defects due to improper positioning and excess material between the ceramic and metal plates, is addressed.
A manufacturing method involving precise alignment of the ceramic and metal plates with dummy parts positioned to contain the spread of brazing material, using thermal expansion considerations and burrs to block the flow of molten brazing material, and ensuring accurate etching by aligning corners for resist printing.
Prevents brazing material from creeping onto the metal plate surface, maintaining board appearance and ensuring accurate etching, thereby producing high-quality insulated circuit boards.
Smart Images

Figure 0007574697000001 
Figure 0007574697000002 
Figure 0007574697000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an insulating circuit board used in a power module or the like for controlling a large current and a high voltage. [Background technology]
[0002] For example, a metal-bonded ceramic substrate (insulated circuit substrate) described in Patent Document 1, which is an insulating circuit substrate used in conventional power modules, includes a ceramic substrate made of AlN (aluminum nitride), Al2O3 (alumina), Si3N4 (silicon nitride), or the like, a circuit layer formed by bonding a first metal plate to one surface of the ceramic substrate, and a metal layer formed by bonding a second metal plate to the other surface of the ceramic substrate. The patent document also describes a manufacturing process in which a metal plate is placed in contact with a ceramic substrate that can be divided into a plurality of ceramic substrates by forming cutting lines (scribe lines), and then these are bonded together by an active metal method or the like, unnecessary portions of the metal plate are removed by etching to form a circuit pattern, and the ceramic substrate is divided along the scribe lines to obtain individual insulating circuit substrates. When brazing a ceramic plate to a metal plate, if the metal plate is a copper or copper alloy plate, an Ag-Ti or Ag-Cu-Ti brazing material containing an active metal is used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5642808 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when manufacturing a bonded body using the etching method, at least two diagonal corners of the ceramic plate must be exposed in order to position the resist printing required for circuit formation, and for this reason, at least two sides of the continuous metal plate must be located inside the outer periphery of the ceramic substrate after bonding. Generally, a "dummy part" exists around the outer periphery of a ceramic plate to protect the ceramic plate that will become the product during the manufacturing process. Usually, the two exposed corners of this ceramic plate are used as the reference for the subsequent resist printing.
[0005] On the other hand, to ensure bondability, a minimum amount of brazing material must be present in the required joining locations. If the positional relationship between the metal plate and the brazing material is inappropriate while ensuring the required brazing material area, excess brazing material will flow out from between the ceramic plate and the metal plate in the area where the ceramic plate is exposed during bonding (the "dummy area"), and creep up onto the surface of the metal plate via the side of the metal plate, causing problems such as poor appearance and poor etching when forming circuits.
[0006] The present invention has been made in consideration of the above circumstances, and aims to suppress the outflow of brazing material into the "dummy part" and prevent poor appearance and etching caused by the brazing material creeping up onto the metal plate surface. [Means for solving the problem]
[0007] The method for producing an insulating circuit board of the present invention includes a lamination step of laminating a rectangular ceramic plate and a metal plate, each having a dividing scribe line formed therein, via a brazing material; a joining step of heating the laminate to melt the brazing material and then cooling the laminate to join the ceramic plate and the metal plate; an etching step of etching the metal plate after the joining step to remove unnecessary portions; and a division step of dividing the ceramic plate along the scribe lines after the etching step to form a plurality of insulating circuit boards, In the lamination step, one corner of the ceramic plate and one corner of the metal plate are aligned to each other, and a dummy portion of the ceramic plate is formed on two sides that constitute a corner opposite to the one corner, In the joining step, in the dummy portion, the outer edge of a spreading region of the molten brazing material is positioned inside the outer edge that spreads due to thermal expansion of the metal plate.
[0008] When joining the ceramic plate and the metal plate, two sides are positioned using one corner as a reference, and the two opposing corners of the ceramic plate exposed in the dummy portions of the remaining two sides also serve as a reference for resist printing during etching. In the joining process, by positioning the outer edge of the spreading area of the molten brazing material in the dummy part inside the outer edge that spreads due to thermal expansion of the metal plate, the molten brazing material is prevented from flowing out onto the ceramic plate of the dummy part, and the brazing material is prevented from creeping up onto the surface of the metal plate.
[0009] This manufacturing method includes a metal plate forming process in which the metal plate is formed by cutting it from a plate material, and in the lamination process, the surface of the cut end of the metal plate having a burr is preferably overlapped on the surface of the dummy portion of the ceramic plate.
[0010] By overlapping the burrs of the metal plate on the surface of the dummy portion, the molten brazing material can be stopped by the burrs during the joining process, preventing it from flowing out of the metal plate.
[0011] In this manufacturing method, the plate material is a long material set to the width of the metal plate, and in the metal plate forming process, the plate material is intermittently transported in the longitudinal direction while being cut to the length of the metal plate by a shear to form the metal plate, and in the stacking process, the cut end of the metal plate on the rear side in the transport direction in the metal plate forming process is placed on the dummy section, and the surface of the cut end with a burr is overlapped on the surface of the dummy section.
[0012] When a plate material is cut by a shear while being conveyed intermittently, the metal plate is cut off on the forward side of the cutting blade in the conveying direction. At this time, the cut end surface of the cut-off metal plate on the rear side in the conveying direction has a rough surface due to a fracture surface caused by the cutting. Furthermore, a burr protruding from the front side of the metal plate is generated by the cutting, and the back side has a droopy surface. Meanwhile, the cut end surface of the plate material after the metal plate is cut off is rubbed by the surface of the cutting blade that is pulled up after cutting the metal plate, resulting in a relatively smooth cut end surface. Furthermore, the front side of the plate material has a droopy surface due to the cutting, and a burr protruding from the back side. However, since it is scraped up by the cutting blade after cutting, the height of the burr is smaller than that of the metal plate. Therefore, by placing the cut end of the cut-off metal plate on the rear side in the transport direction on a dummy part of the ceramic plate and overlapping the burr on the surface of the dummy part, the burr has a great effect of blocking the molten brazing material during the joining process, effectively preventing it from flowing out of the metal plate. Effect of the Invention
[0013] According to the present invention, it is possible to suppress the outflow of the brazing material onto the "dummy portion" and prevent poor appearance and poor etching caused by the brazing material creeping up onto the metal plate surface. [Brief description of the drawings]
[0014] [Figure 1] 1 is a flowchart showing a method for manufacturing an insulating circuit board according to an embodiment of the present invention. [Diagram 2] 1 is a vertical cross-sectional view showing an example of an insulating circuit board manufactured by a manufacturing method according to an embodiment. [Diagram 3] 3 is a plan view showing a ceramic plate in the middle of manufacturing the insulating circuit board of FIG. 2. [Figure 4] 4 is a plan view showing a state in which a brazing material is formed on the ceramic plate shown in FIG. 3. FIG. [Diagram 5] 5 is a perspective view showing a state before a metal plate is laminated on the state shown in FIG. 4. FIG. [Figure 6] 6 is a plan view showing a state in which a metal plate is laminated on the state shown in FIG. 5. FIG. [Figure 7] FIG. 2 is a schematic diagram showing a state in which a plate material is being cut by a shear. [Figure 8] 4 is a cross-sectional view showing both cut ends of a metal plate cut by a shear. FIG. [Figure 9] FIG. 4 is a cross-sectional view showing the vicinity of a cut end portion of the metal plates after joining. [Figure 10] 1 is a graph obtained by measuring the relationship between the load during joining and the spreading rate of the brazing material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the method for producing an insulating circuit board of the present invention will be described. The insulating circuit board 1 manufactured by the manufacturing method of this embodiment is, for example, a power module board used in a power supply circuit. As shown in Fig. 2, this insulating circuit board 1 has a rectangular ceramic substrate 2, a circuit layer 3 formed on one surface of the ceramic substrate 2, and a heat dissipation layer 4 formed on the other surface of the ceramic substrate 2. The circuit layer 3 and the heat dissipation layer 4 are smaller in planar shape than the ceramic substrate 2, and the ceramic substrate 2 is exposed to the periphery. For convenience, both the circuit layer 3 and the heat dissipation layer 4 are shown in Fig. 2 and other figures as being rectangular, but the planar shapes are not particularly limited.
[0016] The ceramic substrate 2 prevents electrical connection between the circuit layer 3 and the heat dissipation layer 4, and may be made of aluminum nitride (AlN), silicon nitride (Si3N4), aluminum oxide (Al2O3), etc., of which silicon nitride is preferred due to its high strength. The thickness of the ceramic substrate 2 is set within the range of 0.2 mm to 1.5 mm.
[0017] The circuit layer 3 can be made of aluminum or an aluminum alloy, or copper or a copper alloy, but copper or a copper alloy, which have excellent electrical properties, is preferred. The heat dissipation layer 4 is also made of the same metal material as the circuit layer 3, for example, copper or a copper alloy. The circuit layer 3 and the heat dissipation layer 4 are formed, for example, by brazing a copper plate made of oxygen-free copper with a purity of 99.96 mass% or more to the ceramic substrate 2 with an active metal brazing material (for example, a brazing material made of Ag-Ti or Ag-Cu-Ti). The thickness of the circuit layer 3 and the heat dissipation layer 4 is set within a range of 0.1 mm to 5 mm.
[0018] A method for manufacturing the insulating circuit board 1 thus configured will be described. 1, this insulating circuit board 1 is manufactured through a ceramic plate forming step S1, a metal plate forming step S2, a lamination step S3, a joining step S4, an etching step S5, and a division step S6. The order of the ceramic plate forming step S1 and the metal plate forming step S2 does not matter, and either may be performed first, or they may be performed simultaneously. The steps are described below in order of the steps. The circuit layer 3 and the heat dissipation layer 4 are formed through a metal plate forming step S2, a lamination step S3, a bonding step S4, and an etching step S5, except that the etching shapes in the etching step are different, and the insulating circuit board 1 having the circuit layer 3 and the heat dissipation layer 4 is formed through a final dividing step S6. In the following, when the circuit layer 3 and the heat dissipation layer 4 are subjected to the same processing, the circuit layer 3 and the heat dissipation layer 4 will be described without any particular distinction between them.
[0019] (Ceramics plate forming process: S1) As shown in FIG. 3 and other figures, a single ceramic plate 11 large enough to form a plurality of ceramic substrates 2 is prepared, and groove-shaped dividing scribe lines (hereinafter simply referred to as scribe lines) 12 are formed on one or both sides of the ceramic plate 11 by laser processing (FIG. 5 and other figures show an example in which the scribe lines 12 are formed on one side). By dividing the ceramic plate 11 along the scribe lines 12, a plurality of ceramic substrates 2 (3×4=12 in the illustrated example) are obtained. The scribe lines 12 are formed vertically and horizontally in the ceramic plate 11, thereby dividing the ceramic plate 11 into a plurality of ceramic substrates 2 (3×4=12 in the illustrated example), and dummy portions 13 that are not used as products are formed on the periphery of the ceramic plate 11. The dummy portions 13 are preferably formed to have a width of 0.3 mm or more and 20 mm or less. If the width is less than 0.3 mm, it may be difficult to divide the ceramic plate 11 in the subsequent dividing step. If the width exceeds 20 mm, material is wasted, resulting in high costs. In FIG. 3 etc., a notch 16 at the upper right of the ceramic plate 11 is provided for identifying the orientation of the ceramic plate 11.
[0020] (Metal plate forming process S1) The metal plate 21 for forming the circuit layer 12 and the heat dissipation layer 4 is large enough to cover all of the ceramic substrates 2 of the ceramic plate 11 divided by the scribe lines 12, and is formed to a size such that its two sides 22a, 22b are aligned with the two sides 15a, 15b that form one corner 14 of the ceramic plate 11, while the other two sides 22a, 22b extend over the dummy portion 13, as shown in Figure 6. Moreover, this metal plate 12 is formed by cutting a long plate material (long material) 31 by a shear 32 while intermittently conveying it in the length direction. The width of this plate material 31 is formed in advance to the width of the metal plate 21, and it can be used as the metal plate 21 by cutting it to the length of the metal plate 21.
[0021] As shown in Fig. 7, the shear 32 that cuts the plate material 31 has a conveyor table 33 that conveys the plate material 31 in the length direction indicated by the arrow M, a plate presser 34 that presses the plate material 31 on the conveyor table 33, an upper blade 35, and a lower blade 36. The lower blade 36 is fixedly provided at the tip of the conveyor table 33, and the upper blade 35 moves up and down. In general, the upper blade 35 is formed at a slight inclination angle (shar angle) with respect to the horizontal direction (the direction perpendicular to the paper surface of Fig. 7).
[0022] Then, the plate material 31 is protruded forward from the cutting position between the upper blade 35 and the lower blade 36 by the length of the metal plate 21, and the upper blade 35 is lowered while the plate material 31 is held down by the plate holder 34, thereby cutting the plate material 31 between the upper blade 35 and the lower blade 36 to form the metal plate 21. After one metal plate 21 has been cut, the plate material 31 is transported a length equivalent to the length of the metal plate 21, and the next metal plate 21 is cut. Thereafter, the metal plates 21 are cut one by one while being transported intermittently in sequence.
[0023] In cutting by the shear 32, burrs 25 are generated on the cut ends 23, 24 of the cut metal sheet 21 at both ends in the conveying direction. In this case, as shown in Fig. 8, at the cut end 23 on the rear side in the conveying direction of the plate material 31 (metal sheet 21), the burr 25 protrudes toward the front surface 21a of the metal sheet 21 (the direction in which the upper blade 35 is disposed) when it is cut off by the upper blade 35. In addition, the cut end surface has a drooped surface 26 on the back surface 21b side, a fractured surface 27 on the side where the burr 25 is protruding (the front surface 21a side), and a relatively smooth sheared surface 28 is formed between the drooped surface 26 and the fractured surface 27.
[0024] Burrs 25 are also generated on the cut end 24 of the plate material 31 (the cut end 24 on the front side of the conveying direction of the plate material 31 (metal plate 21)) after the metal plate 21 is cut off, and a sag surface 26, a shear surface 28, and a fracture surface 27 are formed. However, since the cut is made between the cut end 23 on the rear side of the conveying direction of the metal plate 21, the burrs 25 are formed on the back surface 21b of the metal plate 21 opposite the cut end 23, and the sag surface 26 is formed on the front surface 21a. In addition, when the upper blade 35 of the shear 32 returns to the initial position after cutting the metal plate 21, it comes into contact with the cut end surface of the plate material 31 and moves while scraping it up, so that the burrs 25 and the fracture surface 27 are smaller than those of the cut end 23 on the rear side of the conveying direction of the metal plate 21. In other words, in the metal plate 21, the burrs 25 and the fracture surface 27 are formed larger on the cut end 23 on the rear side of the conveying direction, and the burrs 25 and the fracture surface 27 are formed smaller on the cut end 24 on the front side of the conveying direction than on the cut end 23 on the rear side.
[0025] (Lamination process) First, as shown in Fig. 4 and Fig. 5, the brazing material 41 is placed on the ceramic plate 11. The brazing material 41 may be either a paste-like material or a foil-like material formed into a rectangular shape. In either case, the brazing material 41 is provided so as to cover the dummy portion 13 constituting the two sides 15a, 15b along which the metal plate 21 is aligned, and the entire area of the portion that will become the product (ceramic substrate 2) partitioned by the scribe line 12, and to protrude partly into the dummy portion 13 on the opposite side to the dummy portion 13 constituting the two sides 15a, 15b along which the metal plate 21 is aligned.
[0026] 5 and 6, the metal plate 21 is placed on the brazing material 41. The metal plate 21 is placed in a state where two sides 22a, 22b of the metal plate 21 are positioned and aligned with two sides 15a, 15b constituting one corner 14 of the ceramic plate 11, and in this state, the other two sides 22c, 22d of the metal plate 21 are placed on the dummy portion 13 of the ceramic plate 11. In this dummy portion 13, the brazing material 41 is placed inside the sides 22c, 22d of the metal plate 21.
[0027] In this dummy portion 13, the protruding lengths L1, L2 (distances from the scribe lines 12 that divide the dummy portion 13) of the brazing material 41 and the metal plate 21 are set so that the outer edge of the spreading area of the molten brazing material 41 in the joining process described below is positioned inside the outer edge that spreads due to thermal expansion of the metal plate 21. In other words, they are set so that even if the molten brazing material 41 is pushed and spread by the action of the temperature and load applied during the joining process, it does not protrude from the outer edge of the thermally expanded metal plate 21. In the laminated state shown in FIG. 6, the notch 16 formed in the ceramic plate 11 is exposed.
[0028] Also, as explained above, in the metal plate forming process, burrs 25 are generated on the metal plate 21, but in this lamination process, the cut end 24 that was located on the front side in the conveying direction in the metal plate forming process is located on one of the two sides 22a, 22b that are positioned on the two sides 15a, 15b of the ceramic plate 11, and the cut end 23 that was located on the rear side in the conveying direction is arranged so that its burr 25 overlaps the surface of the dummy portion 13. As a result, the burr 25 on this cut end 23 is arranged facing the surface of the ceramic plate 11 (see FIG. 9). On the other hand, cut end 24, which was positioned on the front side in the conveying direction during the metal plate forming process, has burrs 25 formed in the opposite direction to the protruding direction of burrs 25 of cut end 23 on the rear side in the conveying direction, and the opposite side is formed into a drooping surface 26, so that the drooping surface 26 side is superimposed on ceramic plate 11 (see Figure 9).
[0029] (Joining process) The laminate of the ceramic plate 11 and the metal plate 21 thus laminated via the brazing material 41 is placed in a heating furnace under pressure, heated to a bonding temperature in a vacuum atmosphere, and then cooled, thereby bonding the ceramic plate 11 to the metal plate 21. In this case, the bonding conditions are, for example, pressing the laminate with a load of 0.03 MPa or more and 0.25 MPa or less, and bonding the ceramic plate 11 to the metal plate 21 for 10 minutes. -6 Pa or more 10 -3 Heating is performed in a vacuum atmosphere of 1 Pa or less at a bonding temperature of, for example, 790° C. or more and 850° C. or less for 1 to 60 minutes.
[0030] In this joining process, the brazing material 41 between the ceramic plate 11 and the metal plate 21 melts. In addition, since pressure is applied in the lamination direction, the brazing material 41 is spread between the ceramic plate 11 and the metal plate 21. As described above, the protruding lengths (distances from the scribe lines 12 that divide the dummy portions 13) L1 and L2 of the brazing material 41 and the metal plate 21 in the dummy portions 13 are set so that the molten brazing material 41 does not protrude from the outer edge of the thermally expanded metal plate 21 even if the molten brazing material 41 is spread. Therefore, as shown in FIG. 9, the outer edge of the spreading region of the molten brazing material 41 does not reach the outer edge of the metal plate 21 that expands due to thermal expansion, and is disposed inside the outer edge of the metal plate 21. Therefore, the molten brazing material 41 is prevented from flowing outward from the outer edge of the metal plate 21.
[0031] Furthermore, even if the spreading area of the molten brazing material 41 is large, the burrs 25 can block the outflow of the molten brazing material 41 at the cut end 23 of the metal plate 21 arranged with the burrs 25 facing the surface of the dummy portion 13, thereby preventing the brazing material 41 from adhering to the exposed portion of the dummy portion 13. If the outflow of the brazing material 41 to the exposed portion of the dummy portion 13 can be prevented, the brazing material 41 can also be prevented from creeping up onto the surface of the metal plate 21, preventing the occurrence of brazing stains and the like.
[0032] On the other hand, at the other cut end 24, the sides 15a, 15b, 22a, and 22b of the ceramic plate 11 and the metal plate 21 were aligned in the lamination process, but at the time of bonding, the metal plate 21 protrudes slightly from the ceramic plate 11 due to the difference in thermal expansion between the ceramic plate 11 and the metal plate 21, as shown in Fig. 9. Also, at the cut end 24, the sagging surface 26 of the metal plate 21 faces the surface of the ceramic plate 11. Therefore, excess molten brazing material 41 is stored between the metal plate 21 and the ceramic plate 11, and between the metal plates 21 protruding from the ceramic plate 11. In the portion where the ceramic plate 11 and the metal plate 21 are aligned, even if the molten brazing material 41 flows out onto the side surfaces, it solidifies in a lump shape, and therefore, creeping up onto the surface of the metal plate 21 is prevented.
[0033] (Etching process S4) Using two opposing corners PQ (see FIG. 6) exposed in the ceramic plate 11 as references, a resist film is printed on the metal plate 21, and then etching is performed to remove unnecessary portions of the metal plate 21. Specifically, the portions of the ceramic plate 11 above the scribe lines 12 are removed along the scribe lines 12 by a predetermined width, and the metal plate 21 that will become the circuit layer 3 is formed into a pattern shape required for the circuit layer 3. As described above, since the creeping up of the brazing material 14 onto the surface of the metal plate 21 is suppressed, a resist film can be reliably formed even near the cut end 23 of the metal plate 21, and the occurrence of etching defects is prevented.
[0034] (splitting process) Ceramic plate 11 is divided along scribe lines 12 exposed in the etching process to form a plurality of insulating circuit boards 1, each having a circuit layer 3 on one surface of ceramic substrate 2 and a heat dissipation layer 4 on the opposite surface. Dummy portions 13 are discarded.
[0035] Insulated circuit board 1 manufactured by this manufacturing method is prevented from the phenomenon of brazing material 41 creeping up onto the surface of metal plate 21 during the joining step, so that the portion of metal plate 21 that should be removed can be accurately etched in the subsequent etching step, preventing etching defects. In addition, since the brazing material 41 is prevented from creeping up onto the surface of metal plate 21, so-called brazing stains are prevented, and an insulating circuit board 1 with a good appearance can be obtained.
[0036] The present invention is not limited to the configuration of the above embodiment, and various changes can be made to the details of the configuration without departing from the spirit of the present invention. Although the ceramic plate is sized to be large enough to form a plurality of ceramic substrates, the number of ceramic substrates is not limited. The present invention can be applied to a ceramic plate that is large enough to form a single ceramic substrate. Moreover, the metal plate is formed by cutting a plate material of a predetermined width with a shear, but it may be formed by punching with a press. Furthermore, although the embodiment has been described as a power module substrate, the present invention is applicable to insulating circuit substrates other than power module substrates. EXAMPLES
[0037] A long plate material made of oxygen-free copper (C1020) with a purity of 99.99% by mass or more, 0.8 mm thick and 124 mm wide, was cut to a length of 172 mm using a shear to obtain a metal plate. Then, Ag-Ti brazing material was applied to one side of a ceramic plate (126 mm x 174 mm x 0.32 mm) made of silicon nitride (Si3N4) to a size of 120.2 mm x 168.2 mm x 0.010 mm, and the metal plate was laminated on top of it.
[0038] In this laminate, the load and temperature during joining were changed to examine the spreading rate of the brazing material, the joining reliability, and the creep-up of the brazing material. The spreading rate (%) of the brazing material was calculated by (area after drying of the brazing material paste before joining / area of the brazing material after joining) x 100. The area after drying of the brazing material paste before joining was calculated by measuring with an image dimension measuring device, and the area of the brazing material after joining was calculated by measuring the area where the brazing material was present with an ultrasonic flaw detection device. The bonding reliability was evaluated by using an ultrasonic flaw detector to observe the interface between the ceramic plate and the metal plate after bonding, and measuring the bonding area excluding the non-bonded areas shown in white from the binarized image. A bonding rate of 95% or more relative to the area of the metal plate was evaluated as "good", a bonding rate of 90% or more but less than 95% was evaluated as "good", and a bonding rate of less than 90% was evaluated as "bad".
[0039] The brazing material creep was evaluated as follows: "Good" if no brazing material stains were observed on the surface of the cut end of the metal plate; "Good" if brazing material stains were observed only in a limited area within 100 μm of the cut end; and "Poor" if brazing material stains were observed more than 100 μm from the cut end. If either the joint reliability or the brazing material creep-up was rated as "good", the overall evaluation was rated as "good", if either was "good", the overall evaluation was rated as "good", and if either was "bad", the overall evaluation was rated as "bad". The results are shown in Figure 10. In Figure 10, the top row of the brazing filler metal spreading rate at each load corresponds to a peak joining temperature of 840°C, the intermediate row corresponds to 825°C, and the lower row corresponds to 800°C. The evaluations for each row are also shown in the top, intermediate, and lower rows, respectively.
[0040] As can be seen from Figure 10, there is an appropriate brazing filler metal spreading ratio depending on the load and temperature conditions during joining. For example, when the load during joining is 0.03 MPa, the brazing filler metal spreading ratio at 825°C is 13.8%, and when the load during joining is 0.14 MPa, the brazing filler metal spreading ratio at 825°C is 16.6%, and good results are observed in terms of joint reliability and brazing filler metal creeping up, respectively. When the spreading ratios are smaller than these, good results are observed in terms of brazing filler metal creeping up, but the joint reliability is poor. Conversely, when the spreading ratios are larger than these, brazing filler metal creeping up is observed and the joint reliability is also poor. Therefore, if the area of the metal plates after joining is designed to be larger than the area of the brazing filler metal spread at this brazing filler metal spreading rate, an insulating circuit board can be obtained that is free of brazing filler metal creep-up and has good joining reliability.
[0041] Therefore, a ceramic plate was used that was 126mm x 174mm, a metal plate that was 124mm x 172mm, and the width of the dummy part of the ceramic plate was 3mm, and with the ceramic plate and metal plate positioned based on the two sides that make up one corner, the metal plate and the brazing material were placed on the dummy part and joined with the distance L2 from the scribe line that forms the dummy part to the cut end surface of the metal plate being 1.0mm, and the distance L1 from the scribe line to the outer edge of the brazing material being 0.1mm. Ag-Ti brazing material was used as the brazing material, and the load during joining was 0.14MPa and the temperature was 825℃. As a result, an insulating circuit board with good joint reliability was obtained without any creep-up of the brazing material. [Explanation of symbols]
[0042] 1. Insulated circuit board 2. Ceramic substrate 3 circuit layers 4 Heat dissipation layer 11 Ceramic plate 12 Scribe Line 13 Dummy section 14 Corner Areas 15a and 15b 16 Cutout 21 Metal plate 21a surface 21b Back side Area 22a~22d 23,24 Cut end 25 Bali 26 Droopy Face 27 Fracture surface 28 Shear Surface 31 Board material 32 Shah 33 Transport platform 35 Upper blade 36 Lower blade
Claims
1. A method for manufacturing an insulating circuit board, comprising: a lamination step of laminating a rectangular ceramic plate, on which a dividing scribe line is formed, and a metal plate via a brazing material; a joining step of heating the laminate to melt the brazing material and then cooling to join the ceramic plate and the metal plate; an etching step of etching the metal plate after the joining step to remove unnecessary portions; and a division step of dividing the ceramic plate along the scribe lines after the etching step to form a plurality of insulating circuit boards, In the lamination step, one corner of the ceramic plate and one corner of the metal plate are aligned to each other, and a dummy portion of the ceramic plate is formed on two sides that constitute a corner opposite to the one corner, The method for manufacturing an insulating circuit board, wherein in the joining step, an outer edge of a spreading area of the molten brazing material in the dummy portion is positioned inside an outer edge that spreads due to thermal expansion of the metal plate.
2. 2. The method for manufacturing an insulating circuit board according to claim 1, further comprising: a metal plate forming step of cutting the metal plate from a plate material; and in the laminating step, a surface of a cut end portion of the metal plate having a burr is laminated onto a surface of the dummy portion of the ceramic plate.
3. 3. The method for manufacturing an insulating circuit board according to claim 2, wherein the plate material is a long material set to a width of the metal plate, and in the metal plate forming process, the plate material is cut to the length of the metal plate by a shear while being intermittently transported in the longitudinal direction to form the metal plate, and in the lamination process, a cut end portion of the metal plate on a rear side in the transport direction in the metal plate forming process is placed on the dummy portion, and a surface of the cut end portion having a burr is overlapped on a surface of the dummy portion.
Citation Information
Patent Citations
Control system for shift velocity pattern of cargoohandling machine
JP1981042808A
Manufacture intermediate of power module substrate, and power module substrate manufacturing method
JP2010114166A
Manufacturing method of substrate for power module
JP2010147068A
Substrate for power module and method for manufacturing the same
JP2016039163A
Manufacturing method for ceramic-metal joint material, manufacturing apparatus and ceramic-metal joint material
JP2019127408A