Composite nonwoven fabric and articles containing the same

JP7575476B2Active Publication Date: 2024-10-29TORAY ADVANCED MATERIALS KOREA INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022558253
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2021-03-24
Publication Date
2024-10-29
Estimated Expiration
2041-03-24

AI Technical Summary

Benefits of technology

【0014】 本発明の一具現例による複合不織布は、空気中の微細粒子をフィルタリングするための素材として適用が可能である。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575476000002
    Figure 0007575476000002
  • Figure 0007575476000001
    Figure 0007575476000001
Patent Text Reader

Abstract

The present invention relates to a composite nonwoven fabric and an article including the same, wherein the nonwoven fabric includes an electrically charged meltblown nonwoven fabric layer and a spunbond nonwoven fabric layer on one or both sides thereof, and has a fine dust removal performance retention rate of 80% or more, as expressed by the following mathematical formula 1: [Number 1] Fine dust removal performance retention rate (%) = (fine dust removal efficiency after accelerated aging treatment) / (fine dust removal efficiency before accelerated aging treatment) x 100 In Equation 1, the fine dust is an aerosol containing sodium chloride dispersed in the air, and the accelerated aging treatment means that the composite nonwoven fabric is stored at a temperature of 70°C for 3 days.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite nonwoven fabric and an article including the same, and more particularly to a composite nonwoven fabric having excellent mechanical properties and fine dust removing function, and an article including the same. [Background technology]

[0002] In the case of a mask for removing fine dust, it is constructed by combining inner and outer covering materials with a filter material in the center that filters out fine dust in multiple layers.

[0003] As the filter layer, an electrically charged meltblown nonwoven fabric is mainly used. The meltblown nonwoven fabric has low dimensional stability due to low mechanical strength and high flexibility, and is easily deformed by external impact or friction. Therefore, in order to protect the meltblown nonwoven fabric layer and impart dimensional stability, a nonwoven fabric having high mechanical properties such as dimensional stability and tensile strength is laminated on both sides or one side of the meltblown nonwoven fabric layer to form a mask, and a spunbond nonwoven fabric is mainly laminated through a separate lamination process.

[0004] In addition, spunbond nonwoven fabrics, which are generally applied as inner and outer covering materials on one or both sides of electrostatically treated meltblown materials, have thick filaments and large pores, so they have almost no fine dust removal efficiency and only have the function of imparting shape stability. Therefore, in a multi-layer mask nonwoven fabric configuration, fine dust is filtered only by the filter layer located in the center, so there is a problem that fine dust is concentrated on the filter layer and the filtering efficiency decreases over time, and especially in industrial sites where masks must be worn for long periods of time, such problems also affect the respiratory safety of users.

[0005] In addition, the nonwoven fabrics used as the inner and outer coating layers are mainly laminated by ultrasonic fusion along the outer shape of the mask, so that the structure of the electrostatically treated meltblown nonwoven fabric of the inner layer is changed during the fusion process, resulting in a decrease in filtering performance. Summary of the Invention [Problem to be solved by the invention]

[0006] One embodiment of the present invention provides a composite nonwoven fabric having excellent mechanical properties and fine dust removing function.

[0007] Another embodiment of the present invention provides an article comprising the nonwoven fabric. [Means for solving the problem]

[0008] One aspect of the present invention is The present invention comprises an electrically charged meltblown nonwoven fabric layer and a spunbond nonwoven fabric layer on one or both sides of the electrically charged meltblown nonwoven fabric layer, Provided is a composite nonwoven fabric having a fine dust removal performance retention rate of 80% or more, as represented by the following mathematical formula 1: [Formula 1] Fine dust removal performance retention rate (%) = (Fine dust removal efficiency after accelerated aging treatment) / (Fine dust removal efficiency before accelerated aging treatment) x 100 In Equation 1, the fine dust is an aerosol containing sodium chloride dispersed in the air, and the accelerated aging treatment means that the composite nonwoven fabric is stored at a temperature of 70° C. for 3 days.

[0009] The composite nonwoven fabric has a pressure loss maintenance rate, represented by the following formula 2, of 90% or more: [Formula 2] Pressure loss maintenance rate (%) = (pressure loss after accelerated aging treatment) / (pressure loss before accelerated aging treatment) x 100 In Equation 2, the pressure loss is measured using an aerosol containing sodium chloride dispersed in the air, and the accelerated aging treatment means that the composite nonwoven fabric is stored at a temperature of 70° C. for 3 days.

[0010] The composite nonwoven fabric also has a fine dust removal rate of 18 to 99% after the accelerated aging treatment.

[0011] The electrostatically treated meltblown nonwoven layer and the spunbond nonwoven layer each, independently of the other, comprise a nonconductive polymer, which may also comprise a polyolefin, polystyrene, polycarbonate, polyester, polyamide, copolymers thereof, or combinations thereof.

[0012] The content of the electrically charged meltblown nonwoven fabric layer is 3 to 50 parts by weight based on 100 parts by weight of the total weight of the composite nonwoven fabric.

[0013] Another aspect of the present invention is An article is provided comprising the composite nonwoven fabric. The article can also be a mask for removing fine dust, a filter for air purification, or a filter for an air conditioner. Effect of the Invention

[0014] The composite nonwoven fabric according to an embodiment of the present invention can be used as a material for filtering fine particles in the air.

[0015] In addition, when the composite nonwoven fabric is combined with an electrically charged meltblown filter layer that is used as a filter layer in an existing mask, it is possible to prevent contamination of the filter layer, extend its lifespan, and have excellent shape stability. By forming a multi-layered filter layer, it is possible to improve the performance of the entire mask and the stability of removal efficiency.

[0016] In addition, the composite nonwoven fabric can be used to remove various types of dust, fine dust, bacteria, etc., and is applicable not only to medical masks but also to various household, vehicle, and industrial air conditioners and air cleaners that require air purification. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic diagram of a composite nonwoven fabric manufacturing apparatus used to continuously manufacture a composite nonwoven fabric according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, a composite nonwoven fabric according to an embodiment of the present invention will be described in detail.

[0019] In this specification, the term "non-woven fabric composite" refers to a non-woven fabric in which two or more types of non-woven fabrics are manufactured in one continuous process, rather than a non-woven fabric laminate manufactured by a separate lamination process after manufacturing two or more types of non-woven fabrics separately. The "composite non-woven fabric" is also called a "monolithic non-woven fabric." The composite non-woven fabric has stronger interlayer bonding and excellent shape stability and filtration performance compared to the non-woven fabric laminate.

[0020] In this specification, the "electrically charged meltblown nonwoven fabric layer" is also one produced by a continuous process during the production of a composite nonwoven fabric. Specifically, the "electrically charged meltblown nonwoven fabric layer" is also produced by carrying out "production of a meltblown nonwoven fabric" and "electrically charging" sequentially or simultaneously in a continuous process.

[0021] A composite nonwoven fabric according to one embodiment of the present invention includes an electrically charged meltblown nonwoven fabric layer and a spunbond nonwoven fabric layer on one or both sides thereof.

[0022] The nonwoven fabrics included in the composite nonwoven fabric may be bonded to each other by thermal fusion rather than ultrasonic fusion.

[0023] The composite nonwoven fabric is characterized by having a fine particle collection function due to the inclusion of an electrically charged meltblown nonwoven fabric layer. However, conventional spunbond-meltblown multi-layer nonwoven fabrics have few average pores, at the level of several tens of μm, and therefore have almost no function of removing fine particles at the level of 0.1 to 0.6 μm.

[0024] In addition, the composite nonwoven fabric has a fine dust removal performance retention rate of 80% or more, as represented by the following mathematical formula 1: [Formula 1] Fine dust removal performance retention rate (%) = (Fine dust removal efficiency after accelerated aging treatment) / (Fine dust removal efficiency before accelerated aging treatment) x 100 In Equation 1, the fine dust is an aerosol containing sodium chloride dispersed in the air, and the accelerated aging treatment means that the composite nonwoven fabric is stored at a temperature of 70° C. for 3 days.

[0025] The fine dust removal performance retention rate of 80% or more means that the filtration performance of the composite nonwoven fabric is maintained at a high level for a long period of time.

[0026] In addition, the composite nonwoven fabric has a pressure loss maintenance rate represented by the following formula 2 of 90% or more. [Formula 2] Pressure loss maintenance rate (%) = (pressure loss after accelerated aging treatment) / (pressure loss before accelerated aging treatment) x 100 In Equation 2, the pressure loss is measured using an aerosol containing sodium chloride dispersed in the air, and the accelerated aging treatment means that the composite nonwoven fabric is stored at a temperature of 70° C. for 3 days.

[0027] The pressure loss retention rate of 90% or more means that the shape stability (ie, structural stability) of the composite nonwoven fabric is maintained at a high level for a long period of time.

[0028] In addition, the composite nonwoven fabric has a fine dust removal rate of 18 to 99% after the accelerated aging treatment. If the fine dust removal rate after the accelerated aging treatment is within this range, the filtration performance, shape stability, and productivity of the composite nonwoven fabric can all be maintained at high levels.

[0029] The electrostatically treated meltblown nonwoven layer and the spunbond nonwoven layer each, independently, also comprise a non-conductive polymer.

[0030] The non-conductive polymer may also include polyolefins, polystyrenes, polycarbonates, polyesters, polyamides, copolymers thereof, or combinations thereof.

[0031] The polyolefin may include polyethylene, polypropylene, poly-4-methyl-1-pentene, polyvinyl chloride, or a combination thereof.

[0032] The polyester may also include polyethylene terephthalate, polylactic acid, or a combination thereof.

[0033] The electrically charged meltblown nonwoven layer and the spunbond nonwoven layer each independently further comprise an additive.

[0034] The additives may also include pigments, light stabilizers, primary antioxidants, secondary antioxidants, metal deactivators, hindered amines, hindered phenols, fatty acid metal salts, triester phosphites, phosphates, fluorine-containing compounds, nucleating agents, or combinations thereof.

[0035] In one embodiment, the antioxidant can also function as a charge enhancer. Possible charge enhancers include thermally stable organic triazine compounds, oligomers, or combinations thereof, which compounds or oligomers contain at least one nitrogen atom other than the nitrogen in the triazine ring.

[0036] For example, charge enhancers for improving charging properties are disclosed in U.S. Patent Nos. 6,268,495, 5,976,208, 5,968,635, 5,919,847, and 5,908,598. For example, the charge enhancers may include hindered amine-based additives, triazine additives, or combinations thereof.

[0037] As another example, the charge enhancer may include poly[((6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidyl)imino)] (CHIMASSORB 944, available from BASF), (1,6-hexanediamine·N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl) polymer with 2,4,6-trichloro-1,3,5-triazine, reaction product of N-butyl-1-butanamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine) (CHIMASSORB 2020, available from BASF), or a combination thereof.

[0038] The charge enhancers may also be N-substituted amino aromatic compounds, particularly tri-amino substituted compounds, such as 2,4,6-trianylino-p-(carbo-2'-ethylhexyl-1'-oxy)-1,3,5-triazine (UVINULT-150, BASF). Another charge enhancer is 2,4,6-tris-(octadecylamino)-triazine, also known as tristearylmelamine ("TSM").

[0039] The content of the charge enhancer is 0.25 to 5 parts by weight based on 100 parts by weight of the total weight of the meltblown nonwoven fabric layer. If the content of the charge enhancer is within this range, not only can the high level of charging performance targeted by the present invention be obtained, but also the spinnability is good, the strength of the nonwoven fabric is maintained high, and it is advantageous in terms of cost.

[0040] In addition to the above additives, the composite nonwoven fabric may further contain commonly known additives such as a heat stabilizer and a weathering agent.

[0041] The content of the electrically charged meltblown nonwoven fabric layer is 3 to 50 parts by weight based on 100 parts by weight of the total weight of the composite nonwoven fabric. If the content of the electrically charged meltblown nonwoven fabric layer is within this range, a composite nonwoven fabric having excellent filtration performance, shape stability, and durability can be obtained.

[0042] The composite nonwoven fabric has a basis weight (mass per unit area) of 10 to 500 g / m 2 , for example, 20 to 100 g / m 2 It is also in the range.

[0043] Hereinafter, a method for producing a composite nonwoven fabric according to an embodiment of the present invention will be described in detail.

[0044] A method for manufacturing a composite nonwoven fabric according to an embodiment of the present invention includes a step of continuously forming a spunbond nonwoven fabric layer (S10), and a step of continuously forming a meltblown nonwoven fabric layer on the spunbond nonwoven fabric layer (S20).

[0045] The spunbond nonwoven fabric layer continuous formation step (S10) is a step of forming a fiber yarn by melt extruding, cooling and stretching a thermoplastic nonconductive polymer, and then laminating the fiber yarn on a screen belt to form a web.

[0046] The meltblown nonwoven fabric layer continuous formation step (S20) is a step of forming a fiber yarn by melt extruding a thermoplastic nonconductive polymer and an electrostatic performance improver, stretching the polymer with hot air, and cooling the polymer to form a fiber yarn, and then laminating the fiber yarn on the spunbond web formed in the spunbond nonwoven fabric layer continuous formation step (S10) to form a web.

[0047] Specifically, the step of continuously forming the meltblown nonwoven fabric layer (S20) includes a step of continuously forming free fibers using a nonconductive polymer (S20-1), a step of continuously spinning the free fibers (S20-2), a step of continuously spraying a polar solvent (e.g., water) onto the free fibers to continuously charge the free fibers (S20-3), and a step of continuously accumulating the free fibers to continuously form the meltblown nonwoven fabric (S20-4).

[0048] The free fiber continuous charging step (S20-3) is also performed by continuously injecting the polar solvent together with a gas (eg, air).

[0049] The following will describe in detail why the free fiber continuous charging step (S20-3) is different from the conventional techniques and has a significant effect.

[0050] (1) In general, the methods for electrostatically treating the nonwoven fabric during the meltblowing process include a method of electrostatically treating the nonwoven fabric through friction between a polar solvent and the filaments being melt-spun as in U.S. Patent No. 6,375,886, and a method of electrostatically treating the nonwoven fabric through friction between the nonwoven fabric and the water as the nonwoven fabric is immersed in a polar solvent and water is passed through the nonwoven fabric by a suction device as in U.S. Patent No. 6,969,484. These methods of electrostatically treating the nonwoven fabric using a polar solvent require a separate post-process of drying the polar solvent after the electrostatic treatment, and therefore it is basically impossible to laminate or composite the nonwoven fabric in a continuous process. U.S. Patent No. 6,375,886 and U.S. Patent No. 6,969,484 are incorporated herein by reference in their entirety.

[0051] (2) U.S. Patent No. 5,227,172 discloses a method in which a high potential difference is applied between a melt-blown die and a collector, and the melt-spun resin is induced-charged by the surrounding electric field while being filamentized, and this method can obtain a melt-blown nonwoven fabric that is charged without a separate post-processing process. However, such a nonwoven fabric that is induced-charged by a potential difference exhibits a phenomenon in which the charging efficiency is rapidly reduced due to heat or the surrounding environment, and therefore has a disadvantage in that it is difficult to apply it to applications that require long-term storage during the sales process, such as fine dust removal masks, or that require a long service life, such as air purifying filters. U.S. Patent No. 5,227,172 is incorporated herein by reference in its entirety.

[0052] The inventors have developed an electrostatic charging device that sprays a polar solvent together with air onto a meltblown nonwoven fabric layer in a two-fluid form, and causes the polar solvent particles, which have sufficient kinetic energy with a small amount of spraying, to rub against the filaments being melt-spun, resulting in a highly efficient triboelectric effect.The device is characterized in that a small amount of spraying causes the solvent to be sufficiently heated and evaporated by heated air within the DCD (die to collector distance) section, eliminating the need for a separate drying facility.This feature allows the device to be combined with the nonwoven fabric manufacturing process to produce a composite nonwoven fabric by continuous lamination.

[0053] The nonwoven fabric obtained by electrostatically treating the meltblown nonwoven fabric is in a permanently polarized state in which negative and positive charges exist semi-permanently, and such a nonwoven fabric is called an electret nonwoven fabric.

[0054] As described above, the method for producing the composite nonwoven fabric does not include a separate drying step for removing the polar solvent sprayed in the free fiber continuous charging step (S20-3).

[0055] Also, as described above, the polar solvent continuously sprayed in the free fiber continuous charging step (S20-3) can be continuously heated and evaporated by the heated air in the DCD section of the composite nonwoven fabric manufacturing apparatus.

[0056] The method for producing the composite nonwoven fabric may further include the step of continuously forming another spunbond nonwoven fabric layer on the meltblown nonwoven fabric layer (S30).

[0057] The method for producing the composite nonwoven fabric may further include, after the step of continuously forming the meltblown nonwoven fabric layer (S20) or after the step of continuously forming another spunbonded nonwoven fabric layer (S30), a step of continuously heat-compressing the spunbonded nonwoven fabric layers to one or both sides of the meltblown nonwoven fabric layer (S40).

[0058] Hereinafter, an article according to an embodiment of the present invention will be described in detail.

[0059] An article according to one embodiment of the present invention includes the nonwoven laminate described above.

[0060] The article can also be a mask for removing fine dust, a filter for air purification, or a filter for an air conditioner. EXAMPLES

[0061] The present invention will be described in more detail below through examples. These examples are provided to more specifically explain the present invention, and the scope of the present invention is not limited to these examples.

[0062] Example 1: Preparation of composite nonwoven fabric The polymer for forming the spunbond nonwoven layer (SB) was a propylene homopolymer (H7900 (LG Chem)) with a melt index (MI) of 34g / 10min, and the polymer for forming the meltblown nonwoven layer (MB) was a resin (H7910 (LG Chem)) with a melt flow index (MFR) of 1,000g / 10min. The polymer for forming the meltblown nonwoven layer (MB) was added with 0.5wt% of Chimasorb 944, a hindered amine light stabilizer. Then, a composite nonwoven fabric in the form of spunbond-meltblown-spunbond (SMS) was continuously produced using a composite nonwoven fabric manufacturing apparatus as shown in Figure 1. Specifically, the meltblown nonwoven fabric layer (MB) is continuously charged by contacting with water together with air through a two-fluid nozzle in the composite nonwoven fabric manufacturing equipment, and then laminated on top of the spunbond nonwoven fabric layer (SB), and another spunbond nonwoven fabric layer (SB) is laminated on top of the meltblown nonwoven fabric layer (MB). As a result, an SMS nonwoven fabric laminate is obtained. The SMS nonwoven fabric laminate is then subjected to a heat pressing process between a roll having an embossed pattern and a roll with no irregularities, to produce a composite nonwoven fabric. Here, the overall basis weight of the SMS composite nonwoven fabric is 100 gsm (g / m 2) and the basis weight of the double meltblown nonwoven layer (MB) was adjusted to 22 gsm.

[0063] Example 2: Preparation of composite nonwoven fabric The SMS composite nonwoven fabric was manufactured in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 80 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 30 gsm.

[0064] Example 3: Preparation of composite nonwoven fabric An SMS composite nonwoven fabric was prepared in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 61 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 15 gsm.

[0065] Example 4: Preparation of composite nonwoven fabric An SMS composite nonwoven fabric was prepared in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 55 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 13 gsm.

[0066] Example 5: Preparation of composite nonwoven fabric An SMS composite nonwoven fabric was prepared in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 50 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 25 gsm.

[0067] Example 6: Preparation of composite nonwoven fabric An SMS composite nonwoven fabric was prepared in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 35 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 12 gsm.

[0068] Example 7: Preparation of composite nonwoven fabric An SMS composite nonwoven fabric was prepared in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 35 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 8 gsm.

[0069] Example 8: Preparation of composite nonwoven fabric An SMS composite nonwoven fabric was prepared in the same manner as in Example 1, except that the total basis weight of the SMS composite nonwoven fabric was adjusted to 20 gsm and the basis weight of the meltblown nonwoven fabric layer (MB) was adjusted to 3 gsm.

[0070] Comparative Example 1: Production of meltblown single nonwoven fabric A meltblown single nonwoven fabric was produced in the same manner as in Example 2, except that the spunbond nonwoven fabric layer (SB) was omitted.

[0071] Comparative Example 2: Production of composite nonwoven fabric An SMS composite nonwoven fabric was produced in the same manner as in Example 3, except that the meltblown nonwoven fabric layer (MB) was not subjected to an electrostatic treatment.

[0072] Comparative Example 3: Production of meltblown single nonwoven fabric A meltblown single nonwoven fabric was produced in the same manner as in Example 3, except that the spunbond nonwoven fabric layer (SB) was omitted.

[0073] Comparative Example 4: Production of composite nonwoven fabric An SMS composite nonwoven fabric was produced in the same manner as in Example 7, except that the meltblown nonwoven fabric layer (MB) was not subjected to an electrostatic treatment.

[0074] Comparative Example 5: Production of composite nonwoven fabric An SMS composite nonwoven fabric was produced in the same manner as in Example 8, except that the meltblown nonwoven fabric layer (MB) was not subjected to an electrostatic treatment.

[0075] Comparative Example 6: Production of nonwoven fabric laminate Two spunbond nonwoven layers (SB) and one meltblown nonwoven layer (MB) were separately manufactured and then laminated together to manufacture an SMS nonwoven laminate. The meltblown nonwoven layer (MB) was electrically charged by the method disclosed in U.S. Patent No. 6,375,886. The total basis weight of the SMS nonwoven laminate was set to 100 gsm (g / m2) in the same manner as in Example 1. 2 ) and the basis weight of the double meltblown nonwoven layer (MB) was adjusted to 22 gsm.

[0076] Reference Example 1: Production of nonwoven fabric laminate An SMS composite nonwoven fabric was produced in the same manner as in Example 1, except that the meltblown nonwoven fabric layer (MB) was charged by the charging treatment method disclosed in U.S. Patent No. 5,227,172.

[0077] Evaluation example: Evaluation of the physical properties of nonwoven fabric The fine dust removal performance retention rate and pressure loss retention rate of each of the nonwoven fabrics produced in the above-mentioned Examples 1 to 8, Comparative Examples 1 to 6, and Reference Example 1 were evaluated by the following methods, and the results are shown in Table 1 below. (1) Measuring device: The TSI-8130 model from TSI was used. (2) Aerosol formation: The measuring device contacts an aqueous sodium chloride solution with air, evaporates the water, and measures the sodium chloride dispersed in the air, with an average particle size of 0.3 μm and a sodium chloride particle concentration of 18.5 mg / m 3 An aerosol was formed. (3) Aerosol removal efficiency evaluation: The aerosol permeation flow rate was 95 L / min, and the evaluation area of ​​the nonwoven fabric was 100 cm 2 It was. (4) Pressure loss evaluation: The aerosol permeation flow rate was 30 L / min, and the evaluation area of ​​the nonwoven fabric was 100 cm 2 It was. (5) Accelerated aging treatment: The nonwoven fabric was stored in a dry oven at 70° C. for 3 days. (6) The aerosol removal efficiency and pressure drop were evaluated before and after the accelerated aging treatment. (7) The fine dust removal performance maintenance rate and the pressure loss maintenance rate were calculated using the above formula 1 or 2.

[0078] [Table 1]

[0079] Referring to Table 1, the composite nonwoven fabrics prepared in Examples 1 to 8 had a fine dust removal performance retention rate and a pressure loss retention rate of 80% or more, respectively, and a fine dust removal rate (i.e., aerosol removal rate) after accelerated aging treatment of 18% or more.

[0080] However, the nonwoven fabrics produced in Comparative Examples 1 and 3 had a pressure loss retention rate of 90% or more and a fine dust removal rate of 18% or more after accelerated aging treatment, but the fine dust removal performance retention rate was shown to be less than 80%.

[0081] In addition, the nonwoven fabrics produced in Comparative Examples 2, 4 and 5 had a fine dust removal performance retention rate of 80% or more and a pressure loss retention rate of 90% or more, but the fine dust removal rate after accelerated aging treatment was less than 18%.

[0082] In addition, the nonwoven fabric produced in Comparative Example 6 had a pressure loss retention rate of 90% or more and a fine dust removal rate of 18% or more after accelerated aging treatment, but the fine dust removal performance retention rate was shown to be less than 80%.

[0083] In addition, the nonwoven fabric produced in Reference Example 1 had a pressure loss retention rate of 90% or more, and a fine dust removal rate after accelerated aging treatment of 18% or more, but the fine dust removal performance retention rate was shown to be less than 80%.

[0084] The present invention has been described with reference to the drawings and embodiments, but they are merely illustrative, and those skilled in the art will understand that various modifications and equivalent embodiments are possible therefrom. Therefore, the true technical scope of the present invention is defined by the technical ideas of the claims.

Claims

1. A composite nonwoven fabric comprising a meltblown nonwoven fabric layer and spunbond nonwoven fabric layers on both sides of the meltblown nonwoven fabric layer, The meltblown nonwoven fabric layer is electrically charged by contacting the layer with water together with air through a two-fluid nozzle in a composite nonwoven fabric manufacturing device, The composite nonwoven fabric refers to a monolithic nonwoven fabric manufactured according to a method in which two or more types of nonwoven fabrics are manufactured and integrally formed in one continuous process, and is not a nonwoven fabric laminate manufactured by separately manufacturing two or more types of nonwoven fabrics and then performing a separate post-lamination process.

2. 2. The composite nonwoven fabric of claim 1, wherein the electrostatically treated meltblown nonwoven layer and the spunbond nonwoven layer each, independently of the other, comprise a nonconductive polymer, the nonconductive polymer comprising a polyolefin, a polystyrene, a polycarbonate, a polyester, a polyamide, a copolymer thereof, or a combination thereof.

3. 2. The composite nonwoven fabric according to claim 1, wherein the content of the electrically charged meltblown nonwoven fabric layer is 3 to 50 parts by weight based on 100 parts by weight of the total weight of the composite nonwoven fabric.

4. An article comprising the composite nonwoven fabric of any one of claims 1 to 3.

5. The article according to claim 4 , wherein the article is a mask for removing fine dust, a filter for air purification, or a filter for an air conditioner.

Citation Information

Patent Citations

  • Method for producing electret processed article

    JP2002161467A

  • Infection prevention mask

    JP2005124777A

  • Electret web with charge-enhancing additives

    JP2011506783A

  • JPP4133830B

  • Filter media for purifying air to be introduced into internal combustion engine of vehicle, and method for fabrication the same