Three-way catalytic conversion system for engine exhaust purification treatment and its application
The three-way catalyst conversion system addresses catalyst degradation by using high-temperature resistant oxidation catalysts to pre-process reducing components, ensuring efficient conversion of HC, CO, and NOx while maintaining optimal reaction temperatures.
Patent Information
- Application Number
- JP2023514060
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Existing three-way catalytic conversion systems face performance degradation due to high temperatures generated by excessive combustion of reducing components like HC and CO, leading to catalyst deactivation and reduced efficiency in removing harmful gases such as NOx.
A three-way catalyst conversion system comprising an oxidation section with high-temperature resistant oxidation catalysts and a three-way conversion section, where the oxidation catalysts are located downstream of the engine to pre-process reducing components, followed by the three-way conversion section to maintain optimal reaction temperatures and prevent excessive heat exposure.
The system effectively reduces combustion-induced high temperatures, maintaining catalyst performance and efficiency in converting HC, CO, and NOx, ensuring compliance with emission standards by avoiding catalyst degradation and optimizing reaction conditions.
Smart Images

Figure 0007575577000001 
Figure 0007575577000002 
Figure 0007575577000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an engine exhaust Post-processing System The present invention relates to the field of catalytic converters, and more particularly to three-way catalytic converter systems and their applications for engine exhaust purification treatment. [Background technology]
[0002] Waste gas (exhaust) emitted from an automobile engine operating at a stoichiometric air-fuel ratio contains harmful gases such as HC, CO, and NOx. These gases are generally removed by a three-way catalytic conversion system (TWC system). Current TWC systems rely on the three-way catalytic conversion function of the TWC to convert the HC, CO, and NOx in the exhaust gas into carbon dioxide (CO2), nitrogen gas (N2), and water, thereby achieving the removal of HC, CO, and NOx. The basic components of the three-way catalyst are mainly a porous substrate, an oxygen storage material and a precious metal, the precious metal is mainly platinum (Pt), palladium (Pd) and rhodium (Rh), the precious metal is the active component of the TWC, where the main function of Pt and Pd is to accelerate the oxidation of hydrocarbons (HC) and carbon monoxide (CO) under the condition of lean exhaust (air-fuel ratio λ>1, exhaust oxygen enriched), and to catalyze the steam reforming of HC and the water-gas reaction of CO to remove HC and CO under the condition of rich exhaust (λ<1, exhaust oxygen lean), the main function of rhodium (Rh) is to convert nitrogen oxides (NOx) under the condition of stoichiometric air-fuel ratio (λ=1) and rich (λ<1) exhaust, the basic function of the oxygen storage material is to adjust the value of λ in a small range and reduce the deviation from λ=1 to maintain the three-way reaction under the condition of stoichiometric air-fuel ratio, the oxygen storage material generally needs to be combined with a precious metal to effectively perform its function, the porous substrate is generally PorousIt is an alumina (Al2O3)-based material with a large specific surface area, which mainly functions as a loading material to disperse precious metals and ensure the performance of the catalyst, such as activity and stability. Since Rh is prone to react with Al2O3 at high temperatures and become ineffective, in the TWC catalyst, in order to avoid the catalyst from becoming ineffective, Rh is supported on an oxygen storage material, and the oxygen storage material is loaded on the surface of the alumina-based material, thereby achieving the purpose of separating Rh and Al2O3.
[0003] Generally, in the operation process of the TWC, oxygen reacts rapidly with reducing components such as HC and CO, releasing a large amount of heat and rapidly increasing the TWC temperature; especially when three-way catalytic conversion treatment is performed on exhaust gas with a high oxygen content (such as exhaust gas from an engine operated at a theoretical air-fuel ratio with an oxygen volume content of more than 1%, or even more than 2-3%), the reaction becomes more vigorous and the TWC temperature increases. On the one hand, a large amount of combustion reaction occupies most of the TWC space at the inlet end of the engine exhaust gas of the TWC, and only the rear end part of the TWC can play the role of three-way conversion (i.e., most of the TWC is used for burning reducing components such as HC and CO and consuming oxygen, and only a small part of the TWC is used for three-way conversion). catalystOn the other hand, the high temperature generated by the combustion is generally as high as 950°C or higher, which exceeds the conversion temperature window of the TWC (generally 350-700°C), which is unfavorable to the three-way conversion reaction and affects the conversion efficiency of harmful gases such as NOx. In addition, the high temperature generated by the combustion in the TWC makes the TWC operate at an extremely high temperature (900-980°C). Operating at an extremely high temperature (for example, 950°C) for a long time accelerates the aging of the TWC and significantly reduces the function of the TWC. The main reasons for this are: (1) the pores of the porous substrate collapse and the surface In particular, some of the precious metals are buried, reducing the number of catalytically active sites; (2) the oxygen storage material ages, its combination with the precious metals weakens, and its λ-regulating function is weakened. The water-gas shift reaction of CO and the steam reforming function of HC are reduced, and its protective function for Rh is reduced. Rh is easily deactivated through contact reaction with Al2O3, significantly reducing the catalyst's ability to reduce NOx; and (3) the precious metal particles grow, reducing the three-way catalytic activity of the TWC. Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides a three-way catalytic conversion system for engine exhaust gas purification treatment and its application, which at least solves the problem in the prior art that the temperature becomes too high due to the long-term catalytic combustion of reducing components such as HC and CO with excess TWC, resulting in significant impairment of catalyst performance or limited function. [Means for solving the problem]
[0005] A three-way catalytic conversion system for engine exhaust purification treatment provided by one embodiment of the present invention includes an oxidation section containing a high-temperature resistant oxidation catalyst and a three-way conversion section containing a three-way catalyst, the oxidation catalyst being used to catalyze an oxidation reaction between reducing components in the exhaust gas and oxygen, the oxidation section being located downstream of the engine, and the three-way conversion section being located downstream of the oxidation section.
[0006] According to one embodiment of the present invention, the oxidation catalyst includes a first alumina-based material and palladium supported on the first alumina-based material, and the first alumina-based material has a pore volume of 0.8 cc / g to 1.2 cc / g and a specific surface area of 130 to 180 m. 2 / g, and the specific surface area of the first alumina-based material after aging at 1200±100° C. for 4±0.5 hours is 60 m 2 / g or more.
[0007] According to one embodiment of the present invention, the first alumina-based material comprises gamma-alumina.
[0008] According to one embodiment of the present invention, the first alumina-based material contains a rare earth element, and the mass content of the rare earth element in the first alumina-based material is 0 to 7%.
[0009] According to one embodiment of the present invention, the mass content of palladium in the oxidation catalyst is 0.06 to 1.0%.
[0010] According to one embodiment of the present invention, the number of the oxidation portions is at least two, and the distance between every two adjacent oxidation portions is not less than 150 mm.
[0011] According to one embodiment of the present invention, the oxidation section includes a first support and a first active layer located on a surface of the first support, and the oxidation catalyst is present in the first active layer.
[0012] According to one embodiment of the present invention, the first active layer further includes an adhesive and / or a modification aid, and satisfies at least one of the following characteristics: the adhesive includes aluminum paste and / or silica gel; the modification aid includes a cerium material and / or a zirconium material; and the mass content of the oxidation catalyst in the first active layer is 85% to 98%, with the remainder being the adhesive and / or the modification aid.
[0013] According to one embodiment of the present invention, the material of the first support includes at least one of ceramic and metal.
[0014] According to one embodiment of the present invention, the oxidation catalyst includes a first alumina-based material and palladium supported on the first alumina-based material, and a ratio of a mass of palladium in the oxidation catalyst to a volume of the first support is (3 to 50) grams:cubic feet.
[0015] According to one embodiment of the present invention, the ratio of the mass of the first active layer to the volume of the first support is (100-200) grams:1 liter.
[0016] According to one embodiment of the present invention, the three-way conversion section further includes a second support and a second active layer located on the surface of the second support, and the three-way catalyst is present in the second active layer.
[0017] According to one embodiment of the present invention, the second active layer further includes an adhesive and / or a modifying aid, and satisfies at least one of the following characteristics: the adhesive includes aluminum paste and / or silica gel; the modifying aid includes a cerium material and / or a zirconium material; and the mass content of the three-way catalyst in the second active layer is 85% to 98%, with the remainder being the adhesive and / or the modifying aid.
[0018] According to one embodiment of the present invention, the three-way catalyst comprises a porous substrate, an oxygen storage material and a precious metal, the precious metal comprises platinum, rhodium and palladium, the oxygen storage material is filled in the porous substrate, the rhodium is supported on the oxygen storage material, and the precious metal other than rhodium is supported on the porous substrate or the oxygen storage material.
[0019] According to one embodiment of the present invention, the oxygen storage material comprises CeZrO.
[0020] According to one embodiment of the present invention, the porous substrate comprises a second alumina-based material, and the second alumina-based material has a pore volume of less than 0.8 cc / g; The specific surface area of the second alumina-based material is 130 m 2 / g~240m 2 / g, and the specific surface area of the second alumina-based material after aging at 1200±100° C. for 4±0.5 hours is 40 m 2 / g or more.
[0021] According to one embodiment of the present invention, the second alumina-based material has a pore volume of 0.4 cc / g to 0.8 cc / g.
[0022] According to one embodiment of the present invention, the second alumina based material comprises γ-alumina and / or θ-alumina.
[0023] According to one embodiment of the present invention, the second alumina-based material contains a rare earth element, and the mass content of the rare earth element in the second alumina-based material is 3% to 7%.
[0024] According to one embodiment of the present invention, the material of the second support includes at least one of ceramic and metal.
[0025] According to one embodiment of the present invention, the three-way conversion section further includes a second support and a second active layer located on the surface of the second support, the three-way catalyst is present in the second active layer, and the ratio of the mass of the precious metal in the three-way catalyst to the volume of the second support is (3 to 50) grams:cubic feet.
[0026] According to one embodiment of the present invention, the three-way catalyst further comprises platinum, and the mass ratio of rhodium to platinum is 1:0-15, and / or the mass ratio of rhodium to palladium is 1:2-15.
[0027] Another aspect of the present invention further provides an application of the above-mentioned three-way catalytic conversion system in engine exhaust purification treatment.
[0028] According to one embodiment of the present invention, the engine exhaust comprises an oxygen-rich engine exhaust, and the volume fraction of oxygen in the oxygen-rich engine exhaust is 1% or more.
[0029] According to one embodiment of the present invention, the engine exhaust comprises a stoichiometric engine exhaust. Effect of the Invention
[0030] The three-way catalytic conversion system (TWC system) for engine exhaust purification treatment provided by the present invention first treats the exhaust gas discharged from the engine with an oxidation catalyst, and then oxygen and reducing components such as HC and CO are first combusted under the catalytic action of the oxidation catalyst to remove oxygen, thereby reducing the degree of combustion during the three-way catalytic treatment, and preventing the combustion from occupying most of the space of the three-way catalyst and the generation of high temperatures due to the combustion from adversely affecting the three-way conversion reaction and the structure and performance of the three-way catalyst, thereby ensuring the function of the three-way catalyst and efficiently removing harmful components such as HC, CO and NOx in the exhaust gas, and the exhaust gas treated by the TWC system of the present invention can achieve the target emission standards. [Brief description of the drawings]
[0031] [Figure 1] 4 is a graph showing a curve of variation of the concentration of oxygen in the exhaust gas according to the engine output. [Diagram 2] 4 is a graph showing the curves of change in temperature of the exhaust inlet of the oxidation section and the catalyst in the oxidation section according to the engine output. [Diagram 3] 1 is a graph showing the change curves of the conversion rates of NMHC and CO in the oxidation section according to the aging time of the TWC catalyst. [Figure 4] 1 is a graph showing the change curve of the conversion rate of NMHC and CO according to the aging time of the catalyst in the oxidation section. [Diagram 5] 4 is a graph showing a change curve of NOx concentration according to the catalyst reaction temperature in the oxidation section after engine exhaust is treated by a catalyst system. [Figure 6]2 is a graph showing a change curve of NOx conversion rate in a catalytic system according to a catalytic reaction temperature in an oxidation section; [Figure 7] 4 is a graph showing change curves of the exhaust inlet temperature of the oxidation section B, the temperature of the oxidation catalyst in the oxidation section B, and the exhaust outlet temperature of the oxidation section B according to the engine output in one embodiment of the present invention. [Figure 8] 4 is a graph showing the change curves of the oxygen concentration at the exhaust inlet of the oxidation section B and the oxygen concentration at the exhaust outlet of the oxidation section B according to the engine output in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] In order that those skilled in the art may better understand the aspects of the present invention, the present invention will now be described in further detail.
[0033] The TWC system for engine exhaust gas purification treatment provided by the present invention includes an oxidation section containing an oxidation catalyst and a three-way conversion section containing a three-way catalyst, the oxidation catalyst being used to catalyze the oxidation reaction between reducing components in the exhaust gas and oxygen, the oxidation section being located downstream of the engine, and the three-way conversion section being located downstream of the oxidation section.
[0034] In the present invention, the three-way conversion unit (three-way catalyst) is located downstream / rear end of the oxidation unit (oxidation catalyst), i.e., the exhaust outlet of the engine, the oxidation unit, and the three-way conversion unit are installed in sequence, and the oxidation unit is located between the exhaust outlet of the engine exhaust and the three-way conversion unit, so that the exhaust gas discharged from the engine flows through the oxidation unit and the three-way conversion unit in sequence, and is first treated by the oxidation catalyst of the oxidation unit, and then treated by the three-way catalyst of the three-way conversion unit to purify the exhaust gas. Here, the oxidation catalyst is used to catalyze the reaction between oxygen and reducing components such as HC and CO, consuming most of the oxygen and reducing components such as HC and CO in the exhaust gas, and the exhaust gas after oxidation catalyst treatment is further treated by the rear three-way catalyst, which is used for three-way conversion (mainly converting HC, CO, and NOx simultaneously), and in the treatment process of the three-way catalyst, there is little oxygen and reducing components such as HC and CO remaining in the exhaust gas, which can reduce the degree of combustion, and the three-way catalyst is prevented from being covered by combustion and the three-way catalyst is further purified. catalystWhile ensuring the conversion function, it is possible to avoid the occurrence of excessively high temperatures, so that the three-way catalyst performs the three-way conversion reaction at an appropriate reaction temperature (350 to 700°C), and also to avoid the occurrence of high temperatures having a negative effect on the structure and performance of the three-way catalyst (for example, the collapse of the pores of the porous loading material, the reduction in the activity of the precious metal, the deterioration of the function of the oxygen storage material, etc.), thereby improving the efficiency and durability of the three-way conversion reaction.
[0035] In a specific implementation, the three-way catalyst located at the rear end of the oxidation catalyst must operate at 350 to 700°C (i.e., the temperature in the three-way catalyst treatment process must be controlled to approximately 350 to 700°C), while at the same time, conditions such as the distance between the oxidation catalyst and the three-way catalyst or the relative positions of the two can be adjusted based on factors such as the engine exhaust composition in order to avoid exposing the three-way catalyst to ultra-high temperatures (850 to 950°C) for long periods of time.
[0036] In addition, the exhaust gas is first treated by an oxidation catalyst, and in this treatment process, the oxidation catalyst catalyzes the reaction of reducing components such as HC and CO in the exhaust gas with oxygen, and the source of the oxygen can be oxygen contained in the exhaust gas generated by the engine (i.e., oxygen attached to the exhaust gas generated by the engine), or oxygen can be injected into the inlet of the oxidation catalyst as needed (secondary air injection in the combustion of excess reducing agents in the exhaust gas, which accelerates the temperature rise of the catalyst during the cold start phase). (When the engine is set to run rich) ) is introduced, which consumes most of the reducing components such as HC and CO in the exhaust gas, and prevents combustion during the three-way catalyst treatment, which can cause high temperatures, and allows the three-way catalyst to perform the three-way conversion reaction at an appropriate reaction temperature (350 to 700°C). Therefore, in some embodiments, the oxidation section of At the exhaust inlet connection The intake pipe may include (When the engine is set to run rich)The intake pipe inputs air (oxygen) into the exhaust gas that has entered the oxidation section, so that most of the reducing components such as HC and CO are consumed after the exhaust gas that has entered the oxidation section is treated by the oxidation catalyst. A valve is further installed in the intake pipe, which stops the input of air when there is no need to input oxygen into the exhaust gas that has entered the oxidation section, and inputs air when there is a need to input oxygen into the exhaust gas that has entered the oxidation section, and inputs air (oxygen) into the exhaust gas that has entered the oxidation section through the intake pipe. (When the engine is set to run rich) .
[0037] Oxidation reaction The temperature during oxidation is relatively high, but generally does not exceed 1000°C (the maximum temperature to which the catalyst is exposed can be controlled by the combination of oxidation catalysts), and the oxidation catalyst may be a high-temperature resistant oxidation catalyst, specifically an ultra-high-temperature resistant oxidation catalyst that can withstand about 1000°C to 1100°C, that is, under conditions of about 1000°C to 1100°C, the structure and performance of the oxidation catalyst are basically stable, and for example, pore collapse phenomenon does not basically occur. Specifically, the oxidation catalyst may include a first alumina-based material and palladium supported on the first alumina-based material, and the pore volume of the first alumina-based material may be 0.8cc / g to 1.2cc / g (i.e., cm 3 / g), for example, 0.8cc / g, 0.9cc / g, 1cc / g, 1.1cc / g, 1.2cc / g or any two of them, and the specific surface area is 130 to 180m 2 / g, for example, 130m 2 / g, 140m 2 / g, 150m 2 / g, 160m 2 / g, 170m 2 / g, 180m 2 / g or any two of them, and the specific surface area of the first alumina-based material after aging at 1200±100°C for 4±0.5 hours is 60 m 2 / g or more, and by using the first alumina-based material, the performance of the oxidation catalyst, such as high temperature resistance and stability, can be improved, and the catalytic activity and service life of the oxidation catalyst can be further ensured.
[0038] Specifically, the first alumina-based material may include γ-alumina, which may be doped alumina and / or undoped alumina. In some embodiments, the first alumina-based material contains a rare earth element, which is an oxide of the rare earth element, and the mass content of the rare earth element in the first alumina-based material is 0-7% (i.e., the mass content of the oxide of the rare earth element accounts for 0-7% of the first alumina-based material), such as 0, 1%, 2%, 3%, 4%, 5%, 6%, 7%. When the mass content of the rare earth element is 0, the first alumina-based material is undoped alumina, and when the mass content of the rare earth element is not 0, the first alumina-based material is doped alumina (or called rare earth alumina), and by comparison, the use of doped alumina is advantageous for improving the high temperature resistance performance of the alumina-based material. Optionally, the rare earth element includes, for example, lanthanum (La).
[0039] The first alumina-based material is commercially available or self-made, and generally, the alumina raw material is subjected to high-temperature aging treatment to collapse easily collapsing pores, thereby obtaining a structurally stable high-temperature resistant alumina-based material, which is hardly subject to serious collapse phenomenon when the alumina-based material is applied under high-temperature conditions, thereby improving the high-temperature resistance of an oxidation catalyst using the high-temperature resistant alumina-based material as a substrate. Specifically, in some embodiments, the first alumina-based material may be prepared according to the following steps: the alumina raw material is aged at 1000°C to 1500°C for at least 2 hours to prepare the first alumina-based material, and the first alumina-based material prepared by the aging treatment has good stability below 1000°C, thereby ensuring the high-temperature resistance of the oxidation catalyst. Here, when producing a first alumina-based material not doped with a rare earth element, the alumina raw material is an alumina raw material not doped with a rare earth element, and when producing a first alumina-based material doped with a rare earth element, the alumina raw material is an alumina raw material doped with a rare earth element, and the alumina raw material used in the above process is commercially available or self-produced, and the present invention does not have any particular limitations thereon.
[0040] After the above-mentioned alumina-based material is aged at 1000°C to 1500°C, palladium can be supported on the first alumina-based material by a common method in the art, such as an immersion method (e.g., an equal volume immersion method), to obtain an oxidation catalyst. In a specific implementation, a palladium precursor is dissolved in a first solvent to prepare a first immersion liquid, and the first alumina-based material is immersed in the first immersion liquid, for example, by completely immersing the first alumina-based material in the first immersion liquid, or by spraying the first alumina-based material with the first immersion liquid and immersing it therein, and then drying the material after immersion. Baked Then, the solvent is removed, that is, palladium is supported on the first alumina-based material to obtain the oxidation catalyst, where the first solvent may include water, and the precursor of palladium may include a soluble salt of palladium, such as palladium nitrate. Also, an element having a function of fixing a precious metal, such as barium (Ba), may be added to the oxidation catalyst (or the first coating layer described later) to increase the stability of the precious metal.
[0041] The oxidation unit may further include a first support for supporting the oxidation catalyst, i.e., the oxidation catalyst is disposed on the first support, and in some preferred embodiments, the oxidation unit includes a first support and a first active layer located on the surface of the first support, and the oxidation catalyst is present in the first active layer (i.e., the first active layer includes the oxidation catalyst).
[0042] Typically, the first active layer further comprises an adhesive and / or a modification aid, and the adhesive may comprise an aluminum paste and / or a silica gel, and the modification aid may comprise a cerium material and / or a zirconium material, so as to further improve the performance such as the stability of the oxidation part. In some embodiments, based on the total mass of the first active layer, the mass percentage of the oxidation catalyst is 85%-98% (i.e., the mass content of the oxidation catalyst in the first active layer is 85%-98%), such as 85%, 88%, 90%, 93%, 95%, 98%, or any two thereof, and the remainder is the adhesive and / or the modification aid.
[0043] In a specific implementation, a slurry is produced by mixing an oxidation catalyst, an adhesive and / or a modification aid with a fourth solvent, and the slurry is then applied to the surface of a first support. After undergoing a process such as drying, the first active material layer can be formed on the surface of the first support.
[0044] Optionally, the material of the first carrier may include at least one of ceramic (e.g., cordierite), metal, etc., i.e., the first carrier may be formed of a mixture of one or more of ceramic materials, metals, etc., and the first carrier may be a gasoline particulate filter (GPF) or a honeycomb-shaped carrier, but is not limited thereto.
[0045] According to the research of the present invention, the content of palladium as an active metal component of the catalytic oxidation active material (i.e., the oxidation catalyst) is an important factor affecting the performance of the oxidation catalyst, and in some preferred embodiments, based on the total mass of the oxidation catalyst, the mass percentage of palladium is 0.06-1.0% (i.e., the mass content of palladium in the oxidation catalyst is 0.06-1.0%).
[0046] In the present invention, the number of the oxidation sections containing an oxidation catalyst is at least one, i.e., it may be one, or it may be at least two (i.e., a combination of two or more oxidation catalysts). When the number of oxidation sections is at least two, the distance between two adjacent oxidation sections is usually 150 mm or more (the distance is the distance along the flow direction of the engine exhaust gas). Here, in the two adjacent oxidation sections, the content of palladium in the oxidation catalyst of the oxidation section located upstream is: Located downstream of the oxidation sectionThe content of palladium in the oxidation catalyst may be less than or equal to that of the oxidation catalyst, and may be installed according to need in a specific implementation. By combining at least two oxidation units, each oxidation unit partially oxidizes the reducing agent in the exhaust gas (consuming a portion of oxygen), and no very high temperature rise occurs, that is, the heat of combustion is distributed to two oxidation catalysts with a certain distance between them, and the maximum temperature to which the oxidation catalyst in the oxidation unit is exposed can be controlled, which is advantageous to further improve the purification treatment efficiency and durability of engine exhaust gas.
[0047] In addition, the ratio of the mass of palladium in the oxidation catalyst to the volume of the first support can be (3 to 50) grams:1 cubic foot (i.e., (3 to 50) g / ft3), for example, 3 g:1 cubic foot, 5 g:1 cubic foot, 10 g:1 cubic foot, 20 g:1 cubic foot, 30 g:1 cubic foot, 40 g:1 cubic foot, 50 g:1 cubic foot, or a range consisting of any two ratios thereof, which is advantageous in improving the treatment efficiency of the oxidation catalyst.
[0048] Furthermore, the ratio of the mass of the first active layer to the volume of the first support may be (100 to 200) grams:1 liter (i.e., (100 to 200) g / L), for example, 100 g:1 liter, 150 g:1 liter, 160 g:1 liter, 170 g:1 liter, 180 g:1 liter, 190 g:1 liter, 200 g:1 liter, or a range consisting of any two ratios thereof.
[0049] The present invention can adopt a conventional three-way catalyst (TWC) in the art, and in some embodiments, the three-way catalyst includes a porous substrate, an oxygen storage material and a precious metal, the precious metal includes palladium and rhodium, the oxygen storage material is filled in the porous substrate, the rhodium is supported on the oxygen storage material, the precious metal other than rhodium may be supported on the porous substrate or on the oxygen storage material as necessary, and the palladium may be supported on the porous substrate or on the oxygen storage material. Here, the support of rhodium on the oxygen storage material can protect rhodium and reduce the contact reaction between it and other components such as the porous substrate. Preferably, palladium is supported on the oxygen storage material, and more preferably, all of the above precious metals are supported on the oxygen storage material.
[0050] The present invention uses a conventional method in the art to support the above-mentioned precious metal on the oxygen storage material or the porous substrate, such as a dipping method (for example, an equal volume dipping method), for example, a rhodium precursor is mixed with a second solvent to prepare a second dipping liquid, and the second dipping liquid is used to dipping the oxygen storage material, thereby achieving rhodium being supported on the oxygen storage material, the second solvent may include water, and the rhodium precursor may be a soluble salt of rhodium, such as rhodium nitrate; a platinum precursor is mixed with a third solvent to prepare a third dipping liquid, and the third dipping liquid is used to dipping the porous substrate, thereby achieving platinum being supported on the porous substrate, the third solvent may include water, and the platinum precursor may be a soluble salt of platinum, such as platinum nitrate.
[0051] Oxygen storage materials can achieve a three-way conversion reaction at nearly the stoichiometric air-fuel ratio. conditionsAs in the above, the air-fuel ratio (λ) of the engine exhaust on the catalyst surface can be adjusted. This ensures the efficiency of the three-way conversion reaction and allows each component to perform its function. In some embodiments, the oxygen storage material may include CeZrO, and may further include ZrO2, i.e., a combination of CeO2 and ZrO2, but the present invention is not limited thereto. The porous substrate is used to disperse components such as precious metals to ensure the dispersion and catalytic activity of the three-way catalyst, and in some embodiments, the porous substrate may include a second alumina-based material, and the pore volume of the second alumina-based material is less than 0.8cc / g, and generally preferably 0.4cc / g to 0.8cc / g, for example 0.4cc / g, 0.5cc / g, 0. 6cc / g, 0. 7cc / g, 0. 8cc / g or any two of them, and its specific surface area is 130m 2 / g~240m 2 / g, e.g. 130m 2 / g, 140m 2 / g, 150m 2 / g, 160m 2 / g, 170m 2 / g, 180m 2 / g, 190m 2 / g, 200m 2 / g, 210m 2 / g, 220m 2 / g, 230m 2 / g, 240m 2 / g or any two of them, which is advantageous for dispersing components such as precious metals in the porous substrate and improving the performance of the three-way catalyst. In addition, the specific surface area of the second alumina-based material after aging at 1200±100°C for 4±0.5 hours is generally 40 m 2 / g or more.
[0052] Specifically, the second alumina-based material may include γ-alumina and / or θ-alumina, which may be doped and / or undoped alumina, and the doped alumina may generally be doped with a rare earth element. In some embodiments, the second alumina-based material contains a rare earth element, which is an oxide of the rare earth element, and the mass content of the rare earth element in the second alumina-based material is 3% to 7% (i.e., the mass of the oxide of the rare earth element accounts for 3% to 7% of the second alumina-based material), such as 3%, 4%, 5%, 6%, 7%, or any two of them. Optionally, the rare earth element includes, for example, La. The second alumina-based material may be commercially available or self-produced, and the present invention is not particularly limited in this respect.
[0053] The three-way conversion unit may further include a second support for supporting the three-way catalyst, i.e., the three-way catalyst is placed on the second support, and the three-way catalyst can form a coating layer on the second support, but is not limited thereto. In some preferred embodiments, the three-way conversion unit includes a second support and a second active layer located on the surface of the second support, and the three-way catalyst is present in the second active layer (i.e., the second active layer includes the three-way catalyst).
[0054] Typically, the second active layer further comprises an adhesive and / or a modifying aid, and the adhesive may comprise an aluminum paste and / or a silica gel, and the modifying aid may comprise a cerium material and / or a zirconium material, so as to further improve the performance such as the stability of the three-way conversion section. In some embodiments, based on the total mass of the second active layer, the mass percentage of the three-way catalyst is 85%-98% (i.e., the mass content of the three-way catalyst in the second active layer is 85%-98%), for example, in the range of 85%, 88%, 90%, 93%, 95%, 98%, or any two thereof, and the remainder is the adhesive and / or the modifying aid.
[0055] In a specific implementation, a three-way catalyst, an adhesive and / or a modifying aid are mixed with a fifth solvent to produce a slurry, and the slurry is then applied to the surface of a second carrier. After undergoing treatment such as drying, the second active material layer can be formed on the surface of the second carrier.
[0056] Optionally, the material of the second carrier may include at least one of ceramic (e.g., cordierite), metal, etc., and the second carrier may be a particulate filter (GPF) or a honeycomb carrier, but is not limited thereto, and the second carrier may be the same or different from the first carrier.
[0057] In some embodiments, the precious metal comprises platinum, wherein the mass ratio of rhodium to platinum is 1:0-15, preferably 1:0.5-8, such as 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, or any two of them, and the mass ratio of rhodium to palladium may be 1:2-15, such as 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, or any two of them, wherein the platinum may be supported on a porous substrate or supported on an oxygen storage material.
[0058] In some embodiments, the ratio of the mass of the precious metal in the three-way catalyst to the volume of the second support is in the range of (5-50) grams:cubic feet, e.g., 5 g:cubic feet, 10 g:cubic feet, 20 g:cubic feet, 30 g:cubic feet, 40 g:cubic feet, 50 g:cubic feet, or any two ratios thereof, where the mass of the precious metal is the sum of the masses of all kinds of precious metals in the three-way catalyst, e.g., the precious metals in the three-way catalyst are rhodium, platinum, and palladium, and therefore the mass of the precious metal is the sum of the masses of rhodium, platinum, and palladium in the three-way catalyst.
[0059] The present invention further provides the application of the above-mentioned TWC system in engine exhaust purification treatment. The engine of the present invention can be specifically a fuel oil engine, whose exhaust contains components such as hydrocarbon (HC), carbon monoxide (CO), and nitrogen oxide (NOx). In application, the exhaust generated by the engine is discharged from the exhaust outlet of the engine, and enters the oxidation section through the exhaust inlet, where it contacts with an oxidation catalyst, and under the action of the oxidation catalyst, the reducing components such as HC and CO in the exhaust react with oxygen, and then discharged from the exhaust outlet of the oxidation section, and enters the three-way conversion section through the exhaust inlet, where it contacts with a three-way catalyst in the three-way conversion section to carry out three-way conversion, and the HC, CO, and NOx in the exhaust are converted into carbon dioxide (CO2), nitrogen gas (N2) and water, to obtain purified exhaust, and the purified exhaust is discharged from the exhaust outlet of the three-way conversion section.
[0060] The TWC systems of the present invention may be particularly used to treat oxygen-rich engine exhaust, which in some embodiments includes oxygen-rich engine exhaust, where the volume fraction of oxygen in the oxygen-rich engine exhaust is 1% or greater, e.g., 2%, 2.5%, 3%, 3.5%, etc. or greater.
[0061] The exhaust gas (exhaust) from an engine operating at a stoichiometric air-fuel ratio with a high oxygen content contains oxidizing components such as oxygen (O2) and NOx, and reducing components such as HC and CO, and the reducing components basically correspond to the content of O2 (both of which are high). In a conventional TWC system, the reaction of a large amount of O2 with reducing components such as HC and CO in the TWC releases a large amount of heat and generates high temperatures, which affects the conversion efficiency and aging resistance of the TWC three-way catalyst, and the harmful components in the engine exhaust are Prevent sufficient conversion to meet emissions standards. By employing the three-way catalytic conversion system of the present invention, such problems can be effectively solved, and in some embodiments, the engine exhaust includes stoichiometric engine exhaust, and in particular may be high-oxygen stoichiometric engine exhaust, in which the volumetric oxygen content is greater than 1% (including cases where it is much greater than 1%).
[0062] Specifically, the oxygen (O2) content in the exhaust gas from an engine operating at a stoichiometric air-fuel ratio with a high oxygen content is high, and the amount of reducing components such as HC and CO is basically equivalent to O2, making it more combustible in the conventional TWC treatment process and at the same time generating high temperatures (even higher than 850-980°C). Long-term operation at high temperatures (>850°C) can cause structural destruction of the TWC, affecting the function of the TWC. The catalyst system of the present invention can particularly solve the problem that exhaust gas from an engine operating at a stoichiometric air-fuel ratio with a high oxygen content can cause ultra-high catalyst temperatures, and can be used in engine exhaust aftertreatment systems that exceed the high temperature resistance limit of the TWC.
[0063] In order to make the objectives, technical solutions and advantages of the present invention clearer, the technical solutions of the present invention are described below in combination with specific examples, and it is obvious that the described examples are only a part of the embodiments of the present invention, and not all of the embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative labor belong to the protection scope of the present invention. Example 1
[0064] In this embodiment, the three-way catalytic converter system includes an oxidation section containing an oxidation catalyst and a three-way converter section containing a three-way catalyst, the oxidation catalyst is used to catalyze the oxidation reaction between reducing components such as HC and CO in the exhaust gas and oxygen, the oxidation section is located downstream of the engine, and the three-way converter section is located downstream of the oxidation section, wherein: The oxidation part comprises a first carrier and a first active layer located on a surface of the first carrier, the first active layer includes an oxidation catalyst and an adhesive, the mass content of the oxidation catalyst in the first active layer is 90-98%, and the remaining part is the adhesive, the adhesive is aluminum paste and silica gel, the first carrier is cordierite, and the ratio of the mass of the first active layer to the volume of the first carrier is 160 g:1 L; The oxidation catalyst includes a first alumina-based material and palladium supported on the first alumina-based material, the oxidation catalyst being prepared by impregnating palladium nitrate into the first alumina-based material by an equal volume impregnation method, the first alumina-based material being a high temperature resistant rare earth alumina (wherein the alumina is γ-alumina) from Baizhexing Energy Co., Ltd., the pore volume of which is about 0.94cc / g and the specific surface area of which is about 169.4m 2 / g, and the specific surface area after aging at 1200°C for 4 hours is approximately 61.23 m 2 / g, the rare earth element contained therein is La, and the La oxide (La2O3), the mass content of La in the first alumina-based material is about 4%, The mass content of palladium in the oxidation catalyst is about 0.22% (0.353 g of palladium per liter of oxidation catalyst), and in the oxidation section, the ratio of the mass of palladium in the oxidation catalyst to the volume of the first support is 10 g:1 cubic foot; The three-way catalyst comprises a second carrier and a second active layer located on the surface of the second carrier, the second active layer includes a three-way catalyst and an adhesive, the mass content of the three-way catalyst in the second active layer is 90-98%, and the surplus is an adhesive, the adhesive is aluminum paste and silica gel, and the second carrier is cordierite; The three-way catalyst is composed of a second alumina-based material, CeZrO, and a precious metal, the precious metal being rhodium and palladium, the rhodium and palladium being supported on CeZrO, and the CeZrO being loaded in the second alumina-based material, the second alumina-based material being rare earth alumina (wherein the alumina is γ-alumina) from Baizhexing Energy Co., Ltd., its pore volume is about 0.49cc / g, and its specific surface area is about 145m 2 / g, and the specific surface area after aging at 1000°C for 4 hours is approximately 110 m 2 / g, the rare earth element contained therein is La, and the oxide of La (La2O3), the mass content of La2O3 in the second alumina-based material is about 4%, In the three-way conversion section, the ratio of the mass of the precious metal in the three-way catalyst to the volume of the second support is 10 grams:1 cubic foot, where the mass ratio of rhodium to palladium is 3:7. (Application Example)
[0065] The performance of the above catalyst system is verified by engine bench test below. In the experimental process, the exhaust gas flows through the oxidation section and the three-way conversion section in sequence after being discharged from the engine. The process is briefly described as follows: the exhaust gas generated from the engine is discharged from the exhaust outlet of the engine, then enters the oxidation section through the exhaust inlet of the oxidation section, contacts with the oxidation catalyst in the oxidation section, so that the oxygen in the oxidation section undergoes an oxidation-reduction reaction with the reducing component, and is discharged from the exhaust outlet of the oxidation section, enters the three-way conversion section through the exhaust inlet of the three-way conversion section, contacts with the three-way catalyst in the three-way conversion section to perform three-way conversion, and is discharged from the exhaust outlet of the three-way conversion section to obtain purified exhaust gas. The following experiments 1 to 3, comparative experiments 1 and 2 are carried out by referring to the above process. In the following experiments, NMHC conversion rate = ((amount of NMHC in simulated exhaust gas - amount of NMHC in exhaust gas discharged from the exhaust outlet of the oxidation section after reaction in the oxidation section) / amount of NMHC in simulated exhaust gas) x 100%, CO conversion rate = ((amount of CO in simulated exhaust gas - amount of CO in exhaust gas discharged from the exhaust outlet of the oxidation section after reaction in the oxidation section) / amount of CO in simulated exhaust gas) x 100%, The exhaust from an engine operating at a stoichiometric air-fuel ratio with a high oxygen content was simulated (simulated exhaust). Figure 1 shows the curve of change in the oxygen concentration (volume content) in the exhaust with engine power, and the contents of NMHC and CO are basically equivalent to oxygen. Figure 2 shows the curve of change in temperature at the exhaust inlet of the oxidation section with engine power and the curve of change in temperature in the oxidation section with engine power (the temperature in the oxidation section is high, at over 800°C (between 800 and 950°C), exceeding the TWC conversion temperature window (350 to 700°C)). Here, Figure 2 shows the curves of change in temperature in the oxidation section with engine power for Experiment 1 and Comparative Experiment 1, and in the remaining experiments below, unless otherwise specified, the reaction temperature in the oxidation section will be similar to this.
[0066] Comparative experiment 1: The oxidation catalyst of the oxidation section is a normal TWC (the difference between it and the three-way catalyst of Example 1 is as follows: the ratio of the mass of the precious metal to the volume of the second carrier is 40 g:1 cubic foot, where the mass ratio of palladium to rhodium is 7:1), and as shown in FIG. TWC The reaction time of the catalyst (also called the aging time) is controlled. The conversion rate of NMHC and CO in the oxidation section (at 850°C) Gas before and after the catalyst (Measure the change in concentration) of The change curve according to the aging time in the oxidation section (engine bench at 950°C) (see Figure 3) was measured, and it was found that the conversion efficiency decreased with the increase of aging time, and after aging for 300 hours, the conversion efficiency decreased significantly.
[0067] Experiment 1: The oxidation catalyst of Example 1 was aged at 1050°C. The aged catalyst was used as the oxidation catalyst of the oxidation section. Referring to the process of Experiment 1, the effect of the aged catalyst on the conversion rates of NMHC and CO after the oxidation catalyst was aged at 1050°C for different times (110 to 830 hours) was measured. A change curve (see FIG. 4) of the conversion rates of NMHC and CO (measurement of atmospheric concentration changes before and after the oxidation catalyst at 850°C) with aging time was obtained. It was found that the conversion rates of NMHC and CO were relatively high and tended to stabilize with the increase in aging time, and the above oxidation catalyst has good aging resistance.
[0068] Experiment 2: After aging the oxidation catalyst of Example 1 at 1050°C for 830 hours, the aged catalyst was used as the oxidation catalyst of the oxidation section. The oxidation catalyst reaction temperature of the oxidation section was controlled as shown in Figures 5 and 6. The NOx concentration in the purified exhaust gas from the catalyst system (catalyst of the oxidation section + catalyst of the three-way conversion section) and the NOx conversion rate (the ratio of the amount of NOx in the purified exhaust gas to the amount of NOx in the simulated exhaust gas before entering the oxidation section) were measured with the reaction temperature as shown in Figures 5 and 6. The oxidation catalyst had stable performance after aging at 1050°C for 830 hours, and the NOx concentration in the exhaust gas from the catalyst system (catalyst of the oxidation section + catalyst of the three-way conversion section) was <5 ppm. Standard Meet the requirements.
[0069] Comparative experiment 2: The TWC from comparative experiment 1 was aged at 950°C for 300 hours. The aged TWC was used as the catalyst in the oxidation section. The reaction temperature in the oxidation section was controlled as shown in Figures 5 and 6. The NOx concentration in the exhaust gas purified by the system (catalyst in the oxidation section + catalyst in the three-way conversion section) and the NOx conversion rate (the ratio of the amount of NOx change in the exhaust gas before and after treatment with the catalytic system to the amount of NOx in the simulated exhaust gas before entering the oxidation section) were measured with reaction temperature as shown in Figures 5 and 6. The TWC from comparative experiment 1 showed significant performance degradation after aging at 950°C for 300 hours. The NOx concentration after purification by the catalytic system (catalyst in the oxidation section + catalyst in the three-way conversion section) was >15ppm, which was higher than the emission requirement (<5ppm).
[0070] Experiment 3: The differences between Experiment 1 and Experiment 2 are as follows: the number of oxidation sections in Experiment 3 is two, namely, oxidation section A and oxidation section B, oxidation section B is located upstream of oxidation section A (i.e., the engine exhaust is first treated by the oxidation catalyst in oxidation section B and then by the oxidation catalyst in oxidation section A); oxidation section A is the same as the oxidation section in the above Experiment 1 or Experiment 2 (i.e., it corresponds to adding one oxidation section B upstream of the oxidation section in Experiment 1 or Experiment 2); the ratio of the mass of palladium in the oxidation catalyst of oxidation section B to the volume of the first support is 3 grams:1 cubic foot; and other conditions are the same as those of oxidation section A.
[0071] The change curves of the exhaust inlet temperature of oxidation section B, the temperature of the oxidation catalyst in oxidation section B, and the exhaust outlet temperature of oxidation section B according to the engine power measured by conducting an experiment with reference to the process of Experiment 2 are shown in Figure 7, and the change curves of the oxygen concentration at the exhaust inlet of oxidation section B and the oxygen concentration at the exhaust outlet of oxidation section B according to the engine power are shown in Figure 8. The oxidation catalyst of oxidation section B partially oxidizes the reducing agent in the exhaust and consumes some of the oxygen in the exhaust, so that it can effectively weaken the oxidation-reduction reaction of the exhaust gas in the oxidation catalyst of the downstream oxidation section A, and can suppress the rise in the catalyst temperature caused by the heat generated by the oxidation-reduction reaction.
[0072] The above describes the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included within the protection scope of the present invention.
Claims
1. A three-way catalytic conversion system for exhaust purification treatment of an engine operating at a stoichiometric air-fuel ratio, comprising an oxidation section containing an oxidation catalyst, and a three-way conversion section containing a three-way catalyst, the oxidation catalyst being used to catalyze an oxidation reaction between a reducing component in the exhaust and oxygen, the oxidation section being located downstream of the engine, the three-way conversion section being located downstream of the oxidation section, and the oxidation catalyst being a high-temperature resistant oxidation catalyst capable of withstanding temperatures of 1000°C to 1100°C, the oxidation catalyst includes a first alumina-based material and palladium supported on the first alumina-based material; The three-way catalyst includes a porous substrate, an oxygen storage material, and a precious metal, the precious metal includes platinum, rhodium, and palladium, the oxygen storage material is filled in the porous substrate, the rhodium is supported on the oxygen storage material, the oxygen storage material separates the rhodium from the porous substrate, and the precious metal other than rhodium is supported on the porous substrate or the oxygen storage material, the oxygen storage material can adjust the air-fuel ratio λ value within a preset range, and reduces the deviation degree between the actual air-fuel ratio λ value and λ = 1, and the porous substrate includes a second alumina-based material, The pore volume of the first alumina-based material is 0.8 cc / g to 1.2 cc / g; The second alumina-based material has a pore volume of less than 0.8 cc / g; The first alumina-based material is subjected to high-temperature aging treatment, and the alumina raw material is aged at 1000°C to 1500°C for at least 2 hours to collapse easily collapsing pores, and the specific surface area of the first alumina-based material is 60 m2 / g or more. A three-way catalytic conversion system for engine exhaust purification treatment, comprising:
2. The oxidation catalyst is The specific surface area of the first alumina-based material is 130 to 180 m 2 / g, and The specific surface area of the first alumina-based material after aging at 1200±100° C. for 4±0.5 hours is 60 m2 / g or more; Satisfying at least one of the following characteristics:
2. The three-way catalytic conversion system of claim 1.
3. the first alumina-based material comprises gamma-alumina; 3. The three-way catalytic conversion system of claim 2.
4. The first alumina-based material contains a rare earth element, and the mass content of the rare earth element in the first alumina-based material is 0 to 7%.
3. The three-way catalytic conversion system of claim 2.
5. The mass content of palladium in the oxidation catalyst is 0.06 to 1.0%; 3. The three-way catalytic conversion system of claim 2.
6. The number of the oxidation portions is at least two, and the distance between two adjacent oxidation portions is 150 mm or more.
3. The three-way catalytic conversion system of claim 2.
7. The oxidation section includes a first support and a first active layer located on a surface of the first support, and the oxidation catalyst is present in the first active layer.
2. The three-way catalytic conversion system of claim 1.
8. The first active layer further comprises an adhesive and / or a modifying aid; and The adhesive contains aluminum paste and / or silica gel; the modifying aid comprises a cerium material and / or a zirconium material; and The mass content of the oxidation catalyst in the first active layer is 85% to 98%, and the remainder is the adhesive and / or the modification assistant.
8. A three-way catalytic conversion system according to claim 7.
9. The material of the first support includes at least one of a ceramic and a metal.
8. A three-way catalytic conversion system according to claim 7.
10. The oxidation catalyst includes a first alumina-based material and palladium supported on the first alumina-based material, and a ratio of a mass of palladium in the oxidation catalyst to a volume of the first support is (3 to 50) grams:1 cubic foot.
8. A three-way catalytic conversion system according to claim 7.
11. The ratio of the mass of the first active layer to the volume of the first carrier is (100-200) grams:1 liter; 8. A three-way catalytic conversion system according to claim 7.
12. The three-way conversion section further includes a second support and a second active layer located on a surface of the second support, and the three-way catalyst is present in the second active layer.
2. The three-way catalytic conversion system of claim 1.
13. The second active layer further comprises an adhesive and / or a modifying aid; and The adhesive contains aluminum paste and / or silica gel; the modifying aid comprises a cerium material and / or a zirconium material; and The mass content of the three-way catalyst in the second active layer is 85% to 98%, and the remainder is the adhesive and / or the modifying aid.
13. The three-way catalytic conversion system of claim 12.
14. The oxygen storage material includes CeZrO; 2. The three-way catalytic conversion system of claim 1.
15. The porous substrate is The specific surface area of the second alumina-based material is 130 m 2 / g~240m 2 / g, and The specific surface area of the second alumina-based material after aging at 1200±100° C. for 4±0.5 hours is 40 m 2 / g or more; 2. The three-way catalytic conversion system of claim 1.
16. The pore volume of the second alumina-based material is 0.4 cc / g to 0.8 cc / g; 16. The three-way catalytic conversion system of claim 15.
17. The second alumina-based material includes γ-alumina and / or θ-alumina; 16. The three-way catalytic conversion system of claim 15.
18. The second alumina-based material contains a rare earth element, and the mass content of the rare earth element in the second alumina-based material is 3% to 7%.
16. The three-way catalytic conversion system of claim 15.
19. The second support is made of at least one of a ceramic and a metal.
13. The three-way catalytic conversion system of claim 12.
20. The three-way conversion section further includes a second support and a second active layer located on the surface of the second support, the three-way catalyst is present in the second active layer, and the ratio of the mass of the precious metal in the three-way catalyst to the volume of the second support is (3-50) grams:cubic feet.
2. The three-way catalytic conversion system of claim 1.
21. The three-way catalyst further comprises platinum, and the mass ratio of rhodium to platinum is 1:0-15, and / or the mass ratio of rhodium to palladium is 1:2-15.
2. The three-way catalytic conversion system of claim 1.
22. 22. The application of the three-way catalytic conversion system according to any one of claims 1 to 21 in engine exhaust gas purification treatment.
23. The engine exhaust comprises an oxygen-rich engine exhaust, and the volume fraction of oxygen in the oxygen-rich engine exhaust is 1% or more.
23. The application according to claim 22.
Citation Information
Patent Citations
Exhaust-gas cleaning catalyst
JP2006263582A
Catalyst for cleaning exhaust gas
JP2006263583A
Exhaust emission control catalyst device
JP2009007942A
Limiting NOX emission