Active energy ray curable inkjet black ink and printed matter
The active energy ray-curable inkjet black ink formulation with specific carbon black and polymerizable compounds, along with photopolymerization initiators, addresses stability and curability issues, ensuring high-definition printed matter quality, especially with LED lamps.
Patent Information
- Application Number
- JP2024022367
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-02-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-02-16
AI Technical Summary
Existing active energy ray-curable inkjet black inks face challenges in achieving excellent dispersion stability, ejection stability, and curability, particularly when used with carbon black, which is essential for improving the visibility and legibility of printed matter, especially when combined with LED lamps that emit narrow wavelength range active energy rays.
An active energy ray-curable inkjet black ink formulation comprising carbon black with specific DBP oil absorption and surface area characteristics, a basic pigment dispersion resin with low acid value, and a polymerizable compound including 5-methyl-3-vinyloxazolidin-2-one, along with a balanced ratio of monofunctional, bifunctional, and trifunctional monomers, and a combination of photopolymerization initiators like acylphosphine oxide and thioxanthone compounds, enhances stability and curability.
The ink achieves superior dispersion stability, ejection stability, and curability, resulting in high-definition printed matter with improved visibility and legibility, even when cured with LED lamps, thereby addressing the limitations of previous ink formulations.
Smart Images

Figure 0007575628000001 
Figure 0007575628000002 
Figure 0007575628000003
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an active energy ray-curable inkjet black ink, and a printed matter obtained by printing the active energy ray-curable inkjet black ink on a printing substrate. [Background technology]
[0002] In recent years, digital printing methods have been increasingly adopted in printing markets that emphasize productivity, such as the commercial printing market, the office printing market, the specialty printing market, etc. The reasons for this include the fact that digital printing methods do not require plate making, so printed matter can be produced at low cost and in a short time, the printing equipment is smaller and less expensive than the printing equipment used in plate printing methods, and uniform printed matter can be easily produced regardless of the skill of the person engaged in printing.
[0003] Among these, the inkjet printing method, which is one type of digital printing method, is superior to other digital printing methods in many respects, such as the running costs during printing, the ease of full colorization, the independence of the printing image quality from the installation environment of the printing device, etc. Therefore, there is a particularly high demand for the adoption of the inkjet printing method in the printing market.
[0004] The inks used in the inkjet printing method are diverse, including water-based, oil-based, solvent-based, active energy ray-curable, etc. Among these, the demand for active energy ray-curable inks has been increasing in recent years due to their characteristics such as the ability to print high-quality prints even on non-permeable printing substrates such as resin films and glass, the rapid drying (curing) time, and the strength of prints.
[0005] Incidentally, in the production of printed matter, black color (black color) is an extremely important color in that it can improve the visibility and readability of printed matter of characters and barcodes, the clarity of printed matter such as photographs, etc. However, in active energy ray curable inks used in inkjet printing methods (simply referred to as "active energy ray curable inkjet inks" in this application), it is known that black color is a color in which it is difficult to improve the curability. This is because carbon black, which is generally used as a colorant for black color, absorbs active energy rays. Since insufficient curability leads to a decrease in printing speed, improving the curability of black active energy ray curable inkjet ink is a very important issue when considering development in the above-mentioned printing market, which places importance on productivity.
[0006] In the past, active energy ray-curable inkjet inks that reproduce black by mixing multiple colorants without using carbon black have also been investigated (see, for example, Patent Document 1). However, it is difficult to reproduce a vivid black color using such a method, and further improvements are needed from the standpoint of improving the visibility, readability, and sharpness described above.
[0007] Recently, there has been an increasing demand from the market for environmental considerations. From this perspective, LED lamps are increasingly being used as a method for curing active energy beam-curable inkjet inks. However, LED lamps have the characteristic that the wavelength range of the active energy beams they emit is narrow, and when used in combination with active energy beam-curable inkjet inks, improving the curing properties becomes an issue.
[0008] Studies have been conducted to improve the curability of active energy ray-curable inkjet inks when used in combination with LED lamps. For example, Patent Document 2 discloses a photocurable inkjet printing ink composition that contains 4 to 40% by mass of vinyloxyethoxyethyl acrylate and 10 to 65% by mass of benzyl acrylate, and further contains a monofunctional monomer amount of 50% by mass or more. However, in the examples of Patent Document 2, no printing evaluation is actually performed using an inkjet printer (printing device), and there is no mention of whether printed matter with excellent visibility, readability, etc. can be stably printed. In addition, in consideration of the adoption in the printing market described above, it is considered necessary to further improve the curability of the photocurable inkjet printing ink composition disclosed in Patent Document 2.
[0009] Furthermore, Patent Document 3 discloses an ultraviolet-curable ink composition for inkjet printing, which contains an α-aminoalkylphenone initiator, a thioxanthone initiator, and a tertiary amine (photopolymerization initiator assistant). However, in the examples of Patent Document 3, the curability is evaluated using an inkjet printer employing a multi-pass printing method in which the same location is irradiated with actinic energy rays multiple times. In addition, in the above examples, only a yellow ink composition is evaluated. As described above, it is more difficult to improve the curability of a black actinic energy ray-curable inkjet ink than other colors. Therefore, when considering the adoption in the printing market described above, even if the configuration of Patent Document 3 is simply deployed in a black actinic energy ray-curable inkjet ink, there is a high possibility that the actinic energy ray-curable inkjet ink will not have the desired curability.
[0010] When the composition disclosed in Patent Document 3 is applied to a black active energy ray-curable inkjet ink, it is possible to increase the amount of the α-aminoalkylphenone initiator, the thioxanthone initiator, and the tertiary amine to increase the sensitivity to active energy rays and improve the curability. However, many of the above-mentioned components are solid at room temperature, and adding a large amount of these components can cause deterioration in the ejection stability from the inkjet head and the dispersion state of the colorant (carbon black, etc.). For this reason, simply increasing the amount of the above-mentioned components is not necessarily a good measure.
[0011] As described above, it has been extremely difficult to achieve both dispersion stability and ejection stability of a colorant (carbon black, etc.) and curability and definition of a printed matter, particularly in a black active energy ray-curable inkjet ink (also referred to as "active energy ray-curable black inkjet ink" in the present application) used in combination with an LED lamp.
[0012] In this application, the term "definition of printed matter" refers to the excellent visibility and readability even in the case of printed matter containing minute characters and bar codes. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2008-266548 A [Patent Document 2] International Publication No. 2014 / 014017 [Patent Document 3] JP 2014-136795 A Summary of the Invention [Problem to be solved by the invention]
[0014] The present invention has been made to solve the above-mentioned problems. Another object of the present invention is to provide an active energy ray-curable inkjet black ink that is excellent in all of the dispersion stability of carbon black, ejection stability, curability, and definition of printed matter. [Means for solving the problem]
[0015] As a result of intensive research, the present inventors have found that an active energy ray-curable inkjet black ink having the following composition can solve all of the above-mentioned problems simultaneously and to a high level.
[0016] That is, one embodiment of the present invention relates to an active energy ray-curable inkjet black ink as described in [1] to [7] below, and a printed matter obtained using the active energy ray-curable inkjet black ink as described in [8] below. [1] An active energy ray-curable inkjet black ink comprising carbon black, a basic pigment dispersion resin, and a polymerizable compound, The DBP oil absorption of the carbon black is AC (mL / 100 g), and the specific surface area of the carbon black is SC (m 2 / g), the value expressed by AC × SC is 2,000 to 12,000, The basic pigment dispersion resin has an acid value of 30 mgKOH / g or less, the polymerizable compound comprises 5-methyl-3-vinyloxazolidin-2-one, An active energy ray curable inkjet black ink, wherein the content of a monofunctional polymerizable compound (excluding the 5-methyl-3-vinyloxazolidin-2-one) is 15 mass % or less based on the total amount of the active energy ray curable inkjet black ink. [2] The polymerizable compound contains a radical polymerizable bifunctional monomer represented by the general formula (A), The active energy ray-curable inkjet black ink according to [1], wherein the content of the radical polymerizable bifunctional monomer represented by general formula (A) is 15 to 55 mass % of the total amount of the active energy ray-curable inkjet black ink. General formula (A): CH2=CR 1 -CO-OR 2 -O-CO-CR 1 =CH2 (In general formula (A), R 1 represents a hydrogen atom or a methyl group, and R 2 represents an alkylene group having 3 to 6 carbon atoms, which may have a branched structure. [3] The polymerizable compound contains a radical polymerizable trifunctional monomer represented by the general formula (B), The active energy ray-curable inkjet black ink according to [1] or [2], wherein the content of the radical polymerizable trifunctional monomer represented by general formula (B) is 2 to 15 mass % of the total amount of the active energy ray-curable inkjet black ink. General formula (B): [ka] (In general formula (B), R 3 represents a hydrogen atom or a methyl group, and R 4 is an ethylene group or a propylene group. In addition, l, m, and n each represent an integer of 0 to 9, and l+m+n is an integer of 0 to 9. [4] further comprising a photopolymerization initiator; The active energy ray-curable inkjet black ink according to any one of [1] to [3], wherein the photopolymerization initiator contains an acylphosphine oxide compound. [5] The active energy ray-curable inkjet black ink according to [4], wherein the photopolymerization initiator further contains a thioxanthone compound. [6] The acylphosphine oxide compound contains ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or a polymer of ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, The active energy ray-curable inkjet black ink according to [4] or [5], wherein a total content of the ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and the ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide is 45 to 80 mass % of a total amount of the photopolymerization initiator. [7] The active energy ray-curable inkjet black ink according to any one of [1] to [6], wherein the carbon black has a pH of 2 to 5. [8] A printed matter obtained by printing the active energy ray-curable inkjet black ink according to any one of [1] to [7] on a printing substrate. Effect of the Invention
[0017] The active energy ray-curable inkjet black ink according to one embodiment of the present invention exhibits the effects of being excellent in all of the dispersion stability of the carbon black, the ejection stability, the curing properties, and the definition of the printed matter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] An active energy ray-curable inkjet black ink according to one embodiment of the present invention (hereinafter, also simply referred to as "the inkjet ink of this embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and includes modified examples that are implemented within the scope of the present invention. In this application, the terms "(meth)acrylate", "(meth)acryloyl", and "(meth)acrylic acid" respectively mean "acrylate and / or methacrylate", "acryloyl and / or methacryloyl", and "acrylic acid and / or methacrylic acid".
[0019] First, the mechanism by which the inkjet ink of the present embodiment provides the above-mentioned effects will be described. Note that the mechanism described below is based on the inference of the present inventors and does not limit the present invention in any way.
[0020] First, the inkjet ink of the present embodiment contains 5-methyl-3-vinyloxazolidin-2-one as a polymerizable compound. As described above, it is generally known that a cyclic N-vinyl compound has a higher reaction rate with a radical derived from a photopolymerization initiator than an acrylate compound. The reaction rate of 5-methyl-3-vinyloxazolidin-2-one is particularly high compared to other compounds. The reason for this is considered to be that, unlike N-vinylcaprolactam and N-vinylpyrrolidone, which are generally known as cyclic N-vinyl compounds, 5-methyl-3-vinyloxazolidin-2-one has an oxygen atom in the ring structure. That is, it is considered that the electrons in the ring structure are attracted to this oxygen atom, which makes the vinyl group more likely to react with the radical derived from the photopolymerization initiator. As a result, bleeding of fine characters and thin lines can be suppressed, and it is easy to obtain a highly precise printed matter.
[0021] In addition, by adjusting the content of the monofunctional polymerizable compound (excluding 5-methyl-3-vinyloxazolidin-2-one) to 15 mass % or less of the total amount of the inkjet ink of this embodiment, the reaction between 5-methyl-3-vinyloxazolidin-2-one and radicals is not inhibited, and it is possible to further improve the curability and the definition of the printed matter.
[0022] On the other hand, there is a problem that cyclic N-vinyl compounds such as 5-methyl-3-vinyloxazolidin-2-one tend to deteriorate the dispersion stability of the pigment and the ejection stability of the inkjet ink. The reasons for this are thought to be that the cyclic N-vinyl compounds inhibit the stable adsorption of the pigment dispersant to the pigment surface, and that the vinyl group in the cyclic N-vinyl compound reacts with the acid group present in the pigment dispersant, etc. In addition, in the case of an active energy ray curable inkjet black ink containing carbon black, it is particularly difficult to improve the curability. The reasons for this include that the active energy ray is absorbed by the carbon black and therefore does not easily penetrate into the inkjet ink, and that the quinone group present on the surface of the carbon black traps radicals, etc. Therefore, even if 5-methyl-3-vinyloxazolidin-2-one is simply blended into an active energy ray curable inkjet black ink containing carbon black, the curability becomes insufficient, and the dispersion stability of the carbon black and the ejection stability of the inkjet black ink may deteriorate. Furthermore, the deterioration of the dispersion stability may also have an adverse effect on the definition of the printed matter.
[0023] In the inkjet ink of this embodiment, the DBP oil absorption is AC (mL / 100 g) and the specific surface area is SC (m 2 The carbon black used has a value of 2,000 to 12,000 when the total surface area is 100 μm / g. Carbon black that meets this requirement has large primary particles and relatively small aggregates, which are agglomerates of the primary particles. When such carbon black is used, the amount of active energy rays absorbed is reduced, although the details are unclear, and the small external surface area is thought to reduce the amount of radicals trapped on the surface.
[0024] In addition, in the inkjet ink of this embodiment, a basic pigment dispersion resin having an acid value of 30 mgKOH / g or less is used to disperse the carbon black. Although details will be described later, the basic pigment dispersion resin has a basic group as an adsorption point with the pigment (carbon black). It is considered that such a basic group strongly interacts with a functional group such as a carboxy group, a hydroxyl group, or a quinone group present on the surface of the carbon black, thereby ensuring the dispersion stability of the carbon black and the ejection stability of the inkjet ink even in the presence of 5-methyl-3-vinyloxazolidin-2-one. In addition, by setting the acid value of the basic pigment dispersion resin to 30 mgKOH / g or less (or 0 mgKOH / g) and limiting the amount of acid groups that can react with the vinyl groups in 5-methyl-3-vinyloxazolidin-2-one, the ejection stability of the inkjet ink can be further improved.
[0025] As described above, in order to improve all of the dispersion stability, ejection stability, curing properties, and definition of printed matter of carbon black, an active energy ray-curable inkjet black ink having the above-mentioned configuration is required.
[0026] Next, each of the components constituting the inkjet ink of this embodiment will be described in detail below.
[0027] The inkjet ink of this embodiment is black in color. The "black" inkjet ink includes inkjet ink capable of producing black printed matter, as well as inkjet ink capable of producing light black (gray) printed matter. However, it goes without saying that the inkjet ink must have the above-mentioned configuration in both the former and latter cases.
[0028] <Carbon black> The inkjet ink of this embodiment contains carbon black. The DBP oil absorption of the carbon black is AC (mL / 100 g) and the specific surface area is SC (m 2 / g), the value expressed as AC×SC is 2,000 to 12,000.
[0029] ≪DBP oil absorption amount≫ The DBP oil absorption is a value that indicates how much DBP (dibutyl phthalate) is absorbed in the particle voids present in the aggregate. In general, the more developed the aggregates are in the carbon black, the higher the DBP oil absorption value. The DBP oil absorption of the carbon black that can be used in the inkjet ink of this embodiment is preferably 40 to 100 mL / 100 g, more preferably 40 to 80 mL / 100 g, and particularly preferably 40 to 65 mL / 100 g. An inkjet ink using carbon black having such a DBP oil absorption has excellent curing properties. In addition, since the basic pigment dispersion resin can be firmly adsorbed, the dispersion stability of the carbon black is also improved. The DBP oil absorption can be measured using an "Absorbtometer Type C" manufactured by Brabender or the like in accordance with JIS K 6217-4.
[0030] ≪Specific surface area≫ Generally, carbon black with a large specific surface area has small primary particles and / or many pores. The specific surface area of carbon black that can be used in the inkjet ink of this embodiment is 45 to 120 m. 2 / g, and 50 to 95m 2 / g is particularly preferred. Carbon black having such a specific surface area is less likely to absorb active energy rays that have penetrated into the inkjet ink, and is less likely to trap radicals on the surface of the carbon black, improving the curability. In addition, the amount of carbon black with an excessively large primary particle size is reduced, resulting in good ejection stability. In the present application, the value measured by the nitrogen BET method is used as the "specific surface area" (nitrogen BET specific surface area). The method for measuring the specific surface area of carbon black by the nitrogen BET method is specified in JIS K 6217-2, and can be applied mutatis mutandis to the present application. As a specific example of the measurement method, nitrogen is adsorbed to degassed carbon black at liquid nitrogen temperature, and the specific surface area (m2) is calculated from the amount of adsorbed nitrogen when equilibrium is reached. 2 / g).
[0031] <DBP oil absorption multiplied by specific surface area> As described above, the carbon black contained in the inkjet ink of this embodiment has a DBP oil absorption of AC (mL / 100 g) and a specific surface area of SC (m 2 / g), the value expressed by AC×SC is 2,000 to 12,000. Furthermore, since not only the curability is improved, but also the definition of the printed matter is improved, and the dispersion stability of the carbon black and the discharge stability of the ink-jet ink are also improved by being firmly adsorbed to the basic pigment dispersion resin, the above value is preferably 2,000 to 7,500, and particularly preferably 2,000 to 6,000.
[0032] <pH> In addition to the above-mentioned specifications, the carbon black contained in the inkjet ink of this embodiment preferably has a pH of 2 to 5, and particularly preferably 2 to 4. Carbon black having such a pH value is capable of firmly adsorbing a basic pigment dispersion resin, thereby significantly improving the dispersion stability of the carbon black and the ejection stability of the inkjet ink. The pH of carbon black can be measured by a conventional method. For example, 5 g of carbon black and 50 mL of ion-exchanged water are mixed in a glass container such as a beaker, and the opening of the beaker is covered with a watch glass or the like, and the mixture is heated for 15 minutes. A small amount (about 0.1 mL) of ethanol or acetone may be added to make the carbon black more easily wetted. After boiling, the mixture is cooled to 25°C, and the supernatant liquid is removed to obtain a muddy substance. A pH electrode is inserted into the muddy substance, and the pH is measured. For measuring the pH, for example, a tabletop pH meter "F-71" (manufactured by Horiba, Ltd.) equipped with a pH electrode "9681S-10D" (manufactured by Horiba, Ltd.) can be used.
[0033] <Primary particle size> For the same reason as in the case of the specific surface area described above, i.e., because curability and discharge stability are improved, the primary particle diameter of the carbon black is preferably 20 to 50 nm, more preferably 25 to 50 nm, and particularly preferably 30 to 50 nm. The primary particle size of carbon black can be measured by a conventional method, for example, by observing carbon black with a transmission electron microscope (TEM), measuring the sizes (diameters) of 100 primary particles of carbon black, and then calculating the average value.
[0034] The content of carbon black that satisfies the above-mentioned requirements in the inkjet ink of this embodiment is preferably 0.5 to 3.5 mass % of the total amount of the inkjet ink, and particularly preferably 1.0 to 3.0 mass %. When the content of carbon black that satisfies the above-mentioned requirements is within the above range, the amount of carbon black present in the inkjet ink is suitable, and the inkjet ink has excellent curing properties, ejection stability, and fineness of printed matter.
[0035] Furthermore, the particle size (secondary particle size) of the carbon black contained in the inkjet ink of this embodiment and satisfying the above-mentioned requirements is preferably 80 to 250 nm, and particularly preferably 100 to 200 nm. If the secondary particle size of the carbon black satisfying the above-mentioned requirements is within the above range, the carbon black can be said to be in a favorable dispersion state, and the inkjet ink will be excellent in all of curability, discharge stability, and carbon black dispersion stability.
[0036] For the same reason, that is, because the carbon black is in a favorable dispersed state, the curing property and ejection stability of the inkjet ink, as well as the dispersion stability of the carbon black, are all improved, the secondary particle diameter (unit: nm) is calculated as the specific surface area (unit: m) of the carbon black that satisfies the above-mentioned requirements. 2 The value obtained by dividing by (1 / g) is preferably from 1.0 to 4.0, and particularly preferably from 1.5 to 3.5.
[0037] The secondary particle size refers to a median size measured on a volume basis. The secondary particle size can be measured using a dynamic light scattering particle size distribution analyzer (e.g., Nanotrac UPA-EX150 manufactured by Microtrac-Bell) and inkjet ink diluted with ethyl acetate to a concentration that allows the secondary particle size to be measured by the particle size distribution analyzer.
[0038] The inkjet ink of this embodiment may contain carbon black other than the carbon black that satisfies the above-mentioned requirements (also referred to as "other carbon black" in the present application). However, when the inkjet ink of this embodiment contains other carbon black, the blending amount is preferably an amount that does not inhibit the effect of the carbon black that satisfies the above-mentioned requirements. Specifically, the content of other carbon black contained in the inkjet ink of this embodiment is preferably 0 to 35% by mass, more preferably 0 to 20% by mass, and particularly preferably 0 to 10% by mass, of the total amount of carbon black contained in the inkjet ink.
[0039] In addition, in the present application, the statement "the blending amount (content) is 0 mass %" means that the target component is not contained.
[0040] <Other pigments> The inkjet ink of the present embodiment may contain pigments other than carbon black (also referred to as "other pigments" in the present application) in order to improve the curability and the definition and blackness of the printed matter. When the inkjet ink of the present embodiment contains other pigments, for the same reasons as in the case of the other carbon black described above, that is, the effects of the carbon black satisfying the above-mentioned requirements are effectively expressed, and the curability, ejection stability, and dispersion stability of the carbon black are improved. For these reasons, the content of the other pigments contained in the inkjet ink of the present embodiment is preferably 0 to 50% by mass, more preferably 0 to 35% by mass, and particularly preferably 0 to 20% by mass, relative to the content of the carbon black contained in the inkjet ink satisfying the above-mentioned requirements.
[0041] The other pigments are not particularly limited, but for example, organic pigments or inorganic pigments represented by the following color index names can be used. For example, red pigments include CI Pigment Red 5, 7, 12, 17, 48(Ca), 48(Mn), 49:2, 57(Ca), 57:1, 112, 122, 123, 147, 149, 150, 166, 168, 176, 177, 178, 184, 188, 202, 209, 242, 254, 255, 264, 266, 269, 282, etc.; Violet pigments, such as CI Pigment Violet 19, 23, etc.; Orange pigments, such as CI Pigment Orange 5, 13, 34, 38, 43, 61, 62, 64, etc.; Blue pigments include CI Pigment Blue 1, 2, 3, 15:3, 15:4, 15:6, 16, 22, 60, CI Vat Blue 4, 60, etc.; Green pigments include CI Pigment Green 7, 26, 36, 50, 58, etc.; Yellow pigments, such as CI Pigment Yellow 1, 2, 3, 12, 14, 16, 17, 73, 74, 75, 83, 93, 95, 97, 98, 109, 110, 114, 128, 129, 138, 139, 147, 150, 151, 154, 155, 180, 185, 213, etc.; These pigments can be used arbitrarily depending on the desired curing property, and the definition and blackness of the printed matter. Two or more of the pigments listed above may be used in combination.
[0042] <Basic pigment dispersing resin> The inkjet ink of this embodiment contains a basic pigment dispersion resin. The basic pigment dispersion resin has an acid value of 30 mgKOH / g or less. The acid value may be 0 mgKOH / g, i.e., the basic pigment dispersion resin may have substantially no acid groups.
[0043] In the present application, the term "basic pigment dispersion resin" refers to a dispersion resin in which a basic group serves as an adsorption point for the pigment (carbon black) surface. Examples of the basic group include a primary amino group, a secondary amino group, a tertiary amino group, a quaternary ammonium group, and an imino group. The organic groups bonded to the nitrogen atoms in the tertiary amino group and the quaternary ammonium group may be bonded to each other to form a ring structure (a heterocyclic ring containing the nitrogen atom). Examples of the ring include pyridine, pyrrolidine, pyrrolidone, imidazoline, and caprolactam.
[0044] In addition, even if a pigment dispersion resin has an acid group in addition to a basic group, the basic group functions as the adsorption point, so long as the basic group functions as the adsorption point, it is included in the "basic pigment dispersion resin" in this application. However, as described above, it goes without saying that only those having an acid value of 30 mgKOH / g or less (0 mgKOH / g is also acceptable) can be used as the basic pigment dispersion resin in this application.
[0045] Examples of basic pigment dispersion resins include acrylic resins having the above basic groups, (anhydrous) maleic acid resins having the above basic groups, polyethyleneimine, polyallylamine, polydiallylamine, polyvinylimidazoline, and polyvinylpyrrolidone, as well as graft resins having these resins as the main chain. Examples of commercially available basic pigment dispersion resins include "AJISPER-PB-821", "AJISPER-PB-822", "AJISPER-PB-824", and "AJISPER-PB-881" manufactured by Ajinomoto Fine-Techno Co., Ltd., and "DISPERBYK-162", "DISPERBYK-163", "DISPERBYK-168", "DISPERBYK-182", "DISPERBYK-184", "DISPERBYK-185", and "DISPERBYK-186" manufactured by BYK-Chemie. Examples of such solvents include SPERBYK-2013, DISPERBYK-2155, BYKJET-9150, BYKJET-9151, and BYKJET-9152 manufactured by Lubrizol; Solsperse 24000, Solsperse 32000, Solsperse 33000, Solsperse 35000, Solsperse 39000, Solsperse 86000, Solsperse J200, and Solsperse X300 manufactured by BASF; and EFKA PX4701, EFKA PX4703, and EFKA PX4733 manufactured by BASF.
[0046] The above-mentioned "acrylic resin" refers to a resin using one or more monomers selected from the group consisting of acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters as monomers constituting the resin (a styrene-based monomer may also be used). However, resins using maleic acid (anhydride) (maleic anhydride and / or maleic acid) as the monomer are not included in the above-mentioned "acrylic resin". The "maleic anhydride resin" refers to a resin using at least maleic anhydride as a monomer constituting the resin. The maleic anhydride resin may further use one or more monomers selected from the group consisting of α-olefins, acrylic acid, methacrylic acid, acrylic acid esters, methacrylic acid esters, styrene, and styrene derivatives as the monomer.
[0047] As described above, from the viewpoint of improving the ejection stability and curability of the inkjet ink of this embodiment, the acid value of the basic pigment dispersion resin is 30 mgKOH / g or less (may be 0 mgKOH / g). In addition, from the viewpoint of enabling the basic pigment dispersion resin to be stably present in the inkjet ink, further improvement in the ejection stability can be realized, and furthermore, from the viewpoint of improving the curability of the inkjet ink, it is particularly preferable that the acid value of the basic pigment dispersion resin is 20 mgKOH / g or less (may be 0 mgKOH / g).
[0048] The "acid value" of a basic pigment dispersion resin is the number of milligrams of potassium hydroxide required to neutralize 1 g of resin, and can be determined by potentiometric titration in accordance with JIS K 0070. As an example of a specific measurement method, the target resin is dissolved in a solvent in which diethyl ether and ethanol are mixed in a 1:1 mass ratio, and then titrated by potentiometric titration using a 0.1 mol / L potassium hydroxide-ethanol solution. The acid value can then be calculated using the titration amount read from the obtained titration curve.
[0049] The amine value of the basic pigment dispersion resin is preferably 10 to 50 mgKOH / g, and particularly preferably 15 to 40 mgKOH / g. A basic pigment dispersion resin having an amine value within the above range has a sufficient number of adsorption sites, and can firmly adsorb to carbon black that satisfies the above-mentioned requirements. As a result, the dispersion stability of the carbon black and the ejection stability of the inkjet ink are improved. Furthermore, the adsorption sites (basic groups) do not inhibit the polymerization reaction of the polymerizable compound, and therefore the curability of the inkjet ink is also improved.
[0050] The "amine value" of a basic pigment dispersion resin is the amount of potassium hydroxide (mg) required to neutralize 1g of resin, which is equivalent to the amount of acid. As an example of a method for measuring the amine value, the target resin is dissolved in a solvent that is a mixture of ethanol or tetrahydrofuran and acetic acid, and then titrated by potentiometric titration using a 0.1 mol / L perchloric acid-acetic acid solution. The amine value can then be calculated by converting the titration amount read from the obtained titration curve into mg of potassium hydroxide.
[0051] The mass average molecular weight of the basic pigment dispersion resin is preferably 5,000 to 60,000, more preferably 8,000 to 55,000, and particularly preferably 10,000 to 50,000. When the mass average molecular weight of the basic pigment dispersion resin is within the above range, the compatibility of the basic pigment dispersion resin with the polymerizable compound is improved, and the ejection stability is improved. In addition, since the basic pigment dispersion resin can be firmly adsorbed to the carbon black that satisfies the above-mentioned requirements, the dispersion stability of the carbon black is improved.
[0052] The mass average molecular weight can be measured by gel permeation chromatography (GPC). Specifically, the mass average molecular weight is a value obtained as a polystyrene-equivalent molecular weight measured using a TSKgel column (manufactured by Tosoh Corporation) and a GPC equipped with an RI detector (for example, "HLC-8320GPC" manufactured by Tosoh Corporation) using DMF as a developing solvent.
[0053] The blending amount of the basic pigment dispersion resin is preferably 10 to 100 mass %, more preferably 15 to 70 mass %, and particularly preferably 20 to 50 mass %, based on the total amount of the pigment components contained in the inkjet ink of this embodiment (carbon black satisfying the above-mentioned requirements, and other carbon black and / or other pigments, if contained). By using the basic pigment dispersion resin in the above blending amount range, the dispersion stability of the pigment components including the carbon black satisfying the above-mentioned requirements is improved, and the ejection stability of the inkjet ink of this embodiment is also good.
[0054] <Polymerizable compound> In the present application, the polymerizable compound refers to a compound that undergoes a polymerization reaction or a crosslinking reaction by radicals generated from a photopolymerization initiator or the like described below and has the function of curing a composition containing the polymerizable compound.
[0055] As described above, the inkjet ink of the present embodiment contains 5-methyl-3-vinyloxazolidin-2-one as a polymerizable compound. The content of the monofunctional polymerizable compound excluding the 5-methyl-3-vinyloxazolidin-2-one is 15% by mass or less based on the total amount of the inkjet ink.
[0056] 5-Methyl-3-vinyloxazolidin-2-one As described above, 5-methyl-3-vinyloxazolidin-2-one has particularly excellent curing properties compared to N-vinyl compounds other than 5-methyl-3-vinyloxazolidin-2-one. In addition, 5-methyl-3-vinyloxazolidin-2-one is also excellent in terms of safety and odor, and is therefore an essential material for the inkjet ink of the present embodiment.
[0057] The content of 5-methyl-3-vinyloxazolidin-2-one is preferably 5 to 40% by mass, more preferably 10 to 35% by mass, and particularly preferably 15 to 30% by mass, based on the total amount of the inkjet ink of this embodiment. By setting the content of 5-methyl-3-vinyloxazolidin-2-one within the above range, an inkjet ink with excellent curability can be obtained. As a result, the definition of the printed matter is also improved. Furthermore, since the inhibition of stable adsorption of the basic pigment dispersion resin to the carbon black surface that satisfies the above-mentioned requirements and the reaction with the acid group present in the basic pigment dispersion resin can be suppressed, the dispersion stability of the carbon black and the ejection stability of the inkjet ink are also good.
[0058] <Other polymerizable compounds> The inkjet ink of this embodiment may contain a radical polymerizable compound (also referred to as "other polymerizable compounds" in the present application) other than the above-mentioned 5-methyl-3-vinyloxazolidin-2-one. There is no limitation on the compound that can be used as the other polymerizable compound, and a monomer, oligomer, polymer, etc. having one or more polymerizable groups can be used. Both the "oligomer" and "polymer" are polymers in which multiple monomers are bonded together, and are classified according to the degree of polymerization. In the present application, those with a degree of polymerization of 2 to 10 are called "oligomers," and those with a degree of polymerization of 11 or more are called "polymers."
[0059] Examples of the polymerizable group possessed by the radically polymerizable compound (radical polymerizable compound) include a (meth)acryloyl group, a vinyl ether group, an allyl group, and a vinyl group (excluding a vinyl ether group and an allyl group). Among the above polymerizable groups, it is preferable to use a radical polymerizable compound having one or more polymerizable groups selected from the group consisting of an acryloyl group, a vinyl ether group, and a vinyl group (excluding a vinyl ether group and an allyl group) from the viewpoint of excellent curability.
[0060] As the other polymerizable compound, a monofunctional polymerizable compound (monofunctional polymerizable compound) or a bifunctional or higher (multifunctional) polymerizable compound (multifunctional polymerizable compound) may be used. Furthermore, the other polymerizable compound may be used alone or in combination of a plurality of polymerizable compounds. The term "monofunctional" refers to a compound having only one polymerizable group in one molecule, while "bifunctional" and "trifunctional" refer to a compound having two polymerizable groups in one molecule and a compound having three polymerizable groups in one molecule, respectively. Bifunctional or higher functional compounds are collectively referred to as "polyfunctional".
[0061] As described above, the inkjet ink of the present embodiment can use other polymerizable compounds as desired. On the other hand, in the inkjet ink of the present embodiment, the content of monofunctional polymerizable compounds (excluding 5-methyl-3-vinyloxazolidin-2-one) is set to 15% by mass or less of the total amount of the inkjet ink of the present embodiment. This is to further improve the curability and the definition of the printed matter by limiting the content of monofunctional polymerizable compounds other than 5-methyl-3-vinyloxazolidin-2-one. From this viewpoint, the content of monofunctional polymerizable compounds (excluding 5-methyl-3-vinyloxazolidin-2-one) is preferably as small as possible. Specifically, the content of monofunctional polymerizable compounds (excluding 5-methyl-3-vinyloxazolidin-2-one) is preferably 10% by mass or less of the total amount of the inkjet ink of the present embodiment, more preferably 6% by mass or less, and particularly preferably 3% by mass or less.
[0062] Other examples of the monofunctional radically polymerizable compound (radical-polymerizable monofunctional monomer) that can be used as the polymerizable compound include compounds having one (meth)acryloyl group. Specific examples of the compound include benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, ethylene oxide modified 2-phenoxyethyl (meth)acrylate, propylene oxide modified 2-phenoxyethyl (meth)acrylate, dicyclopentenyl (oxyethyl) (meth)acrylate, 2-methoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, methoxydipropylene glycol (meth)acrylate, dipropylene glycol (meth)acrylate, ethylene oxide modified nonylphenol acrylate, propylene oxide modified nonylphenol acrylate, ethylene oxide modified o-phenylphenol acrylate, ethylene oxide modified 2-ethyl Hexyl acrylate, β-carboxyethyl (meth)acrylate, trimethylolpropane formal (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl acrylate, 4-tert-butylcyclohexyl acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isoamyl (meth)acrylate, isononyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, caprolactone (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 1,Examples of the methacrylate include 4-cyclohexanedimethanol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, (meth)acryloylmorpholine, 2-(diethylamino)ethyl (meth)acrylate, 2-(diisopropylamino)ethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate, morpholinoethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, and N-(meth)acryloyloxyethylhexahydrophthalimide.
[0063] Other examples of radically polymerizable monofunctional monomers that can be used as other polymerizable compounds include polyfunctional radically polymerizable compounds (specific examples will be described later) in which only one polymerizable group is left and a primary or secondary organic amine is added (Michael addition) to the remaining polymerizable group.
[0064] Further, other examples of radical polymerizable monofunctional monomers that can be used as other polymerizable compounds include compounds having one vinyl group (excluding 5-methyl-3-vinyloxazolidin-2-one).Specific examples include N-vinylcaprolactam and N-vinylpyrrolidone.
[0065] Other examples of the difunctional radically polymerizable compound (radical-polymerizable difunctional monomer) that can be used as the polymerizable compound include compounds having two (meth)acryloyl groups. Specific examples of the compound include 1,3-propanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,3-butylenediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, ethylene oxide modified 1,6-hexanediol di(meth)acrylate, propylene oxide modified 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide modified neopentyl glycol di(meth)acrylate, propylene oxide modified neopentyl glycol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 2,4-dimethyl-1,5-Pentanediol di(meth)acrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, 2-ethyl-2-butylbutanediol di(meth)acrylate, ethylene oxide modified cyclohexanemethanol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, bisphenol A di(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, propylene oxide modified bis Phenol A di(meth)acrylate, bisphenol F di(meth)acrylate, ethylene oxide modified bisphenol F di(meth)acrylate, propylene oxide modified bisphenol F di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethylene oxide modified isocyanuric acid di(meth)acrylate, tricyclodecane di(meth)acrylate, dimethylol tricyclodecane di(meth)acrylate, cyclohexane dimethanol di(meth)acrylate, trimethylolpropane di(meth)acrylate, neopentyl glycol modified trimethylolpropane di(meth)acrylate, dicyclopentanyl di(meth)acrylate, etc.,
[0066] Other examples of radically polymerizable monofunctional monomers that can be used as other polymerizable compounds include polyfunctional radically polymerizable compounds (specific examples will be described later) having three or more polymerizable groups, in which two polymerizable groups are left and a primary or secondary organic amine is added (Michael addition) to the remaining polymerizable group.
[0067] Further, other examples of radical polymerizable bifunctional monomers that can be used as other polymerizable compounds include compounds having one (meth)acryloyl group and one vinyl ether group. Specific examples include 2-(2-vinyloxyethoxy)ethyl (meth)acrylate and 2-[2-(2-vinyloxyethoxy)ethoxy]ethyl (meth)acrylate.
[0068] Other examples of trifunctional radically polymerizable compounds (radically polymerizable trifunctional monomers) that can be used as polymerizable compounds include compounds having three (meth)acryloyl groups. Specific examples of such compounds include trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, ethylene oxide modified glycerin tri(meth)acrylate, propylene oxide modified glycerin tri(meth)acrylate, ethylene oxide modified isocyanuric acid tri(meth)acrylate, and ethylene oxide modified trimethylolpropane tri(meth)acrylate. acrylate, propylene oxide modified isocyanuric acid tri(meth)acrylate, propylene oxide modified dipentaerythritol tri(meth)acrylate tetramethylolmethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, tri((meth)acryloyloxyethyl)isocyanurate, hydroxypivalaldehyde modified dimethylolpropane tri(meth)acrylate, sorbitol tri(meth)acrylate, and the like.
[0069] Other examples of tetrafunctional radical polymerizable compounds (radical polymerizable tetrafunctional monomers) that can be used as polymerizable compounds include compounds having four (meth)acryloyl groups. Specific examples of such compounds include pentaerythritol tetra(meth)acrylate, sorbitol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethylene oxide modified pentaerythritol tetra(meth)acrylate, propylene oxide modified pentaerythritol tetra(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate.
[0070] Other examples of the pentafunctional radical polymerizable compound (radical polymerizable pentafunctional monomer) that can be used as the polymerizable compound include compounds having five (meth)acryloyl groups. Specific examples of the compound include sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc.
[0071] Other examples of the hexafunctional radical polymerizable compound (radical polymerizable hexafunctional monomer) that can be used as a polymerizable compound include compounds having six (meth)acryloyl groups. Specific examples of the compound include dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, alkylene oxide-modified hexa(meth)acrylate of phosphazene, and ε-caprolactone-modified dipentaerythritol hexa(meth)acrylate.
[0072] Furthermore, as the other polymerizable compound, a radically polymerizable compound (radical polymerizable oligomer) which is an oligomer can also be used. In this case, a compound having a (meth)acryloyl group as a polymerizable group can be preferably used. The number of polymerizable groups contained in the radically polymerizable oligomer is preferably 1 to 6 per molecule from the viewpoint of the balance of curability, discharge stability, and dispersion stability. The number of the polymerizable groups is more preferably 1 to 4, and particularly preferably 1 to 2. The mass average molecular weight of the radically polymerizable oligomer is preferably 400 to 6,000, and more preferably 500 to 4,500.
[0073] Examples of the radically polymerizable oligomer having a (meth)acryloyl group include urethane (meth)acrylate oligomers such as aliphatic urethane (meth)acrylate oligomers and aromatic urethane (meth)acrylate oligomers; acrylic (meth)acrylate oligomers; polyester (meth)acrylate oligomers; polyether (meth)acrylate oligomers; and epoxy (meth)acrylate oligomers. The oligomers may be modified, for example, by sulfonic acid modification, phosphoric acid modification, amino modification, mercapto modification, etc.
[0074] When the inkjet ink of the present embodiment contains other polymerizable compounds, it is preferable that the inkjet ink of the present embodiment contains a radical polymerizable bifunctional monomer and / or a radical polymerizable trifunctional monomer, because the curability, ejection stability, and definition of the printed matter are all improved. In particular, in the inkjet ink of the present embodiment, it is preferable that the inkjet ink of the present embodiment contains a radical polymerizable bifunctional monomer represented by the following general formula (A) and / or a radical polymerizable trifunctional monomer represented by the following general formula (B) as the other polymerizable compounds.
[0075] General formula (A): CH2=CR 1 -CO-OR 2 -O-CO-CR 1=CH2
[0076] In the above general formula (A), R 1 represents a hydrogen atom or a methyl group, and R 2 represents an alkylene group having 3 to 6 carbon atoms which may have a branched structure.
[0077] General formula (B): [ka]
[0078] In the above general formula (B), R 3 represents a hydrogen atom or a methyl group, and R 4 is an ethylene group or a propylene group. Furthermore, l, m, and n each represent an integer of 0 to 9, and l+m+n is an integer of 0 to 9.
[0079] The radically polymerizable bifunctional monomer represented by the general formula (A) has low viscosity and relatively low surface tension. Therefore, the inkjet ink containing the radically polymerizable bifunctional monomer represented by the general formula (A) has excellent wetting and spreading properties on the printing substrate, resulting in improved curability. In addition, the radically polymerizable bifunctional monomer represented by the general formula (A) is also highly compatible with 5-methyl-3-vinyloxazolidin-2-one, so that the polymerization reaction proceeds quickly, further improving the curability, and the deterioration of the dispersion stability of the carbon black caused by the 5-methyl-3-vinyloxazolidin-2-one is suppressed, thereby improving the dispersion stability of the carbon black.
[0080] Specific examples of the radically polymerizable bifunctional monomer represented by the above general formula (A) include 1,3-propanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,3-butylene diol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, and 3-methyl-1,5-pentanediol di(meth)acrylate.
[0081] From the viewpoints of improving both the curability and the dispersion stability of the carbon black, and further improving the definition of the printed matter, when the inkjet ink of this embodiment contains the radical polymerizable bifunctional monomer represented by the above general formula (A), the blending amount thereof is preferably 15 to 55 mass % and particularly preferably 25 to 45 mass % of the total amount of the inkjet ink.
[0082] On the other hand, the radical polymerizable trifunctional monomer represented by the above general formula (B) has a small viscosity among radical polymerizable trifunctional monomers, so that it is easy to achieve both ejection stability and curability of the inkjet ink. In addition, since it does not inhibit the effect of the above-mentioned 5-methyl-3-vinyloxazolidin-2-one, it is possible to further improve the curability.
[0083] Specific examples of the radical polymerizable trifunctional monomer represented by the above general formula (B) include glycerin tri(meth)acrylate, ethylene oxide modified glycerin tri(meth)acrylate (number of ethylene oxide groups: 3), ethylene oxide modified glycerin tri(meth)acrylate (number of ethylene oxide groups: 9), propylene oxide modified glycerin tri(meth)acrylate (number of propylene oxide groups: 3), and the like.
[0084] From the viewpoint of improving both the curability and the ejection stability and further improving the definition of the printed matter, when the inkjet ink of the present embodiment contains the radical polymerizable trifunctional monomer represented by the above general formula (B), the blending amount thereof is preferably 2 to 15 mass % and particularly preferably 55 to 12 mass % of the total amount of the inkjet ink.
[0085] In one embodiment, it is preferable that the inkjet ink contains both the radical polymerizable bifunctional monomer represented by the above general formula (A) and the radical polymerizable trifunctional monomer represented by the above general formula (B), which makes it easy to obtain an inkjet ink that is excellent in all of curability, ejection stability, carbon black dispersion stability, and fineness of printed matter.
[0086] When the inkjet ink of the present embodiment contains a radical polymerizable bifunctional monomer represented by the above general formula (A) and a radical polymerizable trifunctional monomer represented by the above general formula (B), the content by mass of the radical polymerizable bifunctional monomer represented by the above general formula (A) in the inkjet ink is preferably 2 to 20, and particularly preferably 2.5 to 15, relative to the content by mass of the radical polymerizable trifunctional monomer represented by the above general formula (B) in the inkjet ink being 1.
[0087] From the viewpoint of improving both the curability and the ejection stability, when the inkjet ink of the present embodiment contains a radically polymerizable bifunctional monomer and / or a radically polymerizable trifunctional monomer as another polymerizable compound, the total content of 5-methyl-3-vinyloxazolidin-2-one and the content of the radically polymerizable bifunctional monomer and / or the radically polymerizable trifunctional monomer is preferably 75 to 100 mass%, more preferably 90 to 100 mass%, and particularly preferably 95 to 100 mass%, of the total amount of polymerizable compounds contained in the inkjet ink.
[0088] In addition, since the dispersion stability of carbon black and the ejection stability of ink-jet ink can be improved without impeding the above-mentioned effect of 5-methyl-3-vinyloxazolidin-2-one, the content by mass of other polymerizable compounds is preferably 1 to 15, and particularly preferably 1.2 to 5, relative to the content by mass of 5-methyl-3-vinyloxazolidin-2-one taken as 1.
[0089] As described above, in the inkjet ink of the present embodiment, the content of the monofunctional polymerizable compound other than 5-methyl-3-vinyloxazolidin-2-one is limited. Therefore, it is preferable that the radical polymerizable monofunctional monomer is not used as the other polymerizable compound, or the amount of the radical polymerizable monofunctional monomer used is set to the above-mentioned amount (15% by mass, preferably 10% by mass, more preferably 6% by mass, particularly preferably 3% by mass) or less.
[0090] On the other hand, when a radically polymerizable monofunctional monomer is used as the other polymerizable compound, a (meth)acrylate having an alicyclic structure can be preferably used because it improves the wetting and spreading of the inkjet ink on the printing substrate, resulting in improved curing properties, and can suppress deterioration of the dispersion stability of carbon black. Specific examples of the (meth)acrylate having an alicyclic structure include cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl acrylate, 4-tert-butylcyclohexyl acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.
[0091] <Photopolymerization initiator> The inkjet ink of this embodiment preferably contains a photopolymerization initiator that is a source of radical generation. As the photopolymerization initiator, one or more conventionally known compounds can be arbitrarily used. Specifically, acylphosphine oxide compounds, benzophenone compounds, indane compounds, thioxanthone compounds, hydroxyacetophenone compounds, alkylaminoacetophenone compounds, oxime ester compounds, etc. can be used.
[0092] The term "polymerization initiator" in this application also includes materials that promote the radical generation of other photopolymerization initiators, which are generally called sensitizers. Examples of such materials include aminobenzoate-based compounds, ketocoumarin-based compounds, and anthracene-based compounds.
[0093] Among these photopolymerization initiators, it is preferable to use one or more photopolymerization initiators selected from the group consisting of acylphosphine oxide compounds and thioxanthone compounds, and it is particularly preferable to use at least an acylphosphine oxide compound, since this allows the dispersion stability of carbon black to be maintained in a suitable state while the curability is significantly improved.
[0094] Furthermore, from the viewpoint of obtaining an inkjet ink that is particularly excellent in curability and definition of printed matter, and further, that has good ejection stability and carbon black dispersion stability, it is extremely preferable to use an acylphosphine oxide compound and a thioxanthone compound in combination as the photopolymerization initiator.
[0095] In one embodiment, from the viewpoint of particularly improving the curability, it is preferable to use one or more photopolymerization initiators selected from the group consisting of acylphosphine oxide compounds and thioxanthone compounds in combination with one or more photopolymerization initiators selected from the group consisting of aminobenzoate compounds and ketocoumarin compounds.
[0096] <Acylphosphine oxide compounds> Specific examples of the acylphosphine oxide compound include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, as well as polymers of these compounds. Examples of commercially available acylphosphine oxide compounds include "Omnirad TPO", "Omnirad TPO-L", "Omnirad TPO-H", "Omnirad 819", and "OMNIPOL TP" manufactured by IGM RESINS, and "Speedcure TPO", "Speedcure TPO-L", and "Speedcure BPO" manufactured by Lambson. In addition, for example, acylphosphine oxide compounds described in WO 2017 / 086224 and WO 2020 / 049378, and lithium phenyl(2,4,6-trimethylbenzoyl)phosphinate can also be used. In the inkjet ink of this embodiment, the acylphosphine oxide compounds listed above may be used alone or in combination of two or more.
[0097] Among these compounds, ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or a polymer of ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide can be preferably used because they have high affinity with 5-methyl-3-vinyloxazolidin-2-one and improve curing properties and ejection stability.
[0098] From the viewpoint of being able to improve the curability and the definition of the printed matter without deteriorating the discharge stability and the dispersion stability of the carbon black, the content (total amount) of ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide polymer relative to the total amount of the photopolymerization initiator contained in the inkjet ink of this embodiment is preferably 45 to 80 mass%, and particularly preferably 50 to 70 mass%. It should be noted that the above expression "content (total amount)" refers to the total amount of the contents of ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or polymers of ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide when the inkjet ink of the present embodiment contains two or more types of these compounds, and refers to the content of only one type of compound when the inkjet ink contains only one type.
[0099] When the inkjet ink of the present embodiment contains an acylphosphine oxide compound, the blending amount of the acylphosphine oxide compound is preferably 4 to 15 mass % and more preferably 5 to 12 mass % of the total amount of the inkjet ink, from the viewpoint of obtaining an inkjet ink excellent in all of curability, ejection stability, and carbon black dispersion stability. In addition, from the viewpoint of obtaining an inkjet ink excellent in curability and ejection stability, the content of the acylphosphine oxide compound is preferably 0.15 to 2 and more preferably 0.2 to 0.8 when the content of 5-methyl-3-vinyloxazolidin-2-one is taken as 1.
[0100] <Thioxanthone compounds> Specific examples of the thioxanthone compounds include 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 3-methoxythioxanthone, 2-carboxymethoxythioxanthone, 3-ethoxycarbonylmethoxythioxanthone, 3-butoxycarboxymethoxythioxanthone, 1,3-dimethyl-2-(2-ethylhexyloxy)thioxanthone, 2-[2,2-bis(ethoxycarbonyl)]ethylthioxanthone, 1-chloro-4-propoxythioxanthone, and polymers of these compounds. Examples of commercially available thioxanthone compounds include "Omnirad ITX", "Omnirad DETX", and "OMNIPOL TX" manufactured by IGM RESINS, "SPEEDCURE ITX", "SPEEDCURE 2-ITX", "SPEEDCURE DETX", "SPEEDCURE LTX", "SPEEDCURE CPTX", and "SPEEDCURE 7010" manufactured by Lambson, and "Genopol TX-2" manufactured by RAHN. Of these commercially available products, "OMNIPOL TX", "SPEEDCURE 7010", and "Genopol TX-2" are the above-mentioned multimers. In the inkjet ink of this embodiment, the thioxanthone compounds listed above may be used alone or in combination of two or more.
[0101] When the inkjet ink of the present embodiment contains a thioxanthone compound, from the viewpoint of obtaining an inkjet ink that is excellent in all of curability, ejection stability, and carbon black dispersion stability, the blending amount of the thioxanthone compound is preferably 0.5 to 8 mass %, and particularly preferably 1 to 5 mass %, of the total amount of the inkjet ink.
[0102] As described above, it is preferable that the inkjet ink of this embodiment uses an acylphosphine oxide compound and a thioxanthone compound in combination. In this case, from the viewpoint of obtaining excellent curability and fineness of printed matter, the content of the acylphosphine oxide compound is preferably 1 to 25, and particularly preferably 2 to 12, relative to the content of the thioxanthone compound as 1. From the viewpoint of improving the ejection stability in addition to the curability and the definition of the printed matter, the mass of the acylphosphine oxide compound is preferably 0.1 to 1.0, and particularly preferably 0.2 to 0.85, when the sum of the mass of the thioxanthone compound and the mass of the 5-methyl-3-vinyloxazolidin-2-one is taken as 1.
[0103] <Aminobenzoate compounds> Specific examples of the aminobenzoate compounds include methyl 2-(dimethylamino)benzoate, ethyl 4-(dimethylamino)benzoate, ethyl 4-(diethylamino)benzoate, 2-ethylhexyl 2-(dimethylamino)benzoate, 2-butoxyethyl 2-(dimethylamino)benzoate, bis-[(4-dimethylaminobenzoyl)oxyethylene-1-yl]-methylamine, and polymers of these compounds (e.g., polyethylene glycol-bis(methyl 4-dimethylaminobenzoate)). Examples of commercially available aminobenzoate compounds include "Omnirad EDB", "Omnirad EHA", "Esacure A198", and "Omnipol ASA" manufactured by IGM RESINS, "SPEEDCURE EDB", "SPEEDCURE EHA", "SPEEDCURE BEDB", and "SPEEDCURE 7040" manufactured by Lambson, and "GENOPOL AB-1" and "GENOPOL AB-2" manufactured by Rahn AG. In the inkjet ink of this embodiment, the aminobenzoate compounds listed above may be used alone or in combination of two or more.
[0104] When the inkjet ink of this embodiment contains an aminobenzoate compound, the blending amount thereof is preferably 0.2 to 8 mass %, and particularly preferably 0.5 to 5 mass %, of the total amount of the inkjet ink.
[0105] <Ketocoumarin compounds> Specific examples of the ketocoumarin compounds include 3-benzoyl-7-methoxycoumarin, 3-benzoyl-5,7-dimethoxycoumarin, 3-(4-tert-butylbenzoyl)-5,7-dimethoxycoumarin, 3-(4-hexylbenzoyl)-5,7-dimethoxycoumarin, 3-[4-(2-ethylhexyl)benzoyl]-5,7-dimethoxycoumarin, 5,7-dimethoxy-3-[4-(3,5,5-trimethylhexyl)benzoyl]coumarin, 7-methoxy-3-(4-methylbenzoyl)coumarin, 7-methoxy-3-(4-tert-butylbenzoyl)coumarin, 7-methoxy-3-(4-hexylbenzoyl)coumarin, and 7-methoxy-3-[4-(2-ethylhexyl)benzoyl]coumarin.
[0106] From the viewpoint of particularly improving the curability, it is suitable to use the ketocoumarin compounds listed above in combination with the acylphosphine oxide compounds described above (preferably, ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or a polymer of the ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide).
[0107] When the inkjet ink of this embodiment contains a ketocoumarin compound, the blending amount thereof is preferably 1 to 10 mass %, and particularly preferably 2 to 8 mass %, of the total amount of the inkjet ink.
[0108] <Other photopolymerization initiators> Examples of commercially available photopolymerization initiators other than acylphosphine oxide compounds, thioxanthone compounds, and ketocoumarin compounds (also referred to as "other photopolymerization initiators" in this application) are shown below.
[0109] Examples of commercially available benzophenone compounds include "Omnirad BP," "Omnirad BMS," "Omnirad 4PBZ," "OMNIRAD EMK," and "Esacure 1001M," manufactured by IGM RESINS.
[0110] An example of a commercially available indane compound is "SpeedCure XFs01" manufactured by LAMBSON.
[0111] Examples of commercially available hydroxyacetophenone compounds include "Omnirad 127", "Omnirad 184", "Omnirad 1173", "Omnirad 2959", "Esacure KIP150" and the like manufactured by IGM RESINS.
[0112] Commercially available examples of the alkylaminoacetophenone compounds include "Omnirad 907," "Omnirad 369," and "Omnirad 379," both manufactured by IGM RESINS.
[0113] Examples of commercially available oxime ester compounds include "IRGACURE OXE01", "IRGACURE OXE02", and "IRGACURE OXE04" manufactured by BASF.
[0114] An example of a commercially available product of the anthracene compound is "Anthracure UVS-581" manufactured by Kawasaki Chemical Industries, Ltd.
[0115] In addition to the above-listed photopolymerization initiators, for example, "Omnirad 651" and "Omnirad MBF" manufactured by IGM RESINS can be used.
[0116] When the inkjet ink of this embodiment contains a photopolymerization initiator, the total amount of the photopolymerization initiator is preferably 3 to 20 mass %, more preferably 4 to 17 mass %, and particularly preferably 5 to 15 mass %, based on the total amount of the inkjet ink. By setting the total amount of the photopolymerization initiator within the above range, it is possible to achieve both curability and ejection stability.
[0117] <Other ingredients> In addition to the components described above, the inkjet ink of this embodiment may contain a surface conditioner, a polymerization inhibitor, an organic solvent, water, an inert resin, and other additives.
[0118] <Surface conditioner> The inkjet ink of the present embodiment preferably contains a surface conditioner for the purpose of improving the wetting and spreading of the ink on the printing substrate, the print image quality including the definition of the printed matter, the substrate adhesion, and the ejection stability. As the surface conditioner, for example, a siloxane-based surface conditioner, a fluorine-based surface conditioner, an acetylene glycol-based surface conditioner, an acetylene monool-based surface conditioner, etc. can be used. Among these, it is preferable to use a siloxane-based surface conditioner from the viewpoint of improving the wetting and spreading of the ink on the printing substrate, the print image quality including the definition of the printed matter, the substrate adhesion, and the ejection stability without deteriorating the dispersion stability of the carbon black.
[0119] As the siloxane-based surface conditioner, for example, a compound having a dimethylsiloxane structure and / or a modified product thereof can be used. Among them, a polyether-modified siloxane-based surface conditioner is particularly preferably used. By using a polyether-modified siloxane-based surface conditioner, the effect of 5-methyl-3-vinyloxazolidin-2-one is not inhibited, and the ink that has landed on the printing substrate can be sufficiently wetted and spread, so that it is possible to achieve both curability, print image quality including the resolution of the printed matter, and substrate adhesion while maintaining the ejection stability and the dispersion stability of carbon black in a suitable state. Specific examples of the polyether group include a polyethylene oxide group and a polypropylene oxide group. Either one of these groups or both of these groups may be contained in the molecule as the polyether group.
[0120] Commercially available polyether-modified siloxane-based surface conditioners that can be preferably used include, for example, BYK (registered trademark)-378, 348, 349, 3420, 3760, BYK-UV3500, and UV3510 manufactured by BYK-Chemie; and TEGO (registered trademark) Glide 450, 440, 435, 432, 410, 406, 130, 110, and 100 manufactured by EVONIK.
[0121] When a siloxane-based surface conditioner is used, its content is preferably 0.1 to 5.0% by mass based on the total mass of the inkjet ink. By adjusting the content to 0.1% by mass or more, the wetting and spreading properties on the printing substrate are improved, and the print image quality including the definition of the printed matter and the adhesion are also improved. On the other hand, by adjusting the content to 5.0% by mass or less, it becomes easy to ensure the curability, the dispersion stability of the carbon black, and the ejection stability.
[0122] Polymerization inhibitor In order to improve the ejection stability of the inkjet ink, and further improve the hue stability and suppress hardening wrinkles in the printed matter, a polymerization inhibitor can be blended into the inkjet ink of this embodiment. Specific examples of the polymerization inhibitor include hindered phenol compounds, phenol compounds, hydroquinone compounds, phenothiazine compounds, phosphorus compounds, and nitrosophenylhydroxylamine compounds, and these can be preferably used.
[0123] More specifically, examples of polymerization inhibitors that can be used in the inkjet ink of the present embodiment include 4-methoxyphenol, tert-butylhydroquinone, 2,6-di-tert-butyl-4-methylphenol, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], hydroquinone, methylhydroquinone, phenothiazine, dicumylphenothiazine, triphenylphosphine, and aluminum salt of N-nitrosophenylhydroxylamine.
[0124] The content of the polymerization inhibitor is preferably 0.01 to 2 mass %, more preferably 0.05 to 1 mass %, and particularly preferably 0.1 to 0.8 mass %, based on the total mass of the inkjet ink. When the content is adjusted to the above range, it becomes easy to improve the ejection stability of the inkjet ink while maintaining the curability.
[0125] <Organic solvents, water> In the inkjet ink of this embodiment, an organic solvent and / or water may be used in order to reduce the viscosity of the inkjet ink, improve the wetting and spreading properties and adhesion to the printing substrate, and ensure ejection stability. When an organic solvent and / or water is contained, the content is preferably 0.01 to 20 mass%, more preferably 0.05 to 10 mass%, and particularly preferably 0.1 to 5 mass%, based on the total mass of the inkjet ink. In addition, when an organic solvent is used, it is preferable to use an organic solvent having a boiling point of 140 to 300° C. in terms of ejection stability, and the wetting and spreading properties and adhesion to the printing substrate.
[0126] Examples of the organic solvent that can be used include alkylene glycol monoalkyl ether acetates, alkylene glycol diacetates, alkylene glycol monoalkyl ethers, alkylene glycol dialkyl ethers, alkanediols, lactams, lactones, other nitrogen-containing solvents, and other oxygen-containing solvents.
[0127] Among them, it is preferable to include at least one selected from the group consisting of alkylene glycol monoalkyl ethers, alkylene glycol dialkyl ethers, and alkylene glycol monoalkyl ether acetates. In particular, tripropylene glycol monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, tetraethylene glycol dialkyl ether, ethylene glycol monobutyl ether acetate, and diethylene glycol diethyl ether are preferable. In one embodiment, the organic solvent preferably includes at least one selected from the group consisting of tetraethylene glycol dialkyl ether, ethylene glycol monobutyl ether acetate, and diethylene glycol diethyl ether.
[0128] <Inert resin> The inkjet ink of the present embodiment may contain an inert resin for the purpose of imparting adhesion to various printing substrates and adjusting the viscoelasticity of the ink to improve ejection stability. As the inert resin, a (meth)acrylic resin, a urethane resin, a vinyl chloride-vinyl acetate copolymer resin, a ketone resin, etc. can be used. Among them, from the viewpoint of improving both adhesion and ejection stability, it is preferable that the inert resin contains a (meth)acrylic resin and / or a ketone resin.
[0129] When the inkjet ink of the present embodiment contains an inert resin, the content thereof is preferably 0.1 to 10 mass %, more preferably 0.5 to 5 mass %, and particularly preferably 1 to 3 mass %, based on the total mass of the inkjet ink. When the content is adjusted to within the above range, adhesion and ejection stability can be easily improved without deteriorating curability.
[0130] In the present application, the term "inert resin" refers to a resin that does not participate in the polymerization reaction, contributes to adhesion to the printing substrate, and has solubility in inkjet ink.
[0131] Other additives The inkjet ink of the present embodiment may further contain additives such as an ultraviolet absorber, an anti-fading agent, etc., in addition to the above-mentioned components, as necessary. Any conventionally known compounds can be used as these components.
[0132] <Physical properties of inkjet ink> From the viewpoint of improving the ejection stability, the inkjet ink of the present embodiment preferably has a viscosity at 25°C of 5 to 25 mPa·s, more preferably 8 to 20 mPa·s. If the viscosity is 5 mPa·s or more, the inkjet ink can be ejected well from the inkjet head. If the viscosity is 25 mPa·s or less, ejection accuracy does not decrease, and ejection can be continued stably. In addition, from the viewpoint of imparting high frequency suitability and enabling stable ejection even in high-speed printing, the above viscosity is particularly preferably 8 to 14 mPa·s. The above viscosity can be measured using 1.1 mL of inkjet ink and an E-type viscometer (for example, "TVE25L" manufactured by Toki Sangyo Co., Ltd.) equipped with a cone (diameter 48 mm) with a cone angle of 1°34', under conditions of 25°C and a rotation speed of 20 rpm.
[0133] From the viewpoint of improving all of the ejection stability, the definition of the printed matter, and the curing property, the static surface tension of the inkjet ink at 25°C is preferably 20 to 45 mN / m, and particularly preferably 22 to 40 mN / m. The static surface tension is a value measured by the plate method (Wilhelmy method). Specifically, for example, the static surface tension can be measured in a 25°C environment using an automatic surface tensiometer "CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd. and a platinum plate.
[0134] <Inkjet ink manufacturing method> The inkjet ink of the present embodiment can be produced by a conventionally known method, for example, as described below, but the method for producing the inkjet ink of the present embodiment is not limited to the method described below.
[0135] First, a basic pigment dispersion resin is dissolved in a polymerizable compound in advance to produce a basic pigment dispersion resin varnish. Next, carbon black satisfying the above-mentioned requirements is added little by little to the stirred basic pigment dispersion resin varnish and mixed. After mixing for a certain period of time, a dispersion process is performed using a dispersing machine such as a paint shaker, a sand mill, a roll mill, or a media-less dispersing machine to produce a carbon black dispersion liquid. In addition, from the viewpoint of improving the dispersion stability of carbon black, it is preferable to use a radical polymerizable bifunctional monomer and / or a radical polymerizable trifunctional monomer as the polymerizable compound used to produce the basic pigment dispersion resin varnish, and it is particularly preferable to use a radical polymerizable bifunctional monomer represented by the above general formula (A) and / or a radical polymerizable trifunctional monomer represented by the above general formula (B).
[0136] Thereafter, 5-methyl-3-vinyloxazolidin-2-one, and, if necessary, a photopolymerization initiator, a surface modifier, a polymerization inhibitor, an organic solvent, water, an inert resin, and other additives are added to the carbon black dispersion and thoroughly mixed, and then the mixture is filtered through a filter or the like to remove coarse particles, thereby obtaining the inkjet ink of the present embodiment.
[0137] The amount of carbon black present in the carbon black dispersion is preferably 10 to 50% by mass, more preferably 12 to 40% by mass, and particularly preferably 15 to 30% by mass.
[0138] <Inkjet printing method> The inkjet ink of the present embodiment described above is preferably used in an inkjet printing method, which preferably includes, in this order, a step (step I) of ejecting the inkjet ink of the present embodiment from an inkjet head onto a printing substrate, and a step (step II) of irradiating the inkjet ink ejected onto the printing substrate with active energy rays to cure the inkjet ink.
[0139] In the inkjet printing method, a method of ejecting and applying the same inkjet ink from the same inkjet head multiple times to the same location on the printing substrate, i.e., a method of performing the above-mentioned step I multiple times to the same location on the printing substrate (multi-pass printing method) may be adopted. However, in the case of the inkjet printing method using the inkjet ink of the present embodiment, from the viewpoint that the effect of the inkjet ink, which is excellent in curability and ejection stability, is fully exhibited and a printed matter can be obtained quickly and stably, a method of ejecting and applying the same inkjet ink from the same inkjet head only once to the same location on the printing substrate is preferred. In other words, a method of performing the above-mentioned step I only once to the same location on the printing substrate (one-pass printing method) is preferably adopted.
[0140] The one-pass printing method can be carried out, for example, by using a line printer, etc. In this case, the printing speed (the conveying speed of the printing substrate) is preferably 35 to 150 m / min, more preferably 50 to 125 m / min, and even more preferably 75 to 100 m / min, from the viewpoint of obtaining a printed matter having good productivity and good quality.
[0141] The inkjet ink of the present embodiment is an ink for inkjet printing, and therefore, as described above, an inkjet head is used as the inkjet ink ejection means in the step I.
[0142] Examples of ink ejection methods using an inkjet head include an electrostatic attraction method that ejects ink using electrostatic force, a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electric signal into an acoustic beam and irradiates the ink, and ejects the ink using the radiation pressure at that time, and a thermal inkjet method that heats the ink to form bubbles, and ejects the ink using the generated pressure, etc. Among them, in one embodiment, from the viewpoint of ejection stability, the drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element can be preferably used.
[0143] From the viewpoints of print definition and ejection stability, the drop volume of the inkjet ink droplets ejected from the inkjet nozzle is preferably 1 to 50 pL (picoliters), more preferably 2 to 30 pL, and even more preferably 3 to 20 pL. The design resolution of the inkjet head is preferably 300 dpi or more, more preferably 480 dpi or more, and even more preferably 600 dpi or more. Here, dpi refers to the number of dots per 2.54 cm (1 inch).
[0144] Examples of inkjet heads that satisfy the above conditions include KJ4A-AA, KJ4A-TA, and KJ4A-RH manufactured by Kyocera Corporation, Samba G3L manufactured by Fujifilm Corporation, S3200, S1600, S800, I3200, and I1600 manufactured by Seiko Epson Corporation, KM1024i and KM1024 manufactured by Konica Minolta, and MH5320, MH5340, MH5240, and MH5440 manufactured by Ricoh Co., Ltd., and any of these can be suitably used.
[0145] In one embodiment, the inkjet ink can be discharged while being heated by a heating device such as a heater provided in the inkjet head so that the inkjet ink has an appropriate viscosity. From the viewpoint of continuously and stably discharging the inkjet ink, it is preferable to heat the inkjet ink so that the viscosity of the inkjet ink during discharge is 15 mPa s or less, and more preferably 12 mPa s or less.
[0146] On the other hand, in the above step II, the inkjet ink ejected onto the printing substrate is cured by being irradiated with active energy rays, and a cured film (printed matter) is formed.
[0147] In the present application, the term "active energy rays" refers to energy rays that can provide energy required to generate active species such as radicals, cations, anions, etc. in the irradiated object (inkjet ink). Specific examples of active energy rays include ultraviolet rays, electron beams, visible light, infrared rays, etc., but it is preferable to select ultraviolet rays because they can easily improve the curing property of the inkjet ink and provide a high degree of freedom in designing the inkjet ink and the printing device.
[0148] In addition, the light source of the ultraviolet ray may be, for example, a high pressure mercury lamp, a low pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, an ultraviolet laser, an LED lamp, etc., and any one of them may be used alone or two or more of them may be used in combination. For example, since the LED lamp has a small shape, it is easy to arrange a plurality of them side by side or to use them together with a high pressure mercury lamp or a metal halide lamp, and it is easy to further improve the curing property. In addition, when a plurality of LED lamps are arranged side by side, a plurality of types of LED lamps with different emission peak wavelengths may be used in combination.
[0149] Generally, the ultraviolet rays emitted from an LED lamp have a narrow wavelength range and are excellent in linearity (i.e., poor diffusion), so that active energy ray curable inkjet inks are difficult to cure. In particular, in the case of inkjet inks containing carbon black, it is considered difficult to cure with an LED lamp due to the above-mentioned reasons, that is, the ultraviolet rays are absorbed by the carbon black, and the quinone groups on the carbon black surface may trap radicals. However, the inkjet ink of the present embodiment has particularly excellent curability, so it can be suitably combined with an LED lamp.
[0150] In the inkjet printing method using the inkjet ink of this embodiment, when ultraviolet light is selected as the active energy ray and an LED lamp is used as the light source of the ultraviolet light, the emission peak wavelength is preferably 260 to 450 nm, more preferably 280 to 420 nm, and particularly preferably 320 to 410 nm.
[0151] When an LED lamp that emits ultraviolet light is used in step II, the above-mentioned effects are fully exerted, and from the viewpoint of obtaining a printed matter having excellent print quality including curing property and print definition, the maximum illuminance of the ultraviolet light on the printing substrate is set to 1,000 mW / cm. 2 The maximum illuminance is preferably 2,000 mW / cm or more. 2 More preferably, it is 3,000 mW / cm or more. 2 The integrated amount of light irradiated onto the printing substrate varies depending on the type and content of the polymerizable compound and photopolymerization initiator contained in the inkjet ink, but is preferably 50 mJ / cm or more. 2 The integrated light quantity is preferably 100 mJ / cm or more. 2 More preferably, it is 150 mJ / cm or more. 2 It is particularly preferable that the amount is equal to or more than this.
[0152] In the above step I, after the droplets of the inkjet ink are attached to the printing substrate (i.e., after the above step I is completed), irradiation with active energy rays is started (i.e., the above step II is started). The time from the end of step I to the start of step II is preferably adjusted to 0.03 to 3 seconds. The above time is more preferably 0.04 to 2.5 seconds, and even more preferably 0.6 to 2 seconds. By adjusting the above time within the above range, the dot forming properties of the inkjet ink are improved, and a printed matter with excellent definition can be obtained.
[0153] In the inkjet printing method, the step II can be repeated multiple times. For example, immediately after applying the inkjet ink to the printing substrate, the inkjet ink can be partially cured by irradiating the inkjet ink with active energy rays, and then the inkjet ink can be completely cured by irradiating the inkjet ink with active energy rays again. In this manner, it is easy to obtain a printed matter having particularly excellent print quality including the fineness of the printed matter. In the present application, the above-mentioned step of partially curing the inkjet ink is referred to as "temporary curing", and the step of completely curing the inkjet ink is referred to as "main curing".
[0154] That is, in one embodiment, an inkjet printing method using the inkjet ink of the present embodiment may include, in this order, a step of ejecting the inkjet ink from an inkjet head onto a printing substrate (step I), a step of irradiating the inkjet ink ejected onto the printing substrate with active energy rays to provisionally cure the inkjet ink (step II-A), and a step of fully curing the inkjet ink (step II-B).
[0155] When carrying out the above step II-A, that is, when provisionally curing the inkjet ink discharged onto the printing substrate, it is preferable to use an LED lamp that emits ultraviolet rays. In this case, from the viewpoint of significantly improving the print image quality including the definition of the printed matter, the maximum illuminance of the ultraviolet rays on the printing substrate in the provisional curing is 2 to 20 mW / cm. 2is preferably 5 to 15 mW / cm 2 It is more preferable that:
[0156] Also, when carrying out the above-mentioned step II-B, i.e., when the inkjet ink discharged onto the printing substrate is cured, an LED lamp that emits ultraviolet rays can be used. In this case, the above-mentioned 1,000 mW / cm 2 Maximum illumination of 50mJ / cm 2 It is preferable to use the above integrated light amount.
[0157] On the other hand, in step II-B, ultraviolet light can be irradiated using a high pressure mercury lamp or a metal halide lamp. In this case, the maximum illuminance of the ultraviolet light is 80 mW / cm. 2 More preferably, it should be 120 mW / cm or more. 2 It is more preferable that the integrated light amount is 100 mJ / cm or more. 2 More preferably, it is 150 mJ / cm or more. 2 More preferably, it is 200 mJ / cm or more. 2 More preferably, it is equal to or more than that.
[0158] <Printing base material> The printing substrate used in the printing method using the inkjet ink of this embodiment is preferably a resin film substrate or a paper substrate. The resin film substrate may preferably have a thickness of 10 to 90 μm. In addition, a substrate containing a material selected from the group consisting of polypropylene, polyethylene, polyethylene terephthalate, and nylon is preferably selected as the resin film substrate. Meanwhile, coated paper, art paper, laminated paper, and the like are preferably selected as the paper substrate. In one embodiment, the inkjet ink of this embodiment is preferably used for printing packages formed from the printing substrates listed above. Among the printing of the packages, it is particularly suitable for printing food packaging.
[0159] The "substrate containing a material selected from the group consisting of polypropylene, polyethylene, polyethylene terephthalate, and nylon" is not limited to a single-layer structure, and may have a multilayer structure. That is, the substrate may be a resin film substrate having one layer made of a material selected from the group consisting of polyethylene terephthalate, polyethylene, polypropylene, and nylon, or a resin film substrate (laminated film substrate) having two or more of the above layers. In addition, for the purpose of improving the strength of the package, blocking oxygen, etc., the layers constituting the laminated film substrate may include layers made of AL (aluminum foil) and VM (vacuum deposition) film (aluminum deposition film, transparent deposition film), etc.
[0160] <Printed material> The inkjet ink of the present embodiment can be used to produce a printed matter (a printing substrate on which print information is recorded). The above-mentioned inkjet printing method can be used as a method for producing the printed matter. EXAMPLES
[0161] The present invention will be described in more detail below, but the following examples are not intended to limit the scope of the present invention. In addition, unless otherwise specified, "parts" refers to parts by mass, and "%" refers to % by mass.
[0162] <Ingredients used> In the examples shown below, the carbon blacks used were those shown in Table 1. In Table 3 described later, the carbon blacks used are listed by their abbreviations.
[0163] [Table 1]
[0164] In the examples shown below, the pigment dispersion resins shown in Table 2 were used. In Table 3 described later, the pigment dispersion resins used are listed by abbreviation. Among the pigment dispersion resins shown in Table 2 below, the pigment dispersion resins except for Solsperse 41000 are basic pigment dispersion resins, and the above Solsperse 41000 is an acidic pigment dispersion resin (a pigment dispersion resin whose adsorption points with the pigment are acid groups).
[0165] [Table 2]
[0166] <Production of Carbon Black Dispersion> Carbon black dispersions 1 to 27 were produced using the raw materials listed in each column of Table 3 below. Specifically, first, a pigment dispersion resin and a polymerizable compound were charged into a mixing vessel (volume 8 L) equipped with a stirrer, and the mixture was stirred for 1 hour (premixing) to produce a pigment dispersion resin varnish. Next, carbon black was added little by little to the stirred pigment dispersion resin varnish, and after the addition was completed, the mixture was further stirred for 1 hour (pre-dispersion). After that, the mixture was circulated and dispersed for 2 hours using Shinmaru Enterprises' "Dyno Mill" (volume 0.6 L) filled with zirconia beads having a diameter of 0.8 mm so that the filling rate was 70%, to produce a carbon black dispersion.
[0167] [Table 3]
[0168] [Table 3]
[0169] [Table 3]
[0170] Table 3 also lists the secondary particle size and the pigment dispersion resin content relative to the carbon black content for the carbon black dispersions 1 to 27 produced by the above-mentioned method. Among the abbreviations used in Table 3, details of those not listed in Tables 1 and 2 are as follows: HDDA: 1,6-Hexanediol diacrylate ·DPGDA: Dipropylene glycol diacrylate NDDA: 1,9-nonanediol diacrylate
[0171] <Inkjet ink manufacturing> The materials shown in each column of Table 4 below were added to a mixing vessel equipped with a stirrer. After all the materials were added, the mixture was heated while being stirred until the temperature of the mixture reached 40°C. After the temperature reached 40°C, stirring was continued for another hour while maintaining the temperature. After that, the mixture was filtered through a membrane filter with a pore size of 0.8 μm to produce inkjet inks 1 to 96.
[0172] In the production of the inkjet ink, each material was added while stirring the mixture in the mixing vessel. The order of addition of each material was carbon black dispersion, polymerizable compound other than 5-methyl-3-vinyloxazolidin-2-one, 5-methyl-3-vinyloxazolidin-2-one, photopolymerization initiator, polymerization initiator, and surface conditioner. However, when producing an inkjet ink that does not contain one or more of these components, the component was not added, and the next component was added in the order. In addition, for components that contain two or more materials, the order of addition was from the largest amount to the smallest amount.
[0173] [Table 4]
[0174] [Table 4]
[0175] [Table 4]
[0176] [Table 4]
[0177] [Table 4]
[0178] [Table 4]
[0179] [Table 4]
[0180] [Table 4]
[0181] [Table 4]
[0182] [Table 4]
[0183] Among the abbreviations used in Table 4, details of those not listed in Tables 1 to 3 are as follows: PDDA: 1,3-propanediol diacrylate BDDA: 1,4-butanediol diacrylate ·MPDDA: 3-Methyl-1,5-pentanediol diacrylate GlyTA: Glycerol triacrylate Gly(EO)3TA: Ethylene oxide modified glycerin triacrylate (ethylene oxide group number: 3) Gly(EO)9TA: Ethylene oxide modified glycerin triacrylate (ethylene oxide group number: 9) CHA: Cyclohexyl acrylate IBXA: Isobornyl acrylate BzA: Benzyl acrylate ·VCL: N-vinylcaprolactam PEG400DA: Polyethylene glycol 400 diacrylate TMP(EO)3TA: Ethylene oxide modified trimethylolpropane triacrylate (ethylene oxide group number: 3) · TMP(PO)2TA: Propylene oxide modified trimethylolpropane tri(meth)acrylate (number of propylene oxide groups: 2) MVOZ: 5-Methyl-3-vinyloxazolidin-2-one TPO-L: Ethoxyphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (IGM RESINS "Omnirad TPO-L") OmnTP: Ethoxyphenyl (2,4,6-trimethylbenzoyl) phosphine oxide polymer (IGM RESINS "OMNIPOL TP") Omn819: Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (IGM RESINS "Omnirad 819") DETX: 2,4-diethylthioxanthone (IGM RESINS "Omnirad DETX") OmnTX: Polymer of 3-ethoxycarbonylmethoxythioxanthone ("OMNIPOL TX" manufactured by IGM RESINS) Omn379: 2-(dimethylamino)-2-(4-methylbenzyl)-1-(4-morpholinophenyl)butan-1-one (IGM RESINS "Omnirad 379") ASA: Polyethylene glycol-bis(p-dimethylaminobenzoate) (IGM RESINS "Omnipol ASA") ·BHT: 2,6-di-tert-butyl-4-methylphenol UV3510: Polyether modified siloxane surface conditioner (BYK-UV3510 manufactured by BYK Chemie)
[0184] <Production of printed matter> Using the inkjet ink prepared above, printed matter was produced by the method described below. A temperature-adjustable inkjet head (KJ4A, design resolution 600 dpi) manufactured by Kyocera was installed above the conveyor that can transport the printing substrate. In addition, a main curing LED lamp (FirePower FP300 manufactured by Phoseon (maximum emission wavelength 395 nm, maximum illuminance 16,000 mW / cm) was installed downstream of the transport direction of the printing substrate. 2 )) was installed. The inkjet head was filled with the inkjet ink prepared above. The temperature of the inkjet head was then adjusted so that the viscosity of the inkjet ink at the time of ejection was 6 to 7 mPa·s. After that, a PET substrate "K2411" manufactured by Lintec Corporation was fixed on a conveyor, and the conveyor was driven at a speed of 50 m / min. When the PET substrate passed the area where the inkjet head was installed, inkjet ink droplets were ejected from the inkjet head to perform printing. Specifically, a solid image with a print rate of 100% and a character image (random hiragana characters printed in MS Mincho font at sizes of 4 points, 6 points, and 8 points, 20 of each) were printed under printing conditions of an ejection droplet volume of 11 pL and a printing resolution of 600 dpi x 600 dpi. After printing the inkjet ink, the conveyor was still driven at the same speed, and when the PET substrate passed the area where the main curing LED lamp was installed, ultraviolet light was irradiated to produce a printed product. The illuminance of the ultraviolet light irradiated on the inkjet ink after printing is 6,000mW / cm 2 , and the cumulative light amount is 150 mJ / cm 2The output of the LED lamp was adjusted in advance so that the above-mentioned printing was performed.
[0185] [Examples 1 to 87, Comparative Examples 1 to 9] Using the inkjet inks and printed matter produced by the above-mentioned methods, various evaluations were carried out according to the methods described below. The evaluation results are shown in Table 4.
[0186] <Evaluation 1: Evaluation of dispersion stability> The secondary particle diameter of each of the inkjet inks was measured immediately after production using the measuring device and method described above. Next, each inkjet ink was filled into a 20 mL glass container so that the filling rate was 80% of the container volume. The glass container filled with the inkjet ink was then left to stand for two weeks in a sealed and light-shielded environment at 60°C, and the secondary particle diameter of the inkjet ink after standing was measured again. The dispersion stability was evaluated by calculating the increase rate of the secondary particle diameter before and after standing. The evaluation criteria for the dispersion stability were as follows, and a rating of "2" or higher was deemed practical, and a rating of "3" or higher was deemed practically suitable.
[0187] <Evaluation criteria for dispersion stability> 4: The increase in secondary particle size was less than 10% 3: The increase in secondary particle size was 10% or more but less than 20%. 2: The increase in secondary particle size was 20% or more but less than 30%. 1: The increase in secondary particle size was 30% or more
[0188] <Evaluation 2: Evaluation of ejection stability> Inkjet ink was filled into a jig equipped with a temperature-adjustable Kyocera inkjet head (KJ4A, design resolution 600 dpi). The temperature of the inkjet head was then adjusted so that the inkjet ink viscosity during ejection was 6-7 mPa s. After that, it was confirmed that there were no nozzles from which the inkjet ink was not being ejected, and then inkjet ink was continuously ejected from all nozzles at a drive frequency of 20 kHz. After five minutes of continuous ejection, the number of nozzles from which the inkjet ink was not being ejected (nozzle loss number) was counted to evaluate the ejection stability. The evaluation criteria for the above ejection stability were as follows, and a rating of "2" or higher was deemed to be practical. However, for the inkjet inks that were rated "1" in the above-mentioned dispersion stability evaluation, there was a high risk of damaging the inkjet head, so the ejection stability was not evaluated.
[0189] <Evaluation criteria for ejection stability> 4: The number of nozzle losses was 0 to 2 3: The number of nozzle losses was between 3 and 5 2: The number of nozzle losses was 6 to 9 1: The number of nozzle losses was 10 or more
[0190] <Evaluation 3: Evaluation of curability> The surface of the printed matter of the solid image with a printing rate of 100% produced by the above method was rubbed with a cotton swab to check whether the uncured ink was attached to the cotton swab. If the inkjet ink was attached to the cotton swab, the printed matter was fixed to the conveyor of the inkjet printing device, and the inkjet ink was not printed, but was only irradiated with the main curing LED lamp. After that, the presence or absence of the inkjet ink was checked when the cotton swab was rubbed again. This procedure was repeated, and the number of passes required until the uncured inkjet ink no longer adhered to the cotton swab was investigated to evaluate the curability. The evaluation criteria for the curability were as follows, and a rating of "2" or higher was deemed practical, and a rating of "3" or higher was deemed suitable for practical use.
[0191] <Curability evaluation criteria> 4: After one total pass (without the need for additional UV exposure), the swab had no uncured ink left on it. 3: After two passes (one additional UV exposure), the uncured inkjet ink no longer adheres to the cotton swab. 2: After passing the swab three times in total (with two additional UV exposures), there was no more uncured inkjet ink remaining on the swab. 1: It was necessary to expose the cotton swab to the LED lamp a total of four times until the uncured inkjet ink was no longer attached to the cotton swab.
[0192] <Evaluation 4: Evaluation of print definition (character visibility)> The definition (character visibility) of the printed matter was evaluated by visually checking whether the hiragana characters in the character images created by the above method could be read. The definition evaluation criteria are as follows, with a rating of "2" or higher being deemed usable, and a rating of "3" or higher being deemed suitable for practical use.
[0193] <Evaluation criteria for print definition (text visibility)> 4: All 20 hiragana characters were distinguishable at 4 point, 6 point, and 8 point. 3: All 20 hiragana characters could be distinguished in both 6-point and 8-point fonts, but some hiragana characters printed in 4-point font were indistinguishable. 2: All 20 hiragana characters could be distinguished in all 8-point fonts, but some hiragana characters printed in 6-point font were indistinguishable. Among the hiragana characters printed at 1:8 point, some were indistinguishable.
[0194] As shown in Table 4 above, the inkjet inks of Examples 1 to 87 having the above-mentioned configurations were excellent in all of the dispersion stability of carbon black, the ejection stability, the curing properties, and the definition of the printed matter.
[0195] On the other hand, the inkjet inks of Comparative Examples 1 to 4, which used carbon black having a product (AC×SC) of DBP oil absorption (AC) and specific surface area (SC) of more than 12,000, did not reach a practical level in dispersion stability or ejection stability. In addition, the inkjet inks of Comparative Examples 3 and 4, which have particularly large values of the product, had practical levels in terms of curability and print definition, but did not reach practically suitable levels. In contrast, the inkjet inks of Examples 1 to 7, which used carbon black having a value of the product of 2,000 to 12,000, had practical levels in dispersion stability and ejection stability, and also had practically suitable levels in terms of curability and print definition. From the above results, it was confirmed that controlling the value of the product is important for achieving the above-mentioned effects.
[0196] In addition, the dispersion stability and ejection stability did not reach a practical level in Comparative Example 5, which used an acidic pigment dispersion resin, Solsperse 41000, and Comparative Example 6, which used a basic pigment dispersion resin (DISPERBYK-180) with an acid value of more than 30 mgKOH / g. In these examples, it is believed that the acid value of the pigment dispersion resin used was too high, causing the acid group in the pigment dispersion resin to react with the vinyl group in 5-methyl-3-vinyloxazolidin-2-one, deteriorating the dispersion stability and ejection stability of the carbon black.
[0197] The inkjet ink of Comparative Example 7 is a system in which the content of monofunctional polymerizable compounds other than 5-methyl-3-vinyloxazolidin-2-one is more than 15 mass%, and the evaluation results confirmed that the curability did not reach a practical level. In addition, the definition of the printed matter was at a practical level, but not at a level suitable for practical use.
[0198] In addition, in the inkjet ink of Comparative Example 8, in which N-vinylcaprolactam, a representative example of N-vinyl compounds, was used instead of 5-methyl-3-vinyloxazolidin-2-one, the dispersion stability did not reach a practical level, and the curability and the definition of the printed matter were at a practical level, but not at a practically suitable level. Compared with the inkjet ink of Example 2, in which 5-methyl-3-vinyloxazolidin-2-one was used instead of N-vinylcaprolactam, the inkjet ink of Comparative Example 8 was significantly inferior in quality, and it was confirmed that 5-methyl-3-vinyloxazolidin-2-one is an essential material in the inkjet ink of this embodiment.
[0199] Furthermore, the importance of 5-methyl-3-vinyloxazolidin-2-one in the inkjet ink of the present embodiment was also confirmed by the fact that the curability and the definition of the printed matter of the inkjet ink of Comparative Example 9, which does not contain 5-methyl-3-vinyloxazolidin-2-one, did not reach a practical level.
Claims
1. An active energy ray-curable inkjet black ink comprising carbon black, a basic pigment dispersion resin, and a polymerizable compound, The DBP oil absorption of the carbon black is AC (mL / 100 g), and the specific surface area of the carbon black is SC (m 2 / g), the value represented by AC×SC is 2,000 to 12,000, The basic pigment dispersing resin has an acid value of 30 mgKOH / g or less, the polymerizable compound comprises 5-methyl-3-vinyloxazolidin-2-one, The active energy ray curable inkjet black ink has a content of a monofunctional polymerizable compound (excluding the 5-methyl-3-vinyloxazolidin-2-one) of 15% by mass or less based on a total amount of the active energy ray curable inkjet black ink.
2. the polymerizable compound contains a radically polymerizable bifunctional monomer represented by general formula (A), 2. The active energy ray curable inkjet black ink according to claim 1, wherein the content of the radical polymerizable bifunctional monomer represented by general formula (A) is 15 to 55 mass % of the total amount of the active energy ray curable inkjet black ink. General formula (A): CH 2 =CR 1 -C-O-R 2 -O-CO-CR 1 =CH 2 (In general formula (A), R 1 represents a hydrogen atom or a methyl group, R 2 represents an alkylene group having 3 to 6 carbon atoms which may have a branched structure.
3. the polymerizable compound contains a radical polymerizable trifunctional monomer represented by general formula (B), 3. The active energy ray curable inkjet black ink according to claim 1, wherein the content of the radical polymerizable trifunctional monomer represented by general formula (B) is 2 to 15 mass % of the total amount of the active energy ray curable inkjet black ink. General formula (B): [Formula 1] (In general formula (B), R 3 represents a hydrogen atom or a methyl group, R 4 is an ethylene group or a propylene group. In addition, l, m, and n each represent an integer of 0 to 9, and l+m+n is an integer of 0 to 9.
4. Further, a photopolymerization initiator is included, The active energy ray-curable inkjet black ink according to claim 1 , wherein the photopolymerization initiator comprises an acylphosphine oxide compound.
5. The active energy ray-curable inkjet black ink according to claim 4 , wherein the photopolymerization initiator further comprises a thioxanthone compound.
6. The acylphosphine oxide compound contains ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or a polymer of ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, The active energy ray-curable inkjet black ink according to claim 4 or 5, wherein a total content of the ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and the ethoxyphenyl(2,4,6-trimethylbenzoyl)phosphine oxide is 45 to 80 mass % in a total amount of the photopolymerization initiator.
7. 6. The active energy ray-curable inkjet black ink according to claim 1, 2, 4 or 5, wherein the carbon black has a pH of 2 to 5.
8. 6. A printed matter obtained by printing the active energy ray-curable inkjet black ink according to claim 1, 2, 4 or 5 on a printing substrate.
Citation Information
Patent Citations
Carbon black and black photopolymerizable composition
JP2002265816A
Ultraviolet curable ink composition for ink-jet recording
JP2004027211A
Active energy ray-curable type ink-jet ink composition
JP2006348202A
Photocurable inkjet ink and inkjet recording method
JP2008266548A
Ultraviolet curable ink composition for inkjet printing and printing method