Medical tubing and compositions and methods for making same

Hydrogenated styrene block copolymers with tailored molecular structures enhance medical tubing quality by providing clarity, kink resistance, and mechanical stability, addressing regulatory compliance and usability issues.

JP7576392B2Active Publication Date: 2024-10-31クレイトン·ポリマーズ·ネーデルラント·ベー·フェー
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2019156377
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-10
Filing Date
2019-08-29
Publication Date
2024-10-31
Estimated Expiration
2039-08-29

AI Technical Summary

Technical Problem

There is a need for medical tubing and polymer compositions that exhibit better quality, transparency, flexibility, and mechanical properties while meeting regulatory standards for direct contact with blood and passing pharmacopoeial eluate evaluation tests.

Method used

The development of hydrogenated styrene block copolymers with specific molecular weight ranges and blockiness indices, coupled with optional additives, to create medical tubing with high clarity, kink resistance, and desirable mechanical properties.

Benefits of technology

The hydrogenated styrene block copolymers provide medical tubing with improved clarity, kink resistance, and stable mechanical properties, ensuring compliance with regulatory standards and ease of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576392000001
    Figure 0007576392000001
  • Figure 0007576392000002
    Figure 0007576392000002
Patent Text Reader

Abstract

To provide a medical tube containing a hydrogenated styrene block copolymer having formulae A-B-A, (A-B-A)X or (A-B)X, wherein n is an integer of 2 to 30, and X is a residue of a coupling agent.SOLUTION: Each A block is a monoalkenyl arene homopolymer block having true peak molecular weight of 5 kg / mol to 15 kg / mol before hydrogenation. Each B block is a controlled distribution copolymer block having true peak molecular weight of 30 kg / mol to 200 kg / mol. A hydrogenated styrene block copolymer has content of an intermediate block poly(monoalkenyl arene) of 35 wt.% to 50 wt.% based on total mass of the intermediate block and physical properties useful when a medical tube having kink resistance is manufactured.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to U.S. Provisional Application No. 62 / 729,058, filed Sep. 10, 2018, the disclosure of which is incorporated by reference in its entirety for all purposes.

[0002] FIELD OF THE DISCLOSURE The present disclosure relates to medical tubing and compositions and methods thereof. [Background technology]

[0003] Hydrogenated styrene block copolymers are widely used as an alternative to vulcanized rubber or vinyl chloride monomer-based resins in the preparation of various molded articles, including medical articles. Polyolefin-based resins are also blended with hydrogenated styrene block copolymers to provide polymer compositions that are also used as useful alternatives to vinyl chloride monomer-based resins in applications such as food contact, home appliances, and medical tubing. The latter application is subject to strict regulatory constraints, as the product comes into direct contact with blood and must pass tests for extractables evaluation according to pharmacopoeia protocols. Summary of the Invention [Problem to be solved by the invention]

[0004] There remains a need for better quality medical tubing and polymer compositions therefor that not only address the above deficiencies but also have other desirable characteristics such as good transparency, flexibility and mechanical properties. [Means for solving the problem]

[0005] Summary of the Invention One aspect of the present disclosure is a compound of formula ABA, (ABA) n X, (AB) nA medical tube comprising a hydrogenated styrene block copolymer having X, where n is an integer from 2 to 30, and X is a residue of a coupling agent for the styrene block copolymer having X, or a mixture thereof. Before hydrogenation, each A block is a monoalkenyl arene homopolymer block having a true peak molecular weight of 5 kg / mol to 15 kg / mol, and each B block has a true peak molecular weight of 30 kg / mol to 200 kg / mol. The B block is a controlled distribution copolymer block of at least one conjugated diene and at least one monoalkenyl arene. The coupling efficiency is 30% to 95% for the styrene block copolymer having X. The blockiness index of the midblock monoalkenyl arene is 3% to 15%. The blockiness index of the monoalkenyl arene is the proportion of monoalkenyl arene units in block B having two alkenyl arene neighbors on the polymer chain. After hydrogenation, 0-10% of the arene double bonds are reduced, at least 90% of the conjugated diene double bonds are reduced, and the hydrogenated styrenic block copolymer has a midblock poly(monoalkenyl arene) content of 35% to 70% by weight based on the total weight of the midblock. The hydrogenated styrenic block copolymer has a melt flow ratio of 1.0-10.0 measured at 230°C and 2.16 kg load according to ASTM D-1238; a Shore A hardness of 60-80 measured according to ASTM D-2240; a DMA peak tan δ temperature at 1 Hz of 0°C to 40°C, and an order-disorder transition temperature of 200°C to 300°C measured according to ASTM D-4065.

[0006] Another aspect of the present disclosure is medical tubing consisting essentially of the above-described hydrogenated styrene block copolymer.

[0007] Yet another aspect of the present disclosure is a compound of formula ABA, (ABA) n X, (AB) nA medical tube consisting essentially of a hydrogenated styrene block copolymer having X, where n is an integer from 2 to 30, and X is a residue of a coupling agent for the styrene block copolymer having X, or a mixture thereof. Before hydrogenation, each A block is a styrene homopolymer block having a true peak molecular weight of 5 kg / mol to 15 kg / mol, and each B block has a true peak molecular weight of 30 kg / mol to 50 kg / mol. The B block is a controlled distribution copolymer block of styrene and at least one conjugated diene selected from 1,3-butadiene, isoprene, and mixtures thereof. The coupling efficiency is 80% to 95% for the styrene block copolymer having X, and the blockiness index of the midblock monoalkenyl arene is 3% to 15%. The blockiness index of the monoalkenyl arene is the proportion of monoalkenyl arene units in block B having two monoalkenyl arene neighbors on the polymer chain. After hydrogenation, 0-10% of the arene double bonds are reduced and at least 90% of the conjugated diene double bonds are reduced, and the hydrogenated styrenic block copolymer has a midblock poly(monoalkenyl arene) content of 35% to 50% by weight based on the total weight of the midblock. The hydrogenated styrenic block copolymer has a melt flow ratio of 1.0 to 10.0 measured at 230°C and 2.16 kg load according to ASTM D-1238; a Shore A hardness of 60 to 80 measured according to ASTM D-2240; a DMA peak tan δ temperature at 1 Hz of 0°C to 40°C, and an order-disorder transition temperature of 200°C to 300°C, measured according to ASTM D-4065. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The following terms are used herein and shall have the following meanings:

[0009] "Apparent kink diameter" is the diameter of the semicircular portion of a flexible tube when bent to the point where the tube begins to kink.

[0010] "Midblock styrene blockiness" refers to the proportion of styrene units in the midblock of a polymer that have two styrene units as nearest neighbors on the polymer chain. Styrene blockiness can be determined by 1H NMR spectroscopy using the method described in U.S. Pat. No. 7,244,785 (B2).

[0011] "Controlled distribution" refers to a molecular structure having the following attributes: (1) a terminal region adjacent to a monoalkenyl arene homopolymer ("A") block that is rich in conjugated diene units (i.e., has a greater than average amount of conjugated diene units); (2) one or more regions not adjacent to the A block that are rich in monoalkenyl arene units (i.e., has a greater than average amount of monoalkenyl arene units); and (3) an overall structure with relatively low blockiness. The term "rich" is defined as greater than the average amount, preferably greater than 5% greater than the average amount.

[0012] "Polyolefin-free" means that no polyolefins are intentionally added. In one embodiment, the term means that less than 0.5% by weight of polyolefins are present.

[0013] The present disclosure provides medical tubing comprising hydrogenated styrenic block copolymers having a suitable combination of high clarity, good kink resistance and other physical properties. In another embodiment, the present disclosure provides medical tubing consisting essentially of styrenic block copolymers, e.g., without the addition of polyolefins. The hydrogenated SBCs are useful for making medical tubing.

[0014] Hydrogenated styrene block copolymer (SBC) component: Hydrogenated SBC has the structure ABA, (ABA) n X, (AB) nX, where n is an integer from 2 to 30, and X is a residue of a coupling agent for a styrene block copolymer having X, or a mixture thereof. Before hydrogenation, the A block is preferably a monoalkenyl arene homopolymer block having a true peak molecular weight of 5 kg / mol to 15 kg / mol; each B block is a controlled distribution copolymer block of at least one conjugated diene and at least one monoalkenyl arene, having a true peak molecular weight of 30 kg / mol to 200 kg / mol. In addition, the midblock monoalkenyl arene blockiness index is preferably 5% to 10%. After hydrogenation, the midblock poly(monoalkenyl arene) content in the hydrogenated SBC is 35% to 50% by weight based on the total weight of the midblock. In some embodiments, the coupling efficiency is 30 to 95%.

[0015] In embodiments, the A block has a true peak molecular weight of 5 kg / mol to 15 kg / mol. In embodiments, the B block has a true peak molecular weight of 30 kg / mol to 200 kg / mol, or 30 to 150 kg / mol, or 80 to 150 kg / mol. In embodiments, the blockiness index of the midblock monoalkenyl arene is 3% to 15%. In other embodiments, the hydrogenated SBC has a midblock poly(monoalkenyl arene) content of 35 to 65 wt%, 40 to 65 wt%, or 40 to 60 wt%. In some embodiments, prior to hydrogenation, the SBC has a midblock vinyl content of 30 to 90 mol%, 50 to 70 mol%, 30 to 40 mol%, or 35 to 40 mol%. In embodiments, the total molecular weight of the hydrogenated SBC is 60 to 200 kg / mol or 80 to 120 kg / mol. In other embodiments, the overall block copolymer after hydrogenation has a total poly(monoalkenyl arene) content of from 40 to 80 weight percent, or from 50 to 70 weight percent, or from 60 to 70 weight percent.

[0016] Hydrogenated SBCs can be prepared by methods known in the art. They are generally prepared by contacting one or more monomers with an organoalkali metal compound in a suitable solvent at a temperature range of −150 to 300° C., preferably 0 to 100° C. Hydrogenation of the pendant vinyl groups and the in-chain double bonds present in the block copolymer chain is carried out under conditions such that at least 90 mol %, at least 95 mol %, or at least 98 mol % of the vinyl groups are reduced and 0 to 10 mol % of the arene double bonds are reduced. In the hydrogenation step, a suitable catalyst based on nickel, cobalt, or titanium is used.

[0017] Suitable monoalkenyl arene compounds useful in making the A and B blocks include those having from 8 to 20 carbon atoms and include styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinyltoluene, and vinylxylene or mixtures thereof. In one embodiment, the monoalkenyl arene is styrene.

[0018] Suitable conjugated dienes include those having 4 to 8 carbon atoms, such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. Mixtures of such dienes can also be used. In one embodiment, the conjugated diene is 1,3-butadiene. In another embodiment, the conjugated diene is a mixture of 1,3-butadiene and isoprene.

[0019] Optional components: The polymeric composition having hydrogenated SBC can be made to further include one or more optional additives such as tackifying resins, inorganic fillers, lubricants, oils, and one or more other additives such as heat stabilizers, light stabilizers, UV absorbers, antioxidants, colorants, antistatic agents, flame retardants, water repellents, waterproofing agents, hydrophilic agents, electrical conductivity agents, thermal conductivity agents, electromagnetic shielding agents, translucency control agents, fluorescent agents, slippage agents, transparency agents, antiblocking agents, metal deactivators, and antibacterial agents, so long as they do not adversely affect the intended use of the product. In one embodiment, the polymeric composition can also include a diagnostic agent, such as a color changing or color developing additive, which can act as a visual indicator of the physical integrity of an article made from the composition.

[0020] In one embodiment, the polymer composition can be used as is without blending with another polymer such as polyolefin. It is also possible to blend with a small amount, for example, polypropylene, up to 0.5% by weight in one embodiment, up to 5% by weight in another embodiment, and up to 10% by weight in yet another embodiment. In another embodiment, the polymer composition can be blended with one or more other polymers, such as polyolefins, polyorganosiloxanes, polyesters, polyvinyl chlorides, polycarbonates, polyestercarbonates, polyvinylidene fluorides, and the like. Examples of polyolefins include polyethylene, polypropylene, and polybutylene. In an embodiment, the polymer composition can be blended with up to 50% by weight, or up to 40% by weight, or up to 30% by weight, or up to 20% by weight of polyolefins. In an embodiment, the polyolefin is polypropylene.

[0021] Properties of the hydrogenated SBC: In embodiments, the hydrogenated SBC has a melt flow ratio of 1.0 to 10.0, 2.0 to 8.0, 4.0 to 8.0, or 4.0 to 6.0, measured according to ASTM D-1238 at 230° C. and a load of 2.16 kg.

[0022] In embodiments, the hydrogenated SBC has a Shore A hardness of 60 to 80, or 60 to 70, or 70 to 80, measured according to ASTM D-2240.

[0023] In embodiments, the hydrogenated SBC has a DMA peak tan δ temperature, measured according to ASTM D-4065, of from 10° C. to 40° C., or from 10° C. to 20° C., or from 20° C. to 30° C., or from 30° C. to 40° C.

[0024] In embodiments, the hydrogenated SBC has an order-disorder temperature (ODT) of from 200°C to 300°C, or from 220°C to 280°C, or from 240°C to 260°C, or from 220°C to 260°C, or at least 180°C or less than 350°C.

[0025] In embodiments, the hydrogenated SBC has a tensile strength from 10 to 30 MPa, or from 10 to 20 MPa, or from 7.5 to 15.0 MPa.

[0026] The hydrogenated SBC has a relatively stable hardness over a wide range of application temperatures. In embodiments, the hydrogenated SBC has a percent change in elastic modulus (ΔG) of -9 MPa / °C to -25 MPa / °C, or -12 MPa / °C to -22 MPa / °C, or -15 MPa / °C to -20 MPa / °C, measured over a temperature range of 0°C to 40°C according to ASTM 1640-99. 0℃~40℃ In another embodiment, the polymer composition has a rate of change in elastic modulus (ΔG 20℃~40℃ ).

[0027] In an embodiment, the hydrogenated SBC has an elongation of from 500% to 1000%.

[0028] The hydrogenated SBC can have a combination of two or more of the properties falling within the various ranges described above. In an embodiment, the hydrogenated SBC has a melt flow ratio of 1.0 to 10.0, measured according to ASTM D-1238 at 230° C. and 2.16 kg load; a Shore A hardness of 60 to 80, measured according to ASTM D-2240; a DMA peak tan δ temperature at 1 Hz of 10° C. to 40° C., and an order-disorder transition temperature of 200° C. to 300° C., measured according to STM D-4065. In another embodiment, the polymer composition has a melt flow ratio of 4.0 to 8.0; a Shore A hardness of 70 to 80; a DMA peak tan δ temperature at 1 Hz of 15° C. to 30° C., and an order-disorder transition temperature of 200° C. to 250° C.

[0029] Use of the composition: The various physical properties described above make the hydrogenated SBC valuable in making various articles, such as medical tubing, with high transparency and other desirable properties. In addition to medical tubing, the hydrogenated SBC can also be used to make various other articles, particularly those used in the medical field. Thus, it is also useful to make multi-lumen tubing, multi-layer tubing, and the like. The medical tubing can also be part of other articles used in the medical field, such as IV bags, catheters, and catheters such as those used in infusion, blood transfusion, peritoneal dialysis, catheter treatments such as intravascular catheters and balloon catheters. Other medical articles include blood bags, synthetic vascular prostheses, vascular circuits, syringes, hemodialyzers, blood cell separators, membrane oxygenators, dressings, and medical devices that come into contact with body fluids, particularly blood.

[0030] The composition used to make the article can be made by mixing the above-mentioned components using equipment such as a Henschel mixer, V-blender, ribbon blender, single or twin screw extruder, kneader, or the like. The resulting resin composition can be pelletized. The tube can be made by methods known in the art. For example, the resin composition is fed into an extruder, melted, forced through a die to form a tube shape, and cooled with water or air. There is no particular limit to the size, shape, or cross-sectional size of the tube made from the resin composition. In an embodiment, the outer diameter of the tube is 1 to 60 mm, or 1 to 20 mm, or 1 to 10 mm. The inner diameter of the tube is 1 to 50 mm, or 1 to 25 mm, or 1 to 10 mm. In an embodiment, the thickness of the tube is 0.1 to 20 mm, or 0.5 to 10 mm, or 1 to 5 mm.

[0031] Medical Tubing Application: In an embodiment, medical tubing made from the blend exhibits an X-ray diffraction pattern in which the ratio I(14) / I(15) of the diffraction peak intensity at a scattering angle (2θ) of 15° [I(15)] to the peak intensity at a scattering angle (2θ) of 14° [I(14)] is 1.4 or greater. The I(14) / I(15) ratio provides a measure of the amount of crystalline polypropylene present in the medical tubing.

[0032] In embodiments, medical tubing made using hydrogenated SBC exhibits low surface tack. The tackiness of the polymer surface is due to the nature of the polymer composition. When the outer surfaces of the medical tubing contact each other, the surfaces will not be as sticky due to the lower surface tack. This makes such tubing easier to use. Surface tack can be measured using the "tack index" according to the procedure described in eXPRESS Polymer Letters, Vol 5, No. 11 (2011), pages 1009-1016. In embodiments, the medical tubing has a tack index of 0.45-0.65 when measured at 25°C and 50% relative humidity.

[0033] In an embodiment, medical tubing made therefrom is kink resistant, i.e., can be bent appreciably without kinking. Kink performance is measured by "apparent kink diameter." In an embodiment, a medical tubing having an inner and outer diameter of 5 mm and 7 mm, respectively, has an apparent kink diameter of 30 mm to 40 mm. In another embodiment, a medical tubing having an inner and outer diameter of 3 mm and 4 mm, respectively, has an apparent kink diameter of 20 mm to 30 mm. In yet another embodiment, the medical tubing has a ratio of apparent kink diameter to inner diameter of the tubing of 6 to 10, 7 to 9, 8 to 9, or 9 to 10. In yet another embodiment, the medical tubing has a ratio of apparent kink diameter to outer diameter of the tubing of 4 to 8, 5 to 7, 6 to 7, 7 to 8, or 9 to 10. In another embodiment, the medical tubing has a ratio of apparent kink diameter to tubing wall thickness of 15-30, 15-20, 20-25, or 25-30.

[0034] The medical tubing has good optical clarity, making it easy to view fluid levels and fluid flow. In one embodiment, the medical tubing has a haze level of less than 5%, less than 4%, or less than 3% as measured using ASTM D1003. The high clarity of the tubing allows visual detection of haze or cloudiness in the tubing walls due to polymer degradation.

[0035] Medical tubing made with hydrogenated SBC can also be strongly bonded to other plastic materials using a range of solvents. In medical applications, plastic connectors are made from a variety of materials such as polyolefins, polyesters, polycarbonates, polyvinyl chlorides, polyetherketones, ABS, polystyrenes, polyamides, polyimides, polyoxymethylenes, polyacrylates, polyurethanes, or polysulfones. Connectors are welded to medical tubing using solvent bonding with solvents such as tetrahydrofuran, cyclohexanone, methyl ethyl ketone, and the like. If the bond strength between the medical tubing and the connector is not strong, the connection may become loose and lead to fluid leakage. The bond strength of the weld is measured by determining the peel strength when separating the medical tubing from the connector. In embodiments, medical tubing made with the hydrogenated SBC requires a peel force of 15N to 100N, or at least 30N, or at least 50N, or at least 75N, or less than 125N to separate the solvent-soaked medical tubing from the plastic connector.

[0036] The medical tubing described above has a low tendency to rebound when wound or bent, which makes the wound medical tubing easier to store. EXAMPLES

[0037] The following illustrative examples are non-limiting:

[0038] Polymer molecular weights were determined by gel permeation chromatography (GPC) using polystyrene calibration standards according to ASTM 5296-11. Polymer samples were dissolved in THF and run on an appropriate column set using both RI and UV detectors. The resulting molecular weight values ​​were then converted to true molecular weight using a GPC conversion factor for the total polystyrene content. Coupling efficiency was determined by GPC from the peak integral ratio of the styrene-diene diblock to the higher molecular weight coupling peak.

[0039] Proton NMR techniques were used to determine the total polystyrene content (PSC), vinyl content, and styrene blockiness index, which was measured using the procedure described in U.S. Pat. No. 7,244,785 B2.

[0040] The glass transition temperature (Tg) of all polymer samples was measured by dynamic mechanical analysis using a TA Instruments DMA Q800. Temperature sweep experiments were performed from -80°C to 120°C to obtain the storage modulus (G'), loss modulus (G") and loss factor (tan δ) as a function of temperature. All experiments were performed at a frequency of 1 Hz. The glass transition temperature was reported as the temperature at the peak value of tan δ.

[0041] Tests to determine the ODT (order-disorder transition) rheology were performed on a Bohlin rheometer by Malvern Instruments. Temperature sweep experiments were performed at two frequencies, 0.005 Hz and 0.2 Hz, to measure the complex viscosity. The ODT was reported as the temperature at which the complex viscosity of the polymer was the same at both frequencies.

[0042] Kink resistance tests on tubes were carried out using the Instron method. The tube was first bent and placed between two grips positioned 100 mm apart. The tube was then bent by a downward movement of the crosshead. Once the tube had twisted, the distance (x mm) between the crossheads was measured. The apparent kink diameter is then given by (100-x) mm.

[0043] Mechanical properties were measured using miniature D-die dogbone specimens according to the tensile test method of ASTM D412. Tests were performed on an Instron 3366 equipped with a 1 kN load cell. The gauge length of the specimens was 25.4 mm and tests were performed at an elongation rate of 254 mm / min.

[0044] The Shore A hardness of all samples was measured using an automated hardness tester. Three sheets of the same compound, 2 mm thick, were stacked together and the hardness was measured at the four corners and in the center. The hardness was recorded 10 seconds after the tip of the durometer contacted the material. The average value of the five hardness measurements was reported.

[0045] Examples 1 to 4 Hydrogenated styrene block copolymers shown in Table 1 were prepared. "S" is styrene and "Bd" is butadiene. The numbers in the molecular formula indicate the molecular weight of the S and Bd blocks. The results are shown in Tables 1 and 2. MFR is the melt flow rate measured at 230°C and 2.16 kg according to ASTM D-1238. KD / ID is the ratio of the kink diameter to the tube inner diameter for a tube with an ID of 3 mm and an OD of 4 mm. Tg values ​​were measured by DMA at IHz. NM means not determined.

[0046] Comparative Example 1 is a hydrogenated styrene block copolymer having a total molecular weight of 187 Kg / mol, the styrene block having a true peak molecular weight of 13.5, 30.5 wt% 1,2-butadiene, total polystyrene content of 67 wt%, total blockiness of 34.2, ODT of 260°C-270°C, coupling efficiency of 93%, Tg (DMA, 1 Hz) of 23.4°C, MFR of 4.7 dg / min (230°C / 2.16 Kg) and Shore A hardness (10 sec) of 70.

[0047] [Table 1]

[0048] [Table 2]

[0049] ΔG of competitive material 0~40℃It can be seen from Table 2 that the absolute values ​​of are higher than those of Examples 1, 2, and 3. This indicates that the hardness of the polymers of Examples 1, 2, and 3 is more stable against temperature changes in the range of 0 to 40° C. in contrast to the competitive polymers.

Claims

1. Formula A-B-A, (A-B-A) n X, (A-B) n A medical tubing comprising a hydrogenated block copolymer represented by X, or a mixture thereof, In the formula, n is an integer from 2 to 30, and X is a residue of a coupling agent. each A block is a hydrogenated monoalkenyl arene homopolymer block having a true peak molecular weight of from 5 kg / mol to 15 kg / mol; each B block has a true peak molecular weight of from 30 kg / mol to 200 kg / mol and is a hydrogenated copolymer block of at least one conjugated diene and at least one monoalkenyl arene, the amount of conjugated diene units in a terminal region of the B block adjacent to an A block being greater than the average amount of conjugated diene units in the B block, and the amount of monoalkenyl arene units in one or more regions of the B block not adjacent to an A block being greater than the average amount of monoalkenyl arene units in the B block; the monoalkenyl arene is selected from the group consisting of styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinyltoluene, vinylxylene, and mixtures thereof; the conjugated diene is selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, and mixtures thereof; a midblock monoalkenyl arene blockiness index of 3% to 15%, said monoalkenyl arene blockiness index being the percentage of monoalkenyl arene units in block B that have two monoalkenyl arene neighbors on the polymer chain; 0-10% of the arene double bonds are reduced and at least 90% of the conjugated diene double bonds are reduced; the hydrogenated block copolymer has a midblock poly(monoalkenyl arene) content of 35 wt% to 50 wt%, based on the total weight of the midblock; The hydrogenated block copolymer is having a coupling efficiency of 30% to 95% for the monoalkenyl arene block copolymer having X; having a melt flow ratio of 1.0 to 10.0 measured at 230° C. and a load of 2.16 kg according to ASTM D-1238; having a Shore A hardness of 60 to 80, measured according to ASTM D-2240; having a DMA peak tan δ temperature of 0°C to 40°C at 1 Hz, measured according to ASTM D-4065; has an order-disorder transition temperature of 200°C to 300°C; Medical tubing.

2. 10. The medical tubing of claim 1, wherein the hydrogenated block copolymer has a midblock vinyl content of 30 mol% to 90 mol%.

3. 10. The medical tubing of claim 1, wherein the hydrogenated block copolymer has a tensile strength of 10 MPa to 30 MPa.

4. The hydrogenated block copolymer has a percent change in elastic modulus (ΔG) of −9 MPa / ° C. to −25 MPa / ° C. over the temperature range of 0° C. to 40° C., as measured according to ASTM 1640-99. 0℃~40℃ 2. The medical tubing of claim 1 .

5. 10. The medical tubing of claim 1, wherein the hydrogenated block copolymer has an elongation of from 500% to 1000%.

6. 10. The medical tubing of claim 1, wherein the hydrogenated block copolymer has a total poly(monoalkenyl arene) content of 50% to 70% by weight.

7. 10. The medical tubing of claim 1 having an apparent kink diameter of 30 mm to 40 mm, with inner and outer diameters of 5 mm and 7 mm, respectively.

8. 10. The medical tubing of claim 1 having an apparent kink diameter of 20 mm to 30 mm, with inner and outer diameters of 3 mm and 4 mm, respectively.

9. 2. The medical tubing of claim 1, wherein the ratio of the apparent kink diameter to the inner diameter of the tubing is 6-10, or 4-8, or 15-30.

10. 10. The medical tubing of claim 1 having a haze of less than 3% as measured using ASTM D1003.

11. 10. The medical tubing of claim 1 further comprising a polyolefin in an amount up to 50% by weight.

12. The medical tube according to claim 11, wherein the ratio of the diffraction peak intensity [I(14)] at a scattering angle (2θ) of 14° to the diffraction peak intensity [I(15)] at a scattering angle (2θ) of 15° is 1.4 or more by wide-angle X-ray diffraction.

13. 10. The medical tubing of claim 1, having a cling index of 0.45 to 0.65 when measured at 25° C. and 50% relative humidity.

14. 10. The medical tubing of claim 1, wherein the peel force for separating the solvent soaked medical tubing from the plastic connector is between 15N and 100N, and the plastic connector comprises polyolefin, polyester, polycarbonate, polyvinyl chloride, polyetherketone, ABS, polystyrene, polyamide, polyimide, polyoxymethylene, polyacrylate, polyurethane, or polysulfone.

15. Formula A-B-A, (A-B-A) n X, (A-B) n A medical tubing consisting essentially of a hydrogenated block copolymer represented by X, or a mixture thereof, In the formula, n is an integer from 2 to 30, and X is a residue of a coupling agent. each A block is a hydrogenated monoalkenyl arene homopolymer block having a true peak molecular weight of from 5 kg / mol to 15 kg / mol; each B block has a true peak molecular weight of from 30 kg / mol to 200 kg / mol and is a hydrogenated copolymer block of at least one conjugated diene and at least one monoalkenyl arene, the amount of conjugated diene units in a terminal region of the B block adjacent to an A block being greater than the average amount of conjugated diene units in the B block, and the amount of monoalkenyl arene units in one or more regions of the B block not adjacent to an A block being greater than the average amount of monoalkenyl arene units in the B block; the monoalkenyl arene is selected from the group consisting of styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinyltoluene, vinylxylene, and mixtures thereof; the conjugated diene is selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, and mixtures thereof; a midblock monoalkenyl arene blockiness index of 3% to 15%, said monoalkenyl arene blockiness index being the percentage of monoalkenyl arene units in block B that have two monoalkenyl arene neighbors on the polymer chain; 0-10% of the arene double bonds are reduced and at least 90% of the conjugated diene double bonds are reduced; the hydrogenated block copolymer has a midblock poly(monoalkenyl arene) content of 35 wt% to 50 wt%, based on the total weight of the midblock; The hydrogenated block copolymer is having a coupling efficiency of 30% to 95% with respect to the monoalkenyl arene block copolymer having X; having a melt flow ratio of 1.0 to 10.0, measured according to ASTM D-1238 at 230° C. and a load of 2.16 kg; having a Shore A hardness of 60 to 80, measured according to ASTM D-2240; having a DMA peak tan δ temperature of 0°C to 40°C at 1 Hz, measured according to ASTM D-4065; has an order-disorder transition temperature of 200°C to 300°C; Medical tubing.

16. 16. The medical tubing of claim 1 or 15, which is free of added polyolefins.

Citation Information

Patent Citations

  • Novel block copolymer composition

    JP2009542822A

  • Tube using hydrogenated block copolymer

    WO2017043542A1