Ion Exchange Membrane

The self-supporting ion exchange membrane with balanced cationic and anionic structural units addresses issues of resistance and thickness in conventional membranes, offering improved performance and stability.

JP7576399B2Active Publication Date: 2024-10-31MITSUI CHEMICALS INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020017929
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-05
Publication Date
2024-10-31
Estimated Expiration
2040-02-05

AI Technical Summary

Technical Problem

Conventional ion exchange membranes face issues such as increased membrane resistance, lower charge density, uneven thickness, and potential electrolyte leakage due to the use of porous base films, leading to performance deterioration.

Method used

A self-supporting ion exchange membrane composed of a polymer with specific ion exchange groups, balanced by a combination of cationic and anionic structural units, providing a rigid structure and uniform thickness, which can be used alone or with a porous base material or mesh support for improved handling.

Benefits of technology

The self-supporting membrane achieves low membrane resistance, high charge density, and uniform thickness, reducing defects and enhancing ion exchange performance, while maintaining stability and control over charge density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576399000017
    Figure 0007576399000017
  • Figure 0007576399000001
    Figure 0007576399000001
  • Figure 0007576399000002
    Figure 0007576399000002
Patent Text Reader

Abstract

To provide an ion exchange membrane which can be thinned, and enables reduction of membrane resistance and increase of a charge density.SOLUTION: The ion exchange membrane contains 10 mass% or more of a polymer (P) including: one or two or more kinds of repeating structural unit(s) (A) selected from the group consisting of a repeating structural unit having a cation structure group (a1) where an end terminal constituting a main chain is a group including a 16 group atom of a periodic table, and a repeating structure unit having an anion structure group (a2) where an end terminal constituting a main chain is a group including a 16 group atom of a periodic table; and a repeating structural unit (B) having no cation structure group (a1) and no anion structure group (a2) where an end terminal constituting a main chain is a group containing a 16 group atom of a periodic table, where a content of a total of the cation structure groups (a1) and the inion structure groups (a2) to a total of the structural units (A) and the structural units (B) is 5-90 mol% (provided that a total of the structural units (A) and the structural units (B) is 100%).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ion exchange membrane. [Background technology]

[0002] Ion exchange membranes are used industrially in many fields, such as electrodialysis membranes used in salt production and desalination processes in the food industry, diffusion dialysis membranes used to recover acids from acids containing metal ions generated in the steel industry, and electrolyte membranes for fuel cells. Such ion exchange membranes have a structure including a base film such as a nonwoven fabric or a porous film that has a function as a reinforcing material, and an ion exchange resin. Such ion exchange membranes have both an ion exchange function and a certain membrane strength and shape stability of the membrane. Since ordinary ion exchange resins have many ion exchange groups, they may swell in an aqueous electrolyte solution, and it is said that the membrane strength and shape stability of the ion exchange membrane tend to decrease.

[0003] It has been known to use a porous thermoplastic resin film as the substrate film. For example, there are disclosed a cation exchange membrane for salt production containing a porous stretched polyethylene film as the substrate film (Patent Document 1), an ion exchange membrane containing a porous membrane as the substrate film, which is obtained by laminating two porous resin sheets and bonding them by heat fusion at a temperature equal to or higher than the melting point of the resin constituting the sheets (Patent Document 2), and an ion exchange membrane in which a polymerizable composition for forming an ion exchange resin is filled in the voids of a plurality of laminated porous resin sheets (laminate sheets) and the polymerizable composition is polymerized in this state to form an ion exchange resin (Patent Documents 3 and 4).

[0004] Non-Patent Document 1 discloses that a representative ion exchange membrane, product name Neocepta (manufactured by Astom Corporation), has a structure in which a polyvinyl chloride woven fabric is used as a base material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-096923 A [Patent Document 2] JP 2008-004500 A [Patent Document 3] JP 2012-021099 A [Patent Document 4] JP 2018-183997 A [Non-patent literature]

[0006] [Non-Patent Document 1] Journal of the Japanese Society for Ion Exchange, Vol. 18, No. 3, p. 12 (2007) Summary of the Invention [Problem to be solved by the invention]

[0007] The above-mentioned documents mainly describe ion exchange membranes in which an ion exchange resin is applied or attached to a porous substrate film. However, according to the studies of the present inventors, the method of using the porous substrate film and the ion exchange resin in combination is considered to have the following concerns. That is, 1. The thickness of the ion exchange resin layer tends to be thick due to the influence of the shape of the base film, resulting in high membrane resistance, a decrease in charge density, and poor controllability of charge density. 2. There is a possibility that unevenness in the thickness of the film may occur. 3. There is a possibility that electrolyte leakage may easily occur at the interface between the substrate film and the ion exchange resin. 4. Deterioration of the base film causes the ion exchange resin to peel off, leading to deterioration of performance. etc.

[0008] If there is a demand for improved performance of ion exchange membranes in the future, it will be necessary to solve these problems. Therefore, the main object of the present invention is to obtain an ion exchange membrane that solves the above-mentioned first concern in particular. [Means for solving the problem]

[0009] As a result of the study conducted by the inventors based on the above problems, the inventors found that a free-standing membrane containing a resin having a specific ion exchange function has an excellent balance between low membrane resistance and high charge density, and thus completed the present invention. The configuration of the present invention is also expected to have the potential to solve other problems. Such an invention is specified by the following requirements.

[0010] [1] An ion exchange membrane (I) which is a self-supporting membrane and contains one or more kinds of repeating structural units (A) selected from a repeating structural unit having a cationic structural group (a1) and a main chain terminal which is a group containing a Group 16 atom of the periodic table, and a repeating structural unit having an anionic structural group (a2) and a main chain terminal which is a group containing a Group 16 atom of the periodic table, and a repeating structural unit (B) which does not have the cationic structural group (a1) or the anionic structural group (a2) and a main chain terminal which is a group containing a Group 16 atom of the periodic table, and in which the total content of the cationic structural group (a1) and the anionic structural group (a2) with respect to the total of the structural units (A) and (B) is 5 to 90 mol % (wherein the total of the structural units (A) and (B) is 100 mol %). [2] The ion exchange membrane (I) according to the above [1], which has a thickness of 0.01 to 3.0 μm. [3] The ion exchange membrane (I) according to [1] or [2], wherein the polymer (P) is an aromatic polyether resin containing a structural group (1) represented by the following formula (1) and a structural group (2) represented by the following formula (2):

[0011] [ka] [In formulas (1) and (2), R 1 ~R 10 are each independently H, Cl, F, CF3 or C m H 2m+1 (m represents an integer of 1 to 10), R 1 ~R10 At least one of the following is C m H 2m+1 (m represents an integer of 1 to 10), R 1 ~R 10 may be present in two or more aromatic rings, and C m H 2m+1 If there are two or more C m H 2m+1 may be the same or different from each other. X 1 ~X 5 are each independently H, Cl, F, CF3, a protonic acid group, or an ammonium salt group; X 1 ~X 5 at least one of the groups is a protonic acid group or an ammonium salt group; X 1 ~X 5 may be present in two or more of each of the aromatic rings, and when two or more groups selected from a protonic acid group and an ammonium base are present in one aromatic ring, the groups selected from the protonic acid group and the ammonium base may be the same as or different from each other. A 1 ~A 6 are each independently a direct bond, -CH2-, -C(CH3)2-, -C(CF3)2-, -O- or -CO-. i, j, k and l each independently represent 0 or 1. [4] An ion exchange membrane (IV) having a laminated structure comprising the ion exchange membrane (I) according to any one of the above [1] to [3] and one or more layers selected from a porous substrate (II) and a mesh-like support material (III). [5] The porous substrate (II) has an air permeability of 100 to 400 cm as measured by JIS L 1096 Method A (Fragile method). 3 / cm 2 / s. The ion exchange membrane (IV) according to [4]. [6] The ion exchange membrane (IV) according to [4] or [5], wherein the mesh support (III) has 5 to 2,000 pores per inch. Effect of the Invention

[0012] The ion exchange membrane of the present invention is a self-supporting membrane having ion exchange ability. Therefore, the ion exchange membrane of the present invention has an excellent balance between low membrane resistance and high charge density, and exhibits excellent characteristics such as low membrane resistance and high charge density. In addition, the charge density can be easily controlled by controlling the structure.

[0013] In addition, since the ion exchange membrane of the present invention is a self-supporting membrane, it is expected to have a more uniform membrane quality and fewer defects than conventional ion exchange membranes in which an ion exchange resin is applied or attached to a porous substrate film. This performance may also lead to low membrane resistance. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the ion exchange membrane (IV) of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described. [Ion exchange membrane (I)] One embodiment of the ion exchange membrane of the present invention (hereinafter also referred to as "the ion exchange membrane (I) of this embodiment" or simply "the ion exchange membrane (I)") is characterized in that it contains a polymer having ion exchange capacity (hereinafter also referred to as "polymer (P)") and is a self-supporting membrane.

[0016] In addition, the term "self-supporting membrane" refers to a membrane-shaped molding that can independently maintain its membrane shape in an environment without support, such as in air, even if it is not supported by a substrate. However, in the present invention, the self-supporting membrane can be used together with a porous substrate (II) or a mesh-like support material (III) as described below (for example, a laminated structure of the self-supporting membrane and a porous substrate (II) or a mesh-like support material (III)) for purposes other than ion exchange, such as improving handling.

[0017] The polymer (P) contains a structural unit (A) and a structural unit (B) which will be explained below. The structural unit (A) is one or more types of repeating structural units selected from "a repeating structural unit having a cationic structural group (a1), the main chain of which is terminated by a group containing an atom of Group 16 of the periodic table" and "a repeating structural unit having an anionic structural group (a2), the main chain of which is terminated by a group containing an atom of Group 16 of the periodic table".

[0018] The structural unit (B) is a "repeating structural unit which does not have a cationic structural group (a1) or an anionic structural group (a2), and the terminal of the main chain is a group containing an atom of Group 16 of the periodic table." In the polymer (P), the total content of the cationic structural group (a1) and the anionic structural group (a2) relative to the total of the structural unit (A) and the structural unit (B) is 5 to 90 mol %. However, the total of the structural unit (A) and the structural unit (B) is 100 mol %. The total content of the cationic structural group (a1) and the anionic structural group (a2) is determined from the viewpoint of forming an excellent ion exchange membrane. For example, from the viewpoint of membrane resistance, the total content of the cationic structural group (a1) and the anionic structural group (a2) is preferably 5 mol % or more, more preferably 8 mol % or more; and from the viewpoint of charge density, it is preferably 90 mol % or less, more preferably 60 mol % or less, even more preferably 50 mol % or less, and particularly preferably 45 mol % or less.

[0019] Depending on the application, it may be necessary to keep the charge density low. In such a case, it is preferable that the total content of the cationic structural group (a1) and the anionic structural group (a2) is 25 mol % or more.

[0020] In the polymer (P), the content of the structural unit (A) per 100 moles of the structural unit (B) is preferably 8 moles or more, more preferably 10 moles or more; and preferably 70 moles or less, more preferably 60 moles or less, even more preferably 50 moles or less, and particularly preferably 45 moles or less.

[0021] Depending on the application, it may be necessary to keep the charge density low. In such a case, it is preferable that the content of the structural unit (A) is 30 moles or more. The composition of the structural units as described above can be determined by the amounts of raw materials used in the production of the corresponding resin. It is also possible to determine the composition of the resulting resin coating film by using known structural analysis techniques such as NMR measurement and mass spectrometry (MS) alone or in combination.

[0022] In the present invention, the anionic structural group refers to a group that can take an anionic structure in water, for example, i.e., it is not necessary for the group to always have an anionic structure. For example, it may be a group of an organic acid structure such as a carboxylic acid group, as described below. Similarly, the cationic structural group refers to a group that can take a cationic structure in water, for example, i.e., it is not necessary for the group to always have a cationic structure. For example, it may be a group of an ammonium base structure, as described below.

[0023] Specifically, the ion exchange membrane (I) contains 10% by mass or more of the polymer (P) having ion exchange capacity. It is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, particularly preferably 70% by mass or more, and especially preferably 80% by mass or more. The preferred upper limit is, of course, 100% by mass.

[0024] The above-mentioned ranges are preferable from the viewpoint that the membrane resistance, charge density, and the like are in suitable ranges and can be easily controlled. The polymer (P) is not limited as long as it can form a self-supporting membrane and satisfies the above requirements. The polymer (P) is preferably a polymer containing a polar group that is considered to have ion exchange ability. Examples of the polar group associated with an anion structure include protonic acid groups such as sulfonic acid groups, carboxylic acid groups, phosphonic acid groups, alkylsulfonic acid groups, alkylcarboxylic acid groups, and alkylphosphonic acid groups, among which sulfonic acid groups are preferred. Examples of the polar group associated with a cationic structure include ammonium bases, phosphonium bases, sulfonium salts, imidazolium bases, and pyridinium bases, among which ammonium bases are preferred.

[0025] The polymer (P) has a structure in which the end of the main chain of each structural unit has a group containing a group 16 atom of the periodic table. Examples of the group 16 atom include an oxygen atom and a sulfur atom, and an oxygen atom is preferred. More specifically, a polymer having a rigid structure such as an aromatic skeleton is preferred. Such a polymer is preferably a polymer having a skeleton such as polyether ketone, polyether ether ketone, polyether, polyketone, or polysulfone. Of course, it may be a copolymer having two or more of the above skeletons. Among these, a polyether skeleton, a polyether ketone skeleton, or a polyether ether ketone skeleton is preferred, and a polyether skeleton or a polyether ketone skeleton is more preferred.

[0026] In addition, by using the ion exchange membrane (I) in combination with one or more layers selected from the porous substrate (II) and mesh-like support material (III) described later, the handling property can be improved without substantially impairing the basic performance of the ion exchange membrane. The porous substrate (II) and mesh-like support material (III) can be disposed on a part of the ion exchange membrane (I) or on the entire surface of the ion exchange membrane (I) to form a laminate.

[0027] <Physical properties of ion exchange membrane (I)> The thickness of the ion exchange membrane (I) is usually 3.0 μm or less, preferably 0.01 to 3.0 μm, more preferably 0.01 to 1.5 μm, and particularly preferably 0.1 to 1.0 μm. An ion exchange membrane having a thickness within this range has sufficient membrane strength and exhibits practically excellent membrane resistance and charge density. The thickness of the ion exchange membrane (I) can be controlled by the production conditions of the ion exchange membrane, such as the temperature and pressure during press molding, the varnish concentration and coating thickness during casting, etc.

[0028] As described above, the ion exchange membrane (I) of the present embodiment can be preferably a thin free-standing membrane, and therefore the ion exchange membrane (I) tends to have a lower membrane resistance and a higher charge density than conventional ion exchange membranes obtained by attaching an ion exchange resin to a porous substrate.

[0029] The ion exchange membrane (I) is a self-supporting membrane, and therefore does not necessarily require a substrate (e.g., a sheet or film). For this reason, the structure of the membrane is not disrupted by foreign components such as the substrate, and an interface between the membrane and foreign components is not generated. Furthermore, it is considered that the ion exchange membrane can be made to have a relatively uniform thickness and efficient ion exchange performance.

[0030] The ion exchange membrane (I) also contains polar groups such as sulfonic acid groups and ammonium bases. In general, polar groups are known to be easily microaggregated by electrical attraction. If the aggregation is too strong, the polar groups will be unevenly distributed, and there is a concern that the ion exchange capacity commensurate with the polar group content will not be exhibited. On the other hand, since the ion exchange membrane (I) is a self-supporting membrane, the polymer (P) that forms the membrane tends to be a polymer with a relatively rigid structure. Due to the rigid molecular structure, the aggregation of the polar groups is relatively alleviated, and the polar groups have good dispersibility, so the ion exchange membrane (I) may exhibit excellent ion exchange capacity.

[0031] The ion exchange membrane (I) preferably has a membrane resistance of 0.1 to 2.5 Ω·cm. 2 More preferably, it is 0.15 to 2.0 Ω cm 2 , and more preferably 0.2 to 1.9 Ω cm 2It is.

[0032] The charge density of the ion exchange membrane (I) is preferably 1.0 to 5.0 mol / dm 3 More preferably, it is 1.1 to 4.0 mol / dm 3 , more preferably 1.2 to 3.5 mol / dm 3 It is. It is preferable that either the membrane resistance or the charge density is within the above range, and it is more preferable that both are within the above range.

[0033] <Aromatic polyether resin> Hereinafter, as a representative example of the polymer (P), a protonic acid group- and / or ammonium salt group-containing aromatic polyether resin, which is a polymer having a protonic acid group and / or an ammonium salt group, will be described. The protonic acid group is one type of anionic structural group in the present invention, and corresponds to a structure capable of forming an anion. The ammonium salt group is one type of cationic structural group in the present invention, and corresponds to a structure capable of forming a cation.

[0034] The aromatic polyether resin preferably contains a structural group (1) represented by the following formula (1) and a structural group (2) represented by the following formula (2). 1 ~X 5 is a protonic acid group or an ammonium salt group) corresponds to the above-mentioned structural unit (A), and another part of the structural group (1) and a part of the structural group (2) correspond to the above-mentioned structural unit (B).

[0035] [ka] In formulas (1) and (2), i, j, k and l each independently represent 0 or 1.

[0036] R 1 ~R 10 are each independently H, Cl, F, CF3 or C m H 2m+1(m is an integer from 1 to 10), m H 2m+1 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group.

[0037] R 1 ~R 10 At least one of the following is C m H 2m+1 (m is an integer of 1 to 10). Specifically, i, j, k, and l, as well as R 1 ~R 10 The structural group (1) and / or the structural group (2) are C m H 2m+1 That is, when i, j, k, and l are all 1, R 1 ~R 10 At least one of the following is C m H 2m+1 For example, if i = 0, j = 1, k = 0 and l = 1, then R 1 ~R 3 , R 5 ~R 8 and R 10 At least one of the following is C m H 2m+1 It is.

[0038] R 1 ~R 10 may be present in two or more aromatic rings, and C m H 2m+1 If there are two or more C m H 2m+1 may be the same or different from each other. X 1 ~X 5 are each independently H, Cl, F, CF3, a protonic acid group, or an ammonium salt group.

[0039] X 1 ~X 5 At least one of i and j and X is a protonic acid group or an ammonium salt group. 1 ~X5 is selected so that the structural group (1) has at least one group selected from a protonic acid group and an ammonium salt group. That is, when i=1 and j=1, X 1 ~X 5 At least one of the groups is selected from a protonic acid group and an ammonium base group, but when j=0, X 1 ~X 3 At least one of the groups is selected from a protonic acid group and an ammonium base group, and when i=0 and j=1, X 1 ~X 3 and X 5 At least one of the groups is selected from a protonic acid group and an ammonium salt group.

[0040] X 1 ~X 5 may be present in two or more of each of the aromatic rings, and when two or more groups selected from a protonic acid group and an ammonium base are present in one aromatic ring, the groups selected from the protonic acid group and the ammonium base may be the same as or different from each other.

[0041] A 1 ~A 6 are each independently a direct bond, -CH2-, -C(CH3)2-, -C(CF3)2-, -O- or -CO-; A 1 ~A 6 At least one of the is preferably -CO-.

[0042] The lines at both ends of formulas (1) and (2) indicate bonds between adjacent structural groups. In the present invention, the protonic acid group means a functional group that easily releases a proton or a group in which a hydrogen atom of the functional group is substituted with Na or K. Examples of the protonic acid group include a sulfonic acid group (-SO3H), a carboxylic acid group (-COOH), a phosphonic acid group (-PO3H2), an alkylsulfonic acid group (-(CH2) n SO3H), alkyl carboxylic acid group (-(CH2) n COOH), alkylphosphonic acid group (-(CH2) nExamples of ammonium bases include groups having a typical ammonium salt structure obtained by reacting an amino group with an inorganic acid such as hydrochloric acid or various carboxylic acids.

[0043] n is an integer of 1 to 10. The protonic acid group is -C n' H 2n' -SO3Y (n' is an integer of 0 to 10, preferably 0, and Y is H, Na or K) is preferred.

[0044] The structure group (1) includes, for example, a structure group represented by the following formula (1-1) or (1-2). In these structures, A 1 is preferably -CO-,

[0045] [ka] More specifically, the structural group represented by the following formula (1-3) or (1-4) can be mentioned.

[0046] [ka] (In the formula, each Z is independently a group selected from the protonic acid group and the ammonium base, each s is independently an integer of 0 to 3, each t is independently an integer of 0 to 4, and the lines at both ends represent bonds to adjacent structural groups. The other symbols are as defined above.)

[0047] Examples of the structure group (2) include a structure group represented by the following formula (2-1) or (2-2):

[0048] [ka] More specifically, the structural group represented by the following formula (2-3) or (2-4) can be mentioned.

[0049] [ka] (In the formula, each t is independently an integer of 0 to 4, and the lines at both ends indicate a bond to adjacent structural groups. The symbols other than t are defined as above.)

[0050] The content ratio of the structural group (1) relative to the total amount of the structural group (1) and the structural group (2) is preferably 10 mol% or more and 80 mol% or less, since an ion exchange membrane having high ion permeability can be formed. The preferred lower limit is 15 mol%, more preferably 20 mol%. On the other hand, the preferred upper limit is 70 mol%, more preferably 55 mol%, and even more preferably 45 mol%. In applications requiring a lower charge density, the content is preferably 35 mol% or more.

[0051] Within the above ranges, a free-standing film is formed, the charge density and film resistance are within suitable ranges, and these can be controlled, which is preferable. The aromatic polyether resin may further contain a structural unit derived from a polyfunctional compound described below.

[0052] The aromatic polyether resin may be either crosslinked or non-crosslinked. The weight average molecular weight (Mw) of the aromatic polyether resin measured by GPC (Gel Permeation Chromatography) under the following conditions (1) to (9) is preferably 70,000 or more, more preferably 80,000 or more, and even more preferably 90,000 or more. When the molecular weight is within the above range, the obtained ion exchange membrane has high mechanical properties and is less likely to break during membrane formation or use. In addition, the weight average molecular weight is preferably 180,000 or less from the viewpoint of gel generation rate. (1) GPC equipment: LC-10AT manufactured by Shimadzu Corporation (2) Column oven: CTO-10A, manufactured by Shimadzu Corporation (3) Column: GPC KD-G guard column (manufactured by Showa Denko K.K. (SHODEX)) The column for measuring the molecular weight is appropriately selected depending on the molecular weight of the polymer to be obtained. (4) Measurement temperature: 40℃ (5) Developing solvent: N,N-dimethylformamide (DMF) (6) Flow rate: 0.7ml / min (7) Injection volume: 500μl (8) Detector: UV detector 875-UV type device (manufactured by JASCO), Refractive index detector RID-10A (manufactured by Shimadzu Corporation) (9) Molecular weight standard: Standard polystyrene

[0053] The weight average molecular weight can be controlled by adjusting the molar ratio of raw material monomers and the amount of end-capping agent when producing the aromatic polyether resin. The protonic acid group equivalent of the protonic acid group-containing aromatic polyether resin, i.e., the mass of the protonic acid group-containing aromatic polyether resin per mole of the protonic acid group, is preferably 200 g / mol or more, since an ion exchange membrane that is insoluble in water or methanol, suppresses swelling, and has a small amount of electrolyte permeation through the membrane is obtained. Also, since an ion exchange membrane that has a large water permeation flux and is economical is obtained, the protonic acid group equivalent is preferably 5000 g / mol or less, more preferably 1000 g / mol or less.

[0054] In the following, a method for producing a protonic acid group-containing aromatic polyether resin will be described as an example of a method for producing the above-mentioned preferred resin.

[0055] <Method for producing protonic acid group-containing aromatic polyether resin> The protonic acid group-containing aromatic polyether resin can be obtained by condensation of a monomer having an aromatic ring according to a conventionally known method (for example, the method described in WO 2003 / 33566). For example, the following formulae (1a) and (2a) can be used:

[0056] [ka] and a monomer having a halogen substituent represented by the following formulae (1b) and (2b):

[0057] [ka] The resin can be obtained by condensation polymerization with a monomer having a hydroxyl group represented by the following formula:

[0058] Among the above monomer structures, the structural units derived from the following monomer structures correspond to the structural unit (A) in the polymer (P). X 1 and X 2 A monomer of formula (1a) in which one or more groups selected from the following are protonic acid group structures, and 3 ~X 5 A monomer represented by formula (1b), in which one or more groups selected from the following are protonic acid group structures: 1 , A 2 , A 3 When is a group containing an atom of group 16 of the periodic table, (1a) and (1b) are in the form of multiple structural units linked together.) On the other hand, the structural unit derived from the following monomer structure corresponds to the structural unit (B) in the polymer (P).

[0059] A monomer of formula (2a) and a monomer of formula (2b). 4 , A 5 , A 6 is a group containing an atom of group 16 of the periodic table, (2a) or (2b) is a form in which multiple structural units are linked.) Furthermore, X 1 and X 2 Monomers of formula (1a) in which X is a structure other than a protonic acid group (i.e., H, Cl, F, CF3), and 3 ~X 5 A monomer of formula (1b) in which A is a structure other than a protonic acid group (i.e., H, Cl, F, CF3). 1 , A 2 , A 3When is a group containing an atom of group 16 of the periodic table, (1a) and (1b) are in the form of multiple structural units linked together.) In the formula, Y is a halogen atom, and the meanings of the other symbols are the same as those of the same symbols used in the above formulas (1) and (2). The halogen atoms preferably include fluorine and chlorine.

[0060] It is preferable to use a basic catalyst such as K2CO3 for the condensation. The monomer represented by the above formula (1a) (wherein X 1 ~X 2 at least one of which is a protonic acid group. Examples of the protonic acid group-containing aromatic dihalide compounds include 5,5'-carbonylbis(sodium 2-fluorobenzenesulfonate) and 5,5'-carbonylbis(sodium 2-chlorobenzenesulfonate).

[0061] Examples of the monomer represented by the above formula (2a) include: Aromatic dihalide compounds such as 4,4'-difluorobenzophenone, 3,3'-difluorobenzophenone, 4,4'-dichlorobenzophenone, 3,3'-dichlorobenzophenone, 4,4'-difluorobiphenyl, 4,4'-difluorodiphenylmethane, 4,4'-dichlorodiphenylmethane, and 4,4'-difluorodiphenyl ether; and Alkyl-containing aromatic dihalide compounds such as 3,3'-dimethyl-4,4'-difluorobenzophenone, 3,3'-diethyl-4,4'-difluorobenzophenone, 3,3',5,5'-tetramethyl-4,4'-difluorobenzophenone, 3,3'-dimethyl-4,4'-dichlorobenzophenone, and 3,3',4,4'-tetramethyl-5,5'-dichlorobenzophenone Examples include:

[0062] The monomer represented by the above formula (2b) (or the monomer represented by the above formula (1b) (wherein X 3 ~X 5 are all hydrogen atoms. Aromatic dihydroxy compounds such as 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, 2,2-bis(4-hydroxyphenyl)propane, 1,1,1,3,3,3-hexafluoro-2,2-bis(4-hydroxyphenyl)propane, 1,4-bis(4-hydroxyphenyl)benzene, α,α'-bis(4-hydroxyphenyl)-1,4-dimethylbenzene, α,α'-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-1,3-diisopropylbenzene, 1,4-bis(4-hydroxybenzoyl)benzene, and 3,3'-difluoro-4,4'-dihydroxybiphenyl; and 3,3'-Dimethyl-4,4'-dihydroxybiphenyl, 3,3',5,5'-Tetramethyl-4,4'-dihydroxybiphenyl, 3,3'-Dimethyl-4,4'-dihydroxydiphenylmethane, 3,3',5,5'-Tetramethyl-4,4'-dihydroxydiphenylmethane (also known as bis(3,5-dimethyl-4-hydroxyphenyl)methane), 3,3',5,5'-Tetraethyl-4,4'-dihydroxydiphenylmethane, 3,3'-Dimethyl-4,4'-dihydroxydiphenyl ether, 3,3',5,5'-Tetramethyl-4,4'-dihydroxydiphenyl ether, 2,2-Bis(3-methyl -4-hydroxyphenyl)propane, 2,2-bis(3-ethyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, α,α'-bis(3-methyl-4-hydroxyphenyl)-1,4-diisopropylbenzene, α,α'-bis(3,5-dimethyl-4-hydroxyphenyl)-1,4-diisopropylbenzene, α,α'-bis(3-methyl-4-hydroxyphenyl)-1,3-diisopropylbenzene, and other alkyl group-containing aromatic dihydroxy compounds. Examples include:

[0063] A polyfunctional compound may be copolymerized with the monomer as long as the solvent solubility of the protonic acid group-containing aromatic polyether resin is not impaired. By copolymerizing a polyfunctional compound, the protonic acid group-containing aromatic polyether resin can have a micro-crosslinked structure. Examples of polyfunctional compounds include those having three or more hydroxyl groups in one molecule, such as (2,4-dihydroxyphenyl)(4-hydroxyphenyl)methanone, 4-[1-(4-hydroxyphenyl)-1-methylethyl]-1,3-benzenediol, 4-[(2,3,5-trimethyl-4-hydroxyphenyl)methyl]-1,3-benzenediol, 4-[(4-hydroxyphenyl)methyl]-1,2,3-benzenetriol, (4-hydroxyphenyl)(2,3,4-trihydroxyphenyl)methanone, 4-[(3,5-dimethyl-4 -hydroxyphenyl)methyl]-1,2,3-benzenetriol, 4-[(2,3,5-trimethyl-4-hydroxyphenyl)methyl]-1,2,3-benzenetriol, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bis[benzene-1,2-diol], 5,5'-[1,4-phenylenebis(1-methylethylidene)]bis[benzene-1,2,3-triol], α,α,α'-tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, phloroglucin, pyrogallol, and the like.

[0064] From the viewpoint of preventing a decrease in the solvent solubility of the protonic acid group-containing aromatic polyether resin, a decrease in the fluidity of the resin during membrane formation, and a decrease in the elongation of the ion exchange membrane, the amount of these copolymerizations is preferably 0 to 8 mol% / total OH equivalent (i.e., of the total amount (100 mol%) of OH groups possessed by the monomer of formula (1b), the monomer of formula (2b), and the polyfunctional monomer, 0 to 8 mol% is OH groups derived from the polyfunctional monomer), and more preferably 0 to 5 mol% / total OH equivalent.

[0065] Hereinafter, with regard to the varnish used in the casting method, which is a preferred production method for the ion exchange membrane (I) of this embodiment, the case where the above-mentioned protonic acid group-containing aromatic polyether resin is used will be described as an example.

[0066] <Protonic acid group-containing aromatic polyether resin varnish> The protonic acid group-containing aromatic polyether resin has a molecular structure that is basically linear, and even if it has a crosslinked structure derived from the polyfunctional compound, the amount of the crosslinked structure is small, so that the resin has excellent solvent solubility, and can be made into a varnish by dissolving the resin in a solvent.

[0067] The solvent is not particularly limited, and examples thereof include water, alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and butanol, hydrocarbons such as toluene and xylene, halogenated hydrocarbons such as methyl chloride and methylene chloride, ethers such as dichloroethyl ether, 1,4-dioxane, and tetrahydrofuran, fatty acid esters such as methyl acetate and ethyl acetate, ketones such as acetone and methyl ethyl ketone, cellosolves such as 2-methoxyethanol and 2-ethoxyethanol, and aprotic polar solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, and dimethyl carbonate. These can be used alone or in combination of two or more. Among them, lower alcohols (methanol, ethanol, 1-propanol, 2-propanol, t-butyl alcohol, etc.), tetrahydrofuran, N,N-dimethylformamide, and N-methyl-2-pyrrolidone are preferred because of their water solubility, and mixed solvents of these with water are also preferred. The resin concentration in the varnish can be selected depending on the use of the varnish, but is preferably from 1% by mass to 80% by mass. The ion exchange membrane (I) which is a free-standing membrane of this embodiment can be produced, for example, by a casting method using the above-mentioned varnish. A specific production method will be described later.

[0068] Tensile modulus, tensile breaking strength and elongation The ion exchange membrane (I) which is a free-standing membrane of this embodiment has a tensile modulus of elasticity of preferably 0.8 to 2.0 GPa, more preferably 1.2 to 1.6 GPa. The ion exchange membrane (I) has a tensile breaking strength of preferably 40 MPa or more, the upper limit of which is, for example, 100 MPa. The ion exchange membrane (I) has an elongation percentage of preferably 40% or more, the upper limit of which is, for example, 200%. These tensile modulus, tensile breaking strength and elongation percentage are measured under the following conditions.

[0069] A test piece with a size of length x width x thickness = 100 mm x 10 mm x 5 μm is prepared and pulled at a speed of 50 mm / min using a tensile testing machine. When the test piece breaks (fractures), the strength (tensile load value divided by the cross-sectional area of ​​the test piece) and the elongation are determined.

[0070] The elongation is calculated according to the following formula: Elongation rate (%) = 100 × (L-L0) / L0 (L0: length of test piece before test, L: length of test piece at break) The tensile modulus is defined as the load at break divided by the cross-sectional area of ​​the test piece and the strain at break, that is, (L-L0) / L0. The tensile strength at break and the elongation can be increased by, for example, increasing the molecular weight of the protonic acid group-containing aromatic polyether resin.

[0071] Solubility and mass loss rate The solubility of the ion exchange membrane (I) in dimethyl sulfoxide (hereinafter also referred to as "DMSO") and water can be evaluated by the following mass loss rate, respectively. The mass loss rate is preferably less than 2 mass%, more preferably 1.0 mass% or less, and particularly preferably 0.5 mass% or less.

[0072] The ion exchange membrane (I) is left to stand at 150°C for 4 hours in a nitrogen atmosphere to dry, and then weighed. The ion exchange membrane is immersed in DMSO or water and left to stand at 25°C for 24 hours. The ion exchange membrane is removed from the DMSO or water, left to stand at 150°C for 4 hours in a nitrogen atmosphere to dry, and then weighed. The mass loss rate of the ion exchange membrane (I) is calculated from the following formula based on the masses before and after immersion. Mass reduction rate = (mass of ion exchange membrane before immersion - mass of ion exchange membrane after immersion) / mass of ion exchange membrane before immersion x 100

[0073] The amount of dissolution can be reduced, for example, by crosslinking the protonic acid group-containing aromatic polyether resin, and therefore, even if the protonic acid group equivalent is small, the amount of dissolution can be kept within the above range.

[0074] <Method for producing ion exchange membrane (I)> The ion exchange membrane (I) can be produced as a self-supporting membrane from the protonic acid group-containing aromatic polyether resin, for example. The ion exchange membrane (I) can be easily produced by press molding or extrusion molding the protonic acid group-containing aromatic polyether resin. In addition, the membrane of the protonic acid group-containing aromatic polyether resin may be subjected to a stretching treatment or the like.

[0075] The ion exchange membrane (I) can also be produced by a casting method using the above-mentioned varnish. That is, the varnish is applied onto a support, and the solvent is removed by volatilization to obtain the ion exchange membrane (I). Furthermore, the ion exchange membrane (I) can be peeled off from the support to form a free-standing membrane.

[0076] If the organic solvent used in casting remains in the ion exchange membrane (I), the mechanical strength of the ion exchange membrane (I) may decrease and the membrane may be easily damaged. Therefore, the ion exchange membrane (I) produced by the casting method is preferably thoroughly dried and / or washed with water, an aqueous sulfuric acid solution, hydrochloric acid, or the like.

[0077] In addition, when the protonic acid group of the protonic acid group-containing aromatic polyether resin preferably used for producing the ion exchange membrane (I) is a functional group that easily releases protons, in which a hydrogen atom is substituted with Na or K, a membrane of the protonic acid group-containing aromatic polyether resin may be formed and then the membrane may be brought into contact with an aqueous solution of hydrochloric acid, sulfuric acid, or the like, to substitute the Na or K of the protonic acid group with a hydrogen atom.

[0078] <Suitable examples of ion exchange membrane (I)> A preferred example of the ion exchange membrane (I) is a free-standing membrane comprising the above-mentioned protonic acid group-containing aromatic polyether resin. The ion exchange membrane using the above-mentioned aromatic polyether resin as a raw material can be produced as a free-standing membrane, and this ion exchange membrane (I) can be made into an ion exchange membrane (IV) that can improve the handling property and the like without impairing the performance of the ion exchange membrane (I) by laminating it with a material selected from a mesh-like support material (III) and a porous substrate (II).

[0079] Since such ion exchange membranes (I) and (IV) are self-supporting membranes, the thickness of the ion exchange resin portion is relatively uniform and can be made thin, compared with ion exchange membranes in which an ion exchange resin is applied or attached to a conventional porous resin substrate, and therefore it is expected that the membranes will exhibit stable and high ion exchange performance. In addition, by controlling the resin composition, it is also possible to obtain a membrane with high water permeability and high salt rejection. In addition, unlike conventional embodiments, the fact that the resin having ion exchange performance itself forms a self-supporting membrane means that, for example, in an embodiment in which a mesh-like support material (III) or a porous substrate (II) is used in combination, even if the mesh-like support material (III) or the porous substrate (II) is deteriorated, it is expected that the effect on the ion exchange membrane performance will be small. (It is known that in an embodiment in which an ion exchange resin is attached to a conventional porous resin substrate, problems such as peeling of the ion exchange resin occur when the porous resin substrate is deteriorated.)

[0080] Hereinafter, an embodiment containing the aromatic polyether resin as the ion exchange membrane (I) will be described as a representative example. The ion exchange membrane (I) of this embodiment preferably contains the protonic acid group-containing aromatic polyether resin, which is a suitable polymer having ion exchange ability, in an amount of 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, particularly preferably 70% by mass or more, and especially preferably 80% by mass or more. In the ion exchange membrane (I), the preferred upper limit of the content of the protonic acid group-containing aromatic polyether resin is 100% by mass.

[0081] [Porous base material (II)] Since the ion exchange membrane (I) is preferably thin, a means for ensuring handling properties and strength is often required. From the above-mentioned viewpoint, the ion exchange membrane (I) can be used in combination with a porous substrate (II) or a mesh-like support material (III) described later to form an ion exchange membrane (IV). It is preferable to use these materials as a laminate. In one embodiment, for example, the ion exchange membrane (IV) can be produced by sandwiching the ion exchange membrane (I) between two porous substrates (II) from both sides. In the present invention, the porous substrate (II) has a structure different from that of the mesh-like support material (III).

[0082] However, the presence of such a porous substrate (II) may cause ion concentration polarization in the ion exchange membrane (IV) as a whole, which may reduce the ion separation ability. For this reason, in the present invention, a porous substrate (II) that satisfies the following conditions is preferably used.

[0083] The air permeability of the porous substrate (II) is 100 to 400 cm 3 / cm 2 The air permeability is preferably 1 / s. This air permeability is measured as follows based on Method A (Fragile type method) described in JIS L 1096.

[0084] Attach a 20cm x 20cm test piece to the testing machine, adjust the intake fan and air holes so that the inclined barometer reads 125 Pa, and measure the pressure indicated by the vertical barometer. Using the measured pressure and the type of air hole, calculate the amount of air passing through the test piece using the conversion table attached to the testing machine.

[0085] The thickness of the porous substrate (II) is usually 50 to 700 μm, preferably 80 to 600 μm, and more preferably 100 to 500 μm. It is believed that the ion exchange membrane (IV) has such high air permeability and a thin porous substrate (II), so that the concentration polarization occurring inside the porous substrate (II) during use of the ion exchange membrane (IV) is suppressed, and the resistance when ions permeate the ion exchange membrane (IV) can be reduced, resulting in an increase in the water permeation flux through the ion exchange membrane (IV). The air permeability and thickness of the porous substrate (II) can be controlled by a conventional method.

[0086] Preferred materials constituting the porous substrate (II) include, for example, synthetic resins and natural fibers. Examples of synthetic resins include thermoplastic resins and thermosetting resins, and thermoplastic resins are preferred.Specific examples of thermoplastic resins include olefin polymers, polyester resins, polyamide resins, polyvinyl chloride, and (meth)acrylic resins.Among these, olefin polymers and polyester resins are preferred, and olefin polymers are particularly preferred.

[0087] Specifically, the olefin polymer is a homopolymer or copolymer of an α-olefin, or a copolymer of an α-olefin and another monomer. Examples of the α-olefin include α-olefins having 2 to 8 carbon atoms, such as ethylene, propylene, and 1-butene. Examples of the olefin polymer include polyolefin resins such as polypropylene, polyethylene, poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-4-methyl-1-pentene copolymer, propylene-1-butene copolymer, and 4-methyl-1-pentene-1-decene copolymer, as well as copolymers of α-olefins and other monomers, such as ethylene-vinyl alcohol copolymer.

[0088] Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyamide resins include nylon 6 and nylon 66.

[0089] Examples of natural fibers include plant fibers such as cotton and hemp, and animal fibers such as silk and wool. Of these, cotton and silk are preferred. Examples of the porous substrate (II) include cloth substrates such as woven fabric, nonwoven fabric, knitted fabric, and foam sheets. Among these, cloth substrates are preferred, woven fabric and nonwoven fabric are more preferred, and nonwoven fabric is particularly preferred.

[0090] Examples of nonwoven fabrics include long fiber nonwoven fabrics made by the spunbond method, short fiber nonwoven fabrics made by the meltblown method, long fiber nonwoven fabrics such as flash spun nonwoven fabrics, spunlace nonwoven fabrics, airlaid nonwoven fabrics, thermal bond nonwoven fabrics, needle punch nonwoven fabrics, and chemical bond nonwoven fabrics. Among these, spunbond nonwoven fabrics and meltblown nonwoven fabrics are preferred, spunbond nonwoven fabrics are more preferred, and spunbond nonwoven fabrics of polyethylene terephthalate or polypropylene are particularly preferred.

[0091] The nonwoven fabric may be a composite fiber made of different resins, and may be a core-sheath or side-by-side composite fiber in which the different resin is disposed on the outer surface side of the fiber. Examples of the composite fiber include a core-sheath or side-by-side composite fiber of polyethylene / polypropylene.

[0092] The nonwoven fabric may be a laminated nonwoven fabric, for example, a laminated nonwoven fabric containing a spunbonded nonwoven fabric and a meltblown nonwoven fabric, such as a laminated spunbonded nonwoven fabric and a meltblown nonwoven fabric (SM), or a laminated spunbonded nonwoven fabric, a meltblown nonwoven fabric, and a spunbonded nonwoven fabric (SMS) in this order.

[0093] To obtain such a laminated nonwoven fabric, a spunbonded nonwoven fabric and a meltblown nonwoven fabric are laminated and integrated together to form an integrated fabric. Examples of the integration method include a method of overlapping a spunbonded nonwoven fabric and a meltblown nonwoven fabric and heating and pressurizing them, a method of bonding them together with an adhesive such as a hot melt adhesive or a solvent-based adhesive, and a method of depositing fibers on the spunbonded nonwoven fabric by a meltblown method and heat fusing them.

[0094] The nonwoven fabric may be a laminated nonwoven fabric having a porous film having micropores sandwiched between the nonwoven fabrics. Examples of such laminated nonwoven fabrics include a polypropylene (PP) nonwoven fabric, a porous PP film, and a PP nonwoven fabric (SFS) laminated in this order, and a PP nonwoven fabric, a porous PP film, and a rayon PP nonwoven fabric (SFR) laminated in this order. The weight of the nonwoven fabric (in the case of a laminated nonwoven fabric, the weight of the laminated nonwoven fabric) is preferably 10 to 80 g / m 2 Approximately, more preferably 20 to 40 g / m 2 That's about it.

[0095] [Mesh-like support material (III)] The mesh support material (III) used as necessary in the present invention preferably satisfies the following conditions. The mesh support material (III) preferably has 5 to 2,000 pores per inch, more preferably 5 to 1,000 pores per inch, even more preferably 5 to 500 pores per inch, and even more preferably 5 to 400 pores per inch. The number of pores is more preferably in the range of 5 to 80 pores per inch, even more preferably 5 to 50 pores per inch, and particularly preferably 5 pores per inch or more and less than 20 pores per inch. An especially preferred upper limit of the number of pores is 15 pores per inch.

[0096] The number of holes is the so-called mesh number. The numbers of holes in the first direction (e.g., vertical direction) and the second direction (e.g., horizontal direction) that define the mesh shape may be the same or different, as long as they are within the above range. The first direction and the second direction may or may not be perpendicular to each other.

[0097] The opening ratio of the mesh-like support material (III) is preferably in the range of 10 to 95%, more preferably 20 to 95%, and even more preferably 30 to 95%. In one embodiment, the opening ratio of the mesh-like support material (III) may be in the range of more than 90%. Here, the opening ratio (ε) is defined as ε={A1 / (A1+d1)}×{A2 / (A2+d2)}×100(%). In the above formula, ε is the opening ratio, A1 is the mesh size (mm) in the first direction (e.g., vertical direction), and A2 is the mesh size (mm) in the second direction (e.g., horizontal direction). It is defined as A1=(25.4 / M1)-d1, and A2=(25.4 / M2)-d2. d1 is the fiber diameter of the fiber (e.g., horizontal fiber) extending in the second direction, and M1 is the mesh (the number of holes (pores) per inch) in the first direction (e.g., vertical direction). d2 is the fiber diameter of the fibers extending in the first direction (e.g., vertical fibers), and M2 is the mesh (the number of holes per inch) in the second direction (e.g., horizontal). See Figure 1. In Figure 1, the first direction (vertical) and the second direction (horizontal) are perpendicular to each other, but they do not have to be perpendicular.

[0098] The mesh-like support material (III) preferably has fibers arranged in a lattice pattern. The fiber diameter of the fibers is preferably 5 to 250 μm, preferably 10 to 180 μm, and more preferably 10 to 100 μm.

[0099] The material of the fibers is not particularly limited as long as it has a suitable strength and water resistance, and for example, resin and fibrous metal can be used. Examples of the resin include polyolefins such as polypropylene and polyethylene, polyamides such as nylon, and polyester, and polypropylene and nylon are preferred. Examples of the fibrous metal include stainless steel. Natural fibers such as silk can also be used.

[0100] The type of mesh that can be used may be, for example, any of plain weave, twill weave, plain tatami weave, twill tatami weave, sintered mesh, etc. Among these, plain weave is preferred. As the mesh-like support material (III), commercially available products can be used, and examples thereof include products from Mesh Co., Ltd., Nippon Mesh Kogyo Co., Ltd., Kureha Co., Ltd., Asada Mesh Co., Ltd., NBC Meshtech Co., Ltd., Vantec Co., Ltd., and the like.

[0101] As described above, one of the purposes of using the porous substrate (II) or the mesh-like support material (III) in the present invention is to improve the handleability of the ion exchange membrane (I). Therefore, it is preferable that the porous substrate (II) or the mesh-like support material (III) is in direct contact with at least one surface of the ion exchange membrane (I).

[0102] When the area of ​​the ion exchange membrane (I) is large, the porous substrate (II) or the mesh-like support material (III) may be used with an adhesive or a pressure-sensitive adhesive to fix the ion exchange membrane (I) to these materials, as long as the object of the present invention is not impaired. Specific examples of the use of adhesives and pressure-sensitive adhesives include the following (using a mesh-like support material (III)).

[0103] As a method for laminating the mesh-like support material (III) and the ion exchange membrane (I), the mesh-like support material (III) and the ion exchange membrane (I) may be bonded together via an adhesive or pressure-sensitive adhesive, or the mesh-like support material (III) and the ion exchange membrane (I) may simply be superimposed on each other and their peripheral portions may be sandwiched and fixed with a frame material. From the viewpoint of handling, it is preferable to bond the mesh-like support material (III) and the ion exchange membrane (I) together via an adhesive or pressure-sensitive adhesive. It is preferable to apply the adhesive or pressure-sensitive adhesive only to the base material portion (such as fiber) of the mesh-like support material (III) so as not to block the openings of the mesh-like support material (III).

[0104] As described above, the ion exchange membrane (IV), which is an embodiment in which the ion exchange membrane (I) is combined with the porous substrate (II) or the mesh-like support material (III), has a configuration in which each of the constituent materials is substantially independent. As described above, in the conventional configuration in which the ion exchange resin is attached to the porous substrate, it has been disclosed that peeling of the ion exchange resin due to deterioration of the porous substrate affects the ion exchange performance (Non-Patent Document 1, etc.). On the other hand, it is expected that the ion exchange membrane (IV) is unlikely to suffer performance degradation due to peeling of the ion exchange resin due to its structure, even if the porous substrate (II) or the mesh-like support material (III) deteriorates.

[0105] [Applications of ion exchange membranes] The ion exchange membrane (I) and the ion exchange membrane (IV) thus formed are, for example, appropriately cut into an appropriate size and used or sold.

[0106] The ion exchange membrane (I) and the ion exchange membrane (IV) of the present embodiment can be used without limitation in known applications. For example, they can be used as electrodialysis membranes, diffusion dialysis membranes, reverse electrodialysis membranes, fuel cells (e.g., methanol fuel cells), solid polymer membrane cells, and electrolyte membranes of various secondary batteries. For example, in the electrodialysis membrane, the ion exchange membrane (I) is a low-resistance membrane, so that a reduction in running costs can be expected; in the diffusion dialysis membrane, the ion exchange membrane (I) is thinned, so that a dramatic improvement in ion permeation flux can be expected; in the reverse electrodialysis membrane, the ion exchange membrane has a high transport number and low membrane resistance, so that an improvement in output performance can be expected; and in the electrolyte membrane for fuel cells, the ion exchange membrane (I) is thinned, so that a dramatic improvement in proton conductivity can be expected. EXAMPLES

[0107] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The abbreviations used in this example are as follows: (1) Solvent DMSO: Dimethyl sulfoxide DMF: N,N-dimethylformamide (2) Aromatic polyether components DFBP: 4,4'-Difluorobenzophenone DSDFBP: 5,5'-Carbonylbis(sodium 2-fluorobenzenesulfonate) TMBPF: 3,3',5,5'-Tetramethyl-4,4'-dihydroxydiphenylmethane The test methods used in the examples are as follows.

[0108] Resin evaluation <Weight average molecular weight (Mw)> The weight average molecular weight (Mw) was determined by GPC (Gel Permeation Chromatography) under the following conditions. (1) Measurement temperature: 40℃ (2) Developing solvent: DMF (3) Flow rate: 0.7ml / min (4) Injection volume: 500μl (5) Detector: UV detector (6) Molecular weight standard: Standard polystyrene

[0109] More specifically, the high performance liquid chromatograph (HPLC) used in the GPC measurement is a combination of the following devices in a conventional manner. HPLC: Shimadzu RID-10A-LC-10AT system Column oven: Shimadzu CTO-10A model UV detector: JASCO 875-UV type Guard column: Showa Denko KD-G type column (SHODEX) GPC columns: Two KD805 columns, one KD802.5 column, and one 802 column manufactured by Showa Denko K.K. (SHODEX) were used connected in series.

[0110] <Sulfonic acid unit content> It was determined using the ratio of the amounts of raw materials used in the resin synthesis. -Ion exchange membrane evaluation <Thickness> The thickness was measured using a JASCO spectrophotometer (ellipsometry). Specifically, when light is incident on a film with a refractive index n at a certain angle (θ), the reflected light A from the front side of the film and the reflected light B from the back side interfere with each other, resulting in a wavy interference spectrum. The thickness (d) was calculated from equation (1) by counting the number of peaks (mountains or valleys) (Δm) of the interference spectrum within a certain wavelength range (λ1 to λ2).

[0111]

number

[0112] <Membrane resistance measurement> The sample membrane was immersed in 0.5M NaCl solution and reached swelling equilibrium. The sample membrane was then sandwiched between cells, and the 0.5M NaCl solution was added. The resistance R at 25°C was measured using an LCR meter. l The resistance R0 was measured without the membrane under the same conditions. l The membrane resistance Rm was calculated by subtracting the value of R0 from the above using the following formula. Rm=R l -R0 Here, R l is the resistance when the membrane is set, and R0 is the resistance without the membrane.

[0113] <Membrane charge density> Effective membrane area: 8cm 2 Ag-AgCl electrodes were placed in both chambers of a two-chamber glass cell separated by a cation exchange membrane, and KCl solutions of different concentrations were placed in both cells. The membrane potential was measured by changing the concentrations of both cells while maintaining the concentration ratio of the two cells at r = 3. At this time, the potential was based on the high-concentration side. The relationship between the low-concentration side KCl concentration and the measured membrane potential was analyzed using the Teorell-Meyer and Sievers theoretical formula shown below to calculate the membrane charge density.

[0114]

number

[0115] <Dynamic transport number> Effective membrane area: 8cm 2 A two-chamber glass cell was separated by a cation exchange membrane, and Ag-AgCl electrodes were placed in both chambers. A 0.5 mol / L NaCl aqueous solution was used in both chambers, and the current density was 10 mA / cm. 2 After scanning for 75 min with a charge of 360 C, the negative electrode concentration (C a [mol / dm 3 ]) and the positive electrode concentration (C c [mol / dm 3 The dynamic transport number was calculated from the concentration obtained using the following formula. Theoretical equivalent: Ea = (I×s) / (96500q / mol) = mq: Note I =q / s Negative electrode side concentration:C a [mol / dm 3 ] Positive electrode side concentration:C c [mol / dm 3 ] Equivalent transferred: Δm[meq]=(Cc-Ca) / 2 Dynamic transport number: t + = Δm / Ea

[0116] (Monomer synthesis example 1) According to the method described in paragraph

[0061] (Synthesis Example 1) of JP2014-533A, white crystals of DSDFBP represented by the following formula were obtained. The yield was 155.2 g (0.386 mol, 70% yield).

[0117] [ka]

[0118] (Resin synthesis example 1) In a five-necked reactor equipped with a nitrogen inlet tube, a thermometer, a reflux condenser, and a stirrer, 32.1 g (0.076 mol) of DSDFBP obtained in Monomer Synthesis Example 1, 66.3 g (0.304 mol) of DFBP, 97.4 g (0.380 mol) of TMBPF, and 65.7 g (0.475 mol) of potassium carbonate were weighed out. 783.4 g of DMSO and 261.1 g of toluene were added thereto, and the mixture was stirred under a nitrogen atmosphere and heated at 130° C. for 12 hours. The generated water was removed from the system, and then the toluene was distilled off.

[0119] The reaction was continued at 160°C for 12 hours to obtain a viscous polymer solution. The obtained solution was diluted with 570g of toluene and then poured into 2400g of methanol. The precipitated polymer powder was filtered, washed, and then dried at 150°C for 4 hours to obtain 171.6g of polyetherketone powder (95% yield) (Resin 1). The results of the evaluation of various physical properties are shown in Table 1. Resin (1) is a structural group (1)

[0120] [ka] The structure represented by the following formula (2) is

[0121] [ka] It has a structure represented by the following formula:

[0122] (Resin synthesis example 2) The resin raw materials and solvent were 48.1 g (0.114 mol) of DSDFBP, 58.0 g (0.265 mol) of DFBP, 97.4 g (0.380 mol) of TMBPF, 65.7 g (0.475 mol) of potassium carbonate, 814.4 g of DMSO, and 271.5 g of toluene. Except for this, 175.2 g of polymer powder (93% yield) (Resin 2) was obtained in the same manner as in Resin Synthesis Example 1. The results of the evaluation of various physical properties are shown in Table 1.

[0123] (Resin synthesis example 3) The resin raw materials and solvent were 64.2 g (0.152 mol) of DSDFBP, 49.8 g (0.228 mol) of DFBP, 97.4 g (0.380 mol) of TMBPF, 65.7 g (0.475 mol) of potassium carbonate, 845.4 g of DMSO, and 281.8 g of toluene. Except for this, 168.7 g of polymer powder (86% yield) (Resin 3) was obtained in the same manner as in Resin Synthesis Example 1. The results of the evaluation of various physical properties are shown in Table 1.

[0124] [Table 1]

[0125] [Examples 1, 2, and 3] Resins 1, 2, and 3 produced in Resin Synthesis Examples 1, 2, and 3 were dissolved in DMF to prepare varnishes, which were then cast onto a release sheet and dried at 150°C for 10 minutes to obtain films of resins 1, 2, and 3. These films were peeled off from the release sheet to form free-standing films, and cation exchange membranes 1, 2, and 3 were obtained.

[0126] Next, as a porous substrate, a material having an air permeability of 300 cm as measured by the A method (Fragile type method) described in JIS L 1096 was used. 3 / cm 2 Two sheets of polypropylene nonwoven fabric (Syntex (registered trademark) PS-105, manufactured by Mitsui Chemicals, Inc.) with a diameter of 1 / s and a thickness of 290 μm were prepared, and the cation exchange membranes 1, 2, and 3 were sandwiched between these nonwoven fabrics and integrated to obtain cation exchange membranes 4-1, 4-2, and 4-3. The evaluation results of the cation exchange membranes 4-1, 4-2, and 4-3 are shown in Table 2.

[0127] [Example 4] A cation exchange membrane 4-4 was obtained in the same manner as in Example 2, except that a mesh-like support material (made of polyester, mesh number: 225 / inch2, mesh size: 113x113 μm: pore size: 50x50 μm, opening ratio: 31%) was used instead of the porous substrate. The evaluation results are shown in Table 2.

[0128] [Table 2]

[0129] [Comparative Example] As the cation exchange membrane, Neocepta (registered trademark) CMX manufactured by Astom Co., Ltd. was used. (According to the description in Non-Patent Document 1, Neocepta has a structure in which an ion exchange resin is attached to a substrate film, and the ion exchange resin itself is not a self-supporting membrane.) [Explanation of symbols]

[0130] 1: Ion exchange membrane (I) 2: Porous base material (II)

Claims

1. It is a free-standing membrane, the polymer (P) contains 10% by mass or more of a repeating structural unit (A) selected from a repeating structural unit having a cationic structural group (a1), the end of which, constituting the main chain, is a group containing a Group 16 atom of the periodic table, and a repeating structural unit having an anionic structural group (a2), the end of which, constituting the main chain, is a group containing a Group 16 atom of the periodic table, and a repeating structural unit (B) which does not have the cationic structural group (a1) or the anionic structural group (a2), and the end of which, constituting the main chain, is a group containing a Group 16 atom of the periodic table, and the polymer (P) contains 10% by mass or more of a repeating structural unit (A) which contains a repeating structural unit (A) which contains a Group 16 atom of the periodic table, and a repeating structural unit (B) which does not have the cationic structural group (a1) or the anionic structural group (a2), and the end of which, constituting the main chain, is a group containing a Group 16 atom of the periodic table, and the total content of the cationic structural group (a1) and the anionic structural group (a2) with respect to the total of the structural units (A) and (B) is 5 to 90 mol % (wherein the total of the structural units (A) and (B) is taken as 100 mol %), The membrane resistance is 0.1 to 2.0 Ω·cm 2 , and The polymer (P) is an aromatic polyether resin containing a structural group (1) represented by the following formula (1-1) or (1-2) and a structural group (2) represented by the following formula (2): 【Chemistry 1】 [In formulas (1-1) and (1-2), m represents an integer of 1 to 10; A 1 and A 3 are each independently a direct bond, -CH 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -O- or -CO-; Z is each independently a group selected from a protonic acid group and an ammonium base; s is each independently an integer of 0 to 3; t is each independently an integer of 0 to 4; and the lines at both ends represent bonds to adjacent structural groups. In formula (2), R 6 to R 10 each independently represent H, Cl, F, CF 3 , or C m H 2m+1 (m is an integer of 1 to 10); At least one of R 6 to R 10 is C m H 2m+1 (m is an integer of 1 to 10), Two or more of each of R 6 to R 10 may be present in an aromatic ring, and when two or more C m H 2m+1 are present in one aromatic ring, each C m H 2m+1 may be the same as or different from each other. A 4 to A 6 each independently represent a direct bond, --CH 2 --, --C(CH 3 ) 2 --, --C(CF 3 ) 2 --, --O-- or --CO--. k and l each independently represent 0 or 1. The lines at either end indicate bonds between adjacent structural groups.]

2. The ion exchange membrane (I) according to claim 1, having a thickness of 0.01 to 3.0 μm.

3. The ion exchange membrane (I) according to claim 1 or 2, One or more layers selected from a porous substrate (II) and a mesh-like support material (III); (IV) An ion exchange membrane having a laminated structure comprising:

4. The porous substrate (II) has an air permeability of 100 to 400 cm as measured by JIS L 1096 Method A (Fragile type method). 3 / cm 2 The ion exchange membrane (IV) according to claim 3, wherein:

5. The ion exchange membrane (IV) according to claim 3 or 4, wherein the mesh support (III) has 5 to 2,000 pores per inch.

Citation Information

Patent Citations

  • Proton conductive block copolymer and proton conductive film

    JP2004359925A

  • Porous membrane for fuel cell electrolyte membrane and its manufacturing method

    JP2008004500A

  • Polymer electrolyte membrane, and manufacturing method thereof

    JP2008269884A

  • Cation exchange membrane and method for production thereof

    JP2009096923A

  • Method of manufacturing electrolyte film

    JP2011026565A