Water-absorbent sheet and absorbent article including same
The water-absorbing sheet design with controlled initial absorption speed addresses backflow and side leakage issues in disposable diapers, ensuring effective liquid management and user comfort.
Patent Information
- Application Number
- JP2021008743
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-07
- Filing Date
- 2021-01-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-01-22
AI Technical Summary
Water-absorbing sheets used in disposable diapers experience issues with liquid backflow and side leakage, particularly when exposed to intermittent liquid intake, leading to discomfort and skin irritation.
A water-absorbing sheet design with a first base material, a second base material, and a water-absorbing layer in between, utilizing a particulate water-absorbing agent with an adjusted initial absorption speed of 2.2 to 3.0 seconds, to minimize backflow and side leakage.
Significantly reduces liquid backflow and side leakage even with multiple intermittent liquid introductions, enhancing user comfort and reducing skin irritation.
Smart Images

Figure 0007576986000004 
Figure 0007576986000005 
Figure 0007576986000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-absorbent sheet and an absorbent article including the same. [Background technology]
[0002] Super absorbent polymers (SAPs) are water-swellable, water-insoluble polymer gelling agents that are used in a variety of applications, including hygiene materials such as disposable diapers, sanitary napkins, and adult incontinence products, soil water retention agents in agricultural and horticultural applications, and industrial water-stopping agents.
[0003] These absorbent articles are generally manufactured in paper diaper manufacturing plants as absorbent bodies that are individually molded for each absorbent article by mixing absorbent resin and fibrous material, and are processed into absorbent bodies of various shapes (for example, hourglass-shaped, fox-shaped, oval, etc. when viewed in plan) depending on the purpose. These manufacturing methods for absorbent bodies are the mainstream for current paper diapers, since they can be processed into any shape because they are individually molded, and the amount of fiber and absorbent resin can be easily adjusted for each absorbent article.
[0004] However, in recent years, paper diapers have begun to be manufactured using absorbents (called water-absorbent sheets, usually cut into rectangles about 10 cm wide and several tens of cm long) made by cutting a long water-absorbent sheet with water-absorbent resin fixed between two sheets during the manufacturing process of sanitary materials. By purchasing or manufacturing a long continuous water-absorbent sheet, paper diaper manufacturers can simplify the manufacturing process of paper diapers, and furthermore, by not using pulp, paper diapers can be made thinner. Water-absorbent sheets are configured by sandwiching and fixing water-absorbent resin particles between upper and lower sheets (particularly nonwoven sheets), and usually after a long continuous sheet is manufactured, the long continuous sheet is cut into a rectangle about 10 cm wide and several tens of cm long, which is then incorporated into paper diapers (for example, Patent Document 1).
[0005] Unlike conventional sanitary materials (disposable diapers), disposable diapers made with absorbent sheets have a short history, and the reality is that there has been almost no development of absorbent resins suitable for absorbent sheets or proposals for parameters for them, and the absorbent resins used in conventional disposable diapers are used as is for absorbent sheets. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2010 / 143635 Summary of the Invention [Problem to be solved by the invention]
[0007] The inventors have found that, due to the structure unique to the mainstream water-absorbent sheet being thin, the absorbed liquid is easily released in the direction of the introduction of the absorbed liquid when pressure is applied to the water-absorbent sheet, which is called "backflow". Backflow is also called re-wet. The inventors have found that the occurrence of backflow is more prominent when the liquid is introduced intermittently multiple times (especially three or more times) and the amount of introduced liquid is large. When backflow occurs, the skin in contact with the water-absorbent sheet comes into contact with the backflowed liquid and is exposed to a highly humid state. This not only causes discomfort to the user, but also makes the skin in contact with the water-absorbent sheet more susceptible to rashes.
[0008] In the process of diligently studying how to solve the problem of backflow when liquid is introduced intermittently multiple times (especially three or more times), the inventors conducted research and development to design a water-absorbent sheet so that the absorbed liquid does not return upward (toward the skin), but discovered that this makes it more likely to leak in the surface direction (side leakage). Side leakage is a phenomenon in which, for example, when the water-absorbent sheet is placed vertically or tilted, liquid that cannot be instantly absorbed after reaching the water-absorbing layer leaks out from the water-absorbent sheet in the surface direction. It was discovered that the occurrence of this side leakage is also prominent when liquid is introduced intermittently multiple times (especially three or more times) and the amount of introduced liquid is large.
[0009] Therefore, the present invention has been made in consideration of the above circumstances, and aims to provide a novel water-absorbent sheet that can significantly reduce liquid leakage from the water-absorbent sheet due to backflow and lateral leakage, even if liquid is intermittently introduced multiple times (particularly, three or more times). [Means for solving the problem]
[0010] The present inventors have conducted intensive research to solve the above problems. As a result, they have found that the above problems can be solved by a water-absorbent sheet having a first substrate, a second substrate, and a water-absorbent layer located between the first substrate and the second substrate, the water-absorbent layer containing a particulate water-absorbing agent, the first substrate being located on the side where an aqueous liquid is introduced, and an initial absorption speed adjusted to 2.2 seconds to 3.0 seconds, and have completed the present invention. Effect of the Invention
[0011] According to the present invention, a novel water-absorbent sheet is provided which can significantly reduce liquid discharge from the water-absorbent sheet due to backflow and lateral leakage, even when liquid is intermittently introduced multiple times (particularly, three or more times). [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic diagram illustrating a cross section of a water-absorbent sheet according to one embodiment of the present invention. [Diagram 2] 1 is a schematic diagram illustrating a cross section of a water-absorbent sheet according to one embodiment of the present invention. [Diagram 3] 1 is a schematic diagram illustrating a cross section of a water-absorbent sheet according to one embodiment of the present invention. [Figure 4] 1 is a schematic diagram illustrating a cross section of a water-absorbent sheet according to one embodiment of the present invention. [Diagram 5] FIG. 1 is a schematic diagram showing an apparatus for measuring GPR. [Figure 6] FIG. 2 is a plan view and a right side view showing a sample used in evaluating the amount of return, and shows how the water-absorbent sheet produced in the example is wrapped in a liquid-impermeable sheet. [Figure 7] 1A and 1B are a plan view and a front view of a liquid injection tube used in evaluating the amount of backflow. [Figure 8] FIG. 2 is a front view showing a liquid injection tube placed on the water-absorbent sheet used in the examples of the present application. [Figure 9] FIG. 11 is a front view showing a state in which a sodium chloride aqueous solution is poured into a water-absorbent sheet from a liquid pouring tube using a funnel. [Figure 10] FIG. 1 is a schematic diagram showing an apparatus used for evaluating the amount of leakage in the surface direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described below while showing the best mode. Throughout this specification, the expression of the singular form should be understood to include the concept of the plural form, unless otherwise specified. Therefore, the singular article (for example, in the case of English, "a", "an", "the", etc.) should be understood to include the concept of the plural form, unless otherwise specified. In addition, it should be understood that the terms used in this specification are used in the sense commonly used in the field, unless otherwise specified. Therefore, unless otherwise defined, all technical terms and scientific and technical terms used in this specification have the same meaning as commonly understood by those skilled in the art to which this invention belongs. In the case of conflict, this specification (including definitions) will take precedence. The present invention is not limited to the following embodiments, and various modifications can be made within the scope of the claims.
[0014] [1. Definition or explanation of terms] [1-1. Water-absorbent sheet] The absorbent sheet is in the form of a continuous sheet or a roll obtained by winding up the continuous sheet. When using the absorbent sheet, the continuous sheet is cut into an appropriate shape (such as a rectangle) and then incorporated into an absorbent article (such as a paper diaper, a sanitary napkin, or a pad for incontinent people). Absorbent articles such as paper diapers (disposable diapers), sanitary napkins, and pads for incontinent people have an absorbent body that absorbs and retains bodily fluids such as urine and menstrual blood excreted from the body, a flexible liquid-permeable front sheet arranged on the side that contacts the body, and a liquid-impermeable back sheet arranged on the side opposite to the side that contacts the body. The absorbent sheet can be used as the absorbent body. Conventional paper diapers are absorbent articles that are individually molded for each paper diaper and have a shape that fits the buttocks. Therefore, such absorbents have technical properties that are different from the absorbent sheet of the present invention.
[0015] [1-2. Water-absorbing resin] In this specification, the term "water-absorbent resin" refers to a polymer cross-linked polymer (polymer gel) having a water swelling coefficient (CRC) of 5 g / g or more as defined by ERT441.2-02 and a water-soluble component (Ext) of 50 mass% or less as defined by ERT470.2-02.
[0016] The water-absorbent resin is preferably a hydrophilic cross-linked polymer obtained by cross-linking and polymerizing an unsaturated monomer having a carboxyl group. The shape of the water-absorbent resin may be a sheet, a fiber, a film, a particle, a gel, or the like. The water-absorbent sheet according to one embodiment of the present invention uses a particle-shaped water-absorbent resin.
[0017] In addition, in this specification, the term "water-absorbent resin" is a concept that also includes intermediates in the manufacturing process of the water-absorbent resin. For example, a hydrogel-like crosslinked polymer after polymerization, a dried polymer after drying, a water-absorbent resin powder before surface crosslinking, etc. may also be referred to as a "water-absorbent resin".
[0018] Thus, in this specification, in addition to the water-absorbent resin itself, the water-absorbent resin composition and the intermediate may be collectively referred to as the water-absorbent resin.
[0019] [1-3. Water absorbents, particulate water absorbents] In this specification, the term "water-absorbing agent" refers to a composition (or absorbent gelling agent) for absorbing an aqueous liquid (sometimes simply referred to as "liquid" in this specification) containing a water-absorbing resin as a main component. Here, the aqueous liquid (liquid) is not limited to water, but is any liquid containing water. The aqueous liquid absorbed by the water-absorbent sheet according to one embodiment of the present invention is urine, menstrual blood, sweat, and other body fluids.
[0020] In this specification, the term "particulate water absorbing agent" means a particulate (powdered) water absorbing agent (corresponding to particulate water absorbing resin since the water absorbing agent contains a water absorbing resin as a main component). The concept of the "particulate water absorbing agent" includes both a single particle of the particulate water absorbing agent and an aggregate of a plurality of particulate water absorbing agents. In this specification, "particulate" means having a particle shape. Here, the term "particle" refers to a relatively small divided body of a substance, and has a size of several Å to several mm (see "particle", McGraw-Hill Scientific and Technical Dictionary 3rd Edition, edited by McGraw-Hill Scientific and Technical Dictionary Editorial Committee, Nikkan Kogyo Shimbun, 1996, p. 1929). In this specification, the term "particulate water absorbing agent" may be simply referred to as "water absorbing agent".
[0021] In this specification, the first particulate water absorbing agent and the second particulate water absorbing agent described below may be collectively referred to (i.e., a mixture thereof), or one of them may simply be referred to as the "particulate water absorbing agent."
[0022] The particulate water absorbing agent contains a water absorbent resin as a polymer as a main component. In this specification, the particulate water absorbing agent is not limited to an embodiment in which the total amount (100 mass%) is only the water absorbent resin. As long as the above-mentioned CRC and Ext are satisfied, the particulate water absorbing agent may be a water absorbent resin composition containing an additive to be added internally. The particulate water absorbing agent contains 60 to 100 mass%, preferably 70 to 100 mass%, more preferably 80 to 100 mass%, further preferably 90 to 100 mass%, and particularly preferably 95 to 100 mass% of the water absorbent resin as a polymer. The remainder of the particulate water absorbing agent may contain water, additives that can be added externally (such as inorganic fine particles), and the like. The particulate water absorbing agent used in the examples of the present application contains 80 to 100 mass% of the water absorbent resin.
[0023] That is, the upper limit of the water absorbent resin in the particulate water absorbing agent is, for example, 100 mass%, 99 mass%, 97 mass%, 95 mass%, or 90 mass%, and preferably further contains 0 to 10 mass% of components other than the water absorbent resin, in particular, additives that can be added externally (such as inorganic fine particles).
[0024] The particulate water absorbing agent preferably has a water content of 0.2 to 30% by mass. Even when water is contained, the agent can be called a particulate water absorbing agent.
[0025] Examples of the water-absorbing resin that is the main component of the particulate water-absorbing agent include polyacrylic acid (salt)-based resin, polysulfonic acid (salt)-based resin, maleic anhydride (salt)-based resin, polyacrylamide-based resin, polyvinyl alcohol-based resin, polyethylene oxide-based resin, polyaspartic acid (salt)-based resin, polyglutamic acid (salt)-based resin, polyalginic acid (salt)-based resin, starch-based resin, and cellulose-based resin. Among these, polyacrylic acid (salt)-based resin is preferably used as the water-absorbing resin.
[0026] [1-4. Polyacrylic acid (salt)] In this specification, "polyacrylic acid (salt)" refers to polyacrylic acid and / or its salt. The polyacrylic acid (salt) is a polymer containing repeating units of acrylic acid and / or its salt (hereinafter referred to as "acrylic acid (salt)") as a main component, and further containing a graft component as an optional component. The polyacrylic acid (salt) is obtained by polymerization of acrylic acid (salt), hydrolysis of polyacrylamide, polyacrylonitrile, etc. Preferably, the polyacrylic acid (salt) is obtained by polymerization of acrylic acid (salt).
[0027] Here, "containing as a main component" means that the amount of acrylic acid (salt) used when polymerizing polyacrylic acid (salt) is usually 50 to 100 mol %, preferably 70 to 100 mol %, more preferably 90 to 100 mol %, and even more preferably substantially 100 mol %, based on the total amount of monomers (excluding the internal crosslinking agent) used in the polymerization.
[0028] [1-5. EDANA and ERT] "EDANA" is an abbreviation for European Disposables and Nonwovens Associations. "ERT" is an abbreviation for EDANA Recommended Test Methods, a European standard (effectively a global standard) for measuring water-absorbent resins. In this specification, unless otherwise specified, the physical properties of water-absorbent resins are measured in accordance with the 2002 edition of ERT.
[0029] [1-6.Other] In this specification, the range "X to Y" means "X or more and Y or less."
[0030] In this specification, unless otherwise noted, the unit of mass "t (ton)" means "metric ton." "ppm" means "ppm by mass." "Mass" and "weight," "parts by mass" and "parts by weight," "% by mass" and "% by weight," "ppm by mass" and "ppm by weight" are each treated as having the same meaning.
[0031] In this specification, "acid (salt)" means "acid and / or its salt." "(Meth)acrylic" means "acrylic and / or methacrylic."
[0032] In this specification, the unit of volume "liter" may be written as "l" or "L". "% by mass" may be written as "wt%". When measuring trace components, values below the detection limit may be written as ND (Non Detected).
[0033] [2. Water-absorbent sheet] The water-absorbent sheet of the present invention has a first substrate, a second substrate, and a water-absorbent layer located between the first substrate and the second substrate, the water-absorbent layer contains a particulate water-absorbing agent, the first substrate is located on the side where an aqueous liquid is introduced, and the initial absorption speed is adjusted to 2.2 to 3.0 seconds. This configuration provides a novel water-absorbent sheet that can significantly reduce liquid discharge from the water-absorbent sheet due to backflow and lateral leakage even if liquid is introduced intermittently multiple times (particularly, three or more times).
[0034] As described above, the inventors have found that when liquid is intermittently introduced multiple times, side leakage is likely to occur when trying to solve the problem of backflow. In other words, they have found that there is a trade-off between the specific backflow amount and the specific leakage amount. Here, the specific backflow amount and the specific leakage amount refer to the backflow amount and leakage amount evaluated by the method described in the examples of the present application, respectively.
[0035] In the process of intensively studying to solve this trade-off problem, it was discovered that, phenomenologically, if the initial absorption of liquid by the absorbent sheet is too fast, side leakage is small but backflow is likely to occur, and if the initial absorption of liquid by the absorbent sheet is too slow, backflow is small but side leakage is likely to occur. In order to solve this trade-off, as described below, it was necessary to try and error the type of each substrate, the thickness of the substrate, the basis weight of the substrate, the type of water absorbing agent, the type of adhesive, the amount of adhesive applied, the application method, etc., and complex and excessive consideration was required. Therefore, as a specific physical property value of the absorbent sheet, the absorption speed immediately after the introduction of the aqueous liquid was defined as the "initial absorption speed". In the present invention, the "initial absorption speed" is an index indicating the degree of liquid compatibility of the first substrate with the aqueous liquid introduced into the absorbent body, and is a physical property that greatly affects the initial liquid capture ability in absorbent articles such as paper diapers. In a conventional paper diaper using an absorbent containing pulp, even if the liquid compatibility of the top layer substrate corresponding to the first substrate of the present invention is somewhat poor, the liquid capture property of the paper diaper does not decrease because the liquid capture property of the pulp itself is very high. However, since the water-absorbent sheet is an absorbent that does not contain pulp, the liquid compatibility of the first substrate has a large effect on the liquid capture property of the paper diaper. A method for evaluating the liquid compatibility of a substrate includes a method for measuring the contact angle at the moment when a droplet of an aqueous liquid is dropped on the substrate, but this method can only determine the difference between extreme hydrophilicity and hydrophobicity, and cannot evaluate the slight difference required in the present invention. Therefore, the present inventors have examined various evaluation methods and have found that the time required from the time when a very small amount of colored aqueous liquid is dropped on the substrate at a constant speed to the time when the liquid is completely absorbed by the substrate surface and the color of the liquid disappears can be defined as the "initial water absorption speed", and the above problem can be solved by keeping the "initial absorption speed" within a specific range.
[0036] Thus, the water-absorbent sheet of the present invention has an initial absorption rate adjusted to a specific range. This initial absorption rate is an index for evaluating how long it takes for the water-absorbent sheet to absorb the first aqueous liquid (urine water, 0.9% sodium chloride solution as a substitute for urine water) when the first aqueous liquid is introduced into the water-absorbent sheet from the first substrate side. Specifically, the method described in the Examples is used. If the initial absorption rate exceeds 3.0 seconds, the aqueous liquid cannot penetrate into the substrate at the moment the aqueous liquid contacts the first substrate, making it difficult to solve the problem of the specific leakage amount. On the other hand, if the initial absorption rate is less than 2.2 seconds, the aqueous liquid is instantly absorbed only in the vicinity of the point where the aqueous liquid contacts the first substrate, and the aqueous liquid cannot be diffused throughout the water-absorbent sheet, resulting in insufficient liquid capture, making it difficult to solve the problem of the specific return amount.
[0037] Here, factors that influence the initial absorption rate include the type, structure, and physical properties of the first substrate; the type, physical properties, amount, and application method of the adhesive disposed on the first substrate; and the physical properties of the particulate water absorbing agent (physical properties of the first particulate water absorbing agent and the second particulate water absorbing agent). For example, if the hydrophilicity of the first substrate is high, the initial absorption rate is likely to be inclined toward a faster direction, and conversely, if the hydrophobicity is high, the initial absorption rate is likely to be inclined toward a slower direction. Also, if the hydrophilicity of the adhesive disposed on the first substrate is high, the initial absorption rate is likely to be inclined toward a faster direction, and conversely, if the hydrophobicity is high, the initial absorption rate is likely to be inclined toward a slower direction. Also, it is considered that the larger the droplets of the adhesive (i.e., the sparser the adhesive is dispersed on the first substrate), the faster the initial absorption rate is, and conversely, the smaller the droplets of the adhesive (i.e., the denser the adhesive is dispersed on the first substrate), the slower the initial absorption rate is. Also, it is considered that if the content (amount used) of the adhesive placed on the first base material is small, the initial absorption speed tends to be fast, and conversely, if the content (amount used) of the adhesive placed on the first base material is large, the initial absorption speed tends to be slow. It is considered that if the CRC of the particulate water absorbing agent (particularly the first particulate water absorbing agent) is high, the initial absorption speed tends to be fast. It is considered that if the CRC of the particulate water absorbing agent (particularly the second particulate water absorbing agent) is high, the initial absorption speed tends to be fast. It is considered that if the surface tension of the particulate water absorbing agent (particularly the second particulate water absorbing agent) is high, the initial absorption speed tends to be fast. As described above, the value of the initial absorption speed is considered to depend on several factors. However, a person who intends to practice the present invention can adjust the initial absorption speed to 2.2 to 3.0 seconds by appropriately adjusting the type, structure, and physical properties of the first substrate; the type, physical properties, amount, and application method of the adhesive placed on the first substrate; and the physical properties of the particulate water absorbing agent (physical properties of the first particulate water absorbing agent and the second particulate water absorbing agent) by referring to the above findings and the examples described below.
[0038] <Specific adjustment method> The type and structure of the first substrate used in the present invention is preferably a nonwoven fabric with fewer inter-fiber voids such as an air-laid nonwoven fabric, since it is easier to adjust the initial absorption rate than a nonwoven fabric with many inter-fiber voids such as an air-through nonwoven fabric. In addition, since the adhesive used in the present invention is hydrophobic and may deteriorate the liquid compatibility, it is preferable to use a hydrophilic substrate as the first substrate.
[0039] In the present invention, the amount of the first adhesive applied may be adjusted to within the range of 0.0005 to 0.3 times the amount of the first particulate absorbent. However, even if the type of first substrate is the same, the preferred amount of adhesive applied varies depending on the basis weight of the nonwoven fabric and other conditions. Therefore, to be precise, the amount of adhesive applied must be appropriately adjusted for the selected first substrate.
[0040] In the present invention, the adhesive application method can be "solvent dissolution spraying" in which a liquid solution-type adhesive is sprayed, or "heat melt spraying" in which a solid hot melt adhesive is heated and melted and sprayed. When the adhesive application method is solvent dissolution spraying, although it cannot be generally stated depending on the type of adhesive and the specifications of the nozzle spraying the adhesive, in the case of spraying with a large droplet diameter, specifically, when the discharge amount of the first adhesive to the first substrate is 0.5 g / sec or more, the preferred application amount of the first adhesive relative to the amount of the first particulate absorbent is 0.03 to 0.2 times. On the other hand, in the case of spraying with a small droplet diameter, specifically, when the discharge amount of the first adhesive to the first substrate is less than 0.5 g / sec, the preferred application amount of the first adhesive relative to the amount of the first particulate absorbent is 0.01 to 0.04 times.
[0041] In the present invention, when the adhesive is applied by hot melt spraying, the adhesive strength tends to be higher than that by solvent dissolving spraying, depending on the specifications of the nozzle for spraying the adhesive, so that it is possible to adjust the amount of adhesive applied to be smaller. Specifically, the amount of adhesive applied is preferably 0.005 to 0.03 times the amount of the first particulate absorbent.
[0042] It should be noted that, as described in the present specification, the "specific return amount evaluation" that measures the amount of return when liquid is intermittently introduced multiple times is a different index from the "return amount evaluation" measured under general conditions. Similarly, it should be noted that the "specific leakage amount evaluation" that measures the amount of side leakage when liquid is intermittently introduced multiple times is a different index from the "side leakage evaluation" measured under general conditions. A water-absorbent sheet that has a good "return amount evaluation" measured under general conditions and a good "side leakage evaluation" measured under general conditions does not necessarily have a good "specific return amount evaluation" and "return amount evaluation."
[0043] Thus, the water-absorbent sheet according to one embodiment of the present invention is suitable as an absorbent article (e.g., a diaper) for use by babies who are just learning to run and whose bladders are still small during the daytime when they are actively moving around, and is also suitable as an absorbent article (e.g., a diaper) for use by babies who turn over a lot and have a bad sleeping posture. Of course, the form of use is not limited to this. Furthermore, the mechanisms and the like described in this specification do not limit the technical scope of the claims of this application.
[0044] The water-absorbent sheet according to one embodiment of the present invention can be made thinner than absorbents used in conventional absorbent articles. When the water-absorbent sheet is used in a disposable diaper, the thickness is preferably 15 mm or less, more preferably 10 mm or less, even more preferably 7 mm or less, particularly preferably 5 mm or less, and most preferably 4 mm or less, for example, at 40% RH to 50% RH. On the other hand, the lower limit of the thickness is 0.2 mm or more, preferably 0.3 mm or more, and more preferably 0.5 mm or more, taking into consideration the strength of the water-absorbent sheet and the diameter of the particulate water-absorbing agent. The thickness of the water-absorbent sheet used in the examples of the present application was 3 mm to 5 mm under the above conditions.
[0045] The thickness of the absorbent sheet is measured using a large-type dial thickness gauge (thickness measuring device) (manufactured by Ozaki Seisakusho Co., Ltd., model number: JB, measuring element: anvil top and bottom φ50 mm). The absorbent body is divided into three equal parts in the longitudinal direction, and the measurement points are the center of each part (the intersection of a diagonal line drawn from the end of the absorbent body). For example, in the case of an absorbent sheet with a longitudinal length of 36 cm and a width direction of 10 cm, the measurement points are 6 cm from the left end in the longitudinal direction and 5 cm from both ends in the width direction (left), 18 cm from the left end in the longitudinal direction and 5 cm from both ends in the width direction (center), and 30 cm from the left end in the longitudinal direction and 5 cm from both ends in the width direction (right). Each part is measured twice, and the thickness measurement value is the average value of the total of six points. Specifically, the absorbent sheet is attached flat on a plate of a uniform thickness so that no wrinkles or distortions occur at the measurement point of the sheet, and the plate is then set on the lower probe of the thickness measuring device. Next, the upper probe of the thickness measuring device is brought close to a height of 2 to 3 mm from the absorbent sheet, and then the handle is slowly released and the combined thickness of the absorbent sheet and plate is measured. The thickness of the absorbent sheet is determined by the formula: T1 = T2 - T0 (T0: thickness of plate (mm), T1: thickness of absorbent sheet (mm), T2: thickness of absorbent sheet and plate (mm)).
[0046] The thicknesses of the first substrate, the second substrate, the intermediate sheet, and the wrapping sheet, which will be described later, are also measured in the same manner.
[0047] Hereinafter, the embodiment of the present invention will be described in more detail with reference to the attached drawings. The substrate on the liquid-absorbing side of the water-absorbent sheet may be in direct contact with aqueous liquid such as urine water, or the sheets may be laminated in any manner so long as the initial water absorption rate of the water-absorbent sheet is not hindered. In the description of the drawings, the same elements are given the same reference numerals, and duplicated descriptions are omitted. Also, the dimensional ratios in the drawings are exaggerated for the convenience of explanation, and may differ from the actual ratios.
[0048] FIG. 1 is a schematic diagram showing a cross section of a water-absorbent sheet 40 according to one embodiment of the present invention. In FIG. 1, an arrow indicates the direction in which the aqueous liquid (liquid) to be absorbed is introduced. The first substrate 11 is located on the side where the liquid to be absorbed (liquid to be absorbed) is introduced. That is, the first substrate is disposed on the liquid discharge side (for example, the skin side in the case of a paper diaper). This allows the aqueous liquid to directly contact the first substrate 11. The water-absorbent layer 12 is present between the first substrate 11 and the second substrate 13. The water-absorbent layer 12 includes a particulate water-absorbing agent 14a in contact with (or fixed to) the first substrate and a particulate water-absorbing agent 14b in contact with (or fixed to) the second substrate 13. Therefore, in the water absorbent sheet according to one embodiment of the present invention, the particulate water absorbing agent 14 (14a, 14b) is composed of a first particulate water absorbing agent 14a localized on the surface side of the first substrate 11 facing the second substrate 13, and a second particulate water absorbing agent 14b localized on the surface side of the second substrate 13 facing the first substrate 11. A part of the particulate water absorbing agents 14a, 14b may not be in contact with each substrate 11, 13 (or may not be fixed. They may be detached from each substrate 11, 13). Therefore, the water absorption "layer" does not only refer to a continuous body such as a sheet, but may be in any form as long as it exists with a certain thickness between the first substrate 11 and the second substrate 13. When the particulate water absorbing agents 14a, 14b are fixed to each substrate 11, 13, for example, as shown in FIG. 1, an adhesive 17 (a first adhesive 17a and a second adhesive 17b) may be used. The first adhesive refers to an adhesive disposed on the surface of the first substrate facing the second substrate, and the second adhesive refers to an adhesive disposed on the surface of the second substrate 13 facing the first substrate 11. In this specification, the first adhesive, the second adhesive, and the first' adhesive and the second' adhesive described below may be collectively referred to, or some of them may be simply referred to as "adhesive". A method for producing a water-absorbent sheet using an adhesive will be described in detail in [3.]. The water-absorbent layer 12 may also have an intermediate sheet 16 as necessary.1, a first particulate water absorbing agent 14a localized on the surface of the first substrate 11 facing the second substrate 13 and a second particulate water absorbing agent 14b localized on the surface of the second substrate 13 facing the first substrate 11 are present so as to sandwich an intermediate sheet 16. In this intermediate sheet 16, the water absorbing agent 14 fixed by, for example, adhesives 17 (17a, 17b) or the like may be detached, and the water absorbing agent 14 captured by the intermediate sheet 16 may be present.
[0049] As described above, the water-absorbent sheet 40 shown in FIG. 1 has an initial absorption speed adjusted to 2.2 to 3.0 seconds by appropriately adjusting the type, structure, and physical properties of the first substrate 11; the type, physical properties, amount, and application method of the first adhesive 17a disposed on the first substrate; and the physical properties of the particulate water-absorbing agent 14 (physical properties of the first particulate water-absorbing agent 14a and the second particulate water-absorbing agent 14b).
[0050] FIG. 2 is a schematic diagram showing a cross section of a water-absorbent sheet 40 according to one embodiment of the present invention. The water-absorbent sheet 40 of this embodiment has a wrapping sheet 18. The wrapping sheet is used for the following purposes: to maintain the shape of the water-absorbent sheet 40, which is a structure in which the particulate water-absorbing agent 14 is supported between the first substrate 11 and the second substrate 13; to prevent the particulate water-absorbing agent 14 supported between the first substrate 11 and the second substrate 13 from spilling (falling off); and to prevent the particulate water-absorbing agent 14 from directly contacting the skin when the particulate water-absorbing agent 14 permeates the first substrate 11 and migrates to the outer surface (surface that directly contacts liquid) of the first substrate 11 (the wrapping sheet may be provided for purposes other than those described above). Thus, in one embodiment of the present invention, the water-absorbent sheet is in a form in which the aqueous liquid contacts the first substrate 11 via the wrapping sheet. Although some wrapping sheets have meshes, the wrapping sheet of the embodiment of the present invention has meshes of a size that prevents the particulate water absorbing agent in the water absorbent sheet from migrating to the outside. In the embodiment in FIG. 2, the wrapping sheet 18 is disposed on the surface of the first substrate 11 on the side where the aqueous liquid is introduced. The wrapping sheet 18 is folded over so as to enclose the entire water absorbent layer 12 and the second substrate 13. Thus, the wrapping sheet 18 covers the entire first substrate 11, the water absorbent layer 12, and the second substrate 13. The wrapping sheet 18 does not need to cover the entire first substrate 11, the water absorbent layer 12, and the second substrate 13. For example, the wrapping sheet 18 may be disposed on the first substrate 11, folded over so as to enclose the side of the water absorbent layer 12 and the side of the second substrate 13, and folded over the surface of the second substrate 13 opposite to the surface that absorbs the liquid. In this case, the wrapping sheet 18 covers the first substrate 11, the water-absorbing layer 12, and the side surface of the second substrate 13, and also covers a part of the surface of the second substrate 13 opposite to the surface on which the water-absorbing layer 12 is provided (not shown). In one embodiment of the present invention, the wrapping sheet 18 can be fixed to the substrates 11 and 13 by using, for example, adhesives 17 (17c, 17d) as shown in Fig. 2. In Fig. 2, a first' adhesive 17c is disposed between the wrapping sheet 18 and the first substrate 11.Also, a second' adhesive 17d is disposed between the wrapping sheet 18 and the second base material 13. Note that, although the first' adhesive 17c and the second' adhesive 17d are disposed over the entire surface between the wrapping sheet 18 and each of the base materials 11 and 13 in Fig. 2, as long as the wrapping sheet 18 is fixed to the water-absorbent sheet 40 by a method such as crimping, there may be provided a region in which the first' adhesive 17c and the second' adhesive 17d are not disposed in part or in whole.
[0051] As described above, the water-absorbent sheet 40 shown in FIG. 2 has an initial absorption speed adjusted to 2.2 to 3.0 seconds by appropriately adjusting the type, structure, and physical properties of the first substrate 11; the type, physical properties, amount, and application method of the first adhesive 17a disposed on the first substrate; the physical properties of the particulate water-absorbing agent 14 (physical properties of the first particulate water-absorbing agent 14a and the second particulate water-absorbing agent 14b); and the type, physical properties, amount, and application method of the first' adhesive 17c disposed between the wrapping sheet 18 and the first substrate 11.
[0052] Fig. 3 is a schematic diagram showing a cross section of a water-absorbent sheet 40 according to one embodiment of the present invention. The water-absorbent sheet 40 shown in Fig. 3 is a modified example of the water-absorbent sheet 40 shown in Fig. 2, and the second' adhesive 17d is substantially not present between the wrapping sheet 18 and the second base material 13. In this specification, "substantially no adhesive is present" means that no adhesive is contained at all, or that even if an adhesive is contained, the amount of the adhesive is 0.001 g or less per 1 g of the first and second particulate water-absorbing agents. With such a configuration, the water-absorbent sheet can be efficiently wrapped by the wrapping sheet while achieving the intended effect of the present invention.
[0053] As described above, the initial absorption speed of the water-absorbent sheet 40 shown in FIG. 3 is adjusted to 2.2 to 3.0 seconds by appropriately adjusting the type, structure, and physical properties of the first substrate 11; the type, physical properties, amount, and application method of the first adhesive 17a disposed on the first substrate; the physical properties of the particulate water-absorbing agent 14 (physical properties of the first particulate water-absorbing agent 14a and the second particulate water-absorbing agent 14b); and the type, physical properties, amount, and application method of the first' adhesive 17c disposed between the wrapping sheet 18 and the first substrate 11.
[0054] FIG. 4 is a schematic diagram showing a cross section of a water-absorbent sheet 40 according to one embodiment of the present invention. The water-absorbent sheet 40 shown in FIG. 4 is a modified example of the water-absorbent sheet 40 shown in FIG. 2, and substantially no adhesive (first' adhesive 17c) is present between the wrapping sheet 18 and the first substrate 11. This configuration allows liquid to be easily introduced into the water-absorbent sheet 40, and the initial absorption rate can be increased. In addition, in the water-absorbent sheet 40 of this embodiment, a portion of the adhesive (second' adhesive 17d) is present between the wrapping sheet 18 and the second substrate 13. This configuration allows the water-absorbent sheet to be efficiently wrapped by the wrapping sheet while achieving the intended effect of the present invention. In a further modified example, the water-absorbent sheet 40 shown in FIG. 4 may not substantially have the second' adhesive 17d present between the wrapping sheet 18 and the second substrate 13, as in the embodiment shown in FIG. 3 (not shown).
[0055] As described above, the water-absorbent sheet 40 shown in FIG. 4 has an initial absorption speed adjusted to 2.2 to 3.0 seconds by appropriately adjusting the type, structure, and physical properties of the first substrate 11; the type, physical properties, amount, and application method of the first adhesive 17a disposed on the first substrate; the physical properties of the particulate water-absorbing agent 14 (physical properties of the first particulate water-absorbing agent 14a and the second particulate water-absorbing agent 14b); and the amount (i.e., substantially 0) of the first' adhesive 17c disposed between the wrapping sheet 18 and the first substrate 11.
[0056] Each of the components constituting the water-absorbent sheet will now be described in detail.
[0057] [2-1. First substrate, second substrate and intermediate sheet] The first substrate is a water-permeable sheet located on the side where the aqueous liquid (liquid) to be absorbed is introduced. The liquid to be absorbed is not limited to water, but may be urine, blood, sweat, feces, waste liquid, moisture, steam, ice, a mixture of water and an organic solvent and / or an inorganic solvent, rainwater, groundwater, etc., and is not particularly limited as long as it contains water. Preferred examples include urine, menstrual blood, sweat, and other body fluids.
[0058] The first substrate, the second substrate, and the intermediate sheet used in the absorbent sheet according to one embodiment of the present invention are preferably made of nonwoven fabric. The material of the nonwoven fabric is not particularly limited, but from the viewpoint of liquid permeability, flexibility, and strength of the absorbent sheet, pulp (cellulose) nonwoven fabric, polyolefin fiber (polyethylene (PE), polypropylene (PP), etc.), polyester fiber (polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), etc.), polyamide fiber (nylon, etc.), rayon fiber, pulp (cellulose) fiber, etc. are preferable. Nonwoven fabrics of other synthetic fibers and nonwoven fabrics manufactured by mixing synthetic fibers with cotton, silk, hemp fibers, etc. are also preferable. The nonwoven fabrics described above may be nonwoven fabrics containing only one type of the above-mentioned fiber, or nonwoven fabrics combining two or more types of fibers. The nonwoven fabrics used in the first substrate and the second substrate are preferably manufactured by the airlaid method. The nonwoven fabric used for the first and second substrates is preferably made of pulp (cellulose) fibers.
[0059] As described above, the nonwoven fabric used in the water-absorbent sheet according to one embodiment of the present invention is preferably a hydrophilic nonwoven fabric in order to increase water permeability, but the nonwoven fabric or the fibers that are the material of the nonwoven fabric may be hydrophilized using a hydrophilizing agent (such as a surfactant).
[0060] Examples of hydrophilizing agents include anionic surfactants (aliphatic sulfonates, higher alcohol sulfates, etc.), cationic surfactants (quaternary ammonium salts, etc.), nonionic surfactants (polyethylene glycol fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, etc.), silicone surfactants (polyoxyalkylene-modified silicones, etc.), polyester-based, polyamide-based, acrylic-based, and urethane-based resin-containing stain release agents. Examples of hydrophilizing agents include anionic surfactants (aliphatic sulfonates, higher alcohol sulfates, etc.), cationic surfactants (quaternary ammonium salts, etc.), nonionic surfactants (polyethylene glycol fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, etc.), silicone surfactants (polyoxyalkylene-modified silicones, etc.), polyester-based, polyamide-based, acrylic-based, and urethane-based resin-containing stain release agents.
[0061] The first substrate used in the water-absorbent sheet according to one embodiment of the present invention is a water-permeable sheet, since it is located on the side where the liquid to be absorbed is introduced. The second substrate and the intermediate sheet are also preferably water-permeable sheets having water permeability, and may be the same type or different types. The water permeability of the water-permeable sheet is determined by a coefficient of water permeability (JIS A1218:2009) of 1×10 -5 The water permeability coefficient is preferably 1×10 cm / sec or more. -4 cm / sec or more, more preferably 1×10 -3 cm / sec or more, and even more preferably 1×10 -2 cm / sec or more, and even more preferably 1×10 -1 The water-absorbent sheet according to one embodiment of the present invention is preferably a hydrophilic nonwoven fabric. By using a hydrophilic nonwoven fabric, the intended effect of the present invention can be efficiently achieved.
[0062] The thickness of the first substrate and the second substrate is preferably as thin as possible within a range that allows the substrate to have strength as a water-absorbent sheet, and is independently selected from the range of 0.01 to 2 mm, further 0.02 to 1 mm, 0.03 to 0.6 mm, or 0.05 to 0.5 mm per substrate. The basis weight is preferably 5 to 300 g / m per substrate. 2 , more preferably 8 to 200 g / m 2 , and more preferably 10 to 100 g / m 2 , and even more preferably 11 to 50 g / m 2 It is.
[0063] In the water-absorbent sheet according to one embodiment of the present invention, the nonwoven fabric used for the intermediate sheet is preferably an air-through nonwoven fabric. The nonwoven fabric used for the intermediate sheet is preferably bulky, specifically, 0.5 mm or more, more than 0.5 mm, 0.6 mm or more, more than 0.6 mm, 1 mm or more, or more than 1 mm. The nonwoven fabric described above may contain a small amount of pulp fibers to the extent that the thickness of the water-absorbent sheet is not increased. There is no particular upper limit on the thickness of the nonwoven fabric used for the intermediate sheet, but it is, for example, 4.9 mm or less, 4.8 mm or less, 4.7 mm or less, 4.6 mm or less, 4.0 mm or less, 3.0 mm or less, 2.5 mm or less, or 2.0 mm or less.
[0064] [2-2. Water absorption layer] The water-absorbing layer in the water-absorbent sheet according to one embodiment of the present invention contains a particulate water-absorbing agent.
[0065] (Particulate water absorbing agent) "surface tension" Surface tension is the work (free energy) required to increase the surface area of a solid or liquid, expressed per unit area. The surface tension referred to in this application refers to the surface tension of the aqueous solution when the particulate water absorbing agent is dispersed in a 0.90 mass % sodium chloride aqueous solution. The surface tension of the water absorbing agent is measured by the following procedure. That is, 50 ml of physiological saline adjusted to 20°C is placed in a thoroughly washed 100 ml beaker, and the surface tension of the physiological saline is first measured using a surface tensiometer (K11 automatic surface tensiometer manufactured by KRUSS). Next, a thoroughly washed 25 mm long fluororesin rotor and 0.5 g of the particulate water absorbing agent are placed in the beaker containing the physiological saline adjusted to 20°C after the surface tension measurement, and the mixture is stirred for 4 minutes under the condition of 500 rpm. After 4 minutes, the stirring is stopped, and after the particulate water absorbing agent containing the water is settled, the surface tension of the supernatant liquid is measured again by performing the same operation. In the present invention, a plate method using a platinum plate is adopted, and the plate is thoroughly washed with deionized water and heated and washed with a gas burner before each measurement.
[0066] In the water absorbent sheet according to one embodiment of the present invention, the surface tension of at least one of the particulate water absorbing agent (here, a mixture of the first particulate water absorbing agent and the second particulate water absorbing agent) is preferably 60 mN / m or more, 65 mN / m or more, 66 mN / m or more, 67 mN / m or more, 69 mN / m or more, 70 mN / m or more, 71 mN / m or more, and most preferably 72 mN / m or more. In particular, when the surface tension of the second particulate water absorbing agent is 60 mN / m or more or 65 mN / m or more, the effect of reducing the specific return amount and the specific leakage amount in the water absorbent sheet becomes remarkable. In the water-absorbent sheet according to one embodiment of the present invention, the upper limit of the surface tension of at least one of the particulate water-absorbing agent (here, a mixture of a first particulate water-absorbing agent and a second particulate water-absorbing agent), the first particulate water-absorbing agent, and the second particulate water-absorbing agent is not particularly limited, but is practically 73 mN / m or less.
[0067] In the water absorbent sheet according to one embodiment of the present invention, the CRC (absorption capacity without load) of at least one of the particulate water absorbing agent (here, a mixture of the first particulate water absorbing agent and the second particulate water absorbing agent) is 30 g / g or more, 32 g / g or more, 33 g / g or more, 34 g / g or more, 35 g / g or more, 36 g / g or more, 37 g / g or more, and 38 g / g or more, in the following order of preference. In particular, when the CRC of the first particulate water absorbing agent is 30 g / g or more or 35 g / g or more, the effect of reducing the specific return amount in the water absorbent sheet becomes remarkable. Here, in particular, the CRC of the first particulate water absorbing agent is preferably 30 g / g or more, and more preferably 35 g / g or more. By having such a lower limit, the effect of reducing the return can be obtained significantly. In particular, when the CRC of the second particulate water absorbing agent is less than 35 g / g, there is a risk that the effect of reducing backflow in the water absorbent sheet cannot be obtained. In the water absorbent sheet according to one embodiment of the present invention, the upper limit of the CRC of at least one of the particulate water absorbing agent (here, a mixture of the first particulate water absorbing agent and the second particulate water absorbing agent) is not particularly limited, but is preferably 40 g / g or less, 39 g / g or less.
[0068] In the water absorbent sheet according to one embodiment of the present invention, the AAP (absorption capacity against pressure) of at least one of the particulate water absorbing agent (here, a mixture of the first particulate water absorbing agent and the second particulate water absorbing agent), the first particulate water absorbing agent, and the second particulate water absorbing agent is preferably 25 g / g or more, 28 g / g or more, and 30 g / g or more in the following order of preference from the viewpoint of improving the performance of the water absorbent sheet (reducing the amount of return). There is no particular upper limit, but it is, for example, 37 g / g or less, 32 g / g or less. In the water absorbent sheet according to one embodiment of the present invention, when the AAP of the second particulate water absorbing agent is 28 g / g or more and 35 g / g or less, or less than 31 g / g, the effect of reducing the return and the leakage in the surface direction in the water absorbent sheet becomes remarkable. The AAP of the particulate water absorbing agent is an abbreviation of Absorption Against Pressure defined by ERT442.2-02, and means the water absorption capacity of the particulate water absorbing agent under pressure. Specifically, 0.9 g of the particulate water absorbing agent is subjected to a large excess of a 0.9 mass % sodium chloride aqueous solution for 1 hour at 2.06 kPa (21 g / cm 2 This refers to the water absorption capacity (unit: g / g) after swelling under a load of 0.3 psi (0.2 psi). In addition, ERT442.2-02 states it as Absorption Under Pressure (AUP), but this is essentially the same thing.
[0069] "GPR" Gel Permeation Rate (GPR) In this specification, the "liquid permeability" of the particulate water absorbing agent refers to the flowability of a liquid passing between swollen gel particles under a load. As an index of this, the gel permeability rate (GPR) is used. The gel permeability rate (GPR) of the particulate water absorbing agent contained in the water absorbent sheet according to one embodiment of the present invention is measured by the following procedure, changing the measurement conditions with reference to the Saline Flow Conductivity (SFC) test described in U.S. Pat. No. 5,849,405.
[0070] As a device for the measurement, a device 400 shown in FIG. 5 is used. The device 400 is roughly composed of a container 410 and a tank 420. A cell 411 (inner diameter 6 cm) is provided in the container 410, and a swelling gel 414 (a particulate water absorbing agent absorbed by water) can be stored inside the cell 411, and a liquid 423 can be introduced. In addition, a piston 412 is fitted into the cell 411, so that a pressure can be applied to the swelling gel 414. Wire meshes 413a and 413b (No. 400 stainless steel wire mesh, mesh size 38 μm) are stretched on the bottom surface of the cell 411 and the bottom surface of the piston 412, so that the swelling gel 414 (and the particulate water absorbing agent) cannot pass through. Here, a 0.90 wt % sodium chloride aqueous solution is used as the liquid 423. The tank 420 stores the liquid 423 inside. The liquid 423 is introduced into the cell 411 through the L-shaped tube 422 with a cock. In addition, the glass tube 421 is inserted into the tank 420, and the inside of the glass tube 421 is filled with air. This allows the liquid level at the bottom end of the glass tube 421 and in the cell 411 to be the same. That is, while the liquid level of the liquid 423 in the tank 420 is above the bottom end of the glass tube 421, it is possible to keep the liquid level in the cell 411 constant. In this measurement, the height difference between the lower liquid level of the liquid 423 in the tank 420 (i.e., the bottom end of the glass tube 421) and the bottom surface of the swollen gel 414 was set to 4 cm. That is, according to the device 400, the liquid 423 with a constant hydrostatic pressure can be introduced into the cell 411. Since the piston 412 has a hole 415, the liquid 423 flows through the hole 415 and further flows through the swollen gel 414 layer, and flows out to the outside of the cell 411. The container 410 is placed on a stainless steel wire mesh 431 that does not prevent the passage of the liquid 423. Therefore, the liquid 423 flowing out from the cell 411 is finally collected in a collection container 432. The amount of the liquid 423 collected in the collection container 432 can be weighed by a top-plate balance 433.
[0071] The specific method for measuring the gel permeation rate (GPR) is as follows. The following operations are carried out at room temperature (20 to 25° C.).
[0072] (1) A particulate water absorbing agent (0.900 g) is uniformly placed in the cell 411.
[0073] (2) The particulate water absorbing agent is allowed to absorb a 0.90 mass % sodium chloride aqueous solution for 60 minutes without applying pressure to form a swollen gel 414 .
[0074] (3) A piston is placed on the swollen gel 414 and pressurized to 0.3 psi (2.07 kPa).
[0075] (4) While maintaining the hydrostatic pressure at a constant value of 3923 dyne / cm2, liquid 423 is introduced into cell 411 and allowed to pass through the swollen gel 414 layer.
[0076] (5) The amount of liquid 423 passing through the layer of swollen gel 414 is recorded at 5-second intervals for 3 minutes. In other words, the flow rate of liquid 423 passing through the layer of swollen gel 414 is measured. For the measurement, a top-plate balance 433 and a computer (not shown) are used.
[0077] (6) The flow rates 1 minute to 3 minutes after the start of the flow of liquid 423 are averaged to calculate the gel permeation rate (GPR) [g / min].
[0078] In the water absorbent sheet according to one embodiment of the present invention, the GPR of the first particulate water absorbing agent is preferably 5 g / min or more, more preferably 35 g / min or more, and may be 55 g / min or more, 75 g / min or more, 95 g / min or more, or 110 g / min or more. By adopting such an embodiment, the liquid to be absorbed is easily transferred to the second particulate water absorbing agent after being introduced from the first substrate side, and the second particulate water absorbing agent can be effectively utilized, resulting in an excellent result in the specific return amount evaluation. In the water absorbent sheet according to one embodiment of the present invention, there is no particular limit to the upper limit of the GPR of the first particulate water absorbing agent, but from the viewpoint of preventing side leakage, it is preferably 500 g / min or less, 400 g / min or less, 300 g / min or less, 200 g / min or less, 100 g / min or less, or 50 g / min or less.
[0079] In the water absorbent sheet according to one embodiment of the present invention, the GPR of the second particulate water absorbing agent is preferably 1 g / min or more, more preferably 3 g / min or more, and even more preferably 5 g / min or more. By having such a lower limit, gel blocking is suppressed, diffusibility is increased, and liquid is easily absorbed into the absorbent. In the water absorbent sheet according to one embodiment of the present invention, the upper limit of the GPR of the second particulate water absorbing agent is not particularly limited, but is 500 g / min or less, 400 g / min or less, or 300 g / min or less, 200 g / min or less, 100 g / min or less, 50 g / min or less, 30 g / min or less, 25 g / min or less, 20 g / min or less, 15 g / min or less, or 10 g / min or less. By having such an upper limit, the effect of preventing side leakage is improved.
[0080] "Particle shape" In the water absorbent sheet according to one embodiment of the present invention, the particulate water absorbing agent is not limited in its particle shape, and may be, for example, a spherical particulate water absorbing agent (and its granulated product). In a preferred embodiment, the particulate water absorbing agent is preferably in an irregularly pulverized form. Here, the term "irregularly pulverized form" refers to particles in a pulverized form that are not uniform in shape. This is because the irregularly pulverized form can be easily fixed to a substrate compared with spherical particles obtained by reversed-phase suspension polymerization or gas-phase polymerization. The particulate water absorbing agent according to one embodiment of the present invention is preferably a pulverized product obtained in aqueous solution polymerization. On the other hand, in the case where the pulverization step is not performed, typically spherical particles or granulated products of spherical particles obtained by reversed-phase suspension polymerization or droplet polymerization in which a polymerization monomer is sprayed and polymerized are not in an irregularly pulverized form. In the embodiment of the present invention, when the particulate water absorbing agent has an irregularly pulverized form, the shape of the water absorbent sheet is more easily maintained compared with those having a high average roundness (for example, spherical). In the embodiment of the present invention, the average circularity of the particulate water absorbing agent is preferably 0.70 or less, more preferably 0.60 or less, and further preferably 0.55 or less.
[0081] The calculation method of the average circularity is as follows. 100 or more particulate water absorbing agents were randomly selected, and each particulate water absorbing agent was photographed with an electron microscope (VE-9800 manufactured by Keyence Corporation) (magnification: 50 times) to obtain an image of the particulate water absorbing agent, and the perimeter and area of each particle were calculated using the attached image analysis software. The following formula:
[0082]
number
[0083] The circularity of each particle is obtained, and the average of the obtained values is calculated as the average circularity.
[0084] "Particle size" The particle diameter of the particulate water absorbing agent (or particulate water absorbent resin, water absorbent resin particles) according to one embodiment of the present invention is a weight average particle diameter obtained according to a measurement method of "PSD" specified in ERT420.2-02, and may be 150 to 600 μm.
[0085] The method for producing the particulate water absorbing agent is not particularly limited as long as it is a method for producing a water absorbing agent having desired physical properties, and the particulate water absorbing agent can be produced appropriately by taking into consideration, for example, publications described in the examples.
[0086] [2-3. Wrapping Sheet] As described above, the water-absorbent sheet according to one embodiment of the present invention preferably has at least a wrapping sheet disposed on the surface of the first substrate. The wrapping sheet may be disposed on the surface of the first substrate, but it is more preferable that the wrapping sheet be disposed so as to cover the side surface of the first substrate and the side surface of the water-absorbent layer, and it is even more preferable that the wrapping sheet cover the side surface of the first substrate, the side surface of the water-absorbent layer, and the side surface of the second substrate, and cover a part or the whole surface of the second substrate opposite to the side where the liquid to be absorbed is introduced.
[0087] In one embodiment of the present invention, the thickness of the wrapping sheet is preferably 0.001 mm or more, more preferably 0.005 mm or more, even more preferably 0.01 mm or more, and particularly preferably 0.1 mm or more, for example, at 40% RH to 50% RH. The thickness of the wrapping sheet is preferably less than 0.9 mm, 0.8 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, 0.3 mm or less, or 0.2 mm or less, for example, at 40% RH to 50% RH. In one embodiment of the present invention, the bulk density of the wrapping sheet is 1 g / cm 3 It is preferable that the density is 0.5 g / cm or less. 3 More preferably, it is 0.3 g / cm or less. 3 The bulk density of the wrapping sheet is preferably 0.1 g / cm or less. 3 More preferably, it is 0.12 g / cm 3 More preferably, it is 0.13 g / cm 3 In one embodiment of the present invention, the wrapping sheet has a basis weight of 5 to 100 g / m 2 It is preferable that the thickness is 5 to 70 g / m 2 More preferably, it is 10 to 65 g / m 2 It is even more preferable that:
[0088] The thickness, bulk density, and basis weight of the wrapping sheet can be controlled by the material constituting the wrapping sheet, the manufacturing method of the wrapping sheet, etc., and the thickness and bulk density of the wrapping sheet are determined by the balance between these factors.
[0089] "Materials that make up wrapping sheets" The material constituting the wrapping sheet is not particularly limited as long as it can achieve the purpose of providing the wrapping sheet described above, but examples include paper (sanitary paper, such as tissue paper, toilet paper, and towel paper), net, nonwoven fabric, woven fabric, film, etc.
[0090] The nonwoven fabric to be used is not particularly limited, but from the viewpoint of liquid permeability, flexibility, and strength when made into a water-absorbent sheet, examples include nonwoven fabrics made of polyolefin fibers such as polyethylene (PE) and polypropylene (PP), polyester fibers such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polyethylene naphthalate (PEN), polyamide fibers such as nylon, rayon fibers, and other synthetic fibers, and nonwoven fabrics made by mixing cotton, silk, hemp, pulp (cellulose) fibers, etc. Examples of materials for nonwoven fabrics that can be used as wrapping sheets include rayon fibers, polyolefin fibers, polyester fibers, pulp fibers, and fibers mixed with these, and polyolefin fibers are more preferable. These fibers may be hydrophilized.
[0091] The nonwoven fabric that can be used as the wrapping sheet is not particularly limited, and may be obtained by any method such as the air-through method, the air-laid method, the spunbond method, or the spunlace method, but is preferably obtained by the spunbond method (spunbond nonwoven fabric). A wrapping sheet having water repellency is preferable so that the urine absorbed in the absorbent sheet does not seep out of the sheet (so-called backflow) even when weight is applied (pressurized), such as when an infant wearing an absorbent article such as a paper diaper is sitting on the absorbent sheet, and for example, a spunbond nonwoven fabric is preferable. The method for producing a spunbond nonwoven fabric is a method in which continuous long fibers obtained by melting and spinning a raw material resin are directly accumulated to form a fleece. Examples of raw material resins include polyethylene, polypropylene, and polylactic acid.
[0092] According to one embodiment of the present invention, the manufacturing method of the first substrate and the manufacturing method of the second substrate are different from those of the intermediate sheet and the wrapping sheet. By appropriately changing the manufacturing method of each member constituting the water-absorbent sheet in this manner, the desired effect of the present invention can be efficiently achieved. According to one embodiment of the present invention, the first substrate and the second substrate are air-laid nonwoven fabrics, the intermediate sheet is an air-through nonwoven fabric, and the wrapping sheet is a spunbond nonwoven fabric. This embodiment allows the desired effect of the present invention to be efficiently achieved.
[0093] 3. Method for producing water-absorbent sheet A method for producing a water-absorbent sheet according to an embodiment of the present invention includes at least one of the following steps: (1) spraying a first particulate water-absorbing agent on a first substrate, (2) spraying a second particulate water-absorbing agent on a second substrate, (3) spraying the first particulate water-absorbing agent and / or the second particulate water-absorbing agent on an intermediate sheet, (4) spraying a first adhesive on the first substrate, (5) spraying a second adhesive on the second substrate, and (6) spraying at least one of the first adhesive and the second adhesive on the intermediate sheet. As more specific examples of the production method, the following production methods (a) to (e) can be mentioned.
[0094] (a) A first particulate water absorbing agent (and preferably an adhesive) is uniformly sprayed on a first substrate. An intermediate sheet is placed on top of the first particulate water absorbing agent and pressed. Furthermore, a second particulate water absorbing agent (and preferably an adhesive) is uniformly sprayed on the surface of the intermediate sheet that does not face the first particulate water absorbing agent. The intermediate sheet is placed on top of the first particulate water absorbing agent and pressed (preferably under heating conditions that melt the hot melt adhesive or in a state in which the hot melt adhesive is molten).
[0095] (b) A second particulate water absorbing agent is uniformly sprayed on the intermediate sheet. An adhesive is sprayed on the second substrate. Then, the surface of the intermediate sheet on which the second particulate water absorbing agent is sprayed and the surface of the second substrate on which the adhesive is sprayed are pressure-bonded. Next, a first particulate water absorbing agent is uniformly sprayed on the surface of the intermediate sheet opposite to the surface on which the second particulate water absorbing agent is sprayed after pressure-bonding. An adhesive is sprayed on the first substrate. Then, the surface of the intermediate sheet on which the first particulate water absorbing agent is sprayed and the surface of the first substrate on which the adhesive is sprayed are pressure-bonded. The pressure-bonding is preferably performed under heating conditions in which the hot melt adhesive melts, or in a state in which the hot melt adhesive is molten.
[0096] (c) An adhesive is sprayed onto the second substrate. Next, the second particulate water absorbing agent is sprayed evenly onto the adhesive. Next, an intermediate sheet is placed on top of the adhesive and pressed. Next, an adhesive is sprayed onto the surface of the intermediate sheet that does not face the second particulate water absorbing agent. Next, the first particulate water absorbing agent is sprayed evenly onto the adhesive. Next, the first substrate is placed on top of the adhesive and pressed. The above pressing is preferably performed under heating conditions that melt the hot melt adhesive, or while the hot melt adhesive is in a molten state.
[0097] (d) Spray an adhesive on the second substrate. Next, uniformly spray a second particulate water absorbing agent on the adhesive. Next, place an intermediate sheet on the adhesive and press it. Next, uniformly spray a first particulate water absorbing agent on the surface of the intermediate sheet that does not face the second particulate water absorbing agent. Also, spray an adhesive on the first substrate. Then, the surface of the intermediate sheet on which the first particulate water absorbing agent has been sprayed and the surface of the first substrate on which the adhesive has been sprayed are pressed together. The pressing is preferably performed under heating conditions that melt the hot melt adhesive, or in a state in which the hot melt adhesive is molten.
[0098] (e) An intermediate sheet is placed on the first substrate, and a second particulate water absorbing agent is sprayed on the surface of the intermediate sheet. Next, a second adhesive is sprayed on the surface of the second substrate. Then, the surface of the intermediate sheet on which the second particulate water absorbing agent is sprayed and the surface of the second substrate on which the second adhesive is sprayed are placed face to face, and the two are pressed together. Then, the first substrate is peeled off from the intermediate sheet. Next, a first particulate water absorbing agent is sprayed on the surface of the intermediate sheet opposite to the surface on which the second particulate water absorbing agent is placed. Next, a first adhesive is sprayed on the surface of the peeled off first substrate. Then, the first substrate is pressed together so that the surface of the intermediate sheet on which the first particulate water absorbing agent is sprayed and the surface of the intermediate sheet on which the first adhesive is sprayed face each other, to obtain a water absorbent sheet.
[0099] 2 to 4, the method for producing the water-absorbent sheet according to one embodiment of the present invention includes a step of covering the first substrate, the water-absorbent layer, and the second substrate with the wrapping sheet. For example, a first' adhesive is sprayed on the surface of the first substrate on the side where the aqueous liquid is introduced, as necessary, and the wrapping sheet is placed on at least a part of the surface to cover the first substrate, the water-absorbent layer, and the second substrate.
[0100] In the water-absorbent sheet, methods for bonding substrates to each other, a substrate and a particulate water-absorbing agent, or a substrate and a wrapping sheet include a method of bonding them with water, a water-soluble polymer, or various binders dissolved or dispersed in a solvent, or a method of heat-sealing the substrates at the melting point of the material of the substrate itself, but as described above, a method of using an adhesive and pressing the substrates together as necessary is preferred.
[0101] In one embodiment of the present invention, the locations where the adhesive is placed include at least one of the following: the surface of the first substrate facing the second substrate, the surface of the second substrate facing the first substrate, between the wrapping sheet and the first substrate, and between the second substrate and the wrapping sheet.
[0102] In one embodiment of the present invention, the content (non-volatile content, amount used) of the adhesive (solution type) disposed on the surface of the first base material facing the second base material, i.e., the first adhesive (solution type), is preferably 0.0005 to 0.3 times, 0.001 to 0.25 times, 0.01 to 0.2 times, 0.02 to 0.18 times, 0.02 to 0.15 times, or 0.025 to 0.12 times the mass of the first particulate water absorbing agent, in that order. Such an embodiment has a technical effect of efficiently controlling the initial absorption speed within a desired range. In one embodiment of the present invention, when the first adhesive is styrene butadiene rubber, the content (non-volatile content, amount used) is preferably 0.02 to 0.18 times the mass of the first particulate water absorbing agent. In one embodiment of the present invention, when the first adhesive is styrene butadiene rubber and the basis weight of the first base material is 45 g / m 2 In the case where the content (non-volatile content, amount used) is 0.03 times or more, 0.04 times or more, or 0.05 times or more, and preferably 0.1 times or less, 0.08 times or less, 0.075 times or less, or less than 0.07 times, relative to the mass of the first particulate water absorbing agent. In one embodiment of the present invention, the first adhesive is styrene butadiene rubber, and the basis weight of the first base material is 45 g / m 2 In the case where the content (non-volatile content, amount used) is less than 0.07 times, 0.08 times, or 0.09 times or more, and preferably 0.18 times or less, or 0.15 times or less, relative to the mass of the first particulate water absorbing agent. In one embodiment of the present invention, the first adhesive is an ethylene-vinyl acetate copolymer, and the basis weight of the first base material is 45 g / m 2 If it is more than this amount, the content (non-volatile content, amount used) is preferably 0.01 times or more, or 0.015 times or more, and is preferably 0.06 times or less, 0.05 times or less, 0.04 times or less, or 0.03 times or less, relative to the mass of the first particulate water absorbing agent.
[0103] In one embodiment of the present invention, the content (non-volatile content, amount used) of the adhesive (hot melt type) disposed on the surface of the first substrate facing the second substrate, i.e., the first adhesive (hot melt type), is, in order of preference, 0.0005 to 0.3 times, 0.001 to 0.25 times, 0.003 to 0.2 times, 0.004 to 0.2 times, 0.005 to 0.1 times, 0.005 to 0.05 times, 0.005 to 0.03 times, 0.006 to 0.03 times, 0.007 to 0.02 times, and 0.0075 to 0.015 times the mass of the first particulate water absorbing agent. This embodiment has a technical effect of efficiently controlling the initial absorption speed within a desired range.
[0104] Since adjustment of the amount of adhesive can be one of the important factors for adjusting the initial water absorption rate to a specific range, it is important to determine the initial water absorption rate to be in a specific range.
[0105] In one embodiment of the present invention, the content (non-volatile content) of the adhesive (solution type) disposed on the surface of the second substrate facing the first substrate, i.e., the second adhesive (solution type), is preferably 0.0005 to 0.3 times, 0.001 to 0.25 times, 0.01 to 0.2 times, 0.02 to 0.18 times, 0.02 to 0.15 times, or 0.025 to 0.12 times the mass of the second particulate water absorbing agent, in that order. This embodiment has a technical effect of efficiently controlling the initial absorption speed within a desired range.
[0106] In one embodiment of the present invention, the content (non-volatile content, amount used) of the adhesive (hot melt type) disposed on the surface of the second substrate facing the first substrate, i.e., the second adhesive (hot melt type), is preferably 0.0005 to 0.3 times, 0.001 to 0.25 times, 0.003 to 0.2 times, 0.005 to 0.1 times, 0.006 to 0.05 times, or 0.007 to 0.02 times the mass of the second particulate water absorbing agent, in that order. This embodiment has a technical effect of efficiently controlling the initial absorption speed within a desired range.
[0107] In one embodiment of the present invention, the content (non-volatile content, amount used) of the adhesive disposed between the wrapping sheet and the first base material, i.e., the first' adhesive, is preferably 0 to 0.1 times, more preferably 0 to 0.05 times, and even more preferably 0 to 0.03 times, the mass of the first particulate water absorbing agent. This embodiment has the technical effect of efficiently controlling the initial absorption speed within a desired range. Note that, in order to more efficiently achieve the desired effect of the present invention (particularly the effect of reducing the amount of return), it is preferable that the first' adhesive is not disposed.
[0108] Therefore, in one embodiment of the present invention, the wrapping sheet is placed on the surface of the first substrate on the side where the aqueous liquid is introduced, and there is substantially no adhesive between the wrapping sheet and the first substrate. Since adjustment of the amount of adhesive can be one of the important factors for adjusting the initial water absorption rate to a specific range, it is important to determine the initial water absorption rate to be within a specific range.
[0109] In one embodiment of the present invention, the adhesive disposed between the wrapping sheet and the second base material, i.e., the second' adhesive, may be used to the extent that it does not impede the object of the present invention. It is preferable not to use an adhesive. When an adhesive is used, the content (non-volatile content, amount used) of the adhesive is preferably 0 to 0.01 times, more preferably 0 to 0.008 times, and even more preferably 0 to 0.001 times, the mass of the second particulate water absorbing agent. This embodiment has the technical effect of efficiently controlling the initial absorption speed within a desired range.
[0110] In one embodiment of the present invention, the adhesive may be a solution-based adhesive. A solution-based adhesive refers to an adhesive in which the adhesive is dissolved or dispersed in a solvent, and in one embodiment of the present invention, the solvent of the solution-based adhesive contains at least one of hexane selected from isohexane, cyclohexane, and normal hexane, and ether such as dimethyl ether. The structure and composition of the main component of the solution-based adhesive are the same as those of the hot melt-based adhesive described below, and the difference is whether the adhesive is in a pre-dissolved liquid state or a solid state.
[0111] Since the solvent needs to be removed after spraying, it is preferable to use a volatile organic compound with a low boiling point as the solvent for the solution-type adhesive. From the viewpoints of the labor required for removing the solvent, the odor caused by the remaining solvent, and improving the working environment for manufacturing the sheet, a hot-melt type adhesive that does not substantially contain volatile organic compounds is preferable. Usually, when spraying a solution-type adhesive, the solvent concentration is higher than that of a heat-melt type (hot-melt type). This is because a large amount of solvent is used to lower the viscosity of the adhesive resin and make it sprayable. In contrast, the heat-melt type adhesive is sprayed at a high temperature, and the viscosity drop due to the high temperature is large, which results in a lower solvent concentration.
[0112] It is preferable that the adhesive contained in the sheet contains less volatile organic compounds. Specifically, it is most preferable that the volatile organic compounds are below the detection limit. In one embodiment of the present invention, the volatile organic compounds remaining in the adhesive are below the detection limit. The adhesive having a volatile organic compound below the detection limit may be at least one of the first adhesive, the second adhesive, the first' adhesive, and the second' adhesive, but if the volatile organic compound of the first adhesive is below the detection limit, the desired effect of the present invention can be more efficiently achieved. The volatile organic compounds below the detection limit means 1 ppm or less relative to the adhesive. The remaining volatile organic compounds are measured using gas chromatography or the like.
[0113] The form and melting point of the hot melt adhesive can be appropriately selected, and it may be in the form of particles, fibers, a net, a film, or a liquid that is melted by heating.
[0114] The melting temperature or softening point of the hot melt adhesive is preferably 50 to 200° C., or 60 to 180° C. When a particulate adhesive is used, the particle diameter of the particulate adhesive is about 0.01 to 2 times, 0.02 to 1 times, or 0.05 to 0.5 times the average particle diameter of the particulate water absorbing agent.
[0115] The hot melt adhesive used in the present invention can be appropriately selected, but preferably, one or more selected from ethylene-vinyl acetate copolymer adhesives, styrene-based elastomer adhesives, polyolefin-based adhesives, polyester-based adhesives, etc. can be appropriately used. Specifically, polyolefin-based adhesives include polyethylene, polypropylene, atactic polypropylene, and copolymerized polyolefins. Styrene-based elastomer adhesives include styrene-isoprene block copolymers (SIS), styrene-butadiene block copolymers (SBS), styrene-isobutylene block copolymers (SIBS), styrene-ethylene-butylene-styrene block copolymers (SEBS), and styrene butadiene rubber (SBR). Polyester-based adhesives include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and copolymerized polyesters. Ethylene-vinyl acetate copolymer adhesives include ethylene-vinyl acetate copolymer (EVA) adhesives; ethylene-ethyl acrylate copolymers (EEA), and ethylene-butyl acrylate copolymers (EBA). Since the selection of the adhesive can be one of the important factors for adjusting the initial water absorption rate to a specific range, it is important to determine the initial water absorption rate to be within a specific range. In selecting the adhesive, even if the content ratio of the adhesive to the mass of the particulate water absorbing agent is low (even if a small amount is used in the sheet production), the leakage amount and backflow amount of the obtained sheet can be improved, so a hot melt adhesive is preferable to a solution type adhesive. The assumed mechanism of action is that the hot melt adhesive is unlikely to penetrate into the inside of the substrate, so that the hot melt adhesive effectively adheres (distributes unevenly) to the surface of the substrate.
[0116] In the manufacturing method of the water-absorbent sheet according to one embodiment of the present invention, additives (deodorant, fiber, antibacterial agent, gel stabilizer, etc.) may be appropriately blended. The blending amount of the additives is preferably 0 to 50 mass % and more preferably 0 to 10 mass % based on the mass of the particulate water-absorbing agent. In the above manufacturing method, the particulate water-absorbing agent in which the additives are mixed in advance may be used, or the additives may be added during the manufacturing process.
[0117] The dimensions of the water-absorbent sheet to be manufactured can be designed appropriately. Usually, the width is 10 cm to 10 m, and the length is several tens to several thousand meters (in the form of a continuous sheet or roll). The manufactured water-absorbent sheet is cut according to the purpose (the size of the absorbent body to be used) and used.
[0118] In addition to the above-mentioned examples, methods for producing water-absorbent sheets are disclosed, for example, in the following patent documents: WO 2012 / 174026, WO 2013 / 078109, WO 2015 / 041784, WO 2011 / 117187, WO 2012 / 001117, WO 2012 / 024445, WO 2010 / 004894, WO 2010 / 004895, WO 2010 / 076857, WO 2010 / 082373, WO 2010 / 113754, WO 2010 / 143635, WO 2011 / 043256, WO 2011 / 0 86841, WO 2011 / 086842, WO 2011 / 086843, WO 2011 / 086844, WO 2011 / 117997, WO 2011 / 118409, WO 2011 / 136087, WO 2012 / 043546, WO 2013 / 09 No. 9634, International Publication No. 2013 / 099635, JP 2010-115406, JP 2002-345883, JP 6-315501, JP 6-190003, JP 6-190002, JP 6-190001, JP 2-252558, JP 2-252560, and JP 2-252561. The methods of producing water-absorbent sheets disclosed in these documents are also referred to as appropriate.
[0119] <Particularly preferred combinations of constituent elements of the water-absorbent sheet> The embodiments disclosed in this specification describe particularly preferred combinations, of which all combinations must be considered as disclosed (i.e., they serve as the basis for the legality of amendments in each country).
[0120] (Especially preferred embodiment) The CRC of the first particulate water absorbing agent is 30 g / g or more, or 35 g / g or more; the CRC of the second particulate water absorbing agent is 35 g / g or more, 36 g / g or more, particularly 37 g / g or more, and 40 g / g or less, or 39 g / g or less; the surface tension of the particulate water absorbing agent (particularly, the second particulate water absorbing agent) is 60 mN / m or more, particularly 65 mN / m or more; both the first base material and the second base material are produced by an airlaid method using pulp fiber as a main component; the adhesive is applied by hot melt spraying (hot melt spraying (spraying)); and the first' adhesive is substantially absent.
[0121] The CRC of the first particulate water absorbing agent is 30 g / g or more, or 35 g / g or more; the GPR is 35 g / min or more and 200 g / min or less, 100 g / min or less, particularly 50 g / min or less; the CRC of the second particulate water absorbing agent is 35 g / g or more, 36 g / g or more, particularly 37 g / g or more, and 40 g / g or less, or 39 g / g or less; the AAP is 25 g / g or more, 28 g / g or more, or 30 g / g or more; g or less or 32 g / g or less; the GPR is 5 g / min or more, 30 g / min or less, 25 g / min or less, particularly 10 g / min or less; the surface tension is 60 mN / m or more, particularly 65 mN / m or more; both the first substrate and the second substrate are produced by an airlaid method using pulp fiber as a main component; the adhesive application method is hot melt spraying (hot melt spraying (dispersion)); and the first' adhesive is substantially absent.
[0122] In the particularly preferred embodiment, the surface tension of the particulate water absorbing agent (particularly, the second particulate water absorbing agent) is 65 mN / m or more.
[0123] In the particularly preferred embodiment, the first particulate water absorbing agent has a CRC of 35 g / g or more.
[0124] In the particularly preferred embodiment, the CRC of the second particulate water-absorbing agent is 36 g / g or more and 39 g / g or less.
[0125] In the particularly preferred embodiment, substantially no adhesive is present between the wrapping sheet and the first substrate.
[0126] In the particularly preferred embodiment above, the amount of volatile organic compounds remaining in the first adhesive is below the detection limit.
[0127] [4. Absorbent Articles] The absorbent article according to one embodiment of the present invention has a structure in which the water-absorbing sheet described in [2] is sandwiched between a liquid-permeable sheet and a liquid-impermeable sheet. Here, the liquid-permeable sheet is located on the first substrate side, and the liquid-impermeable sheet is located on the second substrate side. Thus, the absorbent article according to one embodiment of the present invention is an absorbent article that is sandwiched between a liquid-permeable sheet and a liquid-impermeable sheet, the liquid-permeable sheet being located on the first substrate side, and the liquid-impermeable sheet being located on the second substrate side. Specific examples of absorbent articles include paper diapers, incontinence pads, sanitary napkins, pet sheets, food drip sheets, and waterproofing agents for power cables.
[0128] As the liquid permeable sheet and the liquid impermeable sheet, any sheet known in the technical field of absorbent articles can be used without any particular limitation. The absorbent article can be manufactured by a known method. EXAMPLES
[0129] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following production examples, measurement conditions, examples and comparative examples, unless otherwise specified, the operations were performed under the conditions of room temperature (25°C) / relative humidity 40-50%RH.
[0130] <Production Example> With reference to the production examples, examples, and comparative examples described in the following patents, particulate water absorbents (1) to (7) of polyacrylic acid (salt) resins were obtained by appropriately adjusting CRC according to the amount of internal cross-linking agent. The physical properties of the obtained particulate water absorbents are shown in Table 1.
[0131] International Publication No. 2014 / 034897 International Publication No. 2017 / 170605 International Publication No. 2016 / 204302 International Publication No. 2014 / 054656 International Publication No. 2015 / 152299 International Publication No. 2018 / 062539 International Publication No. 2012 / 043821.
[0132] 〔Measurement method for physical properties of particulate water absorbent〕 <Weight average particle diameter> The particle diameter of the particulate water absorbent (or particulate water-absorbing resin, water-absorbing resin particles) according to an embodiment of the present invention is the weight average particle diameter obtained according to the measurement method of "PSD" defined in ERT420.2-02. Here, in this specification, the measurement method of the weight average particle diameter is calculated in the same manner as "(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution" described in U.S. Patent No. 7638570 based on the PSD obtained according to the measurement method of "PSD" defined in ERT420.2-02.
[0133] The weight average particle diameter of each particulate water absorbent is shown in Table 1.
[0134] <CRC (Water absorption ratio under no pressure) (ERT441.2-02)> "CRC" is an abbreviation of Centrifuge Retention Capacity, and means the water absorption capacity of a particulate water absorbing agent without pressure (sometimes called "water absorption capacity"). Specifically, it means the water absorption capacity (unit: g / g) after 0.2 g of the particulate water absorbing agent is placed in a nonwoven bag, immersed in a large excess of 0.9 mass % sodium chloride aqueous solution for 30 minutes to allow free swelling, and then drained with a centrifuge (250G) for 3 minutes.
[0135] <Surface tension> In the present invention, the surface tension means the surface tension of an aqueous solution when the particulate water absorbing agent is dispersed in a 0.90 mass % sodium chloride aqueous solution.
[0136] 50 ml of physiological saline adjusted to 20°C is placed in a thoroughly washed 100 ml beaker, and first, the surface tension of the physiological saline is measured using a surface tensiometer (K11 automatic surface tensiometer manufactured by KRUSS). In the present invention, a plate method using a platinum plate is adopted, and the plate is thoroughly washed with deionized water before each measurement, and heated and washed with a gas burner before use. Next, a thoroughly washed 25 mm long fluororesin rotor and 0.5 g of a particulate water absorbing agent are placed in the beaker containing the physiological saline adjusted to 20°C after the surface tension measurement, and the mixture is stirred for 4 minutes under the condition of 500 rpm. After 4 minutes, the stirring is stopped, and after the water-absorbed particulate water absorbing agent settles, the surface tension of the supernatant liquid is measured again by performing the same operation. Here, the surface tension of the particulate water absorbing agent (unit: mN / m) is obtained by the surface tension of the supernatant liquid when the particulate water absorbing agent is dispersed in the physiological saline. The surface tension of each particulate water absorbing agent is shown in Table 1.
[0137] [Production Example of Acrylic Acid] Commercially available acrylic acid (acrylic acid dimer 2000 ppm, acetic acid 500 ppm, propionic acid 500 ppm, p-methoxyphenol 200 ppm )ofThe distilled oil was supplied to the bottom of a high-boiling impurity separation tower having 50 perforated trays without downcomers, and distilled at a reflux ratio of 1 to remove dimers (acrylic acid dimer) composed of maleic acid and acrylic acid. Crystallization was then carried out to obtain acrylic acid (acrylic acid dimer 20 ppm, acetic acid 50 ppm, propionic acid 50 ppm, furfural 1 ppm or less, and protoanemonin 1 ppm or less), and 50 ppm of p-methoxyphenol was added after distillation.
[0138] [Method for producing aqueous sodium acrylate solution] According to Example 9 of US Patent No. 5,210,298, 1,390 g of the above acrylic acid was neutralized with 48% caustic soda at 20 to 40° C. to obtain a 100% neutralized aqueous sodium acrylate solution with a concentration of 37%.
[0139] <Particulate water absorbing agent (1)> 5.03 g of polyethylene glycol diacrylate (average number of moles of ethylene oxide added: 9) was dissolved in 5500 g (monomer concentration: 38.0% by mass) of an aqueous solution of sodium acrylate having a neutralization rate of 75 mol% obtained by mixing the acrylic acid obtained in the above-mentioned acrylic acid production example, the aqueous sodium acrylate solution obtained by the above-mentioned method for producing an aqueous sodium acrylate solution using the acrylic acid, and deionized water to obtain a reaction solution. Next, the reaction solution was supplied to a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10 L and two sigma-type blades, and the system was replaced with nitrogen gas while maintaining the reaction solution at 30°C to remove dissolved oxygen in the reaction solution. Next, 30.68 g of a 10% by mass aqueous solution of sodium persulfate and 37.76 g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the reaction solution, and polymerization started about 1 minute later. 40 minutes after the start of polymerization, a hydrogel polymer was taken out. The obtained hydrogel polymer was fragmented into particles of about 2 to 4 mm. The fragmented hydrogel polymer was spread on a wire net with a mesh size of 50 mesh (300 μm) and dried with hot air at 175° C. for 65 minutes. The dried product was then pulverized using a roll mill, and further classified and mixed using a wire net with a mesh size of 600 μm to obtain an irregularly pulverized water absorbent resin (1-1) having an average particle size of 380 μm.
[0140] 100 parts by mass of the obtained water absorbent resin (1-1) was mixed by spraying with 3.83 parts by mass of a surface cross-linking agent aqueous solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of 1,4-butanediol, 0.5 parts by mass of propylene glycol, and 3.0 parts by mass of water. The mixture was heat-treated for 45 minutes at a heat medium temperature of 210°C using a paddle-type mixing heat treatment machine to obtain a surface cross-linked water absorbent resin (1-2). 100 parts by mass of the obtained surface cross-linked water absorbent resin (1-2) was mixed by spraying with 1.0 part by mass of water, cured at 60°C for 1 hour in a sealed container, and then passed through a sieve with an opening of 710 μm to obtain a water absorbent resin (1-3). 0.3 parts by mass of Aerosil 200 (hydrophilic amorphous silica, manufactured by Nippon Aerosil Co., Ltd.) was added to the water absorbent resin (1-3) and mixed to obtain a water absorbent resin as a particulate water absorbent (1).
[0141] <Particulate water absorbing agent (2)> 3.93 g of polyethylene glycol diacrylate (average number of moles of ethylene oxide added: 9) was dissolved in 5500 g (monomer concentration: 36.0% by mass) of an aqueous solution of sodium acrylate having a neutralization rate of 75 mol% obtained by mixing the acrylic acid obtained in the above-mentioned acrylic acid production example, the aqueous sodium acrylate solution obtained by the above-mentioned method for producing an aqueous sodium acrylate solution using the acrylic acid, and deionized water to obtain a reaction solution. Next, the reaction solution was supplied to a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10 L and two sigma-type blades, and the system was replaced with nitrogen gas while maintaining the reaction solution at 30°C to remove dissolved oxygen in the reaction solution. Next, 29.07 g of a 10% by mass aqueous solution of sodium persulfate and 35.78 g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the reaction solution, and polymerization started about 1 minute later. 40 minutes after the start of polymerization, a hydrogel polymer was taken out. The obtained hydrogel polymer was fragmented into particles of about 2 to 4 mm. The fragmented hydrogel polymer was spread on a wire net with a mesh size of 50 mesh (300 μm) and dried with hot air at 175° C. for 65 minutes. The dried product was then pulverized using a roll mill, and further classified and mixed using a wire net with a mesh size of 600 μm to obtain an irregularly pulverized water absorbent resin (2-1) having an average particle size of 350 μm.
[0142] 100 parts by mass of the obtained water absorbent resin (2-1) was mixed by spraying with 4.03 parts by mass of a surface cross-linking agent aqueous solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 1.0 parts by mass of propylene glycol, and 3.0 parts by mass of water. The mixture was heat-treated for 40 minutes at a heat medium temperature of 100°C using a paddle-type mixing heat treatment machine to obtain a surface cross-linked water absorbent resin (2-2). 100 parts by mass of the obtained surface cross-linked water absorbent resin (2-2) was mixed by spraying with 3.0 parts by mass of water, cured at 60°C for 1 hour in a sealed container, and then passed through a sieve with a mesh size of 710 μm to obtain a water absorbent resin (2-3). 0.3 parts by mass of Aerosil 90G (hydrophilic amorphous silica, manufactured by Nippon Aerosil Co., Ltd.) was added to the water absorbent resin (2-3) and mixed to obtain a water absorbent resin as a particulate water absorbent (2).
[0143] <Particulate water absorbing agent (3)> 5.82g of polyethylene glycol diacrylate (average number of moles of ethylene oxide added: 9) was dissolved in 5500g (monomer concentration: 33.0% by mass) of an aqueous solution of sodium acrylate having a neutralization rate of 75% by mole, which was obtained by mixing the acrylic acid obtained in the above-mentioned acrylic acid production example, the aqueous sodium acrylate solution obtained by the above-mentioned method for producing an aqueous sodium acrylate solution using the acrylic acid, and deionized water, to obtain a reaction solution. Next, the reaction solution was supplied to a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10L and two sigma-type blades, and the system was replaced with nitrogen gas while maintaining the reaction solution at 30°C, thereby removing dissolved oxygen in the reaction solution. Next, 26.65g of a 10% by mass aqueous solution of sodium persulfate and 32.79g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the reaction solution, and polymerization started about 1 minute later. After 40 minutes from the start of polymerization, 181.5 g of water-absorbent resin fine powder of 150 μm or less was added, and the gel was crushed for 10 minutes by rotating the kneader blade at high speed (130 rpm), and then the hydrogel polymer was taken out. The obtained hydrogel polymer was fragmented into particles of about 1 to 2 mm. The fragmented hydrogel polymer was spread on a wire mesh of 50 mesh (opening size 300 μm) and dried with hot air at 175 ° C for 65 minutes. Next, the dried product was pulverized using a roll mill, and further classified and mixed using a wire mesh with an opening of 600 μm to obtain an irregularly crushed water-absorbent resin (3-1) with an average particle size of 350 μm.
[0144] 100 parts by mass of the obtained water absorbent resin (3-1) was mixed by spraying with 3.83 parts by mass of a surface cross-linking agent aqueous solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of 1,4-butanediol, 0.5 parts by mass of propylene glycol, and 3.0 parts by mass of water. The above mixture was heat-treated for 40 minutes at a heat medium temperature of 210°C using a paddle-type mixing heat treatment machine to obtain a surface cross-linked water absorbent resin (3-2). 100 parts by mass of the obtained surface cross-linked water absorbent resin (3-2) was mixed by spraying with 1.0 part by mass of water, cured at 60°C for 1 hour in a sealed container, and then passed through a sieve with an opening of 710 μm to obtain a water absorbent resin (3-3). 0.3 parts by mass of Aerosil 200 (hydrophilic amorphous silica, manufactured by Nippon Aerosil Co., Ltd.) was added to the water absorbent resin (3-3) and mixed to obtain a water absorbent resin as a particulate water absorbent (3).
[0145] <Particulate water absorbing agent (4)> A reaction solution was prepared by dissolving 4.04 g of polyethylene glycol diacrylate (average number of moles of ethylene oxide added: 9) in 5500 g (monomer concentration: 33.0% by mass) of an aqueous solution of sodium acrylate having a neutralization rate of 75 mol% obtained by mixing the acrylic acid obtained in the above-mentioned acrylic acid production example, the aqueous sodium acrylate solution obtained by the above-mentioned method for producing an aqueous sodium acrylate solution using the acrylic acid, and deionized water. Next, the reaction solution was supplied to a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10 L and two sigma-type blades, and the system was replaced with nitrogen gas while maintaining the reaction solution at 30°C to remove dissolved oxygen in the reaction solution. Next, 26.65 g of a 10% by mass aqueous solution of sodium persulfate and 32.79 g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the reaction solution, and polymerization started about 1 minute later. After 40 minutes from the start of polymerization, 181.5 g of water-absorbent resin fine powder of 150 μm or less was added, and the gel was crushed for 10 minutes by rotating the kneader blade at high speed (130 rpm), and then the hydrogel polymer was taken out. The obtained hydrogel polymer was fragmented into particles of about 1 to 2 mm. The fragmented hydrogel polymer was spread on a wire mesh of 50 mesh (opening size 300 μm) and dried with hot air at 175 ° C. for 65 minutes. Next, the dried product was pulverized using a roll mill, and further classified and mixed using a wire mesh with an opening of 600 μm to obtain an irregularly crushed water-absorbent resin (4-1) with an average particle size of 350 μm.
[0146] 100 parts by mass of the obtained water absorbent resin (4-1) was mixed by spraying with 3.83 parts by mass of a surface cross-linking agent aqueous solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of 1,4-butanediol, 0.5 parts by mass of propylene glycol, and 3.0 parts by mass of water. The mixture was heat-treated for 40 minutes at a heat medium temperature of 195°C using a paddle-type mixing heat treatment machine to obtain a surface cross-linked water absorbent resin (4-2). 100 parts by mass of the obtained surface cross-linked water absorbent resin (4-2) was mixed by spraying with 1.0 part by mass of water, cured at 60°C for 1 hour in a sealed container, and then passed through a sieve with an opening of 710 μm to obtain a water absorbent resin (4-3). 0.3 parts by mass of Aerosil 200 (hydrophilic amorphous silica, manufactured by Nippon Aerosil Co., Ltd.) was added to the water absorbent resin (9-3) and mixed to obtain a water absorbent resin as a particulate water absorbent (4).
[0147] <Particulate water absorbent (5)> 5.29g of polyethylene glycol diacrylate (average number of moles of ethylene oxide added: 9) was dissolved in 5500g (monomer concentration: 35.5% by mass) of an aqueous solution of sodium acrylate having a neutralization rate of 75% by mole, which was obtained by mixing the acrylic acid obtained in the above-mentioned acrylic acid production example, the aqueous sodium acrylate solution obtained by the above-mentioned method for producing an aqueous sodium acrylate solution using the acrylic acid, and deionized water, to obtain a reaction solution. Next, the reaction solution was supplied to a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10L and two sigma-type blades, and the system was replaced with nitrogen gas while maintaining the reaction solution at 30°C, thereby removing dissolved oxygen in the reaction solution. Next, 28.66g of a 10% by mass aqueous solution of sodium persulfate and 35.28g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the reaction solution, and polymerization started about 1 minute later. 40 minutes after the start of polymerization, a hydrogel polymer was taken out. The obtained hydrogel polymer was fragmented into particles of about 2 to 4 mm. The fragmented hydrogel polymer was spread on a wire net with a mesh size of 50 mesh (300 μm) and dried with hot air at 175° C. for 65 minutes. The dried product was then pulverized using a roll mill, and further classified and mixed using a wire net with a mesh size of 600 μm to obtain an irregularly pulverized water absorbent resin (5-1) having an average particle size of 350 μm.
[0148] 100 parts by mass of the obtained water absorbent resin (5-1) was mixed by spraying with 4.03 parts by mass of an aqueous surface crosslinking agent solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 1.0 part by mass of propylene glycol, and 3.0 parts by mass of water. The above mixture was heat-treated at a heat medium temperature of 100° C. for 40 minutes using a paddle-type mixer heat treatment machine to obtain a surface-crosslinked water absorbent resin ( 5 100 parts by mass of the obtained surface cross-linked water absorbent resin (5-2) was mixed with 3.0 parts by mass of water by spraying, cured at 60°C for 1 hour in a sealed container, and passed through a sieve with an opening of 710 μm to obtain a water absorbent resin (5-3). 0.3 parts by mass of Aerosil 90G (hydrophilic amorphous silica, manufactured by Nippon Aerosil Co., Ltd.) was added to the water absorbent resin (5-3) and mixed to obtain a water absorbent resin, which was used as a particulate water absorbent (5).
[0149] <Particulate water absorbing agent (6)> 3.27 g of polyethylene glycol diacrylate (average number of moles of ethylene oxide added: 9) was dissolved in 5500 g (monomer concentration: 38.0% by mass) of an aqueous solution of sodium acrylate having a neutralization rate of 75 mol% obtained by mixing the acrylic acid obtained in the above-mentioned acrylic acid production example, the aqueous sodium acrylate solution obtained by the above-mentioned method for producing an aqueous sodium acrylate solution using the acrylic acid, and deionized water to obtain a reaction solution. Next, the reaction solution was supplied to a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10 L and two sigma-type blades, and the system was replaced with nitrogen gas while maintaining the reaction solution at 30°C to remove dissolved oxygen in the reaction solution. Next, 30.68 g of a 10% by mass aqueous solution of sodium persulfate and 37.76 g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the reaction solution, and polymerization started about 1 minute later. 40 minutes after the start of polymerization, a hydrogel polymer was taken out. The obtained hydrogel polymer was fragmented into particles of about 2 to 4 mm. The fragmented hydrogel polymer was spread on a wire net with a mesh size of 50 mesh (300 μm) and dried with hot air at 175° C. for 65 minutes. The dried product was then pulverized using a roll mill, and further classified and mixed using a wire net with a mesh size of 600 μm to obtain an irregularly pulverized water absorbent resin (6-1) having an average particle size of 350 μm.
[0150] 100 parts by mass of the obtained water absorbent resin (6-1) was mixed by spraying with 3.83 parts by mass of a surface cross-linking agent aqueous solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of 1,4-butanediol, 0.5 parts by mass of propylene glycol, and 3.0 parts by mass of water. The mixture was heat-treated for 45 minutes at a heat medium temperature of 195°C using a paddle-type mixing heat treatment machine to obtain a surface cross-linked water absorbent resin (6-2). 100 parts by mass of the obtained surface cross-linked water absorbent resin (6-2) was mixed by spraying with 1.0 part by mass of water, cured at 60°C for 1 hour in a sealed container, and then passed through a sieve with an opening of 710 μm to obtain a water absorbent resin (6-3). 0.3 parts by mass of Aerosil 200 (hydrophilic amorphous silica, manufactured by Nippon Aerosil Co., Ltd.) was added to the water absorbent resin (6-3) and mixed to obtain a water absorbent resin as a particulate water absorbent (6).
[0151] <Particulate water absorbing agent (7)> [Removal of water-absorbent resin from commercially available disposable diapers] A water-absorbent resin was taken out from a commercially available disposable diaper (NEW Doremi Pants (L size, Lot No. 8-1A042 1489), manufactured by OJI, purchased in 2001) that had been stored in a humidity-controlled environment. When taking out the water-absorbent resin, only the water-absorbent resin was taken out so as not to be mixed with cotton-like pulp or the like. The water-absorbent resin taken out had a particle shape obtained by granulating spherical particles. This water-absorbent resin was designated as a particulate water-absorbing agent (7). The physical properties of the particulate water-absorbing agent (7) are shown in Table 1.
[0152] [Example] In the following Examples and Comparative Examples, unless otherwise specified, operations were carried out under conditions of room temperature (25° C.) and relative humidity of 40 to 50% RH.
[0153] [Example 1] Nonwoven fabric A (corresponding to the first base material, mainly composed of pulp fiber, thickness 0.4 mm, produced by the airlaid method, basis weight: 47 g / m) was cut to a length of 10 cm and a width of 40 cm at room temperature. 2), an air-through nonwoven fabric C (corresponding to an intermediate sheet) having a thickness of 1.4 mm and mainly composed of olefin is placed on top of the nonwoven fabric C, and 6 g (spreading amount: 150 g / m) of a particulate water absorbing agent (2) (corresponding to a second particulate water absorbing agent) is applied to the surface of the nonwoven fabric C. 2 The reason why the particulate water absorbing agent (2) was sprayed on the surface of the nonwoven fabric C in a state where the nonwoven fabric A was placed under the air-through nonwoven fabric C is that the particulate water absorbing agent (2) which can pass through the nonwoven fabric C without being captured by the nonwoven fabric C is received by the nonwoven fabric A.
[0154] Next, nonwoven fabric A (different from the above) was cut to a length of 10 cm and a width of 40 cm (corresponding to the second substrate, mainly composed of pulp fiber, thickness 0.4 mm, produced by the airlaid method, basis weight: 47 g / m 2 0.5 g of an adhesive (solvent-type adhesive) (corresponding to the second adhesive) (Spray Glue 77, manufactured by 3M Japan Ltd.) containing a solvent whose main components were a mixture of isohexane, cyclohexane, and normal hexane, liquefied petroleum gas, dimethyl ether, and styrene-butadiene rubber was evenly sprayed on the surface of the board (amount sprayed: 12.5 g / m). 2 ).
[0155] Thereafter, the surface of nonwoven fabric C on which the particulate water-absorbing agent was sprayed and the surface of nonwoven fabric A on which the adhesive was sprayed were placed face-to-face (in contact with each other) and pressed together. Thereafter, the nonwoven fabrics were turned upside down so that the bottom nonwoven fabric A (corresponding to the first substrate) was on top, and the upper nonwoven fabric A (corresponding to the first substrate) that was not pressed together was peeled off.
[0156] Next, 6 g (amount of application: 150 g / m) of the particulate water absorbing agent (1) (corresponding to the first particulate water absorbing agent) was applied to the surface of the nonwoven fabric C on the side not facing the particulate water absorbing agent (2). 2 ) was distributed evenly.
[0157] Next, 0.5 g of an adhesive (corresponding to the first adhesive) containing styrene-butadiene rubber (Spray Glue 77, manufactured by 3M Japan Ltd.) was evenly sprayed onto the surface of the nonwoven fabric A (corresponding to the first substrate) that had been peeled off earlier (spray amount: 12.5 g / m 2Thereafter, the surface of the nonwoven fabric C on which the particulate water-absorbing agent (1) was sprayed and the surface of the nonwoven fabric A on which the adhesive was sprayed were placed face to face (contacted), and pressed together to obtain a water-absorbent sheet Z.
[0158] Finally, 0.1 g of an adhesive containing styrene-butadiene rubber (corresponding to the first adhesive) (Spray Glue 77, manufactured by 3M Japan Ltd.) was uniformly sprayed (amount sprayed: 2.5 g / m) on the nonwoven fabric A of the water-absorbent sheet Z (the surface of the nonwoven fabric A opposite to the surface on which the particulate water-absorbing agent (1) was sprayed). 2 ), and then cut to a size of 24 cm length and 40 cm width, wrapped in a 0.1 mm thick spunbond nonwoven fabric (wrapping sheet) mainly composed of olefin, and pressed to obtain a water-absorbent sheet (1).
[0159] [Examples 2 to 9, Comparative Examples 1 to 10] A water-absorbent sheet was produced in the same manner as in Example 1, except that the first particulate water-absorbing agent, the second particulate water-absorbing agent, the first substrate, the type of adhesive, the amount of the first adhesive, the amount of the second adhesive, and the amount of the first' adhesive were changed as shown in Table 1.
[0160] [Example 10] A water-absorbent sheet (10) was obtained in the same manner as in Example 1, except that a hot melt adhesive (adhesive containing styrene-butadiene rubber) heated to 140°C was applied using a glue applicator (Nordson Alta Blue Touch) instead of the spray glue 77.
[0161] [Examples 11 and 12, Comparative Example 11] A water-absorbent sheet was produced in the same manner as in Example 10, except that the first particulate water-absorbing agent, the second particulate water-absorbing agent, the first substrate, the type of adhesive, the amount of the first adhesive, the amount of the second adhesive, and the amount of the first' adhesive were changed as shown in Table 1.
[0162] [Method of evaluating water-absorbent sheets] In the following evaluation methods, unless otherwise specified, the operations were carried out under the conditions of room temperature (25° C.) and relative humidity of 40 to 50% RH.
[0163] <Initial absorption rate> A funnel (flow rate 7ml / min) was placed 1.5cm above the absorbent, and 1.00g of physiological saline (0.9% sodium chloride solution) containing 20ppm of Blue No. 1 Reagent was poured into the funnel, after which the time it took for the absorbent to absorb the liquid was measured. In other words, the initial absorption rate (seconds) is the time displayed when a stopwatch is started immediately after pouring in the liquid and stopped when the absorbent has completely absorbed the liquid. N was 5 times, and the arithmetic average of the results was taken as the initial absorption rate.
[0164] <Return amount (specific return amount evaluation)> As shown in Fig. 6, the absorbent sheet 40, which was made to be 10 cm long and 40 cm wide, was wrapped in a liquid-impermeable sheet 21, which was 14 cm long and 40 cm wide, so that an opening was formed at the top. The absorbent sheet 40 wrapped in the liquid-impermeable sheet 21 was placed on a flat surface, and a liquid injection tube 41 (Fig. 7) was placed on top of it in the center of the absorbent sheet 40, as shown in Fig. 8. In this state, 80 g of a 0.9 wt % sodium chloride aqueous solution at 23°C was poured into the liquid injection tube 41 using a funnel 42 capable of pouring liquid at a flow rate of 7 ml / sec (Fig. 9). In this case, the liquid was poured into the absorbent sheet 40 exposed from the liquid-impermeable sheet 21. Ten minutes after the liquid was poured in, twenty pieces of filter paper 43 (type No. 2, manufactured by ADVANTEC; circular, 110 mm diameter) whose weight had been measured in advance were placed in the center of the absorbent sheet 40, and a circular weight 44 (1200 g) with a diameter of 100 mm was further placed on top and held for one minute. After one minute, the weight 44 was removed, and the first amount of backflow (g) was measured from the weight increase of the filter paper 43. One minute after the weight 44 was removed, the same procedure (pouring in the liquid → 10 minutes after pouring, placing the filter paper 43 and weight 44 (1200 g) and holding for one minute → holding for one minute → removing the weight, measuring the amount of backflow) was repeated, and the second amount of backflow (g) and the third amount of backflow (g) were measured. The total of the measured amounts of backflow from the first to third times are shown in Table 2.
[0165] <Leak amount (diagonal evaluation) (specific leak amount evaluation)> The leakage rate was measured using the device shown in FIG.
[0166] In outline, it is a mechanism that uses a commercially available experimental stand 60 and pipes 61 to tilt and fix an acrylic plate 63, then pours saline solution vertically from above using a funnel onto an absorbent sheet fixed on the plate, and measures the amount of leakage. The detailed specifications are shown below.
[0167] The acrylic plate 63 had a length of 400 mm in the direction of the inclined surface, and was fixed by the stand 60 so that the angle it made with the horizontal was 20°. The acrylic plate 63 had a width of 200 mm and a thickness of 3 mm. The surface of the acrylic plate 63 was smooth, so liquid did not accumulate or be absorbed by the plate. Using the stand 60, a funnel 64 was fixed vertically above the inclined acrylic plate 63. The funnel 64 used was one that could input liquid at a rate of 7 mL / sec.
[0168] A metal tray 65 was placed under the acrylic plate 63 to receive all the test liquid that leaked out and record its mass to an accuracy of 0.1 g.
[0169] The inclined leakage test using such an apparatus was carried out as follows: As shown in FIG.
[0170] A mark was made 1.5 cm below the top end of the water-absorbent sheet, and the inlet of the funnel was fixed vertically above the mark at a distance of 15±2 mm.
[0171] 20 mL of saline was poured into the dropping funnel 64 at once. The amount of test liquid that flowed down the inclined acrylic plate 63 without being absorbed by the absorbent sheet 66 and entered the metal tray 65 was measured and recorded as the first leakage amount (mL) in the surface direction. After 10 minutes, 20 mL of saline was poured in the same way and the second leakage amount was measured, and after another 10 minutes, 20 mL of saline was poured in the same way and the third leakage amount was measured. The leakage amount in the table is the total value of the first to third leakage amounts.
[0172] [Table 1-1]
[0173] [Table 1-2]
[0174] <Application method> Solvent dissolving spray: X, Heat melting spray: Y.
[0175] <First substrate> A: Nonwoven fabric A (mainly composed of pulp fiber. Thickness: 0.4 mm. Made by the airlaid method. Basis weight: 47 g / m 2 ), B: Nonwoven fabric B (mainly made of pulp fiber. Thickness: 0.4 mm. Made by the airlaid method. Weight: 42 g / m 2 )).
[0176] <Adhesive> SBR: Styrene butadiene rubber, EVA: Ethylene-vinyl acetate copolymer.
[0177] <Measurement of non-volatile content of solvent-based adhesive> The weight of the nonwoven fabric was measured immediately after spraying the solution-based adhesive (within 10 seconds after spraying), and the difference in weight from the nonwoven fabric before spraying was calculated to measure the amount of solution-based adhesive sprayed. Since the proportion of nonvolatile content in the amount sprayed measured beforehand was 81.16% by mass (the nonvolatile content was measured from the remaining amount at 90°C for 1 hour), the nonvolatile content of the sprayed solution-based adhesive was calculated by multiplying the sprayed weight of the solution-based adhesive by 81.16% by mass.
[0178] <Measurement of non-volatile content of hot melt adhesive> The weight of the nonwoven fabric was measured immediately after spraying the hot melt adhesive (within 10 seconds after spraying), and the difference in weight from the nonwoven fabric before spraying was calculated to measure the amount of hot melt adhesive sprayed. Since the ratio of nonvolatile content to the amount sprayed was essentially 100% by mass (the nonvolatile content was measured from the remaining amount at 90°C for 1 hour), the nonvolatile content of the sprayed hot melt adhesive was taken as the measured amount of hot melt adhesive sprayed.
[0179] The residual solvent in the solvent-based adhesive (volatile organic compounds remaining in the adhesive) was more than 1 ppm in the adhesive.
[0180] [Evaluation Rank] A is the best, E is the worst (not practical). (Leakage amount) A: Less than 2.5 B: 2.5 or more and less than 3 C: 3 or more but less than 4 D: 4 or more but less than 5 E: 5 or above.
[0181] (Return amount) A: Less than 4.5 B: 4.5 or more and less than 5 C: 5 or more and less than 5.5 D: 5.5 or more and less than 6 E:6 or above. [Explanation of symbols]
[0182] 40 Water-absorbent sheet 11 first substrate, 12 water absorption layer, 13 second substrate; 14 Particulate water absorbing agent, 14a a first particulate water absorbing agent; 14b a second particulate water absorbing agent; 17 adhesive, 17a first adhesive, 17b second adhesive; 17c 1st adhesive, 17d 2nd' adhesive, 18 wrapping sheets, 21 Liquid impermeable sheet, 41 Liquid injection tube, 42 funnel, 60 stands, 61 Pipes, 63 Acrylic plate, 64 funnel, 65 Metal Tray, 400 devices, 410 containers, 411 cells, 412 piston, 413a, 413b wire mesh, 414 Swollen gel (particulate water absorbent absorbed), 415 holes, 420 tank, 421 Glass tube, 422 Cock Glass Tube with L-shaped Tube, 423 liquid, 431 Stainless steel wire mesh, 432 Collection vessels, 433 Top plate balance.
Claims
1. A first substrate; A second substrate; a water-absorbing layer located between the first substrate and the second substrate; A water-absorbent sheet having The water absorbing layer includes a particulate water absorbing agent, The first substrate is located on a side where an aqueous liquid is introduced, The initial absorption speed is adjusted to 2.2 to 3.0 seconds. the particulate water absorbing agent comprises a first particulate water absorbing agent localized on a surface side of the first base material facing the second base material, and a second particulate water absorbing agent localized on a surface side of the second base material facing the first base material, A water-absorbent sheet, comprising: a first adhesive disposed on a surface of the first substrate facing the second substrate; the first adhesive being a hot-melt type; and a content (non-volatile content) of the first adhesive being 0.005 to 0.05 times the mass of the first particulate water-absorbing agent.
2. The water-absorbent sheet according to claim 1 , wherein the first particulate water-absorbing agent has a CRC of 30 g / g or more.
3. The water-absorbent sheet according to claim 2 , wherein the first particulate water-absorbing agent has a CRC of 35 g / g or more.
4. The water-absorbent sheet according to any one of claims 1 to 3, wherein the second particulate water-absorbing agent has a surface tension of 60 mN / m or more.
5. The water-absorbent sheet according to any one of claims 1 to 4, wherein the first adhesive contains a volatile organic compound at or below a detection limit.
6. The water-absorbent sheet according to any one of claims 1 to 5, which has a wrapping sheet.
7. The water-absorbent sheet according to claim 6, wherein the wrapping sheet is placed on the surface of the first substrate on which an aqueous liquid is introduced, and there is substantially no adhesive between the wrapping sheet and the first substrate.
8. A water-absorbent article comprising the water-absorbent sheet according to any one of claims 1 to 7 sandwiched between a liquid-permeable sheet and a liquid-impermeable sheet, the liquid-permeable sheet being positioned on the first substrate side and the liquid-impermeable sheet being positioned on the second substrate side.
Citation Information
Patent Citations
Particulate water absorbing agent with water-absorbing resin as main component
JP2006055833A
Absorbent article
JP2010194254A
Disposable wearable article and package structure thereof
JP2017099860A
Water absorbent sheet
WO2010143635A1
Water absorbent sheet
WO2011043256A1