Method for producing recycled perfluoro (co)polymer and method for producing recycled material

The heat treatment of crosslinked perfluoro(co)polymers in an inert gas atmosphere regenerates crosslinking sites, addressing the challenges of recycling these materials by maintaining physical properties and enabling their use in semiconductor manufacturing equipment.

JP7577287B1Active Publication Date: 2024-11-05VALQUA LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024054593
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-05
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Existing methods for recycling crosslinked fluoroelastomers, such as those used in semiconductor manufacturing, face challenges in regenerating crosslinking sites effectively while minimizing mass loss and maintaining the material's physical properties, as they often result in decomposition and insufficient devulcanization.

Method used

A method involving heat treatment of crosslinked perfluoro(co)polymers in an inert gas atmosphere regenerates crosslinking sites, using nitrogen, argon, or helium gas to suppress decomposition and maintain the material's integrity, followed by crosslinking with additives to form recycled materials with comparable properties to virgin products.

Benefits of technology

The method allows for the regeneration of crosslinking sites in crosslinked perfluoro(co)polymers with minimal mass loss, enabling the production of recycled materials with hardness, tensile strength, elongation, and plasma resistance comparable to virgin products, suitable for use in sealing materials for semiconductor manufacturing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577287000001
    Figure 0007577287000001
  • Figure 0007577287000002
    Figure 0007577287000002
  • Figure 0007577287000003
    Figure 0007577287000003
Patent Text Reader

Abstract

Disclosed is a method for producing a regenerated perfluoro(co)polymer by regenerating crosslinking sites of a crosslinked perfluoro(co)polymer, which can sufficiently regenerate the crosslinking sites in a simple manner while suppressing the mass loss of the perfluoro(co)polymer when the crosslinking sites are regenerated. [Solution] A method for producing a regenerated perfluoro(co)polymer includes a step of heat-treating a crosslinked perfluoro(co)polymer formed by crosslinking a perfluoro(co)polymer having crosslinking sites under an inert gas atmosphere to regenerate the crosslinking sites.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a recycled perfluoro (co)polymer and a method for producing a recycled material. [Background technology]

[0002] 2. Description of the Related Art Conventionally, sealing materials have been used widely for various applications. Among these applications, an example of an application of a sealing material that places the greatest load on the sealing material is a sealing material used in semiconductor manufacturing equipment, etc.

[0003] Cross-linkable fluoroelastomers such as fluoroelastomers (FKM) and perfluoroelastomers (FFKM) are used as such sealing materials because they have excellent plasma resistance and radical resistance. FFKM is used particularly in cases where high temperatures or harsh chemicals are used.

[0004] The above-mentioned sealing material made of a crosslinkable fluoroelastomer is usually used as a sealing material by using an elastomer composition obtained by blending the crosslinkable fluoroelastomer with additives such as a crosslinking agent and a crosslinking aid, and molding and crosslinking the elastomer composition.

[0005] As with general molded products, the sealing material may require disposal of molding waste (burrs), defective products, used molded products, etc. However, crosslinked fluoroelastomers have been disposed of by landfilling or the like because their excellent properties hinder chemical treatment, etc., and they generate corrosive decomposition products when burned, making thermal recycling difficult.

[0006] However, in recent years, with increasing awareness of environmental protection through the reduction of landfill waste and the effective use of resources, there is a demand for the development of a method for reusing crosslinked fluoroelastomers that have conventionally been discarded.

[0007] As a method for reusing such crosslinked fluoroelastomers, for example, Patent Document 1 discloses a method in which a crosslinked fluoropolymer is decrosslinked in a supercritical fluid or subcritical fluid of a compound having active hydrogen. Moreover, Patent Document 2 discloses a method of heat treating vulcanized fluororubber in air. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2007-63334 A [Patent Document 2] Japanese Patent Application Publication No. 61-69805 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the method described in Patent Document 1, which uses a supercritical fluid or a subcritical fluid, is not easy to process and cannot be carried out simply and conveniently, and therefore there is room for improvement. Furthermore, as a result of intensive research by the present inventors, it has been found that the method described in Patent Document 2 does not sufficiently devulcanize the vulcanized fluororubber (regenerate crosslinking sites), and that the heat treatment causes decomposition of the vulcanized fluororubber, resulting in a large mass loss rate of the fluororubber before and after the heat treatment.

[0010] The present invention has been made in consideration of the above, and is a method for producing a regenerated perfluoro(co)polymer that regenerates crosslinking sites of a crosslinked crosslinked perfluoro(co)polymer, and an object of the present invention is to provide a method for producing a regenerated perfluoro(co)polymer that can sufficiently regenerate crosslinking sites in a simple manner while suppressing mass loss of the perfluoro(co)polymer when regenerating the crosslinking sites. [Means for solving the problem]

[0011] As a result of intensive research by the present inventors to solve the above problems, they found that the above problems can be solved by the following configuration examples, and completed the present invention. A configuration example of the present invention is as follows.

[0012] [1] A method for producing a regenerated perfluoro(co)polymer, comprising a step of heat-treating a crosslinked perfluoro(co)polymer obtained by crosslinking a perfluoro(co)polymer having crosslinking sites under an inert gas atmosphere to regenerate the crosslinking sites.

[0013] [2] The method for producing a recycled perfluoro (co)polymer according to [1], wherein the crosslinking site is a nitrile group.

[0014] [3] The method for producing a recycled perfluoro(co)polymer according to [1] or [2], wherein the inert gas is at least one selected from nitrogen gas, argon gas and helium gas.

[0015] [4] The method for producing a recycled perfluoro(co)polymer according to any one of [1] to [3], wherein the perfluoro(co)polymer having a crosslinking site is a (co)polymer that does not contain a carbon-hydrogen bond in the main chain of the (co)polymer.

[0016] [5] A method for producing a recycled material, comprising a step of crosslinking a recycled material-forming material containing a recycled perfluoro(co)polymer obtained by the method for producing a recycled perfluoro(co)polymer described in any one of [1] to [4].

[0017] [6] The method for producing a recycled material described in [5], wherein the recycled material-forming material further contains a crosslinking agent.

[0018] [7] The method for producing a recycled material according to [5] or [6], wherein the recycled material-forming material further contains an uncrosslinked perfluoro (co)polymer.

[0019] [8] The method for producing a recycled material described in [7], wherein the content of the recycled perfluoro(co)polymer in the recycled material-forming material is 0.5 parts by mass or more per 100 parts by mass of uncrosslinked perfluoro(co)polymer.

[0020] [9] The method for producing a recycled material according to any one of [5] to [8], wherein the recycled material is a sealing material. Effect of the Invention

[0021] According to the present invention, when regenerating the crosslinking sites of a crosslinked crosslinked perfluoro(co)polymer, the crosslinking sites of the crosslinked perfluoro(co)polymer can be sufficiently regenerated by a simple method while suppressing the mass loss of the perfluoro(co)polymer when regenerating the crosslinking sites. In this way, the crosslinking sites of the crosslinked perfluoro(co)polymer can be sufficiently regenerated while suppressing mass loss, so that even when the resulting regenerated perfluoro(co)polymer is used, a molded product (regenerated material) having physical properties (hardness, tensile strength, elongation at break, compression set, and plasma resistance) comparable to those of a virgin product (uncrosslinked perfluoro(co)polymer) can be formed. Therefore, the recycled material can be suitably used as a sealing material for semiconductor manufacturing equipment, a sealing material for plasma processing equipment, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] <Production method of recycled perfluoro (co)polymer> The manufacturing method of the recycled perfluoro(co)polymer (hereinafter also referred to as "the recycled product") according to the present invention (hereinafter also referred to as "the manufacturing method of the recycled product") includes a step of heat-treating a crosslinked perfluoro(co)polymer (hereinafter also referred to as "the regenerated product") in which a perfluoro(co)polymer having crosslinking sites is crosslinked, under an inert gas atmosphere, thereby regenerating the crosslinking sites.

[0023] Whether or not crosslinking sites have been regenerated in the regenerated product can be determined, for example, by using FT-IR to measure the amount of crosslinking sites in the regenerated product and the amount of crosslinking sites in the obtained regenerated product. The method for producing the recycled product is preferably such that, when the content of crosslinking sites in the regenerated product is taken as 100%, the content of crosslinking sites in the obtained recycled product is preferably 150% or more, more preferably 200% or more, because the obtained recycled product can be used to easily form a recycled material having desired physical properties. The content of the crosslinking sites can be measured using FT-IR, specifically, by the method described in the examples below.

[0024] Furthermore, since the method for producing the present recycled product can easily form a recycled material having desired physical properties using the obtained recycled product, it is desirable that the mass reduction rate due to the heat treatment, specifically the mass reduction rate represented by the following formula (1), is preferably 2% or less, more preferably 1% or less. Mass reduction rate (%) = [(mass of recycled product - mass of main recycled product) / mass of recycled product] × 100 ···(1)

[0025] <Recycled products> The regenerated product is a crosslinked perfluoro(co)polymer obtained by crosslinking a perfluoro(co)polymer having crosslinking sites (hereinafter also referred to as "uncrosslinked perfluoro(co)polymer"). Examples of the crosslinked perfluoro(co)polymer include (unused) molded products such as sealing materials formed using conventional uncrosslinked perfluoro(co)polymers (virgin products), scraps (burrs) or defective products generated during the production of such molded products, and crosslinked perfluoro(co)polymers contained in used molded products. The used molded articles include not only used molded articles used in semiconductor manufacturing equipment, but also used molded articles used in chemical plants, various industrial equipment, and the like. In the method for producing the recycled product, the raw material to be subjected to the heat treatment may be the crosslinked perfluoro (co)polymer itself, the (unused) molded body, the scraps (burrs) or defective products, or the used molded body.

[0026] The crosslinked perfluoro(co)polymer in the regenerated product is a crosslinked product obtained by crosslinking the following uncrosslinked perfluoro(co)polymer (virgin product) by a conventionally known method. The conventionally known method includes crosslinking using a crosslinking agent, and the crosslinking agent may be appropriately selected according to the uncrosslinked perfluoro (co)polymer used, and may include, for example, peroxide-based crosslinking agents, bisphenol-based crosslinking agents, triazine-based crosslinking agents, oxazole-based crosslinking agents, imidazole-based crosslinking agents, thiazole-based crosslinking agents, amidoxime-based crosslinking agents, and amidrazone-based crosslinking agents. In other words, the regenerated product may include a crosslinked perfluoro (co)polymer having at least one crosslinking structure selected from the crosslinking structures derived from these crosslinking agents and intermediate structures (e.g., amidine structures when forming oxazole structures) when forming these crosslinking structures. The degree of crosslinking in the recycled product is not particularly limited, and it is sufficient that the degree of crosslinking is the same as that when a molding such as a sealing material is formed.

[0027] [Uncrosslinked perfluoro (co)polymer] The uncrosslinked perfluoro(co)polymer is a perfluoro(co)polymer having crosslinking sites before crosslinking, and can also be called a "virgin product." The uncrosslinked perfluoro (co)polymer is preferably a perfluoroelastomer (FFKM). The FFKM is not particularly limited, but is preferably a polymer that does not contain hydrogen atoms (carbon-hydrogen bonds) in the polymer main chain (excluding the terminals). Specific examples include tetrafluoroethylene (TFE)-perfluorovinyl ether copolymers having crosslinking sites, and copolymers that contain structural units derived from TFE and structural units derived from perfluorovinyl ether and, if necessary, further contain structural units derived from a crosslinking site-containing monomer are preferred.

[0028] Suitable examples of the perfluorovinyl ether include perfluoro(alkyl vinyl ether) and perfluoro(alkoxyalkyl vinyl ether).

[0029] The perfluoro(alkyl vinyl ether) may be a compound in which the alkyl group has, for example, 1 to 10 carbon atoms. Specific examples include perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether), and perfluoro(propyl vinyl ether), and is preferably perfluoro(methyl vinyl ether).

[0030] The perfluoro(alkoxyalkyl vinyl ether) may be, for example, a compound having 3 to 15 carbon atoms in the group bonded to the vinyl ether group (CF2=CFO-). Specific examples include the following compounds. CF2=CFOCF2CF(CF3)OC n F 2n+1 CF2 = CFO(CF2)3OC n F 2n+1 CF2 = CFOCF2CF(CF3)O(CF2O) m C n F 2n+1 CF2 = CFO(CF2)2OC n F 2n+1 In these formulas, n is, independently, for example, 1 to 5, and m is, for example, 1 to 3.

[0031] The crosslinking site means a site capable of crosslinking reaction, and examples thereof include a nitrile group, a halogen atom (e.g., I, Br), and a perfluorophenyl group. Among these, a nitrile group is preferred in terms of better exerting the effects of the present invention.

[0032] Examples of crosslinking site monomers having a nitrile group as a crosslinking site include nitrile group-containing perfluorovinyl ethers, and specific examples thereof include the following compounds. CF2 = CFO(CF2) n OCF(CF3)CN (n is, for example, 2 to 4) CF2 = CFO(CF2) n CN (n is, for example, 2 to 12) CF2 = CFO[CF2CF(CF3)O] m (CF2) n CN (n is, for example, 1 to 4, m is, for example, 1 to 5) CF2 = CFO[CF2CF(CF3)O] n CF2CF(CF3)CN (n is, for example, 0 to 4) CF2=CF(CF2) n CN (n is, for example, an integer from 1 to 8) CF2=CFCF2(OCF2) n CN (n is an integer from 0 to 5, for example) CF2=CFCF2(OCF(CF3)CF2) m -CN (m is, for example, an integer from 0 to 5, and n is, for example, an integer from 0 to 5) CF2=CF(OCF2CF(CF3)) m O(CF2) n -CN (m is, for example, an integer of 0 to 5, and n is, for example, an integer of 1 to 8) CF2=CF(OCF2CF(CF3)) m -CN (m is, for example, an integer of 1 to 5) CF2 = CFOCF2 (CF(CF3)OCF2) n CF(-CN)CF3 (n is, for example, an integer of 1 to 4) CF2 = CFO(CF2) n OCF(CF3)-CN (n is, for example, an integer of 2 to 5) CF2=CF(OCF2CF(CF3)) n OCF2CF(CF3)-CN (n is, for example, an integer of 1 to 2) CF2 = CFO(CF2CF(CF3)O) m (CF2) n -CN (m is, for example, an integer of 0 to 5, and n is, for example, an integer of 1 to 3) CF2 = CFO(CF2CF(CF3)O) m CF2CF(CF3)-CN (m is an integer equal to or greater than 0) CF2 = CFOCF(CF3)CF2O(CF2) n -CN (n is an integer equal to or greater than 1) CF2=CFOCF2OCF2CF(CF3)OCF2-CN

[0033] Examples of the crosslinking site-containing monomer having a halogen atom as a crosslinking site include halogen group-containing perfluorovinyl ether, specifically, compounds in which the nitrile group in the specific example of the nitrile group-containing perfluorovinyl ether described above is replaced with a halogen atom, etc. Examples of the crosslinking site-containing monomer having a halogen atom include compounds described in International Publication No. 2009 / 119409, JP-A No. 2002-97329, and JP-A No. 2008-56739.

[0034] In FFKM, the content of constituent units derived from TFE is preferably 50.0 to 79.9 mol %, the content of constituent units derived from perfluorovinyl ether is preferably 20.0 to 46.9 mol %, and the content of constituent units derived from crosslinking site-containing monomers is preferably 0.1 to 2.0 mol %.

[0035] <Heat treatment conditions, etc.> The heat treatment in the method for producing the regenerated product is characterized by being carried out in an inert gas atmosphere. By carrying out the heat treatment under an inert gas atmosphere, decomposition of the regenerated product can be suppressed when obtaining a regenerated product from the regenerated product, mass loss can be suppressed, and a regenerated product with a large amount of regenerated crosslinking sites can be easily obtained.

[0036] Specific examples of the inert gas include nitrogen gas, argon gas, and helium gas, and among these, nitrogen gas is preferable. The inert gas may be used alone or in combination of two or more kinds. In order to more effectively exert the effects of the present invention, the inert gas is preferably a gas that does not contain oxygen or a gas that contains a small amount of oxygen. As for the gas containing a small amount of oxygen, since a high oxygen content makes it easier for the thermal decomposition of the product to progress, it is desirable for the oxygen content to be less than 5% by volume, more preferably 3% by volume or less, and even more preferably 1% by volume or less.

[0037] The temperature and time during the heat treatment are not particularly limited as long as they are such that crosslinking sites are regenerated in the regenerated product. The temperature during the heat treatment is usually a temperature exceeding the temperature when the uncrosslinked perfluoro(co)polymer (virgin product) is crosslinked by a conventionally known method, and is preferably 300 to 400°C, more preferably 320 to 390°C, and even more preferably 350 to 380°C. The time for the heat treatment varies depending on the heat treatment temperature, but is preferably 30 minutes to 5 hours, and more preferably 1 to 3 hours. The pressure during the heat treatment is not particularly limited, but it is preferable to carry out the heat treatment under normal pressure.

[0038] <Recycled material manufacturing method> The method for producing a recycled material according to the present invention (hereinafter also referred to as the "method for producing the recycled material") includes a step of crosslinking a recycled material-forming material including the recycled product obtained by the method for producing the recycled product. In the manufacturing method of this recycled material, a recycled product obtained by heat treatment under an inert gas atmosphere is used, making it possible to form a recycled material that has particularly excellent plasma resistance compared to, for example, a case in which a recycled product obtained by heat treatment in air is used.

[0039] <Recycled material forming material> The recycled material-forming material is not particularly limited as long as it contains the present recycled product, and may be a material consisting essentially of the present recycled product, but may also contain other components that have been conventionally known and have been blended into molded bodies such as sealing materials, if necessary. Examples of such other components include uncrosslinked perfluoro(co)polymers (virgin products); crosslinking agents; crosslinking aids; compounds containing ethylenically unsaturated bonds; reactive organosilicon compounds having two or more hydrosilyl groups in the molecule; perfluoropolyethers; non-adhesive agents such as fluorine oils; catalysts; polyol-based compounds; (co)polymers other than the above-mentioned perfluoro(co)polymers (e.g., fluororesins); acid acceptors such as magnesium oxide and calcium hydroxide; organic pigments such as anthraquinone-based pigments, perylene-based pigments, and dioxazine-based pigments; processing aids; vulcanization accelerators; antioxidants; antioxidants; inorganic fillers; and organic fillers. The other components may each be used alone or in combination of two or more.

[0040] [Recycled product] The recycled product used in the recycled material forming material may be one type or two or more types. Taking into consideration a balance between environmental protection, effective utilization of resources, and the ease of forming a recycled material having the desired physical properties, the amount of the recycled product used is preferably 0.5 to 60 mass%, more preferably 1 to 50 mass%, and even more preferably 10 to 40 mass%, relative to 100 mass% of the recycled material-forming material. Furthermore, when an uncrosslinked perfluoro(co)polymer is used as the recycled material forming material, the amount of this recycled product used is preferably 0.5 parts by mass or more, more preferably 0.5 to 90 parts by mass, even more preferably 1 to 80 parts by mass, and particularly preferably 10 to 70 parts by mass, per 100 parts by mass of uncrosslinked perfluoro(co)polymer, from the viewpoint of easily forming a recycled material having desired physical properties, etc.

[0041] [Uncrosslinked perfluoro (co)polymer] It is preferable to use an uncrosslinked perfluoro (co)polymer (virgin product) as the recycled material-forming material, since a recycled material-forming material with excellent moldability can be easily obtained and a recycled material having desired physical properties (hardness, tensile strength, elongation at break, compression set, and plasma resistance) can be easily formed. Examples of the uncrosslinked perfluoro (co)polymer include the same (co)polymers as the uncrosslinked perfluoro (co)polymers described in the section of the regenerated product. As the uncrosslinked perfluoro(co)polymer, a perfluoro(co)polymer having a crosslinking site different from the crosslinking site contained in the recycled product used in the recycled material-forming material may be used, but it is preferable to use a perfluoro(co)polymer having a crosslinking site similar to the crosslinking site contained in the recycled product used in the recycled material-forming material.

[0042] When an uncrosslinked perfluoro(co)polymer is used in the recycled material-forming material, the amount of the uncrosslinked perfluoro(co)polymer used is preferably 40 to 99.5% by mass, more preferably 50 to 99% by mass, and even more preferably 50 to 90% by mass, relative to 100% by mass of the recycled material-forming material, from the viewpoint of easily forming a recycled material having desired physical properties.

[0043] [Crosslinking agent] The recycled material-forming material can be crosslinked without using a crosslinking agent, but it is preferable to use a crosslinking agent appropriate to the type of recycled product or uncrosslinked perfluoro(co)polymer used for the recycled material-forming material, since it is possible to easily form a recycled material that is sufficiently crosslinked and has a good balance of excellent hardness, tensile strength, elongation at break, and tensile stress at 100% elongation (100% Mo).

[0044] As the crosslinking agent, for example, a crosslinking agent described in Japanese Patent No. 5278312 or other conventionally known crosslinking agents can be used without any particular limitation. Specific examples thereof include peroxide-based crosslinking agents, bisphenol-based crosslinking agents, triazine-based crosslinking agents, oxazole-based crosslinking agents, imidazole-based crosslinking agents, thiazole-based crosslinking agents, amidoxime-based crosslinking agents, and amidrazone-based crosslinking agents.

[0045] Examples of peroxide-based crosslinking agents include 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, di-t-butyl peroxide, t-butyldicumyl peroxide, benzoyl peroxide, 2,5-dimethyl-2,5-(t-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and t-butylperoxyisopropyl. Examples of peroxyalkylene oxides include propyl carbonate, di-(4-t-butylcyclohexyl)peroxydicarbonate, p-chlorobenzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxybenzoate, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, α,α-bis(t-butylperoxy)-p-diisopropylbenzene, t-butylperoxybenzene, and t-butylperoxymaleic acid.

[0046] Examples of bisphenol-based crosslinking agents include bisphenol AF and bisphenol S.

[0047] Examples of triazine crosslinking agents include 2,4,6-trimercapto-1,3,5-triazine, 2-hexylamino-4,6-dimercaptotriazine, 2-diethylamino-4,6-dimercaptotriazine, 2-cyclohexylamino-4,6-dimercaptotriazine, 2-dibutylamino-4,6-dimercaptotriazine, 2-anilino-4,6-dimercaptotriazine, and 2-phenylamino-4,6-dimercaptotriazine. The triazine crosslinking agent may be a compound that can act as a catalyst to form a triazine ring only with the nitrile groups contained in the regenerated product or the uncrosslinked perfluoro(co)polymer, such as an organic tin compound such as tetraphenyltin or triphenyltin.

[0048] Examples of oxazole-based crosslinking agents include 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (BOAP), 4,4'-sulfonylbis(2-aminophenol), and 9,9-bis(3-amino-4-hydroxyphenyl)fluorene.

[0049] Examples of imidazole crosslinking agents include 2,2-bis(3,4-diaminophenyl)hexafluoropropane, 2,2-bis[3-amino-4-(N-methylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-ethylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-propylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-perfluorophenylamino)phenyl]hexafluoropropane, and 2,2-bis[3-amino-4-(N-benzylamino)phenyl]hexafluoropropane.

[0050] Examples of thiazole crosslinking agents include 2-mercaptobenzothiazole and dibenzothiazyl disulfide.

[0051] When a crosslinking agent is used in the recycled material forming material, the amount of the crosslinking agent used is preferably 0.2 to 4 parts by mass, more preferably 0.2 to 2.5 parts by mass, per 100 parts by mass of the recycled product and uncrosslinked perfluoro(co)polymer in total, from the viewpoint that the crosslinking reaction proceeds sufficiently and a recycled material having excellent balance in hardness, tensile strength, elongation at break, and 100% Mo can be easily formed.

[0052] [Crosslinking agent] In the recycled material forming material, the crosslinking agent may be used alone, but when a crosslinking agent such as the peroxide-based crosslinking agent is used, it is preferable to use a crosslinking assistant. As the crosslinking assistant, a known crosslinking assistant may be selected according to the type of crosslinking agent.

[0053] For example, examples of crosslinking assistants that can be used when using a peroxide-based crosslinking agent include triallyl isocyanurate, triallyl cyanurate, trimethallyl isocyanurate, triallyl formal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalamide, polyfunctional (meth)acrylates such as ethylene glycol di(meth)acrylate and trimethylolpropane tri(meth)acrylate, and compounds capable of co-crosslinking by radicals (polyfunctional monomers), metal salts of higher carboxylic acids, polyhydric alcohol (meth)acrylates, and metal (meth)acrylic acid salts. Among these, triallyl isocyanurate is preferred because it has excellent reactivity, excellent heat resistance, and allows a sealing material having high hardness and high modulus to be easily obtained.

[0054] When a crosslinking aid is used in the recycled material-forming material, the amount of the crosslinking aid used is preferably 0.5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 6 parts by mass or less, per 100 parts by mass of the total of the recycled product and uncrosslinked perfluoro (co)polymer, from the viewpoints that the crosslinking reaction proceeds sufficiently and a sealing material having excellent balance in hardness, tensile strength, elongation at break, and 100% Mo can be easily formed.

[0055] When a crosslinking agent and crosslinking aid are used in the recycled material-forming material, the mass ratio of the content of the crosslinking aid to the content of the crosslinking agent in the recycled material-forming material (content of crosslinking aid / content of crosslinking agent) is preferably 1 or more, more preferably 2 or more, and is preferably 30 or less, more preferably 20 or less, from the viewpoint of being able to react the crosslinking agent without excess or deficiency and easily form a recycled material exhibiting the desired physical properties.

[0056] [Compounds containing ethylenically unsaturated bonds] Examples of the ethylenically unsaturated bond-containing compound include compounds described in WO 2022 / 065054, JP 2003-183402 A, and JP 11-116684 A.

[0057] [Reactive organosilicon compounds] Examples of the reactive organosilicon compound include the same organosilicon compounds as those described in JP-A Nos. 2003-183402 and 11-116684.

[0058] [catalyst] Examples of the catalyst include the same catalysts as those described in JP-A Nos. 2003-183402 and 11-116684.

[0059] [Organic pigments] Examples of the organic pigment include organic pigments similar to those described in WO 2016 / 043100, Japanese Patent No. 4720501, WO 2004 / 094527, and Japanese Patent No. 5278312.

[0060] [Filling material] Examples of the inorganic filler include particulate (powdered) inorganic materials such as carbon black, silica, barium sulfate, titanium oxide, and aluminum oxide. Examples of the organic filler include particulate (powdered) organic materials such as fluororesins such as PTFE, PFA, FEP, ETFE, and PVDF, polyethylene, polyimide, polyamideimide, polyetherimide, polyetheretherketone, polyetherketone, silicone resin, and melamine resin.

[0061] [Method of preparing recycled material] The recycled material-forming material can be prepared by mixing (kneading) the recycled product and, if necessary, the other components. When mixing the recycled product with the other components, the order of mixing is not particularly limited, and they may be mixed (kneaded) sequentially in any order, or may be mixed (kneaded) all at once, but it is preferable to mix (knead) them sequentially so that each component is uniform.

[0062] In the mixing (kneading) process, a conventionally known mixer (kneader) can be used, and examples of such a mixer include an open roll, a Banbury mixer, a twin-screw roll, and a kneader. Furthermore, during the mixing (kneading) process, the components may be mixed (kneaded) under heating or cooling, if necessary, depending on the mixer (kneader).

[0063] <Process for cross-linking recycled material forming materials> The method for producing the present recycled material is not particularly limited as long as it includes a step of crosslinking the recycled material-forming material.

[0064] When forming a recycled material from the recycled material-forming material, it is preferable to carry out a separating step in order to improve the efficiency of the forming work, reduce the defective rate, etc. This separating step is usually carried out using a roll or the like, and is usually also a step of preliminarily forming the recycled material-forming material into a sheet shape.

[0065] The sheet obtained in the extrusion step is preferably preformed into the desired shape of the recycled material before the crosslinking step. This preforming may involve directly forming the desired recycled material shape from the sheet obtained in the separating process, or the sheet obtained in the separating process may be cut or extruded into a rope-like shape (which also has the same meaning as a ribbon-like or noodle-like shape), and the resulting rope-like material may then be formed into the desired recycled material shape.

[0066] More preferably, the crosslinking step includes a primary crosslinking step and a secondary crosslinking step. The crosslinking step is preferably carried out using a preform having a desired recycled material shape obtained by the preforming step.

[0067] The primary crosslinking step is preferably a step of heating and pressurizing a preformed body having the desired recycled material shape obtained by the preforming step. A specific example of the step is a step of placing the preformed body in a mold and crosslinking the preformed body using a hot press or the like under a pressure of about 2 to 15 MPa at a temperature of, for example, 150 to 200°C for, for example, about 5 minutes to 1 hour.

[0068] The secondary crosslinking step is preferably a step of heating the molded body obtained in the primary crosslinking step, and specifically includes a step of heating the molded body at normal pressure to reduced pressure using various ovens, preferably a vacuum oven, at a temperature of, for example, 150 to 300°C for 1 to 48 hours, more preferably for about 3 to 24 hours. This secondary crosslinking process can promote crosslinking, and even if unreacted components remain after the primary crosslinking process, the unreacted components can be decomposed and evaporated, resulting in a recycled material that emits less gas.

[0069] In the method for producing the recycled material, a step of irradiating with radiation (radiation irradiation step) may be carried out after the crosslinking step, in order to more easily suppress cracks that may occur in the recycled material in a plasma atmosphere, etc. The recycled material obtained through this radiation irradiation step can be said to be a radiation-treated product.

[0070] The radiation to be irradiated in the radiation irradiation step is not particularly limited, but examples thereof include X-rays, gamma rays, electron beams, proton beams, neutron beams, heavy particle beams, alpha rays, and beta rays. Among these, gamma rays and electron beams are preferred. The radiation to be irradiated may be of one type alone or of two or more types.

[0071] When irradiating with radiation, it is desirable to irradiate with radiation so that the absorbed dose is preferably 1 to 120 kGy, more preferably 20 to 100 kGy. When irradiated with radiation in such an amount, unreacted components that may become particles or released gas can be reduced, and the recycled product and the uncrosslinked perfluoro (co)polymer are not excessively reduced in molecular weight, and a recycled material excellent in plasma resistance, crack resistance, etc. can be easily formed. The radiation exposure step may be carried out in two or more stages by changing the conditions.

[0072] Although irradiation with radiation may be performed in air, the presence of oxygen during irradiation may inhibit the crosslinking reaction, leading to a risk of reduced mechanical strength of the resulting recycled material and sticky surface of the resulting recycled material, and therefore the radiation irradiation step is preferably performed in an atmosphere of an inert gas such as nitrogen or argon.

[0073] <Recycled material> The recycled material obtained by this method for producing recycled materials is not particularly limited, but can be used, for example, as gaskets or packings for various components, and can be particularly suitably used as a sealing material for semiconductor manufacturing equipment or a sealing material for plasma processing equipment, and in particular, as a sealing material for driving parts such as gate valves used in the openings of plasma processing chamber units. The recycled material is preferably a sealing material, and examples of the sealing material include O-rings, square rings, gaskets, packing, oil seals, bearing seals, and lip seals. The shape of the recycled material may be appropriately selected depending on the application.

[0074] The semiconductor manufacturing equipment is not limited to equipment specifically for manufacturing semiconductors, but broadly includes all manufacturing equipment used in the semiconductor field where a high degree of cleanliness is required, such as equipment for manufacturing liquid crystal panels, plasma panels, etc., and specific examples include the equipment described in Japanese Patent No. 5278312, etc.

[0075] The IRHD of the recycled material measured in accordance with JIS K 6253-2:2012 is preferably 45 or more, and more preferably 50 or more. The tensile strength of the recycled material, measured by the method described in the examples below, is preferably 7 MPa or more, and more preferably 8 MPa or more. The elongation at break of the recycled material, measured by the method described in the examples below, is preferably 120% or more, and more preferably 130% or more. The mass loss rate of the recycled material measured by the method described in the examples below is preferably 5% or less, more preferably 3% or less, and the lower limit is not particularly limited, but is, for example, 0%. EXAMPLES

[0076] Next, the present invention will be described in more detail by showing examples, but the present invention is not limited to these.

[0077] <Crosslinked perfluoro(co)polymer (recycled product)> The crosslinked perfluoro (co)polymers (products to be regenerated) used in the following Examples and Comparative Examples are as follows: "Crosslinked perfluoro(co)polymer-1": 100 parts by mass of a perfluoroelastomer (PFE131T [3M], a perfluoro(co)polymer in which the crosslinking site is a nitrile group) and 0.5 parts by mass of an oxazole-based crosslinking agent (BOAP, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, Tokyo Chemical Industry Co., Ltd.) are kneaded using an open roll, and the resulting block of elastomer composition is filled into an O-ring-shaped mold and press-molded at 180°C for 30 minutes (primary crosslinking) using a compression vacuum press under a pressure of 5 MPa, and then the press-molded sheet is heated in an oven at 250°C for 24 hours (secondary crosslinking) to produce a molded product (O-ring) (corresponding to an unused or used molded product). "Crosslinked perfluoro(co)polymer-2": 100 parts by mass of a perfluoroelastomer (Tecnoflon PFR94 [manufactured by Solvay], a perfluoro(co)polymer in which the crosslinking site is a halogen atom), 1 part by mass of TAIC (manufactured by Mitsubishi Chemical Corporation, triallyl isocyanurate), and 0.5 parts by mass of Perhexa 25B (manufactured by NOF Corporation) were mixed in an open roll, and the resulting block of elastomer composition was filled into an O-ring shaped mold and press-molded at 170°C for 10 minutes (primary crosslinking) using a compression vacuum press machine under a pressure of 5 MPa, and then the press-molded sheet was heated in an oven at 200°C for 4 hours (secondary crosslinking) to produce a molded product (O-ring) (corresponding to an unused or used molded product).

[0078] [Example 1] The crosslinked perfluoro(co)polymer-1 (regenerated product) was placed in KDF-75Plus manufactured by Yamato Scientific Co., Ltd. and heat-treated at 380°C and 1 atm for 1 hour in a nitrogen atmosphere to obtain a regenerated perfluoro(co)polymer-1 (regenerated product).

[0079] [Example 2] A recycled perfluoro(co)polymer-2 (recycled product) was obtained in the same manner as in Example 1, except that the crosslinked perfluoro(co)polymer-2 (recycled product) was used instead of the crosslinked perfluoro(co)polymer-1.

[0080] [Example 3] The crosslinked perfluoro(co)polymer-1 (regenerated product) was placed in KDF-75Plus manufactured by Yamato Scientific Co., Ltd. and heat-treated at 370°C and 1 atm for 1 hour under a helium gas atmosphere to obtain a regenerated perfluoro(co)polymer-3 (regenerated product).

[0081] [Example 4] The crosslinked perfluoro(co)polymer-1 (regenerated product) was placed in KDF-75Plus manufactured by Yamato Scientific Co., Ltd. and heat-treated at 370°C and 1 atm for 1 hour under an argon gas atmosphere to obtain a regenerated perfluoro(co)polymer-4 (regenerated product).

[0082] [Comparative Example 1] The crosslinked perfluoro(co)polymer-1 (regenerated product) was placed in KDF-75Plus manufactured by Yamato Scientific Co., Ltd. and heat-treated in air at 380°C and 1 atm for 1 hour to obtain a regenerated perfluoro(co)polymer-c1 (regenerated product).

[0083] [Comparative Example 2] A recycled perfluoro(co)polymer-c2 (recycled product) was obtained in the same manner as in Comparative Example 1, except that the crosslinked perfluoro(co)polymer-2 (recycled product) was used instead of the crosslinked perfluoro(co)polymer-1.

[0084] <Crosslinking site content> Using FT-IR (Bruker, HYPERION3000), resolution: 4 cm -1 , Number of scans: 32, Transmission method, Measurement range: 400~4000cm -1 The contents of crosslinking sites in the crosslinked perfluoro(co)polymer (regenerated product) and the regenerated perfluoro(co)polymer (regenerated product) were measured under the above conditions. The results are shown in Table 1. Specifically, 2230-2290cm -1 The maximum intensity when the intensity of the baseline is 2200-2700cm -1 The intensity of the 2500 cm -1 The value obtained by dividing the strength by the strength at 1000 nm was regarded as the content of crosslinking sites (nitrile groups). However, when the result of this calculation (content of crosslinking sites (nitrile groups)) was less than 0.01, the content of crosslinking sites (nitrile groups) was regarded as 0.01.

[0085] In the column for Example 2 in Table 1 below, the content of crosslinked sites is marked as "-". However, in Example 2, it is believed that regeneration of the crosslinked sites (C=C bonds) on the right side of the following formula has occurred sufficiently.

[0086] [ka]

[0087] <Mass reduction rate> The mass of the crosslinked perfluoro(co)polymer (regenerated product) used in the above-mentioned Examples or Comparative Examples before heat treatment was measured, and the mass of the resulting regenerated perfluoro(co)polymer (regenerated product) was also measured. The mass reduction rate (%) was calculated using the following formula. The results are shown in Table 1. Mass reduction rate (%) = [(mass of recycled product - mass of recycled product) / mass of recycled product] x 100

[0088] [Table 1]

[0089] <Uncrosslinked perfluoro (co)polymer (virgin product)> The uncrosslinked perfluoro (co)polymers (virgin products) used in the following Examples and Comparative Examples are as follows: "Uncrosslinked perfluoro (co)polymer-1": PFE131T (3M) "Uncrosslinked perfluoro (co)polymer-2": Tecnoflon PFR94 (manufactured by Solvay)

[0090] [Example 5] A block of elastomer composition was obtained by kneading 60 parts by mass of uncrosslinked perfluoro(co)polymer-1 (virgin product), 40 parts by mass of recycled perfluoro(co)polymer-1 (recycled product), and 0.5 parts by mass of an oxazole-based crosslinking agent (BOAP, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, manufactured by Tokyo Chemical Industry Co., Ltd.) with an open roll. The obtained bulk elastomer composition was filled into an O-ring shaped mold and press molded at 180°C for 30 minutes under a pressure of 5 MPa using a compression vacuum press (primary crosslinking). The press-molded sheet was then heated in an oven at 250°C for 24 hours (secondary crosslinking) to obtain a molded product (O-ring).

[0091] [Comparative Examples 3 to 4] In Example 5, a molded body was obtained in the same manner as in Example 5, except that the uncrosslinked perfluoro(co)polymer and the recycled perfluoro(co)polymer were the (co)polymers of the types and amounts (numbers, parts by mass) shown in Table 2.

[0092] [Example 6] A lump-shaped elastomer composition was obtained by kneading 60 parts by mass of uncrosslinked perfluoro(co)polymer-2 (virgin product), 40 parts by mass of recycled perfluoro(co)polymer-2 (recycled product), 10 parts by mass of PTFE particles (Lubron L5 (manufactured by Daikin Industries, Ltd.)), 0.5 parts by mass of Perhexa 25B (manufactured by NOF Corporation), and 1 part by mass of TAIC (triallyl isocyanurate, manufactured by Mitsubishi Chemical Corporation) with an open roll. The obtained block elastomer composition was filled into an O-ring shaped mold and press molded at 170°C for 10 minutes under a pressure of 5 MPa using a compression vacuum press (primary crosslinking). The press-molded sheet was then heated in an oven at 200°C for 4 hours (secondary crosslinking) to obtain a molded product (O-ring).

[0093] [Comparative Examples 5 to 6] In Example 6, a molded body was obtained in the same manner as in Example 6, except that the uncrosslinked perfluoro(co)polymer and the recycled perfluoro(co)polymer were the (co)polymers of the types and amounts (numbers, parts by mass) shown in Table 2.

[0094] <irhd> The hardness of the obtained molded body was measured at 23° C. using an IRHD hardness measuring device in accordance with JIS K 6253-2:2012. The results are shown in Table 2.

[0095] <Tensile strength and elongation at break> The obtained molded article (O-ring) was pulled at 500 mm / min, and the tensile strength and elongation at break were measured using a Schopper tensile tester at 23° C. The results are shown in Table 2.

[0096] <Compression set> The compression set of the sealing material was determined in accordance with JIS K 6262:2013. The obtained molded body was kept at 200° C. for 72 hours at a compression ratio of 25%, and then the pressure was released and the molded body was allowed to cool at the standard temperature of the test room for 30 minutes, after which the thickness of the molded body was measured. The obtained molded body was kept at 260°C for 72 hours with a compression ratio of 20%, and then the pressure was released and the body was allowed to cool at the standard temperature of the test room for 30 minutes, after which the thickness of the molded body was measured. The compression set (CS) was calculated based on the following formula. The results are shown in Table 2. Compression set rate (%) = {(h0-h1) / (h0-h2)} x 100 [h0: thickness of the compact before compression (mm), h1: thickness of the compact after cooling for 30 minutes (mm), h2: thickness (height) of the spacer (mm)]

[0097] <Mass reduction rate (plasma resistance)> The plasma resistance (mass reduction rate) of the obtained molded body was measured. Specifically, the measurement was performed as follows. The results are shown in Table 2. A fluorine radical exposure test was conducted under the following conditions, in which the obtained molded body (O-ring) was exposed to fluorine radicals generated from NF3 by remote plasma. The mass of the molded body (O-ring) was measured before and after the test, and the mass loss rate was calculated according to the following formula to evaluate the plasma resistance. It can be said that the smaller the mass loss rate, the better the plasma resistance. Mass reduction rate (%) = {(mass before test - mass after test) / (mass before test)} x 100

[0098] (conditions) Plasma source: Remote plasma source Plasma power: 5000W Gas flow rate: NF3; 1.5SLM, Argon; 1.5SLM ·Vacuum level: 7torr Test temperature: 250℃ Test duration: 5 hours

[0099] [Table 2]

[0100] In Example 5, a molded product having the same IRHD and elongation at break as in Comparative Example 4, which used only virgin products, was obtained. A molded product having a smaller compression set and excellent plasma resistance (smaller mass loss rate) compared to Comparative Example 3 was obtained. Furthermore, in Example 6, a molded product having the same IRHD and tensile strength as Comparative Example 6, which used only virgin products, was obtained. Compared to Comparative Example 5, the molded product had a smaller compression set when maintained at 200°C for 72 hours at a compression ratio of 25%, and had excellent plasma resistance (low mass loss rate).< / irhd>

Claims

1. The method includes a step of heat-treating a crosslinked perfluoro(co)polymer obtained by crosslinking a perfluoro(co)polymer having a crosslinking site under an inert gas atmosphere to regenerate the crosslinking site, the crosslinking site is a nitrile group or a halogen atom; A method for producing recycled perfluoro (co)polymers.

2. The method for producing a recycled perfluoro (co)polymer according to claim 1, wherein the crosslinking site is a nitrile group.

3. The method for producing a recycled perfluoro (co)polymer according to claim 1, wherein the inert gas is at least one selected from the group consisting of nitrogen gas, argon gas and helium gas.

4. The method for producing a recycled perfluoro(co)polymer according to claim 1, wherein the perfluoro(co)polymer having a crosslinking site is a (co)polymer that does not contain a carbon-hydrogen bond in the main chain of the (co)polymer.

5. A method for producing a recycled material, comprising a step of crosslinking a recycled material-forming material containing the recycled perfluoro(co)polymer obtained by the method for producing a recycled perfluoro(co)polymer according to any one of claims 1 to 4.

6. The method for producing a recycled material according to claim 5 , wherein the recycled material-forming material further comprises a crosslinking agent.

7. The method for producing a recycled material according to claim 5 , wherein the recycled material-forming material further contains an uncrosslinked perfluoro (co)polymer.

8. The method for producing a recycled material according to claim 7, wherein the content of the recycled perfluoro (co)polymer in the recycled material-forming material is 0.5 parts by mass or more per 100 parts by mass of the uncrosslinked perfluoro (co)polymer.

9. The method for producing a recycled material according to claim 5 , wherein the recycled material is a sealing material.

Citation Information

Patent Citations

  • Treatment of vulcanized fluororubber

    JP1986069805A

  • Supercritical hydroxylating decomposition-treating method of organic synthetic resin containing sulfur atom and supercritical hydroxylating decomposition-treating unit

    JP1998324768A

  • Method for manufacturing regenerated vulcanized fluorinated rubber and composition for unvulcanized fluorinated rubber to be regenerated

    JP2003211460A

  • Decomposition method of vulcanized rubber and decomposed rubber composition

    JP2006070127A

  • Method for producing fluorine-containing polymer

    JP2007063334A