Method for producing polyamide resin-containing phenolic resin fiber

By adding polyamide resin to phenol during phenolic resin synthesis and incorporating a curing step, the method addresses the challenges of producing small-diameter phenolic resin fibers with enhanced strength and flexibility, suitable for activated carbon production.

JP7577455B2Active Publication Date: 2024-11-05FUTAMURA CHEM CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020062985
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-11-05
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Existing methods for producing phenolic resin fibers face challenges in achieving small diameters due to insufficient fiber strength, thread breakage during spinning, and difficulties in uniformly mixing phenolic and polyamide resins, which affects the production of fibrous activated carbon.

Method used

A method involving the addition of 1 to 3 parts by weight of polyamide resin to 100 parts by weight of phenol, followed by mixing with formaldehyde and an acid catalyst, then heating and spinning to produce phenolic resin fibers, with a subsequent curing step to enhance strength, allowing for small-diameter fibers suitable for activated carbon.

Benefits of technology

The method enables the production of small-diameter phenolic resin fibers with improved strength and flexibility, facilitating easier spinning and reducing thread breakage, while maintaining the integrity of the fibers for use in activated carbon applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577455000006
    Figure 0007577455000006
  • Figure 0007577455000001
    Figure 0007577455000001
  • Figure 0007577455000002
    Figure 0007577455000002
Patent Text Reader

Abstract

To provide a manufacturing method of a phenol resin fiber containing a polyamide resin, in which a resin composition of a phenol resin is improved to allow a small-diameter phenol resin fiber to be easily spun, and when it is used as a raw material for a fibrous active carbon, the decrease in fiber strength can be suppressed.SOLUTION: A manufacturing method of a phenol resin fiber containing a polyamide resin comprises: a raw material mixing step of adding a polyamide resin of 1 to 3 pts.wt. and formaldehyde to phenol of 100 pts.wt. and then melting to prepare a raw material; a catalyst addition step of adding an acid catalyst to the raw material to obtain a catalyst-added raw material; a synthesis step of heating the catalyst-added raw material to prepare a polyamide resin-containing phenol resin; and a spinning step of spinning the polyamide resin-containing phenol resin to obtain a resin fiber.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing phenolic resin fibers, and more particularly to a method for producing fine-diameter polyamide resin-containing phenolic resin fibers. [Background technology]

[0002] Phenolic resins are used in various parts and components that require durability, such as circuit board materials, due to their heat resistance and chemical resistance. These properties are also inherited in the form of phenolic resin fibers.

[0003] Phenolic resins are divided into thermoplastic novolac type and thermosetting resol type. Of these, the majority of fibrous resins are novolac type due to the convenience of thread processing. The biggest factor that distinguishes the two types is the difference in the catalyst used in the polymerization of phenol and formaldehyde.

[0004] As the acid catalyst added during the synthesis of novolac-type phenolic resin, organic acids such as oxalic acid and inorganic acids such as hydrochloric acid are usually used (see Patent Documents 1 and 2, etc.). After the synthesis of novolac-type phenolic resin, it is heated and melted, and processed into a fiber shape by spinning. However, since the strength of the phenolic resin at this stage is insufficient, it is further cured. Usually, during curing, the phenolic resin is immersed in a mixed solution of inorganic acid and formaldehyde. Furthermore, various phosphoric acid esters are added to the novolac-type phenolic resin as an improvement to the fibrous novolac-type phenolic resin. As a result, the diameter of the resin fiber becomes thicker and the strength increases (see Patent Documents 3 and 4, etc.). Through the synthesis of a series of novolac-type phenolic resins, it was desired to improve the performance of the resin fiber.

[0005] However, phenolic resin fibers tend to have inferior toughness compared to other synthetic resins, and therefore, when producing thin phenolic resin fibers, thread breakage is likely to occur during the winding process in which molten phenolic resin is extruded, pulled, and stretched, making stable spinning difficult.

[0006] Therefore, a method has been proposed in which 100 parts by weight of phenolic resin is melt-mixed with 5 to 30 parts by weight of polyamide resin to obtain a polyamide-modified novolac-type phenolic resin (see Patent Document 5). In this case, the amount of polyamide resin is too large, which inhibits the polymerization reaction of the resin, resulting in a low-molecular-weight resin, and the melting point of the resin is lowered, making it difficult to stretch during melt spinning. In addition, the polyamide resin burns during carbonization and activation, which significantly reduces the fiber strength of the fibrous activated carbon, making it unsuitable as a raw material for activated carbon.

[0007] Also, a manufacturing method has been proposed in which polyamide resin is mixed after synthesis of phenolic resin to produce polyamide resin-containing phenolic resin fiber (see Patent Document 6). However, since the melting points of phenolic resin and polyamide resin are significantly different, it is not easy to melt-mix the two resins, and it is difficult to mix them uniformly, and there is a risk of the resin burning during melting.

[0008] Furthermore, phenolic resin fibers are attracting attention for their use as fibrous activated carbon. In the case of phenolic resin, the number of carbon atoms in the molecule is relatively large compared to other olefin resins, polyester resins, etc. Therefore, it is preferable for forming a carbon skeleton that remains after carbonization and activation. In addition, the use of activated carbon fibers derived from phenolic resins is expanding due to their flexibility.

[0009] Fibrous activated carbon derived from phenolic resin fibers is in high demand due to its high purity and excellent selectivity and adsorption speed for adsorbed substances. Furthermore, fibrous activated carbon with a small fiber diameter has a large external surface area, which improves the adsorption efficiency per unit weight. For these reasons, there is a demand for phenolic resin that can be spun into fine fibers. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2007-291209 A [Patent Document 2] Patent No. 5250717 [Patent Document 3] Patent No. 5443268 [Patent Document 4] Patent No. 5499007 [Patent Document 5] Japanese Patent Application Publication No. 6-228256 [Patent Document 6] Patent No. 5453373 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in consideration of the above-mentioned points, and provides a method for producing a polyamide resin-containing phenolic resin fiber, which makes it easier to spin a small-diameter phenolic resin fiber by improving the resin composition in the phenolic resin in the phenolic resin fiber, and also suppresses a decrease in fiber strength even when the fiber is used as a raw material for a fibrous activated carbon. [Means for solving the problem]

[0012] That is, the first invention is, A method for producing phenolic resin fibers as a starting material for fibrous activated carbon, comprising the steps of: The present invention relates to a method for producing a polyamide resin-containing phenolic resin fiber, comprising a raw material mixing step of adding 1 to 3 parts by weight of polyamide resin to 100 parts by weight of phenol, melting the mixture, and adding and mixing formaldehyde to prepare a raw material; a catalyst adding step of adding an acid catalyst to the raw material to obtain a catalyst-added raw material; a synthesis step of heating the catalyst-added raw material to prepare a polyamide resin-containing phenolic resin that contains a polyamide resin; and a spinning step of spinning the polyamide resin-containing phenolic resin to obtain a resin fiber.

[0013] The second invention is the same as the first invention, wherein the fineness of the resin fiber is 5.0 (dtex) The present invention relates to a method for producing a polyamide resin-containing phenolic resin fiber according to claim 1, which is as follows.

[0014] The third invention relates to a method for producing a polyamide resin-containing phenolic resin fiber according to the first or second invention, which includes a fiber curing step of immersing the resin fiber in a curing liquid containing an inorganic acid and formaldehyde after the spinning step to obtain a cured resin fiber.

[0015] The fourth invention is the third invention. The polyamide resin-containing phenolic resin fiber was obtained by the method for producing the polyamide resin-containing phenolic resin fiber. The present invention relates to a method for producing an activated carbon adsorbent, which comprises an activation step of carbonizing and activating the cured resin fibers to obtain an activated carbon adsorbent. Effect of the Invention

[0016] According to the method for producing a polyamide resin-containing phenolic resin fiber according to the first aspect of the present invention, A method for producing phenolic resin fibers as a starting material for fibrous activated carbon, comprising the steps of: The process includes a raw material mixing step of adding 1 to 3 parts by weight of polyamide resin to 100 parts by weight of phenol, melting the mixture, and adding and mixing formaldehyde to prepare a raw material; a catalyst adding step of adding an acid catalyst to the raw material to obtain a catalyst-added raw material; a synthesis step of heating the catalyst-added raw material to prepare a polyamide resin-containing phenolic resin that contains a polyamide resin; and a spinning step of spinning the polyamide resin-containing phenolic resin to obtain resin fibers. This makes it easy to spin fine phenolic resin fibers, and also prevents a decrease in fiber strength when the material is used as a raw material for fibrous activated carbon.

[0017] According to the second aspect of the present invention, the method for producing a polyamide resin-containing phenolic resin fiber is the same as that of the first aspect of the present invention, except that the fineness of the resin fiber is 5.0 (dtex) Since the diameter of the phenolic resin fiber is smaller than 100 μm, the phenolic resin fiber can be made small in diameter.

[0018] According to the method for producing a polyamide resin-containing phenolic resin fiber of the third invention, in the first or second invention, a fiber curing process is provided after the spinning process, in which the resin fiber is immersed in a curing liquid containing an inorganic acid and formaldehyde to obtain a cured resin fiber, thereby improving the strength of the resin fiber itself.

[0019] According to the method for producing an activated carbon adsorbent according to the fourth invention, The polyamide resin-containing phenolic resin fiber was obtained by the method for producing the polyamide resin-containing phenolic resin fiber.Since the process includes an activation step in which the cured resin fibers are carbonized and activated to obtain an activated carbon adsorbent, it is possible to obtain fibrous activated carbon with a small diameter. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a process diagram showing a method for producing a polyamide resin-containing phenolic resin fiber of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The method for producing the polyamide resin-containing phenolic resin fiber of the present invention will be described with reference to the process diagram in Fig. 1. First, polyamide resin is added to phenol, which is the raw material of phenolic resin, and melted. After the polyamide resin is melted, the phenol and polyamide resin melt is cooled to about room temperature, and formaldehyde is added and mixed to obtain a mixed raw material ("raw material mixing process").

[0022] When mixing the raw materials, the phenol equivalent (P N ) and formaldehyde equivalent (F N The relationship between the equivalent ratio (R1) and the formaldehyde equivalent (F N ) to the equivalent amount of phenol (P N ) and the equivalent ratio (R1) is preferably in the range of 0.5 to 1.0. In the examples described later, this range is also favorable for the synthesis of phenolic resin. When the equivalent ratio R1 is below 0.5, the amount of phenol is too small, and when the equivalent ratio R1 is above 1.0, the amount of phenol is relatively excessive. Therefore, taking into consideration the catalyst type and reaction system described below, this range of equivalent ratio is appropriate.

number

[0023] In addition, the polyamide resin is in the range of 1 to 3 parts by weight relative to the weight of phenol during synthesis of the phenol resin containing the polyamide resin. In the examples described later, this range is also convenient for synthesis of the phenol resin containing the polyamide resin. If the polyamide resin is less than 1 part by weight, the amount of the polyamide resin is too small, and it is not possible to improve the stretchability during spinning. If the amount of the polyamide resin is more than 3 parts by weight, the amount of the polyamide resin is excessive, which may inhibit the synthesis of the phenol resin and make it impossible to produce a polymer suitable for spinning.

[0024] The raw material phenol includes not only phenol but also phenol compounds (aromatic compounds having a hydroxyl group). For example, cresol (o-, m-, p-position), p-phenylphenol, xylenol (2,3-, 3,5-), resorcinol, various bisphenols, etc. Also, instead of formaldehyde, acetaldehyde, benzaldehyde, glyoxal, furfural, etc. can be used.

[0025] Examples of polyamide resins include nylon 6, nylon 11, nylon 12, nylon 6,6, nylon 6,10, nylon 6T, nylon 6I, nylon 9T, nylon M5T, and nylon 6,12.

[0026] As a catalyst for the purpose of forming crosslinks between the raw material phenol and formaldehyde molecules, an organic acid such as oxalic acid, an inorganic acid such as hydrochloric acid, or an organic phosphorus compound such as a phosphoric acid ester is added ("catalyst addition step").

[0027] After melt mixing the specified amounts of phenol, polyamide resin, formaldehyde, and acid catalyst, the mixture is heated at 80-100°C for 3-10 hours while stirring. The temperature is then raised to 150-220°C, and the dehydration condensation reaction proceeds to synthesize the phenol resin containing the polyamide resin ("synthesis step"). The amount of catalyst added is an amount equivalent to 0.2-5 parts by weight of the weight of phenol.

[0028] Subsequently, the polyamide resin-containing phenolic resin produced in the synthesis step is fed to a spinning device. Since the novolac-type phenolic resin is a thermoplastic resin, the spinning device is maintained at a melting temperature of 110 to 200°C, preferably 120 to 150°C. The diameter of the nozzle of the spinning device is 0.05 to 1.0 mm, preferably 0.1 to 1.0 mm, and the molten phenolic resin is discharged from the nozzle by extrusion or the like and spun. After spinning, the resin is cooled by contact with the outside air, so that the molten resin immediately hardens and fibers of the polyamide resin-containing phenolic resin are formed ("spinning step").

[0029] The fiber shape (cross-sectional shape) of the phenolic resin fiber is circular or elliptical, and depends on the shape of the nozzle of the spinning device. The fiber diameter (cross-sectional diameter) of the resulting phenolic resin fiber is approximately 0.01 to 0.04 mm. The fiber diameter is controlled in the spinning process described above. If the fiber diameter is extremely small, it cannot withstand the heat during carbonization. Also, if it is too thick, it becomes difficult to harden.

[0030] The resin fiber that is discharged from the spinning device and cooled is wound up on a bobbin or the like. The discharge speed from the spinning device nozzle and the winding speed are appropriately adjusted to be in the range of 100 to 3000 m / min, and preferably 200 to 1500 m / min. Of course, the spinning method, device, and conditions are appropriately determined depending on the production scale.

[0031] By completing the spinning process, the polyamide resin-containing phenolic resin fiber is completed. However, the strength of the resin fiber itself tends to be insufficient in its current state. Therefore, it is necessary to improve the strength for the convenience of subsequent handling. Therefore, the resin fiber is immersed in a curing liquid to obtain a cured resin fiber ("fiber curing process"). The curing liquid is a mixture of an inorganic acid such as hydrochloric acid, sulfuric acid, or phosphoric acid and formaldehyde. In addition to formaldehyde, acetaldehyde, benzaldehyde, glyoxal, furfural, etc. can also be used. In the fiber curing process, curing is carried out at 60 to 110°C for 3 to 30 hours. After curing, the phenolic resin fiber is completed through washing with water and drying.

[0032] As can be seen from the illustrated and detailed manufacturing method of phenolic resin fiber, polyamide resin is added during synthesis of phenolic resin. Therefore, it is different from the conventional manufacturing method in which novolac type phenolic resin is synthesized, then mixed with polyamide resin and spun or cured. That is, polyamide resin is directly mixed during synthesis of novolac type phenolic resin. When added or mixed after synthesis, the melting points of the resins are significantly different, making uniform mixing difficult and causing the risk of resin burning, so the manufacturing method of the present invention is advantageous.

[0033] According to the manufacturing method of the present invention, since polyamide resin coexists from the synthesis stage of phenol and formaldehyde, nylon remains evenly in the phenol resin produced by synthesis. In general, polyamide resin shows excellent toughness and flexibility due to hydrogen bonds of amide groups. Due to this action, it is considered that the phenol resin fiber obtained by the manufacturing method of the present invention has the toughness and flexibility due to the polyamide resin and has improved stretchability because the polyamide resin is uniformly present. This makes it easier to stretch the resin and to obtain a fiber with a small diameter. According to the index of the elongation rate of the phenol resin fiber in the examples described later, a high value can be obtained by including polyamide resin during synthesis. Therefore, the fiber diameter can be made small, and the fiber can be easily spun by making it difficult for thread breakage to occur.

[0034] The applications of the phenolic resin fiber prepared by the manufacturing method of the present invention are not necessarily limited. For example, since the phenolic resin fiber is difficult to burn, it is also suitable for fire-resistant protective clothing. In addition to the use as the fiber itself, the phenolic resin fiber is also suitable as a starting material for fibrous activated carbon. Since the diameter is smaller than that of ordinary phenolic resin fibers, the outer surface area can be increased when the phenolic resin fiber is made into fibrous activated carbon. EXAMPLES

[0035] [Preparation of phenolic resin fibers] <Prototype 1> (Synthesis Stage) 100 parts by weight of 90% phenol, 67.5 parts by weight of 37% formaldehyde (formalin), 1 part by weight of nylon 6 (manufactured by Ube Industries, Ltd., "1030B") as a polyamide resin, and 0.5 parts by weight of phosphoric ester (manufactured by Toho Chemical Industry Co., Ltd., "BH-650") as an acid catalyst were charged into a 3 L separable flask equipped with a stirrer and a reflux condenser, and reacted at 90 to 100°C for 5 hours. After the reaction was completed, the temperature was raised to 200°C to carry out dehydration condensation. Thereafter, the pressure inside the reaction vessel was reduced, and moisture and unreacted materials were removed. Then, the reaction vessel was washed by repeatedly adding water through a dropping funnel to remove low polymerized materials. In this way, a solid phenolic resin corresponding to Prototype Example 1 was synthesized. The phenol equivalent (P N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0036] (Spinning and curing stages) Next, the synthesized phenolic resin solid was crushed and put into a melt spinning device. The device temperature was set to 150°C to melt the phenolic resin, and the molten resin was discharged from a nozzle with a diameter of 0.5 mm and wound on a bobbin to obtain a resin fiber. The resin fiber was immersed in a hardening solution containing 18% by weight of hydrochloric acid and 10% by weight of formaldehyde, and hardened at 95°C for 10 hours. After hardening, the fiber was washed with water and dried to prepare a phenolic resin fiber.

[0037] <Prototype Example 2> The synthesis step and the spinning and curing steps were the same as those in Sample 1, except that 1 part by weight of nylon 6,12 (manufactured by Ube Industries, Ltd., "7115U") was used as the polyamide resin, to obtain the phenol resin fiber of Sample 2. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0038] <Prototype 3> The synthesis step and the spinning and curing steps were the same as those in Sample 1, except that 3 parts by weight of nylon 6,12 (manufactured by Ube Industries, Ltd., "7115U") was used as the polyamide resin, to obtain the phenol resin fiber of Sample 3. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0039] <Prototype 4> The synthesis step and the spinning and curing steps were the same as those in Sample 1, except that 5 parts by weight of nylon 6,12 (manufactured by Ube Industries, Ltd., "7115U") was used as the polyamide resin, to obtain the phenol resin fiber of Sample 4. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0040] <Prototype 5> The synthesis step and the spinning and curing steps were the same as those in Sample Example 1, except that 1 part by weight of polyamide elastomer (manufactured by Ube Industries, Ltd., "9040X1") was used as the polyamide resin, to obtain the phenol resin fiber of Sample Example 5. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0041] <Prototype 6> The synthesis step and the spinning and curing steps were the same as those in Sample Example 1, except that 1 part by weight of AQ nylon (manufactured by Toray Industries, Inc., "P-70") was used as the polyamide resin, to obtain the phenol resin fiber of Sample Example 6. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0042] <Prototype 7> The synthesis step and the spinning and curing steps were the same as those in Sample 1, except that 1 part by weight of nylon 6 (Lead City Corporation, "FR-101") was used as the polyamide resin, to obtain the phenol resin fiber of Sample 7. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0043] <Prototype Example 8> The synthesis step and the spinning and curing steps were the same as those of Sample 2, except that 0.5 parts by weight of oxalic acid was used as the acid catalyst, to obtain the phenol resin fiber of Sample 8. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0044] <Comparative Example 1> The same procedure as in Prototype 1 was followed except that the amount of polyamide resin was 0 parts by weight (not added), to obtain a phenol resin fiber of Comparative Example 1. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0045] <Comparative Example 2> The synthesis step and the spinning and curing steps were the same as those of Comparative Example 1, except that 0.5 parts by weight of oxalic acid was used as the acid catalyst, to obtain the phenol resin fiber of Comparative Example 2. N ) and formaldehyde equivalent (F N ) was found to have an equivalent ratio (R1) of 0.8604.

[0046] [Measurement items / Measurement method] [Fineness (dtex) 〕 The fineness (dtex) was measured according to JIS L 1015 (2010) in accordance with Method A of "8.5.1 Correct fineness" of the same standard.

[0047] [Tensile strength] The tensile strength (cN / dtex) was measured in accordance with JIS L 1015 (2010).

[0048] [Elongation rate] The elongation rate (%) was measured according to JIS L 1015 (2010).

[0049] [Molecular weight] As a pretreatment, the resin of each example obtained by the above preparation was dissolved in an eluent (tetrahydrofuran) and filtered through a membrane filter. The filtrate was measured by gel permeation chromatography (GPC). An RI detector was used for detection, and standard polystyrene was used as the molecular weight standard.

[0050] [Melting Point] The temperature was increased at a rate of 10°C / min or less to a temperature 20°C lower than the expected melting temperature, and then the heating rate was increased to 2°C / min, and the temperature at which the phenolic resin completely melted and became liquid was measured.

[0051] Tables 1 and 2 show the measurement results of the resin fibers of each prototype and comparative example.

[0052] [Table 1]

[0053] [Table 2]

[0054] [Results and Discussion] Comparing Comparative Example 1, in which no polyamide resin was added, with Prototype Examples 1 to 3 and 5 to 7, the prototype examples spun from a resin containing a polyamide resin had a higher elongation and were able to produce fibers with a smaller diameter than those in Comparative Example 1. In addition, the tensile strength was about the same despite the small diameter, which showed that even with a small diameter, thread breakage is unlikely to occur during spinning, improving the ease of spinning and improving production efficiency.

[0055] In addition, when Prototype 2 and Comparative Example 1 are compared with Prototype 8 and Comparative Example 2, which used a different catalyst, it was found that similarly fine fibers could be obtained, and that the elongation percentage was also improved along with the tensile strength. This shows that even if the catalyst used to prepare the raw material polyamide resin-containing phenolic resin is changed, fine resin fibers can be obtained and production efficiency can be improved.

[0056] In addition, comparing Prototype 2 to Prototype 4 in which the amount of polyamide resin added was changed, in Prototype 4 in which 5 parts by weight of polyamide resin was added, the fiber diameter became large and it was not possible to produce a fine-diameter resin fiber. This is thought to be because the increase in the content of polyamide resin in the raw material resin lowers the melting point of the resin, shortening the time it takes for the resin to cool (solidify), making spinning difficult. In addition, the lowering of the melting point tends to make it difficult to produce uniform threads, making them difficult to handle. For this reason, it is preferable to set the amount of polyamide resin added to 3 parts by weight or less.

[0057] [Preparation of fibrous activated carbon from phenolic resin fibers] The phenolic resin fibers of each prototype and comparative example were carbonized and activated by a known method using a stationary electric furnace to obtain a desired activation degree, thereby obtaining fibrous activated carbon corresponding to each prototype and comparative example.

[0058] [Measurement items / Measurement method] For each prototype and comparative example, the BET specific surface area (m 2 The results are shown in Tables 3 and 4.

[0059] The BET specific surface area was determined by measuring the nitrogen adsorption isotherm at 77K using an automatic specific surface area / pore distribution measuring device "BELSORP-miniII" manufactured by Microtrack-Bel Corporation, and by the BET method (BET specific surface area).

[0060] [Tensile strength] The test was conducted in accordance with JIS L 1015 (2010), and the load at break (cN) was taken as the tensile strength.

[0061] [Table 3]

[0062] [Table 4]

[0063] [Results and Discussion] If the amount of polyamide resin contained in the raw material of activated carbon is too large, the polyamide resin is decomposed by heat during firing to produce activated carbon and does not remain in the fired product, which may result in a decrease in strength. Since there is no significant change in tensile strength in Prototype Examples 1 to 3 and 5 to 8 compared to Comparative Examples 1 and 2, by setting the content of polyamide resin to 1 to 3 parts by weight, it was possible to obtain a fine-diameter fibrous activated carbon that is easy to handle and is equivalent to conventional fibrous activated carbon.

[0064] In addition, since there is no significant change in the specific surface area of ​​Prototype Examples 1 to 3, 5 to 8 compared to Comparative Examples 1 and 2, it is understood that they have equivalent adsorption performance. In addition, since the fibrous activated carbon with a small fiber diameter has a large external surface area, the adsorption efficiency per unit weight is improved. [Industrial Applicability]

[0065] By adopting the method for producing polyamide resin-containing phenolic resin fibers of the present invention, it is possible to easily obtain resin fibers having a small diameter. In addition, by carbonizing and activating the resin fibers having a small diameter, it is possible to obtain fibrous activated carbon having a smaller diameter than that of the conventional method, which is useful as a new adsorbent to be used in filters and the like.

Claims

1. A method for producing phenolic resin fibers as a starting material for fibrous activated carbon, comprising the steps of: a raw material mixing process in which 1 to 3 parts by weight of polyamide resin is added to 100 parts by weight of phenol, melted, and then formaldehyde is added and mixed to prepare a raw material; a catalyst addition step of adding an acid catalyst to the raw material to obtain a catalyst-added raw material; a synthesis step of heating the catalyst-added raw material to prepare a polyamide resin-containing phenolic resin containing a polyamide resin; A spinning step of spinning the polyamide resin-containing phenolic resin to obtain resin fibers. A method for producing a polyamide resin-containing phenolic resin fiber.

2. 2. The method for producing a polyamide resin-containing phenolic resin fiber according to claim 1, wherein the resin fiber has a fineness of 5.0 (dtex) or less.

3. 3. The method for producing a polyamide resin-containing phenolic resin fiber according to claim 1, further comprising a fiber curing step of obtaining a cured resin fiber by immersing the resin fiber in a curing liquid containing an inorganic acid and formaldehyde after the spinning step.

4. 4. A method for producing an activated carbon adsorbent, comprising the step of carbonizing and activating the cured resin fibers obtained by the method for producing polyamide resin-containing phenolic resin fibers according to claim 3 to obtain an activated carbon adsorbent.

Citation Information

Patent Citations

  • JP1973077112A

  • JP1975031117A

  • Thin film magnetic head

    JP1977012814A

  • Original document depressor plate for copying

    JP1977050717A

  • Production of soft contact lens

    JP1979043268A