Polyurethane resin-forming composition for membrane sealant, and membrane sealant and membrane module using same

The use of an allophanate group-containing polyisocyanate prepolymer and castor oil polymerized polyol in the polyurethane resin-forming composition addresses high viscosity and elution issues, resulting in low-viscosity, castable resin for superior membrane sealing materials and modules.

JP7577919B2Active Publication Date: 2024-11-06TOSOH CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020008738
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-22
Publication Date
2024-11-06
Estimated Expiration
2040-01-22

AI Technical Summary

Technical Problem

Existing polyurethane resin-forming compositions for membrane sealing materials face issues with high viscosity, leading to filling defects during molding, and high elution of low-molecular reaction products and solvents, which affect the integrity and performance of membrane modules.

Method used

A polyurethane resin-forming composition comprising an allophanate group-containing polyisocyanate prepolymer and a curing agent, specifically using diphenylmethane diisocyanate and castor oil polymerized polyol, with a crosslinking group density of 0.65 mmol/g or more, to achieve low viscosity and reduced elution of low-molecular reaction products and solvents.

Benefits of technology

The composition results in a urethane resin with low viscosity and excellent castability, minimizing water and solvent elution, thereby enhancing the formation of high-quality membrane sealing materials and modules with improved mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577919000007
    Figure 0007577919000007
  • Figure 0007577919000001
    Figure 0007577919000001
  • Figure 0007577919000002
    Figure 0007577919000002
Patent Text Reader

Abstract

To provide a polyurethane resin formative composition for a film seal material which has low viscosity and is excellent in cast properties, is reduced in a water elution amount of a low molecular reaction product, and contributes to formation of a urethane resin reduced in a solvent elution amount of a molding, and a seal material and a film module using the formative composition.SOLUTION: A polyurethane resin formative composition for a film seal material contains an allophanate group-containing polyisocyanate prepolymer (A) and a curing agent (B), the allophanate group-containing polyisocyanate prepolymer (A) contains a reaction product of diphenylmethane diisocyanate (a1) and an active hydrogen-containing compound (a2), the curing agent (B) contains castor oil polymerization polyol (b1) containing a castor oil polymer, and a crosslinking group density is 0.65 mmol / g or more with respect to the total mass of the polyisocyanate prepolymer (A) and the curing agent (B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polyurethane resin-forming composition for a membrane sealant, and a membrane sealant and a membrane module using the same. [Background technology]

[0002] Among the hollow fiber membranes used in hollow fiber membrane modules, there is a glycerin-containing hollow fiber membrane in which a retention agent (glycerin) is used to maintain the pores of the membrane. However, in the case of the glycerin-containing hollow fiber membrane, when a polyurethane resin-forming composition containing diphenylmethane diisocyanate (hereinafter abbreviated as MDI) is used during casting, it is known that a low molecular weight reaction product between MDI and glycerin is generated, and this reaction product dissolves into the liquid present around the hollow fiber membrane.

[0003] Therefore, Patent Document 1 discloses a polyurethane resin-forming composition for a sealing material of a membrane module, which contains a polyisocyanate component (base) containing an isocyanate-terminated prepolymer obtained from a reaction product of MDI and castor oil, and a polyol component (curing agent). Furthermore, Patent Document 1 discloses that the amount of elution of the polyurethane resin obtained from the polyurethane resin-forming composition for a sealing material is reduced.

[0004] In addition, allophanate group-containing polyisocyanate prepolymers derived from MDI and monol have low viscosity, little precipitation of MDI at low temperatures, and are easy to handle, and are therefore useful and widely used in the fields of adhesives and sealing materials. Patent Document 2 discloses that an allophanate group-containing polyisocyanate prepolymer derived from MDI and polyether monol has a low viscosity, and that an elastomer obtained from the prepolymer has excellent mechanical properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-25383 [Patent Document 2] JP 2009-030059 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the composition disclosed in Patent Document 1 has a high viscosity of the base agent, and there is a demand for a lower viscosity. Therefore, the composition disclosed in Patent Document 1 has a problem that the initial viscosity of the mixed base agent and curing agent is high, which may cause filling defects during molding. Furthermore, the composition disclosed in Patent Document 2 has a problem in that a large amount of eluted material is eluted from the urethane resin, and it is desired to reduce the amount of eluted material. Therefore, one embodiment of the present disclosure is to provide a polyurethane resin-forming composition that contributes to the formation of a urethane resin that has low viscosity and excellent castability, and that reduces the amount of water elution of the low-molecular-weight reaction product of MDI and glycerin and the amount of solvent elution of the molded product, and a sealing material and a membrane module that use the forming composition. [Means for solving the problem]

[0007] The present disclosure includes the following embodiments. (1): An allophanate group-containing polyisocyanate prepolymer (A), A polyurethane resin-forming composition for a membrane sealant, comprising: The polyisocyanate prepolymer (A) is Diphenylmethane diisocyanate (a1), and an active hydrogen-containing compound (a2), The curing agent (B) contains a castor oil polymerized polyol (b1), The castor oil polymerized polyol (b1) contains a castor oil polymer, A polyurethane resin-forming composition for a membrane sealant, characterized in that the crosslinking group density is 0.65 mmol / g or more based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B). (2): An allophanate group-containing polyisocyanate prepolymer (A), A polyurethane resin-forming composition for a membrane sealant, comprising: The polyisocyanate prepolymer (A) is Diphenylmethane diisocyanate (a1), and an active hydrogen-containing compound (a2), The curing agent (B) contains a castor oil polymerized polyol (b1), The castor oil polymerized polyol (b1) contains a castor oil polymer, The polyurethane resin-forming composition for membrane sealing material, wherein the content of the castor oil polymer is 1% by mass or more and 35% by mass or less based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B). (3): A membrane sealant comprising a cured product of the polyurethane resin-forming composition for a membrane sealant according to (1) or (2) above. (4): A main body portion; A membrane, A membrane sealant that seals a gap between the main body and the membrane, A membrane module, wherein the membrane sealing material is the membrane sealing material described in (3) above. Effect of the Invention

[0008] According to one embodiment of the present disclosure, it is possible to provide a polyurethane resin-forming composition that contributes to the formation of a urethane resin that has low viscosity and excellent castability, and that reduces the amount of water elution of a low-molecular-weight reaction product of diphenylmethane diisocyanate and glycerin and the amount of solvent elution of a molded product, as well as a sealing material and a membrane module using the forming composition. [Brief description of the drawings]

[0009] [Figure 1]FIG. 1 is a conceptual diagram illustrating an example of a configuration of a membrane module according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Exemplary embodiments for carrying out the present invention are described in detail below.

[0011] [First embodiment of polyurethane resin-forming composition for membrane sealant] The polyurethane resin-forming composition for a membrane sealant according to one embodiment of the present disclosure comprises: An allophanate group-containing polyisocyanate prepolymer (A), A polyurethane resin-forming composition for a membrane sealant, comprising: The allophanate group-containing polyisocyanate prepolymer (A) is Diphenylmethane diisocyanate (a1), and an active hydrogen-containing compound (a2), The curing agent (B) contains a castor oil polymerized polyol (b1) containing a castor oil polymer, The crosslinking group density is 0.65 mmol / g or more based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B).

[0012] <Allophanate Group-Containing Polyisocyanate Prepolymer (A)> The allophanate group-containing polyisocyanate prepolymer (A) contains a reaction product of diphenylmethane diisocyanate (a1) and an active hydrogen-containing compound (a2).

[0013] Diphenylmethane diisocyanate (a1) As diphenylmethane diisocyanate (a1), any commonly available diphenylmethane diisocyanate (hereinafter also referred to as MDI) monomer can be used. The isomers of the MDI monomer are usually 0% by mass or more and 5% by mass or less of 2,2'-MDI, 0% by mass or more and 95% by mass or less of 2,4'-MDI, and 5% by mass or more and 100% by mass or less of 4,4'-MDI. As the MDI (a1), it is preferable to use the above-mentioned MDI in order to obtain an allophanate group-containing polyisocyanate prepolymer (A) with a lower viscosity. However, if a certain degree of high viscosity of the allophanate group-containing polyisocyanate prepolymer (A) is acceptable, polymethylene polyphenylene polyisocyanate (polymeric MDI) can also be used as the MDI (a1). In that case, the content of the polymethylene polyphenylene polyisocyanate in the isocyanate component used is preferably 0% by mass or more and 50% by mass or less. If it is 50% by mass or less, the viscosity is sufficiently low and the generation of insoluble matters can be more highly suppressed.

[0014] <<Active hydrogen-containing compound (a2)>> The active hydrogen-containing compound (a2) is not particularly limited as long as it is a compound containing active hydrogen. Examples of the active hydrogen-containing compound (a2) include monoalcohols, castor oil, castor oil-based modified polyols, low molecular weight polyols, polyether-based polyols, polyester-based polyols, polylactone-based polyols, polyolefin-based polyols, and the like. Furthermore, examples of the monoalcohols include aliphatic monoalcohols, aromatic monoalcohols, alicyclic monoalcohols, aromatic aliphatic monoalcohols, polyoxypropylene glycol monoalkyl ethers, and the like.

[0015] Examples of aliphatic monoalcohols include methanol, ethanol, 1- and 2-propanol, 1- and 2-butanol, 1-pentanol, 1-hexanol, 2-methyl-1-pentanol, 4-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 1-octanol, 2-octanol, 2-ethylhexanol, 3,5-dimethyl-1-hexanol, 2,2,4-trimethyl-1-pentanol, 1-nonanol, 2,6 aliphatic monoalcohols such as 1-dimethyl-4-heptanol, 1-decanol, 1-undecanol, 1-dodecanol, 1-tridecanol, 1-tetradecanol, 1-pentadecanol, 1-hexadecanol, 1-heptadecanol, 1-octadecanol, 1-nonadecanol, 1-eicosanol, 1-hexacosanol, 1-heptatricontanol, 1-oleyl alcohol, and 2-octyldodecanol, and mixtures thereof. The number average molecular weight of the aliphatic monoalcohol is preferably from 32 to 1500, and more preferably from 100 to 1000. When the molecular weight is within this range, the polyurethane resin has even better moldability and adhesive strength.

[0016] Examples of aromatic monoalcohols include phenol and cresol.

[0017] Examples of the alicyclic monoalcohol include cyclohexanol and methylcyclohexanol.

[0018] An example of the aromatic aliphatic monoalcohol is benzyl alcohol.

[0019] Examples of the polyoxypropylene glycol monoalkyl ether include reaction products of the above-mentioned aliphatic monoalcohols with polyoxypropylene glycol, such as polyoxypropylene methyl ether, polyoxypropylene ethyl ether, polyoxypropylene butyl ether, polyoxypropylene-2-ethylhexyl ether, polyoxypropylene oleyl ether, polyoxypropylene-2-octyldodecaether, and mixtures thereof. The number average molecular weight of the polyoxypropylene glycol monoalkyl ether is preferably 90 or more and 1500 or less. From the viewpoint of achieving even better moldability and adhesive strength of the polyurethane resin, the number average molecular weight is more preferably 150 or more and 1000 or less.

[0020] The castor oil-based modified polyol includes linear or branched castor oil-based modified polyols obtained by reacting castor oil or castor oil fatty acid with at least one polyol selected from the group consisting of low molecular weight polyols and polyether polyols.Specific examples include diglycerides and monoglycerides of castor oil fatty acid; mono-, di-, and triesters of castor oil fatty acid and trimethylolalkane; mono-, di-, and triesters of castor oil fatty acid and polypropylene glycol; and the like. The main component of castor oil is triglyceride of ricinoleic acid, and castor oil includes hydrogenated castor oil. The main component of castor oil fatty acid is ricinoleic acid, and castor oil fatty acid includes hydrogenated castor oil fatty acid.

[0021] Examples of the trimethylolalkane include trimethylolmethane, trimethylolethane, trimethylolpropane, trimethylolbutane, trimethylolpentane, trimethylolhexane, trimethylolheptane, trimethyloloctane, trimethylolnonane, and trimethyloldecane.

[0022] The number average molecular weight of the castor oil-based modified polyol is preferably from 400 to 3000, more preferably from 500 to 2500. By using a castor oil-based modified polyol having a number average molecular weight of from 400 to 3000, it is possible to form a cured resin having even better physical properties, particularly mechanical properties, required for a membrane sealing material.

[0023] The average hydroxyl value of castor oil and castor oil-based modified polyol is preferably 20 mgKOH / g or more and 300 mgKOH / g or less, more preferably 40 mgKOH / g or more and 250 mgKOH / g or less. By using a castor oil-based modified polyol having an average hydroxyl value of 20 mgKOH / g or more and 300 mgKOH / g or less, it is possible to form a cured resin having better physical properties, particularly mechanical properties, required for a membrane sealant. Furthermore, it is possible to improve the productivity of the membrane sealant and, in turn, the productivity of the hollow fiber membrane module.

[0024] Examples of low molecular weight polyols include dihydric polyols such as ethylene glycol, diethylene glycol, propylene glycol, 1,2-, 1,3- or 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, neopentyl glycol, and hydrogenated bisphenol A, and trihydric to octahydric polyols such as glycerin, trimethylolpropane, hexanetriol, pentaerythritol, sorbitol, and sucrose. The number average molecular weight of the low molecular weight polyol is preferably 50 or more and 200 or less.

[0025] Examples of polyether-based polyols include alkylene oxide (alkylene oxide having 2 to 8 carbon atoms, such as ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above-mentioned low molecular weight polyols, and ring-opening polymers of alkylene oxides, specifically polypropylene glycol, polyethylene glycol, polytetramethylene ether glycol, or copolymers of ethylene oxide and propylene oxide, etc. The number-average molecular weight of the polyether-based polyol is preferably 200 to 7000, more preferably 500 to 5000, from the viewpoint of further excellent moldability during the production of the membrane sealing material.

[0026] The polyester polyol may be, for example, a polyester polyol obtained by condensation polymerization of a polycarboxylic acid and a polyol. Examples of polycarboxylic acids used in the polyester polyols include adipic acid, azelaic acid, dodecanedioic acid, maleic acid, fumaric acid, itaconic acid, dimerized linoleic acid, phthalic acid, isophthalic acid, terephthalic acid, and other aliphatic saturated and unsaturated polycarboxylic acids, as well as aromatic polycarboxylic acids. Examples of the polyol used in the polyester polyol include the low molecular weight polyols and polyether polyols described above.

[0027] The number average molecular weight of the polyester polyol is preferably from 200 to 5000, more preferably from 500 to 3000. By using a polyester polyol having a number average molecular weight of from 200 to 5000, the molding processability during formation of the membrane sealing material is particularly excellent.

[0028] Examples of polylactone polyols include polyols obtained by addition polymerization of ε-caprolactone, α-methyl-ε-caprolactone, ε-methyl-ε-caprolactone, β-methyl-δ-valerolactone, etc., to a glycol or triol polymerization initiator in the presence of a catalyst such as an organometallic compound, a metal chelate compound, or a fatty acid metal acyl compound. The number-average molecular weight of the polylactone polyol is preferably 200 to 5000, more preferably 500 to 3000. By using a polylactone polyol having a number-average molecular weight of 200 to 5000, the molding processability during the formation of a membrane sealant is particularly excellent.

[0029] Examples of polyolefin polyols include polybutadiene polyols in which hydroxyl groups have been introduced at the ends of polybutadiene or copolymers of butadiene and styrene or acrylonitrile.Other examples include polyether ester polyols obtained by addition reaction of alkylene oxides, such as ethylene oxide and propylene oxide, to polyesters having terminal carboxyl groups and hydroxyl groups.

[0030] Among these, as the active hydrogen-containing compound (a2), in consideration of compatibility with the curing agent (B), aliphatic alcohols having 10 or more carbon atoms, castor oil or castor oil-based modified polyols are preferred.

[0031] <<Production method of allophanate group-containing polyisocyanate prepolymer (A)>> The allophanate group-containing polyisocyanate prepolymer (A) is preferably obtained, for example, by subjecting diphenylmethane diisocyanate (a1) to a urethane reaction with an active hydrogen-containing compound (a2), followed by adding a predetermined amount of catalyst (a3) ​​to convert the resulting product to an allophanate, and then terminating the reaction with a catalyst poison (a4).

[0032] <<Catalyst (a3)>> Examples of the catalyst (a3) ​​include zinc acetylacetonate; metal carboxylates of zinc, lead, tin, copper, cobalt, or the like with carboxylic acids, and mixtures thereof; tertiary amines, tertiary amino alcohols, quaternary ammonium salts, and mixtures thereof; and the like. The amount of catalyst (a3) ​​added is preferably in the range of 1 ppm to 500 ppm, more preferably 5 ppm to 300 ppm, based on the total mass of diphenylmethane diisocyanate (a1) and active hydrogen-containing compound (a2). At 1 ppm or more, the reaction becomes more rapid, and at 500 ppm or less, coloration of the prepolymer is more effectively suppressed, which is preferable.

[0033] <<Active methylene compounds>> In the present disclosure, in the allophanation reaction using a tertiary amine or a quaternary ammonium salt, if the reaction is rapid and difficult to control, it is effective to add at least one selected from the group consisting of carboxylic acid amides, sulfonic acid amides, and active methylene compounds represented by formula (1).

[0034] [ka]

[0035] During the ceremony, R 1 is any one selected from the group consisting of a hydrogen atom, an alkyl group, an alkenyl group, a cycloalkyl group, an arylalkyl group, and an aryl group, R 2 and R 3 are each independently any one selected from the group consisting of a hydroxyl group, an alkyl group, an alkenyl group, a cycloalkyl group, an arylalkyl group, an aryl group, an oxyalkyl group, an oxyalkenyl group, an oxycycloalkyl group, an oxyarylalkyl group, and an oxyaryl group.

[0036] Examples of carboxylic acid amides include formamide, acetamide, propionic acid amide, butanoic acid amide, isobutanoic acid amide, hexanoic acid amide, octanoic acid amide, 2-ethylhexanoic acid amide, oleic acid amide, stearic acid amide, benzamide, 2-phenylacetamide, 4-methylbenzamide, 2-aminobenzamide, 3-aminobenzamide, 4-aminobenzamide, and mixtures thereof.

[0037] Examples of sulfonamides include methylsulfonamide, butylsulfonamide, t-butylsulfonamide, phenylsulfonamide, benzylsulfonamide, o-toluylsulfonamide, p-toluylsulfonamide, 3-aminophenylsulfonamide, 4-aminophenylsulfonamide, and mixtures thereof.

[0038] Specific examples of the active methylene compound represented by formula (1) include acetylacetone, 3-methyl-2,4-pentanedione, 3-ethyl-2,4-pentanedione, 3,5-heptanedione, 3,5-heptanedione, 6-methyl-2,4-heptanedione, methyl acetoacetate, ethyl acetoacetate, methyl 3-oxopentanoate, malonic acid, dimethyl malonate, diethyl malonate, etc. The active methylene compound may be a mixture of two or more of these.

[0039] In addition, at least one member selected from the group consisting of the above-mentioned carboxylic acid amides, sulfonic acid amides, and the active methylene compound represented by the above-mentioned formula (1) is preferably added within a period ranging from immediately before the addition of the catalyst to 30 minutes after the addition of the catalyst.

[0040] The higher the temperature at which allophanatization is carried out, the higher the production ratio of allophanate groups and the easier it is to achieve a low viscosity. However, side reactions such as uretdione formation and carbodiimidization are more likely to occur. Also, in the reaction at a low temperature, the amount of isocyanurate groups produced increases and the viscosity becomes high. Therefore, the reaction temperature is preferably 20°C or higher and 200°C or lower. To suppress the production ratio of isocyanurate groups to 20 mol% or less and achieve a lower viscosity, it is preferably 60°C or higher and 160°C or lower.

[0041] <<Catalyst poison (a4)>> As the catalyst poison (a4), an acidic substance is preferred. Examples of the catalyst poison (a4) include hydrogen chloride anhydride, sulfuric acid, phosphoric acid, monoalkyl sulfate ester, alkyl sulfonic acid, alkylbenzene sulfonic acid, mono- or dialkyl phosphate ester, benzoyl chloride, and Lewis acid. The addition amount of the catalyst poison (a4) is preferably added in an equivalent amount or more based on the number of moles of the catalyst (a3), and more preferably added in an amount of 1.0 to 1.5 times the molar equivalent of the number of moles of the catalyst (a3).

[0042] <<Content of MDI monomer>> The content of the MDI monomer is preferably 25% by mass or less based on the total amount of the polyurethane resin-forming composition for the film sealing material in order to further reduce the low molecular weight reaction product of MDI and glycerin.

[0043] <<Reaction temperature>> The urethanization reaction preferably occurs in the temperature range of 40°C or higher and 80°C or lower until the target NCO content is reached. When the temperature is 40°C or higher, the crystal precipitation of the monomer MDI can be better suppressed, and when the temperature is 80°C or lower, the formation of by-products can be more suppressed.

[0044] The allophanatization reaction preferably occurs in the temperature range of 90°C or higher and 130°C or lower until the target NCO content is reached. At 90°C or higher, the reaction becomes faster, and at 130°C or lower, the formation of by-products can be more suppressed.

[0045] <<Content of isocyanate groups>> The content of isocyanate groups in the polyisocyanate prepolymer (A) is preferably from 13.0 to 21.0% by mass, more preferably from 13.5 to 20.5% by mass, and particularly preferably from 14.0 to 20.0% by mass. Within these ranges, the polyurethane resin is further excellent in moldability and adhesive strength.

[0046] <Hardening agent (B)> The curing agent (B) contains a castor oil polymerized polyol (b1). In addition, the curing agent (B) is Castor oil polymerized polyol (b1), and at least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyols. Furthermore, the curing agent (B) Castor oil polymerized polyol (b1), At least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyols; and a hydroxyl group-containing amine compound (b3) other than the castor oil polymerized polyol (b1) and the polyol (b2); The content of the hydroxyl group-containing amine compound (b3) in the curing agent (B) is more preferably 35 mass % or less.

[0047] <<Castor oil polymerized polyol (b1)>> The castor oil polymerized polyol (b1) contains a castor oil polymer. By containing the castor oil polymerized polyol (b1), excellent effects are exhibited in terms of improving processability during molding and suppressing elution.

[0048] The content of the castor oil polymer is preferably 1.0% by mass or more and 35.0% by mass or less, more preferably 2.0% by mass or more and 25.0% by mass or less, and particularly preferably 3.0% by mass or more and 15.0% by mass or less, based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B). Within these ranges, the polyurethane resin is further excellent in moldability and reduction of the amount of elution.

[0049] The castor oil polymerized polyol (b1) may contain castor oil polymers and castor oil (non-polymerized). In this case, the content of castor oil polymers in the castor oil polymerized polyol (b1) can be calculated by regarding those having a molecular weight of 1500 or more as castor oil polymers as determined by GPC (Gel Permeation Chromatography). However, the method of calculating the content of castor oil polymers is not limited to this, and any method may be used as long as it can accurately distinguish between castor oil polymers and castor oil (non-polymerized).

[0050] <<At least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyols>> The castor oil and castor oil-based modified polyol (b2) are not particularly limited. Castor oil is simply castor oil. Examples of the castor oil modified polyol include the same castor oil modified polyols as those exemplified as the active hydrogen-containing compound (a2) described above.

[0051] <<Hydroxyl-containing amine compounds (b3)>> The hydroxyl-containing amine compound (b3) is a hydroxyl-containing amine compound other than the castor oil polymerized polyol (b1) and at least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyol. That is, the hydroxyl-containing amine compound (b3) is a hydroxyl-containing amine compound that does not fall under either the castor oil polymerized polyol (b1) or the polyol (b2).

[0052] Examples of the hydroxyl group-containing amine compound (b3) include alkyldiethanolamines (e.g., linear or branched butyldiethanolamine, hexyldiethanolamine, octyldiethanolamine, lauryldiethanolamine, myristyldiethanolamine, cetyldiethanolamine, stearyldiethanolamine, etc.), low molecular weight polyamines, low molecular weight amino alcohols (e.g., oxyalkylated derivatives of amino compounds such as N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine, N,N,N',N'-tetrakis[2-hydroxyethyl]ethylenediamine, which are adducts of propylene oxide or ethylene oxide of ethylenediamine; mono-, di-, triethanolamine; N-methyl-N,N'-diethanolamine, etc.), and other amine compounds such as amino alcohol derivatives. Among these, preferred are propylene oxide or ethylene oxide adducts of amino compounds such as ethylenediamine, and most preferred is N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine. The use of N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine provides further benefits such as improved processability during molding and reduced amount of elution.

[0053] In addition, the content of the hydroxyl-containing amine compound (b3) in the curing agent (B) is preferably 35% by mass or less, more preferably 5% by mass or more and 34% by mass or less, and particularly preferably 10% by mass or more and 33% by mass or less. When the content of the hydroxyl-containing amine compound (b3) in the curing agent (B) is 5% by mass or more, the hydroxyl-containing amine compound (b3) exhibits a better function of curing promotion and exhibits a further effect. When the ratio of the hydroxyl-containing amine compound (b3) in the curing agent (B) is 35% by mass or less, the reactivity is further suppressed from becoming too high, the workability is further improved, the filling property is ensured, and the hardness of the obtained membrane sealant is further suppressed from becoming too high.

[0054] <<Active hydrogen-containing compound (b4)>> The curing agent (B) may contain an active hydrogen-containing compound (hereinafter referred to as "active hydrogen-containing compound (b4)") other than the castor oil polymerized polyol (b1), the polyol (b2), and the hydroxyl group-containing amine compound (b3). As the active hydrogen-containing compound (b4), the various polyols listed as the active hydrogen-containing compound (a2) can be used.

[0055] In the curing agent (B), the mass ratio (Mb2) / (Mb4) of the content Mb2 of at least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyols to the content Mb4 of the active hydrogen-containing compound (b4) is preferably 50 / 50 or more and 100 / 0 or less, and particularly preferably 100 / 0. That is, it is particularly preferable that the curing agent (B) consists of only castor oil polymerized polyol (b1) and polyol (b2), or only castor oil polymerized polyol (b1), polyol (b2), and hydroxyl group-containing amine compound (b3).

[0056] Furthermore, when the hydroxyl-containing amine compound (b3) is taken into consideration, when the content of the castor oil polymerized polyol (b1) is Mb1 and the content of the hydroxyl-containing amine compound (b3) is Mb3, the mass ratio (Mb3) / {(Mb1)+(Mb2)} is preferably 5 / 95 or more and 35 / 65 or less, and from the viewpoint of curability and filling ability, more preferably 10 / 90 or more and 33 / 67 or less.

[0057] The hydroxyl value of the curing agent (B) is preferably 50 mgKOH / g or more and 1000 mgKOH / g or less, and more preferably 75 mgKOH / g or more and 750 mgKOH / g or less from the viewpoint of easy handling of the curing agent (B). From the viewpoint of excellent moldability and adhesive strength of the polyurethane resin, the hydroxyl value of the curing agent (B) is most preferably 100 mgKOH / g or more and 500 mgKOH / g or less.

[0058] The viscosity of the curing agent (B) at 25°C is preferably 100 mPa·s or more and 6000 mPa·s or less, and from the viewpoint of easy handling of the curing agent (B), more preferably 150 mPa·s or more and 4000 mPa·s or less. From the viewpoint of excellent moldability of the polyurethane resin, the viscosity of the curing agent (B) at 25°C is most preferably 200 mPa·s or more and 2000 mPa·s or less.

[0059] <Crosslinking group density> In order to suppress the amount of dissolution into the solvent, the crosslinking group density of the polyurethane resin-forming composition for membrane sealing material is preferably 0.65 mmol / g or more, more preferably 0.70 mmol / g or more, and particularly preferably 0.75 mmol / g or more and 1.20 or less, based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B). When the crosslinking group density is 1.20 or less, the molding processability becomes better.

[0060] The crosslinking group density means the total content density of groups capable of forming crosslinks and groups which have already formed crosslinks. Therefore, in the case of a trifunctional polyol (e.g., glycerin), one hydroxyl group in one molecule forms a crosslink, and the remaining two hydroxyl groups do not contribute to the crosslink, so in this case, the number of crosslinking groups is one. That is, in the case of a polyurethane resin-forming composition for a membrane sealant containing a trifunctional polyol, the content of crosslinking groups derived from the trifunctional polyol is synonymous with the content of the trifunctional polyol, since the trifunctional polyol has one crosslinking group.

[0061] [Second embodiment of polyurethane resin-forming composition for membrane sealant] Another embodiment of the present invention is a copolymer of an allophanate group-containing polyisocyanate prepolymer (A) and A polyurethane resin-forming composition for a membrane sealant, comprising: The polyisocyanate prepolymer (A) is Diphenylmethane diisocyanate (a1), and an active hydrogen-containing compound (a2), The curing agent (B) contains a castor oil polymerized polyol (b1), The castor oil polymerized polyol (b1) contains a castor oil polymer, The content of the castor oil polymer is from 1% by mass to 35% by mass based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B). Since each component is similar to that of the first embodiment described above, a description thereof will be omitted.

[0062] According to each embodiment of the present disclosure, it is possible to provide a polyurethane resin-forming composition that contributes to the formation of a urethane resin having low viscosity and excellent castability, as well as a reduced amount of water elution of a low-molecular-weight reaction product of diphenylmethane diisocyanate and glycerin and a reduced amount of solvent elution of a molded product, and a membrane sealing material and a membrane module using the forming composition.

[0063] <Membrane sealant> A membrane sealant according to one embodiment of the present disclosure includes a cured product of the above-mentioned polyurethane resin-forming composition for a membrane sealant. The membrane sealant can be suitably formed by reacting and curing the isocyanate component constituting the polyisocyanate prepolymer (A) with the polyol component constituting the curing agent (B) under temperature conditions of 0° C. or higher and 100° C. or lower, preferably 20° C. or higher and 80° C. or lower, and more preferably 30° C. or higher and 60° C. or lower. The gelation time of the membrane sealant can be shortened by molding in a high temperature range, but molding shrinkage is likely to occur, so the reaction temperature can be lowered by adding a catalyst to suppress molding shrinkage.

[0064] <Membrane module> The membrane module according to one embodiment of the present disclosure comprises: A main body portion, A membrane, A membrane sealant that seals a gap between the main body and the membrane, The membrane sealant is the membrane sealant described above.

[0065] Next, a membrane module according to an embodiment of the present disclosure will be described in more detail with reference to the drawings. FIG. 1 is a conceptual diagram showing an example of the configuration of a membrane module according to an embodiment of the present disclosure. The membrane module (hollow fiber membrane module) 100 shown in Fig. 1 includes a housing (main body) 11, the inside of which is filled with a plurality of hollow fiber membranes (membranes) 13. For example, in the case of a hollow fiber membrane module used as a dialyzer, several thousand to several tens of thousands of hollow fiber membranes are filled.

[0066] The housing 11 has a cylindrical shape. A membrane sealant 19 is provided at each of both ends (the left and right ends in FIG. 1 ) inside the housing 11. The membrane sealant fills and seals the gaps between the hollow fiber membranes 13 and the gaps between the hollow fiber membranes 13 and the inner wall of the housing 11, and also binds the multiple hollow fiber membranes 13 together.

[0067] In addition, a first fluid inlet 15 and a first fluid outlet 17 are provided on the side of the housing 11, and a first fluid (gas or liquid) flows in and out of the housing 11 through these. The first fluid that flows in from the first fluid inlet 15 passes through the gaps (outside the hollow fiber membranes) while contacting the multiple hollow fiber membranes 13 filled in the housing 11, and is discharged from the first fluid outlet 17. Since there is no membrane seal material 19 inside the hollow fiber membranes 13, a second fluid (gas or liquid) flows in and out of the hollow fiber membranes 13 through a second inlet (one end side) and a second outlet (the other end side) provided in a cap member (not shown). Then, the first fluid and the second fluid come into contact with each other through the hollow fiber membranes 13, and mass transfer occurs from one fluid to the other fluid (or from the other fluid to the one fluid). For example, in the case of a hollow fiber membrane type dialyzer, waste products and excess water in the blood are transferred to the dialysate when the dialysate comes into contact with the blood.

[0068] The membrane module 100 shown in FIG. 1 includes a plurality of hollow fiber membranes 13, and the membrane sealant 19 seals the gaps at both ends of the membranes, but the membrane module according to the present embodiment is not limited to such a configuration. For example, it may be a single membrane or a plurality of membranes having various shapes such as a flat membrane or a spiral membrane. The membrane sealant is not limited to a configuration provided at both ends of the membrane, but may be provided only on a part of the membrane (one end if the membrane is hollow fiber-shaped), or may be provided on all ends of the membrane, for example, all outer edges of a flat membrane. Furthermore, the sealant may be provided on a part of the membrane other than the ends to seal it. The housing 11 of the membrane module 100 shown in FIG. 1 has a cylindrical shape, but may be any shape other than a cylindrical shape.

[0069] The membrane module 100 seals the gaps between the hollow fiber membranes 13 at the end of a bundle of multiple hollow fiber membranes 13 with the above-mentioned polyurethane resin forming composition for membrane sealing material, and hardens the composition to form the above-mentioned membrane sealing material (the gaps between the hollow fiber membranes are sealed by the membrane sealing material).

[0070] The membrane module according to an embodiment of the present disclosure can be suitably used as a medical module or a module for water treatment, since the amount of elution is effectively reduced. Specific examples of the membrane module include a plasma separator, an artificial lung, an artificial kidney, an artificial liver, and a water treatment device for home or industrial use. EXAMPLES

[0071] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention should not be construed as being limited in any way by these examples. In the following, "%" means "% by mass" unless otherwise specified.

[0072] The following components were used in the examples and comparative examples. [Polyisocyanate prepolymer (A)] a1-1; 4,4'-MDI (Millionate MT, manufactured by Tosoh Corporation) Isocyanate group content = 33.6%) a1-2: A mixture of 2,4'-MDI and 4,4'-MDI (manufactured by Tosoh Corporation) Millionate NM, isocyanate group content = 33.6%) a1-3: Carbodiimide modified 4,4'-MDI (Tosoh Corporation) Millionate MTL-C, isocyanate group content = 28.6%, Crosslinking group density=0.45mmol / g) a2-1: Castor oil fatty acid methyl ester (COFA-MD, manufactured by Ito Oil Mills, OHV=160mgKOH / g) a2-2: Polypropylene glycol (ADEKA PP-1000, OHV=111mgKOH / g) a2-3: Isotridecanol (KH Neochem, OHV=275mgKOH / g) a2-4; 2-Octyldodecanol (Kao Corporation, Kalcol 200GD, Hydroxyl value = 185mgKOH / g) · a2-5; Castor oil (URIC H-30 manufactured by Ito Oil Co., Ltd., OHV=160mgKOH / g, viscosity (25℃)=690mPa·s, Content of castor oil polymers having a number average molecular weight of 1500 or more: 1% or less; Crosslinking group density=0.74mmol / g) A3-1: Zinc acetylacetonate (Tokyo Chemical Industry Co., Ltd.) a3-2;2-[{2-(dimethylamino)ethyl}methylamino]ethanol (Tosoh Corporation, product name: TOYOCAT RX5) Active methylene compounds: Diethyl malonate (Tokyo Chemical Industry Co., Ltd.) a4: Benzoyl chloride (Tokyo Chemical Industry Co., Ltd.)

[0073] [Hardening agent (B)] · b1-1; Castor oil polymer (Ito Oil Polycaster #30, OHV=155mgKOH / g, viscosity (25℃)=4800mPa·s, Content of castor oil polymer with number average molecular weight of 1500 or more: approx. 54% Crosslinking group density=1.84mmol / g) b2-1: Partially dehydrated castor oil (URIC H-41, manufactured by Ito Oil Mills, OHV=120mgKOH / g, crosslinking group density=0mmol / g) b3-1;N,N,N',N'-Tetrakis[2-hydroxypropyl]ethylenediamine (ADEKA EDP-300, OHV=760mgKOH / g, Viscosity (25℃) = 50000mPa s, crosslinking group density = 2.63mmol / g) b3-2; N-lauryldiethanolamine (Amit 102, manufactured by Kao Corporation, OHV = 394 mg KOH / g, Viscosity at 25°C = 100 mPa s, Crosslinking group density=0mmol / g) In the Production Examples, Examples, and Comparative Examples, the "predetermined amount" refers to the composition amount shown in Tables 1 and 2.

[0074] [Crosslinking group density calculation method] The crosslinking group densities shown in Tables 1 to 4 were calculated using the following formula from the number of functional groups and hydroxyl value disclosed by each raw material manufacturer and the number average molecular weight obtained by GPC measurement. The GPC measurement was performed in accordance with the <GPC measurement conditions for curing agent> described later.

[0075]

number

[0076] [Manufacturing Examples 1 to 8] (Production Example 1: Production of Base Agent (A-1)) A 2-liter four-neck flask was charged with 193 g of a1-1 and 450 g of a1-2, and the temperature was adjusted to 50°C while stirring under a nitrogen stream. Next, 269 g of a2-1 and 88 g of a2-2 were added while stirring, and the temperature was raised to 90°C after the heat generated by the urethane reaction had subsided. When the internal temperature stabilized at 90°C, 0.1 g of catalyst a3-1 was added and the reaction was carried out at 90°C for 4 hours, and 0.14 g of catalyst poison a4 was added to stop the reaction, yielding an isocyanate-terminated prepolymer. Hereinafter, this isocyanate-terminated prepolymer will be referred to as "main agent (A-1)". In main agent (A-1), the isocyanate group (NCO) content in the obtained isocyanate-terminated prepolymer was 13.5% by mass, and the viscosity at 25°C was 3330 mPa·s.

[0077] (Manufacturing Examples 2, 4-6) The isocyanate component and polyol component were changed to the compositions shown in Table 1, and prepolymers were synthesized in the same manner as in Production Example 1. All prepolymers were obtained as pale yellow transparent liquids with low viscosity. Hereinafter, these prepolymers will be referred to as main components (A-2), (A-4) to (A-6). The properties of main components (A-2), (A-4) to (A-6) are shown in Table 1.

[0078] [Production Example 3] (Production Example 3: Production of Base Agent (A-3)) 231g of a1-1 and 538g of a1-2 were added to a 2-liter four-neck flask, and the temperature was adjusted to 50°C while stirring under a nitrogen stream. Next, 231g of a2-3 was added while stirring, and the temperature was raised to 110°C after the heat generation from the urethane reaction subsided. When the internal temperature stabilized at 110°C, a specific amount of an active methylene compound and a catalyst a3-2 were added in that order to start the allophanate reaction. The reaction was followed while sampling the internal liquid and measuring the NCO content, and when the NCO content was predicted to be 16.1%, a specific amount of catalyst poison a4 was added to stop the reaction, and a polyisocyanate composition containing an allophanate modified product was obtained. Hereinafter, this polyisocyanate composition is referred to as the main agent (A-3). The main agent (A-3) was a pale yellow transparent liquid with a viscosity of 3630mPa·s at 25°C.

[0079] (Production Example 7: Production of Base Agent (A-7)) 300g of a1-1 and 300g of a1-2 were added to a 1-liter four-neck flask, and the temperature was adjusted to 50°C while stirring under a nitrogen stream. Next, 400g of a2-5 was added while stirring, and after the heat generated by the urethane reaction had subsided, the reaction was carried out at 75°C for 3 hours to obtain a prepolymer. Hereafter, this prepolymer will be referred to as the main agent (A-5). The main agent (A-5) was a pale yellow, transparent liquid with a viscosity of 3750mPa·s at 25°C. Its properties are shown in Table 1.

[0080] [Production Example 8: Production of Base Agent (A-8)] a1-3 (a carbodiimide modified product of 4,4'-MDI, Millionate MTL-C manufactured by Tosoh Corporation) is used as the base material (A-8). The properties of the base material (A-8) are shown in Table 1.

[0081] [Table 1]

[0082] [Preparation Examples 1 to 12 of Curing Agent (B)] The raw materials b1, b2, b3, and a2 were charged according to the compounding ratios shown in Table 2, and then stirred and mixed uniformly to obtain curing agents (B-1) to (B-12). The properties of the curing agents (B-1) to (B-12) are shown in Table 2.

[0083] [Table 2]

[0084] [Examples 1 to 10, Comparative Examples 1 to 9] In Examples 1 to 10 and Comparative Examples 1 to 9, urethane resin compositions having the formulations shown in Tables 3 and 4 were molded. The values ​​shown in Tables 3 and 4 were calculated from the following test results.

[0085] [NCO content measurement] In the main components (A-1) to (A-8) shown in Table 1, the NCO content was measured in accordance with JIS K1603-1:2007.

[0086] [Measurement of MDI monomer content] In the main components (A-1) to (A-8) shown in Table 1, the MDI monomer content (mass %) was determined by GPC measurement under the following conditions and method.

[0087] <GPC measurement conditions for isocyanate prepolymer> (1) Measuring device: "HLC-8120 (product name)" (manufactured by Tosoh Corporation) (2) Column temperature: 40°C (3) Detector: RI (refractive index) (4) Column: Measurements were performed using columns packed with three types of packing materials, TSKgel G3000HXL, TSKgel G2000HXL, and TSKgel G1000HXL (all product names, manufactured by Tosoh Corporation), connected in series. (5) Eluent: tetrahydrofuran (THF) (flow rate: 1 mL / min., 40° C.) (6) Calibration curve: A calibration curve was obtained using the following grades of polystyrene (TSK standard POLYSTYRENE). F-2 (1.81 × 10 4 )F-1(1.02×10 4 )A-5000(5.97×10 3 )A-2500(2.63×10 3 )A-500(Mw=6.82×10 2 , 5.78×10 2 , 4.74××10 2 , 3.70×10 2 , 2.66×10 2 ) Toluene (Mw=92) (7) Sample: 0.05 g of sample in 10 mL of THF

[0088] <Measurement method> First, a calibration curve was obtained from a chart obtained by detecting the refractive index difference using polystyrene as a standard substance. Next, for each sample, the mass percentage of the peak near the peak top molecular weight (number average molecular weight) of 230, which indicates the MDI monomer, was calculated from the chart obtained by detecting the refractive index difference based on the same calibration curve. The obtained value was the content (%) of the MDI monomer.

[0089] [Castor oil polymer content measurement] In the curing agents (B-1) to (B-11) shown in Table 2, the castor oil polymer content (mass%) was determined by GPC measurement under the following conditions and method.

[0090] <GPC measurement conditions for curing agent> (1) Measuring device: "HLC-8120 (product name)" (manufactured by Tosoh Corporation) (2) Column: Four columns packed with two columns of TSKgel G2000HXL and two columns of TSKgel G3000HXL (both trade names, manufactured by Tosoh Corporation) were connected in series. (3) Column temperature: 40°C (4) Detector: RI (refractive index) (5) Eluent: tetrahydrofuran (THF) (flow rate: 1 mL / min., 40° C.) (6) Calibration curve: A calibration curve was obtained using trifunctional polypropylene polyols having the following trade names (all manufactured by Sanyo Chemical Industries, Ltd.). "Sannix GP-250" (number average molecular weight = 250) "Sannix GP-400" (number average molecular weight = 400) "Sannix GP-600" (number average molecular weight = 600) "Sannix GP-1000" (number average molecular weight = 1000) "Sannix GP-3000" (number average molecular weight = 3000) "Sannix GP-4000" (number average molecular weight = 4000) "Sannix GP-5000" (number average molecular weight = 5000) (7) Sample solution: 0.05 g of sample in 10 mL of THF

[0091] <Measurement method> First, a calibration curve was obtained from a chart obtained by detecting the difference in refractive index using polystyrene as a standard substance. Next, for each sample, the mass% of the peak near the peak top molecular weight of 1000, which indicates refined castor oil, was calculated from the chart obtained by detecting the difference in refractive index based on the same calibration curve. Peaks other than refined castor oil have molecular weights of 1500 or more, and these peaks of molecular weights of 1500 or more were determined as peaks of castor oil polymers. In other words, the mass% of the mass other than that of refined castor oil was calculated as the mass% of castor oil polymers.

[0092] [Preparation of samples for methanol extraction test] (Examples 1 to 10, Comparative Examples 1 to 9) The base materials (A-1) to (A-8) and curing agents (B-1) to (B-11) were used in the combinations shown in Tables 3 and 4. Under conditions of a liquid temperature of 25°C or 45°C and an isocyanate group / active hydrogen group ratio of 1.00 or 1.05 (molar ratio), 60g of the base material and then 40g of the curing agent were quickly weighed into a 500ml polycup. The mixture was mixed with a spatula for 30 seconds and vacuum degassed at 50mmHg for 60 seconds. After degassing, the mixture was spread on a release paper to form a sheet with a thickness of 1mm, and left to stand in a thermostatic chamber at 45°C for 2 days.

[0093] [Methanol extraction test] The values ​​of low-molecular-weight eluted substances of the cured resin materials obtained in Examples 1 to 10 and Comparative Examples 1 to 9 were measured by the following method. First, the methanol extraction measurement samples obtained in each Example and Comparative Example were cut into 10 mm squares. Next, 20 g of the cut sample and 200 g of methanol were placed in a 500 ml sample bottle, which was then sealed and shaken at 25°C for 24 hours. After shaking, the bottle was further filtered, and the extract was collected in a 300 ml eggplant flask and evaporated to dryness. The methanol extraction rate was then calculated using the following formula. Methanol extraction rate (%) = {mass of eggplant flask after evaporation to dryness (g) - empty mass of eggplant flask (g)} / sample mass (g) x 100 The methanol extraction rate is preferably less than 1.0%.

[0094] [Creating samples for low molecular weight dissolution tests] (Examples 1 to 10, Comparative Examples 1 to 9) The main agent (A-1) to (A-8) and the curing agent (B-1) to (B-12) were mixed in the combinations shown in Table 3 under the conditions of a liquid temperature of 25°C or 45°C, isocyanate group / active hydrogen group = 1.00 or 1.05 (molar ratio), so that the total mass was 30g, to prepare a mixed liquid. The resulting mixed liquid was then stirred for 15 seconds. 10g of glycerin was then added (assuming the glycerin contained in the hollow fiber) and stirred for 15 seconds to obtain a polyurethane resin cured product. This resin cured product was left to stand in a thermostatic chamber for 10 minutes at 50°C as the first cure condition, and for 2 days at 45°C as the second cure condition.

[0095] [Low molecular weight extractables extraction test] The values ​​of low-molecular-weight eluted substances of the cured resin materials obtained in Examples 1 to 10 and Comparative Examples 1 to 9 were measured by the following method. First, the low molecular weight elution value measurement samples obtained in each Example and Comparative Example were cut into a fan shape and weighed out to 20 g each, immersed in 100 ml of purified water preheated to 40° C., and left at 40° C. for 2 hours to extract low molecular weight elution in the purified water. Next, the obtained extract was decanted and placed in a 50 ml measuring flask to 10 ml, and the liquid adjusted to 50 ml with purified water was used as a test liquid. Then, the UV absorbance of the test liquid was measured (manufactured by Shimadzu Corporation, product name UV-1500). The value of 1 / 10 of the maximum absorbance at 240 to 245 nm was used as the low molecular weight elution value. The low molecular weight elution value is preferably less than 0.07, more preferably less than 0.065.

[0096] [Mixed viscosity and pot life test] In Examples 1 to 10 and Comparative Examples 1 to 9, the mixing viscosity and pot life when obtaining a cured resin product were determined by the following methods. The base agent and curing agent, whose temperatures had been adjusted to 25°C or 45°C in advance, were weighed out and mixed to a total of 50g in a ratio of isocyanate group / active hydrogen group = 1.00 (molar ratio) or 1.05 (molar ratio) to obtain a mixture. The viscosity of the mixture was then measured using a rotational viscometer (B type, No. 4 rotor) in an atmosphere of 25°C. The viscosity 60 seconds after starting to mix the base agent and curing agent was taken as the mixed viscosity, and the time until the viscosity of the mixture reached 50,000 mPa·s was taken as the pot life (seconds). If the mixed viscosity was 1800 mPa·s or less and the pot life was within 1800 seconds, it was judged that the filling property was good, and if the pot life was within 300 seconds, it was judged that the fast curing property was good.

[0097] [Hardness evaluation] The cured products used for the appearance evaluation were measured for Shore D hardness at 25° C. The results are shown in Tables 3 and 4. The hardness was measured in accordance with JIS K 7312:1996.

[0098] [Appearance evaluation] The polyurethane resin-forming compositions for membrane sealing materials in the combinations shown in Tables 3 and 4 were each degassed under reduced pressure at 10 to 20 kPa for 3 minutes, and then poured into a stainless steel mold (100 mm x 100 mm x 8 mm). This was left to stand and cure for 2 days at 45°C, and then demolded to obtain a cured product. The appearance of the obtained cured product was visually evaluated, with A for those without turbidity, B for those with even the slightest turbidity or insufficient curing, and C for those that were cloudy.

[0099] [Table 3]

[0100] [Table 4]

[0101] According to one embodiment of the present disclosure, it is possible to provide a polyurethane resin forming composition that contributes to the formation of a urethane resin having low viscosity and excellent casting properties, and in which the amount of water elution of the low molecular weight reaction product of diphenylmethane diisocyanate and glycerin and the amount of solvent elution of the molded product are reduced, as well as a sealing material and a membrane module using the forming composition. Therefore, the membrane sealing material according to one embodiment of the present disclosure can be suitably used as a membrane sealing material constituting a medical or industrial separation device. [Explanation of symbols]

[0102] 11. Housing 13 Hollow fiber membrane 15 First fluid inlet 17 First fluid outlet 19 Membrane sealant 100 Membrane module (hollow fiber membrane module)

Claims

1. An allophanate group-containing polyisocyanate prepolymer (A), A polyurethane resin-forming composition for a membrane sealant, comprising: The polyisocyanate prepolymer (A) is Diphenylmethane diisocyanate (a1), and an active hydrogen-containing compound (a2), The curing agent (B) contains a castor oil polymerized polyol (b1), The castor oil polymerized polyol (b1) contains a castor oil polymer, which is a homopolymer of castor oil, The curing agent (B) is Castor oil polymerized polyol (b1), At least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyols, and The present invention comprises a hydroxyl group-containing amine compound (b3) other than the castor oil polymerized polyol (b1) and the polyol (b2), The content of the hydroxyl group-containing amine compound (b3) in the curing agent (B) is 35 mass% or less, A polyurethane resin-forming composition for a membrane sealant, having a crosslinking group density of 0.65 mmol / g or more based on the total mass of a polyisocyanate prepolymer (A) and a curing agent (B).

2. The polyurethane resin forming composition for membrane sealing material according to claim 1, wherein the content of the castor oil polymer is 1 mass% or more and 35 mass% or less with respect to the total mass of the polyisocyanate prepolymer (A) and the curing agent (B).

3. An allophanate group-containing polyisocyanate prepolymer (A), A polyurethane resin-forming composition for a membrane sealant, comprising: The polyisocyanate prepolymer (A) is Diphenylmethane diisocyanate (a1), and an active hydrogen-containing compound (a2), The curing agent (B) contains a castor oil polymerized polyol (b1), The castor oil polymerized polyol (b1) contains a castor oil polymer, which is a homopolymer of castor oil, the content of the castor oil polymer is 1% by mass or more and 35% by mass or less based on the total mass of the polyisocyanate prepolymer (A) and the curing agent (B); The curing agent (B) is Castor oil polymerized polyol (b1), At least one polyol (b2) selected from the group consisting of castor oil and castor oil-based modified polyols, and The present invention comprises a hydroxyl group-containing amine compound (b3) other than the castor oil polymerized polyol (b1) and the polyol (b2), A polyurethane resin-forming composition for a membrane sealant, wherein the content of a hydroxyl group-containing amine compound (b3) in the curing agent (B) is 35 mass% or less.

4. A membrane sealant comprising a cured product of the polyurethane resin-forming composition for membrane sealant according to any one of claims 1 to 3.

5. A main body portion, A membrane, A membrane sealant that seals a gap between the main body and the membrane, A membrane module, wherein the membrane seal is the membrane seal according to claim 4.

6. The membrane is a plurality of hollow fiber membranes, The membrane sealant is A gap between the main body and at least a portion of the plurality of hollow fiber membranes, and The membrane module according to claim 5 , wherein at least a part of the gaps between the plurality of hollow fiber membranes is sealed.

Citation Information

Patent Citations

  • Composition for forming polyurethane resin for casting

    JP1994025383A

  • Allophanate-modified diphenylmethane diisocyanates, prepolymers thereof and use thereof for producing polyurea and polyurethane

    JP2009030059A

  • Polyurethane resin formative composition for sealant of membrane module used for blood processing vessel

    JP2017006874A

  • Polyurethane resin-formable composition, and seal material and membrane module using the formable composition

    JP2019056097A

  • Catalyzed non-toxic polyurethane forming compositions and separatory devices employing the same

    US4256617A