Refining method in converter

The refining method optimizes the top blowing lance nozzle configuration to suppress slag foaming during dephosphorization, addressing cost and effectiveness issues in existing methods by enhancing bubble-breaking with controlled nozzle adjustments and flow conditions.

JP7578877B2Active Publication Date: 2024-11-07NIPPON STEEL CORPORATION
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021069563
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-16
Publication Date
2024-11-07
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

Existing methods for suppressing slag foaming in converters are costly or ineffective during dephosphorization blowing, where gas blowing is relatively weak, and require large amounts of sedatives or specialized equipment.

Method used

A refining method that adjusts the top blowing lance nozzle configuration, including increasing the number of holes, controlling the ratio of depression depth to hot metal depth, and optimizing the flow rate and pressure conditions to enhance foaming suppression, even in low gas blowing operations.

Benefits of technology

Effectively suppresses slag foaming during dephosphorization treatment at lower costs by enhancing the physical bubble-breaking effect, reducing the need for costly sedatives and specialized equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578877000002
    Figure 0007578877000002
  • Figure 0007578877000003
    Figure 0007578877000003
  • Figure 0007578877000004
    Figure 0007578877000004
Patent Text Reader

Abstract

To provide a refining method in a converter that can keep the foaming during blowing low at a low cost in operations with relatively weak gas blowing, such as dephosphorization.SOLUTION: In a refining method, oxidizing gas is blown toward hot metal from a top-blown lance while the hot metal is charged into a converter. At this time, a ratio L / L0 between a depth L (mm) of the depression from the static bath surface of the hot metal due to the blowing of the gas and a static bath depth L0 (mm) of the hot metal is greater than 0 and less than 0.30. The top-blowing lance has 7-13 holes in the nozzle arranged around the center axis. Blowing is performed under conditions where an entrainment flow ratio of ambient fluid into the jet is 30.0 or higher and the lance pre-pressure is 0.70-2.00 MPaG.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for refining in a converter, which makes it possible to calm foaming. [Background technology]

[0002] In converter operation, oxygen is blown into the furnace to remove impurities from the molten iron while raising the temperature, and the temperature and component concentrations after blowing are controlled to be within a specified range. At this time, the oxygen blown from the top blowing lance reacts with the carbon in the molten iron to generate carbon monoxide gas, which causes the slag to foam (hereafter referred to as foaming). If foaming becomes excessive, the slag will overflow from the converter (hereafter referred to as slopping). Sloping not only reduces the iron yield, but also leads to interruptions to operations, so methods to calm or suppress slag foaming are being investigated. A common method for calming slag foaming is to add a calming agent to the foamed slag.

[0003] Patent Document 1 discloses a method for suppressing slag foaming, in which carbonaceous material is added from a top blowing lance within 3 minutes after oxygen supply begins. Patent Document 2 discloses a method for calming slag foaming, in which a rod is inserted and removed from above the slag to form an opening in the slag for venting gas.

[0004] Furthermore, Patent Document 3 discloses a method for calming foaming in which a jet stream is collided with the slag surface, and the collision force generated at that time forms gas bubble vent holes in the surface layer of the slag, thereby venting gas bubbles remaining in the slag. Furthermore, Patent Document 4 discloses a method for calming foaming in a standby state in which no blowing treatment is being performed, in which gas is blown from a top blowing lance when foaming occurs. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3888313 [Patent Document 2] Japanese Patent Application Publication No. 10-183217 [Patent Document 3] Patent No. 6221705 [Patent Document 4] JP 2019-94522 A [Non-patent literature]

[0006] [Non-Patent Document 1] Kiyoshi Segawa: Ferrous Metallurgical Reaction Engineering p.94 (1977) [Non-Patent Document 2] N. Rajaratnam: Jet p.46 (1981) Summary of the Invention [Problem to be solved by the invention]

[0007] Foaming occurs even when blowing is not being performed, but refining reactions are particularly active during dephosphorization blowing, and foaming is also intense in operations with relatively weak gas blowing. Therefore, in order to calm the foaming during dephosphorization blowing by adding silencing material, a large amount of silencing material is required, which is very costly.

[0008] In addition, the method described in Patent Document 1 is a method for preventing slag foaming before it occurs, but cannot deal with foaming that actually occurs. In addition, in the method described in Patent Document 3, in order to calm foaming, a top blowing lance that is different from the usual one and can blow gas at high pressure must be installed. This results in a lot of cost. Furthermore, the method described in Patent Document 4 is a method for calming foaming when no blowing process is being performed, so it cannot deal with foaming that occurs during blowing.

[0009] In view of the above problems, an object of the present invention is to provide a refining method in a converter that can inexpensively suppress foaming during blowing in an operation with a relatively weak gas blowing, such as dephosphorization treatment. [Means for solving the problem]

[0010] The present inventors first studied the mechanism by which slag foaming is suppressed. When gas is blown from a top lance in a converter-type refining process, the jet penetrates the slag and collides with the molten iron. At this time, slag is entrained from the side of the jet flow, and the bubbles in the entrained slag are physically destroyed by the jet. For this reason, it is considered that blowing gas from the top lance has a certain degree of foaming suppression effect. Therefore, the present inventors focused on the phenomenon of slag being entrained in the jet flow, and noticed that the foaming suppression effect can be increased by increasing the number of holes in the nozzle at the tip of the top lance and entraining more slag.

[0011] The inventors therefore investigated the detailed conditions for suppressing foaming, and found that when the number of nozzle holes is increased, the ratio of the depth of the cavity formed by blowing gas toward the molten iron surface to the static bath depth of the molten iron is large, and that there is an optimal condition in the relationship between this ratio and the front pressure in the top blowing lance.

[0012] However, it was found that the above-mentioned preferable conditions are limited to operations with relatively strong gas blowing, such as decarburization blowing, and foaming cannot be suppressed when gas blowing is relatively weak and the cavity depth is shallow, such as in general dephosphorization blowing. Therefore, by quantifying and examining the entrainment ratio of the surrounding fluid into the jet flow, the inventors found a preferable condition for the entrainment ratio of the surrounding fluid into the jet flow that can suppress foaming even when the ratio of the cavity depth to the still bath depth of the molten pig iron is small, and arrived at the present invention.

[0013] The present invention is as follows. (1) A refining method in a converter, characterized in that, when molten iron is charged into a converter, an oxidizing gas is blown from a top blowing lance toward the molten iron, the ratio L / L0 of the depth L (mm) of a depression from a still bath surface of the molten iron caused by the blowing of the gas to the still bath depth L0 (mm) of the molten iron, calculated by the following equations (1) and (2), is more than 0 and less than 0.30, the top blowing lance has 7 to 13 nozzle holes arranged around a central axis, the flow rate ratio Q' / Q of an ambient fluid entrained in a jet, calculated by the following equation (3), is 30.0 or more, and the lance front pressure is 0.70 to 2.00 MPaG. L=L h ×exp(-0.78×H / L h ) ···(1) L h =54.1×(Q / (n×d)) 2 / 3 (2) Q' / Q=0.32×H / d (3) Here, H is the distance (mm) from the still bath surface of the molten iron to the nozzle tip of the top lance, and Q is the top blowing flow rate (Nm 3 / hr), and Q' is the flow rate (Nm 3 / hr), n represents the number of holes in the nozzle, and d represents the nozzle outlet diameter (mm). Effect of the Invention

[0014] According to the present invention, in an operation in which the gas blowing is relatively weak, such as a dephosphorization process, foaming can be suppressed to a low level at low cost. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a diagram for explaining the state in which gas is blown toward molten iron from a top blowing lance. [Diagram 2] FIG. 2 is a schematic diagram showing a detailed structure example of the tip portion of a top blowing lance. [Diagram 3] FIG. 13 is a diagram showing the relationship between the number of nozzle holes and the incidence rate of slopping. [Figure 4]FIG. 1 is a graph showing the relationship between the ratio Q′ / Q and the incidence rate of slopping. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a diagram for explaining the state in which gas is blown from a top blowing lance toward molten iron. In Fig. 1, the inside of a furnace body 1 is covered with refractory material, and a plurality of bottom blowing tuyeres (not shown) are provided at the bottom of the furnace body 1. Inert gas for stirring is blown into the furnace body 1 from the bottom blowing tuyeres.

[0017] The top blowing lance 2 can be raised and lowered vertically (up and down in Figure 1) at the opening of the furnace body 1, and an oxidizing gas 3 supplied from a gas supply passage (not shown) connected to the upper end side is blown from the top blowing lance 2 toward the slag 4 and molten iron 5.

[0018] FIG. 2 is a schematic diagram showing a detailed structure example of the tip of the top-blowing lance 2. FIG. 2(a) shows a cross-sectional structure example of the tip of the top-blowing lance 2, and FIG. 2(b) shows a structure example of the top-blowing lance 2 viewed from below in the vertical direction. In FIG. 2(a), the top-blowing lance 2 is composed of a triple tube of an outer tube, a middle tube, and an inner tube, and a range 21 indicates the nozzle outlet diameter. Note that FIG. 2(a) shows an example of a Laval nozzle, but a straight nozzle may also be used. In this embodiment, the nozzle inclination angle 22 is not particularly specified, but if it is too large, the jet collides with the furnace wall, causing severe wear of the refractory, and if it is too small, the jets are too close to each other or merge, reducing the effect of slag entrainment in the jet, so it is preferably 15° to 30°.

[0019] Also, as shown in Fig. 2(b), there is no central hole, and a plurality of peripheral holes 23, which are outlets of a plurality of nozzles, are arranged concentrically around the central axis. Note that the peripheral holes 23 do not necessarily have to be arranged on the same circumference, and do not necessarily have to be arranged at equal intervals. Furthermore, although Fig. 2(b) illustrates an example of a nozzle that does not have a central hole, it may have a central hole.

[0020] 1, the depth L (mm) of the depression from the stationary bath surface of the molten iron caused by gas blowing is defined by the following formulas (1) and (2) based on the calculation method described in Non-Patent Document 1. In this embodiment, the value of L when the correction term k described in Non-Patent Document 1 is set to 0.8 (constant value) is used. L=L h ×exp(-0.78×H / L h ) ···(1) L h =54.1×(Q / (n×d)) 2 / 3 (2)

[0021] Here, H is the distance from the still bath surface of the molten iron to the nozzle tip of the top lance (lance height) (mm), and Q is the top blowing injection flow rate (Nm 3 / hr), n represents the number of nozzle holes in the top blowing lance, and d represents the nozzle outlet diameter (mm).

[0022] Next, the conditions for suppressing foaming in the embodiment of the present invention will be described. In the present embodiment, the ratio L / L0 of the depth L (mm) of the depression to the static bath depth L0 (mm) of the molten iron is mainly focused on the conditions assuming the operation of dephosphorization (including desiliconization). Here, the ratio L / L0 is the penetration ratio of the gas (jet) into the molten iron, and is an important parameter for appropriately controlling the reaction in the furnace.

[0023] The inventors first conducted an experiment to investigate the relationship between the ratio L / L0 and the incidence of slopping. In the experiment, the number of nozzle holes n was fixed at 5, the nozzle outlet diameter d was fixed at 5.3 mm, and the static bath depth L0 was fixed at 200 mm, and the lance height H and the top blowing injection flow rate were changed to calculate the incidence of slopping at various ratios L / L0. As a result, it was confirmed that the incidence of slopping increases when the ratio L / L0 is less than 0.30, which is a general condition for dephosphorization blowing. As described above, the incidence of slopping increases when the ratio L / L0 is small. In this embodiment, however, assuming the operating conditions in the dephosphorization treatment, it is assumed that the ratio L / L0 is more than 0 and less than 0.30. In addition, considering the actual operation of dephosphorization blowing, it is preferable to control the ratio L / L0 to be 0.04 or more and 0.25 or less.

[0024] Next, the number of nozzle holes at the tip of the top-blowing lance will be explained. When changing to a top-blowing lance with a different number of nozzle holes, it is preferable to increase the number of nozzle holes so that the above-mentioned ratio L / L0 is a constant value. The ratio L / L0 is considered to be an index of refining behavior such as the dephosphorization reaction in the furnace. If the value of the ratio L / L0 differs when changing to a top-blowing lance with a different number of nozzle holes, the operator must adjust by raising or lowering the top-blowing lance accordingly, which is not preferable for stable operation.

[0025] The inventors conducted an experiment in which the number of nozzle holes was changed under the condition that the ratio L / L0 was fixed at 0.17. In the experiment, the static bath depth L0 of the molten iron was fixed at 2000 mm, and as can be seen from the above-mentioned formulas (1) and (2), the ratio L / L0 was fixed at 0.17 by making the depth L of the depression the same for each sample. In other words, the lance height H was fixed at 3500 mm, and in formula (2), the top blowing injection flow rate Q was set to 40000 Nm 3 / hr, and the nozzle outlet diameter d was reduced as the number of nozzle holes n increased, and the slopping occurrence rate was calculated.

[0026] FIG. 3 is a diagram showing the relationship between the number of nozzle holes and the incidence of slopping. As shown in FIG. 3, it was confirmed that the incidence of slopping is low when the number of lance holes is 7 or more. From the above results, the number of nozzle holes arranged around the central axis of the top blowing lance is set to 7 or more. Furthermore, when the number of nozzle holes is 14 or more, the lance front pressure becomes too large and the nozzle outlet diameter d becomes small, as will be described in detail later, which may cause nozzle clogging. Therefore, the number of nozzle holes arranged around the central axis of the top blowing lance is set to 7 to 13.

[0027] Next, the entrainment flow rate ratio of the surrounding fluid into the jet flow will be explained. The inventors focused on the entrainment flow rate ratio of the surrounding fluid (air) into the jet flow and found a correlation between this entrainment flow rate ratio of the surrounding fluid and the actual amount of slag entrained. They also found that by controlling this entrainment amount ratio of the surrounding fluid, foaming can be suppressed even when the ratio L / L0 is smaller than 0.30. The entrainment flow rate ratio of the surrounding fluid into the jet flow is defined by the following formula (3) based on the entrainment formula described in Non-Patent Document 2, which means that an axisymmetric jet entrains the surrounding fluid. Q' / Q=0.32×H / d (3)

[0028] Here, H is the distance (mm) from the still bath surface of the molten iron to the nozzle tip of the top lance, and Q is the top blowing flow rate (Nm 3 / hr), and Q' is the flow rate (Nm 3 / hr), and d is the nozzle outlet diameter (mm).

[0029] Next, the inventors set the ratio L / L0 to 0.23 and the top-blowing injection flow rate Q to 35,000 Nm 3Under the condition that the flow rate was fixed at 100 / hr, the number of nozzle holes, the nozzle outlet diameter, and the lance height were changed to investigate the effect of the ratio Q' / Q on the incidence of slopping. FIG. 4 is a diagram showing the relationship between the ratio Q' / Q and the incidence of slopping. As shown in FIG. 4, it was confirmed that the incidence of slopping drops sharply when the ratio Q' / Q reaches 30.0. Therefore, in this embodiment, the ratio Q' / Q of the flow rate of the surrounding fluid entrained in the jet is set to 30.0 or more.

[0030] Next, the conditions of the lance front pressure will be explained. The lance front pressure is the nozzle inlet pressure when gas branches from the center of the top blowing lance to the nozzle. Below, the lance front pressure is shown as a gauge pressure (MPaG), but when converted to absolute pressure (MPa), 0.101 MPa is added. As mentioned above, when the number of nozzle holes and the lance height are increased while the ratio L / L0 is fixed, the lance outlet diameter (and throat diameter in the case of a Laval nozzle) also becomes smaller, so that the lance front pressure tends to increase as the number of nozzle holes and the lance height increase.

[0031] Here, the lance front pressure is set to 0.70 MPaG to 2.00 MPaG. When the ratio L / L0 is in the range of 0.30 or more, a lance front pressure of 1.00 MPaG or more can provide a sufficient physical foam breaking effect, but when the ratio L / L0 is in the range of less than 0.30, the lance front pressure tends to be lower than in the previous range because the blow is soft and the top blowing injection flow rate is small. Therefore, a sufficient physical foam breaking effect can be obtained at 0.70 MPa or more. On the other hand, when the lance front pressure is greater than 2.00 MPaG, the gas blow is too strong, increasing the possibility of damaging the refractory of the furnace wall.

[0032] In the examples shown in Figures 3 and 4, the occurrence rate of slopping is used as an index, but in order to reduce the occurrence rate of slopping, it is sufficient to consider lowering the slag height caused by foaming. In the dephosphorization process, for example, the slag height in the furnace is measured with a slag level meter, and the blowing operation is performed by adjusting the slag basicity (CaO / SiO2), the top-blowing injection flow rate (oxygen flow rate) Q from the top-blowing lance, the lance height H of the top-blowing lance, etc., or by adding a silencing material, depending on the measurement results. Any slag level meter can be used as long as it can measure the vertical height of the slag, and for example, a microwave level meter may be used. EXAMPLES

[0033] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0034] The maximum volume of molten pig iron was charged into a converter with a heat size of 280 tons, and quicklime and other materials were charged for dephosphorization. The static bath depth L0 of the molten pig iron was set to 2000 mm. Dephosphorization blowing was performed using the top-blowing lance shown in Table 1. These top-blowing lances have multiple nozzle holes arranged at equal intervals around the central axis of the top-blowing lance. In the dephosphorization blowing, gas containing more than 99.9 vol% oxygen was blown from the top-blowing lance toward the molten pig iron surface, and the injection flow rate (oxygen flow rate) Q was set under the conditions shown in Table 1. The lance height H and ratio L / L0 of the top-blowing lance were also set under the conditions shown in Table 1.

[0035] During blowing, the vertical height of the slag was measured using a microwave level meter. The "slag height" in Table 1 is ("average slag height (m) measured by microwave level meter (average measured at one point at a specified time interval)" - "static bath depth of molten pig iron (m)") ÷ "height from static bath surface of molten pig iron to throat (m)" × 100 (%), and when it was 60% or less, it was evaluated as having an effect of suppressing foaming. The average slag height (m) is the average slag height obtained by subtracting the distance between the microwave level meter and the throat, which was measured in advance, from the measured distance between the microwave level meter and the slag surface.

[0036] [Table 1]

[0037] The underlines in Table 1 indicate deviations from the conditions of the present invention. As shown in Table 1, in Examples No. 1 to No. 9, the slug height could be suppressed to 60% or less, and it was confirmed that there was an effect of suppressing foaming.

[0038] On the other hand, in the comparative examples No. 10, No. 11 and No. 15, the number of nozzle holes was only four, and the lance front pressure was too low and the ratio Q' / Q was less than 30.0, so the slug height was 80% or more, and the foaming suppression effect could not be confirmed. In the comparative example No. 12, the lance front pressure was too low and the ratio Q' / Q was less than 30.0, so the slug height was 76%, and the foaming suppression effect could not be confirmed.

[0039] In the comparative examples No. 13 and No. 14, the ratio Q' / Q was less than 30.0, so the slag height was larger than that of the examples, and the foaming suppression effect was insufficient. In the comparative examples No. 16 and No. 18, the number of nozzle holes was only four, and the ratio Q' / Q was less than 30.0, so the slag height was larger than that of the examples, and the foaming suppression effect was insufficient. On the other hand, in the comparative examples No. 17 and No. 19, the lance front pressure was too large. In this example, the slag height was reduced to 60% or less, and it was confirmed that there was a foaming suppression effect, but the refractory of the furnace wall was partially damaged, and it was confirmed that the operating conditions were difficult.

Claims

【Claim 1】 When oxidizing gas is blown from a top blowing lance toward molten iron charged in a converter, the depth L (mm) of the depression from the stationary bath surface of the molten iron caused by the blowing of the gas and the stationary bath depth L of the molten iron are calculated by the following formulas (1) and (2). 0 (mm) ratio L / L 0 is more than 0 and less than 0.30, the top blowing lance has 7 to 13 nozzle holes arranged around a central axis, the flow rate ratio Q' / Q of the surrounding fluid entrained in the jet, calculated by the following formula (3), is 30.0 or more, and the lance front pressure is 0.70 to 2.00 MPaG. L=L h ×exp(-0.78×H / L h ) ・・・(1) L h =54.1×(Q / (n×d)) 2 / 3 ・・・(2) Q' / Q = 0.32 × H / d... (3) Here, H represents the distance (mm) from the still bath surface of the molten iron to the nozzle tip of the top lance, and Q represents the top blowing injection flow rate (Nm 3 / hr), and Q' is the flow rate (Nm 3 / hr), n represents the number of holes in the nozzle, and d represents the nozzle outlet diameter (mm).

Citation Information

Patent Citations

  • Converter refining method

    JP1982060004A

  • Active carbon and manufacture

    JP1987021705A

  • Method for restraining slag foaming

    JP1998183217A

  • Lance and method for removing stuck metal in furnace using the lance

    JP1998219329A

  • Method for dephosphorizing molten iron

    JP2010095785A