Method for producing copolymer polyester resin
The method addresses flavor and molecular weight issues in copolymerized polyester resins by controlling linear oligomer content and using staged glycol addition with specific catalysts, resulting in improved transparency and recyclability.
Patent Information
- Application Number
- JP2024527279
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-07
- Filing Date
- 2024-01-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-01-16
AI Technical Summary
Conventional copolymerized polyester resins used for storage containers for beverages suffer from flavor deterioration, coloring, and reduction in molecular weight during recycling due to the presence of specific linear oligomers and poor thermal stability.
A manufacturing method that controls the content of specific linear oligomers by adding glycol components in stages during polymerization, uses a specific combination of catalysts, and adjusts carboxyl terminal group concentration to improve thermal stability, thereby preventing flavor deterioration and molecular weight reduction.
The method produces copolymerized polyester resin with improved transparency, moldability, and flavor properties, maintaining molecular weight and preventing coloration during recycling.
Smart Images

Figure 0007579527000001 
Figure 0007579527000002 
Figure 0007579527000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolymer polyester resin which is excellent in flavor properties and recyclability in addition to transparency and moldability. [Background technology]
[0002] Polyester, in particular polyethylene terephthalate (PET) produced from raw materials terephthalic acid (TPA) and ethylene glycol (EG), has excellent chemical and physical properties and is therefore widely used for containers, films, sheets, fibers, etc.
[0003] In recent years, among polyethylene terephthalate (PET), polyester resins copolymerized with diethylene glycol (hereinafter sometimes abbreviated as DEG) (hereinafter sometimes abbreviated as copolymerized polyester resins) have attracted attention due to their excellent transparency, moldability, impact resistance, heat resistance, etc., and have been used in various applications, particularly as raw material polymers for molded articles such as films, sheets, injection molded articles, and irregularly shaped articles. In this case, depending on the application, aliphatic dicarboxylic acids are further copolymerized in addition to terephthalic acid to lower the melting point and glass transition temperature of the resulting copolymerized polyester resin to impart flexibility, or to adjust the degree of crystallization and crystallization rate.
[0004] In addition, polyester resins copolymerized with sodium sulfoisophthalate (GC) have attracted attention due to their excellent biodegradability, and have been used in various applications, particularly as raw material polymers for molded articles such as films, sheets, injection molded articles, and irregularly shaped articles (see Patent Documents 1 to 6).
[0005] However, when the copolymer polyester resins produced by these conventional techniques are used as molded articles for storing beverages, etc., they have a problem of poor flavor properties, as they may affect the taste and odor of the beverage, etc. Furthermore, these copolymer polyester resins have a problem of coloration of the resin and a decrease in molecular weight during recycling. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-150542 A [Patent Document 2] Patent No. 4755995 [Patent Document 3] Patent No. 4614963 [Patent Document 4] Special Publication No. 2007-500769 [Patent Document 5] Patent No. 4807952 [Patent Document 6] Patent No. 5345749 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been devised to solve such problems in the prior art, and an object of the present invention is to provide a production method for a copolymer polyester resin in which diethylene glycol and sodium sulfoisophthalate are copolymerized to improve transparency and moldability, which prevents a decrease in flavor properties and prevents coloration of the resin and a decrease in molecular weight during recycling. [Means for solving the problem]
[0008] In order to achieve this object, the present inventors have conducted extensive research into the cause of the decline in flavor properties in copolymerized polyester resins obtained by copolymerizing diethylene glycol and sodium sulfoisophthalate, and have found that a specific linear oligomer (by-product oligomer) generated as a by-product during the production of the copolymerized polyester resin is the cause of the decline in flavor properties, and that by suppressing the content of this by-product oligomer to a certain value or less, a copolymerized polyester resin that is almost free of the problem of decline in flavor properties can be provided.Then, the present inventors have found that in order to reduce the content of the by-product oligomer, which is the cause of the decline in flavor properties, it is important to add a part of the glycol component later in the production process of the copolymerized polyester resin, rather than adding all of the glycol component from the beginning.
[0009] In addition, as a result of intensive research into the causes of coloration and molecular weight reduction of resins during recycling, it was found that diethylene glycol and sodium sulfoisophthalate used as materials for copolymerized polyester resins improve transparency and moldability, but also reduce the thermal stability and thermo-oxidative stability of the resulting copolymerized polyester resin. Therefore, it was thought that the resin deteriorates due to heating during film formation or molded product production, causing the film or molded product to become colored or its molecular weight to decrease. In this regard, the present inventors have studied methods for improving the thermal stability and thermo-oxidative stability of copolymerized polyester resins, and have found that it is important to control the carboxyl end group concentration (AV) of the copolymerized polyester resin within a certain range and to use a specific combination of two types of catalysts for polymerization.
[0010] That is, the present invention has been completed based on the above findings, and has the following features (1) to (14). (1) A method for producing a copolymer polyester resin, comprising the steps of: the copolymerized polyester resin contains terephthalic acid as a dicarboxylic acid component main component and ethylene glycol as a glycol component main component, and when the total amount of dicarboxylic acid components in all polyester resin components is taken as 100 mol %, the ratio of terephthalic acid components to all dicarboxylic acid components is 74.95 to 94.95 mol %, the ratio of glutaric acid to all dicarboxylic acid components is 5 to 25 mol %, and the ratio of sodium sulfoisophthalate to all dicarboxylic acid components is 0.05 to 10 mol %; when the total amount of glycol components is taken as 100 mol %, the ratio of diethylene glycol to all glycol components is 1 to 22 mol %; the content of free linear oligomers composed of terephthalic acid, glutaric acid, and ethylene glycol in the copolymerized polyester resin is 90 ppm or less, and the content of free linear oligomers composed of terephthalic acid and ethylene glycol in the copolymerized polyester resin is 100 ppm or less, The production method includes a first step of carrying out an ester formation reaction using at least a portion of the total amount of terephthalic acid, glutaric acid, and sodium sulfoisophthalate as raw material monomers of the dicarboxylic acid component, and at least a portion of the total amount of ethylene glycol and / or at least a portion of the total amount of diethylene glycol as raw material monomers of the glycol component to generate an oligomer; a second step of additionally adding the remaining portion of the total amount of sodium sulfoisophthalate and / or the remaining portion of the total amount of ethylene glycol and / or the remaining portion of the total amount of diethylene glycol to the oligomer product obtained in the first step to carry out an additional ester formation reaction; and a third step of polycondensing the oligomer product obtained in the second step to increase its molecular weight. A method for producing a copolymer polyester resin comprising the steps of: (2) A method for producing a copolymerized polyester resin according to (1), characterized in that the entire amount of ethylene glycol and a portion of the total amount of diethylene glycol are used in the first step, and the remaining portion of the total amount of diethylene glycol is additionally added in the second step. (3) A method for producing a copolymerized polyester resin according to (2), characterized in that the amount of diethylene glycol used in the first step is 92.5 to 70% of the total amount (mol %), and the amount of diethylene glycol used in the second step is 7.5 to 30% of the total amount (mol %). (4) The method for producing a copolymer polyester resin according to (1), wherein the produced copolymer polyester resin has a color b value of −5.0 to 25.0. (5) The method for producing a copolymer polyester resin according to (1), wherein the produced copolymer polyester resin has a carboxyl end group concentration (AV) of 3 to 50 eq / t. (6) A method for producing a copolymerized polyester resin according to (1), characterized in that an aluminum compound and a phosphorus compound are used as polymerization catalysts, the produced copolymerized polyester resin contains aluminum atoms and phosphorus atoms derived from these polymerization catalysts, the content of aluminum atoms in the copolymerized polyester resin is 5 to 40 ppm, and the molar ratio of phosphorus atoms to aluminum atoms in the copolymerized polyester resin is greater than 0 and less than or equal to 2.6. (7) The method for producing a copolymer polyester resin according to (1), wherein an alkali metal compound and / or an alkaline earth metal compound other than sodium sulfoisophthalate is used to improve polymerization activity, the produced copolymer polyester resin further contains alkali metal atoms and / or alkaline earth metal atoms derived from these compounds, and the content of the alkali metal atoms and / or alkaline earth metal atoms in the copolymer polyester resin is 1 to 100 ppm. (8) The method for producing a copolymer polyester resin according to (1), wherein a stepped molded plate obtained by molding the produced copolymer polyester resin has a haze value of 20% or less at a portion having a thickness of 6 mm. (9) A method for producing a molded article, comprising producing a copolymer polyester resin by the production method according to any one of (1) to (8) above, and using the produced copolymer polyester resin to produce a molded article. (10) A method for producing a heat-shrinkable film, comprising producing a copolymer polyester resin by the production method according to any one of (1) to (8) above, and using the produced copolymer polyester resin to produce a heat-shrinkable film. (11) A method for producing fibers, comprising producing a copolymer polyester resin by the production method according to any one of (1) to (8) above, and using the produced copolymer polyester resin to produce fibers. (12) A method for producing a nonwoven fabric, comprising producing a copolymer polyester resin by the production method according to any one of (1) to (8) above, and using the produced copolymer polyester resin to produce a nonwoven fabric. (13) A method for producing an adhesive, comprising producing a copolymer polyester resin by the production method according to any one of (1) to (8) above, and using the produced copolymer polyester resin to produce an adhesive. (14) A method for producing a coating material, comprising producing a copolymer polyester resin by the production method according to any one of (1) to (8) above, and using the produced copolymer polyester resin to produce a coating material. Effect of the Invention
[0011] The copolymer polyester resin produced by the method of the present invention enjoys the advantages of transparency and moldability due to the use of diethylene glycol and sodium sulfoisophthalate, while having a low content of specific linear oligomers and excellent flavor properties, and further, there is no coloration of the resin or a decrease in molecular weight when recycled. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] First, the copolymer polyester resin to be produced by the production method of the present invention will be specifically described. The copolymerized polyester resin obtained by the production method of the present invention is a copolymerized polyester resin containing terephthalic acid as the main component of the dicarboxylic acid component and ethylene glycol as the main component of the glycol component, in which diethylene glycol and sodium sulfoisophthalate are copolymerized for transparency and moldability. The content of specific linear oligomers generated as by-products during polymerization is suppressed to a certain value or less, thereby improving flavor properties. Furthermore, by controlling the carboxyl end group concentration (AV) of the copolymerized polyester resin within a certain range and using a combination of two specific types of catalysts for polymerization, coloration of the resin and reduction in molecular weight during recycling are effectively prevented.
[0013] The copolymerized polyester resin of the present invention contains terephthalic acid as a main component of the dicarboxylic acid component. Specifically, the content of terephthalic acid is 74.95 to 94.95 mol%, preferably 79 to 94.95 mol%, more preferably 85 to 94.95 mol%, and further preferably 90 to 94.95 mol%, relative to the total amount of the dicarboxylic acid components, where the total amount of the dicarboxylic acid components is 100 mol%.
[0014] The copolymerized polyester resin of the present invention further contains glutaric acid as a dicarboxylic acid component in addition to terephthalic acid. Glutaric acid has the role of lowering the melting point and glass transition temperature of the obtained copolymerized polyester resin to impart flexibility, and adjusting the crystallinity and crystallization rate. The content of glutaric acid may be appropriately adjusted depending on the application of the copolymerized polyester resin, but generally, when the total amount of the dicarboxylic acid components is taken as 100 mol%, the ratio of glutaric acid to all dicarboxylic acid components is 5 to 25 mol%, preferably 7 to 23 mol%, and more preferably 8 to 20 mol%. As the content of glutaric acid increases, the melting point, glass transition temperature, crystallinity, and crystallization rate of the obtained copolymerized polyester resin tend to decrease, and the transparency is improved.
[0015] The copolymer polyester resin of the present invention contains sodium sulfoisophthalate as a dicarboxylic acid component in order to improve biodegradability, in addition to terephthalic acid and glutaric acid. Specifically, the content of sodium sulfoisophthalate is 0.05 to 10 mol%, preferably 0.1 to 5 mol%, more preferably 0.2 to 3 mol% relative to the total dicarboxylic acid components, when the total amount of dicarboxylic acid components is 100 mol%. If the content of sodium sulfoisophthalate is less than the lower limit, the haze value tends to be high and the DSC measurement tends to be poor. On the other hand, if the content of sodium sulfoisophthalate exceeds the upper limit, the amount of free linear oligomers described below increases, resulting in poor flavor properties.
[0016] The copolymer polyester resin of the present invention may contain other dicarboxylic acid components other than terephthalic acid, glutaric acid, and sodium sulfoisophthalate. Examples of such other dicarboxylic acid components include (1) aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyl-4,4'-dicarboxylic acid, and diphenoxyethanedicarboxylic acid, and functional derivatives thereof, (2) alicyclic dicarboxylic acids such as hexahydroterephthalic acid, hexahydroisophthalic acid, tetrahydrophthalic acid, and cyclohexanedicarboxylic acid, and functional derivatives thereof, and (3) aliphatic dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and dimer acid, and functional derivatives thereof. When the total amount of the dicarboxylic acid components is taken as 100 mol%, the ratio of the other dicarboxylic acid components to the total dicarboxylic acid components is preferably 0 to 20 mol%, more preferably 0 to 10 mol%, and even more preferably 0 to 5 mol%. As the ratio of the other dicarboxylic acid component increases, the melting point, glass transition temperature, crystallinity and crystallization rate of the resulting copolymerized polyester resin tend to decrease, and the transparency tends to improve.
[0017] The copolymerized polyester resin of the present invention contains ethylene glycol as a main component of the glycol components. Specifically, the content of ethylene glycol is preferably 50 to 99 mol%, more preferably 70 to 99 mol%, further preferably 80 to 99 mol%, and particularly preferably 90 to 99 mol%, relative to the total amount of the glycol components, where the total amount of the glycol components is 100 mol%.
[0018] In addition to ethylene glycol, the copolymerized polyester resin of the present invention contains diethylene glycol as a glycol component to improve transparency and moldability. Specifically, the content of diethylene glycol is 1 to 22 mol%, preferably 1 to 20 mol%, more preferably 1 to 18 mol% relative to the total glycol components when the total amount of glycol components is 100 mol%. When the content of diethylene glycol is within the above range, it is possible to obtain a copolymerized polyester resin that is highly transparent, that is, amorphous. When the content of diethylene glycol is less than the above lower limit, it becomes crystalline, so the transparency of the molded product or film is deteriorated, sufficient transparency cannot be achieved, and commercial value tends to be lost. On the other hand, when the content of diethylene glycol exceeds the above upper limit, recyclability (thermal stability) decreases and the resin tends to be colored.
[0019] Diethylene glycol is also produced by condensation of ethylene glycol during polymerization of copolymer polyester resin. The amount of diethylene glycol produced by this condensation varies depending on the polymerization conditions and the production equipment, but is about 0.5 to 2.0 mol% of the total glycol components. The amount of diethylene glycol to be added as a raw material should be considered taking this amount into account.
[0020] In addition, the term "amorphous" as used herein refers to a sample that has been left in a Yamato DP63 dryer at 120°C for 120 minutes, and is then heated from -100°C to 300°C at 20°C / min using a differential scanning calorimeter (DSC), then cooled to -100°C at 50°C / min, and then heated from -100°C to 300°C at 20°C / min, and shows no melting peak in either of these two heating processes. The copolymerized polyester resin of the present invention is amorphous, and therefore can have a transparency that is suitable for use even in thick molded bodies. In other words, being "amorphous" under these measurement conditions means that the transparency of the film can be maintained at a high quality, and even in thick films, sufficient transparency can be maintained.
[0021] The copolymerized polyester resin of the present invention may contain other glycol components in addition to ethylene glycol and diethylene glycol, such as (1) aliphatic glycols such as tetramethylene glycol, pentamethylene glycol, and hexamethylene glycol, (2) alicyclic glycols such as 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol, and (3) aromatic glycols such as p-xylylene glycol and m-xylylene glycol.
[0022] The copolymerized polyester resin of the present invention preferably contains a polyfunctional compound having three or more carboxyl groups, hydroxyl groups, or ester-forming groups thereof (e.g., trimellitic acid, pyromellitic acid, glycerin, trimethylolpropane, etc.) in an amount of 0.001 to 5 mol % of the acid component and / or glycol component of the copolymerized polyester resin in order to improve the extrusion moldability of the copolymerized polyester resin.
[0023] The copolymerized polyester resin of the present invention has an essential feature of being excellent in flavor properties (aroma retention) since the content of a specific linear oligomer generated as a by-product during polymerization is suppressed to a certain value or less. Specifically, the copolymerized polyester resin of the present invention has a content of free linear oligomers composed of terephthalic acid, glutaric acid, and ethylene glycol of 90 ppm or less, and a content of free linear oligomers composed of terephthalic acid and ethylene glycol of 100 ppm or less.
[0024] In the present invention, the linear oligomer consisting of terephthalic acid, glutaric acid and ethylene glycol refers to a linear oligomer in which terephthalic acid, terephthalic acid, glutaric acid, ethylene glycol, ethylene glycol, ethylene glycol, and ethylene glycol are linearly bonded in this order (hereinafter, abbreviated as L-T2GE4). The content of L-T2GE4 must be 90 ppm or less, preferably 80 ppm or less, and more preferably 70 ppm or less. If the content exceeds the upper limit, the flavor tends to decrease. The lower limit of this content is 1 ppm from the viewpoint of economic efficiency during production. The content of L-T2GE4 is a value quantified by the measurement method of the examples described later.
[0025] In the present invention, the linear oligomer consisting of terephthalic acid and ethylene glycol refers to a linear oligomer in which terephthalic acid and ethylene glycol are linearly bonded in this order (hereinafter, abbreviated as MHET). The MHET content must be 100 ppm or less, preferably 90 ppm or less, and more preferably 80 ppm or less. If the content exceeds the upper limit, the flavor tends to decrease. The lower limit of the content is 1 ppm from the viewpoint of economic efficiency during production. The MHET content is a value quantified by the measurement method described in the Examples below.
[0026] Although the detailed mechanism by which flavor deteriorates with increasing L-T2GE4 content in a copolymerized polyester resin is unclear, L-T2GE4 has low crystallinity and melting point because it contains a glutaric acid component, and furthermore, has a high affinity with water because its terminal is a hydroxyl group. As a result, it is considered that flavor deteriorates with increasing L-T2GE4 content. In addition, although the detailed mechanism by which flavor deteriorates with increasing MHET content in a copolymerized polyester resin is unclear, MHET has a high affinity with water because its terminal is a carboxyl group and its terminal is a hydroxyl group. As a result, it is considered that flavor deteriorates with increasing MHET content. In particular, in a copolymerized polyester resin used as a packaging material for beverages that require low flavor such as mineral water, the decrease in flavor due to these linear oligomers (by-product oligomers) is a major problem. In the present invention, in the manufacturing process of a copolymerized polyester resin, instead of adding all of the glycol components from the beginning, a part of the glycol components is added later to reduce the content of these linear oligomers (by-product oligomers) and prevent the decrease in flavor. The total content of linear oligomers (L-T2GE4 and MHET) in the copolymerized polyester resin of the present invention must be 190 ppm or less, preferably 180 ppm or less, more preferably 130 ppm or less, and most preferably 100 ppm or less. If the total content of linear oligomers exceeds 190 ppm, the flavor property tends to decrease. In the present invention, the "copolymerized polyester resin" refers to a material that contains not only a chemical substance called polyester, but also oligomer components such as L-T2GE4 and MHET, and a catalyst component described later. However, when explaining a chemical substance called polyester, it may be described as a "copolymerized polyester resin" for convenience.
[0027] The copolymerized polyester resin of the present invention has a carboxyl end group concentration of preferably 3 to 50 equivalents per ton of polymer, more preferably 3 to 35 equivalents / ton, and even more preferably 5 to 30 equivalents / ton. The carboxyl end group concentration in the above range can contribute to suppressing coloration of the copolymerized polyester resin. In the case where the coloration of the copolymerized polyester resin is not required to be slightly poor, the carboxyl end group concentration may be 51 equivalents / t or less. If the productivity (reaction time) is not taken into consideration, the lower limit of the carboxyl end group concentration may be 0 equivalents / t.
[0028] The number average molecular weight of the copolymerized polyester resin of the present invention is preferably 2000 to 30000, more preferably 2500 to 28000, and even more preferably 3000 to 27000. If the number average molecular weight is less than the lower limit, the crystallinity increases, the haze increases, and furthermore, the strength and elongation of the molded product is insufficient due to insufficient resin cohesive force, and the molded product may become brittle and unusable. On the other hand, if the number average molecular weight exceeds the upper limit, the melt viscosity increases too much, so that the optimum temperature for various molding processes also increases, and the residence time may be extended, resulting in a decrease in sheet film formability, and furthermore, the amount of the L-T2GE4 increases, resulting in a decrease in flavor properties.
[0029] The glass transition temperature of the copolymerized polyester resin of the present invention is preferably 40°C or more and less than 120°C, more preferably 45°C or more and less than 115°C, even more preferably 50°C or more and less than 110°C, and particularly preferably 50°C or more and less than 70°C. Here, the glass transition temperature refers to a value measured by raising the temperature at 20°C / min using a differential scanning calorimeter (DSC). If the glass transition temperature is less than the above lower limit, the film or the profile extrusion molded product may be thermally deformed when used outdoors in summer, or during product transportation or warehouse storage in a sealed state in summer. In addition, if the glass transition temperature exceeds the above upper limit, the film formability and transparency of the sheet tend to decrease, and it may not be usable depending on the application.
[0030] The color b value of the copolymerized polyester resin of the present invention is preferably -5.0 to 25.0. The lower limit of the color b value is more preferably -3.0, and even more preferably -2.5. The upper limit is more preferably 20.0, and even more preferably 16.0. If the color b value exceeds the upper limit, the copolymerized polyester resin becomes yellowish, which is not preferable in terms of color tone. On the other hand, if the color b value is less than the lower limit, the bluish tinge of the copolymerized polyester resin becomes noticeable, and it may not be usable depending on the application.
[0031] The copolymerized polyester resin of the present invention preferably has a haze value of 20% or less, more preferably 15% or less, and particularly preferably 10% or less, at a portion of a thickness of 6 mm in a stepped molded plate obtained by molding at a mold temperature of 10° C. If the haze value exceeds the upper limit, the transparency of the molded article or film deteriorates, and it may become impossible to use the molded article or film in applications where strict transparency is required.
[0032] The copolymerized polyester resin of the present invention may contain various additives depending on the application and necessity, within the range that does not impair the characteristics of the present invention. Examples of additives include colorants such as pigments, toners, heat stabilizers, antioxidants, ultraviolet absorbers, light stabilizers, plasticizers, modifiers, antistatic agents, flame retardants, dyes, etc., and titanium oxide and toner are preferred for improving the colorability of the polyester resin composition. The amount of titanium oxide added is 0 to 20,000 ppm, preferably 0.1 ppm to 15,000 ppm, and more preferably 0.2 ppm to 13,000 ppm. The amount of toner added is 0.1 ppm to 100 ppm, preferably 0.5 to 90 ppm, and most preferably 1 to 80 ppm. Phthalocyanine-based and stilbene bisbenzoxazole derivatives can be used as the toner. Specifically, these include SOLVAPERM BLUE RLS, PVfastBLUE A4R, and Hostalux KS manufactured by Clariant, and OB-1 manufactured by Eastman Kodak Co., and among these, the Solvent Blue series manufactured by Clariant, which starts to melt at 250° C. or higher and is completed at about 300° C., is particularly preferred. Since such a toner has a melting point similar to that of polyester itself (230 to 265° C.), it has very good mixing and solubility with polyester, has excellent melting uniformity in a melting machine, and provides good spinning operability.
[0033] The copolymerized polyester resin of the present invention can be suitably molded into various molded articles by extrusion blow molding, squeeze molding, injection molding, profile extrusion molding, calendar processing molding, etc., which have been conventionally used for PET and the like. Specifically, the copolymerized polyester resin of the present invention can be suitably used for various applications requiring transparency, moldability, etc., and can be suitably used as a raw material for molded articles, heat-shrinkable films, fibers, nonwoven fabrics, adhesives, paints, etc. In particular, the copolymerized polyester resin of the present invention has a low content of specific linear oligomers and is excellent in flavor, and therefore can be suitably used to form molded articles that serve as storage containers for beverages, etc.
[0034] Next, the method for producing the copolymer polyester resin of the present invention will be described. The method for producing a copolymerized polyester resin of the present invention includes a first step of carrying out an ester formation reaction using at least a portion of the total amount of terephthalic acid, the total amount of glutaric acid, and the total amount of sodium sulfoisophthalate as raw monomers of the dicarboxylic acid component, and at least a portion of the total amount of ethylene glycol and / or at least a portion of the total amount of diethylene glycol as raw monomers of the glycol component to generate an oligomer, a second step of carrying out an additional ester formation reaction by additionally adding the remaining portion of the total amount of sodium sulfoisophthalate and / or the remaining portion of the total amount of ethylene glycol and / or the remaining portion of the total amount of diethylene glycol to the oligomer product obtained in the first step, and a third step of polycondensing the oligomer product obtained in the second step to increase its molecular weight, and is essentially characterized in that the glycol component is not added in its entirety from the beginning, but a part of the glycol component is added later. By such a later additional addition of the glycol component, the content of by-product oligomers, which is the cause of the deterioration of flavor, can be efficiently reduced. Although the detailed mechanism is unknown, it is thought that the addition of additional glycol components such as ethylene glycol or diethylene glycol causes transesterification or esterification, resulting in a reduction in the amount of free L-T2GE4 and MHET.
[0035] In the first step, an ester forming reaction is carried out using at least a part of the total amount of terephthalic acid, glutaric acid, and sodium sulfoisophthalate as raw monomers of the dicarboxylic acid component, and at least a part of the total amount of ethylene glycol and / or at least a part of the total amount of diethylene glycol as raw monomers of the glycol component, to produce an oligomer. Next, in the second step, the remaining part of the total amount of sodium sulfoisophthalate and / or the remaining part of the total amount of ethylene glycol and / or the remaining part of the total amount of diethylene glycol is added to the oligomer product obtained in the first step to carry out an additional ester forming reaction. Either a direct esterification reaction or an ester exchange reaction can be used as the ester forming reaction.
[0036] A part of the total amount of ethylene glycol and a part of the total amount of diethylene glycol may be used in the first step, and the remaining part of the total amount of ethylene glycol and the remaining part of the total amount of diethylene glycol may be additionally added in the second step. In this case, it is preferable that the amounts of ethylene glycol and diethylene glycol used in the first step are 92.5 to 70% of the total amount, respectively, and that the amounts of ethylene glycol and diethylene glycol used in the second step are 7.5 to 30% of the total amount, respectively. However, it is preferable to use the total amount of ethylene glycol and a part of the total amount of diethylene glycol in the first step, and additionally add the remaining part of the total amount of diethylene glycol in the second step, in order to further reduce the amount of L-T2GE4 and MHET produced. In this case, it is preferable that the amount of diethylene glycol used in the first step is 92.5 to 70% of the total amount, and the amount of diethylene glycol used in the second step is 7.5 to 30% of the total amount, in order to reduce the amount of L-T2GE4 and MHET produced. In the second step, it is preferable to additionally add the remaining part of the glycol component, and then stir for 5 minutes or more to sufficiently carry out the additional ester formation reaction. Next, after this second step, in the third step, the oligomer product obtained in the second step is polycondensed to obtain a high molecular weight. The ester formation reactions (direct esterification reaction or ester exchange reaction) in the first and second steps and the polycondensation reaction in the third step may be carried out in a continuous reactor or a batch reactor, but it is preferable to use a continuous reactor in terms of economy and stability of quality.
[0037] The entire amount of sodium sulfoisophthalate may be added in the first step, or a portion of the entire amount may be added in the first step, and the remaining portion of the entire amount may be additionally added in the second step. It is preferable that the amount of sodium sulfoisophthalate used in the first step is 70 to 100% of the total amount, and that the amount of sodium sulfoisophthalate used in the second step is 0 to 30% of the total amount.
[0038] In a continuous reactor (continuous polycondensation method), the esterification reaction, the ester exchange reaction, and the melt polycondensation reaction may each be carried out in one stage, but it is preferable to carry them out in multiple stages. When the esterification reaction or the ester exchange reaction is carried out in multiple stages, the number of reaction vessels is preferably 2 to 3. When the melt polycondensation is carried out in multiple stages, the number of reaction vessels is preferably 3 to 7.
[0039] In the case of producing by the continuous polycondensation method, a slurry containing 1.02 to 1.5 mol, preferably 1.03 to 1.4 mol of all glycols per mol of all dicarboxylic acids or their ester derivatives is prepared, and this is continuously fed to an esterification reaction step containing an oligomer. The esterification reaction temperature is usually 240 to 270°C, preferably 250 to 265°C. The pressure inside the reaction vessel is usually 0.2 MPa or less, preferably 0.01 to 0.05 MPa. The polycondensation reaction temperature is usually 265 to 285°C, preferably 270 to 280°C, and the pressure inside the reaction vessel is usually 1.5 hPa or less, preferably 0.5 hPa or less. The reaction time of the esterification reaction is preferably 5 hours or less, particularly preferably 2 to 3.5 hours. The reaction time of the polycondensation reaction is preferably 3 hours or less, particularly preferably 1 to 2 hours.
[0040] In the case of production by a batch polycondensation method, the esterification reaction temperature is usually 220 to 250°C, preferably 230 to 245°C. The pressure inside the reaction vessel is usually 0.2 to 0.4 MPa, preferably 0.25 to 0.30 MPa. The polycondensation reaction may be carried out in one stage or in multiple stages. When carried out in one stage, the pressure is gradually reduced and the temperature is gradually increased to a final temperature of 260 to 280°C, preferably 265 to 275°C, and the final pressure is usually 3 hPa or less, preferably 0.5 hPa or less. The reaction time of the esterification reaction is preferably 4 hours or less, particularly preferably 2 to 3 hours. The reaction time of the polycondensation reaction is preferably 5 hours or less, particularly preferably 1 to 3 hours.
[0041] When producing a low polycondensate by continuous transesterification, a solution containing dimethyl terephthalate and 1.1 to 1.6 mol, preferably 1.2 to 1.5 mol, of glycol per 1 mol of dimethyl terephthalate is prepared and continuously fed to the transesterification step. The transesterification reaction temperature is usually 200 to 270°C, preferably 230 to 265°C. In the case of the transesterification method, it is necessary to use a transesterification catalyst in addition to the polycondensation catalyst. The obtained low polycondensate is reacted in the same manner as in the continuous polycondensation.
[0042] When producing a low polycondensate by a batch transesterification reaction, dimethyl terephthalate and 2.3 to 2.0 mol, preferably 2.2 to 2.0 mol, of glycol per mol of dimethyl terephthalate are charged into a batch reactor and the reaction is carried out in the presence of a transesterification catalyst. The obtained low polycondensate is polycondensed in the same manner as in the above-mentioned esterification reaction.
[0043] As the polycondensation catalyst, at least one of antimony compounds, germanium compounds, titanium compounds, and aluminum compounds can be used. Examples of the antimony compounds include antimony trioxide, antimony pentoxide, antimony acetate, and antimony glycoxide. Among these, antimony trioxide, antimony acetate, and antimony glycoxide are preferred, and antimony trioxide is particularly preferred. These antimony compounds are preferably contained in an amount of 50 to 400 ppm, more preferably 100 to 350 ppm, and particularly preferably 150 to 300 ppm in terms of antimony element relative to the copolymerized polyester resin to be produced.
[0044] Examples of the germanium compound include compounds such as crystalline germanium dioxide, amorphous germanium dioxide, germanium tetroxide, germanium hydroxide, germanium oxalate, germanium chloride, germanium tetraethoxide, germanium tetra-n-butoxide, and germanium phosphite. Among these, crystalline germanium dioxide and amorphous germanium dioxide are more preferred, and amorphous germanium dioxide is particularly preferred. These germanium compounds are preferably contained in an amount of 10 to 100 ppm, more preferably 30 to 70 ppm, and particularly preferably 30 to 50 ppm as germanium element in the copolymerized polyester resin to be produced.
[0045] Examples of the titanium compound include tetraalkyl titanates such as tetraethyl titanate, tetraisopropyl titanate, tetra-n-propyl titanate, and tetra-n-butyl titanate, and partial hydrolysates thereof; titanyl oxalate compounds such as titanium acetate, titanyl oxalate, ammonium titanyl oxalate, sodium titanyl oxalate, potassium titanyl oxalate, calcium titanyl oxalate, and strontium titanyl oxalate; titanium trimellitate, titanium sulfate, titanium chloride, hydrolysates of titanium halides, titanium bromine, titanium fluoride, potassium hexafluorotitanate, ammonium hexafluorotitanate, cobalt hexafluorotitanate, manganese hexafluorotitanate, titanium acetylacetonate, titanium complexes with hydroxy polycarboxylic acids or nitrogen-containing polycarboxylic acids; composite oxides of titanium and silicon or zirconium; and reaction products of titanium alkoxides with phosphorus compounds. Among these, titanium tetraisopropoxide, titanium tetrabutoxide, and potassium titanyl oxalate are preferred, and titanium tetrabutoxide is particularly preferred. These titanium compounds are preferably contained in an amount of 1 to 50 ppm, more preferably 2 to 20 ppm, and particularly preferably 3 to 10 ppm in terms of titanium element in the resulting copolymerized polyester resin.
[0046] As the polycondensation catalyst, an aluminum compound is particularly preferred from the viewpoint of recyclability (heat resistance, thermal oxidation stability). The aluminum compound is preferably used in combination with a phosphorus compound. As the aluminum compound constituting the polymerization catalyst used in producing the copolymerized polyester resin of the present invention, a known aluminum compound can be used.
[0047] Specific examples of aluminum compounds include aluminum acetate, basic aluminum acetate, aluminum lactate, aluminum chloride, aluminum hydroxide, aluminum hydroxide chloride, aluminum acetylacetonate, aluminum oxalate, and other organic aluminum compounds and partial hydrolysates thereof. Of these, carboxylates, inorganic acid salts, and chelate compounds are preferred, and among these, aluminum acetate, basic aluminum acetate, aluminum lactate, aluminum chloride, aluminum hydroxide, aluminum hydroxide chloride, and aluminum acetylacetonate are more preferred, aluminum acetate, basic aluminum acetate, aluminum chloride, aluminum hydroxide, and aluminum hydroxide chloride are even more preferred, and aluminum acetate and basic aluminum acetate are most preferred.
[0048] The amount of the aluminum compound used in the polymerization catalyst is preferably 5 to 40 ppm, more preferably 10 to 38 ppm, and even more preferably 20 to 35 ppm, of aluminum atoms remaining in the total mass of the polyester resin obtained. If the amount of aluminum atoms remaining is less than the above range, the catalytic activity may be poor. On the other hand, if the amount of aluminum atoms remaining exceeds the above range, the deterioration of thermal stability and thermo-oxidative stability may become a problem, or the generation of foreign matter and the increase in coloring due to aluminum may become a problem. As described above, even if the aluminum compound is placed under a reduced pressure environment during polyester polymerization, almost 100% of the amount used as a polymerization catalyst remains, so the amount used may be considered to be the remaining amount. If the properties of the copolymerized polyester resin can be sacrificed somewhat, the content of aluminum atoms in the copolymerized polyester resin may be 5 to 42 ppm.
[0049] The phosphorus compound used in the polymerization catalyst is not particularly limited, but in terms of the effect of improving the catalytic activity, phosphonic acid compounds and phosphinic acid compounds are preferred, and phosphonic acid compounds are more preferred.
[0050] Among these phosphorus compounds, the use of phosphorus compounds having a phenol moiety in the same molecule is preferred in terms of the effect of improving the thermal stability and thermal oxidation stability of the resin. There are no particular limitations on the phosphorus compounds having a phenol structure, but the use of one or more compounds selected from the group consisting of phosphonic acid compounds and phosphinic acid compounds having a phenol moiety in the same molecule is preferred in terms of both the effect of improving the catalytic activity and the effect of improving the thermal stability and thermal oxidation stability of the resin. Among these, the use of one or more phosphonic acid compounds having a phenol moiety in the same molecule is more preferred in terms of both the effect of improving the catalytic activity and the effect of improving the thermal stability and thermal oxidation stability of the resin.
[0051] Examples of phosphorus compounds having a phenol moiety in the same molecule include compounds represented by the following general formulas (1) and (2).
[0052] TIFF0007579527000001.tif16141
[0053] TIFF0007579527000002.tif19143
[0054] In general formulas (1) to (2), R 1 R represents a hydrocarbon group having 6 to 50 carbon atoms and containing a phenol moiety, a substituent such as a hydroxyl group, a halogen group, an alkoxyl group, or an amino group, and a hydrocarbon group having 6 to 50 carbon atoms and containing a phenol moiety. 4 R represents hydrogen, a hydrocarbon group having 1 to 50 carbon atoms, or a hydrocarbon group having 1 to 50 carbon atoms containing a substituent such as a hydroxyl group, a halogen group, an alkoxyl group, or an amino group. 2 , R 3R each independently represents hydrogen, a hydrocarbon group having 1 to 50 carbon atoms, or a hydrocarbon group having 1 to 50 carbon atoms containing a substituent such as a hydroxyl group or an alkoxyl group. However, the hydrocarbon group may contain a branched structure, an alicyclic structure such as cyclohexyl, or an aromatic ring structure such as phenyl or naphthyl. 2 and R 4 The ends of may be bonded together.
[0055] Examples of the phosphorus compound having a phenol moiety in the same molecule include p-hydroxyphenylphosphonic acid, dimethyl p-hydroxyphenylphosphonate, diethyl p-hydroxyphenylphosphonate, diphenyl p-hydroxyphenylphosphonate, bis(p-hydroxyphenyl)phosphinic acid, methyl bis(p-hydroxyphenyl)phosphinate, phenyl bis(p-hydroxyphenyl)phosphinate, p-hydroxyphenylphenylphosphinic acid, methyl p-hydroxyphenylphenylphosphinate, phenyl p-hydroxyphenylphenylphosphinate, p-hydroxyphenylphosphinic acid, methyl p-hydroxyphenylphosphinate, phenyl p-hydroxyphenylphosphinate, etc. Other examples include phosphorus compounds represented by the following general formula (3).
[0056] TIFF0007579527000003.tif77166
[0057] In the general formula (3), X1 and X2 each represent hydrogen, an alkyl group having 1 to 4 carbon atoms, or a metal having a valence of 1 or more. X1 may be a metal having a valence of 2 or more, and X2 may not be present. Furthermore, an anion corresponding to the excess valence of the metal may be disposed relative to the phosphorus compound. As the metal, Li, Na, K, Ca, Mg, and Al are preferable.
[0058] When these phosphorus compounds having a phenol moiety in the same molecule are added during polyester polymerization, the catalytic activity of the aluminum compound is improved, and the thermal stability and thermal oxidation stability of the polymerized polyester resin are also improved. The reason for this is believed to be that the hindered phenol moiety in the phosphorus compound improves the thermal stability and thermal oxidation stability of the polyester resin. In this case, if the residual amount of the phosphorus compound is less than 31 ppm, the above-mentioned effect of improving the thermal stability and thermal oxidation stability is weakened, and as a result, the effect of improving the thermal stability and thermal oxidation stability of the polyester resin of the present invention and the effect of improving coloring may not be observed.
[0059] Among the above, the phosphorus compound preferably used as the polycondensation catalyst is at least one phosphorus compound selected from the compounds represented by the following chemical formula (4) and chemical formula (5).
[0060] TIFF0007579527000004.tif75166
[0061] TIFF0007579527000005.tif71166
[0062] Irganox1222 (manufactured by BASF) is a commercially available compound represented by the above chemical formula (4), and Irganox1425 (manufactured by BASF) is a commercially available compound represented by the above chemical formula (5).
[0063] The amount of phosphorus compound used in the polymerization catalyst is preferably 31 to 104 ppm, more preferably 39 to 102 ppm, and even more preferably 48 to 92 ppm, of phosphorus atoms remaining relative to the total mass of the copolymerized polyester resin obtained. If the amount is less than the lower limit, the effect of improving thermal stability and thermal oxidation stability may be reduced. On the other hand, if the amount exceeds the upper limit, the polymerization activity may be reduced. As described above, when the phosphorus compound is placed in a reduced pressure environment during polymerization of the polyester resin, a part of the amount of the phosphorus compound initially added to the system as a catalyst is removed outside the system, but this amount removed is almost constant, so it can be said that it is appropriate to specify the amount of phosphorus atoms by taking the removal rate into consideration. When the properties of the copolymerized polyester resin can be somewhat sacrificed, the content of phosphorus atoms in the copolymerized polyester resin may be 19 to 125 ppm. With regard to thermal stability, the thermal oxidation decomposition parameter (TD) described later is preferably 0.7 or less, more preferably 0.6 or less, and most preferably 0.5 or less.
[0064] As described above, in the present invention, the ratio of phosphorus compound to aluminum compound is also important. Specifically, in the present invention, the molar ratio of phosphorus atom to aluminum atom in the polyester resin (P / Al ratio) is preferably more than 0 and not more than 2.6, more preferably 0.2 to 2.4, and even more preferably 0.4 to 2.3. Even if an aluminum compound is used alone as a polymerization catalyst, it cannot fully exert catalytic activity. By using a phosphorus compound in combination with an aluminum compound as a polymerization catalyst in a specific ratio, the catalytic activity can be sufficiently increased. If the molar ratio of phosphorus atom to aluminum atom in the polyester resin is outside the above range, it may not be possible to fully function as a polymerization catalyst.
[0065] In the present invention, in addition to the above-mentioned aluminum compound and phosphorus compound, in order to further improve the catalytic activity within a range that does not impair the effects of the present invention, metal-containing polycondensation catalysts such as titanium compounds, tin compounds, and germanium compounds may be used in combination. In that case, the germanium compound is preferably 10 ppm or less as germanium atoms relative to the mass of the obtained polyester resin, the titanium compound is preferably 3 ppm or less as titanium atoms relative to the mass of the obtained polyester resin, and the tin compound is preferably 3 ppm or less as tin atoms relative to the mass of the obtained polyester resin. However, from the purpose of the present invention, it is preferable not to use metal-containing polycondensation catalysts such as these titanium compounds, tin compounds, and germanium compounds as much as possible. In addition, antimony compounds, which are generally used as polymerization catalysts, are inferior in the effect of improving the thermal stability and thermo-oxidative stability of resins as described above, so it is better to refrain from using them in the present invention.
[0066] In the production of the copolymerized polyester resin of the present invention, an alkali metal compound and / or an alkaline earth metal compound may be used in combination in order to improve the polymerization activity or to reduce the content of linear oligomers (L-T2GE4 and MHET) in the produced copolymerized polyester resin and thereby further improve the flavor properties. Examples of the alkali metal compound and / or alkaline earth metal compound include compounds of lithium, sodium, potassium, rubidium, cesium, francium, calcium, strontium, barium, radium, beryllium, and magnesium, and preferably compounds of lithium, sodium, potassium, calcium, and magnesium, more preferably compounds of lithium, sodium, and potassium, and most preferably compounds of lithium and potassium. Specific examples of the alkali metal compound and / or alkaline earth metal compound include carboxylates such as acetates (e.g., lithium acetate) and alkoxides of these elements. These can be added to the reaction system as powders, aqueous solutions, ethylene glycol solutions, and the like. The amount of the alkali metal compound and / or alkaline earth metal compound used is such that the content of the alkali metal element and / or alkaline earth metal element (e.g., lithium element) in the copolymer polyester resin is 0.1 to 100 ppm, more preferably 0.1 to 60 ppm, and most preferably 0.1 to 50 ppm. This content is a value excluding the content of the sodium element derived from sodium sulfoisophthalate contained as a dicarboxylic acid component in the copolymer polyester resin of the present invention. If the content of the alkali metal element and / or alkaline earth metal element in the copolymer polyester resin exceeds 100 ppm, the thermal stability tends to decrease.
[0067] In the case of the direct esterification method, the polycondensation catalyst can be added before the start of the esterification reaction, or at any time between the end of the pressurized esterification reaction and the start of the initial polycondensation reaction. However, when an antimony compound or a titanium compound is used as the polycondensation catalyst, it is preferable to add it before the esterification reaction. In addition, it is preferable to add other polycondensation catalysts, heat stabilizers, and additives after the esterification reaction.
[0068] In the case of the transesterification method, the polycondensation catalyst can be added at any time from before the start of the transesterification reaction to before the start of the initial polycondensation reaction. However, since the titanium compound functions not only as a polycondensation catalyst but also as a transesterification catalyst, it is preferable to add it before the start of the transesterification reaction. In addition, it is preferable to add other polycondensation catalysts, heat stabilizers, and additives after the end of the transesterification reaction. As the transesterification catalyst, titanium compounds such as manganese acetate, magnesium acetate, and titanium tetrabutoxide are suitable. It is necessary to add the transesterification catalyst before the start of the transesterification reaction.
[0069] In addition, when a catalyst other than the above aluminum compound is used, a phosphorus compound can be used as a stabilizer. Examples of phosphorus compounds include phosphoric acid, phosphorous acid, phosphonic acid, and derivatives thereof. Suitable specific examples include phosphoric acid, trimethyl phosphate, tributyl phosphate, triphenyl phosphate, monomethyl phosphate, dimethyl phosphate, monobutyl phosphate, dibutyl phosphate, phosphorous acid, trimethyl phosphite, tributyl phosphite, methylphosphonic acid, dimethyl methylphosphonate, dimethyl ethylphosphonate, dimethyl phenylphosphonate, diethyl phenylphosphonate, and diphenyl phenylphosphonate. Among these, trimethyl phosphate and phosphoric acid are particularly suitable. These phosphorus compounds are preferably contained in an amount of 1 to 100 ppm, more preferably 3 to 70 ppm, and particularly preferably 5 to 50 ppm, based on the copolymerized polyester produced.
[0070] A cobalt compound can be blended to improve the color tone of the copolymerized polyester resin. The addition of this cobalt compound can particularly reduce the color b value. The cobalt compound is preferably contained in the copolymerized polyester resin at 0.5 to 30 ppm, more preferably 1 to 20 ppm, and particularly preferably 1 to 15 ppm, as cobalt atoms. If the content of cobalt atoms exceeds the above range, the copolymerized polyester resin will darken or become more bluish due to reduction of the cobalt metal, the color L value will be less than 50, and the color b value will be less than -5, and the commercial value will decrease. Examples of the cobalt compound include cobalt acetate, cobalt chloride, cobalt benzoate, and cobalt chromate. Among these, cobalt acetate is preferred.
[0071] The copolymerized polyester resin obtained by the above-mentioned continuous polycondensation method or batch polycondensation method is usually discharged in the form of strands from a discharge port provided at the bottom of a reaction vessel, cooled with water, and then cut into chips or sheets. EXAMPLES
[0072] Next, the present invention will be specifically described using examples and comparative examples, but the present invention is not limited to the aspects of these examples and can be appropriately modified within the scope of the present invention. The characteristic values in the examples were evaluated according to the following methods.
[0073] (1) Composition ratio of copolymer polyester resin Approximately 5 mg of a copolymer polyester resin sample was dissolved in 0.7 ml of a mixed solution of deuterated chloroform and trifluoroacetic acid (volume ratio 9 / 1), 1 The composition ratio was determined using 1 H-NMR (Varian, UNITY50).
[0074] (2) Intrinsic viscosity (IV) 0.1 g of a sample dried at 60° C. for 24 hours was precisely weighed and dissolved in 25 mL of a mixed solvent of phenol / tetrachloroethane (3 / 2 (mass ratio)), and the intrinsic viscosity (IV) was measured at 30° C. using an Ostwald viscometer.
[0075] (3) Number average molecular weight The number average molecular weight was measured by Waters gel permeation chromatography using a chloroform / hexafluoroisopropanol mixture (volume ratio = 9 / 1) as the solvent and polystyrene as the calibration standard. The polystyrene equivalent values were obtained using a chloroform / hexafluoroisopropanol mixture (volume ratio = 9 / 1) as the eluent.
[0076] (4) Carboxyl end group concentration (AV) 0.2g of sample dried at 60℃ for 24 hours was weighed out, and the weight at that time was W (g). 10ml of benzyl alcohol and the weighed sample were added to a test tube, and the test tube was immersed in an oil bath heated to 205℃, and the sample was dissolved while stirring with a glass rod. The samples when the dissolution time was 3 minutes, 5 minutes, and 7 minutes were designated A, B, and C, respectively. Next, a new test tube was prepared, and only benzyl alcohol was added and treated in the same manner, and the samples when the dissolution time was 3 minutes, 5 minutes, and 7 minutes were designated a, b, and c, respectively. Titration was performed using 0.04mol / l potassium hydroxide solution (ethanol solution) whose factor was known in advance. Phenol red was used as the indicator, and the end point was the point where the color changed from yellow-green to pale pink, and the titration amount (ml) of potassium hydroxide solution was calculated. The titration amounts of samples A, B, and C were designated XA, XB, and XC (ml). The titer of samples a, b, and c was designated as Xa, Xb, and Xc (ml). Using the titer XA, XB, and XC for each dissolution time, the titer V (ml) at dissolution time 0 minutes was calculated by the least squares method. Similarly, the titer V0 (ml) was calculated using Xa, Xb, and Xc. Then, AV was calculated according to the following formula 5. AV(eq / t)=[(V-V0)×NF×1000] / W(Equation 5) NF: Factor of 0.04 mol / l potassium hydroxide solution W: sample weight (g)
[0077] (5) Color tone (color b value and color L value) The color of the copolymer polyester resin chips was measured using a color meter (Model 1001DP, manufactured by Nippon Denshoku Industries Co., Ltd.) to determine the color b value and color L value.
[0078] (6) Melting point Measurements were performed using a differential scanning calorimeter (DSC) TAS100 type thermal analysis system manufactured by TA Instruments. 7.5±0.3 mg of polyester resin sample was placed in an aluminum pan, heated to 280°C using a melting point measuring device, held for 1 minute, and then quenched with liquid nitrogen. The sample was then heated from room temperature to 300°C at a heating rate of 20°C / min, and the melting point (Tm) was measured. Tm was the temperature at the maximum of each peak.
[0079] (7) Glass transition temperature (Tg) Using a differential scanning calorimeter (model: DSC220) manufactured by Seiko Denshi Kogyo Co., Ltd., 5 mg of the sample was heated from -40°C to 120°C at a heating rate of 10°C / min, and the endothermic curve was obtained to determine the glass transition temperature (Tg). The temperature at the intersection of the extension of the baseline below the glass transition temperature and the tangent showing the maximum slope at the transition part was determined as the glass transition temperature (Tg).
[0080] (8) Aluminum atom content 0.1 g of the sample was dissolved in 6 M hydrochloric acid solution, left for one day, and then diluted with pure water to obtain a 1.2 M hydrochloric acid measurement solution. The prepared solution sample was analyzed by high-frequency plasma emission spectrometry.
[0081] (9) Phosphorus atom content The phosphorus compound was converted to orthophosphoric acid by dry decomposition of 1 g of sample in the presence of sodium carbonate, or wet decomposition in a mixture of sulfuric acid / nitric acid / perchloric acid or a mixture of sulfuric acid / hydrogen peroxide. Next, molybdate was reacted in a 1 mol / L sulfuric acid solution to produce phosphomolybdic acid, which was then reduced with hydrazine sulfate to produce heteropoly blue. The absorbance at a wavelength of 830 nm was measured using a spectrophotometer (Shimadzu Corporation, UV-150-02). The amount of phosphorus atoms in the sample was quantified using a calibration curve prepared in advance.
[0082] (10) Titanium atom content 1 g of sample was weighed out in a platinum crucible and carbonized and incinerated in an electric furnace. The residue was melted with potassium hydrogen sulfate, and the molten material was dissolved in dilute hydrochloric acid, and the tetrabutyl titanate (TBT) content was measured using the diantipyrylmethane colorimetric method. The unit was expressed as ppm of titanium atom.
[0083] (11) Antimony Atomic Content 1 g of the sample was decomposed in a mixture of sulfuric acid and hydrogen peroxide. Sodium nitrite was then added to convert the antimony atoms to Sb 5+ Brilliant Green was added to generate a blue complex with antimony. After extracting this complex with toluene, the absorbance at a wavelength of 625 nm was measured using an absorption spectrophotometer (Shimadzu Corporation, UV-150-02), and the amount of antimony atoms in the sample was colorimetrically quantified using a calibration curve prepared in advance.
[0084] (12) Cobalt atomic content 1 g of sample was decomposed by incineration in a platinum crucible, and 6 mol / L hydrochloric acid was added and evaporated to dryness. This was dissolved in 1.2 mol / L hydrochloric acid, and the emission intensity was measured using an ICP emission spectrometer (Shimadzu Corporation, ICPS-2000). The amount of cobalt atoms in the sample was quantified using a calibration curve created in advance.
[0085] (13) Lithium atom content 1 g of the sample was weighed into a platinum crucible and pre-carbonized on a hot plate up to 400°C. Then, ashing was performed for 8 hours at 550°C using a Yamato Scientific electric furnace FO610. After ashing, a small amount of 6.0 N hydrochloric acid and hydrofluoric acid was added, acid decomposition was performed on a hot plate, and heating was performed until the acid was completely evaporated. After completion of acid decomposition, the lithium element concentration in the measurement solution obtained by volumetric determination using 20 mL of 1.2 N hydrochloric acid was measured with a high-frequency inductively coupled plasma emission spectrometer (SPECTROBLUE, Hitachi High-Tech Science Corporation), and the lithium element content in the sample was calculated.
[0086] (14) Haze value Using an injection molding machine (Meiki Seisakusho, M-150C-DM), copolymer polyester resin was melted at 280°C and a stepped molded plate with a thickness of 2 to 11 mm was molded at a mold temperature of 20°C. The haze value (%) of a 6 mm thick portion of the molded plate was measured with a haze meter (Nippon Denshoku Co., Ltd., Model NDH2000).
[0087] (15) DSC The sample was left at 120°C for 120 minutes in a Yamato DP63 dryer. Using a differential scanning calorimeter (DSC), the sample was heated from -100°C to 300°C at 20°C / min, then cooled to -100°C at 50°C / min, and then heated from -100°C to 300°C at 20°C / min. It was confirmed whether or not a melting peak was observed during the two heating processes. Those that did not show a melting peak during either of the two heating processes were marked with "○", and those that showed a melting peak during either of the two heating processes were marked with "×".
[0088] (16) Thermal stability evaluation: Thermo-oxidative decomposition parameter (TD) The intrinsic viscosity (IV) of the copolymer polyester resin was measured and recorded as the IV before the heating test ([IV]i). On the other hand, 3 g of dried copolymer polyester resin chips were placed in a glass test tube and immersed in a 280°C oil bath for 120 minutes in a nitrogen atmosphere to melt it, and the IV after heating ([IV] f1 ) was measured. [IV] i and [IV] f1 Then, TD was calculated according to the following formula: TD=0.245{[IV] f1 -1.47 -[IV] i -1.47} The smaller the thermo-oxidative decomposition parameter (TD) of a copolymer polyester resin, the higher its thermal stability.
[0089] (17)L-T2GE4 content 50 mg of copolymerized polyester resin was dissolved in 1 mL of a hexafluoroisopropanol / chloroform mixture (volume ratio = 1 / 9), and 4 mL of chloroform was added to dilute the solution. 10 mL of methanol was added to the solution to precipitate the polymer, and the solution was then centrifuged. The supernatant after centrifugation was concentrated to dryness and redissolved in 0.4 mL of dimethylformamide. This solution was used to measure the L-T2GE4 content by high performance liquid chromatography. Instrument: Waters ACQUITY UPLC Column: Waters BEH-C18 2.1 x 150 mm (Waters)
[0090] (18)MHET content 50 mg of copolymerized polyester resin was dissolved in 1 mL of a hexafluoroisopropanol / chloroform mixture (volume ratio = 1 / 9), and 4 mL of chloroform was added to dilute the solution. 10 mL of methanol was added to the solution to precipitate the polymer, and the solution was then centrifuged. The supernatant after centrifugation was concentrated to dryness and redissolved in 0.4 mL of dimethylformamide. The MHET content was measured using this solution by high performance liquid chromatography. Instrument: Waters ACQUITY UPLC Column: Waters BEH-C18 2.1 x 150 mm (Waters)
[0091] (19) Flavor The flavor was evaluated as follows: when the sum of the L-T2GE4 content and the MHET content was 100 ppm or less, it was marked with an ◎; when it was more than 100 ppm and less than 130 ppm, it was marked with an ◯; when it was more than 130 ppm and less than 190 ppm, it was marked with an ◯△; when it was more than 190 ppm and less than 240 ppm, it was marked with a △; and when it was more than 240 ppm, it was marked with an ×.
[0092] Example 1 A slurry containing purified terephthalic acid (TPA), glutaric acid (dimethyl glutarate), and sodium sulfoisophthalate (GC) (sodium sulfoisophthalate dimethyl ester (GCM)) as dicarboxylic acid components, and ethylene glycol (EG) and diethylene glycol (DEG) as glycol components was prepared. Of these raw monomers, the amounts of terephthalic acid, glutaric acid, sodium sulfoisophthalate (GC), and ethylene glycol (EG) blended in the slurry were such that the resin composition was as shown in Table 1. On the other hand, the remaining diethylene glycol (DEG) was blended in the slurry in only a portion (83.3%) of the amount required to give the resin composition shown in Table 1. The molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to the first esterification reactor in which the reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0093] To the produced oligomer, diethylene glycol was added in an amount equivalent to 20% of the amount added before the esterification reaction (the remaining amount (16.7%) necessary to give the resin composition shown in Table 1), and the mixture was stirred for 15 minutes to carry out an additional esterification reaction.
[0094] To this esterification reaction product, a certain amount of an ethylene glycol solution of an aluminum compound (basic aluminum acetate) and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added as a polymerization catalyst, and the mixture was continuously fed to the first polycondensation reactor, where the polycondensation reaction was carried out at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactant was passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of a strand from the nozzle of the die, cooled with water in a cooling bath, and then cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1.
[0095] (Examples 2 to 4) Examples 2 to 4 are examples in which the amount of sodium sulfoisophthalate (GC) was changed. Specifically, copolymerized polyester resins were obtained in the same manner as in Example 1, except that the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol were changed so that the resin composition had the values shown in Table 1. Details of the obtained copolymerized polyester resins and performance evaluations are shown in Table 1.
[0096] (Examples 5 and 6) Examples 5 and 6 are examples in which the amount of diethylene glycol (DEG) was changed. Specifically, a copolymer polyester resin was obtained in the same manner as in Example 1, except that the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol were changed so that the resin composition had the values shown in Table 1. Details of the obtained copolymer polyester resin and performance evaluation are shown in Table 1.
[0097] (Examples 7 to 9) Examples 7 to 9 are examples in which the number average molecular weight and / or the carboxyl end group concentration (AV) were changed. Specifically, copolymerized polyester resins were obtained in the same manner as in Example 1, except that the reaction conditions (average residence time of the esterification reaction) were adjusted so that the number average molecular weight and / or the carboxyl end group concentration (AV) were the values shown in Table 1. Details of the obtained copolymerized polyester resins and performance evaluation are shown in Table 1.
[0098] (Examples 10 to 12) Examples 10 to 12 are examples in which the amount of aluminum compound and / or phosphorus compound in the polymerization catalyst was changed. Specifically, copolymerized polyester resins were obtained in substantially the same manner as in Example 1, except that the amount of aluminum compound and / or phosphorus compound added was adjusted so that the amount of remaining aluminum atoms and / or phosphorus atoms was the value shown in Table 1. Details of the obtained copolymerized polyester resins and performance evaluation are shown in Table 1.
[0099] (Examples 13 and 14) Examples 13 and 14 are examples in which lithium acetate was further blended into the slurry to further improve flavor properties by reducing the linear oligomer content in the copolymerized polyester resin. Specifically, a slurry was prepared containing high-purity terephthalic acid (TPA) and sodium sulfoisophthalate (GC) as dicarboxylic acid components, glutaric acid, ethylene glycol (EG) and diethylene glycol (DEG) as glycol components, and lithium acetate. Of these raw material monomers, the blending amounts of terephthalic acid, glutaric acid, sodium sulfoisophthalate (GC), and ethylene glycol (EG) in the slurry were such that the resin composition was the value shown in Table 1. On the other hand, for the remaining diethylene glycol (DEG), only a portion (83.3%) of the amount required to give the resin composition shown in Table 1 was blended into the slurry. In addition, the molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to a first esterification reactor in which the reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting esterification reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0100] To the produced oligomer, diethylene glycol was added in an amount equivalent to 20% of the amount added before the esterification reaction (the remaining amount (16.7%) necessary to give the resin composition shown in Table 1), and the mixture was stirred for 15 minutes to carry out an additional esterification reaction.
[0101] To this esterification reaction product, a certain amount of an ethylene glycol solution of an aluminum compound (basic aluminum acetate) and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added as a polymerization catalyst, and the mixture was continuously fed to the first polycondensation reactor, where the polycondensation reaction was carried out at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactant was passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of a strand from the nozzle of the die, cooled with water in a cooling bath, and then cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1.
[0102] Example 15 Example 15 is an example in which an antimony compound and a cobalt compound were used as a polymerization catalyst instead of an aluminum compound. Specifically, a slurry was prepared containing high-purity terephthalic acid (TPA) and sodium sulfoisophthalate (GC) as dicarboxylic acid components, and ethylene glycol (EG) and diethylene glycol (DEG) as glycol components. Of these raw monomers, the amounts of terephthalic acid, glutaric acid, sodium sulfoisophthalate (GC), and ethylene glycol (EG) blended in the slurry were such that the resin composition was as shown in Table 1. On the other hand, the remaining diethylene glycol (DEG) was blended in the slurry in only a portion (83.3%) of the amount required to give the resin composition shown in Table 1. The molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to a first esterification reactor in which reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting esterification reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0103] To the produced oligomer, diethylene glycol was added in an amount equivalent to 20% of the amount added before the esterification reaction (the remaining amount (16.7%) necessary to give the resin composition shown in Table 1), and the mixture was stirred for 15 minutes to carry out an additional esterification reaction.
[0104] To this esterification reaction product, a certain amount of an ethylene glycol solution of an antimony compound (antimony trioxide), an ethylene glycol solution of a cobalt compound (cobalt acetate), and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added as polymerization catalysts, and the mixture was continuously fed to the first polycondensation reactor, where it was subjected to a polycondensation reaction at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactants were passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of strands from the nozzle of the die, cooled with water in a cooling bath, and cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1.
[0105] (Examples 16 and 17) Examples 16 and 17 are examples in which a titanium compound was used as a polymerization catalyst instead of an aluminum compound. Specifically, a slurry was prepared containing high-purity terephthalic acid (TPA) and sodium sulfoisophthalate (GC) as dicarboxylic acid components, glutaric acid, ethylene glycol (EG) and diethylene glycol (DEG) as glycol components, and lithium acetate. Of these raw monomers, the amounts of terephthalic acid, glutaric acid, sodium sulfoisophthalate (GC), and ethylene glycol (EG) in the slurry were such that the resin composition was as shown in Table 1. On the other hand, the remaining diethylene glycol (DEG) was blended in the slurry in only a portion (83.3%) of the amount required to give the resin composition shown in Table 1. The molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to a first esterification reactor in which reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting esterification reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0106] To the produced oligomer, diethylene glycol was added in an amount equivalent to 20% of the amount added before the esterification reaction (the remaining amount (16.7%) necessary to give the resin composition shown in Table 1), and the mixture was stirred for 15 minutes to carry out an additional esterification reaction.
[0107] A certain amount of a 1-butanol solution of tetrabutyl titanate (TBT) and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added to this esterification reaction product as a polymerization catalyst, and the mixture was continuously fed to the first polycondensation reactor, where the polycondensation reaction was carried out at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactant was passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of a strand from the nozzle of the die, cooled with water in a cooling bath, and then cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1.
[0108] (Examples 18 and 19) Examples 18 and 19 are examples in which titanium oxide was further blended to improve colorability. Specifically, the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol, the type and amount of the polymerization catalyst, the carboxyl end group concentration (AV), or the number average molecular weight were changed to the values shown in Table 1, and lithium acetate was blended into the slurry, and titanium oxide CR930 (manufactured by Ishihara Sangyo Kaisha, Ltd.) was added simultaneously with the polymerization catalyst so as to be 0.5 ppm (Example 18) or 12000 ppm (Example 19) relative to the polyester resin. A copolymer polyester resin was obtained in the same manner as in Example 1. Details of the obtained copolymer polyester resin and performance evaluation are shown in Table 1.
[0109] (Examples 20 and 21) Examples 20 and 21 are examples in which a toner was further blended to improve coloring properties. Specifically, the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol, the type and amount of the polymerization catalyst, the carboxyl end group concentration (AV), or the number average molecular weight were changed to the values shown in Table 1, and further, Solvent Blue 45 (Clariant) was added as a toner at the same time as the polymerization catalyst so that the amount was 0.1 ppm (Example 20) or 50 ppm (Example 21) relative to the polyester resin. A copolymer polyester resin was obtained in the same manner as in Example 1. Details of the obtained copolymer polyester resin and performance evaluation are shown in Table 1.
[0110] (Examples 22 and 23) In Examples 22 and 23, the amount of glutaric acid was increased (Example 22) or decreased (Example 23), and the same procedure as in Example 1 was followed to obtain a copolymer polyester resin. Details of the obtained copolymer polyester resin and performance evaluation are shown in Table 1. (Example 24) Example 24 is an example in which the amount of diethylene glycol added was reduced. Specifically, a slurry was prepared containing high-purity terephthalic acid (TPA), glutaric acid (dimethyl glutarate), and sodium sulfoisophthalate (GC) (sodium sulfoisophthalate dimethyl ester (GCM)) as dicarboxylic acid components, and ethylene glycol (EG) and diethylene glycol (DEG) as glycol components. Of these raw monomers, the amounts of terephthalic acid, glutaric acid, sodium sulfoisophthalate (GC), and ethylene glycol (EG) blended in the slurry were such that the resin composition was as shown in Table 1. On the other hand, the remaining diethylene glycol (DEG) was blended in the slurry in only a portion (92.0%) of the amount required to give the resin composition shown in Table 1. The molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to the first esterification reactor in which the reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0111] To the produced oligomer, diethylene glycol was added in an amount equivalent to 8.7% of the amount added before the esterification reaction (the remaining portion (8%) of the amount necessary to give the resin composition shown in Table 1), and the mixture was stirred for 15 minutes to carry out an additional esterification reaction.
[0112] To this esterification reaction product, a certain amount of an ethylene glycol solution of an aluminum compound (basic aluminum acetate) and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added as a polymerization catalyst, and the mixture was continuously fed to the first polycondensation reactor, where the polycondensation reaction was carried out at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactant was passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of a strand from the nozzle of the die, cooled with water in a cooling bath, and then cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1. (Example 25) Example 25 is an example in which the amount of diethylene glycol added was increased. Specifically, a slurry was prepared containing high-purity terephthalic acid (TPA), glutaric acid (dimethyl glutarate), and sodium sulfoisophthalate (GC) (sodium sulfoisophthalate dimethyl ester (GCM)) as dicarboxylic acid components, and ethylene glycol (EG) and diethylene glycol (DEG) as glycol components. Of these raw monomers, the amounts of terephthalic acid, glutaric acid, sodium sulfoisophthalate (GC), and ethylene glycol (EG) blended in the slurry were such that the resin composition was as shown in Table 1. On the other hand, the remaining diethylene glycol (DEG) was blended in the slurry in only a portion (76.9%) of the amount required to give the resin composition shown in Table 1. The molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to the first esterification reactor in which the reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0113] To the produced oligomer, diethylene glycol was added in an amount equivalent to 30% of the amount added before the esterification reaction (the remaining amount (23.1%) necessary to give the resin composition shown in Table 1), and the mixture was stirred for 15 minutes to carry out an additional esterification reaction. (Example 26) Example 26 is an example in which both ethylene glycol and diethylene glycol were additionally added. Specifically, a slurry was prepared containing high-purity terephthalic acid (TPA), glutaric acid (dimethyl glutarate), and sodium sulfoisophthalate (GC) (sodium sulfoisophthalate dimethyl ester (GCM)) as dicarboxylic acid components, and ethylene glycol (EG) and diethylene glycol (DEG) as glycol components. Of these raw material monomers, the amounts of terephthalic acid, glutaric acid, and sodium sulfoisophthalate (GC) in the slurry were such that the resin composition was as shown in Table 1. On the other hand, the remaining ethylene glycol (EG) and diethylene glycol (DEG) were blended in the slurry in only a portion (EG: 90.9%, DEG: 90.9%) of the amount required to give the resin composition shown in Table 1. The molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously fed to a first esterification reactor in which the reactants had previously remained. Next, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C for an average residence time of 3 hours. The resulting reaction product was transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C for an average residence time of 1 hour. Next, the resulting reaction product was transferred to a third esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C.
[0114] To the produced oligomer, diethylene glycol in an amount equivalent to 10% of the amount added before the esterification reaction (the remaining part (9.1%) of the amount necessary to give the resin composition shown in Table 1) and ethylene glycol in an amount equivalent to 10% of the amount added before the esterification reaction (the remaining part (9.1%) of the amount necessary to give the resin composition shown in Table 1) were further added, and the mixture was stirred for 15 minutes to carry out an additional esterification reaction.
[0115] To this esterification reaction product, a certain amount of an ethylene glycol solution of an aluminum compound (basic aluminum acetate) and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added as a polymerization catalyst, and the mixture was continuously fed to the first polycondensation reactor, where the polycondensation reaction was carried out at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactant was passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of a strand from the nozzle of the die, cooled with water in a cooling bath, and then cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1.
[0116] Comparative Example 1 Comparative Example 1 is an example in which glutaric acid and sodium sulfoisophthalate were not used as the dicarboxylic acid component, and only terephthalic acid was used. Specifically, a copolymer polyester resin was obtained in the same manner as in Example 1, except that the blending ratios of terephthalic acid, ethylene glycol, and diethylene glycol were changed so that the resin composition had the values shown in Table 1. Details of the obtained copolymer polyester resin and performance evaluation are shown in Table 1.
[0117] Comparative Example 2 Comparative Example 2 is an example in which the amount of glutaric acid is too small. Specifically, a copolymerized polyester resin was obtained in the same manner as in Example 1, except that the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol were changed so that the resin composition had the values shown in Table 1. Details of the obtained copolymerized polyester resin and performance evaluation are shown in Table 1.
[0118] Comparative Example 3 Comparative Example 3 is an example in which the amount of glutaric acid is too large. Specifically, a copolymerized polyester resin was obtained in the same manner as in Example 1, except that the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol were changed so that the resin composition had the values shown in Table 1. Details of the obtained copolymerized polyester resin and performance evaluation are shown in Table 1.
[0119] Comparative Example 4 Comparative Example 4 is an example in which the amount of diethylene glycol (DEG) is too large. Specifically, a copolymerized polyester resin was obtained in the same manner as in Example 1, except that the blending ratios of terephthalic acid, sodium sulfoisophthalate, glutaric acid, ethylene glycol, and diethylene glycol were changed so that the resin composition had the values shown in Table 1. Details of the obtained copolymerized polyester resin and performance evaluation are shown in Table 1.
[0120] Comparative Example 5 Comparative Example 5 is an example in which no additional glycol component was added. Specifically, a slurry containing high-purity terephthalic acid (TPA), glutaric acid, and sodium sulfoisophthalate (GC) as dicarboxylic acid components, and ethylene glycol (EG) and diethylene glycol (DEG) as glycol components was prepared so that the resin composition was the value shown in Table 1. However, the molar ratio (G / A) of the total glycol components to the dicarboxylic acid components in the slurry was adjusted to 2.2. Next, this slurry was continuously supplied to the first esterification reactor in which the reactants had previously remained. Then, an esterification reaction was carried out under stirring at an internal pressure of 0.15 MPa and 257°C so that the average residence time was 3 hours. The resulting reactants were transferred to a second esterification reactor, and an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and 257°C so that the average residence time was 1 hour. The reaction mixture was then transferred to a third esterification reactor, where an esterification reaction was carried out under stirring at an internal pressure of 0.05 MPa and at 257°C.
[0121] To this esterification reaction product, a certain amount of an ethylene glycol solution of an aluminum compound (basic aluminum acetate) and an ethylene glycol solution of a phosphorus compound (Irganox1222: the compound of the above-mentioned chemical formula (4)) were added as a polymerization catalyst, and the mixture was continuously fed to the first polycondensation reactor, where the polycondensation reaction was carried out at 261°C and 6.7kPa for 1 hour under stirring, then at 272°C and 0.6kPa for 1 hour in the second polycondensation reactor, and further at 275°C and 0.10-0.20kPa for 1 hour under stirring in the final polycondensation reactor. After the polycondensation reaction, the reactant was passed through a polymer filter, and the molten copolymerized polyester resin was extracted in the form of a strand from the nozzle of the die, cooled with water in a cooling bath, and then cut into chips. Details of the obtained copolymerized polyester resin and its performance evaluation are shown in Table 1.
[0122] [Table 1] JPEG0007579527000007.jpg233107
[0123] As can be seen from Table 1, Examples 1 to 26, which satisfy all the requirements of the present invention, are excellent in flavor, transparency value, DSC measurement, and recyclability (thermal stability). In contrast, Comparative Example 1 does not use glutaric acid and sodium sulfoisophthalate as dicarboxylic acid components, but uses only terephthalic acid, and Comparative Example 2 has poor transparency (haze value) and poor recyclability (thermal stability) because the amount of glutaric acid is too small. Comparative Example 3 has a high content of by-product oligomers (L-T2GE4 and MHET) because the amount of glutaric acid is too large, and therefore has poor flavor. Comparative Example 4 has a high amount of diethylene glycol (DEG), and therefore has poor recyclability (thermal stability) and a high color b value. Comparative Example 5 has all the glycol components added from the beginning, and therefore has an extremely high content of by-product oligomers (L-T2GE4 and MHET), and therefore has extremely poor flavor. [Industrial Applicability]
[0124] The copolymer polyester resin obtained by the manufacturing method of the present invention has the advantages of transparency and moldability due to the use of diethylene glycol and sodium sulfoisophthalate, and is also excellent in flavor, and the resin does not become discolored or its molecular weight is not reduced during recycling. Therefore, the present invention will make a great contribution to the industrial world.
Claims
1. A method for producing a copolymer polyester resin, comprising the steps of: The copolymerized polyester resin contains terephthalic acid as a main component of the dicarboxylic acid component and ethylene glycol as a main component of the glycol component, and when the total amount of the dicarboxylic acid components in all the polyester resin components is taken as 100 mol %, the ratio of the terephthalic acid component to all the dicarboxylic acid components is 74.95 to 94.95 mol %, the ratio of the glutaric acid to all the dicarboxylic acid components is 5 to 25 mol %, the ratio of sodium sulfoisophthalate to all the dicarboxylic acid components is 0.05 to 10 mol %, and the total amount of the glycol components is 100 mol %. % by mole, the ratio of ethylene glycol to the total glycol components is 50 to 99 mol %, the ratio of diethylene glycol to the total glycol components is 1 to 22 mol %, the content of free linear oligomers composed of terephthalic acid, glutaric acid, and ethylene glycol in the copolymerized polyester resin is 90 ppm or less and the content of free linear oligomers composed of terephthalic acid and ethylene glycol in the copolymerized polyester resin is 100 ppm or less, and the carboxyl end group concentration (AV) of the copolymerized polyester resin is 3 to 50 eq / t, The production method includes a first step of carrying out an ester formation reaction using at least a portion of the total amount of terephthalic acid, glutaric acid, and sodium sulfoisophthalate as raw material monomers of the dicarboxylic acid component, and at least a portion of the total amount of ethylene glycol and / or at least a portion of the total amount of diethylene glycol as raw material monomers of the glycol component to generate an oligomer; a second step of additionally adding the remaining portion of the total amount of sodium sulfoisophthalate and / or the remaining portion of the total amount of ethylene glycol and / or the remaining portion of the total amount of diethylene glycol to the oligomer product obtained in the first step to carry out an additional ester formation reaction; and a third step of polycondensing the oligomer product obtained in the second step to increase its molecular weight. A method for producing a copolymer polyester resin comprising the steps of:
2. 2. The method for producing a copolymer polyester resin according to claim 1, wherein the first step uses the entire amount of ethylene glycol and a part of the entire amount of diethylene glycol, and the second step additionally adds the remaining part of the entire amount of diethylene glycol.
3. The method for producing a copolymerized polyester resin according to claim 2, characterized in that the amount of diethylene glycol used in the first step is 92.5 to 70% of the total amount (mol %), and the amount of diethylene glycol used in the second step is 7.5 to 30% of the total amount (mol %).
4. 2. The method for producing a copolymer polyester resin according to claim 1, wherein the produced copolymer polyester resin has a color b value of −5.0 to 25.
0.
5. 2. The method for producing a copolymerized polyester resin according to claim 1, wherein an aluminum compound and a phosphorus compound are used as polymerization catalysts, the produced copolymerized polyester resin contains aluminum atoms and phosphorus atoms derived from these polymerization catalysts, the content of aluminum atoms in the copolymerized polyester resin is 5 to 40 ppm, and the molar ratio of phosphorus atoms to aluminum atoms in the copolymerized polyester resin is more than 0 and not more than 2.
6.
6. A method for producing a copolymerized polyester resin as described in claim 1, characterized in that an alkali metal compound and / or an alkaline earth metal compound other than sodium sulfoisophthalate is used, the produced copolymerized polyester resin further contains alkali metal atoms and / or alkaline earth metal atoms derived from these compounds, and the content of the alkali metal atoms and / or alkaline earth metal atoms in the copolymerized polyester resin is 1 to 100 ppm.
7. 2. The method for producing a copolymer polyester resin according to claim 1, wherein a stepped molded plate obtained by molding the produced copolymer polyester resin has a haze value of 20% or less at a portion having a thickness of 6 mm.
8. A method for producing a molded article, comprising: producing a copolymer polyester resin by the method according to any one of claims 1 to 7; and producing a molded article by using the produced copolymer polyester resin.
9. A method for producing a heat-shrinkable film, comprising: producing a copolymer polyester resin by the method according to any one of claims 1 to 7; and producing a heat-shrinkable film by using the produced copolymer polyester resin.
10. A method for producing fibers, comprising producing a copolymer polyester resin by the method according to any one of claims 1 to 7, and using the produced copolymer polyester resin to produce fibers.
11. A method for producing a nonwoven fabric, comprising: producing a copolymer polyester resin by the method according to any one of claims 1 to 7; and producing a nonwoven fabric by using the produced copolymer polyester resin.
12. A method for producing an adhesive, comprising: producing a copolymer polyester resin by the method according to any one of claims 1 to 7; and producing an adhesive by using the produced copolymer polyester resin.
13. A method for producing a paint, comprising: producing a copolymer polyester resin by the production method according to any one of claims 1 to 7; and producing a paint by using the produced copolymer polyester resin.
Citation Information
Patent Citations
Stretched aromatic polyester film and preparation method thereof
JP2001114912A
Method for manufacturing polyester resin and the same obtained thereby
JP2002047340A
Method for continuous production of copolyester
JP2007254660A
Polyester
JP2019131636A
Waterrservice installation