Activated Amino-Containing Metal-Organic Framework (MOF) Compositions, Methods of Making and Using the Same
By washing and drying MOFs with acids to remove modifiers, the process enhances the adsorption properties of larger crystals, addressing handling difficulties and maintaining adsorption efficiency for contaminants.
Patent Information
- Application Number
- JP2022559295
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing metal-organic frameworks (MOFs) with nano-sized crystals are difficult to handle and may not be suitable for certain applications, and the use of modifiers to synthesize larger crystals reduces their gas adsorption activity, particularly when linker molecules have an amino moiety.
A process involving washing as-synthesized MOFs with hydrochloric acid, nitric acid, or sulfuric acid to remove modifiers, followed by drying, restores the adsorption properties of MOFs with amino groups, achieving crystal sizes of at least 1 μm and activating at least 55% of the amino groups to their unsubstituted form.
The process results in MOFs with adsorption properties comparable to nanocrystalline-sized MOFs, enabling effective adsorption of contaminants such as cyanogen chloride and hydrogen sulfide, with increased efficiency and capacity.
Smart Images

Figure 0007579593000004 
Figure 0007579593000005 
Figure 0007579593000006
Abstract
Description
[Technical field]
[0001] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT This invention was made with U.S. Government support under Contract No. W911SR18C0031 awarded by the U.S. Army Combat Capabilities Development Command Chemical Biological Center (CCDC CBC). The Government has certain rights in this invention. CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 003,260, filed March 30, 2020. Technical Field
[0003] The present invention relates to metal organic framework (MOF) compositions having linker molecules with amino groups. The present invention further relates to processes for preparing and activating the amino groups of the MOF compositions, and methods for using the MOF compositions. [Background technology]
[0004] Metal-organic framework (MOF) materials are well known and are used in many applications such as air filtration, gas supply, etc. Most MOFs synthesized consist of nano-sized crystals. However, nanocrystals are difficult to handle and may not be suitable for some applications. Therefore, research is being conducted to control the crystal size of MOFs. One method to control the crystal size of MOFs is to use modifiers such as carboxylic acids, e.g., formic acid, acetic acid, etc.
[0005] Applicants have found that when modulating agents are used to synthesize larger crystal size MOF compositions, their resulting activity for gas adsorption is reduced relative to nanocrystalline size MOF compositions. This is especially true when at least one of the linker molecules has an amino moiety. Applicants have solved this problem by finding a process that involves washing the as-synthesized MOF composition (having an average crystal size of at least 1 μm) with an acid such as hydrochloric acid, nitric acid, or sulfuric acid. When the washed MOFs are dried, they are found to have similar adsorption properties as the nanocrystalline size MOF compositions. Summary of the Invention
[0006] One embodiment of the present invention is a metal-organic framework (MOF) composition comprising a corner metal unit comprising a metal ion atom, the metal being selected from Zr, V, Al, Fe, Cr, Ti, Hf, Cu, Zn, Ni, Ce, and mixtures thereof, and a linker molecule selected from at least one organic ligand comprising an amino group or a combination of at least one organic ligand comprising an amino group and at least one organic ligand not comprising an amino group, the MOF having an average crystal size of 1 μm or more, and at least 55% of the amino groups are activated amino groups in the form of -NH2.
[0007] In another embodiment, the at least one organic ligand comprising an amino group is selected from 2-aminobenzene-1,4 dicarboxylic acid (NH2-BDC), 5-aminoisophthalic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, and mixtures thereof.
[0008] In yet another embodiment, the at least one organic ligand that does not include an amino group is selected from terephthalic acid (BDC), isophthalic acid, benzoic acid, trimesic acid, acrylic acid, and mixtures thereof.
[0009] In certain embodiments, the corner metal unit comprises a zirconium atom and the linker comprises a ligand that is 2-aminobenzene-1,4 dicarboxylic acid (NH2-BDC).
[0010] In another embodiment, the MOF has a molecular weight of at least 1000 m 2 / g BET surface area.
[0011] In yet another embodiment, the MOFs have an average crystal size of from about 1 μm to about 100 μm.
[0012] In another embodiment, the MOF has pores of about 5 to about 30 Å.
[0013] In a further embodiment, at least one corner metal unit of the MOF has at least one free coordination site.
[0014] In another embodiment, the MOFs are capable of adsorbing at least one contaminant from a gas stream.
[0015] In yet another embodiment, the contaminant that the MOF can adsorb may be selected from the group consisting of cyanogen chloride, hydrogen cyanide, hydrogen sulfide, phosgene, sulfur dioxide, boron tribromide, boron trichloride, bromine, bromine chloride, bromine trifluoride, carbonyl fluoride, chlorine, chlorine pentafluoride, chlorine trifluoride, chlorosulfonic acid, dichlorosilane, ethylphosphonic dichloride, fluorine, hydrogen bromide, hydrogen chloride, hydrogen cyanide, hydrogen fluoride, hydrogen iodide, hydrogen sulfide, phosphorus trichloride, silicon tetrafluoride, sulfur dioxide, sulfur trioxide, sulfuric acid, sulfuryl chloride, titanium tetrachloride, tungsten hexafluoride, bromine pentafluoride, hydrogen selenide, nitric acid, nitrogen dioxide, nitrogen tetroxide, nitrogen trioxide, and mixtures thereof.
[0016] Another embodiment is a method for preparing a metal-organic framework (MOF) composition, comprising: a. forming a reaction mixture of a metal compound, the metal being selected from Zr, V, Al, Fe, Cr, Ti, Hf, Cu, Zn, Ni, Ce, and mixtures thereof, a ligand selected from at least one organic ligand comprising an amino group or a combination of at least one organic ligand comprising an amino group and at least one organic ligand not comprising an amino group, a solvent selected from dimethylformamide, water, ethanol, isopropanol, and mixtures thereof, and a modifier selected from an organic acid, preferably a monocarboxylic acid such as formic acid, acetic acid, benzoic acid, dichloroacetic acid, trifluoroacetic acid, and mixtures thereof, optionally mixed with one or more inorganic acids such as hydrochloric acid, nitric acid, and sulfuric acid; b. reacting the reaction mixture at a temperature and for a time to form the MOF; c. isolating the MOF to provide a powder of the MOF; d. washing the MOF with an inorganic acid selected from hydrochloric acid, nitric acid, sulfuric acid, and mixtures thereof, and optionally mixing with one or more organic acids, to provide MOFs characterized in that at least 55% of the amino groups are activated amino groups in the form of -NH2 and have an average crystal size greater than 1 μm.
[0017] In another embodiment, the acid washed MOFs are dried at a temperature of about 60°C to about 150°C or about 60°C to about 200°C.
[0018] A further embodiment is a method for purifying a gas stream comprising contacting the gas stream containing at least one contaminant with a metal-organic framework (MOF) composition, thereby removing at least a portion of the at least one contaminant in the gas stream, wherein the MOF comprises a corner metal unit comprising a metal ion atom, the metal being preferably selected from Zr, V, Al, Fe, Cr, Ti, Hf, Cu, Zn, Ni, Ce, and mixtures thereof, and a linker molecule selected from at least one organic ligand comprising an amino group or a combination of at least one organic ligand comprising an amino group and at least one organic ligand not comprising an amino group, wherein the MOF has an average crystal size of at least about 1 μm, and wherein at least 55% of the amino groups are activated amino groups in the form of -NH2.
[0019] In another embodiment, the gas stream is an air stream and the contaminant is selected from cyanogen chloride, hydrogen cyanide, hydrogen sulfide, phosgene, sulfur dioxide, boron tribromide, boron trichloride, bromine, bromine chloride, bromine trifluoride, carbonyl fluoride, chlorine, chlorine pentafluoride, chlorine trifluoride, chlorosulfonic acid, dichlorosilane, ethylphosphonic dichloride, fluorine, hydrogen bromide, hydrogen chloride, hydrogen cyanide, hydrogen fluoride, hydrogen iodide, hydrogen sulfide, phosphorus trichloride, silicon tetrafluoride, sulfur dioxide, sulfur trioxide, sulfuric acid, sulfuryl chloride, titanium tetrachloride, tungsten hexafluoride, bromine pentafluoride, hydrogen selenide, nitric acid, nitrogen dioxide, nitrogen tetroxide, nitrogen trioxide, and mixtures thereof.
[0020] In still further embodiments, the MOF removes at least 50%, or at least 90%, or at least 99% of the contaminants.
[0021] These and other objects and embodiments will become apparent after a detailed description of the invention. [Brief description of the drawings]
[0022] [Figure 1A]Micrograph of commercial Zr(NH2-BDC) chunks with small nano-sized particles (2.00 μm scale).
[0023] [Figure 1B] A micrograph of Zr(NH2-BDC)-NH2 of Example 1-1, which has a crystal size of 1 to 5 μm (10 μm scale).
[0024] [Figure 2A] 1H-NMR spectra of various Zr(NH2-BDC) decomposition preparations. The inset shows the crystallographic structure of Zr(NH2-BDC) with the formamide group still remaining.
[0025] [Figure 2B] 1 shows the solid-state 15N-NMR spectrum of the Zr(NH2-BDC) formulation before decomposition.
[0026] [Diagram 3] We demonstrate the decomposition of Zr(NH2-BDC) MOF to determine the extent of formamide groups.
[0027] [Figure 4] We show that MOFs bearing formamide groups are washed with acid to convert the formamide groups to free amines. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] In accordance with the disclosure herein, amino-group-containing metal-organic framework (MOF) compositions have been synthesized with an average crystal size of at least about 1 μm or greater, the amino groups have been activated to provide 55% or more of free amino groups in the form of -NH2, and the MOFs have a crystal size of at least 1000 m 2 / g BET surface area. Prior to the invention as disclosed herein, MOFs with crystals of at least about 1 μm (micron) containing linker molecules with free amino groups were difficult to synthesize. Micron-sized MOFs as disclosed herein are advantageous in applications such as air filtration, toxic gas capture, and respirators.
[0029] As used herein, the term "activated" when referring to an amino group means that the amino group is an unsubstituted group of formula -NH2, and the nitrogen atom is bonded to an organic ligand of the MOF.
[0030] In one aspect of the invention, MOFs are the coordination products of metal ions and at least bidentate organic ligands. MOFs contain corner metal units that contain metal ion atoms and linker or ligand molecules to form structures with high surface areas and uniformly sized pores. The metal ions are Li + , Na + , K + , Rb + , Be 2+ , Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ , Sc 3+ , Y 3+ , Ti 4+ , Zri 4+ , Hf 4+ , V 5+ , V 4+ , V 3+ , Nb 3+ , Ta 3+ ,Cr 3+ ,Cr 2+ , Mo 3+ , W 3+ , Mn 3+ , Fe 3+ , Fe 2+ , Ru 3+ , Ru 2+ , Os 3+ , Os 2+ , Co 3+ , Co 2+ , Ni 2+ , Ni+ , Pd 2+ , Pd + , Pt 2+ , Pt + , Cu 2+ ,Cu + , Ag + , Au + , Zn 2+ , Al 3+ , Ga 3+ , In 3+ , Si 4+ , Si 2+ , Ge 4+ , Ge 2+ , Sn 4+ , Sn 2+ , Bi 5+ , Bi 3+ , Cd 2+ , Mn 2+ , Tb 3+ , Gd 3+ , Ce 3+ , La 3+ ,Cr 4+ and mixtures thereof. A preferred set or subset of the above metals includes, but is not limited to, Zr, V, Al, Fe, Cr, Ti, Hf, Cu, Zn, Ni, and Ce.
[0031] The organic ligands that react with the metal ions to form linkers between the corner metal units are selected from at least one organic ligand containing an amino group, or a combination of at least one organic ligand containing an amino group and at least one organic ligand that does not contain an amino group. Examples of organic ligands that contain an amino group include, but are not limited to, 2-aminobenzene-1,4-dicarboxylic acid (NH2-BDC), 5-aminoisophthalic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, and mixtures thereof. Examples of organic ligands that do not contain an amino group include, but are not limited to, terephthalic acid (BDC), isophthalic acid, benzoic acid, trimesic acid, acrylic acid, and mixtures thereof. When the ligands are a combination of at least one organic ligand containing an amino group and at least one organic ligand not containing an amino group, the molar ratio of amino-containing ligands to non-amino-containing ligands in the MOF product varies from 1:99 to 99:1, or 10:90 to 90:10, or 20:80 to 80:20, or 30:70 to 70:30, or 40:60 to 60:40, or 50:50.
[0032] In one embodiment, the metal of the corner metal unit comprises Zr and the organic ligand comprises 2-aminobenzene-1,4 dicarboxylic acid (NH2-BDC). In one embodiment, the MOF is Zr(NH2-BDC), also known as UiO-66-NH2.
[0033] The MOFs of the present invention are characterized by the following properties: One property is a molecular weight of at least 1,000, or at least 1,100, or at least 1,200, or at least 1,300 m 2 / g, or at least 1,400 m 2 / g Brunauer-Emmett-Teller (BET) surface area. Another characteristic is that the MOF has an average crystal size of at least 1 μm, or at least 5 μm, or at least 50 μm along at least one dimension. More specifically, the crystal size is at least about 1 μm to about 100 μm, or about 1 μm to about 10 μm, or about 1 μm to about 5 μm, or about 10 μm to about 50 μm. By crystal size, the size of the individual crystals is meant, not the size of the crystals agglomerated into aggregates. When an average size, e.g., 1 μm, is given, it is understood that the crystals have that particular average size in at least one dimension, but may be less or greater in size in the other two dimensions. That is, the crystals need not have a cubic shape, but can have any shape, such as octahedrons, octahedrons with a truncated top plane, cuboctahedrons, needles, etc.
[0034] MOFs have the general property of having an open pore system. The MOFs of the present invention have an average pore diameter of about 5 to about 30 Å, or about 5 to about 20 Å, or about 5 to about 10 Å.
[0035] The MOFs of the present invention have a pore volume of from about 0.2 cc / g to about 0.8 cc / g, or from about 0.3 to about 0.8 cc / g, or from about 0.4 to about 0.8 cc / g, or from 0.5 to about 0.8 cc / g, or from about 0.4 to about 0.7 cc / g, or from about 0.4 to about 0.6 cc / g.
[0036] The metal ions forming the corner metal units can have all of their coordination sites occupied or at least one free or open coordination site, hi certain embodiments, at least one corner metal unit has at least one free coordination site.
[0037] The MOFs of the present invention have numerous applications. One particular application is the purification of gas streams by at least partially adsorbing at least one contaminant found in the gas stream. Gas streams that can be purified include, but are not limited to, air streams, industrial gas streams, off-gas streams, or polluted gas streams.
[0038] Contaminants that can be adsorbed onto MOFs include, but are not limited to, cyanogen chloride, hydrogen cyanide, hydrogen sulfide, phosgene, sulfur dioxide, boron tribromide, boron trichloride, bromine, bromine chloride, bromine trifluoride, carbonyl fluoride, chlorine, chlorine pentafluoride, chlorine trifluoride, chlorosulfonic acid, dichlorosilane, ethylphosphonic dichloride, fluorine, hydrogen bromide, hydrogen chloride, hydrogen cyanide, hydrogen fluoride, hydrogen iodide, hydrogen sulfide, phosphorus trichloride, silicon tetrafluoride, sulfur dioxide, sulfur trioxide, sulfuric acid, sulfuryl chloride, titanium tetrachloride, tungsten hexafluoride, bromine pentafluoride, hydrogen selenide, nitric acid, nitrogen dioxide, nitrogen tetroxide, nitrogen trioxide, and mixtures thereof.
[0039] MOFs with large crystal sizes of about 1μ or more are preferred over MOFs with small crystal sizes or nanocrystalline, especially for applications involving the adsorption of pollutants. The inventors have found that the modifiers used to synthesize larger than nano-sized crystals of MOFs with amino groups convert the amino groups to amide groups, which do not react when amino functionality is required. The inventors have also found that treatment of as-synthesized MOFs with an acid such as HC1 (see below) essentially cleaves the amide and regenerates, i.e., activates, the amino groups. MOFs treated as disclosed herein have at least 55%, or at least 60%, or at least 65%, or at least 70%, or at least 75%, or at least 80%, or at least 85%, or at least 90%, or at least 95% of their amino groups activated. Such increased amino activation results in an increase in the adsorption capacity or other amino functionality of the MOF relative to untreated MOFs. Thus, the MOFs of the present invention have the advantage that they are large crystals and have the same or substantially the same adsorption capacity or other amino functionality as MOFs with nano-sized crystals, which is a major advance in the synthesis of MOFs with substantially the same adsorption capacity or other amino functionality as nano-sized MOFs for applications where nano-sized MOFs cannot be used.
[0040] As used above and throughout this specification and claims, "substantially" means at least 70%, or at least 80%, or at least 90%, or at least 95%.
[0041] Another aspect of the invention is a method for preparing MOFs with activated amino groups. The first step of the synthesis is to prepare a solution of the desired metal ion and at least one ligand. The metal is introduced as a metal salt. The salt can be a nitrate, halide, sulfate, carbonate, oxyhalide, oxynitrate, oxysulfate, oxycarbonate, etc., and mixtures thereof. Specific examples of salts that can be used include, but are not limited to, zirconium chloride, zirconium bromide, oxynitrate, zirconium, zirconium oxychloride, vanadium chloride, copper sulfate, iron chloride, zinc nitrate, or zinc carbonate, and mixtures thereof.
[0042] As mentioned above, the ligands used may be at least one organic ligand containing an amino group or a combination of at least one organic ligand containing an amino group and at least one organic ligand not containing an amino group. Examples of organic ligands containing an amino group include, but are not limited to, 2-aminobenzene-l,4 dicarboxylic acid (NH2-BDC), 5-aminoisophthalic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, and mixtures thereof. Examples of organic ligands not containing an amino group include, but are not limited to, terephthalic acid (BDC), isophthalic acid, benzoic acid, trimesic acid, acrylic acid, and mixtures thereof. When a mixture of amino and non-amino containing ligands is used in the synthesis, they are added in a molar ratio to achieve the desired molar ratio in the MOF as described above. The molar ratio of the metal salt to the ligand is also adjusted to achieve a specific molar ratio in the MOF.
[0043] The metal salt and at least one ligand are mixed in a solvent or mixture of solvents. Examples of solvents that can be used include, but are not limited to, amides, alcohols, water, and mixtures thereof. Specific mixtures include dimethylformamide, water, ethanol, isopropanol, etc.
[0044] The modifier is added to the reaction mixture either before, during, or after the addition of other reagents. Preferably, the modifier comprises at least one monocarboxylic acid. Specific examples of monocarboxylic acid modifiers include, but are not limited to, formic acid, acetic acid, benzoic acid, dichloroacetic acid, trifluoroacetic acid, and mixtures thereof. Optionally, the modifier can be a mixture of one or more monocarboxylic acids and one or more inorganic acids, such as hydrochloric acid, nitric acid, and sulfuric acid. Those skilled in the art will recognize that the order of addition of reagents can be changed to optimize solubility and reaction conditions.
[0045] Once the reaction mixture is formed, i.e., all components are solubilized, the reaction mixture is reacted at a temperature and for a time to form the desired MOF. The reaction temperature can vary from about 50° C. to about 200° C., or from about 75° C. to about 125° C. The reaction mixture is reacted at the desired temperature for a time selected from about 1 hour to about 78 hours, about 8 hours to about 48 hours, about 22 hours to about 48 hours, about 12 hours to about 24 hours. Once the MOF is formed, it is isolated by a method such as filtration or centrifugation.
[0046] When amino-containing MOFs are prepared with a modifier in the reaction mixture, the result can be a product in which at least one of the hydrogen atoms of the amino group is replaced with another site, thereby interfering with the desired activity of the amino group. The replacement site can be a residue of a modifier, such as a monocarboxylate. For example, when formic acid is used as a modifier, the formic acid group can become a substituent of the amino group, resulting in a formamide group instead of the desired unsubstituted amino group. Furthermore, when DMF is used as a solvent, a portion of the solvent can react with a portion of the amino group to form a formamide group.
[0047] According to one aspect of the invention, this problem is solved by washing the MOFs with an inorganic acid to cleave the substituents from the amino groups and restore the amino groups to their unsubstituted activated form, as shown in FIG. 4. In one embodiment, the MOF powder isolated from the metal-ligand reaction mixture is then washed with an acid wash comprising at least one inorganic acid, such as hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, hydrofluoric acid, and mixtures thereof, to provide MOFs with activated amino groups. Optionally, the acid wash can be a mixture of one or more inorganic acids and one or more organic acids. Preferred inorganic acids include hydrochloric acid, nitric acid, and sulfuric acid. Preferred organic acids include formic acid. Prior to use in a particular application, the wet and acid-treated MOFs are dried at a temperature of about 40° C. to about 250° C., or at a temperature of about 75° C. to about 150° C. The time for drying the wet MOF can vary substantially, but is typically from about 2 hours to about 336 hours, or from about 8 hours to about 168 hours, or from about 8 hours to about 48 hours, or from about 48 hours to about 168 hours.
[0048] When MOFs are used as adsorbents, MOFs treated with acid washing as disclosed herein adsorb more of the contaminants than as-synthesized MOFs. For example, the acid-treated MOFs can adsorb at least 10% more, at least 20% more, at least 30% more, at least 40% more, at least 50% more, at least 60% more, at least 70% more, at least 80% more, or at least 90% more than as-synthesized MOFs. The acid-treated MOFs can adsorb 2, 3, 5, 10, 15, 20, 30, 50, or 100 times more of the contaminants than as-synthesized MOFs.
[0049] As mentioned above, the MOFs of the present invention are characterized in that they are capable of (reversibly) adsorbing various molecules. They can therefore be used to purify gas streams by at least partially adsorbing at least one pollutant in the gas stream. Gas streams that need to be purified include, but are not limited to, air streams, industrial gas streams, off-gas streams, polluted gas streams, etc. Contaminants present in these streams that may be removed by the MOFs of the invention include, but are not limited to, cyanogen chloride, hydrogen cyanide, hydrogen sulfide, phosgene, sulfur dioxide, boron tribromide, boron trichloride, bromine, bromine chloride, bromine trifluoride, carbonyl fluoride, chlorine, chlorine pentafluoride, chlorine trifluoride, chlorosulfonic acid, dichlorosilane, ethylphosphonic dichloride, fluorine, hydrogen bromide, hydrogen chloride, hydrogen cyanide, hydrogen fluoride, hydrogen iodide, hydrogen sulfide, phosphorus trichloride, silicon tetrafluoride, sulfur dioxide, sulfur trioxide, sulfuric acid, sulfuryl chloride, titanium tetrachloride, tungsten hexafluoride, bromine pentafluoride, hydrogen selenide, nitric acid, nitrogen dioxide, nitrogen tetroxide, nitrogen trioxide, and mixtures thereof. The amount of contaminant that the MOF can remove is at least 50%, or at least 60%, or at least 70%, or at least 80%, or at least 90%, or at least 95%, or at least 99% of the contaminant. In one embodiment, the gas stream is an air stream, the contaminant is NO2, and the MOF removes at least 80% of the NO2 in the air stream. In another embodiment, a vessel having an inlet and an outlet port is filled with the MOF material through which the gas stream flows, thereby substantially removing the contaminant from the stream. To achieve the desired amount of removal, the gas stream is flowed through the MOF at a rate of about 10 L / min to about 500 L / min, or at a rate of about 30 L / min to about 200 L / min, or at a rate of about 50 L / min to about 120 L / min.
[0050] The MOF composition of the present invention can be used in the form of a powder, but may be advantageously formed into various shapes, such as pellets, spheres, disks, monoliths, irregular particles, extrudates, etc. Methods for forming these types of shapes are well known in the art. The MOF material can be formed into various shapes by itself or by including a binder. When selecting a binder, it is important to select a binder that does not adversely affect the surface area and adsorption capacity after the desired shape is formed. Materials that can be used as binders include, but are not limited to, cellulose, silica, carbon, alumina, and mixtures thereof.
[0051] The forming process typically involves preparing a thick paste-like material by mixing the MOF composition with a solvent or binder + solvent. Once the paste-like material is formed, it can be extruded through a die with holes of about 1-2 mm to form extrudates of various lengths, e.g., 6-10 mm. The paste, or even the powder itself, can be pressed under high pressure to form pellets or tablets. Other means of forming shapes include pressure molding, metal forming, pelletizing, granulation, extrusion, rolling, and marmalizing.
[0052] Another aspect of the invention involves depositing a catalytic metal on the shaped MOF bodies or MOF powder. The catalytic metal can be selected from zinc, copper, nickel, chromium, molybdenum, tungsten, niobium, rhenium, vanadium, silver, platinum, palladium, rhodium, iridium, and mixtures thereof. Deposition of the catalytic metal on the shaped MOF support is usually carried out by conventional means, including taking a solution containing a compound of the desired metal and impregnating it into the shaped MOF bodies, followed by drying and optional treatments such as calcination and / or reduction.
[0053] In yet another aspect of the present invention, the MOF material can be deposited on articles such as, but not limited to, monoliths, spherical supports, ceramic foams, glass fibers, woven fabrics, nonwoven fabrics, membranes, pellets, extrudates, irregular particles, and mixtures thereof. If the desired article is a monolith, spherical support, ceramic foam, pellets, extrudates, or irregular particles, a slurry of the MOF composition is prepared and deposited on the article by means such as dipping, spray drying, and then dried and optionally calcined. In the case of a membrane, it is possible to form the MOF composition directly on the membrane. The MOF composition of the present invention can be deposited or dispersed on fabrics (woven and nonwoven) or polymers by techniques such as electrospinning, direct crystal growth, and layer-by-layer deposition.
[0054] The MOF-containing articles described in the previous paragraph can be used as is to purify air or other gas streams containing pollutants. The air or other gas stream can be flowed through the article, e.g., monolith, foam, membrane, fabric, whereby the MOFs adsorb at least a portion of the pollutants in the percentage amounts detailed above. The MOF articles can also be placed in various types of rigid containers. For example, the extrudates or tablets or spheres can be contained in a bed through which the air or other gas stream is flowed. The bed can be placed in various types of housings, such as a filter canister having an inlet and an outlet. The fabrics (both woven and non-woven) can also be formed into filters, such as, but not limited to, pleated filters. This filter can also be contained in a rigid container, such as a cartridge through which the stream to be treated flows. The pleated filters can also be supported on frames of various shapes and sizes, through which the gas stream can flow. The frames can be made of various types of materials, such as, but not limited to, metal, wood, plastic, etc. Glass fibers can be formed into glass wool and contained in a rigid filter frame.
[0055] In the following examples, unless otherwise specified, all N2 gas adsorption and desorption measurements were performed using a Micromeritics Tristar II 3020 system (Micromeritics, Norcross, GA) at 77K. The surface area for N2 was calculated using the Brunauer - Emmet - Teller (BET) model in the range of 0.005 < P / Po < 0.05. The N2 adsorption amount was measured at P / Po = 0.9. Here, P / Po is the measured pressure relative to atmospheric pressure.
[0056] In the following examples, all nitrogen dioxide adsorption and desorption measurements were carried out at 25 °C on a Micromeritics 3Flex Surface Characterization Analyzer (Micromeritics, Norcross GA) by dosing to absolute pressure and using an equilibration interval of 3 seconds. Examples Example 1
[0057] A series of experiments were conducted to synthesize a series of Zr(NH2 - BDC) MOF. The parameters used in each experiment are shown in Table 1. The general procedure included first dissolving NH2 - BDC in DMF at room temperature. Once NH2 - BDC was dissolved, an acid regulator was added to the reaction mixture and heated to 90 °C. When the target temperature was reached, Zr0(NO3)2 was added by single dosing or dosing at a predetermined flow rate. After the addition was complete, the final reaction mixture was reacted for the desired time. The resulting MOF powder was isolated by filtration, washed with DMF and acetone, and dried at 100 °C for 12 hours. Table 1 Parameters for MOF synthesis
Table 1
[0058] The samples of the above examples were treated at 100 °C for 12 hours under vacuum, and their BET surface area, nitrogen adsorption amount, and pore volume were investigated. These results are shown in Table 2. Table 2 Characterization evaluation of the synthesized MOF [Table 2]
[0059] For comparison, a control sample of UiO-66-BDC-NH2MOF was purchased from Strem Chemicals, Inc, Newburyport, MA, catalog no. 40-1109, which is stated to have a particle size of 0.1-0.5 microns and a pore volume of 0.31-0.41 cc / g.
[0060] Figure 1A is a 2 micron scale photomicrograph of the control sample showing agglomerations of much smaller particles that appear to be nanoparticles. Figure 1B is a 10 micron scale photomicrograph of the product of Example 1-1 showing crystallite sizes of 1-5 μm. It can be seen that greater magnification is required to see the particle structure of the control sample, and even under greater magnification the particles of the control sample appear to be poorly formed and agglomerated.
[0061] The nanoparticle agglomerates of the control sample and Examples 1-7 are less suitable for use in filtering air pollutants than the MOFs of the present invention, which are synthesized using modifiers and provide single crystals in the 1-5 μm range or larger. Additionally, the surface areas of the control MOFs are less than 800-1075 m2. 2 / g range. The MOFs synthesized according to the present invention using modifiers and acid washing herein result in materials with improved surface area, improved crystal size, and improved amino functionality. Example 2 A large amount of MOFs were prepared using the procedure of Example 1-1. Samples of the resulting MOFs were treated with different acids to activate the amino groups on the MOFs by hydrolyzing the formamide substituents to expose the amino groups and release formic acid according to the reaction as shown in Figure 4. The procedure involves taking the MOFs, washing them with acid, and then drying them. For each of the samples B-0 herein, 200 g of Zr(NH2-BDC) MOFs were washed with 2 L of acid at various concentrations to determine the extent of hydrolysis of the amides and retention of porosity. 200 g of MOFs were stirred with 2 L of acid solution at different temperatures for 12 hours. After the acid wash, the MOFs were washed with acetone to remove any remaining acid, water, or hydrolyzed formic acid cleaved from the amides. After the acetone wash, the MOFs were dried at 100 °C for 12 hours and the BET surface area, N2 adsorption, and NO2 adsorption were measured (Table 3). Sample A is a sample of the material of Example 1-1 that was not washed with acid, and the control sample is a sample of a commercially available material that was not washed with acid. Table 3. Characterization of acid-washed MOFs [Table 3]
[0062] Table 3 shows the results of these experiments using different acids and different concentrations of acid wash. Sample A in Table 3 shows the characterization of the MOF of Example 1-1, which was not acid washed. The ratio of formic acid to MOF linker was found to be 2.55:1 (which includes formic acid groups directly attached to the metal framework and formic acid groups attached to organic ligands). Comparing this to Sample B, after acid washing, the ratio of formic acid to MOF linker was significantly reduced to 0.08:1, even though the MOF surface area was only slightly reduced. This reduction in the ratio of formic acid to NH2-BDC indicates that the acid washing step hydrolyzed the formamide groups and regenerated the amino groups.
[0063] Table 3 also shows how different acids and acid concentrations affect the hydrolysis of amide groups and the surface area of the MOFs. For all three acids (HC1, HNO3, and H2SO4), decreasing the molar concentration from 1M to 0.05M reduces the amount of hydrolysis that takes place. At a concentration of 0.05M, the ratio of formic acid to NH2-BDC decreased from 2.55:1 to 1.10:1. Decreasing the concentration of the acid has less effect on the surface area of the MOFs. For all three acids, increasing the temperature from room temperature (rt) to 60°C increases the amount of amide hydrolyzed, but the surface area decreases more relative to the room temperature treatment. In the case of nitric acid, higher acid concentrations (1M to 0.25M) result in a larger decrease in surface area. Similarly, treating a 1M solution of sulfuric acid while hydrolyzing the amide groups results in a larger decrease in surface area.
[0064] The degree of hydrolysis of the amide is 1 The measurements were performed using a H-NMR spectrophotometer as follows. Each MOF sample, washed and dried to activate the amino groups as described above, was treated with a NaOD / EEO solution to decompose the MOFs and completely cleave the formamide groups, leaving a mixture of activated NH2-BDC (the linker cleaved from the MOF structure) and cleaved formic acid, according to the reaction scheme shown in Figure 3. 1 H-NMR spectrum was measured and used to calculate the amount of formamide groups remaining after acid washing. 1 H-NMR spectra are used comparing Hc on the NH2-BDC linker (δd, 7.55 ppm) with Hd on the cleaved formic acid (δs, 8.3 ppm). A higher percentage of cleaved formic acid indicates that the MOF had a higher percentage of formamide groups before degradation, whereas a lower percentage of cleaved formic acid indicates that the MOF had a lower percentage of formamide groups before degradation, i.e., the acid wash step had hydrolyzed the formamide groups to activate the amino groups.
[0065] FIG. 2A shows the results of the four degraded samples, with spectrum A corresponding to sample B, spectrum B the control sample, spectrum C the non-acid washed Examples 1-7 (Table 1), and spectrum D the sample A from Table 3. 1 The H-NMR spectrum of the MOF is shown in Fig. 2A. The illustration in Fig. 2A shows the MOF structure before acid washing and which protons on the MOF structure are 1 The H-NMR peaks shown in the figure correspond to the H-NMR peaks. The peak at 8.3 ppm represents the sum of the signals from Hd protons on the carbon atoms of the formamide groups attached to the MOF ligands and the MOF corner metal units, as shown in the inset of Figure 2A. This peak is found to be highest in spectrum D, which corresponds to sample A, which uses formic acid as a modifier in the MOF synthesis and does not have an acid wash. Significant formamide peaks are also seen in the commercial control sample (spectrum B) and the sample with HC1 (spectrum C). In spectrum A, which corresponds to sample B, where the MOF was washed with 1.0 M HC1, the formamide peak is negligible.
[0066] These results are consistent with the solids of these same samples shown in Figure 2B, where the peaks indicate the presence of amide and amine groups. 15 The N-NMR is consistent with that of the free ligand. For reference, spectrum E shows the chemical shift of the free amine peak. 15 NH2-BDC. Spectrum F is the product of Sample B, Spectrum G is the product of Examples 1-7 (Table 1), and Spectrum H is Sample A. These spectra demonstrate the presence of formylamide in all Zr(NH2-BDC) formulations that were not acid washed. Sample A, which was not acid washed (Spectrum H), showed substantial amide peaks and almost no amine peaks, while Sample B, which was acid washed (Spectrum F), showed substantial no amide peaks and a strong amine peak.
[0067] Corresponding to the removal of formamide groups, the increase in free amino groups increases the amount of NO2 adsorbed as measured by NO2 one-component isotherms (Table 3). Specifically, the NO2 adsorption capacity measured at 50 Torr and 25 °C for the untreated MOF (sample A in Table 3) was only 0.58 mmol / g, whereas washing with HC1 increased the NO2 capacity to 8.3 mmol / g at 50 Torr and 25 °C (sample B; Table 3). Similar results were obtained with nitric acid (sample H) and sulfuric acid (sample N).
[0068] Additionally, the control MOF exhibits as little as 45% of amide groups reducing the available amino groups for reactivity (Figure 2A (spectrum B) and Table 3). In contrast, the acid-treated MOF exhibits a reduction in the incorporation of undesirable amide groups (including formamide groups attached to the ligands and those attached to the corner metal units) from 255% incorporation to 3-8% incorporation (Figure 2A (spectrum A) and Table 3), thus freeing a majority of the amino groups for reactivity with polluted air. These improved properties of increased crystal size, increased reactive free amines, and high surface area result in a MOF with more desirable properties than commercially available materials, particularly for air filtration.
Claims
[Claim 1] a. forming a reaction mixture of a metal compound, wherein the metal is selected from Zr, V, Al, Fe, Cr, Ti, Hf, Cu, Zn, Ni, Ce, and mixtures thereof; one or more ligands selected from at least one amino-containing organic ligand or a combination of at least one amino-containing organic ligand and at least one non-amino-containing organic ligand; a solvent selected from dimethylformamide, water, ethanol, and isopropanol, and mixtures thereof; and a modifier comprising at least one monocarboxylic acid; b. reacting the reaction mixture at a temperature and for a time to form MOFs; c. isolating the MOF to provide a powder of the MOF; d. washing the powder of MOFs with an acid wash comprising at least one inorganic acid to provide MOFs having activated amino groups and an average crystal size of greater than 1 μm; 1. A method for preparing a metal-organic framework (MOF) composition comprising:
Citation Information
Patent Citations
Preparation method for synthesizing metal organic framework UiO-66 adsorbents by aid of mixed ligands
CN109395698A
Mothod for preparation of metal-organic-framework and metal-organic-framework prepared by the same
KR1020190074374A
Removal of nitrogen dioxide from gas environments using metal-organic frameworks
US9868107B1
Aldehyde removal material
WO2015046417A1
Metal-organic frameworks for the removal of multiple liquid phase compounds and methods for using and making same
WO2020046768A1