Carbon material for positive electrodes of non-aqueous secondary batteries and method for producing same
A carbon material with optimized specific surface area and crystallite diameter for non-aqueous secondary battery electrodes addresses the challenge of maintaining energy capacity and preventing gas generation at low temperatures, enhancing battery performance and safety.
Patent Information
- Application Number
- JP2020102612
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-06-12
AI Technical Summary
Existing non-aqueous secondary batteries face challenges in maintaining energy capacity at low temperatures due to side reactions between the carbon material and electrolyte, leading to gas generation and potential battery casing damage, while conventional solutions to enhance energy capacity, such as using activated carbon with high surface area, also increase costs.
A carbon material for non-aqueous secondary battery positive electrodes with a BET specific surface area of 1100 m²/g to 1400 m²/g and a crystallite diameter of 3.50 nm to 5.15 nm, produced through activation and heat-treatment processes, is used to suppress gas generation and maintain energy capacity.
The carbon material effectively suppresses gas generation and maintains energy capacity in low temperature ranges by balancing specific surface area and crystallite diameter, preventing side reactions while ensuring sufficient lithium ion adsorption.
Smart Images

Figure 0007579647000002 
Figure 0007579647000003 
Figure 0007579647000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a carbon material for a positive electrode of a non-aqueous secondary battery and a method for producing the same. [Background technology]
[0002] In recent years, there has been an increasing demand for non-aqueous secondary batteries as power sources for vehicles, personal computers, and the like.
[0003] Among non-aqueous secondary batteries, lithium ion batteries have a high energy capacity, and one of the issues to be addressed is how to suppress the decrease in energy capacity at low temperatures.
[0004] As one means for suppressing a decrease in energy capacity in the low temperature range, for example, Patent Document 1 discloses the addition of a carbon material with a large specific surface area, such as activated carbon, to the positive electrode active material layer in addition to a carbon material with high conductivity, such as carbon black.
[0005] As another means for suppressing the decrease in energy capacity in the low temperature range, Non-Patent Document 1 discloses the use of an electrolyte solution having a high concentration of lithium salt.
[0006] Incidentally, as disclosed in Non-Patent Document 2, in a non-aqueous secondary battery using a carbon material in the positive electrode active material layer, the carbon material may react with the electrolyte at high voltage to generate gas, and therefore, it is also required to suppress the generation of gas during use of the non-aqueous secondary battery.
[0007] Other examples using carbon materials include the techniques disclosed in Patent Documents 2-4.
[0008] Patent Document 2 discloses the use of carbon black in a positive electrode active material layer having an OAN in the range of 100 to 250 mL / 100 g and a crystallite size (La) of at least 30 Å as measured by Raman spectroscopy.
[0009] In addition, Patent Document 3 discloses a positive electrode active material layer having a thickness of 130 to 700 m. 2 It is disclosed to use carbon black having a BET surface area in the range of 0.5 to 1 / g and a STSA / BET ratio in the range of 0.5 to 1.
[0010] In addition, Patent Document 4 discloses a positive electrode active material layer having a specific surface area of 700 to 1500 m 2 / g and the first carbon material with a specific surface area of 600 m 2 / g or less, and a second carbon material such that the content of the first carbon material is 5 mass % to 10 mass % with respect to the mass of the total carbon materials. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2007-317582 A [Patent Document 2] Special Publication No. 2016-526257 [Patent Document 3] Special Publication No. 2016-527668 [Patent Document 4] JP 2005-293931 A [Non-patent literature]
[0012] [Non-Patent Document 1] J. Wang et. al, “Superconcentrated electrolytes for a high-voltage lithium-ion battery”, Nature Communications, June 29, 2016,7,Article number 12032 (2016) [Non-Patent Document 2] Kajiyama, “Study on the interaction between active materials and conductive materials for the purpose of suppressing gas generation in high voltage positive electrodes”, Powder and Powder Metallurgy, Japan Powder and Powder Metallurgy Association, November 2015, Vol. 62, No. 11, pp. 538-542 Summary of the Invention [Problem to be solved by the invention]
[0013] One possible means for suppressing the decrease in energy capacity of a nonaqueous secondary battery in the low temperature range is to use activated carbon with a large specific surface area in the positive electrode active material layer, as disclosed in Patent Document 1.
[0014] However, activated carbon has a small crystal size and many hexagonal plane ends in its crystal structure. These hexagonal plane ends have higher activity than other parts of the crystal structure, such as flat parts, and are more likely to react with the electrolyte to generate gas.
[0015] In addition, as described in Non-Patent Document 1, by increasing the amount of lithium ions in the electrolyte, the energy capacity can be maintained even when the viscosity of the electrolyte increases in the low temperature range. However, the use of such an electrolyte leads to high costs for non-aqueous secondary batteries.
[0016] The present disclosure aims to provide a carbon material for a positive electrode of a nonaqueous secondary battery, which can suppress a decrease in energy capacity in a low temperature range while suppressing the generation of gas due to a side reaction between the carbon material and an electrolyte, and a method for producing the same. [Means for solving the problem]
[0017] The present inventors have found that the above object can be achieved by the following means: Aspect 1 A carbon material for a positive electrode of a non-aqueous secondary battery, comprising: BET specific surface area is 1100m 2 / g~1400m 2 / g, and The crystallite size according to X-ray diffraction analysis using CuKα radiation is 3.50 nm to 5.15 nm. Carbon materials. Aspect 2 BET specific surface area is 1150m 2 / g~1300m 2 / g. Aspect 3 3. The carbon material according to aspect 1 or 2, wherein the crystallite size determined by X-ray diffraction analysis using CuKα radiation is 3.85 nm to 5.15 nm. Aspect 4 A non-aqueous secondary battery having a positive electrode active material layer, a negative electrode active material layer, a separator, and an electrolyte solution, The positive electrode active material layer contains the carbon material according to any one of aspects 1 to 3, and The electrolyte solution contains an organic solvent and a lithium salt. Non-aqueous secondary battery. Aspect 5 5. The nonaqueous secondary battery according to embodiment 4, wherein the organic solvent is an aprotic solvent such as carbonates, esters, ethers, nitriles, sulfones, or lactones. Aspect 6 6. The nonaqueous secondary battery according to claim 4 or 5, wherein the lithium salt is one or more lithium salts selected from LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, and the like. Aspect 7 A method for producing a carbon material for a positive electrode of a non-aqueous secondary battery, comprising the steps of: performing an activation treatment on a precursor carbon material of the carbon material to increase the specific surface area of the precursor carbon material; and performing a heat treatment on the precursor carbon material after the activation treatment to increase the crystallite size of the precursor carbon material; Contains The carbon material for the positive electrode of non-aqueous secondary batteries produced by this process has a BET specific surface area of 1100 m 2 / g~1400m 2 / g, and the crystallite size measured by X-ray diffraction analysis using CuKα radiation is 3.50 nm to 5.15 nm. Manufacturing method. Aspect 8 8. The method according to claim 7, wherein the activation treatment comprises contacting the precursor carbon material with 150 parts by mass to 350 parts by mass of an activator per 100 parts by mass of the precursor carbon material at 650° C. to 750° C. Aspect 9: The manufacturing method according to aspect 7 or 8, wherein the heat treatment is carried out at a temperature of 1500°C to 1690°C. Effect of the Invention
[0018] According to the present disclosure, it is possible to provide a carbon material and a manufacturing method thereof that can suppress the decrease in energy capacity in a low temperature range while suppressing the generation of gas due to a side reaction between the carbon material and an electrolyte solution. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a graph showing the relationship between the specific surface area and the crystallite size of each example of carbon material for a positive electrode of a nonaqueous secondary battery. [Diagram 2] FIG. 2 is a graph showing the relationship between the results of measuring the current by cyclic voltammetry and the results of measuring the energy capacity in the low temperature range for each example of the carbon material for a positive electrode of a nonaqueous secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0021] Carbon materials for positive electrodes of non-aqueous secondary batteries The carbon material for the positive electrode of a nonaqueous secondary battery disclosed herein has a BET specific surface area of 1100 m 2 / g~1400m 2 / g, and the crystallite size as determined by X-ray diffraction analysis using CuKα rays is 3.50 nm to 5.15 nm.
[0022] Without being limited by the theory, the principle by which the use of the carbon material of the present disclosure as a material for the positive electrode active material layer of a nonaqueous secondary battery can suppress the decrease in energy capacity in the low temperature range of the nonaqueous secondary battery while suppressing the generation of gas due to a side reaction between the carbon material and the electrolyte is as follows.
[0023] In non-aqueous secondary batteries, the internal resistance increases and the energy capacity decreases at low temperatures. One possible method for suppressing the decrease in the energy capacity of non-aqueous secondary batteries at low temperatures is to use a carbon material with a large specific surface area in the positive electrode.
[0024] Carbon materials are known to have capacitance by electrically adsorbing and desorbing lithium ions in lithium ion capacitors and the like, and this is also considered to be the case in the positive electrode active material layer of non-aqueous secondary batteries. Therefore, by using a carbon material with a large specific surface area for the positive electrode active material layer, it is possible to suppress the decrease in energy capacity even if the internal resistance increases in the low temperature range. Similarly, by using a carbon material with a large specific surface area for the positive electrode active material layer, it is possible to suppress the voltage change during discharge even in the normal temperature range.
[0025] From this viewpoint, conventionally, a carbon material having a large specific surface area, such as activated carbon, has been used in the positive electrode active material layer.
[0026] However, activated carbon has many pores on its surface to increase its surface area, which results in a small crystallite size. This small crystallite size results in many edges of the highly active carbon hexagonal mesh planes.
[0027] The large specific surface area and small crystallite size of activated carbon make it easy for the activated carbon to react with the electrolyte, and therefore, in non-aqueous secondary batteries that use activated carbon as the carbon material for the positive electrode active material layer, gases such as carbon dioxide gas derived from the organic solvent in the electrolyte are likely to be generated.
[0028] If gas is generated inside the nonaqueous secondary battery, the exterior body of the nonaqueous secondary battery may swell, and even the exterior body may be damaged.
[0029] As described above, with conventional carbon materials, it has not been possible to simultaneously suppress the decrease in energy capacity in the low temperature range and to suppress the generation of gas due to a side reaction between the carbon material and the electrolyte.
[0030] In this regard, the carbon material of the present disclosure for use in a positive electrode of a non-aqueous secondary battery has a BET specific surface area of 1100 m 2 / g~1400m 2 / g, the specific surface area is large, and the decrease in energy capacity at low temperatures can be suppressed. In addition, the carbon material of the present disclosure has a crystallite size of 3.50 nm to 5.15 nm as determined by X-ray diffraction analysis using CuKα radiation, and therefore has a large crystallite size and therefore fewer highly active carbon hexahedral net plane edges, making it possible to suppress the generation of gas due to a side reaction between the carbon material and the electrolyte.
[0031] As a result, the carbon material of the present disclosure can suppress the decrease in energy capacity in the low temperature range of a nonaqueous secondary battery, while suppressing the generation of gas due to a side reaction between the carbon material and the electrolyte.
[0032] <BET specific surface area> The carbon material for the positive electrode of a nonaqueous secondary battery disclosed herein has a BET specific surface area of 1100 m 2 / g~1400m 2 / g.
[0033] BET specific surface area is 1100m 2 / g or more, the amount of lithium ions in the electrolyte can be increased in the positive electrode active material layer of the nonaqueous secondary battery, and the decrease in the energy capacity of the nonaqueous secondary battery in the low temperature range can be further suppressed. 2 When the carbon material has a molecular weight of 1000 or less, the side reaction between the carbon material and the electrolyte does not become too large.
[0034] The BET specific surface area of the carbon material disclosed herein is 1100 m2 / g or more, or 1150m 2 / g or more, 2 / g or less, 1350m 2 / g or less, or 1300m 2 / g or less.
[0035] The carbon material for the positive electrode of a non-aqueous secondary battery of the present disclosure has a BET specific surface area of 1150 m 2 / g~1300m 2 When the BET specific surface area is within this range, in combination with the crystallite size defined below, it is possible to achieve a good balance between suppressing the decrease in the energy capacity of a nonaqueous secondary battery in a low temperature range and suppressing the generation of gas due to a side reaction between the carbon material and the electrolyte.
[0036] The BET specific surface area can be determined by the nitrogen pore distribution method using, for example, a surface area and pore distribution analyzer Quadrabsorb SI manufactured by Quantachrome Instruments Japan LLC. Specifically, in nitrogen gas at 77.4K, the nitrogen gas adsorption amount (cc / g) of the carbon material at each pressure P is measured while increasing the nitrogen gas pressure P (mmHg). Next, the pressure P is divided by the saturated vapor pressure Po of nitrogen gas to obtain the relative pressure P / Po, and the nitrogen gas adsorption amount is plotted against each relative pressure P / Po to obtain an adsorption isotherm. Then, a BET plot is performed to calculate the specific surface area.
[0037] <Crystallite size> The carbon material for a positive electrode of a nonaqueous secondary battery according to the present disclosure has a crystallite diameter of 3.50 nm to 5.15 nm as determined by X-ray diffraction analysis using CuKα radiation.
[0038] When the crystallite size is 3.50 nm or more, even if the specific surface area of the carbon material is large, the end of the highly active carbon hexagonal net plane is small, so that the reaction between the carbon material and the electrolyte is unlikely to occur, and gas generation can be suppressed. On the other hand, when the crystallite size is more than 5.15 nm, gas generation can be suppressed, but the specific surface area of the carbon material cannot be sufficiently large.
[0039] In other words, when the crystallite size is in the above range, the generation of gas due to the side reaction between the carbon material and the electrolyte can be sufficiently suppressed, and the specific surface area of the carbon material can be sufficiently increased. Therefore, when the crystallite size is in the above range, in combination with the specific surface area in the above range, the suppression of the decrease in the energy capacity of the non-aqueous secondary battery in the low temperature range and the suppression of the generation of gas due to the side reaction between the carbon material and the electrolyte can be realized in a well-balanced manner.
[0040] The crystallite size of the carbon carbon material of the present disclosure may be 3.60 nm or more, 3.70 nm or more, 3.80 nm or more, 3.85 nm or more, or 3.90 nm or more, and may be 5.15 nm or less, 5.10 nm or less, 5.05 nm or less, or 5.0 nm or less.
[0041] The carbon-carbon material of the present disclosure may particularly have a crystallite size of 3.85 nm to 5.15 nm.
[0042] The crystallite diameter of the carbon material of the present disclosure, i.e., the dimension of the a-axis of the crystallite, is specifically determined from a diffraction peak profile obtained by X-ray diffraction analysis using CuKα radiation, as follows: ( 10 ) side The half-width of the diffraction line is measured, and the value can be calculated according to the Scherrer formula.
[0043] 《Non-aqueous secondary battery》 The non-aqueous secondary battery of the present disclosure is a non-aqueous secondary battery having a positive electrode active material layer, a negative electrode active material layer, a separator, and an electrolyte, the positive electrode active material layer contains the carbon material for the non-aqueous secondary battery positive electrode of the present disclosure, and the electrolyte contains an organic solvent and a lithium salt. The separator is disposed between the positive electrode active material layer and the negative electrode active material layer. The non-aqueous secondary battery of the present disclosure may further have a positive electrode current collector electrically connected to the positive electrode active material layer, and a negative electrode current collector electrically connected to the negative electrode active material layer. Furthermore, the non-aqueous secondary battery of the present disclosure may have an exterior body that seals the positive electrode active material layer, the negative electrode active material layer, the separator, and the electrolyte.
[0044] In the nonaqueous secondary battery of the present disclosure, the carbon material of the present disclosure is used as a material for the positive electrode active material layer, and thus the decrease in energy capacity at low temperatures is suppressed and gas generation due to a side reaction between the carbon material and the electrolyte is suppressed.
[0045] <Cathode active material layer> The positive electrode active material layer of the present disclosure contains a positive electrode active material and the carbon material of the present disclosure.
[0046] The positive electrode active material layer can be prepared, for example, by applying a paste or slurry-like composition (positive electrode mixture) in which a positive electrode active material, a carbon material of the present disclosure, and optionally a binder or the like are dispersed in a suitable solvent to a positive electrode current collector, and then drying the composition.
[0047] The positive electrode active material may be any positive electrode active material that can be used in a non-aqueous secondary battery. Known active materials can be used as the positive electrode active material. Examples of the positive electrode active material include TiS2, TiS3, MoS3, FeS2, and Li (1-x) MnO2, Li (1-x) Mn2O4, Li (1-x) CoO2, Li (1-x) Examples of the positive electrode active material include compounds such as NiO2 and V2O5. Here, x is 0 to 1. A mixture of these compounds may be used as the positive electrode active material. 1-x Mn 2+x O4, LiNi1-x Co x The positive electrode active material may be LiMn2O4 or LiNiO2 in which a part of the transition metal element is replaced with at least one other transition metal element or Li, such as O2.
[0048] As the positive electrode active material, composite oxides of lithium and transition metals such as LiMn2O4, LiCoO2, LiNiO2, etc. are more preferable. These positive electrode active materials have excellent performance as active materials such as excellent diffusion performance of electrons and lithium ions, so that a battery having high charge / discharge efficiency and good cycle characteristics can be obtained. Furthermore, as the positive electrode active material, it is preferable to use LiMn2O4 because of its low material cost.
[0049] The binder can be appropriately selected from, for example, a water-soluble polymer that dissolves in water, a polymer that disperses in water, a polymer that dissolves in a non-aqueous solvent (organic solvent), etc. Also, only one type may be used alone, or two or more types may be used in combination.
[0050] Examples of the water-soluble polymer include carboxymethyl cellulose (CMC), methyl cellulose (MC), cellulose acetate phthalate (CAP), hydroxypropyl methylcellulose (HPMC), hydroxypropyl methylcellulose phthalate (HPMCP), polyvinyl alcohol (PVA), and the like.
[0051] Examples of the water-dispersible polymer include fluorine-based resins such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and ethylene-tetrafluoroethylene copolymer (ETFE); vinyl acetate copolymer, styrene-butadiene block copolymer (SBR), acrylic acid-modified SBR resin (SBR latex); and rubbers such as gum arabic.
[0052] Examples of polymers that dissolve in non-aqueous solvents (organic solvents) include polyvinylidene fluoride (PVDF), polyvinylidene chloride (PVDC), polyethylene oxide (PEO), polypropylene oxide (PPO), and polyethylene oxide-propylene oxide copolymer (PEO-PPO).
[0053] The amount of binder added may be appropriately selected depending on the type and amount of the positive electrode active material.
[0054] <Negative electrode active material layer> The negative electrode active material layer contains a negative electrode active material.
[0055] The negative electrode active material layer can be prepared, for example, by applying a paste or slurry-like composition (negative electrode mixture) in which a negative electrode active material and, optionally, a binder or the like are dispersed in a suitable solvent to a negative electrode current collector, and then drying the composition.
[0056] As the negative electrode active material, one or more of materials conventionally used in lithium ion secondary batteries can be used without any particular limitation. For example, carbon particles can be mentioned as a suitable negative electrode active material. Particulate carbon materials (carbon particles) containing at least a graphite structure (layer structure) in a part thereof are preferably used. Any carbon material having a structure such as so-called graphitic material (graphite), non-graphitizable carbonaceous material (hard carbon), easily graphitizable carbonaceous material (soft carbon), or a combination of these can be preferably used. In particular, graphite particles such as natural graphite can be preferably used. Graphite particles have excellent conductivity because they can suitably occlude lithium ions as charge carriers. In addition, because the particle size is small and the surface area per unit volume is large, they can be a negative electrode active material suitable for more rapid charging and discharging (for example, high-output discharging).
[0057] The amount of the negative electrode active material contained in the negative electrode active material layer is not particularly limited, and can be preferably about 90% by mass to 99% by mass, and more preferably about 95% by mass to 99% by mass.
[0058] The binder may be the same as that used in the positive electrode active material layer, and may be used alone or in combination of two or more. The amount of binder added may be appropriately selected depending on the type and amount of the negative electrode active material.
[0059] <Separator> As the separator, various separators used in general lithium ion secondary batteries can be used without any particular restrictions. For example, a porous film made of a polyolefin resin such as polyethylene or polypropylene can be suitably used. The film may be a single layer or a multilayer. Such a resin film may be provided with an inorganic filler layer containing one or more types of ceramic particles such as titania (titanium oxide; TiO2), alumina, silica, magnesia, zirconia, zinc oxide, iron oxide, ceria, yttria, etc. The thickness of the separator may be appropriately selected.
[0060] The non-aqueous electrolyte to be impregnated into the separator can be prepared by dissolving an appropriate electrolyte in a non-aqueous solvent. As the electrolyte, any electrolyte used in a general lithium ion secondary battery can be used without any particular limitation. For example, one or more lithium salts selected from LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, etc. can be used. The concentration of the electrolyte in the electrolyte is not particularly limited, and can be, for example, the same as the concentration of the electrolyte used in a conventional lithium ion secondary battery. In addition to the electrolyte, various additives and the like may be added to the electrolyte.
[0061] <Electrolyte> The electrolyte contains an organic solvent and a lithium salt.
[0062] The organic solvent may be an aprotic solvent such as, for example, carbonates, esters, ethers, nitriles, sulfones, lactones, and the like.
[0063] More specifically, the organic solvent may be, for example, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), 1,2-dimethoxyethane (DME), 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, 1,3-dioxolane, diethylene glycol dimethyl ether, ethylene glycol dimethyl ether, acetonitrile, propionitrile, nitromethane, N,N-dimethylformamide, dimethyl sulfoxide, sulfolane, γ-butyrolactone (BL), or other organic solvents generally used in lithium ion secondary batteries, and may be used alone or in combination of two or more kinds.
[0064] The lithium salt contained in the electrolyte of the nonaqueous secondary battery of the present disclosure may be one or more lithium salts selected from, for example, LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, etc.
[0065] <Current collector> The material used for the positive electrode current collector and the negative electrode current collector is not particularly limited, and any material that can be used in a non-aqueous secondary battery can be appropriately adopted. For example, the material used for the current collector may be, but is not limited to, stainless steel, aluminum, copper, nickel, iron, titanium, carbon, etc. Among them, the material of the positive electrode current collector is preferably aluminum, and the material of the negative electrode current collector is preferably copper.
[0066] The shape of the current collector is not particularly limited, and examples thereof include a foil, a plate, and a mesh.
[0067] <Method for producing carbon material> The manufacturing method disclosed herein is a method for manufacturing a carbon material for a positive electrode of a nonaqueous secondary battery, and includes performing an activation treatment on a precursor carbon material to increase the specific surface area of the precursor carbon material, and performing a heat treatment on the precursor carbon material after the activation treatment to increase the crystallite size of the precursor carbon material, thereby enabling the manufactured carbon material for a positive electrode of a nonaqueous secondary battery to have a BET specific surface area of 1100 m 2 / g~1400m 2 / g, and the crystallite size as determined by X-ray diffraction analysis using CuKα rays is 3.50 nm to 5.15 nm.
[0068] Without being limited by the theory, the manufacturing method according to the present disclosure can manufacture a carbon material for a positive electrode of a nonaqueous secondary battery that can suppress the decrease in energy capacity in a low temperature range while suppressing the generation of gas due to a side reaction between the carbon material and the electrolyte solution, and the carbon material can be manufactured based on the following principle.
[0069] As described above in the section Carbon materials for positive electrodes of non-aqueous secondary batteries, the BET specific surface area is 1100 m 2 / g~1400m 2 / g and a crystallite size of 3.50 nm to 5.15 nm as determined by X-ray diffraction analysis using CuKα radiation can suppress the generation of gas due to a side reaction between the carbon material and the electrolyte in a nonaqueous secondary battery while suppressing a decrease in energy capacity.
[0070] In the manufacturing method of the present disclosure, a precursor carbon material is subjected to an activation treatment to roughen the surface of the precursor carbon material to increase the specific surface area, and then the precursor carbon material is subjected to a heat treatment to increase the crystallites, thereby making it possible to manufacture a carbon material for a non-aqueous secondary battery positive electrode having the above-mentioned BET specific surface area and crystallite size.
[0071] <Carbon precursor material> The precursor carbon material used in the manufacturing method of the present disclosure may be any carbon material used as a carbon material for a positive electrode of a non-aqueous secondary battery. Examples of the precursor carbon material include, but are not limited to, resin, coconut shell, coal, coke, and pitch.
[0072] Activation Treatment The manufacturing method of the present disclosure includes performing an activation treatment on a precursor carbon material to increase the specific surface area of the precursor carbon material.
[0073] The activation treatment may be any activation treatment capable of increasing the surface area of the precursor carbon material, including, but not limited to, contacting the precursor carbon material with an activator and heating.
[0074] The activation treatment may include contacting the precursor carbon material with 150 parts by mass to 350 parts by mass of an activator per 100 parts by mass of the precursor carbon material at, for example, 650°C to 750°C.
[0075] The temperature at which the activation treatment is carried out in the heating furnace may be 600° C. or more, 675° C. or more, or 700° C. or more, and may be 750° C. or less, or 725° C. or less.
[0076] When the activation treatment is carried out using microwaves, for example, in the case of 35 g of the precursor carbon material, the power may be 1400 W or more, 1450 W or more, or 1500 W, and may be 1600 W or less, or 1550 W or less.
[0077] The amount of the activator may be 150 parts by mass or more, or 250 parts by mass or more, and may be 350 parts by mass or less, or 320 parts by mass or less, relative to 100 parts by mass of the precursor carbon material.
[0078] The activation treatment time may be 1.33 hours to 4 hours. The activation treatment time may be 1 hour or more, and may be 10 hours or less, 8 hours or less, 6 hours or less, or 4 hours or less.
[0079] The method for contacting the precursor carbon material with the activator is not particularly limited, and may be, for example, a method of kneading a powdered precursor carbon material with a powdered activator.
[0080] The activator may be any strong alkaline compound. The activator may be, for example, a hydroxide of an alkali metal or an alkaline earth metal. More specifically, the activator may be, for example, sodium hydroxide, potassium hydroxide, calcium hydroxide, or a combination of at least two of these. Activation may also be performed using a gas such as water vapor or carbon dioxide.
[0081] <Heat Treatment> The manufacturing method of the present disclosure includes subjecting the precursor carbon material after the activation treatment to a heat treatment, thereby increasing the crystallinity of the precursor carbon material.
[0082] The heat treatment is carried out at a temperature and for a time that can increase the crystallite diameter of the precursor carbon material to 3.50 nm to 5.15 nm. The increase in the crystallite diameter of the carbon material tends to be greater as the temperature and time of the heat treatment are longer. Therefore, the temperature and time of the heat treatment can be appropriately set according to the material of the precursor carbon material used and the desired crystallite diameter after the heat treatment.
[0083] The heat treatment is preferably carried out at a temperature of 1500°C to 1690°C.
[0084] The crystallite size of the carbon material is particularly likely to increase when the heat treatment temperature is from about 1500° C. to 1650° C. Therefore, by setting the heat treatment temperature to 1500° C. to 1650° C., the crystallite size can be increased efficiently.
[0085] The temperature of the heat treatment may be 1500°C or more, 1525°C or more, 1550°C or more, 1575°C or more, or 1600°C or more, and may be 1650°C or less.
[0086] The heat treatment time may be 0.03 to 0.7 hours.
[0087] The heat treatment time may be shorter as the heat treatment temperature is higher, and may be longer as the heat treatment temperature is lower. The heat treatment time may be 0.03 hours or more, and may be 0.7 hours or less, 0.6 hours or less, or 0.5 hours or less. EXAMPLES
[0088] Examples 1 to 3, Reference Examples 1 to 7, and Comparative Example 1 Example 1 (Preparation of carbon materials for non-aqueous secondary battery positive electrodes) A commercially available coal-based raw material was used as the precursor carbon material.
[0089] Next, this precursor carbon material was subjected to activation treatment. Specifically, 100 parts by mass of the precursor carbon material was mixed with 256 parts by mass of powdered potassium hydroxide and 64 parts by mass of sodium hydroxide, and then heated under a nitrogen atmosphere. Heating was performed in a microwave heating furnace manufactured by Hirotec Corporation at 1500 W for 1.33 hours.
[0090] This activation treatment converted the precursor carbon material into activated carbon.
[0091] The obtained activated carbon was filtered and washed with pure water until the pH reached about 11 to 12, and then further washed with 0.1N nitric acid to remove residual alkaline components adhering to the activated carbon. Next, the activated carbon was repeatedly filtered and washed with pure water until the pH reached 6 to 7 based on JIS K 1474. Next, the activated carbon was filtered and subjected to a drying treatment. Specifically, the activated carbon was dried at 115° C. for 12 hours or more.
[0092] Next, the dried activated carbon was pulverized using a ball mill until the average particle size became about 3 μm.
[0093] The pulverized activated carbon was then heat-treated in an argon atmosphere using a high-temperature furnace manufactured by Fuji Electric Industries Co., Ltd. The heating rate was set at 10°C / min, and after the temperature reached 1600°C, this temperature was maintained for 0.5 hours.
[0094] In this way, a carbon material for a positive electrode of a nonaqueous secondary battery of Example 1 was obtained.
[0095] Example 2 (Preparation of carbon materials for non-aqueous secondary battery positive electrodes) As the precursor carbon material, a commercially available coal-based raw material was used.
[0096] Next, this precursor carbon material was subjected to activation treatment. Specifically, 100 parts by mass of the precursor carbon material was mixed with 320 parts by mass of powdered potassium hydroxide, and heated in a nitrogen atmosphere. Heating was performed in a Mino Ceramics furnace at a temperature rise rate of 2°C / min, and the temperature was maintained for 4 hours after reaching 700°C.
[0097] This activation treatment converted the precursor carbon material into activated carbon.
[0098] The obtained activated carbon was filtered and washed with pure water until the pH reached about 11 to 12, and then further washed with 0.1N nitric acid to remove residual alkaline components adhering to the activated carbon. Next, the activated carbon was repeatedly filtered and washed with pure water until the pH reached 6 to 7 based on JIS K 1474. Next, the activated carbon was filtered and subjected to a drying treatment. Specifically, the activated carbon was dried at 115° C. for 12 hours or more.
[0099] Next, the dried activated carbon was pulverized using a ball mill until the average particle size became about 3 μm.
[0100] The pulverized activated carbon was then heat-treated in an argon atmosphere using a high-temperature furnace manufactured by Fuji Electric Industries Co., Ltd. The heating rate was set at 10°C / min, and after the temperature reached 1650°C, this temperature was maintained for 0.5 hours.
[0101] In this way, a carbon material for a nonaqueous secondary battery positive electrode of Example 2 was obtained.
[0102] Example 3 (Preparation of carbon materials for non-aqueous secondary battery positive electrodes) In Example 3, commercially available alkali-activated carbon (activated carbon) was pulverized in the same manner as in Example 1. Specifically, the carbon was pulverized using a ball mill until the average particle size became approximately 3 μm.
[0103] The pulverized activated carbon was then heat-treated in an argon atmosphere using a high-temperature furnace manufactured by Fuji Electric Industries Co., Ltd., at a heating rate of 10°C / min. After the temperature reached 1600°C, it was maintained at this temperature for 0.03 hours.
[0104] In this way, a carbon material for a positive electrode of a nonaqueous secondary battery of Example 3 was obtained.
[0105] <Reference examples 1 to 7> A carbon material for a non-aqueous secondary battery positive electrode was obtained in the same manner as in Example 2, except that the manufacturing conditions were changed as described in the manufacturing conditions in Table 1. However, in Reference Examples 1 and 3, a high-temperature firing furnace manufactured by Hasida Giken Kogyo Co., Ltd. was used for the heat treatment, in Reference Examples 2 and 6, a firing furnace manufactured by Kurata Giken Co., Ltd. was used for the heat treatment, and in Reference Examples 4 and 7, a firing furnace manufactured by Fuji Denpa Co., Ltd. was used for the heat treatment. In addition, in Reference Example 5, the material was fired at 1600°C for 0.5 hours using a high-temperature firing furnace manufactured by Hasida Giken Kogyo Co., Ltd., and then heat-treated in a high-temperature firing furnace manufactured by Fuji Denpa Co., Ltd.
[0106] Comparative Example 1 The activated carbon of Example 3 after the activation treatment but before the heat treatment was used as the carbon material of Comparative Example 1.
[0107] <Preparation of Non-Aqueous Secondary Battery> The carbon material for the non-aqueous secondary battery positive electrode of each example was vacuum dried at 110 ° C for 2 hours. Next, 44 parts by mass of the carbon material of each example, 44 parts by mass of carbon black as a conductive assistant, and 11 parts by mass of polyvinylidene fluoride as a binder were added to a solvent and stirred to prepare a slurry for the positive electrode active material layer. Next, this slurry was applied onto a positive electrode current collector, and the coating was dried at 110 ° C. Aluminum foil was used as the positive electrode current collector. In this manner, a positive electrode laminate consisting of a positive electrode current collector and a positive electrode active material layer having a thickness of 50 μm was obtained.
[0108] The positive electrode laminate is 1.77 cm 2 The coin-shaped electrode was punched out. A three-electrode cell was constructed using this coin-shaped positive electrode (working electrode), metallic lithium as a negative electrode (counter electrode), metallic lithium as a reference electrode, a separator, and a non-aqueous electrolyte. Specifically, a three-electrode cell was fabricated in which a negative electrode (counter electrode) was placed on both sides of a positive electrode via a separator, and metallic lithium was used as a reference electrode. A 30 μm cellulose-based separator was used as the separator. As the non-aqueous electrolyte, a mixed solvent containing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:1 was used, containing LiPF6 as a lithium salt at a concentration of about 1.5 mol / L.
[0109] Evaluation of the physical properties of carbon materials for use in positive electrodes of non-aqueous secondary batteries (BET specific surface area) The BET specific surface area of the carbon material for the positive electrode of a nonaqueous secondary battery in each example was determined by a nitrogen adsorption method using a specific surface area / pore distribution analyzer Quadrasorb SI manufactured by Anton Paar Japan K.K.
[0110] Specifically, the nitrogen gas adsorption amount (cc / g) of the carbon material was measured at each pressure P (mmHg) while increasing the nitrogen gas pressure P in nitrogen gas at 77.4 K. Next, the pressure P was divided by the saturated vapor pressure Po of the nitrogen gas to obtain the relative pressure P / Po, and the nitrogen gas adsorption amount was plotted against each relative pressure P / Po to obtain an adsorption isotherm.
[0111] Then, a BET plot was performed and the specific surface area was calculated.
[0112] The calculation results are shown in Table 1 and FIG.
[0113] (Crystallite diameter) The crystallite diameter of the carbon material for the positive electrode of a nonaqueous secondary battery in each example, i.e., the dimension of the a-axis of the crystallite, was determined from the diffraction peak profile obtained by X-ray diffraction analysis using CuKα radiation. ( 10 ) side The half-width of the diffraction line was measured and calculated according to the Scherrer formula.
[0114] The calculation results are shown in Table 1 and FIG.
[0115] <Evaluation of the performance of non-aqueous secondary batteries> (Energy capacity at low temperatures) The energy capacity of the nonaqueous secondary battery in each example in the low temperature range was calculated by the following method.
[0116] First, the nonaqueous secondary battery of each example was placed in a thermostatic chamber and left at -20°C for 1 hour or more to cool it down.
[0117] The cooled non-aqueous secondary batteries of each example were placed in a battery charge / discharge device HJ-1001SD8 manufactured by Hokuto Denko Corporation, and the voltage was increased to 3.0 V, and then the battery was charged at 5 mA / cm 2 The battery was charged at a constant current of 5 mA / cm until the cell voltage reached 4.4 V, and then left to stand for 10 minutes. 2 The battery was discharged at a constant current of 1000 V until the cell voltage reached 2.2 V. The low-temperature energy capacity was calculated from the discharge capacity at that time.
[0118] The calculation results are shown in Table 1 and FIG.
[0119] (Level of gas generation) As disclosed in Non-Patent Document 2, gas may be generated due to a side reaction between the carbon material and the electrolyte in the positive electrode active material layer of a non-aqueous secondary battery. The extent of this side reaction was evaluated by subjecting the non-aqueous secondary battery to cyclic voltammetry (CV) and measuring the current value.
[0120] Specifically, first, the nonaqueous secondary battery of each example was left at 25°C for 1 hour or more, and then placed in a multi-electrochemical measurement system HZ-Pro manufactured by Hokuto Denko Corporation. After increasing the cell voltage to 3.0V, the voltage was changed at 1mV / g / sec until the cell voltage reached 4.2V, and the anode reaction current was measured. Then, the voltage was changed at 1mV / g / sec until the cell voltage reached 3.0V, and the cathode reaction current was measured. The anode reaction current value at the maximum voltage of 4.4V was taken as the cyclic voltammetry (CV) current value.
[0121] The calculation results are shown in Table 1 and FIG.
[0122] [Table 1]
[0123] As shown in Table 1 above and Figures 1 and 2, the BET specific surface area is 1100 m 2 / g~1400m 2 In the carbon material of the embodiment having a specific surface area of 1.0 to 1.5 nm / g and a crystallite diameter of 3.50 to 5.15 nm, the suppression of the decrease in energy capacity in the low temperature range and the suppression of the generation of gas due to the side reaction between the carbon material and the electrolyte were simultaneously realized. In contrast, in the carbon materials of the reference examples and comparative examples in which at least one of the BET specific surface area and the crystallite diameter does not satisfy this condition, the preferable effect as in the carbon material of the embodiment was not obtained. In particular, as shown in Comparative Example 1, the activated carbon, that is, the carbon material that has only been activated, has a large BET specific surface area, which can suppress the suppression of the decrease in energy capacity in the low temperature range, but the crystallite diameter is also large, which cannot suppress the generation of gas due to the side reaction between the carbon material and the electrolyte.
Claims
1. A carbon material for a positive electrode of a non-aqueous secondary battery, comprising: BET specific surface area is 1100m 2 / g~1400m 2 / g, The crystallite size determined by X-ray diffraction analysis using CuKα radiation is 3.50 nm to 5.15 nm, and The crystallite size is the dimension of the a-axis of the crystallite, and is calculated by measuring the half-width of the diffraction line from the (10) plane from a diffraction peak profile obtained by X-ray diffraction analysis using CuKα radiation, and then calculating it according to Scherrer's formula. Carbon materials (excluding those having a BET specific surface area of 1200 m 2 / g or more and 1650 m 2 / g or less and a crystallite size of 4.5 nm or more).
2. BET specific surface area is 1150m 2 / g~1300m 2 The carbon material according to claim 1, wherein the molecular weight is 1 / g.
3. The carbon material according to claim 1 or 2, wherein the crystallite size determined by X-ray diffraction analysis using CuKα radiation is 3.85 nm to 5.15 nm.
4. A non-aqueous secondary battery having a positive electrode active material layer, a negative electrode active material layer, a separator, and an electrolyte solution, The positive electrode active material layer contains the carbon material according to any one of claims 1 to 3, and The electrolyte solution contains an organic solvent and a lithium salt. Non-aqueous secondary battery.
5. 5. The nonaqueous secondary battery according to claim 4, wherein the organic solvent is an aprotic solvent selected from the group consisting of carbonates, esters, ethers, nitriles, sulfones, and lactones.
6. The lithium salt is LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiN(CF 3 SO 2 ) 2 , LiC(CF 3 SO 2 ) 3 6. The nonaqueous secondary battery according to claim 4, wherein the lithium salt is one or more selected from the group consisting of LiI and LiI.
7. A method for producing the carbon material according to any one of claims 1 to 3, comprising the steps of: performing an activation treatment on the precursor carbon material to increase the specific surface area of the precursor carbon material; and The precursor carbon material after the activation treatment is subjected to a heat treatment to increase the crystallite size of the precursor carbon material.
8. 8. The method according to claim 7, wherein the activation treatment comprises contacting the precursor carbon material with 150 parts by mass to 350 parts by mass of an activator relative to 100 parts by mass of the precursor carbon material at 650° C. to 750° C.
9. The method according to claim 7 or 8, wherein the heat treatment is carried out at a temperature of 1500°C to 1690°C.
Citation Information
Patent Citations
Nonaqueous electrolyte cell
JP2002015782A
Pyrolytic hard carbon material, its manufacturing method and applications
JP2003535803A
Electrode for lithium secondary battery and lithium secondary battery
JP2004296431A
Nonaqueous electrolyte secondary battery
JP2005293931A
Activated carbon, its manufacturing method and polarizable electrode and electric double-layer capacitor using the activated carbon
JP2007112704A