Method for producing modified graphite, secondary battery, battery module, battery pack, and power consumption device

Modified graphite production using coal-based needle coke with a surface coating layer addresses surface defects in conventional graphite, enhancing lithium-ion battery performance by reducing side reactions and improving cycle life.

JP7579874B2Active Publication Date: 2024-11-08CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022553132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-31
Publication Date
2024-11-08
Estimated Expiration
2041-08-31

AI Technical Summary

Technical Problem

Conventional graphite used in lithium-ion secondary batteries suffers from surface defects that cause side reactions with the electrolyte, leading to depletion of active lithium ions, reducing cycle performance and service life.

Method used

A method involving the production of modified graphite using coal-based needle coke as a precursor, subjected to sealed heat treatment to enrich volatile content on its surface, forming a coating layer that reduces surface roughness and improves interfacial performance.

Benefits of technology

The modified graphite enhances initial Coulombic efficiency and cycle performance by minimizing side reactions, resulting in improved energy density and extended service life of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579874000004
    Figure 0007579874000004
  • Figure 0007579874000005
    Figure 0007579874000005
  • Figure 0007579874000006
    Figure 0007579874000006
Patent Text Reader

Abstract

This application provides a method for producing modified graphite, a secondary battery, a battery module, a battery pack, and a power consumption device, which includes a crushing step of crushing coal-based needle coke to obtain material A, a shaping step of shaping material A and removing fines to obtain material B, a heat treatment step of putting material B into a reactor and cooling it to room temperature to obtain material C, and a graphitization step of putting material C into a graphitization furnace and graphitizing it to room temperature, where the obtained product is modified graphite.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of lithium battery technology, in particular to modified graphite, secondary batteries, battery modules, battery packs and power consuming devices. [Background technology]

[0002] In recent years, as the scope of application of lithium-ion secondary batteries becomes wider and wider, lithium-ion secondary batteries are widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, as well as in many fields such as electric tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As lithium-ion secondary batteries have made great strides in development, higher requirements are being placed on their energy density, cycle performance and safety performance. Graphite has become the first candidate for modified graphite in commercial lithium-ion secondary batteries due to its low cost, easy production, and actual capacity close to the theoretical capacity.

[0003] Graphite as anode material generally includes natural graphite and artificial graphite, etc., but the defects on the surface of artificial graphite are generally relatively active and easily react with electrolyte, consuming active lithium, while the loss of active lithium ions reduces the cycle performance of lithium ion secondary battery and damages the service life of lithium ion secondary battery, so the conventional modification technology for artificial graphite still needs to be improved. Summary of the Invention [Problem to be solved by the invention]

[0004] The present application has been made in consideration of the above-mentioned problems, and aims to provide a method for producing modified graphite that can provide a secondary battery containing modified graphite with a relatively high energy density, relatively good cycle performance and safety performance.

[0005] To achieve the above objective, the present application provides a method for producing modified graphite, a secondary battery, a battery module, a battery pack, and a power consuming device. [Means for solving the problem]

[0006] A method for producing modified graphite according to a first aspect of the present application comprises the following steps:

[0007] In the crushing step, the coal-based needle coke is crushed to obtain material A.

[0008] In the shaping step, the material A is shaped and fine powder is removed to obtain the material B.

[0009] In the heat treatment step, the material B is put into a reaction vessel for heat treatment, and then cooled to room temperature to obtain the material C.

[0010] Graphitization step: the material C is put into a high-temperature graphitization furnace for high-temperature graphitization, and then cooled to room temperature, and the resulting product is modified graphite.

[0011] Therefore, in this application, a volatile coal-based needle coke is selected as a precursor and subjected to a sealed heat treatment, so that the volatile matter contained in the coal-based needle coke escapes and is enriched on the surface of the coal-based needle coke precursor, and is uniformly coated on the surface of the coal-based needle coke precursor, that is, the self-coating before graphitization. After graphitization, the resulting modified graphite has a coating layer, and when used as a negative electrode material, it can improve the initial coulombic efficiency of a secondary battery. Although the mechanism is not yet fully understood, it is speculated that the coating layer reduces the surface roughness of the modified graphite, repairs the surface defects of the modified graphite, and makes the specific surface area BET value fall within an appropriate range.

[0012] Among them, coal-based needle coke is obtained by pyrolysis of coal pitch. Coal pitch is a complex mixture containing a large amount of condensed ring aromatic hydrocarbons, and has suitable intermolecular interaction. Compared with petroleum pitch, it has high aromaticity and high carbon yield, so coal tar pitch is an ideal raw material for synthesizing high-quality needle coke. The production method of coal-based needle coke is usually to pretreat coal pitch, then delay coke it and calcinate it at high temperature, and finally obtain coal-based needle coke. Examples of coal-based needle coke include Shin-Nichika coke, Mitsubishi coke, and Anshan coke.

[0013] In any embodiment, the coal-based needle coke has the following, in weight percent: a volatile content of 5-9%, optionally 6-8%, a sulfur content of 0.2% or less, optionally 0.1% or less, an ash content of 0.2% or less, optionally 0.1% or less, a quinoline insoluble content of 0.2% or less, optionally 0.1% or less, a true density of 1.35-1.48 g / cm 3 and optionally, 1.39 to 1.45 g / cm 3 Thus, the present application provides a method for selecting a coal-based needle coke having a specific component as a raw material, so that the volatile matter contained in the raw material can be used as a coating agent, and a coating layer can be formed on the surface without the addition of an additional coating agent, thereby improving the interface performance of the negative electrode material when used as a negative electrode material. The volatile matter refers to some liquid (in this case, in a vapor state) and gaseous products with relatively small molecular weights that are produced when organic matter in the coal-based needle coke is decomposed by heat. The ash refers to inorganic matter (e.g., iron oxide, silicon oxide, etc.) that is finally left after the coal-based needle coke is calcined in an air or oxygen atmosphere.

[0014] In any embodiment, in the heat treatment step, the heat treatment temperature is 400-800° C., optionally 500-700° C., and the constant temperature time is 2-8 hours, optionally 3-6 hours. Thus, by selecting the heat treatment temperature and constant temperature time within the above ranges, the present application can allow the volatile matter in the coal-based needle coke to escape and be sufficiently melted, and form a uniform coating layer on the particle surface.

[0015] In any embodiment, in the heat treatment step, the heating rate is 1-15° C. / min, optionally 5-12° C. / min. Thus, by selecting a heating rate within the above range, the present application can heat the coal-based needle coke at a constant rate, so that the volatile matter gradually overflows and adheres uniformly to the particle surface to form a coating layer.

[0016] In an optional embodiment, in the graphitization step, the graphitization temperature is 2500-3200° C., and the graphitization incubation time is 55-65 hours. Thus, the present application has a good graphitization degree by selecting the graphitization temperature and graphitization incubation time within the above ranges, and when used as a negative electrode material, the manufactured secondary battery has excellent initial coulombic efficiency and cycle performance.

[0017] In any embodiment, in the shaping step, material B must satisfy Dv50=5-12 μm, optionally 8-11 μm, and 5 μm≧Dn10≧1.5 μm, optionally 5 μm≧Dn10≧2.0 μm. Thus, the present application selects material B having the above particle size to facilitate the processing of the subsequent process, thereby obtaining modified graphite with excellent electrochemical performance.

[0018] In any embodiment, in the crushing step, material A has Dv50=3-12 μm, and optionally Dv50=6-9 μm.Therefore, the present application crushes the raw material to the above particle size to ensure the convenience of subsequent processing, and the produced negative electrode material has good electrochemical performance.

[0019] The modified graphite according to the second aspect of the present application is produced by the method of the first aspect of the present application.

[0020] The negative plate according to the third aspect of the present application comprises the modified graphite of the second aspect of the present application.

[0021] A secondary battery according to a fourth aspect of the present application includes the negative electrode plate according to the third aspect of the present application.

[0022] A battery module according to a fifth aspect of the present application includes the secondary battery according to the fourth aspect of the present application.

[0023] A battery pack according to a sixth aspect of the present application includes the battery module of the fifth aspect of the present application.

[0024] A power consumption device according to a seventh aspect of the present application includes at least one selected from the secondary battery according to the fourth aspect of the present application, the battery module according to the fifth aspect of the present application, or the battery pack according to the sixth aspect of the present application. Effect of the Invention

[0025] This application provides a method for producing modified graphite, a negative electrode plate, a secondary battery, a battery module, a battery pack, and a power consumption device. Coal-based needle coke is selected as raw material, and the raw material contains a certain amount of volatile matter. Before graphitization, the coal-based needle coke is subjected to a sealed heat treatment to dissipate the volatile matter contained therein and enrich it on the precursor surface, so that the precursor surface is uniformly coated, that is, the self-coating before graphitization. After graphitization, the obtained modified graphite has a coating layer, which reduces the surface roughness of the modified graphite, repairs the surface defects of the modified graphite, and reduces the consumption of active lithium ions by the modified graphite and the side reaction with the electrolyte, thereby improving the initial coulombic efficiency of the secondary battery containing the modified graphite, and has better cycle performance and service life. [Brief description of the drawings]

[0026] [Figure 1] 1 is a scanning electron micrograph of the modified graphite of the present application. [Diagram 2] FIG. 2 is an initial charge / discharge diagram of Example 1 of the present application. [Diagram 3] FIG. 1 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Figure 4] FIG. 4 is an exploded view of the secondary battery shown in FIG. 3 according to an embodiment of the present application. [Diagram 5] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Figure 6] FIG. 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Figure 7] FIG. 7 is an exploded view of the battery pack of one embodiment of the present application shown in FIG. 6. [Figure 8] 1 is a schematic diagram of a power consuming device that uses a secondary battery as a power source according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, the modified graphite and its manufacturing method, negative electrode plate, secondary battery, battery module, battery pack, and power consumption device of the present application will be described in detail with reference to the drawings as appropriate. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and repeated description of the same structure may be omitted. This is to avoid unnecessary redundancy of the following description and to facilitate understanding by those skilled in the art. Note that the drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0028] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting lower and upper limits that define the boundaries of the particular range. Such defined ranges may or may not include the end values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are recited for a particular parameter, it can be understood that ranges of 60-110 and 80-120 are also contemplated. It can be understood that if minimum range values ​​1 and 2 and maximum range values ​​3, 4 and 5 are recited, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 are all contemplated. In this application, unless otherwise stated, the numerical range "ab" represents a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" represents all real numbers between "0-5" and is merely a shorthand for these numerical combinations. Also, when a parameter is expressed as an integer ≧2, this is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0029] Unless otherwise stated, all the embodiments and optional embodiments in the present application can be combined with each other to form a new technical solution.

[0030] Unless otherwise stated, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0031] Unless otherwise stated, all steps in the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b) to indicate that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method further includes step (c) to indicate that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0032] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the listed ingredients.

[0033] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the term "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or both A and B are true (or exist).

[0034] Manufacturing of modified graphite In one embodiment of the present application, the present application proposes a method for producing modified graphite, which includes a crushing step of crushing coal-based needle coke to obtain material A, a shaping step of shaping the material A and removing fine powder to obtain material B, a heat treatment step of putting the material B into a reaction vessel and cooling it to room temperature to obtain material C, and a graphitization step of putting the material C into a graphitization furnace and graphitizing it and cooling it to room temperature, with the resultant product being the negative electrode material.

[0035] Among them, coal-based needle coke is obtained by pyrolysis of coal pitch. Coal pitch is a complex mixture containing a large amount of condensed ring aromatic hydrocarbons, and has suitable intermolecular interaction. Compared with petroleum pitch, it has high aromaticity and high carbon yield, so coal tar pitch is an ideal raw material for synthesizing high-quality needle coke. The production method of coal-based needle coke is usually to pretreat coal pitch, then delay coke it and calcinate it at high temperature, and finally obtain coal-based needle coke. Examples of coal-based needle coke include Shin-Nichika coke, Mitsubishi coke, and Anshan coke.

[0036] Although the mechanism is not yet fully understood, the applicant has found that by selecting a coal-based needle coke containing a certain content of volatile matter as the precursor, the volatile matter escapes and is enriched on the surface of the precursor through sealed heat treatment, and the surface of the precursor is uniformly coated, that is, self-coated before graphitization. After graphitization, the obtained modified graphite has a coating layer. Figure 1 shows a scanning electron micrograph of the prepared modified graphite, in which the modified graphite has a smooth and flat particle surface, proving that the coating layer effectively reduces the surface roughness of the modified graphite, repairs the surface defects of the modified graphite, reduces the side reaction between the modified graphite surface and the electrolyte, and achieves the purpose of improving its initial coulombic efficiency.

[0037] In some embodiments, the coal-based needle coke has, in mass percent, a volatile content of 5-9%, optionally 6-8%, a sulfur content of 0.2% or less, optionally 0.1% or less, an ash content of 0.2% or less, optionally 0.1% or less, a quinoline insoluble content of 0.2% or less, optionally 0.1% or less, and a true density of 1.35-1.48 g / cm 3 and optionally, 1.39 to 1.45 g / cm 3When the coal-based needle coke is used as a precursor, the volatile components contained in the coal-based needle coke can be used as a coating agent, and a coating layer can be formed on the surface of the precursor without the need for additional coating agents, thereby repairing defects on the particle surface and reducing the roughness of the particle surface. The modified graphite modified with the coating layer reduces the consumption of active lithium ions, thereby improving the initial coulombic efficiency. At the same time, the true density of the precursor has a certain effect on the tap density of the modified graphite produced. Therefore, by selecting a coal-based needle coke with a true density within the above range as a precursor, the modified graphite produced also has a relatively good tap density, and the energy density of the secondary battery using this modified graphite can be improved.

[0038] In some embodiments, in the heat treatment step, the heat treatment temperature is 400-800°C, optionally 500-700°C, and the constant temperature time is 2-8 hours, optionally 3-6 hours. The heat treatment temperature and the constant temperature time are very important for the formation of the coating layer of modified graphite. The heat treatment temperature is within the above range, so that the following situations can be avoided. If the heat treatment temperature is too low and the constant temperature time is too short, the volatile matter in the coal-based needle coke may not melt sufficiently and overflow to form a coating layer on the particle surface, which may result in the loss of the effect of modifying particle surface defects; if the heat treatment temperature is too high and the constant temperature time is too long, the energy consumption in the production process may be too high, which may increase the production cost and result in unnecessary waste. In other words, the heat treatment temperature and isothermal time within the above ranges can overflow and fully melt the volatile matter in the coal-based needle coke, form a uniform coating layer on the particle surface, reduce the consumption of active lithium ions, and further improve the initial coulombic efficiency, without additionally increasing production costs due to high energy consumption.

[0039] In some embodiments, in the heat treatment step, the heating rate is 1-15°C / min, optionally 5-12°C / min. When the heat treatment is within the above range, the following situation can be avoided: When the heating rate is too fast and reaches the heat treatment temperature, the volatile matter of the coal-based needle coke may overflow quickly within a short time, and the volatile matter cannot uniformly cover the particle surface and may cause particle aggregation. That is, with a heating rate within the above range, the coal-based needle coke can receive heat uniformly and be heated at a constant rate, and the volatile matter can uniformly and gradually adhere to the particle surface to form a coating layer, and the modified graphite produced accordingly also has a high initial Coulombic efficiency and better cycle performance.

[0040] In some embodiments, in the graphitization step, the graphitization temperature is 2500-3200° C., and the graphitization incubation time is 55-65 hours. With the graphitization temperature and graphitization incubation time within the above ranges, the modified graphite produced by this method has a good graphitization degree, and the good interlayer distance facilitates the absorption and release of lithium ions, and further improves the initial coulombic efficiency and cycle performance of the modified graphite.

[0041] In some embodiments, in the heat treatment step, the material B must satisfy Dv50=5-12 μm, optionally 8-11 μm, and 5 μm≧Dn10≧1.5 μm, optionally 5 μm≧Dn10≧2.0 μm. By selecting material B having the above particle size, the subsequent process can be easily performed, and the resulting modified graphite has a high tap density and excellent electrochemical performance.

[0042] In some embodiments, in the crushing step, the material A has a Dv50 of 3-12 μm, and optionally a Dv50 of 6-9 μm. When the raw material is crushed to the above particle size and the raw material is subjected to heat treatment and graphitization, the raw material is uniformly and sufficiently heat-treated to ensure that the particle size is uniformly distributed, and the modified graphite produced has a uniform particle size distribution, a complete coating layer, and a high degree of graphitization. Furthermore, when the modified graphite is used as a negative electrode material, it has a high initial coulombic efficiency and good cycle performance.

[0043] The volatile content of the coal-based needle coke can also be tested by methods known in the art, for example, by reference to YB / T5189-2007.

[0044] The sulfur content of the coal-based needle coke can be tested by methods known in the art, for example, as measured with reference to GB / T 2286-2008.

[0045] The ash content of the coal-based needle coke can be tested by methods known in the art, for example, as measured with reference to GB / T 1429-2009.

[0046] The quinoline insoluble matter refers to the components in the coal-based needle coke that are insoluble in quinoline, and the quinoline insoluble matter content of the coal-based needle coke can be tested by methods known in the art, for example, measured with reference to GB / T2293-97.

[0047] The average volume distribution particle size Dv50 refers to the particle size corresponding to the cumulative volume distribution percentage of the modified graphite reaching 50%. In the present invention, the volume average particle size Dv50 of the modified graphite can be measured by adopting a laser diffraction particle size analysis method. For example, refer to standard GB / T 19077-2016 and measure with a laser particle size analyzer (e.g., Malvern Master Size 3000).

[0048] The specific surface area (BET) test of the modified graphite can be performed using a specific surface area analyzer to test the specific surface area of ​​the sample in accordance with GB / T 19587-2017 / ISO9277:2010 "Determination of the specific surface area of ​​solid materials by gas adsorption BET method".

[0049] The graphitization degree of the modified graphite can be tested by using an X-ray diffraction device according to JB / T 4220-2011, "Method for determining lattice parameter of artificial graphite", to test the graphitization degree of the sample, where the graphitization degree is g=(3.440-d002) / (3.440-3.354).

[0050] The true density of the modified graphite can be determined by using a tap density tester to test the tap density of a sample according to GB / T 5162-2006 "Measurement of Tap Density of Metal Powders".

[0051] The secondary battery, battery module, battery pack and power consuming device of the present application will be described below with appropriate reference to the drawings.

[0052] In one embodiment of the present application, a secondary battery is provided.

[0053] Typically, a secondary battery includes a positive electrode plate, a negative electrode plate, an electrolyte, and a separator. During the charge and discharge process of the battery, active ions shuttle between the positive electrode plate and the negative electrode plate to store and release. The electrolyte functions to conduct ions between the positive electrode plate and the negative electrode plate. The separator is provided between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short-circuiting between the positive and negative electrodes, while allowing ions to pass through.

[0054] [Positive plate] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer including a positive electrode material.

[0055] For example, the positive electrode current collector has two surfaces opposing each other in the thickness direction thereof, and the positive electrode film layer is disposed on either one or both of the two opposing surfaces of the positive electrode current collector.

[0056] In the secondary battery of the present application, the positive electrode current collector may adopt a metal foil sheet or a composite current collector. For example, an aluminum foil may be adopted as the metal foil sheet. The composite current collector may include a polymeric material base layer and a metal layer formed on at least one surface of the polymeric material base layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0057] In the secondary battery of the present application, the positive electrode material may adopt a positive electrode material for a battery well known in the art. Exemplarily, the positive electrode material may include at least one material selected from the group consisting of lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode materials for batteries may also be used. These positive electrode materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (may be abbreviated as LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523(may be abbreviated as LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (may be abbreviated as LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (may be abbreviated as LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05 Examples of the lithium-containing phosphate having an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (which may be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.

[0058] In the secondary battery of the present application, the positive electrode membrane layer optionally further includes an adhesive. Exemplarily, the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic ester resin.

[0059] In the secondary battery of the present application, the positive electrode film layer optionally further includes a conductive agent. Exemplarily, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0060] In the secondary battery of the present application, the positive plate can be manufactured in the following manner: The above-mentioned components for manufacturing the positive plate, such as the positive electrode material, conductive agent, adhesive and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry, which is then applied onto a positive electrode current collector, and the positive plate is obtained through processes such as drying and cold pressing.

[0061] [Negative plate] The negative plate includes a negative current collector and a negative film layer disposed on at least one surface of the negative current collector, said negative film layer including the modified graphite of the second aspect of the present application.

[0062] For example, the negative electrode current collector has two surfaces opposing each other in the thickness direction thereof, and the negative electrode film layer is disposed on either one or both of the two opposing surfaces of the negative electrode current collector.

[0063] In the secondary battery of the present application, the negative electrode current collector may adopt a metal foil sheet or a composite current collector. For example, a copper foil may be adopted as the metal foil sheet. The composite current collector may include a polymeric material base layer and a metal layer formed on at least one surface of the polymeric material base layer. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0064] In the secondary battery of the present application, the negative electrode membrane layer optionally further includes an adhesive, which may be selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0065] In the secondary battery of the present application, the negative electrode film layer optionally further includes a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0066] In the secondary battery of the present application, the negative electrode membrane layer may optionally further contain other auxiliary agents, such as a thickener (eg, sodium carboxymethylcellulose (CMC-Na)).

[0067] In the secondary battery of the present application, the negative electrode plate can be manufactured in the following manner. The above-mentioned components for manufacturing the negative electrode plate, for example, the negative electrode material, the conductive agent, the adhesive, and any other components, are dispersed in a solvent (for example, deionized water) to form a negative electrode slurry, and the negative electrode slurry is applied onto a negative electrode current collector, followed by processes such as drying and cold pressing to obtain the negative electrode plate.

[0068] [Electrolyte] The electrolyte serves to conduct ions between the positive and negative plates. The present application is not specifically limited to the type of electrolyte, which can be selected according to need. For example, the electrolyte may be liquid, gel, or all solid.

[0069] In some embodiments, the electrolyte employs an electrolytic solution, the electrolytic solution including an electrolyte salt and a solvent.

[0070] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonimide, lithium bistrifluoromethanesulfonimide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluoro(oxalato)borate, lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, and lithium tetrafluoro(oxalato)phosphate.

[0071] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, ethyl methyl sulfone, and diethyl sulfone.

[0072] In some embodiments, the electrolyte solution optionally further includes additives. For example, the additives may include a negative electrode film-forming additive and a positive electrode film-forming additive, and may further include additives that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature or low temperature performance of the battery, etc.

[0073] [Separator] In secondary batteries using liquid electrolytes and some secondary batteries using solid electrolytes, a separator is further included. In the present application, there is no particular limitation on the type of separator, and any well-known separator with a porous structure having good chemical stability and mechanical stability may be selected.

[0074] In some embodiments, the material of the separator may be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer film or a multi-layer composite film, and there is no particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, and there is no particular limitation.

[0075] In some embodiments, the positive plate, the negative plate and the separator can be manufactured into an electrode component by a winding process or a lamination process.

[0076] In some embodiments, the secondary battery may include an exterior packaging, which may be used to package the electrode components and electrolyte.

[0077] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft bag, such as a pouch-type soft bag. The material of the soft bag may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0078] The present application is not particularly limited to the shape of the secondary battery, which may be cylindrical, rectangular or any other shape. For example, FIG. 3 shows a secondary battery 5 with a rectangular structure as an example.

[0079] In some embodiments, referring to FIG. 4, the exterior may include a case 51 and a cover plate 53. The case 51 may include a bottom plate and a side plate connected on the bottom plate, and the bottom plate and the side plate surround and form a receiving cavity. The case 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be installed on the opening to close the receiving cavity. The positive electrode plate, the negative electrode plate and the separator can be formed into an electrode component 52 by a winding process or a lamination process. The electrode component 52 is packaged in the receiving cavity. The electrolyte is infiltrated into the electrode component 52. The number of electrode components 52 included in the secondary battery 5 may be one or more, and may be selected by those skilled in the art according to actual specific needs.

[0080] In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries included in the battery module may be one or more, with the specific number being selected by one skilled in the art based on the application and capacity of the battery module.

[0081] Fig. 5 shows an example of a battery module 4. Referring to Fig. 5, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by a fastener.

[0082] Optionally, the battery module 4 may further include a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.

[0083] In some embodiments, the battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack may be one or more, and the specific number may be selected by one skilled in the art based on the application and capacity of the battery pack.

[0084] 6 and 7 show an example of a battery pack 1. Referring to Fig. 6 and Fig. 7, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 can shield the lower housing 3 and form a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0085] The present application further provides a power consuming device, the power consuming device including at least one of the secondary battery, battery module, or battery pack according to the present application. The secondary battery, battery module, or battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may include, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), a train, a ship, a satellite, an energy storage system, etc.

[0086] The power consumption device can be selected as a secondary battery, a battery module, or a battery pack according to the demands of its use.

[0087] 8 shows an example of a power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. The power consuming device may employ a battery pack or a battery module to meet the demand for high power and high energy density for secondary batteries.

[0088] Another example of the device may be a mobile phone, a tablet computer, a notebook computer, etc. This device usually requires light weight and thinness, and can employ a secondary battery as a power source.

[0089] Working Example The following describes the examples of the present application. The examples described below are illustrative and are used only to interpret the present application, and should not be understood as limiting the present application. In the examples, specific techniques or conditions are not specified, and are carried out according to the techniques or conditions described in the technical literature or product instructions. For reagents or equipment used, those without the manufacturer are all common products that can be purchased commercially.

[0090] Example 1 The coal-based needle coke raw material is crushed by an LHJ-type mechanical crusher (manufacturer: Weifang Zhengyuan Powder Engineering Equipment Co., Ltd.). The sulfur content of the coal-based needle coke is 0.08%, the ash content is 0.05%, the volatile matter content is 5.1%, and the true density is 1.42g / cm3. The coal-based needle coke is crushed to Dv50=6-9μm, and then classified, so that the particle size distribution of the obtained particle product can be easily adjusted later. The crushed coal-based needle coke is shaped by an LHV-type shaping machine (manufacturer: Weifang Zhengyuan Powder Engineering Equipment Co., Ltd.), the main machine frequency is 8Hz, and fine powder is removed, and the coke is processed to Dv50=9.8μm. The shaped material is placed in a WHR-type horizontal heating reaction vessel (manufacturer: Wuxi Qing Jin Powder Equipment Co., Ltd.) for heat treatment, where it is heated to 600°C at 10°C / min and kept at a constant temperature for 4 hours. The product obtained by the heat treatment is placed in a graphitization furnace, heated to 3000°C, and kept at that temperature for 60 hours to perform high-temperature graphitization, obtaining artificial graphite. The modified graphite produced in this way has a Dv50 of 9.0 μm, Dv10 of 5.4 μm, and BET of 1.34 m. 2 / g, graphitization degree = 95.3%, tap density 1.21 g / cm 3 It is.

[0091] Example 2 The heat treatment temperature was adjusted to 500°C, and the particle size after the shaping treatment was Dv50 = 11.4 μm. Other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 10.5 μm, Dv10 = 5.3 μm, and BET = 1.35 μm. 2 / g, graphitization degree = 95.1%, tap density = 1.18g / cm 3 It is.

[0092] Example 3 The heat treatment temperature was adjusted to 400°C, and the particle size after the shaping treatment was Dv50 = 10.3 μm. Other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 9.7 μm, Dv10 = 5.8 μm, and BET = 1.37 m. 2 / g, graphitization degree = 95.0%, tap density = 1.17 g / cm 3 It is.

[0093] Example 4 The heat treatment temperature was adjusted to 800°C, and the particle size after the shaping treatment was Dv50 = 10.0 μm. The other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 9.5 μm, Dv10 = 6.1 μm, and BET = 1.38 m. 2 / g, graphitization degree = 95.2%, tap density 1.20g / cm 3 It is.

[0094] Example 5 The heat treatment time was adjusted to 6 hours, and the particle size after the shaping treatment was Dv50 = 10.8 μm. The other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 10.2 μm, Dv10 = 5.4 μm, and BET = 1.33 m. 2 / g, graphitization degree = 95.3%, tap density = 1.18g / cm 3 It is.

[0095] Example 6 The heat treatment time was adjusted to 2 hours, and the particle size after the shaping treatment was Dv50 = 9.4 μm. Other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 8.8 μm, Dv10 = 5.1 μm, and BET = 1.35 μm. 2 / g, graphitization degree = 95.2%, tap density = 1.19 g / cm 3 It is.

[0096] Example 7 The heat treatment time was adjusted to 8 hours, and the particle size after the shaping treatment was Dv50 = 9.7 μm. The other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 9.1 μm, Dv10 = 5.5 μm, and BET = 1.36 m. 2 / g, graphitization degree = 95.3%, tap density = 1.17g / cm 3 It is.

[0097] Example 8 The volatile matter content of the coal-based needle coke is 6.4%, the sulfur content is 0.06%, the ash content is 0.03%, the quinoline insoluble matter content is 0.07%, and the true density is 1.43 g / cm 3The other conditions were the same as in Example 1, except that the particle size after the shaping treatment was Dv50 = 10.1 μm. The modified graphite produced by this method had Dv50 = 9.5 μm, Dv10 = 5.1 μm, and BET = 1.31 m. 2 / g, graphitization degree = 95.1%, tap density = 1.23 g / cm 3 It is.

[0098] Example 9 Volatile matter content 6.8%, sulfur content 0.07%, ash content 0.04%, quinoline insoluble content 0.03%, true density 1.36g / cm 3 The other conditions were the same as in Example 1, except that the particle size after the shaping treatment was Dv50 = 10.5 μm. The modified graphite produced by this method had Dv50 = 10.1 μm, Dv10 = 5.3 μm, and BET = 1.33 μm. 2 / g, graphitization degree = 95.0%, tap density = 1.21 g / cm 3 It is.

[0099] Example 10 Volatile matter content 7.5%, sulfur content 0.06%, ash content 0.07%, quinoline insoluble content 0.04%, true density 1.48g / cm 3 The other conditions were the same as in Example 1, except that the particle size after the shaping treatment was Dv50 = 9.7 μm. The modified graphite produced by this method had Dv50 = 9.5 μm, Dv10 = 5.1 μm, and BET = 1.31 m. 2 / g, graphitization degree = 95.1%, tap density = 1.25g / cm 3 It is.

[0100] Comparative Example 1 The LHJ-type mechanical crusher (manufacturer: Weifang Zhengyuan Powder Engineering Equipment Co., Ltd.) is used to crush the coal-based needle coke raw material. The sulfur content of the coal-based needle coke is 0.08%, the ash content is 0.05%, the volatile matter content is 1.2%, the quinoline insoluble matter content is 0.04%, and the true density is 1.4 g / cm. 3The coal-based needle coke is crushed to Dv50=6~9μm, and then classified, so that the particle size distribution of the resulting particle product can be easily adjusted later. The crushed coal-based needle coke is shaped in an LHV-type shaping machine (manufacturer: Weifang Zhengyuan Powder Engineering Equipment Co., Ltd.), the main machine frequency is 8Hz, and fine powder is removed and processed to Dv50=10.7μm. The shaped material is placed in a WHR-type horizontal heating reaction kettle (manufacturer: Wuxi Qingjin Powder Equipment Co., Ltd.) for heat treatment, heated to 600℃ at 10℃ / min, and kept at a constant temperature for 4 hours. The product obtained by the heat treatment is placed in a graphitization furnace, heated to 3000℃, and kept at 3000℃ for 60 hours to perform high-temperature graphitization, and artificial graphite is obtained. The modified graphite produced in this way has Dv50=9.2μm, Dv10=5.6μm, BET=1.57m 2 / g, graphitization degree = 95.2%, tap density = 1.13 g / cm 3 It is.

[0101] Comparative Example 2 The raw material was converted to ordinary petroleum coke, the volatile matter content was adjusted to 10%, the sulfur content was 0.21%, the ash content was 0.07%, there was no quinoline insoluble matter, the true density was 1.45g / cm3, and the particles after shaping treatment had Dv50=10.2μm. Other conditions were the same as those in Comparative Example 1. The modified graphite produced thereby had Dv50=16.5μm, Dv10=6.8μm, BET=1.52m 2 / g, graphitization degree = 93.1%, tap density = 1.09g / cm 3 It is.

[0102] Comparative Example 3 The step of heat treating the coal-based needle coke was omitted, and the other conditions were the same as in Example 1, except that the particles after the shaping treatment had a Dv50 of 9.7 μm. The modified graphite produced thereby had Dv50 of 9.0 μm, Dv10 of 5.4 μm, and BET of 1.61 μm. 2 / g, graphitization degree = 95.0%, tap density = 1.17 g / cm 3 It is.

[0103] Comparative Example 4 The raw material is converted into ordinary petroleum coke, and the volatile matter content is adjusted to 0.9%, the sulfur content is 0.30%, the ash content is 0.15%, and the true density is 1.44g / cm 3 The heat treatment step was cancelled, and the particle size after the shaping treatment was Dv50 = 10.7 μm. The other conditions were the same as those of Comparative Example 2. The modified graphite produced thereby had Dv50 = 10.3 μm, Dv10 = 6.0 μm, and BET = 1.49 μm. 2 / g, graphitization degree = 94.0%, tap density = 1.26 g / cm 3 It is.

[0104] Comparative Example 5 The heat treatment temperature was adjusted to 200°C, the heat treatment time was 1 hour, and the particle size after the shaping treatment was Dv50 = 9.5 μm. The other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 8.9 μm, Dv10 = 5.2 μm, BET = 1.53 m 2 / g, graphitization degree = 95.2%, tap density = 1.03 g / cm 3 It is.

[0105] Comparative Example 6 The heat treatment time was adjusted to 1 hour, and the particle size after the shaping treatment was Dv50 = 9.5 μm. Other conditions were the same as in Example 1. The modified graphite produced thereby had Dv50 = 9.0 μm, Dv10 = 5.1 μm, and BET = 1.51 m. 2 / g, graphitization degree = 95.0%, tap density = 1.24 g / cm 3 It is.

[0106] The production parameters for the modified graphites of Examples 1 to 10 and Comparative Examples 1 to 6 are as shown in Table 1 below.

[0107] [Table 1]

[0108] The modified graphite obtained in the above Examples 1 to 10 and Comparative Examples 1 to 6 was subjected to an average volume particle size distribution test, a BET test, a graphitization degree test, and a tap density test. The test results are shown in Table 2.

[0109] [Table 2]

[0110] In addition, the modified graphite obtained in the above Examples 1 to 10 and Comparative Examples 1 to 6 is manufactured into a button battery and a secondary battery as described below, and an electrochemical performance test is carried out. The test results are shown in Table 3.

[0111] (1) Manufacture of button batteries The modified graphite, conductive agent Super P, and adhesive (PVDF) in each of the above examples and comparative examples were uniformly mixed with a solvent NMP (N-methylpyrrolidone) in a mass ratio of 91.6:1.8:6.6 to prepare a slurry. The prepared slurry was applied to a copper foil current collector, dried in an oven, and then cold pressed for use. The compaction range was 1.4 to 1.6 g / cm. 3 A lithium metal plate is used as the counter electrode, a polyethylene (PE) film is used as the separator, ethylene carbonate (EC), ethylene carbonate (EMC), and diethylene carbonate (DEC) are mixed in a volume ratio of 1:1:1, and LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, in which the concentration of LiPF6 is 1mol / L. In a glove box protected by argon, the above parts can be assembled into a CR2430 button cell battery.

[0112] (2) Initial gram capacity and initial coulombic efficiency tests for button batteries After the obtained button battery is left to stand for 12 hours, it is discharged at a constant current of 0.05C to 0.005V using LAND CT2001A, left to stand for 10 minutes, discharged at a constant current of 50μA to 0.005V, left to stand for 10 minutes, discharged at a constant current of 10μA to 0.005V, the total of the three discharge capacities is the discharge capacity c0, and then charged at a constant current of 0.1C to 2.000V, and the charge capacity c is recorded. The gram capacity of the produced negative electrode material = charge capacity c / negative electrode material mass m, and the initial coulombic efficiency = (charge capacity c / discharge capacity c0) * 100%.

[0113] (3) Manufacture of secondary batteries The modified graphite in each of the above examples and comparative examples is used as the negative electrode active material, and acetylene black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener are thoroughly mixed in a weight ratio of 90:5:2:2:1 in deionized water solvent and stirred to homogeneity, and then the mixture is applied to copper foil, dried, and cold pressed to obtain a negative electrode plate.

[0114] The positive electrode material is made by thoroughly mixing the conductive agent acetylene black and the adhesive polyvinylidene fluoride (PVDF) in a weight ratio of 94:3:3 in N-methylpyrrolidone solvent until homogeneous, then applying the mixture to copper foil, drying, and cold pressing to obtain the positive electrode plate.

[0115] A porous polymeric film made of polyethylene (PE) is used as the separator.

[0116] The positive electrode plate, the separator and the negative electrode plate are stacked in order, the separator serves to isolate the positive and negative electrodes, and the bare cell is then wound up to obtain a bare cell. The bare cell is then placed in an outer casing, and the electrolyte used in the above (1) button battery manufacturing process is injected and packaged to obtain a secondary battery.

[0117] (4) Cycle performance test of secondary batteries at 45℃ Each secondary battery prepared above is first charged at 25°C at 1 / 3C to 3.65V (C is the nominal capacity of the battery), charged at a constant voltage of 3.65V to 0.05C, and then discharged at 1 / 3C to 2.5V, and the discharge capacity C0 is recorded. The cycle performance of the battery is tested in an environment of 45°C, and the battery is subjected to a charge-discharge cycle at a rate of 1C0 / 1C0 between 2.5 and 3.65V, and the discharge capacity of the battery at the 100th cycle is C0. 100 The cycle capacity retention rate at the 100th cycle is C 100 / C0.

[0118] [Table 3]

[0119] As can be seen from the above results, in Examples 1 to 10, when no additional coating agent is added, the volatile components contained in the coal-based needle coke itself are used as a coating agent, and the modified graphite produced has a coating layer, which improves the particle surface roughness and reduces the consumption of active lithium in the electrolyte, and thus improves the electrochemical performance of the modified graphite produced. As shown in FIG. 2, FIG. 2 is the initial charge / discharge diagram of the modified graphite of Example 1 of the present application. The modified graphite of Example 1 shows excellent electrochemical performance with an initial discharge gram capacity of 376.9 mAh / g, an initial charge gram capacity of 358.1 mAh / g, and an initial coulombic efficiency of 95.0%. Overall, the initial coulombic efficiencies of the modified graphites of Examples 1 to 10 are all above 95.0%, and the capacity retention rates after 100 cycles at 45° C. are all greater than 97.0%.

[0120] In contrast, in Comparative Example 1, under the same heat treatment process conditions as in Example 1, the volatile matter content of the coal-based needle coke is relatively low, so the volatile matter cannot fully and uniformly cover the particle surface, and the coating layer cannot fully improve the interface performance of the graphite, so the initial coulombic efficiency of the modified graphite produced is relatively low. In Comparative Example 2 and Comparative Example 4, compared to Examples 1 to 10, ordinary petroleum coke is used as the raw material. In Comparative Example 2, adhesion effect occurs during the heat treatment process of ordinary petroleum coke, causing particle aggregation, and the initial coulombic efficiency of the modified graphite produced cannot be effectively improved. In Comparative Example 4, the volatile matter content of the ordinary petroleum coke is relatively low, and the heat treatment process therefor is canceled, so the modified graphite produced does not have a coating layer and there are still defects on the particle surface, so the effect of reducing the consumption of active lithium and improving its initial coulombic efficiency is not good.

[0121] The differences between Comparative Example 3, Comparative Example 5, and Comparative Example 6 and Example 1 are mainly the heat treatment temperature and heat treatment time. In Comparative Example 3, the heat treatment of the coal-based needle coke is canceled, and the volatile matter cannot uniformly coat the particle surface to form a coating layer, and the interface performance of the produced modified graphite cannot be improved, so that the cycle performance and initial coulombic efficiency are not as good as those of the modified graphite in Examples 1 to 10. In Comparative Example 5, the heat treatment temperature is relatively low, the volatile matter cannot be sufficiently enriched on the particle surface, and the heat treatment time is relatively short, and the volatile matter cannot form a complete core-shell structure to improve the particle surface. Therefore, the effect on improving the interface performance and electrochemical performance of the graphite is not good. In Comparative Example 6, the heat treatment time of the coal-based needle coke is relatively short, and the side reaction occurring between the modified graphite and the electrolyte cannot be reduced by forming a coating layer on the particle surface. Therefore, there is a limit to the improvement effect on the electrochemical performance and interface performance of the produced modified graphite.

[0122] In addition, in Table 2, it was found that the BET of the modified graphite in Examples 1 to 10 was smaller than that of the modified graphite in Comparative Examples 1 to 6 from Examples 1 to 10 and Comparative Examples 1 to 6. When the modified graphite is used as the negative electrode material of the secondary battery, the BET is related to the initial Coulombic efficiency, and for example, the larger the BET, the easier the negative electrode material is to side-react with the electrolyte, and the active lithium is consumed, thereby affecting the cycle performance of the negative electrode material. Therefore, the modified graphite in Examples 1 to 10 has a relatively small BET compared to the modified graphite in Comparative Examples 1 to 6, which means that the modified graphite in Examples 1 to 10 has a better initial Coulombic efficiency as a negative electrode material. The data in Table 3 also fully proves this point. In addition, the modified graphite in Examples 1 to 10 has a larger tap density than the modified graphite in Comparative Examples 1 to 6. The negative electrode material with a high tap density also ensures the energy density of the entire secondary battery.

[0123] It should be explained that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea and having the same action and effect within the scope of the technical proposal of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of to the embodiment are implemented within the scope of the gist of the present application, and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application. [Explanation of symbols]

[0124] 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 case, 52 electrode component, 53 top cover component

Claims

1. A method for producing modified graphite, comprising the steps of: A crushing step of crushing the coal-based needle coke to obtain material A; A shaping step of shaping the material A and removing fine powder to obtain a material B; A heat treatment step of putting the material B into a reaction vessel, performing a heat treatment, and then cooling it to room temperature to obtain a material C; a graphitization step of putting the material C into a graphitization furnace to perform graphitization, and then cooling it to room temperature, and the resulting product is the modified graphite; The coal-based needle coke has, in mass percent, a volatile matter content of 5 to 9%, a sulfur content of 0.2% or less, an ash content of 0.2% or less, and a quinoline insoluble content of 0.2% or less, and a true density of 1.35 to 1.48 g / cm 3 and In the heat treatment step, the heat treatment temperature is 400 to 800° C., and the heat treatment time is 2 to 8 hours. A method for producing modified graphite.

2. The method for producing modified graphite according to claim 1, characterized in that in the heat treatment step, the temperature increase rate is 1 to 15° C. / min.

3. The method for producing modified graphite according to claim 1 or 2, characterized in that in the graphitization step, the graphitization temperature is 2500 to 3200° C., and the graphitization time is 55 to 65 hours.

4. In the shaping step, the material B satisfies Dv50=5 to 12 μm, The method for producing modified graphite according to any one of claims 1 to 3, characterized in that 5 μm ≧ Dn10 ≧ 1.5 μm is satisfied.

5. The method for producing modified graphite according to any one of claims 1 to 4, characterized in that, in the crushing step, the material A satisfies Dv50 = 3 to 12 μm.

Citation Information

Patent Citations

  • Electrode material and secondary battery

    CN109704323A

  • Electrode material and secondary battery

    CN109704324A

  • Method for producing negative electrode active material for lithium secondary battery

    CN113226986A

  • Manufacture of graphite powder for lithium ion secondary battery negative electrode

    JP2001023638A