Doped photovoltaic semiconductor layers and methods of manufacture - Patents.com
By incorporating Group V dopants into CdTe absorber layers and treating them in a reducing environment with passivating agents, the method addresses the inefficiencies of mobile dopants in CdTe-based photovoltaic devices, enhancing charge carrier concentration and stability, thereby improving device efficiency.
Patent Information
- Application Number
- JP2023126839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-02-24
- Filing Date
- 2023-08-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2038-02-22
AI Technical Summary
Existing photovoltaic devices face challenges in efficiently doping CdTe-based materials with p-type dopants, such as copper, which are mobile and lead to device degradation, and there is a need for scalable and cost-effective manufacturing processes to enhance charge carrier concentration and stability.
A method involving the use of Group V dopants like arsenic, antimony, or phosphorus in CdTe absorber layers, followed by a reducing environment heat treatment with passivating agents like CdCl2 and hydrogen, to incorporate dopants into the crystal lattice, promoting high hole density and stability.
This approach enhances charge carrier concentration, reduces defects, and improves device efficiency by increasing open-circuit voltage and fill factor, leading to more stable and efficient photovoltaic performance.
Smart Images

Figure 0007579930000002 
Figure 0007579930000003 
Figure 0007579930000004
Abstract
Description
[Technical field]
[0001]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 463,579, filed February 24, 2017, which is incorporated herein by reference in its entirety. [Background technology]
[0002]
[0002] Photovoltaic devices use semiconductor materials that exhibit the photovoltaic effect to generate power by converting light into direct current electricity. Photovoltaic devices produce electric current when light absorption excites charge carriers, electrons, or holes, to a higher energy state through the photovoltaic effect. When a charge carrier moves to a higher energy state, for example when an electron is excited from the valence band to the conduction band, a minimum activation energy is required to overcome the band gap and move the charge carrier to allow electric current to flow. The conductivity of a semiconductor is proportional to the product of the charge carrier mobility and the charge carrier concentration.
[0003]
[0003] Dopants are used in the semiconductor materials of photovoltaic devices to adjust the Fermi level and increase the charge carrier concentration. The addition of dopants to semiconductors can be used to produce materials with predominantly negatively charged (n-type) or positively charged (p-type) charge carriers.
[0004]
[0004] In CdTe-based photovoltaic devices, the open circuit voltage (V OC) is due in part to the low majority carrier concentration and short minority carrier lifetime in CdTe. The effective carrier concentration of CdTe can be enhanced by doping with p-type dopants. Further problems limiting the device efficiency of CdTe solar cells include the high work function of CdTe and the high back contact resistance at the interface between CdTe and a metallic back contact layer. The back contact resistance can be improved by increasing the majority carrier concentration at the back interface. For example, for p-type CdTe material, the carrier concentration amount is increased to increase the p-type carriers in the CdTe material and form an "ohmic contact layer" on the back side of the CdTe layer that contacts the back contact layer.
[0005]
[0005] While dopants are somewhat effective in adjusting the Fermi level and increasing the charge carrier concentration, some dopants have also been found to contribute to device degradation, to migrate under operating conditions, to contribute to carrier recombination, or to generate fewer mobile charge carriers than expected.
[0006]
[0006] For example, copper is used in p-type doped II-VI semiconductor materials such as CdTe. Copper dopants are highly mobile and move over time under bias. Copper dopants do not remain fixed within the crystal lattice of polycrystalline thin films. Through these mechanisms, dopants can adversely affect device lifetime, long-term stability, and performance.
[0007]
[0007] There are three types of p-type dopants that are likely to be used in polycrystalline CdTe: substitution of Cd with single acceptor metals such as copper or silver, vacancies at Cd sites, and substitution of Te with group V elements. As discussed in US Patent Application Publication No. 2012 / 0042950, substitution of Te with group V elements is believed to be nearly impossible because the substitution of Te is thermodynamically unfavorable compared to the substitution of Cd. Also, Cd has a higher vapor pressure compared to Te, so Cd evaporates more easily from the film, forming a Te-rich, Cd-poor film under the high temperature processing conditions used in photovoltaic device fabrication. Thus, photovoltaic star Reliable substitution of Te by group V elements in polycrystalline CdTe thin films in the SiO2 / ...
[0008]
[0008] It has been a challenge to efficiently dope CdTe and CdTe alloys to achieve the desired mobile p-type charge carrier concentration in efficient and stable devices. A further challenge is to fabricate such devices using a scalable and cost-effective manufacturing process. It would therefore be desirable to provide improved photovoltaic devices and methods for forming doped semiconductor materials. Summary of the Invention
[0009]
[0009] The embodiments set forth in the drawings are exemplary and illustrative in nature and are not intended to limit the subject matter defined by the claims. The following detailed description of illustrative embodiments can be understood when read in conjunction with the following drawings, in which like structure is designated with like reference numerals and in which: [Brief description of the drawings]
[0010] [Figure 1]
[0010] FIG. 1 is a diagram showing an overview of a functional layer in an embodiment of a photovoltaic element. [Diagram 2]
[0011] 1A-1D illustrate an exemplary method for forming and processing an absorber layer of a photovoltaic device according to an embodiment of the present disclosure. [Diagram 3]
[0012] FIG. 1 shows an overview of the functional layers of a photovoltaic stack in a partially formed device. [Figure 4]
[0013] 1 is a flow chart illustrating an exemplary process for manufacturing a photovoltaic device, including forming and processing semiconductor layers according to embodiments of the present disclosure. [Diagram 5]
[0014] FIG. 13 shows Raman spectra of an absorber film with and without pretreatment. [Figure 6]
[0015] 1 is a graph plotting normalized luminescence (PL) intensity values for absorber films with and without pretreatment. [Figure 7]
[0016] FIG. 1 shows normalized quantum efficiency (QE) versus wavelength for absorber films with and without pretreatment. [Figure 8]
[0017] FIG. 1 shows capacitance-voltage (CV) measurements of charge carrier concentration versus depth in atoms per cm 3 (top) and phase angle (bottom) for treated arsenic-doped CdTe absorbers with and without pretreatment. [Figure 9]
[0018] FIG. 13 shows the depth distribution of elemental concentrations measured by DSIMS for the treated arsenic doped absorber film. [Figure 10]
[0019] FIG. 1 shows CV measurements of charge carrier concentration versus depth comparing devices treated with selected concentration levels of hydrogen gas. [Figure 11]
[0020] FIG. 1 shows VOC measurements of control (left) and treated (right) elements. [Figure 12]
[0021] FIG. 1 shows current-voltage (IV) curves for control (left) and treated (right) devices. [Figure 13A]
[0022] FIG. 1 shows the results of measurements on an arsenic doped device processed according to an embodiment of the method, showing the DSIMS distribution of arsenic dopants in the processed device. [Figure 13B] FIG. 13 shows CV measurements of charge carrier concentration for an arsenic doped device processed according to an embodiment of the method. [Figure 13C] FIG. 13 shows measurement results for an arsenic doped device processed according to an embodiment of the present method, showing an IV curve for the arsenic doped device with a measured VOC of 883 mV. [Figure 14A]
[0023] FIG. 1 shows measurement results for arsenic doped devices processed according to an embodiment of the method. FIG. 2 shows QE measurement results for arsenic doped devices. [Figure 14B] FIG. 13 shows CV measurements of charge carrier concentration for an arsenic doped device processed according to an embodiment of the method. [Figure 14C] FIG. 13 shows measurement results for an arsenic doped device processed according to an embodiment of the present method, showing the IV curve for the device with a measured VOC of 806 mV and FF of 78.3%. [Figure 15]
[0024] FIG. 13 shows capacitance-voltage measurements plotting charge carrier concentration versus depth for the treated antimony-doped CdTe absorber. [Figure 16]
[0025] FIG. 13 shows capacitance-voltage measurements plotting charge carrier concentration versus depth for a treated phosphorus-doped CdTe absorber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011]
[0026] Methods, structures, and compositions are provided for use in photovoltaic (PV) devices. Embodiments provide thin film photovoltaic devices having a p-type absorber layer. Embodiments include methods for p-type doping II-VI semiconductor polycrystalline thin films with a Group V dopant and heat treating in a reducing environment to achieve high hole density in an efficient and stable device. Embodiments include a II-VI semiconductor absorber layer having a Group V dopant incorporated into vacancies of a Group VI semiconductor element in the polycrystalline lattice.
[0012]
[0027] The detailed description given below in conjunction with the accompanying drawings is intended to illustrate examples and is not intended to represent the only manner in which the examples may be constructed or utilized. The term "exemplary" as used herein means "serving as an example, instance, or illustration." Thus, as being "exemplary," any embodiment described herein should not necessarily be construed as preferred or advantageous over other embodiments. All embodiments described herein are provided to enable one skilled in the art to make or use the embodiments described herein, and are not intended to limit the scope of the disclosure, which is defined by the claims. Furthermore, there is no intention to be bound by any theory, expressed or implied, presented herein.
[0013]
[0028] In the specification, drawings, and claims, method-related embodiments are not limited by a particular sequence of steps, unless the context clearly dictates otherwise. Thus, in some embodiments, two or more steps of the method may be performed simultaneously. Alternatively, in some embodiments, two or more steps of the method may be performed sequentially. Method-related embodiments are not limited to the order of steps described in the claims, drawings, or specification. The order of process steps may be interchanged, unless the resulting order is logically inconsistent. Relative terms such as first and second may be used to distinguish one entity or operation from another, and do not require or imply a context or order between such entities or operations, unless specified.
[0014]
[0029] In the following specification and claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. As used herein, the term "or" is not intended to be used in an exclusive sense and means at least one of the referenced elements being considered, unless the context clearly dictates otherwise, and includes cases where combinations of the referenced elements may be considered.
[0015]
[0030] Typically, thin-film photovoltaic devices are made from various layers of different materials formed on a substrate, each layer performing a function. Thin-film photovoltaic devices include a front electrode and a back electrode that provide electrical access to the photovoltaic semiconductor layer or other layers sandwiched between them.
[0016]
[0031] Each layer described in the following embodiments may be composed of two or more layers or films. Each layer may cover all or a portion of the PV element and / or all or a portion of the material underlying the layer or layers. For example, a "layer" may mean any amount of material in contact with an entire surface or a portion of a surface. During the process of forming one of the layers, the layer being created is formed on the outer surface, usually the top surface, of the substrate or substrate structure. The substrate may include a base layer that is introduced in the deposition process, and any other or additional layers that may have been deposited on the base layer in a previous deposition process or previous deposition processes. Layers may be deposited over the entire substrate and certain portions of the material may be removed later through laser ablation, scribing, or other material removal processes.
[0017]
[0032] Fabrication of photovoltaic devices typically involves sequentially arranging functional layers or layer precursors into a stack through one or more processes, including but not limited to sputtering, spraying, evaporation, molecular beam deposition, pyrolysis, close space sublimation (CSS), pulsed laser deposition (PLD), chemical vapor deposition (CVD), electrochemical deposition (ECD), atomic layer deposition (ALD), or vapor transport deposition (VTD). Conditions may be adjusted during deposition to adjust the presence or absence of reactants and precursor compounds to modify the layer during formation. After a layer is formed, it may be desirable to modify the physical properties of the layer through subsequent processing steps.
[0018]
[0033] Photovoltaic devices generally include multiple layers of materials disposed on a substrate. The layers include a semiconductor absorber for converting photon energy into electrical current, and front and back contacts for collecting and conducting the resulting current to or from the device. One or more layers of material can be used to form a p-n junction, such as a homojunction or heterojunction. Functionally, the one or more layers of material can include an absorber layer, a window layer, a buffer, a transparent layer, an interface layer, or a combination thereof. Many other layers may be optionally present to improve the performance of the device.
[0019]
[0034] In this disclosure, when a layer is described as being disposed or located "on" another layer or substrate, it should be understood that the layers may be in direct contact with each other or may have one (or more) layers or features between them. Furthermore, the term "on" describes the relative location of layers and does not necessarily mean "on top of", since above or below, which describes a relative location, depends on the orientation of the element relative to the viewer. Furthermore, "top", "bottom", "above", "below", and variations of these words are used for convenience and do not require any particular orientation of the components unless otherwise stated. However, the orientation remains consistent with each embodiment or example, such as if B is "on" A and C is "on" B, B does not need to be in contact with either, but is necessarily between A and C, etc. In this disclosure, when an object is described as being "adjacent," the word adjacent should be understood to mean "next to" and "in direct contact with" another object, and is not synonymous with the word "on" although an object may be "on" or "adjacent" another object.
[0020]
[0035] Throughout this specification and the claims, the approximating words used herein are used to modify any quantitative expression that may vary within a permissible range without causing a change in the basic function to which it relates. Thus, values modified by a term or terms such as "about", "approximately", and "substantially" are not limited to the exact value specified. In some instances, the approximating words may correspond to the precision of an instrument that measures the value. Here, and throughout this specification and the claims, range limitations may be combined and / or substituted, and unless otherwise indicated by context or language, such ranges are treated the same and include all subranges contained therein.
[0021]
[0036] The presently disclosed embodiments relate to a method for treating a semiconductor layer. The term "semiconductor layer" as used herein refers to a layer of semiconductor material that may be further disposed on one or more other layers. In some embodiments, the semiconductor layer includes an absorber layer. The term "absorber layer" as used herein refers to a semiconducting layer, where the absorption of electromagnetic radiation excites electrons in the absorber layer from a lower energy "ground state" or "valence band," where electrons are bound to specific atoms in the solid, to a higher "excited state" or "conduction band," where charge carriers can move around in the solid.
[0022]
[0037] The term "chalcogenide" as used herein refers to a compound of at least one chalcogen and at least one electropositive element. The term "chalcogen" refers to tellurium, selenium, or sulfur. Suitable chalcogenide materials include binary, ternary, or quaternary compounds such as cadmium telluride, magnesium telluride, mercury telluride, lead telluride, zinc telluride, cadmium selenide, mercury selenide, lead selenide, zinc selenide, cadmium sulfide, mercury sulfide, zinc sulfide, lead sulfide, cadmium selenium telluride, cadmium zinc telluride, cadmium sulfur telluride, cadmium manganese telluride, cadmium magnesium telluride, or combinations thereof. The semiconductor materials mentioned above may be used alone or in combination. Furthermore, these materials may be present in two or more layers, with each layer having a different type of semiconductor material or each layer having a combination of materials in a separate layer. In some embodiments, the semiconductor layer comprises cadmium telluride (CdTe). In some embodiments, the semiconductor layer comprises p-type CdTe. In some embodiments, the semiconductor layer consists essentially of CdTe. In some embodiments, the semiconductor layer comprises cadmium selenium telluride (CdSeTe).
[0023]
[0038] The embodiments of the present disclosure include photovoltaic devices that include II-VI semiconductors. At the atomic level, these semiconductor materials tend to form lattice structures in which the group II elements, such as cadmium and zinc, are in stoichiometric equilibrium and approximately equivalent with the group VI elements, such as sulfur, selenium, and tellurium. In some embodiments, the composition of the layer is adjusted to be "rich" in one or more elements. For example, a Cd-rich layer in a CdTe layer has more cadmium than tellurium.
[0024]
[0039] The composition of a layer may be said to be "substantially homogeneous" throughout the thickness of the layer. Unless otherwise specified, "substantially homogeneous" indicates that the composition in a particular region varies by less than 10%, either in atomic ratio or dopant concentration.
[0025]
[0040] A gradient of dopant or semiconductor alloy composition may be formed throughout the thickness of the layer. The gradient may be formed in one or more ways, for example, by depositing materials with a selected material distribution, by varying conditions during deposition of the layer, or the gradient may be formed by depositing separate layers of material that are then annealed to produce the desired concentration distribution. The gradient may be a continuous increase in concentration, or a step change in concentration, etc. Such a gradient may be applied to atomic ratios in ternary or quaternary alloys where the atomic ratios vary throughout the thickness of the absorber, or the gradient may be applied to dopants in the layer. Gradients may be used to tune the band gap of CdTe-based alloys, reduce surface recombination, reduce charge carrier recombination, provide a diffusion barrier, provide a buffer, improve ohmic contacts, and / or increase solar absorption to improve power conversion efficiency.
[0026]
[0041] The power output of a PV device is the product of current (I, or sometimes J, the current density per unit area) and voltage (V), and can be shown on an I-V curve. The maximum voltage occurs at zero current, or "open circuit" (V OC ), zero voltage, or a "short circuit" results in maximum current (ISC ). These products give the total potential power (P T ), which cannot be achieved in practice. MAX ) is the maximum product I MP ×V MP The fill factor (FF) is defined by the point where P T P for MAX The ratio of I MP ×V MP The product of I SC ×V OC The conversion efficiency of a PV device is defined as the quotient of the total potential power (P T ) total incident power (P in ), and efficiency = (I SC ×V OC ×FF) / P in It can be mathematically expressed as:
[0027]
[0042] As used herein, the term "effective carrier density" refers to the average concentration of holes or electrons in a material. As used herein, an "n-type layer" refers to a semiconductor layer that has an excess of electron donors as majority carriers, while a "p-type layer" refers to a semiconductor layer that has an excess of electron acceptors (also known as "holes") as majority carriers. In either case, the excess carriers (electrons or holes) can be provided by chemically doping the semiconductor with an appropriate dopant, or can be generated by defects inherently present in the material.
[0028]
[0043] Semiconductors that are doped to be p-type or n-type are sometimes further characterized based on the density of the respective majority charge carriers. Although the boundary is not precise, typically materials have about 1×10 electron acceptor carriers (i.e., "holes") 11 cm -3 From about 1×10 16 cm -3 If the acceptor carrier density is in the range of 1×10, it is considered to be p-type. 16 cm -3Similarly, a material is considered to be p+ type if it has an electron donor carrier density of about 1×10 11 cm -3 From about 1×10 16 cm -3 In the range of 1×10, the donor carrier density is approximately 1×10. 16 cm -3 Regardless of the absolute carrier density, a layer can be p+ for a layer that is p-type (or n+ for a layer that is n-type) if the carrier concentration is at least two orders of magnitude (i.e., 100 times) higher, so the boundary is not exact and can overlap. Also, approximately 1×10 18 cm -3 charge density greater than 0.01 is sometimes considered to be of "++" type, so that a layer of either n-type or p-type can be "++" to a layer of the same type that is itself "+" to a further, third layer if the carrier density of the same type in the ++ layer is more than 100 times the carrier density of the + layer.
[0029]
[0044] In the following description, reference is made to the accompanying drawings, which form a part hereof, and which are shown by way of illustration, specific embodiments, or examples. Referring now to the drawings, in which like numerals indicate like elements throughout the several views, aspects of photovoltaic devices and manufacturing processes are described.
[0030]
[0045] 1 shows a photovoltaic device 100 according to an embodiment of the present disclosure, in which a number of layers are shown and described. The layers, materials used, and / or methods of forming the layers described for the photovoltaic device 100 may be substituted, included in addition to the layers described, or absent in the embodiments described below and illustrated in the figures. It is further understood that each layer may be deposited in a monolayer deposition from a single material, by a multilayer process from a single material, or by a multilayer process from multiple materials.
[0031]
[0046] 1 includes a substrate layer 110, a front contact layer 120, a transparent n-type layer 130, a p-type absorber layer 140, and a back contact layer 150. In some embodiments, the front contact layer 120 is also the transparent n-type layer 130. Thus, the transparent n-type layer 130 may be omitted.
[0032]
[0047] As used herein, the term "transparent layer" refers to a layer that allows for an average transmission of at least 70% for incident electromagnetic radiation having a wavelength in the range of about 300 nm to about 1,300 nm, such as about 400 nm to about 800 nm, etc. In some embodiments, a transparent layer may transmit electromagnetic radiation over a wider range of wavelengths, which may include infrared or ultraviolet wavelengths.
[0033]
[0048] In a typical embodiment, light enters from the substrate layer 110 and passes through the front contact layer 120 and the transparent n-type layer 130 until it reaches the p-type absorber layer 140 where it is absorbed, inducing the emission of charge carriers. The heterojunction between the p-type absorber layer 140 and the transparent n-type layer 130 forms a p-n junction, allowing for directional charge carrier flow. As a result, current is conducted by the front contact layer 120 and the back contact layer 150.
[0034]
[0049] The photovoltaic device 100 further includes electrical connections that provide a current path to carry the generated current, for example from one photovoltaic cell to an adjacent cell in a module, or from one photovoltaic module to an adjacent module in an array, or alternatively, the electrical connections may direct the current to an external load device that is powered by the photogenerated current.
[0035]
[0050] The substrate layer 110 provides a surface on which material layers are placed to create a photovoltaic device. The substrate layer 110 comprises any suitable substrate, such as soda-lime glass, float glass, or low-iron glass. Alternatively, the substrate layer 110 may comprise a polymeric, ceramic, metallic, or other material that provides a suitable structure to form the base of a photovoltaic cell. The substrate is not required, but is a substantial medium for coating with subsequent layers. Although the layers of a superstrate structure, in which front-side light is incident from the substrate, are generally described herein, a true "substrate" structure with a substrate on the back contact side is also suitable for use in the described method.
[0036]
[0051] In some embodiments, device 100 may further include one or more of an anti-reflective layer, an anti-soiling layer, an encapsulant, an interface layer, a buffer layer, a capping layer, and an optically reflective layer.
[0037]
[0052] FIG. 2 illustrates an exemplary method 200 of forming and treating the absorber layer 140. With joint reference to FIGS. 1 and 2, a partially formed device including a window stack 310 is provided 210 and placed in a deposition chamber. In some embodiments, the window stack 310 includes a substrate layer 110, a front contact layer 120, and a transparent n-type layer 130. In some embodiments, the window stack 310 includes a glass substrate layer 110, a transparent conductive oxide (TCO) on the substrate layer 110, and an undoped semiconductor layer on the TCO. In some embodiments, the window stack 310 includes a substrate layer, a transparent conductive oxide (TCO) adjacent to the substrate layer, a high resistivity transparent (HRT) layer adjacent to the TCO, and one or more semiconductor layers on the HRT layer.
[0038]
[0053] During the absorber deposition step 220, a II-VI type semiconductor material and a pnictogen dopant are deposited on the window stack 310 of the partially formed device to form a photovoltaic stack 300 including a doped absorber layer 340 on the window stack 310, as shown in FIG. 3. In some embodiments, the dopants are co-deposited to form a photovoltaic stack 300 having a substantially uniformly doped doped absorber layer 340. In some embodiments, the II-VI semiconductor material is deposited during the deposition step 220, and the dopant is deposited sequentially before or after the semiconductor material. The dopant then diffuses into the semiconductor layer to form a doped absorber layer 340 with a dopant gradient across the thickness of the layer. In some embodiments, the II-VI semiconductor material is CdTe. In some embodiments, the II-VI semiconductor material is CdTe alloyed with one or more of CdS, CdSe, ZnTe, and HgTe.
[0039]
[0054] Doping of a semiconductor layer, such as CdTe, can be done in several ways. For example, the dopant can be provided during deposition with a CdTe source. The dopant can be introduced as a powder (i.e., single-phase or multi-phase material) or in a carrier gas. The dopant can be introduced during, before, after, or between deposition of the semiconductor layer by depositing one or more layers. For example, adjacent layers may contain a dopant that can diffuse into the CdTe layer. In some embodiments, the semiconductor material is a chalcogenide and the dopant or dopant precursor comprises a group V element. According to some embodiments, multiple dopants are deposited during deposition step 220, at least one of which comprises a pnictogen.
[0040]
[0055] In a typical embodiment, the semiconductor material includes CdTe deposited by molecular beam epitaxy (MBE) with a pnictogen dopant. In another typical embodiment, the semiconductor material includes CdTe deposited with an arsenic dopant by thermal evaporation of CdTe with Cd2As3 or AsH3. In a typical embodiment, the semiconductor material includes a CdTe alloy deposited by vapor transport deposition (VTD) with a pnictogen dopant. In some embodiments, the semiconductor is deposited by VTD using a mixed or alloyed powder consisting essentially of cadmium, tellurium, and arsenic elements. In some embodiments, the mole fraction of the pnictogen in the feedstock is 0.05% to 5.0%. In a typical embodiment using an arsenic dopant, the concentration of arsenic in the absorber film is about 1×10 16 cm -3 From about 5 × 10 20 cm -3 In some embodiments using arsenic dopants, the concentration of arsenic in the absorber film is about 1×10 18 cm -3 From about 5 × 10 18 cm -3 In a typical embodiment using an antimony dopant, the concentration of antimony in the absorber film is about 1×10 17 cm -3 From about 2 × 10 20 cm -3In another exemplary embodiment, phosphorus dopants are incorporated by thermally evaporating the semiconductor material with cadmium phosphide (Cd3P2). In another exemplary embodiment, antimony dopants are incorporated by thermally evaporating the semiconductor material with antimony telluride (Sb2Te3), cadmium-antimony alloy, or metallic antimony. Suitable doping precursors include, but are not limited to, Cd3As2, As2Se3, AsH3, Bi2Te3, Sb2Te3, Cd3P2, Zn3P2, Bi(NO3)3, Bi2S3, PCl3, PH3, SbH3, and AsCl3, as well as elemental forms of dopants. Suitable doping precursors include alloys of the above-listed compounds with CdTe or other II-VI materials.
[0041]
[0056] A typical deposition chamber includes a deposition distributor connected to a deposition vapor source. To deposit different layers, the distributor can be connected to multiple vapor sources, or the substrate can be moved through multiple different deposition stations, each with their own vapor distributor and source.
[0042]
[0057] In an embodiment, during the dopant and absorber deposition step 220, the deposition chamber is substantially free of oxygen gas or water vapor. For example, the deposition chamber can be considered to be substantially oxygen-free. As used herein, substantially oxygen-free can mean that the partial pressure from oxygen in the chamber is less than about 1 Torr, such as less than about 500 mTorr in one embodiment, less than about 100 mTorr in another embodiment, in a range from very low pressure to about 500 mTorr in a further embodiment, or in a range from very low pressure to about 25 mTorr in yet another embodiment, etc. Similarly, the chamber can be considered to be substantially anhydrous steam. As used herein, substantially anhydrous steam can mean that the partial pressure from water vapor in the deposition chamber is less than about 1 Torr, such as less than about 500 mTorr in one embodiment, less than about 250 mTorr in another embodiment, or less than about 100 mTorr in a further embodiment. As used herein, "very low pressure" refers to a pressure that is somewhat above zero, such as less than about 10 mTorr, which was the detection limit of the equipment used for testing. -4 Pa (approx. 10 -6 In a further embodiment, the deposition conditions further include providing a chemical reducing agent to the deposition chamber during the dopant and absorber deposition step 220. The dopant and absorber deposition step 220 results in the photovoltaic stack 300.
[0043]
[0058] During the processing step 240, the photovoltaic stack 300 is thermally treated, contacted with a passivation agent, and provided with a reducing agent. The reducing agent can be oxidized more energetically favorably than the group V dopant. That is, the Gibbs free energy change (ΔG) of the oxidation reaction of the reducing agent in the chamber is more negative than that of the group V dopant. The photovoltaic stack 300 is maintained in a reducing environment at high temperature. In some embodiments, the processing step 240 further includes low pressure conditions.
[0044]
[0059] A passivation agent is provided in process step 240. In some embodiments, the passivation agent is CdCl2. Other suitable passivation agents include MnCl2, MgCl2, NH4Cl, ZnCl2, or TeCl4. The passivation agents may be used alone or in combination. In some embodiments, the photovoltaic stack 300 is contacted with the passivation agent in a reducing environment at elevated temperature. In other embodiments, the photovoltaic stack 300 is placed in a reducing environment at elevated temperature after contacting with the passivation agent.
[0045]
[0060] In some embodiments, the reducing agent is or includes H2. In some embodiments, the reducing agent is provided as a component of a forming gas consisting essentially of a mixture of a reducing agent and an inert gas, such as a mixture of H2 and N2. Other suitable reducing agents include methane (CH4), carbon monoxide (CO), hydrogen sulfide (H2S), and ammonia compounds (NH3). In an embodiment, the processing step includes providing an environment having a mixture of about 50.0% to about 99.4% N2 and about 0.6% to about 3.0% H2. In an embodiment, the processing step includes providing a gas to the chamber to create an environment including H2. As defined herein, the chamber may be substantially oxygen-free. Alternatively, or in addition, the chamber may be substantially anhydrous steam. In an embodiment, the processing step includes providing a gas to the chamber to create an environment consisting essentially of 100% H2. In an embodiment, the treatment step includes providing an environment containing an atomic fraction of H2 in the range of about 0.5% to about 100%, such as in one embodiment about 0.06% to about 3.0% H2, or in another embodiment about 0.6% to about 3.0% H2. In an embodiment, the process step includes supplying hydrogen gas to the chamber, where the partial pressure of H2 in the chamber ranges from about 0.24 torr to about 50 torr, such as from about 3 torr to about 50 torr in one embodiment, from about 2.4 torr to about 12 torr in another embodiment, from about 4.2 torr to about 21 torr in a further embodiment, or from about 3 torr to about 15 torr in yet another embodiment. As mentioned above, the chamber can be substantially free of oxygen vapor. Thus, the partial pressure ratio of the reducing agent to oxygen in the chamber can be greater than about 0.24, such as greater than about 3 in one embodiment, greater than about 100 in another embodiment, or greater than about 1,000 in a further embodiment.
[0046]
[0061] In some embodiments, the elevated temperature is a temperature greater than about 300° C., greater than about 350° C., greater than about 400° C., less than about 800° C., less than about 600° C., less than about 550° C., or less than about 500° C. The photovoltaic stack or stacks may be thermally processed for a suitable period of time, including, for example, greater than about 5 minutes, greater than about 15 minutes, greater than about 20 minutes, greater than about 30 minutes, greater than about 30 minutes, less than about 90 minutes, less than about 60 minutes, or less than about 40 minutes.
[0047]
[0062] Without wishing to be bound by theory, it is suggested that the heating step performed in the reducing environment creates Te vacancies and promotes the migration of group V dopants to the Te vacancy sites. In some embodiments, the temperature and pressure of the reducing environment are sufficient to induce or promote a reaction between hydrogen gas in the reducing environment and the semiconductor layer containing the CdTe alloy to form hydrogen telluride (H2Te). In some embodiments, the temperature and pressure selected are below the phase transition temperature of the absorber film.
[0048]
[0063] In the treatment step 240, the anions of the II-VI semiconductor compound react with H2, or other reducing agent, and / or with a passivation agent such as CdCl2, depleting the chalcogen elements from the layer and forming volatile species such as TeCl2 and H2Te. This promotes further activation of the incorporated dopants during recrystallization after chalcogen vacancies are formed. For example, in CdTe, the group V dopant occupies Te vacancies formed in the polycrystalline lattice through the reaction between H2-Te forming volatile H2Te. Further examples include the reaction of H2 with compounds such as ZnTe, CdS, or CdSe. Without wishing to be bound by theory, it is believed that the passivation and heat treatment in a reducing environment causes the Te vacancies (V Te ) and Cd enrichment, the incorporation of group V element dopants into Te vacancies in the crystal lattice (e.g., Bi Te , Sb Te , As Te , P Te), resulting in enhanced dopant activation. This step also achieves passivation of grain boundaries and defects through chlorination.
[0049]
[0064] In an exemplary embodiment of the processing step 240, the photovoltaic stack with the doped CdTe absorber layer 340 was coated with a thin layer of CdCl2 by the CSS system to produce a CdCl2 coating over the absorber layer 340. As described in U.S. Pat. No. 9,318,642, which is incorporated herein by reference, CdCl2 can also be delivered as a vapor during the heat treatment, which delivery can be performed with the addition of a reducing agent. The CdCl2 layer can also be delivered by, for example, spin coating, spraying, or roll coating. The photovoltaic stack with the CdCl2 coating over the absorber layer 340 was then thermally processed in a reducing environment with a mixture of N2 and H2 for about 10 to 20 minutes. The total gas pressure was about 300 torr to about 600 torr, with the H2 partial pressure being about 3 torr to about 50 torr. The temperature of the substrate 110 during the process step 240, including the anneal, ranged from about 375° C. to about 475° C.
[0050]
[0065] In another exemplary embodiment of processing step 240, the photovoltaic stack 300 is held in a heat treatment environment at a pressure ranging from about 200 Torr to about 800 Torr, a temperature ranging from about 350° C. to about 500° C., and a reducing environment with a hydrogen partial pressure ranging from about 3 Torr to about 50 Torr for about 5 minutes to about 45 minutes. In a further exemplary embodiment of processing step 240, the photovoltaic stack is held in a chamber at a temperature ranging from about 400° C. to about 500° C. for a period of about 5 minutes to about 30 minutes, and a reducing environment consisting of nitrogen gas, hydrogen gas, and cadmium chloride vapor is supplied to the chamber. The chamber can be substantially oxygen-free.
[0051]
[0066] Turning now to FIG. 4, an example of a method 400 for forming a device having a doped absorber layer 340 is shown.
[0067] A window stack 310 is formed 410. During a deposition step 420, II-VI semiconductors and dopants are deposited on the window stack 310 to form the photovoltaic stack 300.
[0052]
[0068] During the preconditioning step 430, the photovoltaic stack 300 is heated and annealed in a substantially oxygen-free environment. In some embodiments, the preconditioning step 430 is performed under vacuum or at low pressure. In some embodiments, the preconditioning step 430 is performed at or below atmospheric pressure, such as about 760 Torr. In some embodiments, the preconditioning step 430 is performed in a vacuum environment at a pressure of about 0.13 Pa (about 0.1 milliTorr) or less. In some embodiments, the pressure of the vacuum environment is about 1×10 -4 Torr) to approximately 1.3 × 10 -6 Pa (approx. 1×10 -9 Torr), etc., about 1.3 Pa (about 1 x 10 -2 Torr) to approximately 1.3 × 10 -6 Pa (approx. 1×10 -9 In other embodiments, the pretreatment step 430 is performed in a low pressure environment at a pressure of about 550 Torr or less. In some embodiments, the pressure of the low pressure environment is in the range of about 25 Torr to about 550 Torr. In an exemplary embodiment, the photovoltaic stack 300 is annealed under vacuum at a temperature in the range of about 300° C. to about 500° C. (e.g., in the range of about 300° C. to about 450° C.) for a period of time in the range of about 10 minutes to about 60 minutes.
[0053]
[0069] Without wishing to be bound by theory, it is suggested that pretreatment of the doped absorber layer 340 at reduced pressure and elevated temperature reduces defects, produces a more chemically uniform absorber film, promotes grain growth, contributes to the restoration of stoichiometry, and promotes dopant incorporation throughout the II-VI semiconductor layer. The pretreatment step is particularly beneficial for absorber layers deposited at temperatures below about 300° C. and at low pressures, such as conditions used in physical vapor deposition (PVD) techniques.
[0054]
[0070] During processing step 440, the photovoltaic stack 300 is contacted with a passivation agent and maintained in a reducing environment at elevated temperature, as illustrated in the process shown in FIG.
[0071] The photovoltaic stack is maintained in a heated and oxygenated environment during processing step 450. In an exemplary embodiment, the photovoltaic stack is maintained in air at a temperature ranging from about 150° C. to about 200° C., at or near ambient pressure, for a period of about 30 minutes to about 120 minutes.
[0055]
[0072] A back contact material is formed on or coated onto the photovoltaic stack during the back contact formation step 460. Suitable back contact materials include, but are not limited to, alloys, metal stacks, conductive oxides, and graphite compounds.
[0056]
[0073] 4 results in an embodiment of a photovoltaic device having a doped absorber layer 340 in which the dopant is incorporated into the crystal lattice of a polycrystalline semiconductor material. In one embodiment, the concentration of Group V dopant in the doped semiconductor absorber layer 340 is about 5×10 16 cm -3 From about 2 × 10 18 cm -3 (e.g., about 5 × 10 17 cm -3 From about 1×10 18 cm -3), and the treated doped semiconductor absorber layer 340 has a p-type charge carrier concentration of about 5×10 15 cm -3 From about 5 × 10 17 cm -3 range (e.g., about 5×10 15 cm -3 From about 5 × 10 16 cm -3 ). Thus, the apparent activation fraction of the group V dopant is from about 0.25 at% to about 10 at% (e.g., from about 1 at% to about 5 at%) of the group V dopant in absorber layer 340. In one embodiment, The concentration of Group V dopant in the processed doped semiconductor absorber layer 340 is about 1×10 14 cm -3 From about 1×10 18 cm -3 and about 0.5 at% to about 5.0 at% of the Group V dopant occupies Te vacancies in the CdTe crystal lattice. In certain embodiments, the activation level of the dopant is about 1% to about 10%, and wherein after heating the absorber film in a reducing environment, about 1 at% to about 10 at% of the Group V dopant in the absorber layer occupies Group VI type vacancies in the II-VI semiconductor polycrystalline lattice. In certain embodiments, the activation level of the Group V dopant is about 2% or more.
[0057]
[0074] In some embodiments, the window stack preparation step 410 includes forming a window layer as described in U.S. Pat. No. 9,082,903. In some embodiments, the window stack preparation step 410 further includes depositing one or more semiconductor layers on the TCO layer. For example, the window stack preparation step 410 further includes depositing a CdS layer and / or a CdSe layer, followed by an optional undoped CdTe layer on the CdS or CdSe layer. In some embodiments, the absorber and dopant deposition step 420 is performed by a high temperature process (about 350° C. to 1,200° C.) without a pretreatment step, resulting in a photovoltaic device having a doped absorber layer with dopants incorporated into the crystal lattice of the polycrystalline semiconductor material. In an exemplary embodiment, the prepare window stack step 410 is followed by an absorber and dopant deposition step 420 for a pnictogen dopant with deposition of CdTe by VTD at a temperature of about 450° C. to about 600° C. deposited on the semiconductor layers of the window stack 310 to form the photovoltaic stack 300. The photovoltaic stack is then treated in a defect passivation and dopant activation step 440. In the defect passivation and dopant activation step 440, the photovoltaic stack 300 is treated with heat, CdCl2, and H2 in a substantially oxygen-free reducing environment. Exemplary conditions include a hydrogen partial pressure of about 3 torr to about 20 torr, a total pressure of about 250 torr to about 760 torr, a temperature of about 350° C. to about 475° C., and a total duration of about 5 minutes to about 90 minutes.
[0058]
[0075] During processing step 440, the defects are passivated and the pnictogen dopant is activated, whereby the pnictogen dopant atoms occupy tellurium sites in the crystal lattice. Processing of the photovoltaic stack 300 by processing step 440 may result in an absorber layer 340 having a thickness of about 0.5 microns to about 3.5 microns, such as between about 1 micron and about 3 microns in one embodiment, about 1.0 micron in another embodiment, or about 3.0 microns in a further embodiment.
[0059]
[0076] During the processing step 440, or in a separate annealing step, the absorber layer 340 may be annealed with the adjacent semiconductor layers on the back side of the window stack 310 to form an absorber layer 340 having a graded composition, for example an absorber layer 340 including an alloy of cadmium, tellurium, and selenium or sulfur. The processing step may consume substantially all of the adjacent semiconductor layers (e.g., CdS and / or CdSe layers) or a portion of the adjacent semiconductor layers, such as the CdS and / or CdSe layers, may remain between the TCO layer of the window stack and the doped CdSeTe / CdTe absorber layer 340. Similarly, the processing step may cause substantially all of the adjacent semiconductor layers on the back side of the window stack 310 to intermix with the doped CdTe layer or a portion of the CdTe layer may remain substantially free of selenium or sulfur adjacent to the back contact.
[0060]
[0077] Following the defect passivation and dopant activation process step 440, the absorber surface is cleaned and a back contact is formed 460. In some embodiments, the back contact is The contacts may include ZnTe and may be formed as described in U.S. Patent Application Publication No. 2014 / 0261667.
[0061]
[0078] In some embodiments, the photovoltaic stack 300 is processed through selected steps. In some embodiments, some steps are combined or omitted. In a typical embodiment, the partially formed device is grown sequentially only through an absorber deposition step 420, in which chalcogenides and dopants are deposited to form the photovoltaic stack 300, a pretreatment step 430, in which the photovoltaic stack is annealed in a substantially oxygen-free, low pressure environment, and a treatment step 440, in which the photovoltaic stack 300 is passivated and heat treated in a reducing environment. In another typical embodiment, the partially formed device is grown sequentially from an absorber deposition step 420, in which chalcogenides and dopants are deposited to form the photovoltaic stack 300, to a treatment step 440, in which the photovoltaic stack 300 is passivated and heat treated in a reducing environment, resulting in dopant activation.
[0062]
[0079] In some embodiments, the photovoltaic stack 300 is processed sequentially through all of the steps 420, 440, and 460. In some embodiments, the photovoltaic stack 300 is processed sequentially through all of the steps 410, 420, 430, 440, 450, and 460. In some embodiments, the processing steps are performed sequentially and quickly, with substantially no intervening time between the steps. In some embodiments, the processing steps are not performed quickly. In some embodiments, the steps are repeated. In some embodiments, one or more intervening steps are performed, such as a cooling step, a cleaning step, a chemical rinse, a passivation step, an additional annealing step, an additional dopant deposition, and / or deposition of an intervening layer, such as a buffer layer, an electron reflecting layer, or an optical reflecting layer. In some embodiments, one or more additional layers are coated on the absorber layer 340 of the photovoltaic stack 300 before the back contact formation. EXAMPLES
[0063]
[0080] CdTe:As sample Samples were prepared by depositing a transparent conductive oxide (TCO), e.g., fluorine-doped tin oxide, on a glass substrate, followed by deposition of a window layer on the TCO to form a series of window stack sections. A cadmium telluride (CdTe) layer was then deposited on the window layer. CdTe deposition and processing steps were performed as described further below: with and without arsenic dopant; with and without a post-deposition pretreatment vacuum anneal step; and with an activation heat treatment with CdCl2 in a reducing or inert environment.
[0064]
[0081] In one series of samples, a layer of arsenic-doped cadmium telluride was deposited on the window layer of the window stack. The arsenic-doped cadmium telluride (CdTe:As) layer had a doping density of approximately 1×10 18 cm -3 The arsenic doping concentration was substantially uniform.
[0065]
[0082] The resulting series of photovoltaic stacks were then subjected to a vacuum annealing pretreatment step at about 300° C. to about 420° C. for about 20 minutes to about 60 minutes.
[0083] The pretreated parts were then subjected to a CdCl2 heat treatment in a reducing or inert atmosphere at about 350°C to about 500°C for about 5 minutes to about 40 minutes. The absorber surface was covered by evaporation with about 1 μm of CdCl2. During the heat treatment, the pressure was maintained at a total pressure ranging from about 400 torr to about 800 torr. The reducing environment consisted essentially of nitrogen and hydrogen. That is, the reducing environment was substantially oxygen-free and substantially anhydrous steam. The inert gas of the reducing environment consisted essentially of nitrogen. A series of parts were treated at selected forming gas concentrations in various reducing environments supplied with an inert gas consisting of nitrogen. The forming gases used were 3% H2 and 97% N2. Thus, the forming gas was diluted with an inert gas and the tests described herein were performed.
[0066]
[0084] The sample was then placed in an air environment at normal pressure and about 170° C. for about 1 hour, after which it was covered with a metallic back contact.
[0085] CdTe:As / CdSe sample The samples were prepared by depositing a TCO on a glass substrate, followed by depositing an oxide window layer on the TCO, followed by depositing a cadmium selenide (CdSe) layer to form a series of window stack sections. A cadmium telluride (CdTe) layer with an arsenic dopant was then deposited on the CdSe layer to form a series of photovoltaic stacks with arsenic-doped absorber layers. Samples deposited below about 350°C were subjected to a vacuum anneal pretreatment, while samples deposited at the high temperature process were not pretreated. The photovoltaic stacks were then subjected to an activation treatment with a CdCl2 heat treatment in a selected reducing environment formed with forming gas and an inert control. CdCl2 can be coated as a liquid, powder, or vapor immediately before or during the heat treatment with the reducing agent. The absorber surface of the sample was contacted with CdCl2 vapor in a reducing environment at a temperature ranging from about 350°C to about 450°C and a total pressure of about 400 torr to about 700 torr for a period of between about 10 minutes and about 180 minutes in an environment supplying a reducing agent. The reducing agent used in this series of samples was provided by forming gas. The forming gas contained about 3% hydrogen and about 97% nitrogen. The reducing agent was provided at a selected concentration, with nitrogen making up the balance of the gas supplied to the reducing environment. The inert control contained 100% nitrogen. The total pressure can be provided by optionally diluting the forming gas with any amount of inert control. Thus, in the embodiment tested, the maximum partial pressure of the reducing agent (i.e., H2) was between about 1,600 Pa (about 12 Torr) and about 2,800 Pa (about 21 Torr), and the minimum partial pressure of the inert gas (nitrogen) was between about 51,729 Pa (about 388 Torr) and about 90,526 Pa (about 679 Torr). The sample was then covered with a back contact.
[0067]
[0086] CdTe:Sb sample A series of antimony-doped samples were prepared by depositing 1-5 μm layers of cadmium telluride (CdTe) with antimony dopant onto the window layer of a partially formed device to form a series of photovoltaic stacks. The photovoltaic stacks were then subjected to an activation treatment using a CdCl2 heat treatment in a reducing environment with about 100% forming gas, at a pressure of about 400 torr to about 600 torr, and at a temperature of about 400 °C to about 500 °C.
[0068]
[0087] CdTe:P sample A series of phosphorus-doped samples were prepared by depositing 1-5 μm layers of cadmium telluride (CdTe) with phosphorus dopant onto the window stack to form a series of photovoltaic stacks, which were then subjected to activation by a CdCl2 heat treatment in a reducing environment with about 100% forming gas, at a pressure of about 400 torr to about 600 torr, and at a temperature of about 400 °C to about 500 °C.
[0069]
[0088] result As shown in the figures and evaluated by the experimental results, the vacuum anneal pretreatment promoted stoichiometric re-equilibration of Cd and Te, defect amelioration, and substantially uniform As dopant incorporation throughout the absorber layer. Passivation of the defects, increase in carrier concentration, reduction of the depletion width, and V Te Through this processing step, the dopants were activated and the device efficiency improved.
[0070]
[0089] FIG. 5 shows the Raman spectrum of a CdTe absorber film where the absorber and arsenic dopant were co-deposited at temperatures ranging from about 200° C. to about 250° C. FIG. 5 compares a control film (corresponding to curve 160) and an effective film (corresponding to curve 162). A post-deposition vacuum heat pretreatment was performed on the control and effective films at temperatures ranging from about 300° C. to about 420° C. for periods ranging from about 20 minutes to about 60 minutes. The control film shows a very strong Te phase present in the film, indicating a Te-rich layer. A vacuum anneal at about 300° C. to about 420° C. for about 20 minutes to about 60 minutes promotes stoichiometric re-equilibration and eliminates the Te peak. Similar results were found in films doped during the deposition step with either AsH3 or Cd3As2.
[0071]
[0090] Arsenic-doped CdTe devices prepared at deposition temperatures between about 200°C and about 250°C were compared with and without pretreatment to evaluate the dopant concentration and distribution throughout the absorber layer. The controls showed a spike of As dopant at the front interface of the absorber film at or adjacent to the TCO, with reduced dopant concentration and an average concentration an order of magnitude lower than the spike throughout the absorber. The dopant distribution of stacks that underwent a post-deposition vacuum anneal pretreatment was more uniform and homogeneous throughout the absorber, with a narrower dopant concentration range and higher average concentration levels.
[0072]
[0091] 6 shows plots of normalized photoluminescence (PL) intensity values comparing the distribution and intensity of PL wavelengths for untreated (corresponding to curve 164) and treated arsenic doped CdTe devices annealed in vacuum at about 300° C. to about 420° C. for about 20 minutes to about 60 minutes (corresponding to curve 166). The higher intensity values, and peak shaped PL curves indicate that the treated devices have fewer defects than the control.
[0073]
[0092] FIG. 7 shows normalized quantum efficiency (QE) versus wavelength for arsenic doped CdTe devices. The QE measurements compare devices that were subjected to vacuum pretreatment (corresponding to curve 168) with a control (corresponding to curve 170) as described above. Both the control and pretreated devices were subjected to an equivalent activation treatment using CdCl2 in a reducing environment containing hydrogen and nitrogen gas at temperatures ranging from about 400° C. to about 500° C. for periods ranging from about 5 minutes to about 45 minutes. By comparing the QE measurements of the vacuum heat pretreated device (curve 168) with the control (curve 170), the measurements show that the overall QE of the treated device is improved by the pretreatment. The V of a typical device prepared using a vacuum pretreatment followed by an activation treatment is OC The measurement result was approximately 740mV.
[0074]
[0093] FIG. 8 shows CV curves illustrating charge carrier concentration and phase angle versus depth for an arsenic doped CdTe element. The phase angle measures the phase difference between the voltage applied to an impedance and the current passing through it, and gives an indication as to whether the element is "leaky" or prone to charge carrier recombination. Measurements are shown for an arsenic doped element with vacuum heat pretreatment (corresponding to curve 172) and an arsenic doped element without vacuum heat pretreatment (corresponding to curve 174). In comparing the measurements, the pretreated element (curve 172) shows better performance characteristics compared to the arsenic doped control without pretreatment (curve 174). The treated elements have an average p-type doping of 2×10 15 cm -3 The graph shows that the device not treated by vacuum anneal has a lower measured phase angle, indicating that the device is prone to leakage and high recombination rates.
[0075]
[0094] The results show that arsenic doped absorber layers deposited by thermal evaporation at temperatures ranging from about 200° C. to about 250° C., followed by a pre-VCHT vacuum anneal (pre-VCHT VA) and activation treatment in a reducing environment, lead to devices with fewer defects, less recombination, and longer mobile charge carrier lifetimes. As measured, vacuum heat treatment of the doped devices generally increases the efficiency and V OC increased current density, increased short circuit current density, improved fill factor, decreased resistance, decreased shunt current, and improved performance.
[0076]
[0095] FIG. 9 shows the depth distribution of elemental concentrations for an example of an arsenic doped CdTe alloy after a CdCl2 activation treatment in a reducing environment. The depth distribution for As176, Te (raw ion count)178, and Sn180 was measured by dynamic secondary ion mass spectrometry (DSIMS). The absorber layer is shown extending from the zero depth point on the left side of the graph to a depth of about 2 μm. After the CdCl2 heat treatment, the device shows good dopant distribution throughout the absorber, and high dopant concentration levels.
[0077]
[0096] FIG. 10 shows the CV curves of charge carrier concentration versus depth for an arsenic doped sample that was subjected to a vacuum anneal pretreatment followed by treatment with CdCl2 and heat in a selected reducing environment as described above. The selected reducing environments included 100% forming gas (curve 182), 20% forming gas (curve 184), 2% forming gas (curve 186), and 0% forming gas as a control (curve 188). Nitrogen gas (N2) made up the balance of the environment. The total pressure was about 500 Torr. Thus, for example, an environment into which 100% forming gas is provided would consist essentially of a mixture of hydrogen and nitrogen gases with about 3% hydrogen (partial pressure about 2,000 Pa (about 15 Torr)) and about 97% nitrogen (partial pressure about 64,661 Pa (about 485 Torr)), and an environment into which 20% forming gas is provided would consist essentially of a mixture of hydrogen and nitrogen gases with about 0.6% hydrogen (partial pressure about 400 Pa (about 3 Torr)) and about 99.4% nitrogen (partial pressure about 66,261 Pa (about 485 Torr)). The environment provided with 2% forming gas consisted essentially of a mixture of hydrogen gas and nitrogen gas with a partial pressure of about 0.06% hydrogen (about 0.3 Torr) and about 99.94% nitrogen (about 499.7 Torr), and the control environment provided with 0% forming gas consisted essentially of nitrogen. Curve 182 at a distance of about 0.1-0.4 μm from the junction corresponds to a 100% forming gas process. Curve 184 at a distance of about 0.5-1.2 μm from the junction corresponds to a 20% forming gas process. Curve 186 at a distance of about 1.4-2.2 μm from the junction corresponds to a 2% forming gas process. Curve 188, at a distance of about 2.8-3.0 μm from the junction, corresponds to the control with 0% forming gas. As shown, with increasing H2 concentration in the process step, the carrier concentration increases and the void width decreases. The control is essentially depleted.
[0078]
[0097] Figure 11 shows the V of the arsenic-doped element after CdCl2 heat treatment. OCA comparison of the measured results is shown. Data point 190 shows the V OC The measured results are shown in data point 192, which shows the higher V OC The results are shown below. The samples treated by CdCl2 heat treatment in a reducing environment showed higher V OC It shows well.
[0079]
[0098] 12 shows the current-voltage (IV) curves for a control arsenic doped device, curve 194, and a treated arsenic doped device, curve 196. The treated device was activated in a selected reducing environment having about 100% forming gas, as previously described for this sample.
[0080]
[0099] 13A-13C show measurements of the processed arsenic doped device. FIG. 13A shows the DSIMS distribution of arsenic dopants in the processed device. FIG. 13B shows the CV measurement of the charge carrier concentration. FIG. 13C shows the measured V OC 2 shows IV curves (dark curve 250, and light curve 252) for an arsenic doped device with a Vref of 883 mV.
[0081]
[0100] The p-type or n-type nature of a semiconductor can be determined by measuring both CV and QE. Once the p-type properties have been defined, the p-type charge carrier concentration can be determined using the DSIMS data which indicates the concentration level. For a single element, the ratio between the CV apparent doping amount and the DSIMS concentration indicates the fraction of active dopant. For example, FIG. 13A shows that the p-type charge carrier concentration is approximately 2×10 18 / cm 3 Figure 13B shows a DSIMS concentration of about 4.5 x 10 16 / cm 3 The device shows a p-type doped carrier concentration of 1000 Å. Therefore, an activation of about 2% is shown. The device shows high doping levels, good depth distribution, chemical incorporation of the dopants, and high V OC Shows.
[0082]
[0101] 14A-14C show the measurement results of the processed arsenic doped device. FIG. 14A shows the QE measurement results. FIG. 14B shows the measured V OC 14C shows the IV curves (thick curve 250 and light curve 252) for a device with a IF of 806 mV and a FF of 78.3%. FIG. 14C shows the CV measurements of the charge carrier concentration. It was observed that the quantum efficiency at shorter wavelengths of about 400 nm to about 600 nm was improved from about 15% to about 25% by treatment with forming gas.
[0083]
[0102] Compared to many other dopants, arsenic has a low sticking coefficient. Activation is of increased importance as the overall dopant incorporation may be reduced. Embodiments of devices fabricated using the described methods include dopant levels of parts per million in the absorber layer. In some embodiments, arsenic at a mole fraction of 1% mixed with the CdTe starting powder results in an atomic fraction of about 0.01% throughout the absorber, or 1.5×10 per cubic centimeter. 18 In some embodiments, the doped semiconductor absorber layer has a p-type charge carrier concentration of about 1×10 15 cm -3 From 8×10 16 cm -3 In some embodiments, the p-type charge carrier concentration of the doped semiconductor absorber layer is in the range of about 1×10 16 cm -3 From 6×10 16 cm -3 The range is.
[0084]
[0103] Experiments were carried out by varying the concentration of arsenic dopant. An embodiment having about 2.4×10 arsenic can be obtained using the described method. 16 cm -3 As shown in the example results in Table 1, activation levels of about 3% to about 5% can be achieved over a wide range of doping concentrations.
[0085] [Table 1]
[0086]
[0105] Figure 15 shows the results for the CdCl2 heat treatment carried out in a 100% forming gas environment. 1 shows capacitance-voltage measurements plotting charge carrier concentration versus depth for an antimony doped sample after activation treatment with .
[0087]
[0106] FIG. 16 shows that in a reducing environment with about 100% forming gas, 1 shows capacitance-voltage measurements plotting charge carrier concentration versus depth for phosphorus-doped CdTe absorbers after activation treatment with a CdCl heat treatment performed at pressures from about 29 Pa (about 400 Torr) to about 79,993 Pa (about 600 Torr) and temperatures from about 400 °C to about 500 °C.
[0088]
[0107] Dopant composition and levels are varied to incorporate additional semiconductor compounds into the stack. A series of representative devices were further prepared by varying the deposition conditions, pretreatment parameters, and processing parameters. The data collected is consistent with the results obtained from the examples given.
[0089]
[0108] As shown in the examples and control samples, conventional deposition in air or N2 Post-deposition passivation cannot be used to activate polycrystalline CdTe absorber films that have been incorporated with Group V dopants.
[0090]
[0109] Method for activating group V dopants in polycrystalline II-VI semiconductor absorber layers Exemplary method steps include providing an absorber film doped with a Group V dopant; optionally subjecting the absorber film to a first heat treatment in a first heat treatment environment, which comprises a substantially oxygen-free atmosphere and may be low pressure or vacuum; contacting a surface or a portion of the absorber film with a halogen or a passivating agent; and subjecting the absorber film to a second heat treatment in a second heat treatment environment; providing a reducing agent, such as hydrogen gas, in the second heat treatment environment to form a reducing environment; thereby activating the dopant in the absorber film, whereby the activated dopant occupies a Group VI type vacancy in the II-VI semiconductor crystal lattice.
[0091]
[0110] As described herein, in a cadmium telluride polycrystalline absorber layer, as well as in a cerium oxide polycrystalline absorber layer, A disclosed method has been shown for activating group V dopants in polycrystalline absorber layers of cadmium telluride alloys with materials containing arsenic and zinc. The method improves lifetime and device performance. Suitable methods include post-deposition annealing. Stoichiometric adjustment, dopant distribution, and defect reduction are achieved by a pre-treatment annealing step performed under vacuum or in a substantially oxygen-free environment. Dopant activation, grain growth, and defect passivation are achieved by treating the semiconductor stack with cadmium chloride, or other passivation agent, and heating the stack while supplying a reducing gas.
[0092]
[0111] In some embodiments, the methods, devices, and / or structures are The present invention provides the following: forming an absorber layer; incorporating dopants into chalcogenide vacancies in a polycrystalline semiconductor lattice; forming Te vacancies; activating group V dopants to increase charge carrier mobility and density; repairing defects in the crystalline grain structure; reducing shunting, reducing carrier recombination; optionally grading the semiconductor layer composition to optimize the structure and reduce interface recombination; producing highly doped materials grown on a superstrate or substrate and processed in situ to form one or more doped absorber layers; reducing electron and hole recombination; and providing a cost-effective photovoltaic structure. In an embodiment, the described features allow for control of light absorption and charge carrier flow in the device to optimize performance. The disclosed method and structure provide a short circuit current (J SC ), open circuit voltage (V OC It is possible to provide a photovoltaic device having improved surface roughness (SQ) and fill factor (FF).
[0093]
[0112] According to embodiments provided herein, a method for treating a photovoltaic semiconductor absorber layer includes the steps of: The method may include providing a reducing agent to create a reducing environment. The method may include contacting at least a portion of the absorber layer with a passivating agent while subjecting the absorber layer to a reducing environment. The absorber layer may be doped with a Group V dopant. The absorber layer may include cadmium and tellurium. The method may include heating the absorber layer in the reducing environment at a selected temperature and a selected pressure for a selected treatment period.
[0094]
[0113] According to embodiments provided herein, the photovoltaic device may include an absorber layer. The absorber layer can include cadmium, selenium, and tellurium, and a Group V dopant. The concentration of the Group V dopant in the absorber layer is about 1×10 through the thickness of the absorber layer. 16 cm -3 From about 5 × 1020 cm -3 Between 1 at% and 10 at% of the group V dopant can be activated. A portion of the active group V dopant can occupy Te vacancies in the CdTe crystal lattice.
[0095]
[0114] The principles and implementation aspects of the embodiments of the present disclosure have been illustrated and described with examples. However, the embodiments described herein may be implemented in ways other than as specifically illustrated and described without departing from the scope of the present disclosure. Although exemplary embodiments are presented, it should be understood that many variations exist. It should also be understood that the exemplary embodiment or exemplary embodiments are merely examples and are in no way intended to limit the scope, applicability, or configuration of the present disclosure. Rather, the detailed description provides a guide for those skilled in the art to implement the exemplary embodiments of the present disclosure. It should be understood that various changes may be made in the function and arrangement of elements described in the exemplary embodiments without departing from the scope of the present disclosure as set forth in the appended claims. [Mode of the invention] [1] 1. A method for treating a photovoltaic semiconductor absorber layer, comprising the steps of: providing a reducing agent to create a reducing environment; contacting at least a portion of the absorber layer with a passivation agent while subjecting the absorber layer to the reducing environment, the absorber layer being doped with a Group V dopant and the absorber layer being doped with a Group V dopant; The absorber layer comprises cadmium and tellurium, and in said reducing environment, at a selected temperature, and at a selected pressure, for a selected treatment period; Heating the absorber layer. The method includes: [2] 10. The method of claim 1, wherein the reducing agent comprises H2, hydrogen sulfide, methane, carbon monoxide, ammonia compounds, or combinations thereof. [3] 3. The method of claim 2, wherein the reducing agent comprises H2. [4] 4. The method of claim 3, wherein H2 is provided at a partial pressure of at least 32 Pa (0.24 Torr). [5] 3. The method of claim 2, wherein the reducing environment comprises at least a trace amount of oxygen, and the ratio of the partial pressure of the reducing agent to the partial pressure of the oxygen is at least 3. [6] 3. The method of claim 2, wherein the reducing agent is provided at a partial pressure in the range of 400 Pa (3 Torr) to 6,666 Pa (50 Torr). [7] The method of claim 1 , wherein the reducing environment is substantially free of oxygen. [8] The method of claim 1 , wherein the reducing environment is formed predominantly of an inert gas. [9] The method of claim 8 , wherein the inert agent comprises N2.
[10] 2. The method of claim 1, wherein the passivation agent comprises CdCl2.
[11] The method of claim 1 , wherein the absorber layer comprises selenium.
[12] The method of claim 11 , wherein the Group V dopant comprises arsenic.
[13] 10. The method of claim 1, wherein the selected temperature is in the range of 350 to 500, the selected pressure is in the range of 200 torr to 800 torr, and the selected treatment duration is in the range of 5 minutes to 45 minutes.
[14] The absorber layer has a thickness of 1×10 16 cm -3 From 5×10 20 cm -3 %. and heating the absorber layer in the reducing environment activates between 1 at. % and 10 at. % of the Group V dopant.
[15] and vacuum annealing the absorber film before the absorber layer contacts the passivation agent, the vacuum annealing step being performed at a pressure of 1.3×10 -7 Pa(1×10 -9 Torr) to 1.3 Pa (1 x 10 -2 2. The method of claim 1, wherein the absorber film is exposed to a vacuum in the range of 300 to 500 Torr and a temperature in the range of 10 to 60 minutes. How to.
[16] 2. The method of claim 1, wherein the passivation agent comprises one or more of MnCl2, MgCl2, NH4Cl, ZnCl2, and TeCl4.
[17] The method of claim 1 , wherein the Group V dopant is selected from bismuth, antimony, arsenic, phosphorus, nitrogen, and combinations thereof.
[18] 1. A photovoltaic device comprising an absorber layer having a thickness of about 0.5 μm to 3.5 μm and comprising cadmium, selenium, and tellurium and comprising a Group V dopant, The concentration of the Group V dopant in the absorber layer is about 1×10 through the thickness of the absorber layer. 16 cm -3 From about 5 × 10 20 cm -3 Between A photovoltaic device in which 1 at % to 10 at % of said Group V dopant is active.
[19] 20. The photovoltaic device of claim 18 including a back contact overlying the absorber layer, the back contact comprising nitrogen-doped ZnTe.
[20] 20. The photovoltaic device of claim 18 or 19, wherein the Group V dopant comprises antimony. [twenty one] 20. The photovoltaic device of claim 18 or 19, wherein the Group V dopant comprises phosphorus. [twenty two] 20. The photovoltaic device of claim 18 or 19, wherein the Group V dopant comprises arsenic. [twenty three] 5. The method according to claim 2, wherein the reducing environment comprises at least trace amounts of oxygen and the ratio of the partial pressure of the reducing agent to the partial pressure of the oxygen is at least 3. [twenty four] 24. The method of any one of claims 2 to 4 or 23, wherein the partial pressure of the reducing agent is in the range of 400 Pa (3 Torr) to 6,666 Pa (50 Torr). [twenty five] 25. The method of any one of claims 2 to 4 or 23 to 24, wherein the reducing environment is substantially free of oxygen.
[26] 26. The method according to any one of claims 2 to 4 or 23 to 25, wherein the reducing environment is formed predominantly by an inert gas.
[27] 27. The method of claim 26, wherein the inert agent comprises N2.
[28] 28. The method of any one of claims 2-4 or 23-27, wherein the reducing agent comprises methane, carbon monoxide, an ammonia compound, or a combination thereof.
[29] 29. The method of any one of claims 2 to 4 or 23 to 28, wherein the passivation agent comprises CdCl2.
[30] 30. The method of any one of claims 2 to 4 or 23 to 29, wherein the absorber layer comprises selenium.
[31] 31. The method of any one of claims 2-4 or 23-30, wherein the Group V dopant comprises arsenic.
[32] 32. The method of any one of claims 2-4 or 23-31, wherein the selected temperature is in the range of 350 to 500, the selected pressure is in the range of 200 torr to 800 torr, and the selected treatment duration is in the range of 5 minutes to 45 minutes.
[33] The absorber layer has a thickness of 1×10 16 cm -3 From 5×10 20 cm-3 % to 10 at. % of the Group V dopant, and heating the absorber layer in the reducing environment activates between 1 at. % and 10 at. % of the Group V dopant.
[34] and vacuum annealing the absorber film before the absorber layer contacts the passivation agent, the vacuum annealing step being performed at a pressure of 1.3×10 -7 Pa(1×10 -9 Torr) to 1.3 Pa (1 x 10 -2 34. The method of any one of claims 2-4 or 23-33, wherein the absorber film is exposed to a vacuum in the range of pressure (pressure) and temperature in the range of 300 to 500 Torr for a period of time in the range of 10 minutes to 60 minutes.
[35] 35. The method of any one of claims 2-4 or 23-34, wherein the passivation agent comprises one or more of MnCl2, MgCl2, NH4Cl, ZnCl2, and TeCl4.
[36] 36. The method of any one of claims 2-4 or 23-35, wherein the Group V dopant is selected from bismuth, antimony, arsenic, phosphorus, nitrogen, and combinations thereof.
[37] 1. A method for treating a photovoltaic semiconductor absorber layer, comprising the steps of: providing an absorber film doped with a Group V dopant, the absorber film comprising a polycrystalline II-VI semiconductor; contacting at least a portion of the absorber film with CdCl2; providing a reducing gas to create a reducing environment; and heating the absorber film in the reducing environment at a selected temperature and a selected pressure for a selected treatment period. The method includes:
[38] 38. The method of claim 37, wherein the II-VI semiconductor comprises CdTe, the reducing gas comprises hydrogen, and the reducing environment is substantially free of oxygen or other oxidizing agents. method.
[39] The method further includes vacuum annealing the absorber film prior to the contacting step, the vacuum annealing step being performed at a pressure of 1.3×10 -7 Pa(1×10 -9 Torr) to 0.013 Pa (1 x 10 -4 39. The method of claim 37 or 38, wherein the absorber film is exposed to a vacuum in the range of (100 torr) and a temperature in the range of 300-400 C for a period of 10 minutes to 60 minutes.
[40] 1. A method for activating a Group V dopant in a polycrystalline II-VI semiconductor absorber layer, comprising: providing an absorber film doped with a Group V dopant; Optionally, subjecting the absorber film to a first heat treatment in a first heat treatment environment, the first heat treatment environment comprising low pressure or vacuum; passivating the absorber film by contacting at least a portion of the absorber film with a passivation agent; subjecting the absorber film to a second heat treatment in a second heat treatment environment; and providing a reducing gas to the second heat treatment environment to create a reducing environment, thereby activating the dopant, whereby the activated dopant occupies a Group VI vacancy in a II-VI semiconductor crystal lattice; The method includes:
[41] The step of subjecting the absorber film to the second heat treatment includes: 41. The method of claim 40, further comprising exposing the absorber film to the second heat treatment environment for a period of time ranging from about 5 to 45 minutes, the second heat treatment environment having a pressure ranging from about 200 to 800 Torr, a temperature ranging from 350 to 500 C, and a gas composition including a hydrogen partial pressure ranging from about 3 to 50 Torr.
[42] 1. A method of forming a doped semiconductor absorber layer, comprising: disposing an absorber layer of a photovoltaic stack to form an absorber layer, the absorber layer comprising depositing a first material and a second material in one or more layers on the window stack in a first deposition environment; the first material comprises a II-VI semiconductor or a II-VI semiconductor precursor; the second material comprises a Group V dopant or a Group V dopant precursor; Optionally, subjecting the absorber film to a first heat treatment in a first heat treatment environment; contacting at least a portion of the absorber film with a third material, the third material comprising a passivation agent; subjecting the absorber film to a second heat treatment in a second heat treatment environment; and providing a reducing gas to the second heat treatment environment to create a reducing environment. The method includes:
[43] 43. The method of claim 42, further comprising depositing a buffer semiconductor layer over the window stack prior to depositing the first material and the second material.
[44] 44. The method of claim 43, wherein the buffer semiconductor layer comprises CdSe.
[45] the reducing gas is selected from one or more of hydrogen, methane, and carbon monoxide; the passivation agent is a halogen compound selected from one or more of CdCl2, MnCl2, MgCl2, NH4Cl, ZnCl2, and TeCl4; 45. The method of any one of claims 42 to 44, wherein the Group V dopant is selected from bismuth, antimony, arsenic, phosphorus, nitrogen, and combinations thereof.
[46] The Group V dopant precursors are Cd3As2, AsH3, Bi2Te3, Sb2Te3, Cd3P2, Zn3P2, Bi(NO3)3, Bi2S3, PCl3, PH3, Sb 46. The method of any one of claims 42 to 45, wherein the agonist is selected from the group consisting of H3, and AsCl3, and combinations thereof.
[47] 47. The method of any one of claims 42 to 46, wherein the first material comprises selenium.
[48] the II-VI semiconductor includes CdTe; the Group V dopant consists essentially of arsenic; the buffer semiconductor layer further comprises substantially undoped CdTe; the step of disposing the absorber layer further comprises simultaneously depositing the first material and the second material onto the buffer semiconductor layer at a temperature in the range of about 450 to 600 C to form the absorber film; The concentration of arsenic in the absorber film is about 1×10 16 cm -3 From about 5 × 10 20 cm -3 and the passivation agent consists essentially of CdCl2; The reducing gas comprises hydrogen, The step of performing the second heat treatment includes performing the second heat treatment at a temperature in the range of about 375 to 500° C. and a hydrogen partial pressure in the range of 400 to 6,666 Pa (3 to 50 Torr). 43. The method of claim 42, further comprising treating the absorber film at a pressure of about 400-600 Torr for a period of time ranging from 15 to 60 minutes.
[49] The II-VI group semiconductor includes CdTe, and the first heat treatment includes a step of vacuum annealing the absorber film, the step of vacuum annealing being performed at a pressure of 1.3×10 -7 Pa(1×10 -9 Torr) to 0.013 Pa (1 x 10 -449. The method of any one of claims 42 to 48, wherein the absorber film is exposed to a vacuum in the range of 100 torr and a temperature in the range of 300-400C for a period of 10 minutes to 30 minutes, whereby the absorber film comprises Cd-rich CdTe after the first heat treatment.
[50] 50. The method of any one of claims 42 to 49, wherein the II-VI semiconductor comprises CdTe, the method further comprising facilitating the occupation of the Group V dopant into Te vacancies in a CdTe crystal lattice by promoting a reaction between Te and the reducing gas to form a Te-deficient absorber film.
[51] The doped semiconductor absorber layer has a doping ratio of about 1×10 15 cm -3 From 5×10 16 cm -3 51. The method of claim 42, having a p-type charge carrier concentration in the range of
[52] The concentration of the Group V dopant in the doped absorber layer is about 1×10 16 cm -3 From about 5 × 10 20 cm -3 and after the step of heating the absorber film in a reducing environment, 1-10 at. % of the Group V dopant in the absorber layer occupies Group VI type vacancies in a II-VI semiconductor polycrystalline lattice.
[53] 53. The method of any one of claims 42 to 52, wherein the II-VI semiconductor comprises CdTe, the passivation agent comprises CdCl2, and the second heat treatment environment provides a temperature and pressure sufficient to promote a reaction of the reducing gas with the II-VI semiconductor to form hydrogen telluride, HTe.
[54] 54. The method of any one of claims 42 to 53, wherein the second material is deposited simultaneously with the first material.
[55] 55. The method of any one of claims 42 to 54, wherein the steps of subjecting the second heat treatment and contacting the absorber film with the passivation agent are performed simultaneously.
[56] 55. The method of any one of claims 42 to 54, wherein the steps of contacting the absorber film with the passivation agent and subjecting the absorber film to the second heat treatment are performed sequentially, with the contacting step preceding the second heat treatment.
[57] substrate, a transparent conductive oxide (TCO) layer formed on said substrate; a CdSe layer formed on said TCO layer; a back contact comprising nitrogen-doped ZnTe; and an arsenic-doped absorber layer containing cadmium and tellurium and having a thickness of about 0.5 μm to 3.5 μm formed between the CdSe layer and the back contact; wherein the concentration of arsenic dopant in the doped semiconductor absorber layer is about 1×10 through the thickness of the absorber layer. 16 cm -3 From about 5 × 10 20 cm -3 and 0.5 to 5.0 at % of a Group V dopant occupies Te vacancies in the CdTe crystal lattice.
Claims
1. 1. A method for treating a photovoltaic semiconductor absorber layer, comprising the steps of: providing a reducing agent to create a reducing environment; contacting at least a portion of an absorber layer with a passivating agent while subjecting said absorber layer to said reducing environment, wherein said absorber layer is doped with a Group V dopant and said absorber layer comprises cadmium and tellurium; and Annealing the absorber layer with the passivation agent in the reducing environment at a selected temperature and a selected pressure for a selected treatment period. Including, the reducing environment has a total pressure in the range of 200 Torr to 800 Torr, a partial pressure of oxygen in the reducing environment is greater than or equal to 25 millitorr and less than 1 Torr, and a ratio of the partial pressure of the reducing agent to the partial pressure of oxygen is at least 3; method.
2. The method of claim 1 , wherein the reducing environment is formed predominantly of an inert gas.
3. The method of claim 2 , wherein the reducing environment consists essentially of a mixture of hydrogen gas and nitrogen gas.
4. The passivation agent is CdCl 2 The method of claim 1 , comprising:
5. The method of claim 1 , wherein the absorber layer comprises selenium.
6. The method of claim 1 , wherein the Group V dopant comprises arsenic.
7. 2. The method of claim 1, wherein the selected temperature is in the range of 350° C. to 500° C., the selected pressure is in the range of 200 Torr to 800 Torr, and the selected treatment duration is in the range of 5 minutes to 45 minutes.
8. The absorber layer has a thickness of 1×10 16 cm -3 From 5 x 10 20 cm -3 5. The method of claim 1 , wherein the absorber layer comprises a concentration of the Group V dopant between 1 atomic % and 10 atomic % and annealing the absorber layer in the reducing environment activates between 1 atomic % and 10 atomic % of the Group V dopant.
9. The passivation agent is MnCl 2 , MgCl 2 , N.H. 4 Cl, ZnCl 2 , and TeCl 4 The method of claim 1 , comprising one or more of:
10. The method of claim 1 , wherein the Group V dopant is selected from bismuth, antimony, arsenic, phosphorus, nitrogen, and combinations thereof.
11. The method of claim 1 , wherein the reducing environment comprises 99.4% nitrogen.
12. The reducing agent is H 2 , hydrogen sulfide, methane, carbon monoxide, ammonia compounds, or combinations thereof.
13. The reducing agent is H 2 The method of claim 12, comprising:
14. The reducing agent is H 2 and H 2 2. The method of claim 1, wherein the pressure is applied at a partial pressure between 0.24 Torr and 50 Torr.
15. The method of claim 1, wherein the absorber layer is provided in a photovoltaic stack having a substrate, and wherein annealing the absorber layer in the reducing environment is performed after moving the substrate through a plurality of different deposition stations, the plurality of different deposition stations having their own vapor distributors and vapor sources.
16. 13. The method of claim 1, wherein the absorber layer is disposed in the photovoltaic stack through one or more of the following processes: sputtering, spraying, evaporation, molecular beam deposition, pyrolysis, close-proximity sublimation, pulsed laser deposition, chemical vapor deposition, electrochemical deposition, atomic layer deposition, or vapor transport deposition.
17. After the annealing step, the absorber layer has a thickness of 1×10 15 cm -3 ~5×10 16 cm -3 2. The method of claim 1 , wherein the p-type charge carrier concentration is in the range of
Citation Information
Patent Citations
Manufacture of solar cell
JP1993218474A
Manufacture of solar cell
JP1994085297A
Compound semiconductor solar battery and manufacture thereof
JP1998004205A
Cds / cdte thin film solar cells and manufacturing method thereof
KR1020100085769A
Method of providing chloride treatment for a photovoltaic device and a chloride treated photovoltaic device